Polyimide powder and its manufacturing method

The described method addresses the challenges of high precipitation temperatures and uneven particle sizes in polyimide production by using a solvent-catalyst combination to achieve high intrinsic viscosity and uniform particle sizes, enhancing processability and reducing defects in polyimide powder formation.

JP2024536174AActive Publication Date: 2024-10-04PI ADVANCED MATERIALS CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024519395
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-02
Filing Date
2022-09-30
Publication Date
2024-10-04
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

Existing methods for producing polyimide materials face challenges such as high polyimide precipitation temperatures, uneven particle sizes, low intrinsic viscosity, and reduced processability due to complex two-step processes and high imidization temperatures, making it difficult to achieve high molecular weight and uniform particle formation.

Method used

A method involving the reaction of dianhydride and diamine monomers with a solvent and a catalyst to produce polyimide powder, utilizing a polymerization and imidization process that includes specific solvent combinations and controlled heating to achieve lower precipitation temperatures and uniform particle sizes, enhancing intrinsic viscosity and processability.

Benefits of technology

The method results in polyimide powder with high intrinsic viscosity, uniform particle size, and improved processability, facilitating easier molding and reducing defects, while maintaining excellent mechanical and electrical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536174000001
    Figure 2024536174000001
  • Figure 2024536174000002
    Figure 2024536174000002
  • Figure 2024536174000003
    Figure 2024536174000003
Patent Text Reader

Abstract

The present invention relates to a polyimide powder and a method for producing the same. The polyimide powder and method for producing the same according to the present invention can simplify the production process to increase process efficiency, produce polyimide in powder form to facilitate molding, have a low precipitation temperature, a high intrinsic viscosity to facilitate processing, and have uniform particle size to provide excellent processability.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyimide powder and a method for producing the same. [Background technology]

[0002] Generally, polyimide (PI) is a polymer of imide monomer formed by solution polymerization of dianhydride and diamine or diisocyanate, and has excellent mechanical properties such as strength, chemical resistance, weather resistance, and heat resistance due to the chemical stability of the imide ring. In addition, polyimide is in the spotlight as a highly functional polymer material that can be applied to a wide range of industrial fields such as electronics, communications, and optics due to its excellent electrical properties such as insulation properties and low dielectric constant.

[0003] However, due to polyimide's high heat and chemical resistance, it is difficult to manufacture molded products using the thermal melting method used for general polymer resins. Therefore, polyamic acid, which is a precursor, is generally synthesized by reacting dianhydride and diamine in a solvent, and then it is dispersed or coated according to the application and then imidized. However, this general method is complicated because it involves two reaction steps: the polyamic acid production step and the imidization step of polyamic acid, and the imidization step requires high temperatures of over 300℃, making it difficult to obtain high molecular weight polyimide.

[0004] To solve this problem, a synthesis method is known in which a precursor polyamic acid is reacted in the presence of a solvent and then heated to precipitate polyimide powder. However, this method has problems in that the precipitation temperature of the polyimide powder is still high, and the polyimide powder produced by this method has low intrinsic viscosity and non-uniform particle size, which frequently causes defects during molding and reduces processability. Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to solve the problems and technical issues of the prior art as described above. The present invention provides a polyimide powder and a method for producing the polyimide powder, which is easily molded by producing a polyimide in a powder form, has a low precipitation temperature, a high intrinsic viscosity, is easily processed, and has a uniform particle size and excellent processability. [Means for solving the problem]

[0006] The present invention relates to a polyimide powder and a method for producing the polyimide powder, which comprises reacting a dianhydride monomer component, a diamine monomer component and a catalyst in a solvent, and then heating the resulting mixture to precipitate the polyimide powder.

[0007] Specifically, the method for producing polyimide powder according to the present invention includes a polymerization step of dissolving a dianhydride monomer component and a diamine monomer component in a solvent to proceed with a reaction, and an imidization step of adding a catalyst to the reaction solution produced in the polymerization step to imidize the solution and precipitate a polyimide powder.

[0008] The dianhydride monomer is not particularly limited as long as it can react with the diamine monomer to form a polyimide. For example, the dianhydride monomer according to the present invention may include at least one selected from the group consisting of pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), 4,4-(hexafluoroisopropylidene)diphthalic anhydride (6-FDA) and p-phenylenebis(trimellitate anhydride) (TAHQ).

[0009] The dianhydride monomer may be, for example, pyromelitic dianhydride (PMDA), oxydiphthalic dianhydride (ODPA), or a mixture thereof. In this case, the molar ratio of pyromelitic dianhydride (PMDA) and oxydiphthalic dianhydride (ODPA) in the dianhydride monomer may be 9:1 to 1:9, for example, the molar ratio of pyromelitic dianhydride (PMDA) and oxydiphthalic dianhydride (ODPA) may be 9:1 to 7:3. The dianhydride monomer may be selectively used as appropriate components in terms of heat resistance and flexibility. In addition, when a part of pyromelitic dianhydride (PMDA) consisting of a rigid aromatic ring is mixed with a dianhydride monomer containing a hetero element, such as oxydiphthalic dianhydride (ODPA), the precipitation temperature of the polyimide powder can be lowered and the color can be brightened.

[0010] The diamine monomer is not particularly limited as long as it can react with the dianhydride monomer to form a polyamic acid. For example, the diamine monomer according to the present invention may include at least one selected from the group consisting of 1,4-diaminobenzene (PPD), 1,3-diaminobenzene (MPD), 2,4-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminodiphenyl ether (ODA), 4,4'-methylenediamine (MDA), 4,4-diaminobenzanilide (4,4-DABA), N,N-bis(4-aminophenyl)benzene-1,4-dicarboxamide (BPTPA), 2,2-dimethylbenzidine (M-TOLIDINE), 2,2-bis(trifluoromethyl)benzidine (TFDB), 1,4-bisaminophenoxybenzene (TPE-Q), bisaminophenoxybenzene (TPE-R), 2,2-bisaminophenoxyphenylpropane (BAPP), and 2,2-bisaminophenoxyphenylhexafluoropropane (HFBAPP).

[0011] The diamine monomer may include a heteroatom in the monomer to decentralize the aromatic electron distribution, thereby improving brightness. For example, the diamine monomer may be 4,4'-diaminodiphenyl ether (ODA).

[0012] The catalyst is a tertiary amine. In general, in a method for producing polyimide via polyamic acid, an amine is used to imidize the polyamic acid, and specifically, the amine catalyst can promote a dehydration reaction to produce a polyimide through a ring-closing reaction of the polyamic acid. However, a method using a tertiary amine in a process for producing a polyimide powder has not been reported, but the present inventors have found that the deposition temperature of the polyimide powder can be lowered by using a tertiary amine in a method for producing a polyimide powder. In addition, the polyimide powder produced using the catalyst has a high intrinsic viscosity, which makes it easy to process during molding, significantly reduces the occurrence of cracks, and improves the yield.

[0013] Specifically, the catalyst may be pyridine, β-picoline, 1,4-diazabicyclo[2.2.2]octane (DABCO), triethylamine (TEA), isoquinoline, or a mixture thereof. In particular, when the tertiary amine contains an unshared electron pair, it is more effective in lowering the deposition temperature of the polyimide powder and increasing the intrinsic viscosity. For example, the catalyst may be pyridine, β-picoline, or isoquinoline.

[0014] The catalyst may be included in an amount of 0.1 to 500 parts by mole based on 100 parts by mole of the diamine monomer component. For example, the catalyst may be 0.1 parts by mole or more, 0.5 parts by mole or more, 1 part by mole or more, 5 parts by mole or more, 10 parts by mole or more, 50 parts by mole or more, or 100 parts by mole or more relative to the diamine monomer, and the upper limit is not particularly limited, but may be 400 parts by mole or less, 300 parts by mole or less, or 200 parts by mole or less. If the amount of the catalyst is less than the above range, the effect of lowering the deposition temperature of the polyimide powder and the effect of increasing the intrinsic viscosity cannot be expected, and if it exceeds the above range, the rate of change of the effects due to the catalyst is small, leading to an increase in costs. If the above range is satisfied, the intrinsic viscosity can be increased and the polyimide deposition temperature can be decreased without deteriorating the physical properties of the polyimide powder.

[0015] The solvent may be benzene, toluene, xylene, acetone, hexane, heptane, chlorobenzene, methanol, ethanol, n-propanol, isopropanol, N-methyl-2-pyrrolidone (NMP), N,N-dimethylacetamide, N,N-diethylacetamide, N,N-dimethylformamide, N,N-diethylformamide, N-methylcaprolactam, hexamethylphosphoramide, tetramethylene sulfone, dimethylsulfoxide, o-cresol, m-chloride, ethylhexylbenzene ... Resole, p-cresol, phenol, p-chlorophenol, 2-chloro-4-hydroxytoluene, diglyme, triglyme, tetraglyme, dioxane, γ-butyrolactone, dioxolane, cyclohexanone, cyclopentanone, dichloromethane, chloroform, 1,2-dichloroethane, 1,1,2-trichloroethane, dibromomethane, tribromomethane, 1,2-dibromoethane, 1,1,2-tribromoethane, and the like may be used alone or in combination.

[0016] From the viewpoints of compatibility with the catalyst and lowering the polyimide deposition temperature, the solvent is preferably a solvent containing at least one nitrogen element. For example, the solvent suitable for the present invention may be N-methyl-2-pyrrolidone (NMP), xylene, or m-cresol, which may be used alone or in combination.

[0017] The solvent according to the present invention may also be a composite solvent including a first solvent containing at least one nitrogen element and a second solvent having at least one hydroxyl group (-OH), for example, the first solvent may be N-methyl-2-pyrrolidone (NMP) and the second solvent may be m-cresol.

[0018] At this time, the weight ratio of the first solvent to the second solvent is 5:5 to 9:1, and may be, for example, 6:4 to 9:1, 7:3 to 9:1, 7:3 to 8:2, 3:7 to 10:0, 4:6 to 9:1, or 5:5 to 8:2. If the weight ratio of the first solvent is higher than the above range, the precipitation temperature of the polyimide powder becomes high, and if it is lower than the above range, polymerization similar to suspension polymerization occurs, making it difficult to obtain the powder and the brightness of the produced powder may become dark.

[0019] By including the composite solvent as described above, the present invention can dissolve the dianhydride monomer and the diamine monomer uniformly, and the precipitated polyimide powder can form uniform particles with less aggregation.

[0020] In addition, in the composite solvent according to the present invention, the difference between the boiling points of the first solvent and the second solvent may be 10°C or less, for example, the difference between the boiling points of the first solvent and the second solvent may be 5°C or less, 4°C or less, 3°C or less, 2°C or less, or 1°C or less.

[0021] By minimizing the difference in boiling point between the mixed solvents as described above, the precipitation temperature of the polyimide powder can be lowered when the polymer is heated, and the intrinsic viscosity of the produced polyimide powder can be increased.

[0022] The polymerization step may be performed by dispersing or dissolving the dianhydride monomer component together with the diamine monomer component in a solvent, or by preparing a solution in which the dianhydride monomer component is dispersed in a solvent and a solution in which the diamine monomer component is dispersed in a solvent, respectively, and then adding a catalyst to the polymer obtained by mixing the two. Also, one of the dianhydride monomer component and the diamine monomer component may be first dissolved in a solvent, and then the remaining component may be dissolved in the solution.

[0023] In one embodiment, the polymerizing step may include heating a solvent, dissolving a diamine monomer component in the heated solvent, and reacting a dianhydride monomer component with the diamine-dissolved solution.

[0024] The step of heating the solvent may be performed at a temperature of 50 to 100° C., for example, the temperature may be 60 to 90° C. or 60 to 80° C. The step of dissolving the diamine monomer component in the heated solvent may be performed at a temperature of 50 to 100° C. for 1 to 60 minutes. In this case, the temperature may be, for example, 60 to 90° C. or 60 to 80° C., and the time may be 1 to 30 minutes.

[0025] The step of reacting the dianhydride monomer component with the solution in which the diamine is dissolved may be carried out for 1 to 6 hours at a temperature of 50 to 100° C. In this case, in the step of reacting the dianhydride monomer component with the solvent in which the diamine is dissolved, the dianhydride monomer component may be added at a rate of 0.01 mol / s to 10 mol / s, for example, 0.05 mol / s to 10 mol / s, 0.1 mol / s to 10 mol / s, 1 mol / s to 10 mol / s, 1 mol / s to 5 mol / s, or 1 mol / s to 3 mol / s.

[0026] By preparing the polymer in the above manner, the side reaction can be suppressed to increase the product yield, and the content of residual dianhydride or diamine can be reduced to brighten the color of the polyimide powder.

[0027] In addition, by adding the dianhydride at the above rate, the side reaction can be suppressed to increase the product yield, and the content of the residual dianhydride or diamine can be reduced to brighten the color of the polyimide powder.

[0028] In the polymerization step, the content of the dianhydride monomer and the diamine monomer is 1 to 30 wt% based on the total weight of the entire solution, and for example, the content of the dianhydride monomer and the diamine monomer in the solution may be 1 to 20 wt%, 1 to 15 wt%, 3 to 15 wt%, 5 to 15 wt%, or 5 to 10 wt% based on the total weight of the entire solution. If the solid content exceeds the above range, stirring may be difficult, and the yield may decrease or the quality may decrease, and if the solid content is lower than the above range, the manufacturing cost may increase.

[0029] The polymerization step is a step of polymerizing the dianhydride monomer and the diamine monomer by heating. The heating temperature in the polymerization step is 30 to 100°C, and may be, for example, 40 to 100°C, 50 to 90°C, or 60 to 80°C.

[0030] If the heating temperature is lower than the above range, the reaction proceeds too slowly, resulting in a reduced yield of polyimide powder, whereas if the heating temperature is higher than the above range, the particle size may increase.

[0031] In the polymerization step, the reaction time may be 1 to 10 hours, for example, 1 to 8 hours, 1 to 6 hours, 1 to 4 hours, or 1 to 3 hours.

[0032] If the reaction time is shorter than the above range, the reaction yield may decrease and the mechanical properties such as elongation and tensile strength of the powder may decrease, whereas if the reaction time is longer than the above range, the color of the powder may become dark and the particle size may increase.

[0033] The imidization step is a step of imidizing the polymerized polymer by heating and pressurizing. The heating temperature in the imidization step is 150 to 300°C, and may be, for example, 160 to 200°C, 170 to 200°C, or 180 to 200°C.

[0034] If the heating temperature is lower than the above range, the reaction proceeds too slowly, resulting in a reduced yield of polyimide powder, whereas if the heating temperature is higher than the above range, the particle size may increase.

[0035] The reaction time in the imidization step may be 1 to 10 hours, for example, 1 to 8 hours, 1 to 6 hours, 1 to 4 hours, or 1 to 3 hours.

[0036] If the reaction time is shorter than the above range, the reaction yield may decrease and mechanical properties such as elongation and tensile strength may decrease, whereas if the reaction time is longer than the above range, the color of the powder may become dark and the particle size may increase.

[0037] The present invention can precipitate polyimide powder through the imidization step. In this case, the polyimide powder may be precipitated at a precipitation temperature of 100 to 200°C. For example, the lower limit of the precipitation temperature may be 105°C or more, 110°C or more, 115°C or more, 120°C or more, 125°C or more, or 130°C or more, and the upper limit of the precipitation temperature may be 195°C or less, 190°C or less, 185°C or less, 180°C or less, 175°C or less, 170°C or less, 165°C or less, 160°C or less, 155°C or less, 150°C or less, 145°C or less, 140°C or less, or 135°C or less. The precipitation temperature is affected by the composition of dianhydride monomer and diamine, the type and content of catalyst, and solvent.

[0038] The method for preparing a polyimide powder according to the present invention may further include a filtering and drying step after the imidization step. The filtering and drying method is not particularly limited, and the drying method may be, for example, vacuum drying or drying in a high-temperature oven. Specifically, the drying step may be drying in an oven at 100° C. or higher for 24 hours or more.

[0039] The present invention also provides a polyimide powder produced by the method for producing a polyimide powder.

[0040] The polyimide powder, which is produced by the above-mentioned production method, has advantages of high intrinsic viscosity, ease of processing, uniform particle size, and excellent processability.

[0041] For example, the polyimide powder may have an intrinsic viscosity of 0.9 dl / g or more, 0.95 dl / g or more, 1.0 dl / g or more, 1.05 dl / g or more, 1.1 dl / g or more, 1.15 dl / g or more, 1.2 dl / g or more, 1.25 dl / g or more, 1.3 dl / g or more, 1.35 dl / g or more, 1.4 dl / g or more, 1.45 dl / g or more, 1.5 dl / g or more, 1.55 dl / g or more, 1.6 dl / g or more, 1.65 dl / g or more, 1.7 dl / g or more, or 1.75 dl / g or more. The intrinsic viscosity may be measured by placing 50 mg of the polyimide powder in a vial and dissolving it in 10 g of concentrated sulfuric acid at 30° C. using an Ubbelohde viscometer.

[0042] The polyimide powder according to the present invention is 50 For example, the polyimide powder according to the present invention may have a diameter of 150 μm or less. 50 The upper limit of D may be 120 μm or less, 110 μm or less, 105 μm or less, 100 μm or less, 95 μm or less, 90 μm or less, 80 μm or less, or 60 μm or less, 50 The lower limit may be 10 μm or more, 20 μm or more, 25 μm or more, or 30 μm or more.

[0043] The polyimide powder according to the present invention is 99.9For example, the polyimide powder according to the present invention may have a diameter of 500 μm or less. 99.9 The upper limit of may be 300 μm or less, 250 μm or less, 210 μm or less, or 200 μm or less, and D 99.9 The lower limit may be 10 μm or more, 50 μm or more, or 100 μm or more.

[0044] Here, "D n " means the size of the particle when the cumulative percentage of the particle size distribution reaches n volume %. 99.9 " means the size of particles when the cumulative percentage of the particle size distribution reaches 99.9 volume %, and the above "D 50 " means the size of particles when the cumulative percentage of the particle size distribution reaches 50 volume %. The particle size distribution means a particle size distribution graph of the polyimide powder analyzed using a laser particle size analyzer, and specifically, the particle size distribution may be measured using a laser diffraction light scattering type particle size distribution analyzer (e.g., Malvern Mastersizer 3000).

[0045] D 50 When and D satisfy the above ranges, appropriate molding conditions can be easily set when molding the polyimide powder, and cracks and breaks during molding can be effectively prevented, resulting in excellent processability.

[0046] The polyimide powder according to the present invention is also 99.9 / D 50 For example, the polyimide powder according to the present invention may have a D 99.9 / D 50 The upper limit of may be 14 or less, 13 or less, 12 or less, or 11 or less, and D 99.9 / D 50 The lower limit may be 5 or more, 7 or more, or 10 or more.

[0047] As described above, the polyimide powder according to the present invention can provide a uniform powder with small variation in particle size, thereby reducing the defective rate during powder molding and increasing the yield.

[0048] The present invention also provides a molded article containing the polyimide powder. The polyimide powder produced by the present invention may be manufactured into a molded article by various molding methods, for example, compression molding, injection molding, slush molding, blow molding, extrusion molding or spinning methods may be used to manufacture the required molded article. The molded article may be a plate, a rod, a film, a sheet, a pellet, a belt or a tube.

[0049] The polyimide powder produced by the present invention may be used in various fields such as electrical / electronic, semiconductor, display, automotive, medical, battery and aerospace. Effect of the Invention

[0050] The polyimide powder and the method for producing the same according to the present invention can simplify the production process to increase the process efficiency, produce polyimide in powder form to facilitate molding, have a low precipitation temperature, a high intrinsic viscosity to facilitate processing, and have uniform particle size to provide excellent processability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0051] The present invention will be described in more detail below with reference to examples according to the present invention and comparative examples not according to the present invention, but the scope of the present invention is not limited to the following examples.

[0052] <Preparation of polyamic acid solution> Example 1 A 1000ml reactor equipped with a stirrer and nitrogen inlet and outlet pipe was equipped with a Dean-Stark trap, and a solvent made by mixing N-methyl-2-pyrrolidone (NMP) and m-cresol in a weight ratio of 5:5 was heated to 70°C while injecting nitrogen, and 4,4'-diaminodiphenyl ether (ODA) was completely dissolved in the heated solvent. Then, pyromellitic dianhydride (PMDA) was completely dissolved in the solvent and reacted at 75°C for 2 hours. Pyridine (PR) was added as a catalyst to the reaction solution in an amount of 200 mol parts per 100 mol parts of ODA, and the mixture was heated to 200°C while stirring, and further heated for 2 hours to precipitate polyimide powder.

[0053] For reference, the boiling point of N-methyl-2-pyrrolidone (NMP) is 202°C, and the boiling point of m-cresol is 202.2°C.

[0054] Examples 2 to 14 Polyimide powder was prepared in the same manner as in Example 1, except that the monomer components, solvent and catalyst were adjusted as shown in Table 1 below.

[0055] Comparative Examples 1 to 3 Polyimide powder was prepared in the same manner as in Example 1, except that the monomer components, solvent and catalyst were adjusted as shown in Table 1 below.

[0056] [Table 1]

[0057] Experimental Example The physical properties of the prepared polymerization product and polyimide powder were measured by the following methods, and the results are shown in Table 2 below.

[0058] Experimental Example 1 - Intrinsic Viscosity The viscosity was measured using an Ubbelohde viscometer at 30° C. Specifically, 50 mg of polyimide powder was placed in a vial and dissolved in 10 g of concentrated sulfuric acid, after which the viscosity was measured using the Ubbelohde viscometer.

[0059] Experimental Example 2 - Deposition Temperature After the polymerization reaction, the temperature at which the transparent solution became blurred due to imidization was measured.

[0060] Experimental Example 3 - Particle size distribution of polyimide powder The particle size distribution (D 50 ) was measured using a laser diffraction light scattering particle size distribution analyzer (Malvern Mastersizer 3000).

[0061] [Table 2]

Claims

1. a polymerization step of reacting the dianhydride monomer component and the diamine monomer component in a solvent; The method for producing polyimide powder includes an imidization step of adding a catalyst to a reaction solution produced in a polymerization step to imidize the reaction solution and precipitate a polyimide powder.

2. 2. The method for producing a polyimide powder according to claim 1, wherein the catalyst is a tertiary amine.

3. 2. The method for producing a polyimide powder according to claim 1, wherein the catalyst is contained in an amount of 0.1 to 500 parts by mole based on 100 parts by mole of the diamine monomer component.

4. The polymerization stage is heating the solvent; dissolving a diamine monomer component in a heated solvent; and reacting a dianhydride monomer component with the solution in which the diamine is dissolved.

5. The method of claim 4, wherein the step of heating the solvent is performed at a temperature of 50 to 100°C.

6. 5. The method of claim 4, wherein the step of dissolving the diamine monomer component in the heated solvent is carried out at a temperature of 50 to 100° C. for 1 to 60 minutes.

7. 5. The method of claim 4, wherein the step of reacting the dianhydride monomer component with the diamine-dissolved solvent is carried out at a temperature of 50 to 100° C. for 1 to 6 hours.

8. 5. The method of claim 4, wherein the step of reacting the dianhydride monomer component with the solvent in which the diamine is dissolved comprises adding the dianhydride monomer component at a rate of 0.01 mol / s to 10 mol / s.

9. The solvent is a composite solvent including a first solvent having at least one nitrogen element and a second solvent having at least one hydroxyl group (—OH); 2. The method for producing a polyimide powder according to claim 1, wherein the difference in boiling point between the first solvent and the second solvent is 10° C. or less.

10. 2. The method for preparing a polyimide powder according to claim 1, wherein the imidization step is carried out at a temperature of 150 to 300° C. for 1 to 10 hours.

11. 2. The method for producing a polyimide powder according to claim 1, wherein the dianhydride monomer comprises at least one selected from the group consisting of pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), 4,4-(hexafluoroisopropylidene)diphthalic anhydride (6-FDA) and p-phenylenebis(trimellitate anhydride) (TAHQ).

12. The diamine monomers are 1,4-diaminobenzene (PPD), 1,3-diaminobenzene (MPD), 2,4-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminodiphenyl ether (ODA), 4,4'-methylenediamine (MDA), 4,4-diaminobenzanilide (4,4-DABA), N,N-bis(4-aminophenyl)benzene-1,4-dicarboxamide (BPTPA), 2,2-dimethylbenzidine (M 2. The method for producing a polyimide powder according to claim 1, wherein the polyimide powder comprises at least one selected from the group consisting of 1,4-bis(aminophenoxyphenyl)propane (TPE-Q), 2,2-bis(trifluoromethyl)benzidine (TFDB), 1,4-bisaminophenoxybenzene (TPE-R), 2,2-bisaminophenoxyphenylpropane (BAPP), and 2,2-bisaminophenoxyphenylhexafluoropropane (HFBAPP).

13. A polyimide powder produced by the method for producing a polyimide powder according to claim 1.

14. 14. The polyimide molded article according to claim 13, wherein the polyimide powder has an intrinsic viscosity of 0.9 dl / g or more.

15. Polyimide powder D 50 The polyimide powder according to claim 13, wherein the average particle diameter is 150 μm or less.

16. A polyimide molded article comprising the polyimide powder according to claim 13.

Citation Information

Patent Citations

  • Thermoplastic polyimide adhesive film as well as preparation method and application thereof

    CN102199290A

  • Gas separating material

    JP1982015819A

  • Production of polyimide powder

    JP1991050234A

  • Manufacture of imido-oligomer molded product

    JP1991292130A

  • Production of polyimide resin powder

    JP1992142332A