Method for producing composite resistance material and resistance material obtained by the method
The method of bonding ceramic and ductile layers with a thermosetting polymer enhances the impact resistance and multi-hit absorption of composite materials, addressing the limitations of existing resistant materials by providing lightweight, high-strength protection suitable for ballistic armor.
Patent Information
- Application Number
- JP2024506757
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-08-04
- Filing Date
- 2022-07-27
- Publication Date
- 2024-09-18
AI Technical Summary
Existing resistant materials face limitations in withstanding concentrated impacts, high-speed object penetration, and are brittle, requiring careful handling, while also being heavy and costly to maintain.
A method for producing lightweight composite materials using ceramic and ductile layers bonded by a thermosetting polymer, enhancing impact resistance and multi-hit absorption with reduced weight and cost.
The composite materials provide high-strength protection with reduced weight, meeting Level 4 ballistic resistance standards and improving multi-hit absorption, suitable for ballistic armor with reduced delamination and weight compared to conventional solutions.
Smart Images

Figure 2024533971000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a composite resistant material intended to withstand mechanical loads, in particular concentrated impacts and explosions.
[0002] Products of this kind are, for example, reinforcing or cover plates, shatterproof panels and protective covers or bulletproof armour. [Background technology]
[0003] Currently, a wide variety of materials intended to withstand intensive mechanical loads in concrete applications are known and commercially available.
[0004] From US Pat. No. 5,399,533 a method is known to obtain a resistance plate comprising a ceramic layer obtained from sintered nanoparticles and joined by a thermal adhesive to a layer of ductile material, for example Kevlar®.
[0005] However, known types of resistance materials have significant limitations in their ability to withstand concentrated impacts, as well as their ability to withstand and penetrate the passage of objects at high speeds.
[0006] Furthermore, known types of materials based on resistant ceramic plates are fragile in use and are not suitable for use as bulletproof plates and must be handled with care.
[0007] Generally, it is desirable for this type of material not only to withstand stress, but also to be lightweight and compact, to be manufactured with readily available technology, and to last for long periods of time without requiring maintenance. There is therefore a felt need to be able to provide a method that allows the production of lightweight, highly protective composite resistant materials, even against violent impacts and high strength, for example the impact of penetrating projectiles. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] U.S. Patent No. 8,545,652 Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention aims to overcome the drawbacks of the already known solutions and to propose a method for producing high strength composite materials with limited weight per unit of coated surface. [Means for solving the problem]
[0010] These objects have been achieved by a productive method and material, for example a composite plate according to at least one of the appended claims.
[0011] The first advantage is that the treatment of the present invention makes it possible to significantly improve the impact resistance performance of the composite material, which has a high ability to counteract detachment delamination of the material's components, thus preserving its resistance characteristics against subsequent impacts.
[0012] A second advantage of the present invention is that it provides the same level of protection but weighs at least 10-35% less than currently used solutions and has a significant improvement in terms of multi-hit absorption capacity compared to currently used solutions.
[0013] A further advantage of the present invention is that a high performance, lightweight composite plate, particularly suitable for use as turret and ballistic protection for armored vehicles or aircraft, is available at limited cost and with industrial processes, reducing the use of aluminum or steel in armored vehicle armor.
[0014] A further advantage of the present invention is that the resulting plates exhibit superior results in terms of strength / resilience against extreme marine and atmospheric conditions.
[0015] A further advantage of the present invention is that the resulting plates meet the requirements of Level 4 (AP-API projectile resistance) of the Ballistic Resistance of Body Armor NIJ Standard-0101.06 published by the United States Department of Justice. [Brief description of the drawings]
[0016] These and other advantages will be better understood by those skilled in the art from the following description and the accompanying drawings, given by way of non-limiting example. [Figure 1a] An exploded view is shown. [Figure 1b] 1 shows the plate inserted into the mould during manufacture. [Figure 1c] A cross-sectional view of the resulting composite plate is shown. [Figure 1d] 4 shows a further embodiment of a plate according to the invention. [Figure 1e] 13 shows a further embodiment of a plate inserted into a mould during production. [Figure 1f] 13 shows a further embodiment of a plate inserted into a mould during production. [Diagram 2] 2 shows a second embodiment of a plate according to the invention in a cross-sectional view. [Diagram 3] 3 shows a third embodiment of a plate according to the invention in a cross-sectional view. [Figure 4] 1 shows a composite plate according to the invention constructed from hexagonal prismatic sectors in a top view. [Diagram 5] 1 illustrates a schematic representation of a method according to the invention; [Figure 6a] 1 shows an image of an inlet hole in a conventional aluminum plate for bulletproof armor. [Figure 6b] 1 shows an image of an exit hole in a conventional aluminum plate for bulletproof armor. [Figure 7a] 1 shows an image of an inlet hole of a composite plate according to the present invention. [Figure 7b] 1 shows an image of the exit holes of a composite plate according to the present invention. [Figure 8a]13 shows an image of inlet and outlet holes of a second composite plate according to the invention that has been hit by multiple hits. [Figure 8b] 13 shows an image of inlet and outlet holes of a second composite plate according to the invention that has been hit by multiple hits. [Figure 9a] FIG. 1 shows stress-strain diagrams for two different sets of samples produced by the method of the present invention. [Figure 9b] FIG. 1 shows stress-strain diagrams for two different sets of samples produced by the method of the present invention. [Figure 10a] FIG. 9 shows the results of mechanical characterization measurements of the sample shown in the diagram of FIG. 9a. [Figure 10b] FIG. 9 shows the results of mechanical characterization measurements of the sample shown in the diagram of FIG. 9a. [Figure 11a] 1 shows the arrival side of a prior art resistance plate where a penetration hit has arrived. [Figure 11b] 1 shows the exit side of a prior art resistance plate where a penetration hit has been received. [Figure 12] 1 shows an incendiary penetrator projectile. [Figure 13] 1 shows an example of a helmet manufactured using the resistive material according to the present invention.
[0017] With reference to the attached drawings, a preferred embodiment of the method according to the invention for manufacturing a composite material, for example a composite plate 5 starting from at least two spaced apart component bodies in a gap 11 (FIGS. 1 to 3), of the example illustrated starting plates 13, 14, each made of a metallic material, for example steel, aluminium, brass, lead, titanium, or a ceramic material, for example alumina, boron or silicon oxide, or a fibre material, for example carbon fibre plates, aramid fibres or Kevlar fibres, metallic fibres and / or non-metallic inorganic fibres, non-woven or woven fabrics, or even a plastic material, for example polyamide.
[0018] FIG. 4 shows a further embodiment of a resistor plate 5′ obtained using the material according to the invention, in which the component body consists of hexagonal prisms 20, 21 of ceramic material, joined together with a gap 11 and possibly housed by a frame 22.
[0019] By way of example, ceramic materials suitable for use are those having a Vickers hardness greater than 1500, and in the case of boron carbide up to about 2500 Vickers, i.e. materials having a hardness much greater than the material from which the projectile is made, for example.
[0020] By way of example, suitable ceramic materials are boron carbide, which has a specific weight of about 2.6 g / cm3 and a Vickers hardness of 2500 / 2600, silicon carbide, which has a specific weight of about 3.2 g / cm3 and a Vickers hardness of 2200 / 2300, or alumina or aluminum oxide, which has a specific weight of about 3.9 g / cm3 and a Vickers hardness of 1800 / 2000.
[0021] According to the method of the invention, which is shown diagrammatically in FIG. 5, adjacent outer surfaces 23, 24 of the component body are subjected to a cleaning step F1, preferably a mechanical cleaning step, for example by shot peening or sandblasting or tumbling, until complete removal of residues from the surfaces, in particular oxidation traces in the case of plates in oxidized material, and the production of an improved pretreated surface for adhesion of the adhesive. The cleaning step may include removing dust generated, for example, by surface shot peening.
[0022] As a preferred example, surface cleaning of the plates is carried out with Almen shot peening at 16 degrees, for example by using four 5 kW centrifugal impellers, which has proven to be particularly effective.
[0023] A coating formed by an adhesive, also called primer or glue, is then applied to the cleaned and pretreated surface of the plate (step F2), for example by pouring, coating, casting, dipping or spraying.
[0024] Once coating is complete, the component body is dried (step F3) in a moisture-free environment, preferably at a temperature between 15° C. and 25° C. The drying step is continued by pre-heating the plate (step F4), which is extended until the surface viscosity of the adhesive is reduced, for example by heating at a temperature between 50° C. and 200° C., to facilitate the subsequent bonding of a compatible thermosetting polymer adapted to bond to the adhesive, which at this step is sticky to the touch.
[0025] The above treatments can be applied separately to each component body or to component bodies assembled by spacer distribution.
[0026] In the case of the plates shown in Figures 1 to 3, the spacer is formed by a block 12 interposed between the joined starting plates, arranged to provide a gap 11 between them, while in the example of Figure 4 the prisms 20, 21 may be spaced apart by a frame 22 or may be arranged in suitably spaced sheets.
[0027] At the end of the preheating step, the component bodies, i.e. in the described case the starting plates 13, 14 assembled with the spacers 12, or the spaced apart prisms 20, 21, are then subjected to a joining step (step F5) of the material already coated with adhesive in a viscous state, using a thermosetting polymer composed of two or more components, at least one of which is compatible with the adhesive.
[0028] Within the scope of this disclosure, an adhesive-compatible polymer component is to be understood as a component that can be combined with an adhesive to establish an adhesive bond between the polymer and the adhesive-coated surface.
[0029] The joining step can be performed by injection, casting, coating, dipping, lining, spraying, or other techniques adapted to apply the polymer, depending on the shape and composition of the material.
[0030] Preferably, the polymer is a two-component polyurethane, such as that commercially available under the trademark adiprene®, although different types of polymers, such as silicone polymers, and polymers having different numbers of components can be used, as long as at least one of them is compatible with the adhesive used and capable of forming an adhesive bond.
[0031] Preferably, the step of linking with the polymer can be carried out by casting the polymer into a form 10 for containing the plates until it fills the gap 11 between the starting plates 13, 14 so as to constitute an intermediate bonding layer P.
[0032] Advantageously, it has been found that the diffusion of the polymer in the gap 11 is facilitated by pre-heating the component body of material, thus making it possible to form an intermediate polymer bonding layer P even with a very small thickness, on the order of millimeters.
[0033] Preferably, the gap is obtained by blocking a spacer 12 between the plates 13, 14, which has a thickness predetermined based on the desired strength characteristics of the final plate 5 and which may be made of the same polymer material as used for the joining step and which may optionally be subjected to the same treatments as are performed on the starting plates.
[0034] The plate 5 assembled with the starting plate linked to the polymer is then treated (step F6) to obtain full curing and full activation of the bond between the polymer and the adhesive.
[0035] Preferably, the step of curing and activating the bond is carried out by heating, e.g. in an oven, preferably for 10 minutes to several hours, e.g. 3-5 hours, at a temperature of e.g. 50°C to 200°C, depending on the heat resistance of the material of the starting plate, until the polymer cures and the bond between said adhesive and polymer is fully activated.
[0036] However, this step may be carried out at room temperature depending on the polymer used.
[0037] The plate 5 obtained using the material of the invention has been found to be particularly effective as ballistic armor when the first plate 13, placed on the impact side of a projectile, for example an API incendiary penetrator projectile of the type shown in FIG. 13, consisting of a casing I housing a penetrating core NP and an incendiary bullet C, is an aluminum plate and the second plate 14 is a plate of ceramic material, for example boron, silicon or alumina carbide (FIGS. 1, 1c).
[0038] Preferably, the structure of FIG. 1c can be associated with a further steel layer 16 applied to the exit side of the projectile in the manner of the present invention, in which case the resulting structure is as shown diagrammatically in FIG. 1d.
[0039] Advantageously, the material of the invention can furthermore be provided with an outer layer of polymer P on one or more of the outer faces of the composite plate obtained by this method.
[0040] In Figures 1e and 1f, respectively, a plate of the type of Figure 1d including a complete shell with polymer P obtained by providing spacers 12 arranged on both the surface and the sides, and a formwork 10 suitable for this purpose are shown diagrammatically by way of example.
[0041] It was found that in this configuration, the ceramic material reached by the projectile, although it can be crossed, is not dispersed by its intimate bonding with the polymer layer, counteracting the delamination of the composite material and thus preventing the ceramic from breaking free, making it possible to withstand multiple hits, unlike known arms based on ceramic plates, which tend to break after the first hit and therefore become useless.
[0042] To that effect, the ceramic actually consumes the material of the projectile passing through it, which has a much lower hardness, reducing its residual energy at the exit side, where it can advantageously provide a further absorbing plate of the residual impact, which is due, for example, to the kinetic energy of the remaining core of the projectile, preferably made of a plastic material, for example polyamide, or a fiber or steel material, which, due to its resistance and ductility, is able to deform and accommodate the residual mass of the projectile, avoiding or reducing trauma to the wearer of the armour.
[0043] In general, it has been found that the plate of the invention makes it possible to absorb the kinetic energy caused by the impact with a projectile so as to avoid significant changes in the structure.
[0044] In particular, it has been found that the combination of the presence of an aluminum first plate (or other ductile material) on the arrival side of the projectile, together with the presence of a polymeric bonding layer that strongly adheres to the adjacent plate, has the effect of suppressing the tendency to delaminate, as described above, thus minimizing the size of the entrance hole and preventing the typical "artichoke" outwardly bent opening (Figures 6a, 6b) that conventional armor (in the example shown, a 25 mm aluminum plate) experiences on the entrance side of the projectile due to the high energy released by the projectile, while the composite plate of the invention makes it possible to reduce both the damage of the first plate (Figures 7a, 8a) and the same exit of the projectile (Figures 7b, 8b).
[0045] In this regard, Figures 11a-11b show the entry and exit side holes F of a penetrating shot received by a traditional ballistic plate composed of a ceramic body CC coupled to a fibrous layer, e.g. Dyneema®.
[0046] Figures 8a, 8b show an example of a plate according to the invention that received 18 multiple hits of two penetrations type 30-06 API and type SS 109 NATO-NATO, in Figure 8a it is possible to see the presence of various inlet holes, and in Figure 8b the absence of outlet holes.
[0047] To clarify the distance between hits received, the dimensions of the plate shown in Figures 8a and 8b are defined as 115mm x 115mm and 25mm thick.
[0048] FIG. 2 shows a preferred embodiment of a plate for use as bulletproof armor, said plate comprising: a first aluminum starting plate 13, preferably having a thickness of 1 to 4 mm, preferably 3 mm; a second ceramic plate 14, for example alumina, or boron or silicon oxide, preferably having a thickness of 4 to 6 mm, preferably 5 mm, possibly formed of a plurality of plates 14, 14' arranged side by side; a third starting plate 15 having a thickness of preferably 4 mm to 6 mm, preferably 5 mm; Preferably, the plate 15 comprises carbon or Kevlar fibers, aramid fibers, or high melting and non-combustible metallic and / or non-metallic inorganic fibers, such as those sold under the name "nextel" by the company 3M®, capable of further reducing the temperature caused by projectiles or hollow-point darts and useful for example for stopping anti-tank missiles according to the specifications Stag 4569 for darts and Stag 2920 AEP 55 for projectiles, and a fourth starting plate 16, preferably made of steel, having a thickness of 2 to 4 millimeters, preferably 2 mm; an intermediate layer P of binder polymer between the plates 13, 14, 15, 16, preferably 3 mm thick; It consists of:
[0049] FIG. 3 shows a curved configuration of the plate of FIG. 2, having a convex curvature towards the expected direction of impact arrival (d) according to the orientation shown diagrammatically in FIG. 3, which is particularly useful as a bulletproof armor for protecting against accidental impacts against the first plate 13.
[0050] Advantageously, the plates of Figures 2 and 3 have an overall thickness of about 25 mm and make it possible to obtain high ballistic protection whilst significantly reducing the weight with respect to conventional armour having the same performance, and are therefore suitable for use as ballistic armour.
[0051] In a preferred embodiment, the plate of the invention has a thickness of 1 mm to 1.5 mm, preferably 1.2 mm, and consists of a steel layer coupled with an aluminum layer of 1 mm and a polymer interlayer of about 1 mm; Figures 9 and 10 show, respectively, the stress / strain diagrams and mechanical characterization tables of two different series of three samples (Figures 9a, 10a) and three strips (Figures 9b, 10b) thus produced. Advantageously, in this configuration, the plate, with a thickness of about 3 mm, shows a tensile strength of just under 1800 MPa, while at the same time proving capable of significant elongation and therefore suitable for machining and forming.
[0052] By way of example, the plate of the present invention may be Civilian locations and vehicles such as embassies, consulates, pipelines / oil pipelines, nuclear power plants, railway stations, airports, cars, trucks, ships, ambulances, hospitals (also for simultaneous protection from X-rays using lead plates), containers of dangerous goods, anti-riot vehicles, bank security vaults, etc. Armored storehouses, ammunition depots, military ambulances, military field hospitals, security barriers (gates, checkpoints, observation posts), helicopters and aircraft (seats and floors), command rooms, operating theatres, nuclear bunkers, ships and submarines, protective clothing, e.g. vests and helmets, military locations and vehicles (Figure 13) It can be used for.
[0053] Although the present invention has been described with reference to preferred embodiments, it is contemplated that equivalent modifications may be made without departing from the scope of the present invention.
Claims
1. A method for producing a composite resistance material (5, 5'), comprising the steps of: Providing at least two component bodies (13, 14, 15, 16, 20, 21) each made of a material selected from a fibrous material, such as carbon fibres, aramid fibres, metallic or non-metallic inorganic fibres, or a ceramic material, such as alumina, boron or silicon carbide, or a metallic material, such as aluminium, brass, lead, steel, or a plastic material, such as polyamide; cleaning at least one external coupling surface (23, 24) of each of said bodies (13, 14, 15, 16), preferably by mechanical cleaning by shot peening or sand blasting or tumbling until any surface impurities are removed, followed by optional dusting; Providing at least two adjacent component bodies having a free intermediate gap (11) between their respective coupling surfaces; coating the clean coupling surfaces of said bodies (13, 14, 15, 16) with an adhesive; drying said coated body (13, 14, 15, 16) in the absence of moisture, preferably at a temperature between 15°C and 25°C; pre-heating said body (13, 14, 15, 16) preferably at a temperature between 50°C and 200°C until the surface viscosity of said adhesive is reduced; coupling the coupling surfaces of the bodies (13, 14, 15, 16) coated with the adhesive in a viscous state with a quantity of a thermosetting polymer consisting of two or more components, at least one of which is compatible with the adhesive, arranged to fill the gaps (11) to form an intermediate layer of polymer (P) between the bodies (13, 14, 15, 16); curing the polymer to fully activate the bond between the adhesive and the polymer; A method comprising:
2. The method according to claim 1, wherein said curing occurs by heating said bodies (13, 14, 15, 16) coupled to said polymer, preferably at a temperature between 50°C and 200°C.
3. 3. The method according to claim 1 or 2, wherein the at least two bodies are in the form of a monolithic plate or are composed of several parts.
4. 3. The method according to claim 1 or 2, wherein the at least two bodies are in the form of hexagonal prisms (20, 21) of ceramic material, joined to each other via a gap (11) and possibly housed by a frame (22).
5. 5. The method according to any one of claims 1 to 4, wherein the coupling is carried out by injection, spreading, casting, dipping or spraying.
6. 6. The method according to any one of claims 1 to 5, wherein the coupling step is performed by injecting or casting the polymer into a form (10) containing the bodies (13, 14, 15, 16) until it fills the gaps (11) and forms an intermediate binder layer (P) between adjacent bodies.
7. 7. The method according to claim 1, wherein the polymer is selected from polyurethanes or silicones having two or more components.
8. The method according to any one of the preceding claims, wherein the gap is formed by a spacer (12), preferably of the same material as the coupling polymer.
9. A composite resistance plate obtainable by the method according to any one of claims 1 to 8, At least two component bodies (13, 14, 15, 16, 20, 21) each made of a material selected from a fibrous material, such as carbon fibers, aramid fibers, metallic or non-metallic inorganic fibers, or a ceramic material, such as alumina, boron or silicon carbide, or a metallic material, such as aluminum, brass, lead, steel, or a plastic material, such as polyamide; each of said bodies (13, 14, 15, 16) having at least one outer coupling surface (23, 24) cleaned, preferably by mechanical cleaning by shot peening or sand blasting or tumbling, until any surface impurities are removed, and optionally dusted, said cleaned coupling surface of said bodies (13, 14, 15, 16) being coated with an adhesive; an intermediate gap (11) between the respective coupling surfaces of at least two adjacent component bodies (13, 14, 15, 16) filled with a quantity of a thermosetting polymer consisting of two or more components, at least one of which is compatible with the adhesive, to form an intermediate layer of polymer (P) between the at least two adjacent component bodies (13, 14, 15, 16); A composite resistance plate comprising:
10. 10. The composite plate according to claim 9, wherein the at least two component bodies (13, 14, 15, 16) comprise a first starting plate (13) of a metallic material, preferably aluminum, arranged on an impact arrival side, and a second plate (14) of a ceramic material.
11. 11. Plate according to claim 10, wherein said at least two component bodies (13, 14, 15, 16) further comprise at least a third plate of shock absorbing material, preferably made of plastic material or fibre or steel.
12. The third at least two component bodies (13, 14, 15, 16) A first aluminum starting plate (13) preferably having a thickness of 2-4 mm, preferably 3 mm; a second ceramic starting plate (14), for example alumina, or boron or silicon oxide, preferably with a thickness of 4 to 6 mm, preferably 5 mm; a third starting plate (15) of fibrous material selected from carbon or Kevlar fibers, or inorganic, metallic and / or non-metallic fibers; a fourth starting plate (16) preferably made of steel with a thickness of 2-4 mm, preferably 2 mm; Including, A plate according to claim 11, further comprising an intermediate binder layer (P) of polymer, preferably 2 to 4 mm thick, preferably 3 mm thick.
13. 13. Plate according to any one of claims 9 to 12, wherein the second ceramic plate is formed by arranging several ceramic plates (14, 14') side by side.
14. 14. A plate according to any one of claims 10 to 13, shaped to have a convex curvature towards the expected direction of impact arrival (d).
15. Use of a plate according to any one of claims 9 to 14 as bulletproof armour, preferably as a vehicle or aircraft or protective clothing.
Citation Information
Patent Citations
Burster block of composite structure and manufacturing method of burster block
CN105444622A
Sandwich board for improved structure
JP2007512977A
Protective member and protective device using the same
JP2008275208A
Composite bulletproof plate
JP2009264692A
Helmets comprising ceramic for protection against high energy fragments and rifle bullets
JP2018025388A