Synthesis of zeolites with ferrierite structure.

JP2024511575A5Active Publication Date: 2024-10-08CHEVRON USA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023555530
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-03-19
Filing Date
2022-03-15
Publication Date
2024-10-08
Estimated Expiration
2042-03-15

AI Technical Summary

Technical Problem

Existing methods for synthesizing FER framework type zeolites are limited in efficiency and versatility, particularly in utilizing structure-directing agents and crystallization conditions.

Method used

A method involving a reaction mixture comprising silicon, aluminum, structure-directing agents such as n-propylamine, n-butylamine, or isobutylamine, alkali metals, hydroxide ions, water, and seed crystals, under controlled crystallization conditions, to form FER framework type zeolites with specific molar ratios and subsequent treatment to remove structure-directing agents.

Benefits of technology

The method produces high-quality FER framework type zeolites with controlled pore contents and improved crystallization selectivity, allowing for effective catalyst components in conversion processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Zeolites having a ferrierite framework structure are prepared using one or more of n-propylamine, n-butylamine, isobutylamine and n-amylamine as structure directing agents.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for preparing zeolites having a FER framework type. [Background technology]

[0002] Molecular sieve materials are classified by the Structure Committee of the International Zeolite Association according to the IUPAC Zeolite Nomenclature Rules, according to which framework-type zeolites and other crystalline microporous materials with well-defined structures are assigned three-letter codes with the meanings set forth in "Atlas of Zeolite Framework Types" by Ch. Baerlocher, LB McCusker and DH Olson (Elsevier, Sixth Revised Edition, 2007).

[0003] One of the known molecular sieve materials with an established structure is a material designated as FER, which is a molecular sieve with a unique two-dimensional 10- / 8-membered ring channel system. Examples of FER framework type zeolites include ferrierite, FU-9, ISI-6, NU-23, and ZSM-35. FER framework type zeolites are useful catalytic components for various conversion processes such as the isomerization of olefins.

[0004] According to the present disclosure, it has been found that FER framework type zeolites can be synthesized using one or more of n-propylamine, n-butylamine, isobutylamine and n-amylamine as structure directing agents, particularly using alumina-coated silica as a composite source of silicon and aluminum. Summary of the Invention

[0005] In one aspect, a method of synthesizing a FER framework-type zeolite is provided, the method including: (1) forming a reaction mixture comprising: (a) a source of silicon; (b) a source of aluminum; (c) a structure directing agent (Q) comprising n-propylamine, n-butylamine, isobutylamine, n-amylamine, or any combination thereof; (d) a source of alkali metal (M); and (e) a source of hydroxide ions; (f) water; and (g) seed crystals; and (2) treating the reaction mixture under crystallization conditions sufficient to form zeolite crystals.

[0006] In another embodiment, a FER framework type zeolite is provided which, in its as-synthesized form, contains within its pores one or more of n-propylamine, n-butylamine, isobutylamine and n-amylamine. [Brief description of the drawings]

[0007] [Figure 1] 1 shows a powder X-ray diffraction (XRD) pattern of the as-synthesized zeolite of Example 1.

[0008] [Diagram 2] 1 shows a powder XRD pattern of the ammonium-type zeolite of Example 2.

[0009] [Diagram 3] 1 shows scanning electron microscope (SEM) images of the ammonium form of the zeolite of Example 2 at various magnifications.

[0010] [Figure 4] 1 shows the powder XRD pattern of the synthesized zeolite of Example 3.

[0011] [Diagram 5] 1 shows the powder XRD pattern of the synthesized zeolite of Example 4.

[0012] [Figure 6]1 shows the powder XRD pattern of the synthesized zeolite of Example 5.

[0013] [Figure 7] 1 shows the powder XRD pattern of the synthesized zeolite of Example 6.

[0014] [Figure 8] 1 shows a powder XRD pattern of the ammonium-type zeolite of Example 7.

[0015] [Figure 9] 1 shows SEM images of the ammonium form of the zeolite of Example 7 at various magnifications.

[0016] [Figure 10] 1 shows a powder XRD pattern of the ammonium-type zeolite of Example 8.

[0017] [Figure 11] 1 shows SEM images of the ammonium form of the zeolite of Example 8 at various magnifications.

[0018] [Figure 12] 1 shows the powder XRD pattern of the synthesized zeolite of Example 9.

[0019] [Figure 13] 1 shows the powder XRD pattern of the synthesized zeolite of Example 10.

[0020] [Figure 14] 1 shows the powder XRD pattern of the synthesized zeolite of Example 11.

[0021] [Figure 15] 1 shows the powder XRD pattern of the synthesized zeolite of Example 12.

[0022] [Figure 16] 1 shows the powder XRD pattern of the synthesized zeolite of Example 13.

[0023] [Figure 17] 1 shows the powder XRD pattern of the synthesized zeolite of Example 14.

[0024] [Figure 18] 1 shows the powder XRD pattern of the synthesized zeolite of Example 15.

[0025] [Figure 19] 1 shows the powder XRD pattern of the synthesized zeolite of Example 16.

[0026] [Figure 20] 1 shows the powder XRD pattern of the synthesized zeolite of Example 17.

[0027] [Figure 21] 1 shows the powder XRD pattern of the synthesized zeolite of Example 18.

[0028] [Figure 22] 1 shows the powder XRD pattern of the synthesized zeolite of Example 19.

[0029] [Figure 23] 2 shows the powder XRD pattern of the synthesized zeolite of Example 20.

[0030] [Figure 24] 2 shows the powder XRD pattern of the synthesized zeolite of Example 21.

[0031] [Diagram 25] 2 shows the powder XRD pattern of the synthesized zeolite of Example 22.

[0032] [Figure 26] 2 shows the powder XRD pattern of the ammonium-type zeolite of Example 23.

[0033] [Figure 27]1 shows SEM images of the ammonium form of the zeolite of Example 23 at various magnifications.

[0034] [Figure 28] 2 shows the powder XRD pattern of the ammonium-type zeolite of Example 24.

[0035] [Figure 29] 1 shows SEM images of the ammonium form of the zeolite of Example 24 at various magnifications.

[0036] [Diagram 30] 2 shows the powder XRD pattern of the synthesized zeolite of Example 25.

[0037] [Diagram 31] 2 shows the powder XRD pattern of the synthesized zeolite of Example 26.

[0038] [Diagram 32] 2 shows the powder XRD pattern of the synthesized zeolite of Example 27.

[0039] [Diagram 33] 2 shows the powder XRD pattern of the synthesized zeolite of Example 28.

[0040] [Diagram 34] 2 shows the powder XRD pattern of the synthesized zeolite of Example 29. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0041] definition The term "framework type" as used herein has the meaning as set forth in "Atlas of Zeolite Framework Types" by Ch. Baerlocher, LB McCusker and DH Olson (Elsevier, Sixth Revised Edition, 2007).

[0042] The term "FER" refers to the FER topological type recognized by the International Zeolite Association Structure Committee.

[0043] The term "post-synthetic" refers to the form of the zeolite after crystallization and before removal of the structure directing agent.

[0044] The term "SiO2 / Al2O3 molar ratio" may be abbreviated as "SAR."

[0045] Zeolite synthesis FER framework type zeolites are synthesized by (1) forming a reaction mixture comprising (a) a source of silicon, (b) a source of aluminum, (c) a structure directing agent (Q) comprising n-propylamine, n-butylamine, isobutylamine, n-amylamine, or any combination thereof, (d) a source of alkali metal (M), (e) a source of hydroxide ions, (f) water, and (g) seed crystals; and (2) subjecting the reaction mixture to crystallization conditions sufficient to form zeolite crystals.

[0046] The molar ratio composition of the reaction mixture may be within the ranges shown in Table 1. [Table 1] wherein Q comprises n-propylamine, n-butylamine, isobutylamine, n-amylamine, or a combination thereof.

[0047] Suitable silicon sources include colloidal silica, fumed silica, alkali metal silicates, and tetraalkylorthosilicates.

[0048] Suitable aluminum sources include hydrated alumina, aluminum hydroxide, alkali metal aluminates, aluminum alkoxides, and water-soluble aluminum salts (eg, aluminum nitrate).

[0049] Additionally or alternatively, a combined source of silicon and aluminum can be used. The combined source of silicon and aluminum can be an alumina-coated silica. The alumina-coated silica can have a SiO2 / Al2O3 molar ratio of at least 30 (e.g., 30 to 170, or 35 to 100). Two or more alumina-coated silica materials having different silica-alumina molar ratios can be used. The alumina-coated silica material can be used as the sole or primary source of silicon and aluminum in the reaction mixture. If present, another silicon source (e.g., colloidal silica) can be included.

[0050] The structure directing agent (Q) includes one or more of n-propylamine [CH3(CH2)2NH2], n-butylamine [CH3(CH2)3NH2], isobutylamine [(CH3)2CHCH2NH2], and n-amylamine [CH3(CH2)4NH2].

[0051] The alkali metal (M) is usually introduced into the reaction mixture along with a source of hydroxide ions. Examples of such metals include sodium and / or potassium, as well as lithium, rubidium, and cesium.

[0052] The reaction mixture typically contains seed crystals of FER framework zeolite, preferably in an amount of 0.01 to 10,000 ppm (e.g., 100 to 5000 ppm) by weight based on the weight of the reaction mixture. Seeding can be advantageous to improve the selectivity of FER and / or to shorten the crystallization process.

[0053] Crystallization of the desired zeolite from the above reaction mixture can be carried out in a suitable reactor vessel (e.g., polypropylene jars or Teflon-lined or stainless steel autoclaves) under static, tumbling, or stirred conditions at temperatures between 125° C. and 200° C. (e.g., 140° C. to 185° C.) for a time sufficient for crystallization to occur at the temperature employed (e.g., about 24 hours to 240 hours (e.g., 36 hours to 100 hours)). Crystallization is typically carried out under pressure in an autoclave, with the reaction mixture subjected to autogenous pressure.

[0054] Once the desired zeolite crystals have formed, the solid product can be separated from the reaction mixture using standard mechanical separation techniques such as centrifugation or filtration. The recovered crystals are washed with water and then dried for a few seconds to a few minutes (e.g., 5 seconds to 10 minutes for flash drying) or for several hours (e.g., 4 hours to 24 hours for oven drying at 75°C to 150°C) to obtain the as-synthesized zeolite crystals. The drying step can be carried out under vacuum or at atmospheric pressure.

[0055] As a result of the crystallization process, the recovered crystalline zeolite product contains within its pores at least a portion of the structure directing agent used in its synthesis.

[0056] The synthesized zeolite may be subjected to heat treatment, ozone treatment, or other treatment to remove some or all of the structure directing agent used in the synthesis. Removal of the structure directing agent may be accomplished using a heat treatment (e.g., calcination), in which the synthesized material is heated in an atmosphere selected from air, nitrogen, or mixtures thereof at a temperature sufficient to remove some or all of the structure directing agent. Although reduced pressure may be used for the heat treatment, for convenience, atmospheric pressure is preferred. The heat treatment is performed at a temperature of at least 370°C (e.g., 400°C to 700°C) for at least 1 minute and typically not more than 20 hours (e.g., 1 to 8 hours).

[0057] The FER framework type zeolite may contain one or more non-framework alkali metals. It is usually desirable to remove the alkali metal cations by ion exchange and replace them with hydrogen, ammonium, or any metal ion. Thus, the zeolite may be a Na-form zeolite, a K-form zeolite, or a combination of Na-, K-form, etc., or may be an H-form zeolite, an ammonium-form zeolite, or a metal-exchanged zeolite. A typical ion exchange technique involves contacting the synthetic zeolite with a solution containing the desired replacement cation or salt of the cation. Representative ion exchange techniques are widely known in the art. Ion exchange occurs after synthesis and may be performed either before or after the zeolite is calcined. After contact with the salt solution of the desired replacement cation, the zeolite is usually washed with water and dried at a temperature of 65°C to 315°C (e.g., 80°C to 150°C).

[0058] Zeolite characterization In the as-synthesized and anhydrous form, the FER framework zeolites can have chemical compositions, expressed as molar ratios, within the ranges shown in Table 2. [Table 2] wherein Q comprises n-propylamine, n-butylamine, isobutylamine, n-amylamine, or a combination thereof.

[0059] The FER framework zeolites synthesized by the method described herein are characterized by their powder XRD patterns. Representative powder XRD patterns of FER framework zeolites can be found in "Collection of Simulated XRD Powder Patterns for Zeolites" by MMJ Treacy and JB Higgins (Elsevier, Fifth Revised Edition, 2007).

[0060] The X-ray diffraction data reported here were collected by standard techniques using copper Kα radiation. Changes in the molar ratio of framework species in a particular sample due to changes in lattice constants can result in subtle changes in the diffraction pattern. In addition, sufficiently small crystals can affect peak shape and intensity, causing noticeable peak broadening. Subtle changes in the diffraction pattern can also result from changes in the organic compounds used in the preparation. Calcination can also cause slight shifts in the XRD pattern. Despite these small perturbations, the fundamental crystal lattice structure remains unchanged.

[0061] In some embodiments, the FER framework zeolites prepared as described herein have a H of 350 μmol of composition as measured by n-propylamine temperature programmed desorption (TPD). + / g ~ 500 μmol H + / g (e.g., 375 μmol H + / g~450μmolH + The polymer may have a total Bronsted acid site density in the range of (1 / g). EXAMPLES

[0062] The following illustrative examples are not intended to be limiting.

[0063] In the synthesis of Examples 1-29 below, the starting materials were loaded into a 23 mL Teflon liner. The Teflon liner was then capped and sealed inside a steel Parr autoclave. The autoclave was then heated in a convection oven at rolling conditions (43 rpm) with a holding temperature of 170°C for 2-3 days. The products were isolated by filtration, washed with copious amounts of deionized water, and finally dried in air at 85°C.

[0064] The molar ratios and conditions used in the synthesis of Examples 1-29 are summarized in Table 3 below.

[0065] Example 1 4.42 g of 1M NaOH was mixed with 2.43 g of deionized water and 4.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids) was added. Next, 0.35 g of isobutylamine was added, followed by 0.05 g of zeolite FER seeds.

[0066] The powder XRD pattern of the product is shown in Figure 1 and indicates that the material is a FER framework type zeolite.

[0067] Example 2 5.53 g of 1M NaOH was mixed with 5.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids). Next, 0.43 g of isobutylamine was added, followed by 0.05 g of zeolite FER seeds.

[0068] The recovered composite was calcined in air by placing a thin layer in a calcination dish and heating from room temperature to 120 °C at a rate of 1 °C / min and holding at 120 °C for 2 hours. The temperature was then increased at a rate of 1 °C / min to 540 °C and held at 540 °C for 5 hours. The temperature was again increased at 1 °C / min to 595 °C and held at 595 °C for 5 hours. The material was cooled to room temperature.

[0069] The calcined material was converted to the ammonium form by heating in a solution of ammonium nitrate (typically 1 g NH4NO3 / 1 g zeolite in 10 mL H2O at 85 °C for at least 3 h). The material was then filtered. This was repeated twice for a total of 3 exchanges. Finally, the material was washed with deionized water to a conductivity of less than 100 μS / cm and dried in air at 85 °C.

[0070] The acid site density was measured using n-propylamine temperature programmed desorption (TPD) with 423 μmol H + / g.

[0071] Nitrogen micropore volume is 0.14 cm 3 / g (t-plot analysis) and the BET surface area is 324 m 2 / g.

[0072] The material had a SiO2 / Al2O3 molar ratio (SAR) of 30 as determined by inductively coupled plasma-atomic emission spectroscopy (ICP-AES).

[0073] The powder XRD pattern of the ammonium-form material is shown in Figure 2 and indicates that the material is a FER framework-type zeolite. SEM images of the material at various magnifications are shown in Figure 3.

[0074] Example 3 4.42 g of 1M KOH was mixed with 2.45 g of deionized water and 4.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids). Then, 0.35 g of isobutylamine was added, followed by 0.05 g of zeolite FER seeds.

[0075] The powder XRD pattern of the product is shown in FIG. 4 and indicates that the material is a FER framework type zeolite.

[0076] Example 4 In a 23 mL Teflon autoclave, 5.41 g of 1 M NaOH was mixed with 2.45 g of deionized water, 4.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids), and 0.39 g of LUDOX AS-30 colloidal silica. Then, 0.42 g of isobutylamine was added, followed by 0.05 g of zeolite FER seeds.

[0077] The powder XRD pattern of the product is shown in FIG. 5 and indicates that the material is a FER framework type zeolite.

[0078] Example 5 In a 23 mL Teflon autoclave, 5.41 g of 1 M NaOH and 3.15 g of deionized water were mixed with 4.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids) and 0.69 g of LUDOX AS-30 colloidal silica. Then, 0.42 g of isobutylamine was added, followed by 0.05 g of zeolite FER seeds.

[0079] The powder XRD pattern of the product is shown in FIG. 6 and indicates that the material is a FER framework type zeolite.

[0080] Example 6 In a 23 mL Teflon autoclave, 4.74 g of 1 M NaOH was mixed with 2.86 g of deionized water, 3.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids) and 1.00 g of LUDOX AS-30 colloidal silica. Then, 0.37 g of isobutylamine was added, followed by 0.05 g of zeolite FER seeds.

[0081] The powder XRD pattern of the product is shown in FIG. 7 and indicates that the material is a FER framework type zeolite.

[0082] Example 7 In a 23 mL Teflon autoclave, 4.74 g of 1 M NaOH was mixed with 2.86 g of deionized water, 3.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids) and 1.00 g of LUDOX AS-30 colloidal silica. 0.37 g of isobutylamine was then added, followed by 0.05 g of zeolite FER seeds.

[0083] The recovered compound was calcined and then converted to the ammonium form according to the method of Example 2.

[0084] The acid site density was characterized using n-propylamine TPD and found to be 421 μmol H+ / g.

[0085] The nitrogen micropore volume is 0.13 cm 3 / g (t-plot analysis) and the BET surface area is 285 m 2 / g.

[0086] The SiO2 / Al2O3 molar ratio (SAR) was 41 as determined by ICP-AES.

[0087] The powder XRD pattern of the ammonium-form material is shown in Figure 8 and indicates that the material is a FER framework-type zeolite. SEM images of the material at various magnifications are shown in Figure 9.

[0088] Example 8 4.74 g of 1M NaOH was mixed with 3.05 g of deionized water, 2.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids) and 1.80 g of LUDOX® AS-30 colloidal silica. 0.37 g of isobutylamine was then added, followed by 0.05 g of zeolite FER seed crystals.

[0089] The recovered compound was calcined and then converted to the ammonium form according to the method of Example 2.

[0090] The acid site density was characterized using n-propylamine TPD and 400 μmol H + / g.

[0091] The SiO2 / Al2O3 molar ratio (SAR) was 57 as determined by ICP-AES.

[0092] The powder XRD pattern of the ammonium-form material is shown in Figure 10 and indicates that the material is a FER framework-type zeolite with a small amount of STI. SEM images of the material at various magnifications are shown in Figure 11.

[0093] Example 9 4.74 g of 1M NaOH was mixed with 3.14 g of deionized water, 1.50 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids) and 2.20 g of LUDOX® AS-30 colloidal silica. 0.37 g of isobutylamine was then added, followed by 0.05 g of zeolite FER seeds.

[0094] The powder XRD pattern of the composite is shown in FIG. 12 and indicates that the material is a FER framework type zeolite with a small amount of STI.

[0095] Example 10 4.74 g of 1M NaOH was mixed with 3.24 g of deionized water, 1.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids) and 2.59 g of LUDOX® AS-30 colloidal silica. 0.37 g of isobutylamine was then added, followed by 0.05 g of zeolite FER seeds.

[0096] The powder XRD pattern of the composite is shown in FIG. 13 and indicates that the material is a FER framework type zeolite with a small amount of STI.

[0097] Example 11 3.71 g of 1M NaOH was mixed with 2.29 g of deionized water and 3.00 g of Nalco alumina-coated silica DVSZN007 (SAR=100, 26.5% solids). Then, 0.29 g of isobutylamine was added, followed by 0.05 g of zeolite FER seeds.

[0098] The powder XRD pattern of the synthesis shows that the material is a FER framework type zeolite with a small amount of STI, as shown in FIG.

[0099] Example 12 4.63 g of 1M NaOH was mixed with 2.96 g of deionized water and 3.00 g of Nalco alumina-coated silica DVSZN007 (SAR=100, 26.5% solids), followed by the addition of 0.66 g of LUDOX® AS-30 colloidal silica, 0.36 g of isobutylamine, followed by the addition of 0.05 g of zeolite FER seeds.

[0100] The powder XRD pattern of the synthesis shows that the material is a FER framework type zeolite with a small amount of STI, as shown in FIG.

[0101] Example 13 3.71 g of 1M NaOH was mixed with 2.42 g of deionized water and 2.00 g of Nalco alumina-coated silica DVSZN007 (SAR=100, 26.5% solids), followed by the addition of 0.883 g of LUDOX® AS-30 colloidal silica. Next, 0.29 g of isobutylamine was added, followed by the addition of 0.05 g of zeolite FER seeds.

[0102] The powder XRD pattern of the composite shows that the material is a FER framework type zeolite with a small amount of STI, as shown in FIG.

[0103] Example 14 4.32 g of 1M NaOH was mixed with 2.91 g of deionized water and 1.75 g of Nalco alumina-coated silica DVSZN007 (SAR=100, 26.5% solids). Then, 0.34 g of isobutylamine was added, followed by 0.05 g of zeolite FER seeds.

[0104] The powder XRD pattern of the synthesis shows that the material is a FER framework type zeolite with a small amount of STI, as shown in FIG.

[0105] Example 15 6.32 g of 1M NaOH was mixed with 0.60 g of deionized water and 2.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids), followed by the addition of 2.93 g of LUDOX® AS-30 colloidal silica. Next, 0.50 g of isobutylamine was added, followed by the addition of 0.05 g of zeolite FER seeds.

[0106] The powder XRD pattern of the composite shows that the material is a FER framework type zeolite with a small amount of STI, as shown in FIG.

[0107] Example 16 5.53 g of 1M KOH was mixed with 0.20 g of deionized water and 3.50 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids), followed by the addition of 1.17 g of LUDOX® AS-30 colloidal silica. Next, 0.43 g of isobutylamine was added, followed by the addition of 0.05 g of zeolite FER seeds.

[0108] The powder XRD pattern of the synthesis shows that the material is a pure phase FER framework zeolite, as shown in FIG.

[0109] Example 17 6.32 g of 1M KOH was mixed with 0.61 g of deionized water, 2.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids) and 2.93 g of LUDOX® AS-30 colloidal silica. 0.53 g of isobutylamine was then added, followed by 0.05 g of zeolite FER seeds.

[0110] The powder XRD pattern of the synthesis is shown in FIG. 20 and indicates that the material is a FER framework type zeolite with small amounts of STI and layered phases.

[0111] Example 18 5.29g of 1M NaOH was mixed with 5.13g of deionized water, then 0.10g of Reheis F2000 hydrated alumina was added and mixed well. To this was added 1.13g of CAB-O-SIL® M-5 fumed silica and mixed until uniform. 0.41g of isobutylamine was then added, followed by 0.05g of zeolite FER seed crystals.

[0112] The powder XRD pattern of the synthesis is shown in FIG. 21 and indicates that the material is a phase-pure FER framework-type zeolite.

[0113] Example 19 5.66 g of 1M NaOH was mixed with 5.51 g of deionized water, then 0.075 g of Reheis F2000 hydrated alumina was added and mixed well. To this mixture, 1.22 g of CAB-O-SIL® M-5 fumed silica was added and mixed until uniform. 0.44 g of isobutylamine was then added, followed by 0.05 g of zeolite FER seed crystals. The molar ratios are shown in Table 2.

[0114] The powder XRD pattern of the synthesis is shown in FIG. 22 and indicates that the material is a phase-pure FER framework-type zeolite.

[0115] Example 20 5.66 g of 1M NaOH was mixed with 5.52 g of deionized water, then 0.05 g of Reheis F2000 hydrated alumina was added and mixed well. To this mixture, 1.22 g of CAB-O-SIL® M-5 fumed silica was added and mixed until uniform. 0.44 g of isobutylamine was then added, followed by 0.05 g of zeolite FER seed crystals.

[0116] The powder XRD pattern of the composite is shown in FIG. 23 and indicates that the material is a FER framework type zeolite with a small amount of STI.

[0117] Example 21 5.28 g of 1M NaOH was mixed with 5.16 g of deionized water, then 0.035 g of Reheis F2000 hydrated alumina was added and mixed well. To this mixture, 1.13 g of CAB-O-SIL® M-5 fumed silica was added and mixed until uniform. 0.42 g of isobutylamine was then added, followed by 0.05 g of zeolite FER seed crystals.

[0118] The powder XRD pattern of the synthesis is shown in FIG. 24 and indicates that the material is a FER framework type zeolite with small amounts of STI and layered phases.

[0119] Example 22 5.29 g of 1M NaOH was mixed with 4.00 g of Nalco alumina-coated silica DVSZN007 (SAR=100, 26.5% solids). 0.39 g of isobutylamine was then added, followed by 0.05 g of zeolite FER seeds.

[0120] The powder XRD pattern of the composite is shown in FIG. 26 and indicates that the material is a FER framework type zeolite with a small amount of STI.

[0121] Example 23 4.94 g of 1M NaOH was mixed with 0.24 g of deionized water and 4.00 g of Nalco alumina-coated silica DVSZN007 (SAR=100, 26.5% solids). 0.39 g of isobutylamine was then added, followed by 0.05 g of zeolite FER seeds.

[0122] The recovered compound was calcined and then converted to the ammonium form according to the method of Example 2.

[0123] The acid site density was characterized using n-propylamine TPD and 425 μmol H + / g.

[0124] The nitrogen micropore volume was estimated to be 0.06 cm by t-plot analysis.3 / g and the BET surface area is 147 m 2 / g.

[0125] The SiO2 / Al2O3 molar ratio (SAR) was 77 as determined by ICP-AES.

[0126] The powder XRD pattern of the ammonium-form material is shown in Figure 26 and indicates that the material is a FER framework-type zeolite with small amounts of impurities. Figure 27 shows SEM images of the material at various magnifications.

[0127] Example 24 4.41 g of 1M NaOH was mixed with 0.75 g of deionized water and 4.00 g of Nalco alumina-coated silica DVSZN007 (SAR=100). 0.39 g of isobutylamine was then added, followed by 0.05 g of zeolite FER seed crystals. The molar ratios are shown in Table 2.

[0128] The recovered compound was calcined and then converted to the ammonium form according to the method of Example 2.

[0129] The acid site density was characterized using n-propylamine TPD and found to be 424 μmol H + / g.

[0130] The nitrogen micropore volume was estimated to be 0.05 cm by t-plot analysis. 3 / g and the BET surface area is 134 m 2 / g.

[0131] The SiO2 / Al2O3 molar ratio (SAR) was 81 as determined by ICP-AES.

[0132] The powder XRD pattern of the ammonium-form material is shown in Figure 28 and indicates that the material is a FER framework-type zeolite with small amounts of impurities. Figure 29 shows SEM images of the material at various magnifications.

[0133] Example 25 3.53 g of 1M NaOH was mixed with 1.59 g of deionized water and 4.00 g of Nalco alumina-coated silica DVSZN007 (SAR=100, 26.5% solids). 0.39 g of isobutylamine was then added, followed by 0.05 g of zeolite FER seeds.

[0134] The powder XRD pattern of the composite is shown in FIG. 30 and indicates that the material is a FER framework type zeolite with small amounts of STI and layered phases.

[0135] Example 26 4.42 g of 1M NaOH was mixed with 4.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids), then 0.28 g of n-propylamine was added, followed by 0.05 g of zeolite FER seed crystals.

[0136] The powder XRD pattern of the synthesis is shown in FIG. 31 and indicates that the material is a pure FER framework zeolite.

[0137] Example 27 4.42 g of 1M NaOH was mixed with 4.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids), then 0.48 g of dipropylamine was added, followed by 0.05 g of zeolite FER seed crystals.

[0138] The powder XRD pattern of the synthesis is shown in FIG. 32 and indicates that the material is an MFI framework type zeolite.

[0139] Example 28 4.42 g of 1M NaOH was mixed with 4.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids), then 0.35 g of n-butylamine was added, followed by 0.05 g of zeolite FER seed crystals.

[0140] The powder XRD pattern of the synthesis is shown in FIG. 33 and indicates that the material is a pure FER framework zeolite.

[0141] Example 29 4.42 g of 1M NaOH was mixed with 4.00 g of Nalco alumina-coated silica DVSZN007 (SAR=35, 24.5% solids). 0.41 g of n-amylamine was then added, followed by 0.05 g of zeolite FER seed crystals.

[0142] The powder XRD pattern of the composite is shown in FIG. 34 and indicates that the material is a mixture of FER and MFI framework-type zeolites. [Table 3] [Table 3] [Table 3] [Table 3] (a) Note: "Nalco(35)" stands for Nalco alumina-coated silica (SAR=35), "Nalco(100)" stands for Nalco alumina-coated silica (SAR=100), "Ludox" stands for LUDOX® AS-30 colloidal silica, "Cabosil" stands for CAB-O-SIL® M-5 fumed silica, and "Reheis" stands for Reheis F2000 hydrated alumina.

Claims

1. 1. A method for synthesizing a FER framework type zeolite, the method comprising: (1) forming a reaction mixture, the reaction mixture comprising: (a) a source of silicon; (b) a source of aluminum; (c) a structure directing agent (Q) consisting of isobutylamine, n-amylamine, or a combination thereof; (d) a source of alkali metal (M); (e) a source of hydroxide ions; (f) water, and (g) forming a seed crystal; and (2) subjecting the reaction mixture to crystallization conditions sufficient to form crystals of the zeolite; The process, wherein the molar ratio composition of the reaction mixture is as follows: 【Table 1B】

2. 10. The method of claim 1, wherein the reaction mixture comprises alumina-coated silica as a combined source of silicon and aluminum.

3. The method of claim 1 , wherein the alkali metal is sodium, potassium, or a combination thereof.

4. The method of claim 1 , wherein the seed crystals comprise a FER framework type zeolite.

5. 10. The method of claim 1, wherein the reaction mixture comprises from 0.01 ppm to 10,000 ppm by weight of seed crystals.

6. 10. The method of claim 1, wherein the crystallization conditions include heating the reaction under autogenous pressure at a temperature between 125° C. and 200° C. for a period of 24 hours to 240 hours.

7. A zeolite of the FER framework type, which in its as-synthesized form contains within its pores one or more of isobutylamine and n-amylamine.

8. SiO 2 / Al 2 O 3 The zeolite according to claim 7, wherein the molar ratio of is in the range of 20 to 100.

9. SiO 2 / Al 2 O 3 The zeolite according to claim 7, wherein the molar ratio of is in the range of 25 to 85.

10. Bronsted acid site density is 350 μmol H + / g to 500 μmol H + The zeolite of claim 7, wherein the molecular weight is in the range of 1 / g.