Method for preparing a laminated article comprising a silicone pressure sensitive adhesive bonded to a silicone rubber

JP2024535742AActive Publication Date: 2024-10-02DOW SILICONES CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024513962
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2022-07-21
Publication Date
2024-10-02
Estimated Expiration
2042-07-21

Smart Images

  • Figure 2024535742000020
    Figure 2024535742000020
  • Figure 2024535742000021
    Figure 2024535742000021
  • Figure 2024535742000001
    Figure 2024535742000001
Patent Text Reader

Abstract

The laminate article comprises a silicone pressure sensitive adhesive adhered to an article comprising a silicone rubber.A method for making a laminate article is provided.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims the benefit under 35 U.S.C. §119(e) of U.S. Provisional Patent Applications Nos. 63 / 241,550 and 63 / 335,733, filed September 8, 2021 and April 28, 2022, respectively. U.S. Provisional Patent Applications Nos. 63 / 241,550 and 63 / 335,733 are incorporated herein by reference.

[0002] FIELD OF THEINVENTION The present invention relates to a method for preparing a silicone pressure sensitive adhesive composition that can be cured to form a silicone pressure sensitive adhesive having good adhesion to silicone rubber. More particularly, the present invention relates to a method for preparing a peroxide curable silicone pressure sensitive adhesive composition that cures to form a silicone pressure sensitive adhesive. A laminate article comprises a silicone pressure sensitive adhesive adhered to an article comprising silicone rubber. [Background technology]

[0003] Introduction U.S. Patent No. 8,247,502 discloses an addition reaction curable silicone pressure sensitive adhesive composition. However, the addition reaction curable silicone pressure sensitive adhesive composition may suffer from the drawback of poor adhesion to silicone rubber (e.g., typically ≦1,000 gf / inch).

[0004] Currently commercially available silicone pressure sensitive adhesives can suffer from the drawback of providing relatively poor adhesive strength to silicone rubber substrates, which often fails to meet the needs of applications in which they are used to bond to silicone rubber, such as in electronics, automotive, and masking tape applications. Summary of the Invention

[0005] A method for making a laminate article is provided, the method comprising: (a) combining starting materials under conditions which effect a condensation reaction, the starting materials being: (P) a bis-hydroxyl terminated polydiorganosiloxane having a weight average molecular weight of 10,000 g / mol to <200,000 g / mol as measured by GPC; (R) a hydroxyl-functional polyorganosilicate resin having a weight average molecular weight of 15,000 g / mol to 30,000 g / mol as measured by GPC, a hydroxyl-functional polyorganosilicate resin, wherein the starting materials (R) and (P) are present in a weight ratio (R) / (P) of 2.27 / 1 to <3.88 / 1; (S) a solvent, thereby forming a reaction mixture; (b) adding to the reaction mixture (C) a condensation reaction catalyst, thereby forming a catalyzed reaction mixture; (c) heating the catalyzed reaction mixture at a temperature >RT to 145°C to remove water, thereby forming a silicone pressure sensitive adhesive composition; (d) coating a surface of a backing substrate with a silicone pressure sensitive adhesive composition; (e) drying the silicone pressure sensitive adhesive composition; and (f) curing the silicone pressure sensitive adhesive composition to form a silicone pressure sensitive adhesive layer having a surface adhered to a surface of a backing substrate, the silicone pressure sensitive adhesive layer further including an opposing surface opposite the surface of the backing substrate; (g) adhering an opposing surface of the silicone pressure sensitive adhesive to a surface of a silicone rubber article. A laminate article comprising a silicone pressure sensitive adhesive adhering to a silicone rubber article can be prepared by this method. [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is a partial cross-sectional view of laminate article 100. [Diagram 2] FIG. 2 is a partial cross-sectional view of laminate article 200.

[0007] Reference number 100 Partial cross section of laminated article 101 Backing material 101b Surface of backing substrate 101 102 Silicone pressure sensitive adhesive 102a Surface of silicone pressure sensitive adhesive 102 102b: opposite surface of silicone pressure sensitive adhesive 102 103 Silicone rubber articles 103a Surface of silicone rubber article 103 200 Partial cross section of laminated article 201 Backing material containing silicone rubber 201b Surface of the backing substrate 201 202 Silicone pressure sensitive adhesives 202a Surface of silicone pressure sensitive adhesive 202 202b: opposite surface of silicone pressure sensitive adhesive 202 DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The method for making a laminate article comprises: (1) combining starting materials under conditions which effect a condensation reaction, the starting materials being: (P) a bis-hydroxyl terminated polydiorganosiloxane having a weight average molecular weight of 10,000 g / mol to <200,000 g / mol as measured by GPC, wherein starting material (P) is present in an amount of >20.5 weight percent based on the combined weight of starting materials (P) and (R); (R) a hydroxyl-functional polyorganosilicate resin having a weight average molecular weight of 15,000 g / mol to 30,000 g / mol as measured by GPC, wherein the starting material (R) is present in an amount of <79.5 wt.%, based on the combined weight of the starting materials (P) and (R); (S) a solvent; and optionally, (N) a neutralizing agent; starting materials (R) and (P) are present in a weight ratio (R) / (P) of 2.27 / 1 to <3.88 / 1, thereby forming a reaction mixture; (2) adding (C) a condensation reaction catalyst to the reaction mixture, thereby forming a catalyzed reaction mixture; (3) heating the catalyst reaction mixture at a temperature >RT to 145°C to remove water; Optionally, (4) recovering the condensation reaction product of (P) and (R); and optionally, (5) adding up to 4 weight percent, based on the combined weight of (R) and (P), of an (X) peroxide crosslinking agent, thereby forming a silicone pressure sensitive adhesive composition; Optionally, (6) treating the surface of the backing substrate; and (7) coating a surface of a backing substrate with a silicone pressure sensitive adhesive composition; (8) drying the silicone pressure sensitive adhesive composition; and (9) curing the silicone pressure sensitive adhesive composition to form a silicone pressure sensitive adhesive layer having a surface adhered to a surface of a backing substrate, the silicone pressure sensitive adhesive layer further including an opposing surface opposite the surface of the backing substrate; Optionally, (10) treating a surface of the silicone rubber article; and (11) adhering an opposing surface of the silicone pressure sensitive adhesive to a surface of the silicone rubber article.

[0009] Step (1) of the above process can be carried out by any convenient means, for example, by mixing the starting materials including (P), (R), (S), and optionally (N) as introduced above and described in detail below, in a batch reactor, optionally equipped with stirring and jacketing. The condensation reaction can be carried out at a temperature between 20° C. and 150° C., or from RT to the reflux temperature of the starting materials (S), solvent. The reaction time depends on various factors including the selection of starting materials and temperature, but the condensation reaction in step (1) can be carried out for, for example, 0.5 hours to 20 hours, or 1 hour to 10 hours. The condensation reaction can be carried out, for example, as described in U.S. Patent No. 5,916,981 to Cifuentes et al., by changing the appropriate starting materials to those described below.

[0010] (P) Bis-hydroxyl terminated polydiorganosiloxane The starting material (P) is the bis-hydroxyl terminated polydiorganosiloxane (polymer) used in step (1). This polymer has the formula

[0011] [ka] wherein each R 1 are independently selected alkyl groups of 1 to 6 carbon atoms, and the subscript a represents the average number of difunctional siloxane units per molecule, where 250≦a≦3,000, alternatively 270≦a≦2,000. Alternatively, the subscript a can be at least 250, alternatively at least 270, alternatively at least 300, alternatively at least 350, alternatively at least 400, alternatively at least 450, alternatively at least 500, while the subscript a can be up to 3,000, alternatively up to 2,500, alternatively up to 2,100, alternatively up to 2,000, alternatively up to 1,900, alternatively up to 1,800. 1Examples of alkyl groups include methyl, ethyl, propyl (including n-propyl and isopropyl), butyl (including n-butyl, tert-butyl, sec-butyl, and isobutyl), pentyl (including n-pentyl, cyclopentyl, and branched isomers having 5 carbon atoms), and hexyl (including n-hexyl, cyclohexyl, and branched isomers having 6 carbon atoms). 1 may be methyl or ethyl, alternatively methyl.

[0012] Suitable polymers for starting material (A) are known in the art and commercially available from a variety of sources, such as Gelest Inc. (Morrisville, Pennsylvania, USA) and DSC. Examples of suitable polymers include bis-hydroxyl terminated polydimethylsiloxanes having a Mw of 20,000 g / mol to 150,000 g / mol, alternatively 40,000 g / mol to 135,000 g / mol, where Mw can be measured by GPC.

[0013] (R) Polyorganosilicate resin The starting material (R) is the hydroxyl-functional polyorganosilicate resin (resin) used in step (1). The resin has the formula R 1 3SiO 1 / 2 and a monofunctional unit of formula SiO 4 / 2 wherein R 1 is as above. Alternatively, the monofunctional unit may be of the formula (MeSiO 1 / 2 The polyorganosilicate resin is soluble in solvents such as those described below as starting material (S), exemplified by aliphatic and / or aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, heptane, and combinations thereof.

[0014] As prepared, the resin contains the monofunctional and tetrafunctional units described above, the resin further contains units having silicon-bonded hydroxyl groups, and has the formula Si(OSiR 13) may contain a neopentamer of 4, where R 1 is as above), for example, the neopentamer can be tetrakis(trimethylsiloxy)silane. The concentration of silanol groups present in the resin can be measured using FTIR spectroscopy according to ASTM standard E-168-16. The molar ratio of mono- to tetrafunctional units is expressed as {M(resin)} / {Q(resin)}, or M:Q, excluding mono- and tetrafunctional units from the neopentamer. The M:Q ratio represents the molar ratio of the total number of triorganosiloxy groups (monofunctional units) in the resinous portion of the polyorganosilicate resin to the total number of silicate groups (Q units) in the resinous portion. The M:Q ratio can be from 0.5:1 to 1.5:1.

[0015] The Mn of the polyorganosilicate resin is determined by the R 1 The Mn of the polyorganosilicate resins depends on various factors including the type of alkyl group represented by Mn=Mw / Mw. The Mn of the polyorganosilicate resins refers to the number average molecular weight measured using GPC when the peak representing the neopentamer is excluded from the measurement. The Mn of the polyorganosilicate resins may be greater than 3,000 Da, alternatively >3,000-8,000 Da. Alternatively, the Mn of the polyorganosilicate resins may be 3,500-8,000 Da. The Mw of the polyorganosilicate resins refers to the weight average molecular weight measured using GPC. The Mw of the polyorganosilicate resins may be 15,000 Da-30,000 Da, alternatively 20,000 Da-30,000 Da, alternatively 21,000 g / mol-29,500 g / mol.

[0016] The polyorganosilicate resins can be prepared by any suitable method, such as cohydrolysis of the corresponding silanes or by silica hydrosol capping methods. The polyorganosilicate resins can be prepared by silica hydrosol capping methods, such as those disclosed in U.S. Pat. No. 2,676,182 to Daudt et al., U.S. Pat. No. 4,611,042 to Rivers-Farrell et al., and U.S. Pat. No. 4,774,310 to Butler et al. The above-mentioned Daudt et al. method involves reacting a silica hydrosol under acidic conditions with a hydrolyzable triorganosilane, such as trimethylchlorosilane, a siloxane, such as hexamethyldisiloxane, or a mixture thereof, and recovering a copolymer having monofunctional units and Q units. The resulting copolymer generally contains 2 to 5 weight percent hydroxyl groups.

[0017] The intermediates used to prepare the polyorganosilicate resins can be triorganosilanes and silanes or alkali metal silicates containing four hydrolyzable substituents. The triorganosilanes are represented by the formula R 1 3SiX 1 wherein R 1 is as above, and X 1 represents a hydrolyzable substituent such as hydroxyl. Silanes with four hydrolyzable substituents have the formula SiX 2 4, wherein each X 2 is halogen, alkoxy, or hydroxyl. Suitable alkali metal silicates include sodium silicate.

[0018] The resin selected for the starting material (R) has the unit formula (R 1 3SiO 1 / 2 ) b (SiO 4 / 2 ) c (HO 1 / 2 ) d wherein each R 1are independently selected alkyl groups of 1 to 6 carbon atoms, as above, subscripts b and c represent the mole fractions of monofunctional and tetrafunctional units, respectively, subscripts b and c have values ​​such that 0.4≦b≦0.5, 0.5≦c≦0.6, and the amount (b+c)=1, and subscript d represents the amount of hydroxyl groups in the resin, subscript d having a value sufficient to provide the resin with a hydroxyl content of 2% to 5% by weight. The resin may have a Mw of 15,000 g / mol to 30,000 g / mol as measured by GPC. Alternatively, the resin may have a Mw of from 20,000 g / mol to 30,000 g / mol, alternatively from 21,000 g / mol to 30,000 g / mol, alternatively from 21,000 g / mol to 29,500 g / mol, alternatively from 21,000 g / mol to 29,100 g / mol. Suitable resins are known in the art and commercially available, for example, from DSC.

[0019] The resin (R) and polymer (P) are present in a weight ratio (R) / (P) of >2.27 / 1 to <3.88 / 1. Alternatively, (R) / (P) can be from 2.9 / 1 to <3.88 / 1, or (R) / (P) can be from 2.9 / 1 to 3 / 1. Without wishing to be bound by theory, it is believed that an (R) / (P) of ≦2.27 / 1 can result in a silicone pressure sensitive adhesive having poor adhesion to silicone rubber, while an (R) / (P) of >3.88 / 1 can result in a silicone pressure sensitive adhesive that is glassy while at the same time lacking sufficient adhesion to silicone rubber.

[0020] (S) Solvent The starting material (S) is a solvent. Solvents may be added during step (1) and optionally later steps, such as step (2), to facilitate the introduction of certain starting materials, such as (R) resin. Solvents that may be used herein are those that aid in fluidizing the starting materials but do not essentially react with the starting materials. The solvent may be selected based on the solubility of the starting materials and the volatility of the solvent. "Solubility" refers to the solvent being sufficient to dissolve and / or disperse the starting materials. "Volatility" refers to the vapor pressure of the solvent. Without wishing to be bound by theory, it is believed that if the solvent is too volatile (has too high a vapor pressure), the solvent may evaporate too quickly from the reaction mixture during step (3). However, if the solvent is not volatile enough (has too low a vapor pressure), too much solvent may remain in the condensation reaction product prepared in step (3) and / or water produced as a by-product of the condensation reaction may not be sufficiently removed during step (3) and, if present, step (4).

[0021] Suitable solvents include polyorganosiloxanes having suitable vapor pressures, such as hexamethyldisiloxane, octamethyltrisiloxane, hexamethylcyclotrisiloxane and other low molecular weight polyorganosiloxanes, such as DOWSIL™ 200 fluids and DOWSIL™ OS fluids, 0.5-1.5 cSt, which are commercially available from DSC.

[0022] Alternatively, the solvent may comprise an organic solvent. The organic solvent may be a ketone such as acetone, methyl ethyl ketone, or methyl isobutyl ketone; an aromatic hydrocarbon such as benzene, toluene, ethylbenzene, or xylene; an aliphatic hydrocarbon such as heptane, hexane, or octane; a glycol ether such as propylene glycol methyl ether, dipropylene glycol methyl ether, propylene glycol n-butyl ether, propylene glycol n-propyl ether, or ethylene glycol n-butyl ether; a halogenated hydrocarbon such as dichloromethane, 1,1,1-trichloroethane, or methylene chloride; chloroform; dimethyl sulfoxide; dimethylformamide, acetonitrile; tetrahydrofuran, white spirit; mineral spirit, naphtha, n-methylpyrrolidone; or a combination thereof.

[0023] The amount of solvent varies depending on various factors, such as the type of solvent selected and the amount and type of other starting materials selected for the release coating composition. However, the amount of solvent may range from 1% to 99%, alternatively 2% to 90%, based on the weight of all starting materials in step (1). All or a portion of the solvent may be optionally removed during and / or after step (3). For example, water may be formed as a by-product of the condensation reaction in steps (2) and (3). To allow the reaction to proceed, some or all of this water may be removed, for example, by azeotropic distillation with the solvent.

[0024] (N) Neutralizer The neutralizing agent starting material (N) is optional. The neutralizing agent may include a silyl phosphate. Without being bound by theory, it is believed that the neutralizing agent may be added to remove impurities in the (R) resin and / or (P) polymer described above before the condensation reaction. The neutralizing agent may be, for example, a silyl phosphate. Silyl phosphates such as bis(trimethylsilyl) hydrogen phosphate are commercially available from DSC.

[0025] The amount of neutralizing agent will depend on a variety of factors, including the type of (P) polymer and (R) resin selected, but the amount of neutralizing agent can be from 0.005% to 0.02% based on the combined weight of the starting materials (P), (R), (C), and (N).

[0026] (C) Condensation reaction catalyst The starting material (C) added in step (2) is a condensation reaction catalyst capable of catalyzing the condensation reaction of the hydroxyl groups of the above-mentioned (P) polymer and (R) resin. The condensation reaction catalyst is not particularly limited and may include an acid or a base condensation reaction catalyst. For example, suitable base catalysts include metal hydroxides such as lithium hydroxide, sodium hydroxide, potassium hydroxide and calcium hydroxide, carbonates such as sodium carbonate and potassium carbonate, bicarbonates such as sodium bicarbonate and potassium bicarbonate, metal alkoxides such as sodium methoxide and potassium butoxide, organometallic compounds such as butyl lithium and potassium silanolate, and nitrogen compounds such as ammonia gas, aqueous ammonia, methylamine, trimethylamine and triethylamine. Alternatively, the condensation reaction catalyst may be an acid, for example, organic acids such as acetic acid, benzoic acid, octanoic acid and citric acid, and mineral acids such as hydrochloric acid, sulfuric acid and phosphoric acid are suitable. Alternatively, the condensation reaction catalyst may be an acid catalyst such as an organic acid, for example, benzoic acid.

[0027] Suitable condensation reaction catalysts are commercially available from a variety of sources, such as Sigma Aldrich, Inc. (St. Louis, Missouri, USA) and Acros. The amount of catalyst will depend on a variety of factors, including the type of catalyst selected and the temperature of step (1), but the amount of catalyst may be 0.1% to 0.5% based on the combined weight of the starting materials (P), (R), (C), and (N).

[0028] Step (4) in the above method is optional. After the condensation reaction product of (P) polymer and (R) resin is formed, the condensation reaction product may further contain unreacted starting materials, solvent, and water as a by-product. In step (4), the condensation reaction product may be recovered, for example, the solvent, water, and unreacted starting materials may be removed, for example, by distillation and / or stripping, optionally under heating and / or reduced pressure.

[0029] Step (5) in the above method is optional. The reaction product after step (3) or step (4), if present, can be used to form a silicone pressure-sensitive adhesive composition. Alternatively, if other conditions such as temperature are kept constant, (X) a peroxide crosslinker can be added in step (5) to form a silicone pressure-sensitive adhesive composition that can cure faster than if the peroxide crosslinker is not present.

[0030] (X) Peroxide crosslinking agent The starting material (X) added when step (5) is present is a peroxide crosslinking agent. The peroxide crosslinking agent may be an organic peroxide or hydroperoxide, such as benzoyl peroxide; 4-monochlorobenzoyl peroxide; t-butyl peroctoate; t-butyl peroxybenzoate, tert-butyl peroxybenzoate, tert-butylcumyl peroxide, tert-butyl oxide 2,5-dimethyl-2,5-di-tert-butylperoxyhexane; 2,4-dichlorobenzoyl peroxide; di-tertbutylperoxy-diisopropylbenzene; 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 2,5-di-tert-butylperoxyhexane-3,2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane; cumyl-tert-butyl peroxide; dicumyl peroxide, di-t-butyl peroxide, t-butyl hydroperoxide, cumene hydroperoxide; di-t-amyl peroxide, and combinations of two or more thereof. In addition, di-peroxide crosslinkers may be used alone or in combination with other di-peroxide crosslinkers. Such di-peroxide crosslinkers include, but are not limited to, 1,4-bis-(t-butylperoxycarbo)cyclohexane, 1,2-di(t-butylperoxy)cyclohexane, and 2,5-di(t-butylperoxy)-3-hexyne. Suitable peroxide crosslinkers for use as starting material (X) are known in the art and are commercially available from various suppliers, such as Sigma-Aldrich, Inc. (St. Louis, Missouri, USA).

[0031] Starting material (X) may include one peroxide crosslinking agent or a combination of two or more peroxide crosslinking agents. The amount of starting material (X) added in step (5) depends on various factors, including the type and amount of peroxide crosslinking agent selected, and the selection of the (P) polymer and (R) resin, but the amount of peroxide crosslinking agent, if present, may be from 0.1% to 4% by weight, alternatively from 1% to 4% by weight, alternatively from 2% to 3% by weight, based on the combined weight of starting materials (P), (R), (C), and (S).

[0032] Step (6) in the method described herein is optional. However, step (6) may be included in the method to improve the bonding of the silicone pressure-sensitive adhesive to the backing substrate. Thus, the method for forming an adhesive article may optionally further include (6) treating the surface of the backing substrate before applying the silicone pressure-sensitive adhesive composition. Treating the surface may be carried out by any convenient means, such as applying a primer or subjecting the surface to a corona discharge treatment, etching, or plasma treatment before applying the silicone pressure-sensitive adhesive composition to the surface. Alternatively, treating the surface may include applying a primer to the surface of the backing substrate.

[0033] Step (7), coating the silicone pressure-sensitive adhesive composition onto the surface of the backing substrate, can be carried out by any convenient means. For example, the silicone pressure-sensitive adhesive composition can be applied by a gravure coater, a comma coater, an offset coater, an offset gravure coater, a roller coater, a reverse roller coater, an air knife coater, a slot die, or a curtain coater.

[0034] In the methods described herein, steps (7)-(9) can be carried out via wet casting or dry casting, in which the silicone pressure sensitive adhesive layer can be permanently adhered to a backing substrate such as a polymeric film and / or foam, as described below.

[0035] The backing substrate can be any material that can withstand the curing conditions used in step (9) to cure the silicone pressure sensitive adhesive composition to form a silicone pressure sensitive adhesive on the surface of the backing substrate. For example, any backing substrate that can withstand heat treatment at a temperature of 120°C or higher, or even 150°C, is suitable. Examples of materials suitable for such backing substrates include polymer films and / or foams, which may include polyimide (PI), polyetheretherketone (PEEK), polyethylenenaphthalate (PEN), liquid crystal polyarylate, polyamideimide (PAI), polyethersulfide (PES), polyethyleneterephthalate (PET), polycarbonate (PC), polymethylmethacrylate (PMMA), thermoplastic polyurethane (TPU), thermoplastic elastomer (TPE), polyethylene (PE), or polypropylene (PP). Alternatively, the backing substrate can be glass. Alternatively, the backing substrate can be a release liner, for example, when the silicone pressure sensitive adhesive is used in a dry casting process. The thickness of the backing substrate is not critical. However, the thickness may be from 5 μm to 300 μm, alternatively from 10 μm to 200 μm. Alternatively, the backing substrate used in step (7) may be selected from the group consisting of PE, PU, ​​TPE, and TPU.

[0036] Step (8) of the method includes drying the silicone pressure sensitive adhesive composition. Drying can be carried out by any convenient means, such as by heating at a temperature and for a time sufficient to evaporate all or a portion of the solvent, but insufficient to completely cure the silicone pressure sensitive adhesive composition. For example, drying can be carried out by heating at a temperature of from 50° C. to 120° C., alternatively from 70° C. to 100° C., alternatively from 70° C. to 80° C., for a time sufficient to remove all or a portion of the solvent (e.g., from 30 seconds to 1 hour, alternatively from 1 minute to 5 minutes).

[0037] After drying, the method further includes step (9), curing the silicone pressure-sensitive adhesive composition to form a laminate article comprising a silicone pressure-sensitive adhesive layer having a surface adhered to a surface of a backing substrate, the silicone pressure-sensitive adhesive layer further comprising an opposing surface opposite the surface of the backing substrate.

[0038] Curing the pressure-sensitive adhesive composition in step (9) can be carried out by heating at a temperature of 80°C to 200°C, alternatively 90°C to 210°C, alternatively 150°C to 205°C, alternatively 180°C to 205°C, for a time sufficient to cure the pressure-sensitive adhesive composition (e.g., 30 seconds to 1 hour, alternatively 1 minute to 5 minutes). If the cure rate needs to be increased or the process oven temperature needs to be reduced, the amount of (X) peroxide crosslinker can be increased. This forms a silicone pressure-sensitive adhesive on the surface of the backing substrate. Curing can be carried out by placing the backing substrate in an oven. The amount of silicone pressure-sensitive adhesive composition applied to the backing substrate depends on the particular application, but the amount can be sufficient such that the silicone pressure-sensitive adhesive can have a thickness of 5 micrometers to 100 micrometers after curing.

[0039] The methods described herein may optionally further include additional steps after step (9). The additional steps include, for example, applying a removable release liner to the opposite surface of the silicone pressure-sensitive adhesive layer opposite the backing substrate to protect the silicone pressure-sensitive adhesive prior to use (e.g., when the backing substrate is a polymeric film and / or foam, or glass). The release liner may be applied before, during, or after curing the silicone pressure-sensitive adhesive composition.

[0040] The silicone pressure sensitive adhesive prepared in step (9) adheres to a silicone rubber article. Without wishing to be bound by theory, it is believed that the silicone pressure sensitive adhesive prepared in step (9) may have an adhesion to silicone rubber of >1,000 gf / in, alternatively >1,200 gf / in, alternatively >1,500 gf / in, while the adhesion may be up to 2,600 gf / in, alternatively up to 2,500 gf / in, alternatively up to 2,300 gf / in, when tested according to the Peel Adhesion Test Method described in the Examples below.

[0041] Although treatment of the silicone rubber article is not required for this adhesion, the method may optionally further comprise treating the surface of the silicone rubber article, step (10), which may promote and / or improve adhesion of the silicone pressure sensitive adhesive to the surface of the silicone rubber article. Treating the surface of the silicone rubber article may be carried out by any convenient means, such as, for example, cleaning the silicone rubber surface with an alcohol, such as isopropanol, or any of the surface treatments described above in step (6).

[0042] The silicone rubber article is not particularly limited. The silicone rubber article may have a durometer, Shore A, of 30 to 75, alternatively 30 to 50, as measured by ASTM D2240. Liquid silicone rubber (LSR) and high viscosity rubber (HCR) may be used for the silicone elastomer. LSR is known in the art and may be made by known methods, such as those disclosed in U.S. Patent No. 5,777,002 to Conway et al. or U.S. Patent No. 8,198,357 to Jeram et al. Alternatively, the silicone rubber article may be selected based on the desired end use of the laminate article prepared herein.

[0043] For example, optical silicone elastomers (optical LSRs) are known in the art and are described, for example, in U.S. Patent No. 8,859,693 to Hasegawa et al. and U.S. Patent No. 8,853,332 to Akitomo et al. Optical LSRs are commercially available. For example, optical LSRs include moldable optical silicone elastomers SILASTIC™ MS-1001, MS-1002, MS-1003, MS-4001, MS-4002, and MS-4007, as well as SYLGARD™ 182, 184, and 186, which are other optical silicone elastomers, all of which are commercially available from DSC.

[0044] Alternatively, LSR such as XIAMETER™ RBL-2004-30, XIAMETER™ RBL-2004-50 SILASTIC™ 9202-50 LSR, SILASTIC™ LCF 3760, and SILASTIC™ LCF3600, or Varox™ DBPH-50 from TDCC, or SILASTIC™ RBC 7600-50, XIAMETER™ RBB 2000-35, XIAMETER™ RBB 2001-65, XIAMETER™ RBB-2030-40EN, XIAMETER™ RBB-6660-60EN, XIAMETER™ RBB-2002-30, each from DSC. An HCR such as Base, XIAMETER™ RBB-2004-60, or XIAMETER™ RBB-2220-70 may be used.

[0045] The method described herein further comprises, as step (11), adhering the opposite surface of the silicone pressure sensitive adhesive described in step (9) to the surface of a silicone rubber article. Step (11) can be carried out by any convenient means, such as contacting the surface of the silicone rubber article with the opposite surface of the silicone pressure sensitive adhesive and applying pressure. If a release liner is used to protect the opposite surface of the silicone pressure sensitive adhesive, the release liner is removed before contacting the surface of the silicone rubber article with the opposite surface of the silicone pressure sensitive adhesive. The product obtained by preparing in step (11) is a laminated article. In the above wet casting method, the laminated article can include a backing substrate selected from a polymer film, a polymer foam or glass, the above silicone pressure sensitive adhesive, and a silicone rubber article.

[0046] Alternatively, when dry casting is used in steps (7)-(9) above, the backing substrate includes a release liner. The release liner may be removed after step (9) to form the silicone pressure sensitive adhesive layer as a free-standing film. Alternatively, the release liner may be removed after step (11). When dry casting is performed, the method further comprises: Optionally, (12) treating a surface of the second silicone rubber article; and (13) adhering a surface of the silicone pressure sensitive adhesive layer (exposed by removal of the release liner) to a surface of a second silicone rubber article.

[0047] The second silicone rubber article is as described above for use in step (11). The second silicone rubber article can be the same as the silicone rubber article used in step (11). Alternatively, the second silicone rubber article can be different from the silicone rubber article used in step (11). In this case, the laminated article formed by the present method has a silicone pressure sensitive adhesive layer sandwiched between the silicone rubber article and the second silicone rubber article.

[0048] FIG. 1 shows a partial cross-sectional view of a laminate article (100) prepared by the method described above. The laminate article (100) comprises a silicone pressure sensitive adhesive (102) having a surface (102a) and an opposing surface (102b). The opposing surface (102b) of the silicone pressure sensitive adhesive (102) adheres to a surface (103a) of a silicone rubber article (103) with a peel adhesion of >1,000 gf / in, as measured by the test method described in the Examples below. The silicone pressure sensitive adhesive (102) may have a thickness of 10 μm to 200 μm. The silicone pressure sensitive adhesive (102) adheres to a backing substrate (101) having a surface (101b). The surface (102a) of the silicone pressure sensitive adhesive (102) is in contact with the surface (101b) of the backing substrate (101). The backing substrate (101) may be selected from the group consisting of PE, PU, ​​TPU, and TPE and may have a thickness of 10 μm to 200 μm. The silicone rubber article (103) may be LSR or HCR, as described above.

[0049] The silicone pressure sensitive adhesive composition can be used in the fabrication of a laminate article (100) by wet casting. For example, the silicone pressure sensitive adhesive composition can be applied to the surface (101b) of a backing substrate (101) and cured to form a silicone pressure sensitive adhesive (102). Alternatively, the silicone pressure sensitive adhesive composition can be applied to the surface (103a) of a silicone rubber article (103) and cured to form a silicone pressure sensitive adhesive (102). Alternatively, the silicone pressure sensitive adhesive composition can be applied to the surface of a release liner and cured to form a silicone pressure sensitive adhesive (102). The surface (103a) of the silicone rubber article (103) can then be brought into contact with the opposite surface (102b) of the silicone pressure sensitive adhesive (102), and the surface (101b) of the backing substrate (101) can be brought into contact with the surface (102a) of the silicone pressure sensitive adhesive (102). Pressure may be applied to adhere the layers of the backing substrate (101), the silicone pressure sensitive adhesive (102), and the silicone rubber article (103) together.

[0050] Alternatively, wet casting may be used to prepare a laminate article comprising a backing substrate comprising the silicone rubber and silicone pressure sensitive adhesive described above, and optionally a (second) silicone rubber article. In this method, the backing substrate may be the same or a different silicone rubber article as the (second) silicone rubber article used in step (11), described below. Alternatively, the backing substrate may comprise two or more constituent materials, such as a mesh impregnated with silicone rubber (which may be fabricated from a polymeric material, as described above). This method for fabricating a laminate article includes: (1) combining starting materials under conditions which effect a condensation reaction, the starting materials being: (P) a bis-hydroxyl terminated polydiorganosiloxane having a weight average molecular weight of 10,000 g / mol to <200,000 g / mol as measured by GPC, wherein starting material (P) is present in an amount of >20.5 weight percent based on the combined weight of starting materials (P) and (R); (R) a hydroxyl-functional polyorganosilicate resin having a weight average molecular weight of 15,000 g / mol to 30,000 g / mol as measured by GPC, wherein the starting material (R) is present in an amount of <79.5 wt.%, based on the combined weight of the starting materials (P) and (R); (S) a solvent; and optionally, (N) a neutralizing agent; starting materials (R) and (P) are present in a weight ratio (R) / (P) of 2.27 / 1 to <3.88 / 1, thereby forming a reaction mixture; (2) adding (C) a condensation reaction catalyst to the reaction mixture, thereby forming a catalyzed reaction mixture; (3) heating the catalyst reaction mixture at a temperature >RT to 145°C to remove water; Optionally, (4) recovering the condensation reaction product of (P) and (R); and optionally, (5) adding up to 4 weight percent, based on the combined weight of (R) and (P), of an (X) peroxide crosslinking agent, thereby forming a silicone pressure sensitive adhesive composition; Optionally, (6) treating a surface of the backing substrate with silicone rubber; and (7) coating a surface of a backing substrate with a silicone pressure sensitive adhesive composition; (8) drying the silicone pressure sensitive adhesive composition; and (9) curing the silicone pressure sensitive adhesive composition to form a silicone pressure sensitive adhesive having a surface adhered to a surface of a backing substrate, the silicone pressure sensitive adhesive layer further comprising an opposing surface opposite the surface of the backing substrate. Optionally, (10) treating a surface of the silicone rubber article; and (11) adhering an opposing surface of the silicone pressure sensitive adhesive to a surface of the silicone rubber article.

[0051] FIG. 2 shows a partial cross-sectional view of a laminated article (200) prepared by the method described above. The laminated article (200) comprises a silicone pressure sensitive adhesive (202) having a surface (202a) and an opposing surface (202b). The silicone pressure sensitive adhesive (202) can have a thickness of 10 μm to 200 μm. The silicone pressure sensitive adhesive (202) is adhered to a backing substrate comprising a silicone rubber (201) and having a surface (201b) with a peel adhesion of >1,000 gf / in as measured by the test method described in the Examples below. The surface (202a) of the silicone pressure sensitive adhesive (202) is in contact with the surface (201b) of the backing substrate (201). The backing substrate (201) can be a silicone rubber article such as an LSR or HCR, as described above. Alternatively, the backing substrate (201) can comprise a mesh impregnated with silicone rubber.

[0052] The silicone pressure sensitive adhesive composition can be used in the fabrication of the laminate article (200) by wet casting. For example, the silicone pressure sensitive adhesive composition can be applied to a surface (201b) of a backing substrate (201) and cured to form a silicone pressure sensitive adhesive (202). EXAMPLES

[0053] The following examples are provided to illustrate the invention to one of ordinary skill in the art and should not be construed as limiting the scope of the invention as set forth in the claims. The starting materials used in these examples are listed in Table 1.

[0054] [Table 1]

[0055] TDCC means The Dow Chemical Company, Midland, Michigan, USA. DSC means Dow Silicones Corporation, Midland, Michigan, USA.

[0056] In this Reference Example 1, the condensation reaction product (thickened resin) was prepared as follows: PDMS polymer, MQ resin, solvent, and neutralizer were combined in a three-neck flask at RT. The contents of the flask were stirred at 250 rpm for 20 minutes using a medium-neck stainless steel stirring paddle. The condensation catalyst was then added while stirring. Another neck was connected to a Dean-Stark trap, which was then connected to a condenser with tap water cooling capability. The last neck contained a thermometer and a nitrogen sweep adapter to close the system. Finally, the three-neck flask with the mixture inside was mounted on a heating mantle with temperature control and heated to a reaction temperature of 145°C. The reaction was allowed to continue for 3 hours from the start of reflux. Following this procedure, thickened resins IE1-IE6 and CE1-CE19 were prepared.

[0057] In this Reference Example 2, a comparative silicone pressure sensitive adhesive composition, CE20, was prepared as follows: The starting materials were added to a dental mixer cup and mixed at 3500 rpm for 30 seconds until homogenous. This cold blended PSA was immediately used in the coating / curing process.

[0058] In this Reference Example 3, a peroxide crosslinker was added to form a peroxide curable silicone pressure sensitive adhesive composition, which was coated onto a backing substrate and cured as follows. For the peroxide curable silicone pressure sensitive adhesive compositions (IE1-IE6 and CE1-CE21), peroxide crosslinker (in toluene) and solvent 1 were added to each composition prepared as described in Reference Examples 1 and 2 above in a dental mixer cup to reach a solids level of 50 wt% and a peroxide crosslinker level of 2 wt%. For sample IE6, the peroxide crosslinker level was varied in the curing process (IE6A for 0 wt% peroxide crosslinker level, IE6B for 1 wt% peroxide crosslinker level, and IE6C for 3 wt% peroxide crosslinker level). The resulting sample was mixed at 3500 rpm for 30 seconds until homogenous. Each sample was prepared for application testing by coating onto a 2 mil thick polyester (PET) sheet using a 3 mil coating bar. Each sheet was then cured in an oven at 80°C for 2 minutes, followed by a 2 minute cure at 180°C.

[0059] In this Reference Example 4, a comparative hydrosilylation-curable pressure-sensitive adhesive composition CE22 was prepared as follows: PSA was added to a dental mixer cup first. Catalyst 3 was then added to the mixture and mixed at 3500 rpm for 30 seconds until homogenous.

[0060] In this Reference Example 5, the hydrosilylation-curable pressure-sensitive adhesive composition CE22 was coated onto 2 mil thick polyester (PET) sheets using a 3 mil coating bar. Each sheet was then cured in a 150° C. curing oven for 3 minutes.

[0061] The starting materials and the amounts used to prepare each sample are shown in Tables 2-7 below.

[0062] In this Reference Example 6, the silicone rubber substrate was prepared as follows. The liquid silicone rubber (LSR) substrates were XIAMETER™ RBL-2004-30 LSR and XIAMETER™ RBL-2004-50 LSR samples from DSC. To mix Part A and Part B, 100g of Part A and 100g of Part B were added to a dental mixer cup and mixed for 3 cycles, each cycle for 20 seconds at 1800 rpm. The cup was scraped and mixed by hand between cycles to ensure that the material did not stick to the bottom and corners of the dental cup. The mixture was transferred to a polished book mold or Teflon lined chase and cured at 350°F for 5 minutes.

[0063] A peroxide cured high viscosity rubber (HCR) substrate was prepared by blending 60 parts per million (phr) of XIAMETER® RBB 2000-35 and 40 phr of XIAMETER® RBB 2001-65 on a two roll mill. 1.0 phr of Varox® DBPH-50 (45% 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and 55% calcium carbonate / silica) was ground into the blend. The material was sheeted from the mill, placed into a 10" x 10" x 0.78" chase, and press cured at 350°F for 10 minutes under 30 tons of pressure. The chase was removed from the press, cooled, and a slab was removed from the chase.

[0064] The platinum cured HCR substrate was prepared as follows: SILASTIC™ RBC 7600-50 was ground in a two roll mill. The material was sheeted from the mill and placed into a 10 inch x 10 inch x 0.78 inch chase and press cured at 350°F for 10 minutes under 30 tons of pressure. The chase was removed from the press, cooled, and a slab was removed from the chase.

[0065] In this Reference Example 7, the adhesion of the pressure-sensitive adhesives prepared according to Reference Examples 3 and 5 to the silicone rubber prepared according to Reference Example 6 was measured as follows.

[0066] Peel Adhesion: Peel adhesion (180°) was tested according to PSTC-101 standard. Silicone pressure sensitive adhesive coated on 2 mil polyester film (tape) was laminated onto a silicone rubber surface or clean stainless steel panel, typically after 1 day after curing. The silicone rubber surface was wiped with isopropyl alcohol to clean the surface and allowed to dry for 5 minutes under ambient conditions before laminating the silicone pressure sensitive adhesive to it. After lamination, a 2 kg rubber covered roller was applied to the resulting article (5 times each before and after), and the article was allowed to rest for 20 minutes dwell time at room temperature before peel adhesion testing. A TMI peel and adhesion tester was used to pull 1 inch wide tape from the silicone rubber or stainless steel substrate at 12 inches / minute.

[0067] The results of the adhesion tests are shown in Tables 8 to 14 below.

[0068] [Table 2]

[0069] [Table 3]

[0070] [Table 4]

[0071] [Table 5]

[0072] [Table 6]

[0073] Samples CE14-CE19 used a high Mw gum (instead of a polydiorganosiloxane polymer) in formulating the silicone pressure sensitive adhesive composition and these samples showed reduced adhesion compared to sample IE1, which used a polydiorganosiloxane polymer as described herein. Samples CE8-CE18 all showed poor adhesion under the conditions tested.

[0074] [Table 7]

[0075] [Table 8]

[0076] [Table 9]

[0077] The data in Tables 8 and 9 show that increasing the resin to polymer ratio increases adhesion to silicone rubber under the conditions tested. PSAs made with high resin to polymer ratios had no adhesion to steel substrates but high adhesion to silicone rubber substrates under the conditions tested.

[0078] [Table 10]

[0079] The data in Table 10 show that the use of a high Mw resin resulted in a PSA with strong adhesion to silicone rubber. However, the use of a resin with too low Mw resulted in a PSA (CE7) with poor adhesion under the conditions tested. Without wishing to be bound by theory, it is believed that IE6, IE6A, IE6B, and IE6C indicate that a lower amount of peroxide crosslinker (0-2% in samples IE6A, IE6, and IE6B) may provide higher peel adhesion to LSR.

[0080] [Table 11]

[0081] [Table 12]

[0082] The data in Tables 9, 11, and 12 show that under the conditions tested, the use of the polydiorganosiloxane polymers described herein results in a PSA with strong adhesion to silicone rubber (IE1), while the use of a high Mw gum polymer results in poor adhesion (CE19). Other comparative compositions (CE) show that low resin to polymer ratios in the PSA, low Mw resins, or high Mw gum polymers result in poor adhesion to silicone rubber.

[0083] [Table 13]

[0084] Without wishing to be bound by theory, it is believed that the data in Table 13 indicated that PSA samples made via low temperature blending exhibited poor adhesion to silicone rubber under the conditions tested.

[0085] [Table 14]

[0086] The examples (IE1, IE3, IE5, and IE6) showed approximately twice the adhesive strength to silicone rubber compared to VS 3M commercial 9731 tape.

[0087] In this Example 8, samples of laminate articles were prepared by a method involving wet casting (Method 2) as follows. 1. Two samples of silicone pressure sensitive adhesive compositions were prepared by mixing peroxide crosslinker (in toluene) and solvent 1 with each of compositions IE6 and CE21 (prepared as above) in a dental mixer cup to reach a solids level of 50% by weight and a peroxide crosslinker level of 2% by weight. Each resulting sample was mixed at 3500 rpm for 30 seconds until homogenous. 2. Four silicone rubber substrates (two each of 50 durometer LSR and Pt cured HCR) were prepared as described above in Reference Example 6. The surface of each silicone rubber substrate was cleaned by wiping with isopropyl alcohol and drying under ambient conditions for 5 minutes. 3. Each sample of the silicone pressure sensitive adhesive composition was coated onto the cleaned surface of a silicone rubber substrate using a 3 mil coating bar. Each coated substrate was then placed in an oven at 80° C. for 2 minutes, followed by 180° C. for 2 minutes to prepare a laminate of a (cured) silicone pressure sensitive adhesive layer on each silicone rubber sheet. 4. Four silicone rubber substrates (two each of 50 durometer LSR and Pt cured HCR) were prepared as described above in Reference Example 6. The surface of each silicone rubber substrate was cleaned by wiping with isopropyl alcohol and drying under ambient conditions for 5 minutes. 5. One day after step 3, the surface of each silicone pressure sensitive adhesive layer was contacted with the cleaned surface of each silicone rubber substrate from step 4. A 2 kg rubber covered roller was applied to the resulting articles (five times each before and after) as above, except that no polyester film backing substrate was used, and the articles were allowed to rest for 20 minutes dwell time at room temperature before peel adhesion testing according to PSTC-101 standard. A TMI peel and adhesion tester was used to pull the 1 inch wide tape from the silicone rubber substrate at 12 inches / minute. The peel adhesion test results are shown in Table 15 below.

[0088] [Table 15]

[0089] The data in Table 15 show that when the silicone rubber article is used as a backing substrate in a method using wet casting, the silicone pressure sensitive adhesive prepared by the methods described herein has a higher peel adhesion than commercially available PSA 2 (CE21) applied to a backing substrate using a wet casting method.

[0090] In this Example 9, samples of laminate articles were prepared by a method involving dry casting (Method 3) as follows. 1. Two samples of silicone pressure sensitive adhesive compositions were prepared by mixing peroxide crosslinker (in toluene) and solvent 1 with each of compositions IE6 and CE21 (prepared as above) in a dental mixer cup to reach a solids level of 50% by weight and a peroxide crosslinker level of 2% by weight. Each resulting sample was mixed at 3500 rpm for 30 seconds until homogenous. 2. Each sample of the silicone pressure sensitive adhesive composition was coated onto a fluorosilicone release liner using a 3 mil coating bar. Each coated liner was then placed in an oven at 80° C. for 2 minutes, followed by 180° C. for 2 minutes to prepare a laminate of a (cured) silicone pressure sensitive adhesive layer on each fluorosilicone release liner. Each laminate was aged at RT for 1 day. 3. Four silicone rubber substrates (two each of 50 durometer LSR and Pt cured HCR) were prepared as described above in Reference Example 6. The surface of each silicone rubber substrate was cleaned by wiping with isopropyl alcohol and drying under ambient conditions for 5 minutes. 4. The surface of each silicone pressure sensitive adhesive layer from step 2 was contacted with the cleaned surface of each silicone rubber substrate from step 3. 5. Four silicone rubber substrates (two each of 50 durometer LSR and Pt cured HCR) were prepared as described above in Reference Example 6. The surface of each silicone rubber substrate was cleaned by wiping with isopropyl alcohol and drying under ambient conditions for 5 minutes. 6. One day after step 4, the fluorosilicone release liner was removed from each laminate and the resulting exposed surface of each silicone pressure sensitive adhesive layer was contacted with the cleaned surface of the silicone rubber substrate from step 5. A 2 kg rubber covered roller was applied to the resulting articles (five times each before and after) as described above, except that no polyester film backing substrate was used, and the articles were allowed to rest for 20 minutes dwell time at room temperature before peel adhesion testing according to PSTC-101 standard was performed. A TMI peel and adhesion tester was used to pull the 1 inch wide tape from the silicone rubber substrate at 12 inches / minute. The peel adhesion test results are shown in Table 16 below.

[0091] [Table 16]

[0092] The data in Table 16 show that when a laminate article comprising a silicone pressure sensitive adhesive between two silicone rubber substrates is prepared by a dry casting method, the silicone pressure sensitive adhesive prepared by the methods described herein has a higher peel adhesion than commercially available PSA 2 (CE21).

[0093] Definitions and Use of Terms All amounts, ratios and percentages are by weight unless otherwise indicated. The amounts of all starting materials in the composition total 100% by weight. The Summary and Abstract of the Invention are incorporated herein by reference. The articles "a", "an" and "the" each refer to one or more, unless otherwise indicated by the context of the specification. The singular includes the plural unless otherwise indicated. The terms "comprising" and its derivatives, such as "comprise" and "comprises", are used herein in their broadest sense to mean and include the notion of "including," "include," "consist(ing) essentially of," and "consist(ing) of." The use of "for example," "eg," "such as," and "including" to list examples is not limited to only the examples listed. Thus, "for example" or "such as" means "for example, but not limited to" or "such as, but not limited to" and includes other similar or equivalent examples.

[0094] It is to be understood that the appended claims are not limited to the specific compounds, compositions, or methods described therein to express a "detailed description," and may vary among specific embodiments within the scope of the appended claims. With respect to any Markush group relied upon in this specification to describe specific features or aspects of various embodiments, different, special, and / or unexpected results may result from each element of the respective Markush group independent of all other Markush elements. Each element of the Markush group may be relied upon individually and / or in combination to provide sufficient support for specific embodiments within the scope of the appended claims.

[0095] Abbreviations used herein are defined in Table 17 below.

[0096] [Table 17]

[0097] The Mn, Mw, and molecular weight distribution of the polymer and condensation reaction products can be determined by GPC using an Agilent Technologies 1260 Infinity chromatograph and toluene as the solvent. The instrument is equipped with two PLgel Mixed C columns. Calibration was performed using polystyrene standards. Samples were prepared by dissolving the polymer in toluene (approximately 10 mg / mL) and then immediately analyzing the material by GPC (flow rate of 1 mL / min and column temperature of 45° C.).

[0098] The Mn, Mw, and molecular weight distribution of the resins can be determined by GPC using an Agilent Technologies 1260 Infinity chromatograph and ethyl acetate as the solvent. The instrument is equipped with two columns, namely, Agilent PLgel Mixed-D and PLgel Mixed-E columns. Calibration was performed using polystyrene standards. Samples were prepared by dissolving the polymer in toluene (approximately 20 mg / mL) and then immediately analyzing the material by GPC (flow rate of 1 mL / min and column temperature of 35° C.).

Claims

1. 1. A method for making a laminate article, the method comprising: (1) combining starting materials under conditions which effect a condensation reaction, said starting materials being: (P) a bis-hydroxyl terminated polydiorganosiloxane having a weight average molecular weight of 10,000 g / mol to <200,000 g / mol as measured by GPC, wherein starting material (P) is present in an amount of >20.5 weight percent based on the combined weight of starting materials (P) and (R); (R) a hydroxyl-functional polyorganosilicate resin having a weight average molecular weight of 15,000 g / mol to 30,000 g / mol as measured by GPC, wherein the starting material (R) is present in an amount of <79.5 wt.%, based on the combined weight of the starting materials (P) and (R); (S) a solvent; and optionally, (N) a neutralizing agent; starting materials (R) and (P) are present in a weight ratio (R) / (P) of 2.27 / 1 to <3.88 / 1, thereby forming a reaction mixture; (2) adding (C) a condensation reaction catalyst to the reaction mixture, thereby forming a catalyzed reaction mixture; (3) heating the catalyst reaction mixture at a temperature >RT to 145° C. to remove water; Optionally, (4) recovering the condensation reaction product of (P) and (R); and optionally, (5) adding up to 4 weight percent, based on the combined weight of (R) and (P), of (X) a peroxide crosslinker, thereby forming a silicone pressure sensitive adhesive composition; Optionally, (6) treating the surface of the backing substrate; and (7) coating the surface of the backing substrate with the silicone pressure sensitive adhesive composition; (8) drying the silicone pressure sensitive adhesive composition; and (9) curing the silicone pressure sensitive adhesive composition to form a silicone pressure sensitive adhesive having a surface adhered to the surface of the backing substrate, the silicone pressure sensitive adhesive layer further comprising an opposing surface opposite the surface of the backing substrate; and Optionally, (10) treating a surface of the silicone rubber article; and (11) adhering said opposing surface of a silicone pressure sensitive adhesive to said surface of said silicone rubber article.

2. The starting material (P), said bis-hydroxyl terminated polydiorganosiloxane, has the formula 【Chemistry 1】 wherein each R 1 2. The method of claim 1, wherein: a is an independently selected alkyl group of 1 to 6 carbon atoms; and the subscript a represents the average number of difunctional siloxane units per molecule, where 250≦a≦3,000.

3. The hydroxyl-functional polyorganosilicate resin starting material (R) has the unit formula (R 1 3 SiO 1/2 ) b (SiO 4/2 ) c (HO 1/2 ) d wherein each R 1 2. The method of claim 1, wherein: b is an independently selected alkyl group of 1 to 6 carbon atoms; subscripts b and c represent the mole fractions of mono- and tetrafunctional units, respectively, with subscripts b and c having values ​​such that 0.4≦b≦0.5, 0.5≦c≦0.6, and the amount (b+c)=1; and subscript d represents the amount of hydroxyl groups in the resin, with subscript d having a value sufficient to provide the resin with a hydroxyl content of 2% to 5% by weight.

4. 2. The method of claim 1, wherein (R) / (P) is from 2.9 / 1 to <3.88 / 1.

5. 5. The method of claim 4, wherein (R) / (P) is from 2.9 / 1 to 3 / 1.

6. 2. The method of claim 1, wherein (N) the neutralizing agent is present and the neutralizing agent comprises a silyl phosphate.

7. The method of claim 1 , wherein (C) the condensation reaction catalyst is an acid.

8. 2. The method of claim 1, wherein step (5) is present and (X) the peroxide crosslinking agent comprises benzoyl peroxide.

9. The method of claim 1 , wherein step (6) is present and step (6) comprises applying a primer to the surface of the backing substrate.

10. 10. The method of claim 1, wherein step (10) is present and step (10) comprises cleaning the surface of the silicone rubber with alcohol.

11. 2. The method of claim 1, wherein in step (11), the silicone rubber has a durometer of 30 to 50.

12. A laminated article prepared by the method of any one of claims 1 to 11.

13. The backing substrate in step (7) comprises a release liner, and the process further comprises: removing the release liner after step (9); and Optionally, (12) treating a surface of the second silicone rubber article; and 13. The method of claim 1, further comprising adhering said surface of said silicone pressure sensitive adhesive layer to said surface of said second silicone rubber article.

14. 1. A method for making a laminate article, the method comprising: (1) combining starting materials under conditions which effect a condensation reaction, said starting materials being: (P) a bis-hydroxyl terminated polydiorganosiloxane having a weight average molecular weight of 10,000 g / mol to <200,000 g / mol as measured by GPC, wherein starting material (P) is present in an amount of >20.5 weight percent based on the combined weight of starting materials (P) and (R); (R) a hydroxyl-functional polyorganosilicate resin having a weight average molecular weight of 15,000 g / mol to 30,000 g / mol as measured by GPC, wherein the starting material (R) is present in an amount of <79.5 wt.%, based on the combined weight of the starting materials (P) and (R); (S) a solvent; and optionally, (N) a neutralizing agent; starting materials (R) and (P) are present in a weight ratio (R) / (P) of 2.27 / 1 to <3.88 / 1, thereby forming a reaction mixture; (2) adding (C) a condensation reaction catalyst to the reaction mixture, thereby forming a catalyzed reaction mixture; (3) heating the catalyst reaction mixture at a temperature >RT to 145° C. to remove water; Optionally, (4) recovering the condensation reaction product of (P) and (R); and optionally, (5) adding up to 4 weight percent, based on the combined weight of (R) and (P), of (X) a peroxide crosslinker, thereby forming a silicone pressure sensitive adhesive composition; Optionally, (6) treating a surface of the backing substrate with silicone rubber; and (7) coating the surface of the backing substrate with the silicone pressure sensitive adhesive composition; (8) drying the silicone pressure sensitive adhesive composition; and (9) curing the silicone pressure sensitive adhesive composition to form a silicone pressure sensitive adhesive layer having a surface adhered to the surface of the backing substrate, the silicone pressure sensitive adhesive layer further comprising an opposing surface opposite the surface of the backing substrate.

15. Optionally, (10) treating a surface of the silicone rubber article; and 11. The method of claim 14, further comprising: adhering said opposing surface of a layer of silicone pressure sensitive adhesive to said surface of said silicone rubber article.

Citation Information

Patent Citations

  • Production of pressure-sensitive silicone adhesive

    JP1998130617A

  • Pressure-sensitive silicone adhesive composition

    JP1998324860A

  • Silicone-based pressure-sensitive adhesive composition, pressure-sensitive adhesive sheet, and silicone rubber laminate

    JP2009155515A

  • Aqueous pressure sensitive adhesive composition

    JP2018506612A

  • Method to activate silicone rubber surfaces

    US20120322954A1