Organotemplate-free FER synthesis

The preparation of ferrosteine ​​zeolite by the non-organic template method solves the problems of high synthesis cost and insufficient catalytic performance in the prior art, and realizes efficient NOx conversion and low-cost process, which improves the activity of the catalyst.

CN118984808APending Publication Date: 2024-11-19JOHNSON MATTHEY PLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032951.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-17
Filing Date
2023-05-17
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art has problems with high cost and low yields when synthesizing ferrosteine ​​zeolite (FER) catalysts, and the catalytic performance of conventional methods is insufficient, making it difficult to effectively reduce the NOx conversion rate.

Method used

The zeolite is formed by using an inorganic template method. The zeolite is prepared by forming a reaction gel containing an aluminum source, sodium hydroxide and silica sol and heating at a suitable temperature to grow the FER zeolite, avoiding the use of seed crystals and organic structure guides. FER zeolite with improved catalytic properties.

Benefits of technology

The efficient catalytic performance of FER zeolite is achieved, especially in the significant improvement in NOx conversion rate, while reducing the cost of synthesis process and improving the Al distribution and Fe species formation, the activity of the catalyst is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005073732470000141
    Figure BDA0005073732470000141
  • Figure BDA0005073732470000151
    Figure BDA0005073732470000151
  • Figure HDA0005073732480000011
    Figure HDA0005073732480000011
Patent Text Reader

Abstract

An organotemplate-free process for the manufacture of a ferrierite (FER) zeolite and a ferrierite that can be produced by the process. The method comprises (i) forming a reaction gel comprising an aluminum source, sodium hydroxide and / or potassium hydroxide, and a silica sol; and (ii) heating the reaction gel to a temperature suitable for growth of the FER zeolite and for a duration suitable for growth of the FER zeolite. The reaction gel does not contain seed crystals. In addition, the reaction gel does not contain an organic structure directing agent (OSDA). The ferrierite (FER) zeolite has the following features: a) a SAR of between 11 and 20; b) a BET surface area between 320 m < 2 > / g and 380 m < 2 > / g; and c) a micropore volume of between 0.1 cm < 3 > / g and 0.2 cm < 3 > / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to ferrierite (FER) zeolite. The present invention also relates to a method for making ferrierite. The present invention also relates to a catalyst article comprising ferrierite and a method for treating exhaust gas comprising contacting the exhaust gas with a catalyst article comprising FER zeolite. Background Art

[0002] Zeolites are crystalline or quasicrystalline aluminosilicates composed of repeating TO4 tetrahedral units (or combinations of tetrahedral units), where T is most commonly Si and Al. These units are linked together to form a framework with regular cavities and / or molecular-sized channels within the crystal. Many types of synthetic zeolites have been synthesized, and each zeolite has a unique framework based on a specific arrangement of its tetrahedral units. According to the IUPAC nomenclature, each topological type is designated by a unique three-letter code (e.g., "FER") (http: / / www.iza-structure.org / data / ) of the International Zeolite Association (IZA).

[0003] Zeolites have many industrial applications, and certain framework zeolites such as FER are known to be effective catalysts for treating combustion exhaust gases in industrial applications including internal combustion engines, gas turbines, coal-fired power plants, etc. In one example, nitrogen oxides (NO x ) can be reduced by the so-called selective catalytic reduction (SCR) process (whereby NO x The compound is contacted with a reducing agent in the presence of a zeolite catalyst).

[0004] Synthetic zeolites of the FER topology type are generally produced using a structure directing agent (SDA) (also known as a "template" or "templating agent") when prepared as aluminosilicate compositions. The SDA used to prepare aluminosilicate FER topology type materials is generally a complex organic molecule that guides or directs the molecular shape and pattern of the zeolite framework. Generally speaking, the SDA can be thought of as a mold around which the zeolite crystals are formed. After the crystals are formed, the SDA is removed from the internal structure of the crystal, leaving behind a molecularly porous aluminosilicate cage.

[0005] In a typical synthesis technique, solid zeolite crystals are formed from a reaction mixture containing framework reactants (e.g., a silica source and an alumina source), a hydroxide ion source (e.g., NaOH), and SDA. Such synthesis techniques typically require several days (depending on factors such as the crystallization temperature) to achieve the desired crystallization. When crystallization is complete, the solid product containing the zeolite crystals is separated from the discarded mother liquor. The discarded mother liquor contains unused SDA (which is typically degraded due to the harsh reaction conditions) and unreacted silica.

[0006] The SDA used in the synthesis of FER zeolites is relatively expensive and constitutes a significant portion of the cost of manufacturing the zeolites, and also generates a large amount of waste. In addition, conventional methods for synthesizing zeolite FER based on SDA (a key component of the reaction mixture) have relatively poor yields, which also affects the manufacturing cost.

[0007] Various prior art documents disclose the synthesis of FER without an organic structure directing agent (OSDA), but use zeolite seeds to assist the synthesis (see Chemical Engineering & Technology, 2002, 25, 273; JACS, 2012, 134, 11542; Microporous and Mesoporous Materials, 2014, 196, 89; and Journal of Materials Chemistry, 2011, 21, 9494). Other methods use templates to prepare FER (see WO 2020 / 021054 and Microporous and Mesoporous Materials, 2020, 296, 109988). US 4,650,654 discloses the synthesis of FER zeolites without using an organic mineralizer and without using aqueous colloidal silica as a silica source. However, the FER prepared by these methods did not show improved catalytic performance.

[0008] The present inventors have found that the FER zeolite formed by the present invention has improved catalytic performance compared to the prior art. Without being bound by theory, it is believed that the specific method of preparing FER as outlined herein allows for control of the Al distribution in the FER framework and thus positively affects the Fe species formation by promoting monomer and dimer active species.

[0009] There remains a need in the art for improved FER zeolites with improved catalytic properties, such as improved NOx conversion. Additionally, it would be desirable to reduce the cost of the synthesis process, preferably in a manner that has a low impact on the environment. The present invention satisfies these needs, among others. Summary of the invention

[0010] One aspect of the present disclosure relates to a ferrierite (FER) zeolite having the following characteristics:

[0011] a) SAR between 11 and 20;

[0012] b) between 320m 2 / g and 380m 2 / g;

[0013] c) between 0.1cm 3 / g and 0.2cm 3 / g of micropore volume.

[0014] Another aspect of the present disclosure relates to an organotemplate-free method for making a ferrierite (FER) zeolite, the method comprising:

[0015] (i) forming a reaction gel comprising an aluminum source, sodium hydroxide and / or potassium hydroxide and silica sol,

[0016] (ii) heating the reaction gel to a temperature suitable for the growth of FER zeolite and for a period of time suitable for the growth of FER zeolite,

[0017] wherein the reaction gel does not contain seed crystals, and further wherein the reaction gel does not contain an organic structure directing agent (OSDA).

[0018] Another aspect of the present disclosure relates to a catalyst article for treating exhaust gas, the catalyst article comprising a FER zeolite as described herein or obtainable by a method as described herein.

[0019] Another aspect of the present disclosure relates to a method for treating an exhaust gas, the method comprising contacting the exhaust gas with a catalyst article described herein. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Powder X-ray diffraction (XRD) patterns of the H-type FER structures prepared in Examples 2 and 7 and Comparative Examples CE2 and CE3 are shown.

[0021] Figure 2 A scanning electron micrograph (SEM) of the H-FER from Example 2 is shown.

[0022] Figure 3 The H-type FER sample from Example 2 is shown. 27 Al solid-state MAS NMR.

[0023] Figure 4 Shown are the NOx conversions of fresh and aged iron FER samples (H-type Example 2) for selective catalytic reduction (SCR) of NOx compared to Comparative Example CE2.

[0024] Figure 5 Shown are the NOx conversions of fresh and aged iron FER samples (H-type Example 7) compared to Comparative Example CE3 for Selective Catalytic Reduction (SCR) of NOx. DETAILED DESCRIPTION

[0025] A first aspect of the present invention relates to a ferrierite (FER) zeolite having the following characteristics:

[0026] a) SAR (SiO2 / Al2O3) between 11 and 20;

[0027] b) between 320m 2 / g and 380m 2 / g; and

[0028] c) between 0.1cm 3 / g and 0.2cm 3 / g of micropore volume.

[0029] The present disclosure will now be further described. In the following paragraphs, different aspects / embodiments of the present disclosure are defined in more detail. Unless there is a clear contrary description, each aspect / embodiment so defined may be combined with any other aspect / embodiment or multiple aspects / embodiments. In particular, any feature indicated as being preferred or advantageous may be combined with any other one or more features indicated as being preferred or advantageous.

[0030] The FER zeolite according to the present invention may be a hydrogen-type (H-type) FER zeolite. The term "H-type" FER zeolite refers to a FER zeolite in which the framework charge is substantially balanced by protons. In this form, the FER zeolite generally contains H in the exchange sites. + and a mixture of alkali metal and / or alkaline earth metal cations. The H-form of the FER zeolite may be ≥90%, ≥95%, ≥96%, ≥97%, ≥98% or ≥99% (by weight) of the H-form. The amount of the H-form of the FER zeolite may vary depending on the specific FER zeolite batch and the method used to form the FER zeolite.

[0031] Preferably, the FER zeolite of the present invention has a SAR of at most 20, preferably at most 19, preferably at most 18, more preferably at most 17 and even more preferably at most 16. In some embodiments, it is also preferred that the CHA zeolite has a SAR of at least 11 or at least 12. In some embodiments, it is preferred that the CHA zeolite has a SAR of 11 to 20, 12 to 19, 13 to 18, 14 to 17 or 15 to 16 (e.g., 11 to 19, 11.5 to 17.5 or 12 to 17).

[0032] As used herein, SAR (SiO2 / Al2O3) refers to a synthesized zeolite crystal, and not an initial synthetic gel. The SAR of a zeolite can be determined by conventional analysis. This ratio is intended to be as close as possible to the ratio in the rigid atomic framework of the zeolite crystal, and is intended to exclude silicon or aluminum in the binder or in the form of cations or other forms in the channel. Since it may be difficult to directly measure the silica to alumina ratio (SAR) of a zeolite after combining a zeolite with a binder material, particularly an alumina binder, these silica to alumina ratios will be relative to the SAR zeolite itself (i.e., before the zeolite is combined with other catalyst components).

[0033] In combination with the desired SAR, the present invention can provide FER zeolites having the following BET surface areas: 320 m 2 / g to 380m 2 / g; preferably, 330m 2 / g to 375m 2 / g, for example 340m 2 / g to 370m 2 / g; 345m 2 / g to 365m 2 / g, 348m 2 / g to 364m 2 / g, 349m 2 / g to 363m 2 / g, 350m 2 / g to 360m 2 / g, 351m 2 / g to 359m 2 / g, 352m 2 / g to 358m 2 / g or 353m 2 / g to 357m 2 / g.

[0034] In combination with the desired SAR, the present invention can provide FER zeolites with micropore volumes of: 0.1 cm 3 / g-0.2cm 3 / g; preferably 0.11cm 3 / g-0.18cm 3 / g; or more preferably 0.11cm 3 / g-0.15cm 3 / g, for example 0.11cm 3 / g to 0.14cm 3 / g or 0.12cm 3 / g to 0.13cm 3 In another embodiment, the micropore volume of the FER zeolite is 0.12 cm3 / g.

[0035] The present invention, alone or in combination with any of the desired features described herein, can provide a FER zeolite having a mesopore volume of: 0.01 cm 3 / g to 0.1cm 3 / g, preferably 0.015cm 3 / g to 0.08cm 3 / g, more preferably 0.02cm 3 / g to 0.05cm 3 / g, 0.025cm 3 / g to 0.045cm 3 / g, for example 0.03cm 3 / g to 0.04cm 3 In a preferred embodiment, the mesopore volume is 0.01 cm 3 / g to 0.06cm 3 / g, for example 0.015cm 3 / g to 0.05cm 3 / g.

[0036] The present invention can provide a device having a diameter of less than 35 m 2 / g, preferably not more than 30m 2 / g, more preferably not more than 25m 2 / g of external surface area. In some embodiments, the FER zeolite may have an external surface area of ​​no greater than 24 m 2 / g, not more than 22m 2 / g, not more than 21m 2 / g, not more than 20m 2 / g, not more than 19m 2 / g, not more than 18m 2 / g, not more than 17m 2 / g, not more than 16m 2 / g, not more than 15m 2 / g, not more than 14m 2 / g, not more than 12m 2 / g or not more than 10m 2 In certain embodiments, the FER zeolite may have an external surface area of ​​0 m 2 / g-35m 2 / g, 1m 2 / g-30m 2 / g, 2m 2 / g-25m 2 / g or 3m 2 / g-24m2 / g, 4m 2 / g-22m 2 / g, 5m 2 / g-20m 2 / g, 6m 2 / g-18m 2 / g, 7m 2 / g-17m 2 / g, 8m 2 / g-15m 2 / g or 9m 2 / g-12m 2 / g (e.g. 8m 2 / g to 25m 2 / g, for example 9m 2 / g to 20m 2 / g, 10m 2 / g to 19m 2 / g, 11m 2 / g to 18m 2 / g, 12m 2 / g to 17m 2 / g or 13m 2 / g to 16m 2 In a preferred embodiment, the surface area is 10 m 2 / g to 20m 2 / g.

[0037] Any conventional technique in the art can be used to measure the external surface area. For example, according to the Brunauer-Emmett-Teller (BET) method, the Ar or N adsorption isotherms on the activated sample are measured at 87K or 77K, respectively. Prior to the measurement, the sample is heated under vacuum to remove physically adsorbed water. The pore size distribution is measured by non-local density functional theory (NLDFT). The external surface area is calculated by the difference between the apparent BET and the micropore surface area.

[0038] Preferably, the FER zeolite has a crystallinity greater than 95%, such as greater than 97% or greater than 98%. The FER zeolite may be substantially free of other crystalline phases, and typically it is not an intergrowth of two or more framework types. As used herein, the term "substantially free" means that the zeolite contains less than about 5, 4, 3, 2, 1, 0.5, 0.1, 0.05, 0.01 weight percent of a specified framework impurity or all impurities.

[0039] Preferably, the FER zeolite has a platelet-like morphology. That is, preferably, the zeolite has a morphology in which the zeolite crystals have a substantially planar or one-dimensional shape, or disc-like or plate-like particles having a two-dimensional shape as opposed to particles having a three-dimensional shape.

[0040] Preferably, the FER zeolite has an average longest side crystal size of no greater than 1 micron, preferably no greater than 0.9 micron. In some embodiments, the FER zeolite may have an average longest side crystal size of 0.01 micron to 1 micron (e.g., 0.1 micron to 0.9 micron, 0.2 micron to 0.8 micron, 0.25 micron to 0.7 micron, 0.3 micron to 0.6 micron, or 0.4 micron to 0.5 micron). This average crystal size can be determined using standard microscopic techniques such as scanning electron microscopy (SEM). The measurement is performed on a statistically significant portion of the produced zeolite.

[0041] In another embodiment, the 6-twice Al is less than or equal to 15%, for example, less than 15%, less than 14%, less than 12%, less than 10%. In some embodiments, the 6-twice Al is 3% to 15%, 3.5% to 14%, 4% to 13%, 5% to 12%, 6% to 10%. The 6-twice Al can be prepared using standard techniques such as 27 The Al solid state MAS-NMR spectrum can be quantified by integrating over the range of 80 ppm to -30 ppm to cover all observed isotropic peaks and over the range of 15 ppm to -30 ppm to cover only the 6-fold Al. These measurements can be performed on the hydrogen form of the FER zeolite.

[0042] In a preferred embodiment, the FER zeolite according to the present invention does not contain or is substantially free of one or more of the following: fluorine, fluorine-containing compounds and fluoride ions. Preferably, the FER zeolite according to the present invention does not contain or is substantially free of all of the following: fluorine, fluorine-containing compounds and fluoride ions. By "substantially free" is meant that the zeolite contains less than 0.1% (e.g., less than 0.08%, less than 0.05%, less than 0.03%, less than 0.02%, less than 0.01%, less than 0.005%, less than 0.001%) (by weight based on the total weight of the zeolite) of undesirable components.

[0043] In another aspect of the present invention, there is provided a method for producing a ferrierite (FER) zeolite, the method comprising:

[0044] (i) forming a reaction gel comprising an aluminum source, sodium hydroxide and / or potassium hydroxide and silica sol,

[0045] (ii) heating the reaction gel to a temperature suitable for the growth of FER zeolite and for a period of time suitable for the growth of FER zeolite,

[0046] wherein the reaction gel does not contain seed crystals, and further wherein the reaction gel does not contain an organic structure directing agent (OSDA).

[0047] It is particularly preferred that the process described herein is used to prepare the FER zeolites described herein.

[0048] The method for preparing ferrierite may include forming a reaction gel, which may also be referred to as a reaction mixture. Such reaction gels are well known in the field of zeolite synthesis. The reaction gel of the method for preparing ferrierite comprises an aluminum source, sodium hydroxide / potassium hydroxide and a silica sol. Examples of aluminum sources include sodium aluminate, aluminum salts such as aluminum sulfate, aluminum nitrate, aluminum chloride, aluminum hydroxide, aluminum alkoxide and aluminum oxide, preferably one or more of sodium aluminate and aluminum hydroxide. A silica sol is a colloidal suspension of silicon dioxide in water. In a preferred embodiment, the reaction gel comprises sodium aluminate, sodium hydroxide and a silica sol solution.

[0049] As is known in the art, the reaction composition can be described in terms of the equivalents of SiO2, Al2O3, M2O (where M is an alkali metal and / or alkaline earth metal), and H2O present in the reaction gel. In other words, the reaction gel composition can be described by the ratio Al2O3:aSiO2:bM2O:cH2O, where the reaction composition is normalized to the molar amount of Al2O3 equivalents (1 mole). It should be understood that the scale and absolute molar number of the reaction can vary.

[0050] In some embodiments, the amount of M2O equivalents, i.e., the total amount of all M2O equivalents (e.g., one or both of Na2O and K2O may be present), is at least 1 mole, preferably 1 to 10 moles, more preferably 2 to 8 moles, and more preferably 2.2 to 6 moles, relative to the molar amount of Al2O3 equivalents. Similarly, it can be said that "b" in the gel composition can be any of these ranges or values. In some particularly preferred embodiments, the amount of M2O equivalents is 1 to 8 moles relative to the molar amount of Al2O3 equivalents in the reaction gel. When a lower amount of M2O equivalents is preferred, the amount of M2O equivalents is preferably 1.5 to 7 moles, preferably 2 to 6 moles. M can be selected from one or more alkali metals or alkaline earth metals. Preferably, M is selected from one or more of the list comprising (e.g., consisting of) the following items: Na, K, Li, Cs, Sr and Ba. In a preferred embodiment, M is Na.

[0051] In some embodiments, it is preferred that the gel comprises an amount of SiO2 equivalents of at least 10 moles, preferably 10 to 50 moles, 12 to 40 moles, or 13 to 35 moles, relative to the molar amount of Al2O3 equivalents. Likewise, it can be said that "a" in the gel composition can be any of these ranges or values. For example, in some embodiments, higher amounts of SiO2 equivalents are preferred, such as 14 to 33 moles, preferably 15 to 30 moles, or 20 to 25 moles. In some preferred embodiments, about 20 moles of SiO2 equivalents are preferred.

[0052] In some embodiments, it is preferred that the gel contains water and that the water is present in an amount of at least 700 moles, preferably 750 moles to 4000 moles, relative to the molar amount of Al2O3 equivalents. Likewise, it can be said that "c" in the gel composition can be any of these ranges or values. For example, in some embodiments, higher amounts of water are preferred (especially when adding higher amounts of SiO2 equivalents or M2O equivalents), such as 800 moles to 3000 moles, preferably 900 moles to 1250 moles, such as about 1000 moles.

[0053] In some embodiments, the reaction gel composition has a Na2O / SiO2 ratio of 0.05 to 0.3 (e.g., 0.06 to 0.25, 0.07 to 0.22, 0.08 to 0.2, 0.09 to 0.19, 0.1 to 0.18, 0.11 to 0.17, 0.12 to 0.16, 0.13 to 0.17, or 0.14 to 0.16). In a preferred embodiment, the Na2O / SiO2 ratio is 0.08 to 0.21, 0.09 to 0.2, or 0.1 to 0.18.

[0054] In some embodiments, the reaction gel composition has a K2O / (K2O+Na2O) ratio of less than 0.1 (e.g., less than 0.099, less than 0.095, less than 0.09, less than 0.08, less than 0.07). In some embodiments, the reaction gel has a K2O / (K2O+Na2O) ratio of 0 to 0.099, 0.01 to 0.095, or 0.015 to 0.09.

[0055] In some embodiments, the reaction gel composition has a H2O / SiO2 ratio of 45 to 110 (eg, 50 to 100).

[0056] The reaction gel used to prepare ferrierite is a gel that does not contain an organic structure directing agent, that is, the reaction gel does not contain an organic structure directing agent (OSDA). The so-called "does not contain an organic structure directing agent" means that the reaction gel contains less than 1 wt% of an organic structure directing agent, such as less than 0.9 wt%, less than 0.5 wt%, less than 0.3 wt%, less than 0.2 wt%, less than 0.1 wt% or less than 0.01 wt% of an organic structure directing agent based on the total weight of the reaction gel. In a preferred embodiment, the reaction gel contains 0 wt% of an organic structure directing agent.

[0057] A particular advantage of the process of the present invention is that the inventors have found that the process does not require the use of seed crystals to form the desired FER zeolite. Therefore, the reaction gel does not contain seed crystals (e.g., FER seed crystals). By "does not contain seed crystals" is meant that the reaction gel contains less than 0.1% seed crystals, e.g., less than 0.08%, less than 0.05%, less than 0.03%, less than 0.02%, less than 0.01%, less than 0.005%, less than 0.001% seed crystals, based on the total weight of the reaction gel. In a preferred embodiment, the reaction gel contains 0% by weight of seed crystals.

[0058] In a preferred embodiment, the reaction gel contains no or substantially no one or more of the following: fluorine, fluorine-containing compounds and fluoride ions. Preferably, the reaction gel contains no or substantially no all of the following: fluorine, fluorine-containing compounds and fluoride ions. By "substantially free", it is meant that the zeolite contains less than 0.1% (e.g., less than 0.08%, less than 0.05%, less than 0.03%, less than 0.02%, less than 0.01%, less than 0.005%, less than 0.001%) (by weight based on the total weight of the zeolite) of undesirable components.

[0059] In a particularly preferred embodiment of the invention, the reaction gel consists of an aluminum source, sodium hydroxide, silica sol and water and optionally other sodium and / or potassium salts.

[0060] The heating of the reaction gel for preparing ferrierite is carried out at a temperature suitable for the growth of FER zeolite and for a time suitable for the growth of FER zeolite. Preferably, the temperature to which the reaction gel is heated for such a suitable time is 100°C to 220°C; more preferably 110°C to 210°C, 120°C to 200°C, 130°C to 190°C or even 140°C to 180°C. The time for which the reaction gel is heated to a suitable temperature is preferably at least 10 hours, more preferably 20 hours to 8 days, 1 day to 7 days, for example 1 day to 6 days. It is particularly preferred that the reaction gel is heated to these temperatures and maintained at these temperatures for these time periods, for example at a temperature of 100°C to 220°C for at least 10 hours.

[0061] Preferably, the FER zeolite product produced by heating the reaction gel to such a temperature and duration is recovered by typical vacuum filtration. Preferably, the filtered product is washed with demineralized (also called deionized) water to remove residual mother liquor. Preferably, the zeolite product is washed until the filtrate conductivity is less than 0.1 mS. Preferably, the filtered and washed product is then dried at a temperature greater than 100° C., preferably about 120° C. The FER zeolite product can be filtered by vacuum filtration and washed with demineralized water.

[0062] The method of the present invention may also include one or more steps to remove metal ions such as alkali metal ions from the FER ion exchange sites. Typically, alkali metal ions react with non-metallic cations such as ammonium ions (NH4 + ) or protons (H + ) exchange. Ion exchange with ammonium ions can be performed by mixing the zeolite into an aqueous ammonium sulfate solution followed by stirring. In addition, ion exchange for protons can be performed by ion exchanging the zeolite with ammonia and calcining it, preferably in an oxygen-containing environment (such as in air) at a temperature of about 450° C. to 600° C., preferably about 500° C. to 550° C., for a period of about 25 hours to 40 hours (e.g., about 30 hours to 35 hours).

[0063] The FER zeolite of the present invention can be used as a catalyst and / or adsorbent. In a preferred example, one or more catalytically active metals or metals that otherwise improve the performance of the catalyst composition (collectively referred to as "enhancing metals") are exchanged into the FER zeolite. The exchange of the enhancing metal can be completed after the zeolite is synthesized via incipient wetness impregnation, solid-state ion exchange, or during the preparation of the carrier coating slurry, or in situ during the synthesis step by adding the enhancing metal to the reaction mixture. Any of the above metals can be used in combination with any of the other methods, for example, to incorporate two or more enhancing metals into the zeolite.

[0064] Preferably, the enhancing metal is a non-framework metal. As used herein, a "non-framework metal" is a metal located within the pores of the zeolite and / or on at least a portion of the surface of the zeolite, preferably as an ionic species, excluding aluminum, and excluding atoms that make up the framework of the zeolite. Preferably, the presence of the enhancing metal promotes the treatment of exhaust gases such as exhaust gases from diesel engines, including such as NO x Reduction, NH3 oxidation and NO x Storage method.

[0065] Enhancement metals include certain transition metals such as copper (Cu), iron (Fe), manganese (Mn), nickel (Ni), molybdenum (Mo) and zinc (Zn), preferably copper and / or iron, and most preferably copper. Certain enhancement metals are noble metals such as gold (Au) and silver (Ag), and platinum group metals such as platinum (Pt), palladium (Pd), ruthenium (Ru) and rhodium (Rh). In addition, the enhancement metal can be one or more rare earth metals such as cerium (Ce), praseodymium (Pr), neodymium (Nd), europium (Eu), erbium (Er), gadolinium (Gd), ytterbium (Yb) and yttrium (Y), which can be used to improve catalytic performance, especially when used in combination with transition metals. (Although yttrium can be described as a transition metal, it is referred to as a rare earth metal herein due to its lanthanide-like properties.)

[0066] One or more enhancing metals are preferably present in a concentration of about 0.1 weight percent (wt%) to about 10 wt%, such as about 0.5 wt% to about 5 wt%, about 0.5 wt% to about 1 wt%, about 1 wt% to about 1.5 wt%, about 1 wt% to about 2 wt%, about 1 wt% to about 5 wt%, about 2.5 wt% to about 3.5 wt%, and about 3.5 wt% to about 5 wt%, based on the total weight of the zeolite. For embodiments utilizing two or more enhancing metals, each metal may be independently present in the above amounts.

[0067] When copper, iron or combinations thereof are used as enhancing metals, they are preferably present in the FER zeolite material at a concentration of about 1 weight percent to about 5 weight percent, more preferably about 2.5 weight percent to about 4.5 weight percent of these transition metals based on the total weight of the FER zeolite.

[0068] In another embodiment, the method for preparing ferrierite may further include the step of loading iron onto the FER zeolite formed in step ii) by ion exchange (e.g., by using an iron source, such as an iron source selected from iron (II) chloride or ammonium ferric oxalate). For example, the method for preparing ferrierite may further include the step of loading iron onto the FER zeolite by ion exchange with an iron source selected from iron (II) chloride or ammonium ferric oxalate.

[0069] In another embodiment, ferrierite as described herein or as obtained by a process as described herein may be present in the catalyst composition.

[0070] The catalyst composition may contain a noble metal, such as Pt, Pd, Ru, Rh, Os, Ir, Ag, or Au. In other embodiments, the catalyst composition may be substantially free of any noble metal.

[0071] Alternatively, the catalyst composition can be substantially free of precious metals other than palladium, platinum, and rhodium, substantially free of precious metals other than palladium and platinum, or substantially free of precious metals other than palladium.

[0072] The catalyst composition may be substantially free of any non-framework transition metals. Alternatively, the catalyst composition may be substantially free of non-framework transition metals other than copper and iron. In certain examples, the catalyst is substantially free of any non-framework transition metals other than copper.

[0073] In another aspect of the present invention, a catalyst article for treating exhaust gas is provided, the catalyst article comprising a FER zeolite as described herein. The catalyst article may comprise a FER zeolite as described herein disposed on and / or within a substrate. The substrate may be a metal plate or a honeycomb structure. The FER zeolite as described herein may be a carrier coating on a substrate (e.g., a honeycomb structure). The honeycomb structure may be an extruded catalyst, a wall flow filter, or a flow-through honeycomb structure.

[0074] In yet another aspect, a method for treating exhaust gas is provided, the method comprising contacting the exhaust gas with a catalyst article as described herein. The method for treating exhaust gas may also include contacting a catalyst article containing NO x and / or NH3 is contacted with the catalyst article described herein to convert NO x At least a portion of the N2O is selectively reduced to N2 and H2O and / or at least a portion of the oxidized NH3 is oxidized. Thus, in one embodiment, the catalyst article can be formulated to facilitate the reduction of nitrogen oxides with a reducing agent (i.e., an SCR catalyst). Examples of such reducing agents include hydrocarbons (e.g., C3-C6 hydrocarbons) and nitrogen-containing reducing agents such as ammonia and hydrazine ammonia or any suitable ammonia precursor such as urea ((NH2)2CO), ammonium carbonate, ammonium carbamate, ammonium bicarbonate, or ammonium formate. Preferably, the catalyst has a low N2O selectivity. The N2O selectivity is defined as the number of moles of N2O formed divided by the number of moles of NO converted. x The number of moles (NO x Defined as NO and NO2). Lower N2O selectivity is desirable because it is necessary to reduce N2O formation.

[0075] A method for treating exhaust gas may include reducing NO in the gas x A method for oxidizing NH3 in a compound or gas, the method comprising subjecting the gas to a catalytic reduction of NO as described herein x The catalyst article containing the FER zeolite is contacted with the compound for a period of time sufficient to reduce the NO in the gas. xCompounds and / or NH3 levels over time. In certain embodiments, a catalyst article (e.g., a catalyst article comprising an FER zeolite as described herein) having an ammonia slip catalyst disposed downstream of a selective catalytic reduction (SCR) catalyst is provided. In such embodiments, the ammonia slip catalyst oxidizes at least a portion of any nitrogen-containing reductant that is not consumed by the selective catalytic reduction process. For example, in certain embodiments, the ammonia slip catalyst is disposed on the outlet side of a wall-flow filter, and the SCR catalyst is disposed on the upstream side of the filter. In certain other embodiments, the ammonia slip catalyst is disposed at the downstream end of a flow-through substrate, and the SCR catalyst is disposed at the upstream end of a flow-through substrate. In other embodiments, the ammonia slip catalyst and the SCR catalyst are disposed on separate blocks within the exhaust system. These separate blocks may be adjacent and in contact with each other, or separated by a specific distance, provided that they are fluidly connected to each other and provided that the SCR catalyst block is disposed upstream of the ammonia slip catalyst block.

[0076] In certain embodiments, the SCR and / or AMOX process is carried out at a temperature of at least 150°C. In another embodiment, the process is carried out at a temperature of about 160°C to about 750°C. In a specific embodiment, the temperature range is from about 175°C to about 550°C. In another embodiment, the temperature range is from 175°C to 400°C. In another embodiment, the temperature range is from 450°C to 900°C, preferably from 500°C to 750°C, 500°C to 650°C, 450°C to 550°C, or 650°C to 850°C. Embodiments utilizing temperatures greater than 450°C are particularly useful for treating exhaust from heavy-duty and light-duty diesel engines equipped with exhaust systems including (optionally catalyzed) diesel particulate filters, which filters are actively regenerated, for example, by injecting hydrocarbons into the exhaust system located upstream of the filter, wherein the FER zeolite as described herein (or a catalyst article comprising the FER zeolite as described herein) is located downstream of the filter.

[0077] According to another aspect of the present invention, there is provided a method for reducing NO in gas. X A method for reducing NO in said gas by contacting the gas with a catalyst article as described herein comprising a FER zeolite. X The method of the present invention may include one or more of the following steps: (a) accumulating and / or burning soot in contact with the inlet of the catalytic filter; (b) introducing a nitrogen-containing reductant into the exhaust gas stream before contacting the catalytic filter, preferably without involving treatment of NO x and an intermediate catalytic step of a reducing agent; (c) by NO xAdsorbent catalyst or dilute NO x (d) contacting the exhaust gas stream with a DOC to oxidize a hydrocarbon-based soluble organic fraction (SOF) and / or carbon monoxide to CO2, and / or oxidize NO to NO2, which in turn can be used to oxidize particulates in a particulate filter; and / or reduce particulate matter (PM) in the exhaust gas; (e) contacting the exhaust gas with one or more flow-through SCR catalyst devices in the presence of a reductant to reduce NOx concentration in the exhaust gas; and (f) contacting the exhaust gas with an ammonia slip catalyst, preferably downstream of the SCR catalyst, to oxidize most, if not all, of the ammonia before the exhaust gas is discharged to the atmosphere, or passing the exhaust gas through a recirculation loop before the exhaust gas enters / re-enters the engine.

[0078] In another embodiment, all or at least a portion of the nitrogen-based reductant (specifically NH3) consumed in the SCR process can be provided by a NOx filter disposed upstream of the SCR catalyst (e.g., the SCR catalyst of the present invention disposed on a wall-flow filter). X Adsorbent Catalyst (NAC), Dilute NO X Trap (LNT) or NO X Storage / reduction catalyst (NSRC) is provided. The NAC components that can be used in the present invention include a catalyst combination of an alkaline material (such as an alkali metal, an alkaline earth metal or a rare earth metal, including an alkali metal oxide, an alkaline earth metal oxide and a combination thereof) and a noble metal (such as platinum), and an optional reduction catalyst component (such as rhodium). Specific types of alkaline materials that can be used in NAC include cesium oxide, potassium oxide, magnesium oxide, sodium oxide, calcium oxide, strontium oxide, barium oxide, and a combination thereof. The noble metal is preferably present at about 10 g / ft 3 About 200g / ft 3 , such as 20g / ft 3 Up to 60g / ft 3 Alternatively, the catalyst may be characterized by an average concentration of the noble metal of about 40 g / ft 3 About 100g / ft 3 .

[0079] Under certain conditions, during periodic enrichment regeneration events, NH3 can be present in NO x NO is generated on the adsorbent catalyst. x An SCR catalyst downstream of the adsorbent catalyst can improve overall system NO xReduction efficiency. In the combined system, the SCR catalyst is able to store NH3 released from the NAC catalyst during a rich regeneration event and utilize the stored NH3 to selectively reduce NO that slips through the NAC catalyst during normal lean operating conditions. x some or all of .

[0080] The method for treating exhaust gases as described herein can be performed on exhaust gases originating from combustion processes such as from internal combustion engines (whether mobile or stationary), gas turbines, and coal-fired or oil-fired power plants. The method can also be used to treat gases from industrial processes such as refining, from refinery heaters and boilers, heating furnaces, chemical processing industries, coke ovens, municipal waste treatment plants and incinerators, etc. In a specific embodiment, the method is used to treat exhaust gases from a vehicle lean-burn internal combustion engine (such as a diesel engine, a lean-burn gasoline engine, or an engine powered by liquid petroleum gas or natural gas).

[0081] In another aspect of the present invention, a system for treating exhaust gas containing NOx is provided, the system comprising the catalyst article described herein and a source of a reductant, wherein the source of the reductant is upstream of the catalyst article.

[0082] In certain aspects, the system is used to treat exhaust gas produced by a combustion process, such as from an internal combustion engine (whether mobile or stationary), a gas turbine, a coal-fired or oil-fired power plant, etc. Such a system includes a catalyst article comprising a FER zeolite as described herein and at least one additional component for treating the exhaust gas, wherein the catalyst article and the at least one additional component are designed to function as a coherent unit. In certain embodiments, the system includes a catalyst article comprising a FER zeolite as described herein, a conduit for directing the flowing exhaust gas, and a source of nitrogen-containing reductant disposed upstream of the catalyst article. The system may include a method for only determining that the zeolite catalyst is capable of catalyzing NO at an efficiency equal to or greater than a desired efficiency, such as at temperatures above 100°C, above 150°C, or above 175°C. x A controller that meters nitrogenous reductant into the flowing exhaust gas only when reducing. The metering of nitrogenous reductant can be arranged so that 60% to 200% of the theoretical ammonia is present in the exhaust gas entering the SCR catalyst, calculated at 1:1 NH3 / NO and 4:3 NH3 / NO2.

[0083] In another embodiment, the system includes an oxidation catalyst (e.g., a diesel oxidation catalyst (DOC)) for oxidizing nitrogen monoxide in the exhaust gas to nitrogen dioxide, which can be located upstream of the point where the nitrogen-containing reductant is metered into the exhaust gas. In one embodiment, the oxidation catalyst is suitable for producing a gas stream entering the SCR zeolite catalyst, the gas stream having a ratio of NO to NO2 of about 4:1 to about 1:3 by volume at an exhaust gas temperature of 250° C. to 450° C. at the oxidation catalyst inlet, for example. The oxidation catalyst may include at least one platinum group metal (or some combination of these), such as platinum, palladium, or rhodium, coated on a flow-through monolithic substrate. In one embodiment, the at least one platinum group metal is platinum, palladium, or a combination of both platinum and palladium. The platinum group metal may be supported on a high surface area carrier coating component such as alumina, a zeolite such as an aluminosilicate zeolite, silica, a non-zeolitic silica alumina, ceria, zirconia, titania, or a mixed or composite oxide comprising both ceria and zirconia.

[0084] In another embodiment, a suitable filter substrate is located between the oxidation catalyst and the SCR catalyst. The filter substrate may be selected from a wall-flow filter, a flow-through filter, a particle filter, a catalytic filter, preferably a wall-flow filter. In the case of a catalytic filter, for example with an oxidation catalyst, the point of metering the nitrogenous reductant is preferably located between the filter and the zeolite catalyst. Alternatively, if the filter is uncatalyzed, the means for metering the nitrogenous reductant may be located between the oxidation catalyst and the filter.

[0085] Example

[0086] Examples 1 to 8 and Comparative Examples 1 to 3

[0087] The synthesis gel was prepared by first dissolving an aluminum source such as sodium aluminate (52.75% Al2O3, 42.47% Na2O, 4.70% H2O) and / or aluminum hydroxide (55.80% Al2O3) in sodium hydroxide (50.0% aqueous solution) and deionized (DI) water. Potassium was added as raw materials using potassium hydroxide (45.0% aqueous solution) and / or potassium sulfate (99%) when necessary. Silica sol (40% SiO2) was then finally added to the sodium aluminate solution under vigorous stirring. The gel composition is listed in Table 1. For crystallization, the gel was heated at 180°C at 200 to 400 rpm for 1 to 6 days. After crystallization, the solid phase was filtered, washed thoroughly with DI water, and dried at 120°C. To obtain the H-type FER zeolite, the sample was ion exchanged at 100°C using a 5% ammonium sulfate solution and then activated at 550°C for two hours at a heating rate of 1°C / min.

[0088] Each product was analyzed by powder XRD and SEM. The powder XRD patterns of the H-type FER zeolites from Examples 2 and 7 and Comparative Examples CE2 and CE3 were Figure 1 The SEM image of the product from Example 2 is shown in Figure 2 The H-type FER zeolite from Example 2 27 Al solid-state MAS-NMR spectroscopy Figure 3 SAR determined by X-ray fluorescence spectroscopy (XRF) and BET, external surface area, micropore and mesopore volumes determined by Ar adsorption isotherms are listed in Table 1.

[0089]

[0090]

[0091] a All molar amounts are given as ratios to 1.0 Al2O3.

[0092] b Sodium aluminate was used instead of aluminum hydroxide as the aluminum source.

[0093] c All syntheses were carried out at 180 °C.

[0094] d Determined by XRF.

[0095] e The micropore volume and BET / surface area were determined by t-plot method and Rouquerol

[0096] Optimization method evaluation.

[0097] f Determined by integrating 27Al solid state MAS-NMR over the range 80 ppm to -30 ppm to cover all observed isotropic peaks and over the range 15 ppm to -30 ppm to cover only the 6-fold Al.

[0098] Table 1 - Summary of Examples 1-8 and Comparative Examples 1-3 .

[0099] Example 2: Selective Catalytic Reduction (SCR) Performance

[0100] The H-type FER zeolites from Examples 2 and 7 and Comparative Examples CE2 and CE3 were impregnated with the required amount of ammonium ferric oxalate dissolved in demineralized water. The Fe-impregnated zeolite was dried at 100°C overnight and then calcined in N2 and H2O at a temperature between 500°C and 700°C for 1 hour. In this case, iron was added to the zeolite to achieve a FER with 3.0 wt% iron based on the total weight of the zeolite.

[0101] A portion of each Fe FER zeolite sample was hydrothermally aged at 650° C. in air containing 10% by volume H 2 O for 50 hours.

[0102] Pelletized fresh and aged Fe-FER zeolite samples were placed in a test apparatus. To evaluate the SCR performance of the zeolite over a range of temperatures, the zeolite was subjected to a simulated diesel engine exhaust stream having the following properties: 525 ppm NH3, 500 ppm NO, 12% O2, 5% H2O, 200 ppm CO and 4.2% CO2, SV = 60 K h -1 The samples were exposed to the above gas mixture at 150°C, and the NOx conversion and N2O selectivity were measured at various steady-state temperatures ranging from 150°C to 450°C.

[0103] like Figure 4 and Figure 5 As shown in both examples, the fresh iron FER from Examples 2 and 7 achieve significantly higher NO in the temperature range between 250°C and 300°C compared to the two comparative examples 2 and 3 with similar SAR. x Conversion. Both FER samples from Examples 2 and 7 achieved higher NOx conversions in the temperature range between 250°C and 350°C after hydrothermal aging of the samples.

[0104] Example 3—Solid State NMR

[0105] The TopSpin 4.0 software was used on a Bruker Advance Neo console at 14.1T (ν0( 1 Solid-state NMR spectra were obtained at a static magnetic field strength of 100 MHz (H) = 600 MHz. The zeolite samples were stored overnight in a humid environment before measurement. The powdered samples were filled into a zirconia MAS rotor with a Kel-F cover. Compressed air purified at room temperature was used to rotate the rotor. The rotation frequency was 14 kHz and the cycle delay was 0.4 seconds. The spectrum was quantified by integrating in the range of 80 ppm to -30 ppm to cover all observed isotropic peaks and integrating in the range of 15 ppm to -30 ppm to cover only hexacoordinated AlO6.

Claims

1. A ferrierite (FER) zeolite, the FER zeolite having the following characteristics: a) SAR between 11 and 20; b) between 320m 2 / g and 380m 2 / g; and c) between 0.1cm 3 / g and 0.2cm 3 / g of micropore volume. 2 . The FER zeolite according to claim 1 , wherein the SAR is from 11 to 18, preferably from 12 to 17.

3. The FER zeolite according to claim 1 or claim 2, wherein the BET surface area is between 347 m 2 / g to 355m 2 / g, preferably 348m 2 / g to 352m 2 / g.

4. A FER zeolite according to any preceding claim, wherein the micropore volume is 0.12 cm 3 / g.

5. A FER zeolite according to any preceding claim, wherein the zeolite has a crystallinity greater than 95%.

6. A FER zeolite according to any preceding claim, wherein the zeolite has a crystal size of no greater than 1 micron, preferably no greater than 0.9 micron.

7. A FER zeolite according to any preceding claim, wherein the 6-twin Al is less than or equal to 15%.

8. A FER zeolite according to any preceding claim, wherein the external surface area is less than or equal to 20 m 2 / g.

9. An organotemplate-free process for making a ferrierite (FER) zeolite, the process comprising: (i) forming a reaction gel comprising an aluminum source, sodium hydroxide and / or potassium hydroxide and silica sol, (ii) heating the reaction gel to a temperature and for a time suitable for the growth of the FER zeolite, wherein the reaction gel does not contain seed crystals, and further wherein the reaction gel does not contain an organic structure directing agent (OSDA).

10. The method according to claim 9, wherein the temperature of step (ii) is 100 to 200°C, preferably 110 to 190°C.

11. The method according to claim 9 or claim 10, wherein the duration of step (ii) is at least 20 hours, preferably 1 day to 6 days.

12. The method according to any one of claims 9 to 11, wherein the reaction gel composition has a K2O / (K2O+Na2O) ratio of less than 0.

1.

13. A method according to any one of claims 9 to 12 for preparing a FER zeolite according to any one of claims 1 to 8.

14. A catalyst article for treating exhaust gases, the catalyst article comprising a FER zeolite according to any one of claims 1 to 8 or obtainable by a process according to any one of claims 9 to 12.

15. The catalyst article of claim 14, wherein the FER zeolite is disposed on and / or within a substrate.

16. A method for treating exhaust gas, the method comprising contacting the exhaust gas with a catalyst article according to claim 14 or claim 15.

17. The method for treating exhaust gas according to claim 16, wherein the method comprises subjecting a x and / or NH3 combustion exhaust gas is contacted with the catalyst product to convert the NO x At least a portion of the NH3 is selectively reduced to N2 and H2O and / or at least a portion of the NH3 is oxidized.

18. A system for treating exhaust gas containing NOx, the system comprising a catalyst article according to claim 14 or claim 15 and a source of reducing agent, wherein the source of reducing agent is upstream of the catalyst article.