Novel binding compositions for multiple uses

Aqueous binding compositions using reducing sugars, sulfamates, and lactams via the Maillard reaction address formaldehyde emissions and strength issues, achieving comparable bonding strength to phenolic resins and meeting environmental regulations.

JP2024535780APending Publication Date: 2024-10-02STM TECH SRL
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024515433
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-07
Filing Date
2022-09-06
Publication Date
2024-10-02

AI Technical Summary

Technical Problem

Existing mineral fiber bonding compositions emit formaldehyde, which is a carcinogen, and do not provide bonding strength comparable to phenolic resins, while also failing to meet stringent environmental regulations regarding volatile compound emissions.

Method used

Aqueous binding compositions comprising reducing sugars, sulfamates, ammonium hydroxide, and lactams, which polymerize via the Maillard reaction, providing improved bonding strength and eliminating formaldehyde emissions.

Benefits of technology

The compositions achieve bonding strength comparable to phenolic resins, with enhanced mechanical properties and compliance with environmental regulations, producing mineral fiber materials with reduced formaldehyde emissions and improved mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024535780000001
    Figure 2024535780000001
  • Figure 2024535780000002
    Figure 2024535780000002
  • Figure 2024535780000003
    Figure 2024535780000003
Patent Text Reader

Abstract

The present invention relates to an aqueous binding composition comprising at least one reducing sugar, at least one sulfamate and / or sulfamic acid, a pH modifier consisting of ammonium hydroxide (NH4OH), organic and / or inorganic ammonium salts, and / or organic amines, or combinations thereof, and at least one lactam. The binder can be effectively used to bind cotton fibers, cellulose fibers, organic textiles, carbon powder, natural and man-made inorganic fibers to obtain products with high mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] In a more general aspect, the present invention relates to an aqueous binding composition (binder) that has multiple uses.

[0002] In particular, the present invention relates to an aqueous binding composition comprising at least one reducing sugar, at least one sulfamate, and a lactam, preferably caprolactam. [Background technology]

[0003] Mineral fiber materials are widely used, for example in civil or industrial construction, as thermal and acoustic insulation materials and are known in the art. These materials are formed by mineral fibers bound together by a binding composition (binder), usually aqueous, that contains a curing / crosslinking agent and is thermosetting and capable of firmly binding the fibers by high-temperature thermomechanical processing. In this respect, the process for preparing these mineral fiber materials generally includes a first step in which so-called "loose" (i.e. not bound together) mineral fibers are formed, followed by a step of high-temperature impregnation of the loose fibers with a binding composition that polymerizes after contact and high temperature, thereby firmly and integrally binding the fibers and giving the shape and consistency of the final product.

[0004] Typically, the bonding composition applied to the mineral fibers is in the form of an aqueous solution containing a thermosetting resin and additives such as crosslinking catalysts for the resin, silanes that aid in chemical bonding between the fibers and the resin, anti-dust mineral oils, etc. The bonding composition is typically applied to the fibers by spraying.

[0005] The properties of the bonding composition vary greatly depending on the properties of the resin. From an application standpoint, the adhesive composition must have good sprayability and be capable of being deposited onto the surface of the fiber in order to effectively bond to it.

[0006] Also, because the bonding composition is generally prepared at the time of use by mixing the resin and additives described above, the resin must be stable for a certain period of time before it is used to form the bonding composition.

[0007] With regard to compliance with current regulations, the resin must not be polluting, i.e., it must contain the minimum possible amount of compounds that may be harmful to human health or the environment, and should generate the minimum possible amounts during or after the bonding process.

[0008] The most commonly used thermosetting resins are phenolic resins of the resole type, which, in addition to being able to crosslink well at the application temperatures for mineral fibers, are relatively inexpensive.

[0009] The most common resoles are obtained by condensation of phenols with formaldehyde in the presence of a basic catalyst. These resoles contain a certain proportion of free monomers, especially formaldehyde, the presence of which is undesirable due to its known harmful effects.

[0010] Formaldehyde has long been found to be a dangerous carcinogen, therefore resole-based resins are commonly treated with urea, which reacts with the free formaldehyde, thereby forming a phenol-urea-formaldehyde copolymer.

[0011] However, it has been noted that under the crosslinking temperature conditions of the resin, urea-formaldehyde condensates are unstable and they decompose to give formaldehyde and urea again, the latter of which decomposes at least in part to ammonia, which is released into the environment (especially the processing environment).

[0012] Environmental protection regulations are becoming increasingly strict, forcing manufacturers of thermal and acoustic insulation products to find solutions making it possible to further reduce the levels of undesirable emissions (volatile compounds), especially formaldehyde.

[0013] To this end, various aqueous binding compositions containing compounds that are polymerizable via the Maillard reaction are known in the art (for a comprehensive reference on the Maillard reaction, see, for example, J. Am. Soc. Soc. 1999, 143: 1111-1122), such as those that further comprise sugars and proteins, or poly- or mono-carboxylic acids and an ammonia source, and various polymerization / cross-linking agents.

[0014] For example, US Pat. No. 5,399,633 discloses a bonding composition comprising at least one monosaccharide and an organic salt as a hardener / crosslinker selected from ammonium sulfamate or an alkali metal or alkaline earth metal sulfamate.

[0015] The organic resins produced by polymerization of these bonding compositions on mineral fibers are highly biocompatible and formaldehyde-free at detectable levels, but the bond strength of said organic resins does not have the same effectiveness as that guaranteed by phenolic resins. For example, the tensile strength of the final product is satisfactory, but is less than that of a similar product obtained using phenolic resins.

[0016] Patent Document 2 discloses a formaldehyde-free mineral fiber binding composition comprising the polymerization product of a carbohydrate reagent and a primary polyamine, such as 1,6-diaminohexane (HDMA), in a ratio ranging from 1:1 to 30:1. The binding composition may further comprise caprolactone as a non-aqueous moisturizing agent. A similar binding composition is also disclosed in Patent Document 3.

[0017] US Pat. No. 5,399,633 discloses a method for applying a polymeric binding composition onto mineral fibers, the binding composition comprising a prepolymer prepared by reaction between at least one reducing sugar and HDMA in an amount of 2% by weight or more, the prepolymer having a molecular weight of 1 to 500 kDa. [Prior art documents] [Patent documents]

[0018] [Patent Document 1] International Publication No. 2013 / 179323 [Patent Document 2] European Patent No. 2566904 [Patent Document 3] European Patent No. 2817374 [Patent Document 4] European Patent No. 2834256 [Non-patent literature]

[0019] [Non-Patent Document 1] GP Ellis et al.,Advances in Carbohydrate Chem,1959,pp.63-134 Summary of the Invention [Problem to be solved by the invention]

[0020] In view of the above, the main object of the present invention is to provide a novel bonding composition having improved bond strength as well as final products obtained by the use of such a novel bonding composition which does not emit formaldehyde so as to meet the most stringent regulations regarding environmental protection and to overcome the drawbacks previously mentioned with respect to the prior art.

[0021] It is another object of the present invention to provide a bonding composition as above which has a bond strength comparable to that of phenolic resin based bonding compositions.

[0022] A further object of the present invention is to provide a process for producing end products, in particular fibrous materials, starting from "free" mineral fibres with a composition as described above, which have improved mechanical strength properties. [Means for solving the problem]

[0023] These objectives are: at least one reducing sugar, at least one sulfamate and / or sulfamic acid, a pH adjuster consisting of ammonium hydroxide (NH4OH), organic and / or inorganic ammonium salts, and / or organic amines, or a combination thereof; At least one lactam This is primarily achieved by a formaldehyde-free aqueous bonding composition comprising:

[0024] The Applicant has surprisingly found that aqueous binding compositions as described above have an improved bond strength, comparable to that of aqueous binding compositions based on resole resins, and at the same time do not emit polluting emissions (in particular formaldehyde) as aqueous binding compositions that are polymerizable via the Maillard reaction, such as those disclosed in WO 2013 / 179323.

[0025] When used as binders for mineral fibres such as rock or glass fibres, the aqueous binding composition according to the invention advantageously makes it possible to obtain textile products with improved mechanical properties, in particular greater strength against static friction and / or compression, and surprisingly also makes it possible to obtain insulating textile products such as glass fibres with better thickness recovery of wound and compressed textile products, a very important property to ensure sufficient thermal strength.

[0026] The above object is therefore also achieved by a process for preparing a mineral fibre material using an aqueous binding composition as described above, said process comprising the steps of: forming free mineral fibres of a glass or rock material; applying an aqueous binding composition as described above to said loose mineral fibers to form a mineral fiber aggregate comprising said binding composition; subjecting said aggregates to a heat treatment at a temperature capable of curing said binding composition, thereby obtaining said fibrous material; Includes.

[0027] The above object is also achieved by a bonded mineral fibre-based fibre material obtainable by a process as described above.

[0028] In one embodiment, the mineral fiber material obtained according to the process of the present invention comprises: Density: 6~110kg / m 3 , Bond content is 5-20%, Separation strength of at least 170g / gf according to ASTM C685-90; At least 100% nominal thickness recovery according to EN824 for mats rolled under pressure (compression ratio > 4.5) and at least 100% thickness recovery for panels packed under pressure It is a glass wool fiber material having the following characteristics.

[0029] In another embodiment, the mineral fiber material obtained according to the process of the present invention comprises: Density: 20~250kg / m 3 , Bond content is 1-20%, Compression at least 60KPa according to EN826; 100% nominal thickness recovery for pressure packed panels It is a rock wool fiber material having the following characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] In this specification and in the claims that follow, "aqueous binding composition" refers to an aqueous solution obtained by dissolving or dispersing the components of the composition as such or at least partially pre-reacted in water to form a prepolymer (also called pre-condensate) comprising one or more reaction products obtained from at least one reducing sugar and at least one nitrogen-containing component that forms the binding composition as a latent binding agent (binder) for fibrous materials.

[0031] For the purposes of the present invention, when referring to the binding composition according to the invention or to the final product (textile material) obtained through its use, the term "formaldehyde-free" means that the binding composition and / or the final product has a formaldehyde content of 8 μg / m 2 / h, preferably less than 5 μg / m 2 / h, and even more preferably less than 3 μg / m 2 / h. Preferably, this measurement is carried out according to ISO 16000, a standard for aldehyde emission testing.

[0032] Unless otherwise specified, the percentages of ingredients in a composition according to the invention indicate the percentage by weight of said ingredient relative to the total weight of said ingredients of the composition considered in its dry state, i.e. in the absence of water (dry composition).

[0033] For purposes of this specification and the claims that follow, unless otherwise stated, all numbers expressing quantities, amounts, percentages, and the like, shall be meant as modified in each instance by the term "about." Also, all ranges include any combination of the maximum and minimum points recited, and include any intermediate ranges therein, which may or may not be specifically recited herein.

[0034] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.

[0035] The features of the embodiments of the invention described herein may be combined in any manner to form further embodiments not expressly described but which are within the scope of the invention.

[0036] The compositions of the present invention may be conveniently used in preparing fibrous materials, such as glass or rock wool, typically for use as thermal and / or acoustic insulation, which may be prepared by known techniques involving the initial formation of free glass or rock fibres, followed by impregnation of the fibres with a binding composition (binder) and subsequent thermal polymerization of the binder composition to firmly bind the mineral fibres together.

[0037] As mentioned above, the aqueous binding composition according to the present invention comprises at least one reducing sugar. Preferably, the at least one reducing sugar is present in a total amount in the range of 50% to 80% (i.e. including all reducing and non-reducing sugars present in the composition).

[0038] The term "reducing sugar" is intended in its conventional sense, i.e. it may be any monosaccharide or polysaccharide having a free hemiacetal OH group that has a reducing action, especially in copper alkaline solutions.

[0039] The monosaccharides may be trioses, pentoses and / or hexoses having both ketones and aldehydes, both L and D anomeric configurations, or mixtures thereof. Thus, examples of usable monosaccharides are glucose, fructose, galactose, xylose, arabinose, ribose, lyxose, mannose, rhamnose, etc. The monosaccharides may be used as purchased or may be obtained through known methods, for example chemical reduction of disaccharides or polysaccharides in general (e.g. sucrose, maltose, etc., among others).

[0040] In a preferred embodiment, the monosaccharides are selected from fructose and glucose (also called dextrose) and combinations thereof, preferably in a total amount ranging from 50% to 80% by weight.

[0041] In one embodiment, the composition comprises at least one or two monosaccharides, at least one of which is preferably glucose, hi another embodiment, the composition comprises at least one aldehyde monosaccharide (such as glucose) and at least one ketone monosaccharide (such as fructose).

[0042] In particular, the presence of at least glucose makes it possible to obtain improved binding properties of the composition and stability properties of the fibre material.

[0043] When present, both aldehyde (e.g. glucose) and ketone (e.g. fructose) monosaccharides may preferably be in a weight ratio of about 1:1 to each other, or one of both monosaccharides is present in slight excess, for example preferably in a ratio ranging from 1:1.05 to 1:1.2. In one embodiment, the composition comprises fructose and glucose in a ratio of 1:1.05 to 1:1.1 in a total amount ranging from 50% to 80% by weight relative to the weight of the dry composition.

[0044] The reduced polysaccharides in the binding composition according to the invention are chosen from reduced polysaccharides having a weight average molecular weight of less than 1,000,000, preferably less than 100,000, more preferably less than 50,000, advantageously less than 10,000, and better still more than 180.

[0045] Preferably, the reduced polysaccharide comprises at least one glucose unit. Polysaccharides consisting mainly (more than 50% by weight) of glucose units are particularly preferred.

[0046] The polysaccharide is treated in an acid environment prior to use.

[0047] The aqueous binding composition according to the present invention further comprises at least one sulfamate.

[0048] The term "sulfamate" is intended to include salts of sulfamic acid, especially compounds (salts) that are non-volatile and sufficiently stable for storage. Preferably, the sulfamate is selected from the group consisting of ammonium sulfamate, alkali metal or alkaline earth metal sulfamates, sodium N-cyclohexylsulfamate, and combinations thereof. The aqueous binding composition according to the present invention may further comprise sulfamic acid alone or in combination with one or more sulfamates as previously described.

[0049] In one embodiment, the sulfamate is selected from ammonium sulfamate, alkali metal or alkaline earth metal sulfamates, and combinations thereof. Preferably, the sulfamate is ammonium sulfamate.

[0050] Sulfamates act as hardening / crosslinking agents and in particular contribute to the formation of melanoidin derivatives by polymerization, generally via the Maillard reaction, with at least one reducing sugar (e.g. monosaccharide) during the preparation of fiber materials. In particular, the Maillard reaction leads to the formation of aromatic molecules or blends of aromatic and / or nitrogen-containing polymers (melanoidins) with high molecular weight, which allows the composition to have the necessary binding and thermosetting properties to effectively act as a binder for mineral fibers. In particular, the melanoidins can vary significantly in carbon / nitrogen ratio and degree of unsaturation and aromaticity depending on temperature (for general references, see Ames et al. The Maillard Browning Reaction, Chemistry and Industry, 1988, 7, 558-561).

[0051] Examples of sulfamates that can be used are selected from sodium, potassium, calcium, magnesium and ammonium sulfamates, with ammonium sulfamates (CAS N: 7773-06-0) being preferred. In particular, ammonium sulfamates have the general formula H2NSO3 - NH4 +(CHEBI:81950), but is classified as an organic (non-carboxylic) salt, which is easy to handle due to its low toxicity and lack of irritation on skin contact. It can be prepared, for example, by hydrolysis of the reaction product obtained by treating urea with oleum, or it can be purchased on the market. In the aqueous binding composition according to the invention, at least one sulfamate and / or sulfamic acid, in particular ammonium sulfamate and / or an alkali metal or alkaline earth metal sulfamate, is preferably present in a total amount ranging from 5 to 20% by weight, in particular from 5 to 12% by weight.

[0052] The bonding composition according to the present invention further comprises a pH adjuster consisting of ammonium hydroxide (NH4OH), organic and / or inorganic ammonium salts, and / or organic amines, and combinations thereof, which introduce amino groups into the final resin.

[0053] In one embodiment, the pH adjuster also serves as an ammonia source and is selected from ammonium hydroxide (NH4OH), organic or inorganic ammonium salts, and combinations thereof.

[0054] In this respect, examples of organic ammonium salts which can be used are the salts of mono- or polycarboxylic organic acids, preferably those selected from citric acid, tartaric acid, glycolic acid, malic acid, lactic acid and glutamic acid.Usable inorganic ammonium salts are preferably selected from ammonium phosphates and ammonium sulfates.

[0055] In another embodiment of the invention, the pH adjuster is selected from one or more primary, secondary or tertiary organic amines, optionally bearing further functional groups (e.g. alkanolamines), used alone or in combination with hydroxides and / or ammonium salts in partial substitution.

[0056] Preferably, the organic amine is selected from the group consisting of 2-amino-2-methyl-propanol (AMP), hexamethylenediamine (HDMA), bis(hexamethylene)triamine and triethanolamine.

[0057] The use of at least one organic amine, in particular at least one amine as described above, in the binding composition according to the invention advantageously makes it possible to further increase the cohesion of the binding composition on the fibers, as will become apparent from the experimental part further reported in this document.

[0058] In the compositions according to the invention, the pH adjusting agents, whether ammonium hydroxide, ammonium salts and / or organic amines, are present in a total amount of at least 2% by weight, preferably 2 to 20% by weight, relative to the weight of the dry composition, so as to adjust the pH of the compositions according to the invention to a value in the range from 6 to 10, for example from 6 to 9.

[0059] At this pH, a higher polymerization rate of the composition is observed during preparation of the mineral fiber material.

[0060] The binding composition according to the invention further comprises at least one lactam, i.e. a cyclic amide obtained by intramolecular condensation between a carboxyl group (-COOH) and an amino group (-NH2). In the present invention, the lactam may be selected from β-lactam, γ-lactam, δ-lactam and ε-lactam.

[0061] In a particularly preferred embodiment, the lactam is ε-caprolactam.

[0062] Preferably, the at least one lactam is present in the binding composition in an amount ranging from 1% to 15%, preferably from 6 to 10%.

[0063] Surprisingly, it has been found that lactam, especially caprolactam, by binding to one or more reducing sugars, acts synergistically with sulfamate during the curing of the binding composition for preparing fiber material, acting as a crosslinking agent for reducing sugars.This allows the binding composition according to the invention to have thermosetting properties and a binding capacity for mineral fibers that can be significantly higher than that of a similar binding composition that contains sulfamate as crosslinking agent but does not contain lactam, and that contains lactam but does not contain sulfamate.This effect is even more pronounced when the binding composition according to the invention contains an organic amine such as HDMA in addition to lactam.

[0064] The composition of the invention may also contain further components capable of further increasing the cohesion of the composition on the fibre, in particular one or more amino acids, such as glycine and glutamic acid, which may preferably be present in the composition in a total amount ranging from 1% to 25% by weight, for example from 3% to 10% by weight.

[0065] The compositions of the present invention may also include additional components used, for example, to improve resistance to temperature and / or to further enhance the polymerization process of the composition during formation of the mineral fiber material.

[0066] In particular, the possible additional components, present individually or mixed with each other, may include acrylic components as described in detail below, mineral oils, which are generally present as emulsions in amounts ranging from 2 to 6% by weight, aminosilanes, preferably in amounts ranging from 0.1% to 0.2% by weight, polysiloxanes, preferably in amounts ranging from 0.1% to 0.5% by weight, urea and lignosulfonates, such as calcium lignosulfonate or ammonium lignosulfonate. The possible additional components may be present individually or mixed with each other. In particular, in one embodiment of the present invention, the acrylic components present as the above-mentioned additional components may be selected from acrylic resins, preferably in emulsion form, having an acidic pH (generally ranging from 2 to 4), and carboxylic acid polymers mixed with polyols. In this respect, heat-resistant aqueous resins selected from Acrodur®Plus 2580 (BASF), corresponding DOW and others similar, are usable acrylic resins.

[0067] Preferred carboxylic acid polymers are derived from acrylic acid or methacrylic acid as starting materials.

[0068] The polyol is selected from, for example, polyether, polypropylene glycol, polyester, etc. Preferably, the molecular weight of the acrylic component is in the range of 500 to 10,000 Daltons, preferably 500 to 8,000 Daltons.

[0069] When present, the acrylic component can be used in an amount of up to 20% by weight, preferably up to 15% by weight, and even more preferably up to 10% by weight of the total weight of the dry composition. This addition advantageously makes it possible to increase the cohesive strength of the composition, which in turn improves the mechanical and elastic properties of the glass or rock fiber material comprising the composition, for example with regard to the elastic recovery after compression of glass fiber felts, which are commonly used as thermal and acoustic insulation materials.

[0070] Advantageously, the aqueous binding composition (binder) of the present invention is further characterized by being stable for long periods of time (even for several days) and by not showing any formation of mold, gelling or decomposition products, etc., which are often present when storing prior art aqueous binding compositions containing other polymerizers / crosslinkers.

[0071] The bonding composition of the present invention can be easily and quickly prepared without using potential formaldehyde sources through a process that uses water as a solvent and is easily applicable even on an industrial scale.

[0072] Generally, the minimum amount of water necessary to dissolve the components of the composition and / or to obtain an aqueous solution of the specified concentration is used.

[0073] In other words, the binding composition according to the invention which is useful for the preparation of fibrous mineral materials is at least one reducing sugar, at least one sulfamate and / or sulfamic acid, pH adjusters consisting of ammonium hydroxide (NH4OH), organic and / or inorganic ammonium salts, organic amines, and combinations thereof; at least one lactam, optionally one or more amino acids (e.g., glycine and lysine); Possible additional ingredients and in water in weight percentages according to each of the above embodiments.

[0074] In this respect, the binding composition (binder) according to the invention in the form of an aqueous solution may preferably have a weight concentration on application onto the fibres ranging from 5% to 15%, intended as the weight of all components relative to the total weight of the solution.

[0075] In one embodiment, the aqueous binding composition (binder) can be prepared by mixing the desired amount of each single component in water at room temperature (i.e., a temperature ranging from about 15° C. to about 40° C.), typically in a mixing tank, and then simply adding the minimum amount of water necessary to obtain the desired concentration value.

[0076] In another embodiment, the binding composition according to the invention can be prepared by mixing an aqueous solution containing at least one reducing sugar, at least one sulfamate and additional components considered as pH adjusters as previously described, with at least one lactam, a considered amino acid and, optionally, additional water as required to obtain the preferred concentration values.

[0077] In a further embodiment, the binding composition according to the invention may be pre-reacted, thereby comprising at least one prepolymer (also called pre-condensate), comprising one or more reaction products between at least one reducing sugar and at least one nitrogen-containing component forming the binding composition.

[0078] In one embodiment, the at least one polymer or pre-condensate may be obtained by mixing in water at least one reducing sugar, at least one sulfamate and a pH adjuster selected from the group consisting of ammonium hydroxide (NH4OH), organic and / or inorganic ammonium salts and / or at least one organic amine, preferably selected from those mentioned above, followed by heating the resulting aqueous solution at a temperature ranging from 50°C to 90°C, in particular from 70 to 80°C, for at least 20 minutes, preferably from 20 to 40 minutes.

[0079] In this way, an aqueous solution of prepolymers comprising one or more reaction products of the above components is obtained, to which, after cooling, at least one lactam, such as caprolactam, and optionally one or more amino acids and any additional components as described above are added to obtain the binding composition of the invention in the desired concentration. Alternatively, at least one organic amine, at least one lactam, such as caprolactam, and / or amino acids can be mixed with at least one reducing sugar, at least one sulfamate, optionally ammonium hydroxide (NH4OH), and / or organic and / or inorganic ammonium salts to form a starting aqueous solution from which, after heating as described above, a binding composition comprising at least one prepolymer as described above is obtained.

[0080] It should be noted that all components of the binding composition of the present invention are readily retrievable and commercially available, and many of them (such as reducing sugars) are of natural origin.

[0081] In a further aspect, the present invention relates to the use of the bonding composition in the preparation of glass or rock mineral fibers.

[0082] In this direction, the present invention refers to a fibrous material comprising mineral fibres, preferably glass or rock fibres, bonded together by using the aqueous binding composition (binder) of the present invention. A further subject of the present invention is therefore a mineral fibrous material obtained starting from free mineral fibres by a process comprising at least one polymerization step of said binding composition of the present invention at a temperature such that said binding composition hardens and polymerises.

[0083] In this respect, the mineral fibre material: forming free fibres, preferably by melting a glass material (such as a mixture of alkali borosilicates) or a rock material (such as a mixture of basalt, dolomite, slag and limestone); applying an aqueous binding composition, preferably as described above, to the free mineral fibers by spraying said composition onto said free fibers to form a mineral fiber aggregate comprising the binding composition of the present invention; subjecting the aggregate to a heat treatment at a temperature capable of hardening and polymerizing the bonding composition; It can be conveniently prepared by a process comprising:

[0084] The latter heat treatment is typically carried out in a polymerization oven at a temperature of at least 180° C., preferably at a temperature in the range of 180° C. to 250° C., more preferably at a temperature in the range of 180° C. to 220° C., to bring about a polymerization process of the binding composition of the invention, which is stably bonded to the fibers, thereby forming the final ready-to-use fiber material. The heat treatment can be carried out, for example, by the use of hot air circulated in the oven by a variable pressure fan for a variable time depending on the oven speed as a function of the weight per unit of surface area of ​​the final product.

[0085] If necessary, a fiber orientation step (or "crimping") is carried out before the step of heat treatment for polymerization / curing of the bonding composition, which makes it possible to orient the fibers in a vertical position, thereby increasing their strength in compression.

[0086] The step of applying the binding composition onto the loose fibers is preferably carried out by impregnation, in particular by spraying the aqueous composition of the invention onto the freshly thermoformed loose fibers, using equipment known in the art that is commonly used for the preparation of mineral fiber materials. At the end of the application step, an aggregate of mineral fibers is obtained that comprises the composition of the invention, in the form of a panel or rolled-up felt, typically with a parallelepiped cross section.

[0087] Generally, the binder content in the cured textile product is in the range of 1% to 20% by weight based on the total weight of the textile material.

[0088] Similarly, the step of forming the loose fibers (generally designated the "fiberization process") can be conveniently carried out by operations known to those skilled in the art, which involve melting the starting glass or rock material and then passing it through an extrusion die connected to a rotor with thousands of holes that, while rotating at high speed, project very thin fiber filaments (glass) outwardly, ready for contact with the binding composition according to the application process described above (internal centrifugation). In the case of rock fibers, it is fed in the form of hot lava to a wheel, also rotating at high speed, that provides the centrifugal force necessary to thin it down into fibers, also ready for contact with the aqueous binder (external centrifugation).

[0089] The final fiber material, once cut to the required size, is packaged and used as thermal and / or acoustic insulation, and may also exhibit excellent mechanical strength, heat resistance and elastic return properties, the latter being intended as the difference in the nominal thickness of the material before and after its packaging. Thus, in a further aspect, the present invention relates to a mineral fiber material obtained through a process as described above. Such fiber materials generally have a layered structure when viewed from the side, and a coloration characterized in that dark fibers, such as brownish (dark brown), black, blue or greenish, are intertwined with lighter fibers (e.g. light brown), so that fibers of different shades can be clearly distinguished. The undulations and curls of the lighter fibers can create an aesthetic effect, like clouds, against the background of the darkest fibers.

[0090] Further features and advantages of the present invention will become apparent from the following non-limiting examples. EXAMPLES

[0091] Experimental Department Example 1: Preparation of the binding composition (binder) Aqueous binder compositions (binders) A-E according to the invention and comparative aqueous binder compositions F-G were prepared using the components shown in Table 1 below, in their respective weight percentages based on the dry weight of the composition. [Table 1]

[0092] Binders A and B were prepared by mixing the components in water at room temperature and had a solids content of 34.8% and a pH of 8-8.5.

[0093] Binder C was prepared by mixing the ingredients in water at room temperature and had a solids content of 36.6% and a pH of 8.

[0094] Binder D is a pre-reacted binder prepared by mixing the ingredients in water and heating the resulting mixture at 80° C. for 35 minutes, thereby obtaining an aqueous solution containing at least one prepolymer, and optionally diluting it to a solids content of 29.06% and a pH of 7.

[0095] Binder E is a pre-reacted binder prepared by mixing the ingredients in water and heating the resulting mixture at 80° C. for 35 minutes, thereby obtaining an aqueous solution containing at least one prepolymer, and optionally diluting it to a solids content of 26.10% and a pH of 10.

[0096] Comparative binders F and G were prepared by mixing the components in water at room temperature, both having a solids content of 35% and a pH of 8.

[0097] Example 2: Preparation of fiber material The inventive binders A-E and comparative binders F-G of Example 1, as well as a commercially available resole resin (formaldehyde-phenol-urea) (DYNEA Prefere72-5235) as a reference, were used to form glass wool-based insulation products.

[0098] Glass wool was produced by the internal centrifugation technique, in which a molten glass composition is converted into fibers by a rotor called a "spinner" operating at high rotational speed, which comprises a peripheral band (or disk) provided with a number of small orifices (internal centrifugation). As a result of the centrifugal forces, the melt projects against the perforated peripheral band, from which primary filaments of molten mineral material emerge through the orifices and are then stretched by the action of hot gases from an annular burner around the disk to form thin fibers.

[0099] The bonding composition was applied to the resulting fine fibers exiting the rotor by an annular sprayer positioned below the rotor to distribute the bonding composition evenly onto the fibers and to obtain an agglomerate ("mat") of fibers impregnated with the bonding composition.

[0100] The agglomerates were collected on a belt conveyor and sent to an oven maintained at a temperature of at least 180°C, where they were left for a time sufficient to allow the composition to polymerize (cure) and bond with the fibers, thereby obtaining a substantially parallelepiped shaped fibrous material.

[0101] The fibrous materials were prepared using the process described above with the same fiberization parameters, the same content (7%) of binder composition, and substantially the same density (20 kg / m 3 ) and thickness (approximately 100 mm).

[0102] The mechanical properties of these fibrous materials are referred to as tensile strength and were measured according to ASTM Standard C685-90 "Separation Strength of Mineral Fiber Batt and Bracket Type Insulation" by measuring the breaking load (gram force "gf") and calculating the tensile strength as the "separation strength", which is the gram force per gram of sample required by the relevant ASTM standard. The samples tested have substantially the same fiber diameter, the same density and approximately the same binder content.

[0103] The results are summarized in Table 2 below. [Table 2]

[0104] From Table 2 above, it is noted that all the fiber materials obtained using the bonding compositions according to the invention (A to E) have better mechanical strength properties than the fiber materials obtained using the bonding composition containing sulfamate but not caprolactam (comparative composition F) or the bonding composition containing caprolactam but not sulfamate (comparative composition G).

[0105] The presence of an amino acid such as glycine (composition B) or glutamic acid (composition C) in addition to caprolactam in the binding composition can result in a slight increase in the mechanical strength properties of the fiber material obtained using this composition compared to the mechanical strength properties of the fiber material obtained using a similar binding composition containing caprolactam but not an amino acid or glutamic acid (e.g. composition A).

[0106] Similarly, the use of a pre-reacted bonding composition may result in a slight increase in the mechanical strength properties of the fibrous material obtained using this composition compared to the mechanical strength properties of the fibrous material obtained using a similar bonding composition that contains caprolactam but has not been pre-reacted (see, for example, composition D vs. composition A).

[0107] The fibrous material obtained using the pre-reacted bonding composition comprising caprolactam in combination with an organic amine such as HDMA (composition E) has the best mechanical strength properties of the bonding compositions according to the invention used in the above tests.

[0108] Additionally, exemplary bonding compositions according to the present invention have mechanical strength properties substantially comparable to those of reference phenolic resins, but unlike phenolic resins, do not contain or emit formaldehyde.

Claims

1. at least one reducing sugar; at least one sulfamate and / or sulfamic acid; Ammonium hydroxide (NH 4 OH), an organic and / or inorganic ammonium salt, and / or an organic amine, or a combination thereof; At least one lactam 1. A formaldehyde-free aqueous bonding composition comprising:

2. 2. The binding composition according to claim 1, wherein the at least one reducing sugar is present in a total amount ranging from 50% to 80% and is selected from monosaccharides, preferably glucose, fructose, galactose, xylose, arabinose, ribose, lyxose, mannose, rhamnose, in particular glucose and fructose, and polysaccharides having a weight average molecular weight of less than 1,000,000, preferably less than 100,000, more preferably less than 50,000, and wherein the polysaccharide is used after acid treatment.

3. 3. The bonding composition of claim 1 or 2, wherein the at least one sulfamate is selected from the group consisting of ammonium sulfamate, alkali metal or alkaline earth metal sulfamates, sodium N-cyclohexyl sulfamate, and combinations thereof.

4. 4. A bonding composition according to any one of claims 1 to 3, wherein the at least one sulfamate is present in a total amount ranging from 5 to 20% by weight, preferably from 5 to 12% by weight.

5. 5. A bonding composition according to any one of claims 1 to 4, wherein the pH adjusting agent is present in an amount of at least 2%, preferably 2% to 20%, so as to adjust the pH to a value in the range of 6 to 10, for example 6 to 9.

6. 6. The bonding composition according to claim 1, wherein the organic ammonium salt is an ammonium salt of an acid selected from citric acid, tartaric acid, glycolic acid, malic acid and lactic acid.

7. 7. The bonding composition of claim 1, wherein the organic amine is selected from the group consisting of 2-amino-2-methyl-propanol (AMP), hexamethylenediamine (HDMA), bis(hexamethylene)triamine, and triethanolamine (TEA).

8. A bonding composition according to any one of claims 1 to 7, wherein the at least one lactam is present in an amount ranging from 1% to 15%, preferably from 6 to 10%.

9. The bonding composition of any one of claims 1 to 8, wherein the at least one lactam is caprolactam.

10. 10. The binding composition according to any one of claims 1 to 9, further comprising one or more amino acids, preferably glycine, lysine and / or glutamic acid, in a total amount ranging from 1% to 25% by weight, preferably from 3% to 10% by weight.

11. 11. The binding composition of claim 1, wherein the composition is pre-reacted and comprises at least one prepolymer obtained as one or more reaction products of the at least one reducing sugar and at least one of the nitrogen-containing components described above that form the binding composition.

12. The bonding composition of any one of claims 1 to 11, further comprising one or more mineral oils, and / or one or more aminosilanes, and / or one or more siloxanes, or mixtures thereof.

13. The bonding composition of any one of claims 1 to 12, further comprising at least one acrylic component having a molecular weight in the range of 500 to 10,000.

14. Use of an aqueous binding composition according to any one of claims 1 to 13 in the preparation of a mineral fibre material.

15. 1. A process for preparing a fiber material starting from free mineral fibers, comprising: forming free mineral fibers of glass or rock material; applying an aqueous binding composition according to any one of claims 1 to 13 to said loose mineral fibres, thereby forming a mineral fibre aggregate comprising said binding composition; subjecting the aggregate to a heat treatment at a temperature capable of curing the binding composition, thereby obtaining the fibrous material; A process involving:

16. 16. The process of claim 15, wherein the heat treatment is carried out at a temperature of at least 180°C.

17. 17. A mineral fibre material obtainable by the process according to claim 15 or 16.

18. Density: 6 to 110 kg / m 3 , Bond content is 5-20%, Separation strength according to ASTM C685-90 of at least 170 g / gf; At least 100% nominal thickness recovery per EN 824 for mats rolled up under pressure (compression ratio greater than 4.5) and at least 100% thickness recovery for panels packed under pressure 18. The mineral fiber material according to claim 17, which is a glass wool fiber material having the following properties:

19. Density: 20 to 250 kg / m 3 , Bond content is 1-20%, Compression according to EN826 of at least 60 KPa; 100% nominal thickness recovery for pressure packed panels 18. The mineral fiber material according to claim 17, which is a rock wool fiber material having the following properties:

Citation Information

Patent Citations

  • Carbohydrate-based binder system and method for producing the same

    JP2014525488A

  • Binder composition, molded body, method for producing molded body and cured product of binder

    JP2020196866A

  • Ceiling board and tile with reduced discoloration

    US20200095712A1

  • Formaldehyde free binding composition, for mineral fibres

    WO2013179323A1

  • Carbohydrate polyamine binders and materials made therewith

    EP2566904A1