Complex Wear Parts

A hierarchical composite wear part with a three-dimensional network of ceramic-metal granules and in-situ formed carbide particles addresses the challenge of high TiC concentration, enhancing wear resistance and ductility by minimizing porosity and cracking, resulting in improved mechanical properties.

JP2024536825APending Publication Date: 2024-10-08MAGOTTEAUX INTERNATIONAL SA
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024518474
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-23
Filing Date
2022-09-01
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing composite wear parts struggle to achieve a high concentration of titanium carbide (TiC) while maintaining a balance between wear resistance and ductility, often leading to porosity, cracking, and uncontrolled exothermic reactions during the casting process.

Method used

A hierarchical composite wear part is created with a three-dimensional network of millimeter-level ceramic-metal composite granules and millimeter-level gaps, filled with a cast metal matrix, containing micrometer-level carbide particles formed in situ through carbide-forming metal powders and a carbon source, ensuring a high concentration of TiC without excessive porosity or cracking.

Benefits of technology

The solution results in wear parts with enhanced resistance to abrasion and impact, maintaining structural integrity and mechanical properties by achieving up to 62% volume concentration of TiC, reducing defects, and improving wear performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536825000001_ABST
    Figure 2024536825000001_ABST
Patent Text Reader

Abstract

The present invention relates to a hierarchical composite wear part comprising a reinforced portion and a non-reinforced portion, the reinforced portion comprising a three-dimensionally interconnected network of millimeter-scale ceramic-metal composite particulates periodically arranged with millimeter-scale gaps, the ceramic-metal composite particulates containing at least 52 volume %, preferably at least 61 volume %, more preferably at least 70 volume % of micrometer-scale titanium carbide particles embedded in a first metal matrix, the ceramic-metal composite particulates having a porosity of less than 5 volume %, preferably less than 3 volume %, most preferably less than 2 volume %, and the volume fraction of porosity of the particulates embedded in the first metal matrix is ​​in accordance with ISO 14021. % and preferably at least 3 vol. % of micrometer-level carbide particles selected from the group consisting of tungsten carbide, vanadium carbide, molybdenum carbide, titanium carbide, niobium carbide, hafnium carbide and zirconium carbide or mixtures thereof, and the volume percentage of additional carbides in the second metal matrix is ​​measured according to ISO 13383-2:2012.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hierarchical composite wear part obtained by casting technology with improved resistance to combined abrasive forces / impact stresses, said wear part having a three-dimensional network of strongly coherent millimeter-level ceramic-metal composite grains with millimeter-level interstices, TiC-based micrometer-level particles embedded in a binder, called "first metal matrix", said millimeter-level interstices being filled during the casting process of the wear part by a casting metal, called "second metal matrix" in the present invention, which further contains micrometer-level carbide particles formed in situ via carbide-forming metal powders combined with a carbon source coming from either an organic binder or the casting metal itself. [Background technology]

[0002] The present invention relates to wear parts used in the crushing and grinding industry, such as cement plants, quarries and mines. These parts are often exposed to high mechanical stresses in the bulk and high wear due to abrasion at the working surface. It is therefore desirable that these parts should exhibit high wear resistance and some ductility to withstand mechanical stresses such as impacts.

[0003] Because it is difficult to combine these two properties in the same material composition, composite parts have been proposed in the past that have a core made from a relatively ductile alloy with an embedded ceramic insert that has good wear resistance.

[0004] Document US Patent No. 4,119,459 (Sandvik, 1977) discloses a composite wear body consisting of crushed granules of cast iron and sintered cemented carbide. The cemented carbide in the binder metal is of the WC-Co-type with possible additions of carbides of Ti, Ta, Nb or other metals. No indication is given regarding a possible volume percentage of TiC in the granules or in the reinforcing part of the composite wear body.

[0005] The document US Patent No. 4,626,464 (Krupp, 1984) discloses a beater for mounting on a hammer, comprising a metal alloy base material and a wear-resistant zone containing hard metal particles in addition to a ferroalloy, the diameter of said hard metal particles being between 0.1 and 20 mm, the percentage of hard metal particles in the wear-resistant zone being between 25 and 95 volume percent, said hard particles being firmly embedded in said metal alloy base material. A possible average volume concentration of TiC in the reinforcement is not disclosed in this document.

[0006] US Patent No. 5,066,546 (Kennametal, 1989) discloses a hierarchical wear body comprising at least one layer of a series of carbide materials, where titanium carbide is embedded in a cast steel matrix. The grain size of the carbide material is between 4.7 and 9.5 mm, and the carbide material is present in the form of crushed pieces, powder or compacts having irregular shapes. The document does not disclose the average concentration of TiC in the reinforced portion of the wear body, nor the configuration of the reinforcement structure.

[0007] The document US Patent No. 8,999,518 (Magotteaux) discloses a hierarchical composite material comprising an iron-based alloy reinforced with titanium carbide according to a defined geometric form, said reinforcement comprising a macro-micro alternating structure of millimeter-level regions of titanium carbide globular particles, separated by millimeter-level regions substantially free of titanium carbide globular particles, said regions being filled with an iron-based alloy. In this patent, the maximum concentration of TiC is 72.2 vol.% when a powder blend of Ti and C is molded at its maximum relative density of 95%. The porosity of the grains is more than 5 vol.% and, in the absence of any possible reaction moderator, there is only one metal matrix, the cast metal. The hierarchical composite material is obtained by self-propagating high-temperature synthesis (SHS), where the reaction temperature is usually above 1,500°C or even reaches 2,000°C. Only a small amount of energy is required to initiate the reaction locally. The reaction then spontaneously propagates throughout the mixture of reagents. Example 4 of this document will be used herein as a comparative example for the present invention.

[0008] The hierarchical composites of this document are obtained by reaction in a mold of granules containing a mixture of carbon and titanium powders. After initiation of the reaction, the reaction front advances and propagates spontaneously (self-propagating) allowing titanium carbide to be obtained from titanium and carbon. The titanium carbide thus obtained is said to be "obtained in situ" since it is not provided by the cast iron-based alloy (the Ti+C→TiC SHS reaction is highly exothermic with a theoretical adiabatic temperature of 3290 K). The reaction is initiated by the casting heat of the cast iron or steel used to cast the entire part.

[0009] Unfortunately, the temperature rise of most of the carbon and titanium causes the degassing of the reactants, i.e. the volatiles contained therein (H2O in carbon, H2, N2 in titanium). All impurities contained in the reactant powder, organic or inorganic components around or inside the powder / formed grains are volatilized. To weaken the strength of the reaction between carbon and titanium, iron-based alloy powder is added to it as a moderator to absorb the heat and reduce the temperature. Nevertheless, this also reduces the maximum TiC concentration that can be obtained in the final wear parts, and the theoretical concentration of 72.2% mentioned above is practically unreachable on a production scale.

[0010] Document WO 2010 / 031663 relates to a composite impact member for impact crushers, said impact member comprising an iron alloy at least partially reinforced with titanium carbide in a defined shape according to a method similar to that previously described in document US Pat. No. 8,999,518. To weaken the strength of the reaction between carbon and titanium, an iron-based alloy powder is added. In the examples of this document, the reinforced zone comprises a global volume percentage of TiC that is about 30%. To achieve this goal, a strip is obtained by molding with a relative density of 85%. After crushing of the strip, the granules obtained are sieved to dimensions between 1 and 5 mm, preferably between 1.5 and 4 mm. 2 g / cm 3 A bulk density in the range of 45% intergranular space + 15% porosity in the granules is obtained. The granules in the reinforced wear section thus contain 55% by volume of porous granules. In such cases, especially with grains having high porosity before the SHS reaction, the concentration of TiC in the reinforced area is only 30%, which is not always sufficient and may have a detrimental effect on the wear performance of the casting.

[0011] The document US Patent Application No. 2018 / 0369905 discloses a method to provide more precise control of the SHS process during the casting process by using a moderator. The casting insert is made from a powder mixture containing TiC forming reactants and a moderator having the composition of a cast high manganese steel containing 21% Mn. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] U.S. Patent No. 4,119,459 [Patent Document 2] U.S. Patent No. 4,626,464 [Patent Document 3] U.S. Patent No. 5,066,546 [Patent Document 4] U.S. Patent No. 8,999,518 [Patent Document 5] International Patent Application No. 2010 / 031663 [Patent Document 6] U.S. Patent Application No. 2018 / 0369905 Summary of the Invention [Problem to be solved by the invention]

[0013] The present invention provides a hierarchical composite wear part manufactured by a conventional casting process that includes a metal matrix of cast iron or steel, and integrates a reinforcing structure with a high concentration of micrometer-level titanium carbide particles embedded in a metal binder, referred to herein as a first metal matrix, and forms a low porosity ceramic-metal composite particulate. The first metal matrix containing micrometer-level titanium carbide particles in the reinforcing portion is different from the metal matrix present in other portions of the composite wear part. The reinforcing structure also includes millimeter-level interstices periodically alternating with the ceramic-metal composite particulate, the millimeter-level interstices including micrometer-level carbide particles formed in situ during the casting operation and embedded in a second metal matrix.

[0014] The objective of the present invention is to increase the carbide concentration even in the interstices filled by the second metal matrix (cast metal).

[0015] Another object of the present invention is to provide a safe manufacturing process for reinforced composite wear parts that provides improved composite wear parts with good resistance to impact and corrosion while avoiding outgassing.

[0016] In the present invention, the expression "interstitial spaces" should be understood as spaces separating at least two strongly agglomerated millimeter-level ceramic-metal composite grains. During the casting process, the interstitial spaces are filled with a casting metal that is substantially free of ceramic-metal composite particles, but contains at least 3% of dispersed carbide particles formed in situ through the presence of carbide-forming metals present around the millimeter-level ceramic-metal composite grains. The strongly agglomerated millimeter-level ceramic-metal composite grains forming a three-dimensional interconnected network are covered or coated with a powder of a carbide-forming metal that easily bonds with an organic adhesive used to weakly agglomerate the grains. In an alternative process, the weak agglomerates of millimeter-level ceramic-metal composite grains are immersed in a solution or dispersion of metal particles or metal salts to wet the carbide-forming metals in the interstitial spaces of the millimeter-level grains, and then dried.

[0017] In the present invention, the expression "ceramic-metal composite granules" is to be understood as ceramic-metal composite particles, i.e. mainly containing ceramic particles embedded in a first metal matrix, said particles being granular particles of the order of several millimeters, which are subsequently embedded in a second metal matrix, the cast metal matrix, during the casting operation.

[0018] The non-uniform spaces created by particles of different sizes and properties cannot be described other than by the definition of spaces that are filled or unfilled by the particles. As shown in Figures 5 and 6, the grains are bonded, preferably by an organic adhesive, into a three-dimensional ceramic composite network, creating a three-dimensional structure of the reinforced wear part with interstices that are filled during the casting process. [Means for solving the problem]

[0019] A first aspect of the present invention is a hierarchical composite wear part comprising a reinforced portion and a non-reinforced portion, the reinforced portion comprising a three-dimensionally interconnected network of millimeter-sized ceramic-metal composite particulates periodically arranged with millimeter-sized gaps, the ceramic-metal composite particulates containing at least 52% by volume, preferably at least 61% by volume, more preferably at least 70% by volume, of micrometer-sized titanium carbide particles embedded in a first metal matrix, the three-dimensionally interconnected network of millimeter-sized gaps ceramic-metal composite particulates being embedded in a second metal matrix, the reinforced portion comprising a three-dimensionally interconnected network of millimeter-sized gaps ceramic-metal composite particulates being embedded in a second metal matrix, the ceramic-metal composite particulates being at least 52% by volume, preferably at least 61% by volume, more preferably at least 70% by volume, of micrometer-sized titanium carbide particles embedded in a first metal matrix, the ceramic-metal composite particulates being at least 52% by volume, preferably at least 61% by volume, more preferably at least 70% by volume, of micrometer-sized titanium carbide particles embedded in a first metal matrix, the ceramic-metal composite particulates being at least 52% by volume, preferably at least 61% by volume, more preferably at least 70% by volume, the ceramic-metal composite particulates being at least 52% by volume, more ... the strong portion contains an average of at least 23 vol. %, more preferably at least 28 vol. %, and most preferably at least 30 vol. % titanium carbide; the composition of the first metal matrix is ​​substantially different from the composition of the second metal matrix, said second metal matrix containing an iron-based cast alloy present in the millimeter-level interstices of the reinforcement portion, said millimeter-level interstices further containing at least 1 vol. %, preferably 3 vol. %, of micrometer-level carbide particles selected from the group consisting of tungsten carbide, vanadium carbide, molybdenum carbide, titanium carbide, niobium carbide, hafnium carbide and zirconium carbide or mixtures thereof, the volume percentages being measured according to ISO 13383-2:2012.

[0020] According to preferred embodiments of the invention, the composite wear part is further characterized by one of the following features, or a suitable combination thereof: - Density of ceramic-metal composite granules is 4.8g / cm 3 From 6g / cm 2 between 0.2 and 5 g / cm 3 from 5.6 g / cm 3 More preferably, between 5.2 g / cm 3 from 5.4 g / cm 3 wherein said density is measured prior to the casting step of the second metal matrix in accordance with ISO 3369:2006. The ceramic-metal composite particulates have a porosity of less than 5% by volume, preferably less than 3% by volume, most preferably less than 2% by volume, or even less than 0.5% by volume. - the average particle size d of the embedded ceramic-metal composite particles 50 is between 0.5 and 10 mm, preferably between 1 and 5 mm. - the average particle size d of the titanium carbide particles embedded in the first metal matrix 50 is between 0.1 and 50 μm, preferably between 1 and 20 μm. - an average particle size d of micrometer-level carbide particles selected from the group consisting of tungsten carbide, vanadium carbide, molybdenum carbide, titanium carbide, niobium carbide, hafnium carbide and zirconium carbide or mixtures thereof embedded in a second metal matrix; 50 is between 0.1 and 50 μm, preferably between 0.5 and 10 μm, the average grain size of the carbide particles embedded in the second metal matrix being measured by the linear-intercept method according to ISO 4499-3:2016. said first metal matrix is ​​selected from the group consisting of ferro-based alloys, ferromanganese-based alloys, ferrochromium-based alloys and nickel-based alloys, the composition of said ferro-based alloy differing from the composition of the iron-based casting alloy representing the second metal matrix. the second metal matrix contains an iron-based alloy, in particular a high-chromium white cast iron or a steel.

[0021] The present invention further comprises: - crushing a powder composition containing titanium carbide particles, titanium nitride particles, titanium carbonitride particles, or a mixture thereof and metal particles of a first metal matrix in the presence of an antioxidant solvent, such as alcohol or heptane, to obtain an average particle size d 50 between 1 and 20 μm, preferably between 1 and 10 μm; - mixing 1 to 10%, preferably 1 to 6%, of a paraffin wax or a solid lubricant such as Ca / Zn stearate into the powder composition; - removing the solvent by vacuum drying to obtain a weakly agglomerated powder; - forming the weakly cohesive powder into a strip, sheet or rod; - Average particle size d 50 grinding the strip, sheet or rod into ceramic-metal composite particles having a diameter of between 0.05 and 10 mm, preferably between 0.1 and 5 mm; - sintering the granules at high temperature in a vacuum or in an argon atmosphere; A method for making a ceramic-metal composite particulate comprising:

[0022] The present invention relates to - mixing the ceramic-metal composite particulates obtained according to the invention with about 1 to 8% by weight, preferably 2 to 6% by weight, of an organic binder; - adding from 5 to 20% by weight (relative to the atomic weight of the metal) of a carbide-forming metal powder to the granules obtained in the previous step, said carbide-forming metal powder being selected from the group consisting of tungsten, vanadium, molybdenum, titanium, niobium, hafnium and zirconium or mixtures thereof, said carbide-forming powder having an average particle size d 50 is between 10 and 500 μm; - casting and shaping the admixture into a first mold; - curing the organic adhesive; - punching the dried blend to obtain a three-dimensionally interconnected network of periodically alternating millimeter-sized ceramic-metal composite grains with millimeter-sized interstices, said grains being coated / covered with said metal capable of forming in situ metal carbides, which are used to reinforce the worn parts of the layered wear parts; Further disclosed is a method for producing a three-dimensional interconnected network of periodically alternating millimeter-sized ceramic-metal composite grains with millimeter-sized gaps that are coated with a carbide-forming metal powder, comprising:

[0023] The present invention further comprises: - disposing a three-dimensionally interconnected network of millimeter-scale ceramic-metal composite particulates coated with a carbide-forming metal powder, said particulates being periodically arranged in alternating fashion with millimeter-scale gaps in a volume of a first mold of a reinforced hierarchical composite cast wear part; - casting a second metal matrix into a second mold and simultaneously penetrating the millimeter-level interstices of the three-dimensional interconnected network and forming additional carbides in the interstices via an in-situ reaction with a metal capable of forming carbides; - A process for punching out hierarchical composite casting wear parts; A method for producing a hierarchical composite cast wear part is disclosed, comprising:

[0024] The present invention further discloses a hierarchical composite cast wear part obtainable by the method of the present invention. [Brief description of the drawings]

[0025] [Figure 1] 1 shows the anvil ring of a milling machine on which tests for the present invention were conducted. [Diagram 2] 2 represents a single anvil of the anvil ring of FIG. [Diagram 3] It depicts a single worn anvil. [Figure 4] FIG. 13 is a schematic diagram of the placement of reinforcing structures in the most worn portion of a single anvil. [Diagram 5] This shows the overall picture of a reinforcing structure defined as a three-dimensional interconnected network of millimeter-level ceramic-metal composite grains periodically arranged with millimeter-level gaps, the grains being coated with metal particles capable of forming metal carbides in situ. [Figure 6] FIG. 6 depicts an enlarged image of the reinforcement structure of FIG. 5 showing the presence of metal particles forming carbides at the surface of the TiC grains. [Figure 7] It represents a close-up of the reinforcement structure of Figure 5 showing the presence of metal particles forming carbides on the surface of the TiC grains (Figure 7 = optical microscope image). [Figure 7a] The SEM images show strong agglomerates of "clean" ceramic-metal composite grains without any metal particles forming carbides on the surface. [Figure 7b] The SEM images show the coated ceramic-metal composite grains with metal particles forming carbides on the surface. [Figure 8] FIG. 2 shows a cross-sectional detail of a cast wear part having millimeter-sized ceramic-metal composite grains with interstices filled with a second metal matrix (cast metal matrix). [Figure 9] 8 depicts the interface between a composite TiC-metal particulate and a second metal matrix showing microspherical TiC particles (black) embedded in the first metal matrix, with a binder of TiC particles and microspherical NbC particles (white) embedded in the interstitial filling second metal matrix formed in situ. The image is a high magnification image of the interface between the TiC particulate and the second metal matrix depicted in FIG. [Figure 10]1 is a schematic diagram of the inventive concept based on the scale difference between micrometer-level TiC particles embedded in a first metal matrix forming millimeter-level grains of a ceramic-metal composite integrated with a three-dimensional network morphology in the reinforcement portion of the wear part, with additional carbides formed in situ from the carbide-forming metal particles being represented in the gaps between the millimeter-level grains. [Figure 11] 1 is a representative view of a cross-section of a particulate-containing sample, which cross-section is used in a method (described below) for obtaining the average particle size of the ceramic-metal particulates. [Figure 12] FIG. 1 is a schematic diagram of a method for measuring Feret diameters (with minimum and maximum Feret diameters) that are used in a method (described below) for obtaining the average particle size of a ceramic-metal particulate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The present invention relates to a hierarchical composite wear part manufactured by a conventional casting process, said hierarchical composite wear part consisting of a metal matrix with a specific reinforcing structure comprising dense (low porosity <5%) irregular ceramic-metal composite grains with an average diameter on the millimeter scale of 0.5 to 10 mm, preferably 0.8 to 6 mm, more preferably 1 to 4 mm, even more preferably 1 to 3 mm.

[0027] It has been observed that the use of additional metal powder in conjunction with the ceramic metal particulate allows for a supplemental increase in carbide concentration via the carbon source (organic binder) within the interstices once filled by the cast metal.

[0028] The aim of the present invention is to increase the carbide concentration even inside the gaps filled by the cast metal (second metal matrix). Even a small amount of additional micrometer-level carbide particles in the gaps shows a favorable effect on the wear / impact resistance combination of the wear parts. Thus, the hierarchical composite according to the present invention contains in its reinforcement part at least 3% by volume of micrometer-level carbide particles other than the chromium carbides naturally present in high chromium white cast iron, placed in the gaps between the millimeter-level grains obtained via the presence of a carbon source from the carbide-forming metal powder (Ti, Nb, V, W, Mo, Zr, etc.) and the second metal matrix or from the organic binder used to mold the millimeter-level grains of the cermet powder, as well as in the millimeter-level gaps periodically alternating with the millimeter-level ceramic-metal composite grains.

[0029] The ceramic-metal composite is composed of ceramic particles bonded together by a metallic binder, referred to in this invention as a first metal matrix. Additional micrometer-level carbide particles are also provided in a second metal matrix (cast metal) in the millimeter-level interstices between the millimeter-level ceramic-metal composite grains.

[0030] For wear applications, the ceramic provides high wear resistance, while the metal improves toughness, among other properties. TiC ceramic-metal composites contain micrometer-level titanium carbide spherical particles (52 to 95% by volume of the particles, preferably 61 to 90% by volume, more preferably 70 to 90% by volume, with a diameter of 0.1 to 50 μm, preferably 0.5 to 20 μm, more preferably 1 to 10 μm) bonded by a metallic phase (first metal matrix), which may be, for example, an Fe-, Ni- or Mo-based alloy. An iron-based alloy, preferably high-chromium white cast iron or steel (second metal matrix), is cast in a mold and penetrates the interstices of the reinforcing structure.

[0031] In the present invention, the expression TiC, or other metal carbides, is to be understood as titanium carbide in its crystallographic structure, and not in a strict stoichiometric sense. Titanium carbide has a wide composition range, with a C / Ti stoichiometry ranging from 0.47 to 1, and preferably with a C / Ti stoichiometry higher than 0.8.

[0032] The volume content of the ceramic-metal composite particulates in the inserts which make up the reinforcing volume of the wear parts (excluding hollows or recesses, if any) is usually comprised between 45 and 65 vol.%, preferably between 50 and 60 vol.%, resulting in an average TiC concentration in the reinforcing volume comprised between 23 and 62 vol.%, preferably between 28 and 60 vol.%, more preferably between 30 and 55 vol.%.

[0033] The millimeter-level gaps periodically interleaved with the millimeter-level ceramic-metal composite particulates contain at least 3% by volume, preferably at least 5% by volume, of micrometer-level carbide particles selected from the group consisting of tungsten carbide, vanadium carbide, molybdenum carbide, titanium carbide, niobium carbide, hafnium carbide and zirconium carbide or mixtures thereof.

[0034] The hierarchical reinforcement portion of the wear part is made from agglomerates of irregular millimeter-level ceramic-metal composite particulates having an average diameter of approximately between 0.5 and 10 mm, preferably between 0.8 and 6 mm, more preferably between 1 and 4 mm, and even more preferably between 1 and 3 mm (see Figures 5, 6 and 7).

[0035] The ceramic-metal composite granules coated with carbide-forming metal powder are usually agglomerated into the desired three-dimensional shape using known sodium or potassium or silicate glass inorganic adhesives, but in the present invention, organic adhesives such as polyurethane or phenolic resins are preferred as an additional carbon source for the carbide-forming metal. The agglomerates may be placed in a container or behind a barrier. The desired shape forms a weakly agglomerated / strongly agglomerated ceramic-metal composite granules coated with metal powder bonded by a binder, or an open structure formed of a three-dimensionally interconnected network that is held in shape by a container or barrier, and the packing of the granules leaves open gaps at the millimeter level between the granules, which can be filled by liquid casting metal (second metal matrix). The agglomerates are placed or placed in a mold before the step of casting an iron-based alloy to form the reinforcement part of the wear part. The liquid metal is then poured into the mold, and the liquid metal fills the open gaps between the granules. Millimeter-level gaps are to be understood as gaps of 0.1 to 5 mm, preferably 0.5 to 3 mm, depending on the shape of the reinforcing structure and the diameter of the granules.

[0036] Ceramic-metal composite particulates are usually produced in a conventional manner by powder metallurgy techniques in which a blend of ceramic and metal powders having an appropriate particle size distribution is shaped followed by liquid phase sintering.

[0037] Typically, the powders have a diameter of 0.1 to 50 μm and contain TiC as the main component and 5 to 48 percent of a metal binder, which may be a single-component powder or an already alloyed powder (first metal matrix). The powders are first mixed and / or crushed (depending on the initial powder size) in a ball mill (e.g. with alcohol or hexane to avoid metal powder oxidation) by dry crushing or wet crushing methods. Some organic processing aids may be added to aid dispersion or shaping. In the case of wet crushing, a drying step may be required. This can be done, for example, by vacuum drying or spray drying. Shaping is usually performed by cold uniaxial, isostatic pressing or injection molding or any other shaping method to form strips, rods or sheets.

[0038] The strips of the sheet may have an average grain size of d 50 The granules can be ground and optionally sieved to a grain size of between 0.05 and 10 mm, preferably between 0.1 and 5 mm. It can be advantageous to achieve an irregular grain shape without easy drawing orientation (grains that are very well mechanically held in the cast metal). The granules are then sintered at a suitable temperature under low or high vacuum, inert gas, hydrogen or a combination thereof. During liquid phase sintering, grain rearrangement occurs, facilitated by capillary forces. The sintered granules are then mixed with an organic binder and with a carbide-forming metal powder selected from the group consisting of tungsten, vanadium, molybdenum, titanium, niobium, hafnium and zirconium or mixtures thereof, and the carbide-forming powder has an average particle size d 50 between 20 and 500 μm. The admixture contains 1 to 20% by volume, preferably 5 to 15% by volume, of the carbide-forming metal powder and 80 to 99% by volume, preferably 85 to 95% by volume of the ceramic-metal composite particulates.

[0039] The casting alloy (second metal matrix) in which the ceramic-metal composite grains of the wear part are embedded is preferably an iron-based alloy (high chromium white cast iron, steel, manganese steel, etc.) or a nickel or molybdenum alloy, which can be selected to achieve locally optimized properties depending on the final stresses to which the wear part will be subjected (e.g. manganese steel may provide high impact resistance, high chromium white cast iron may provide relatively high wear resistance, nickel alloys may provide relatively good heat and corrosion resistance, etc.).

[0040] The carbide-forming metal powders are selected to achieve locally optimized properties depending on the final stresses to which the wear part is subjected. The choice of carbide-forming metals depends on various criteria, such as low solubility in relatively large crystals (Zr, Hf), or availability and average solubility (Ti, W, Mo) and price.

[0041] advantage The present invention makes it possible to obtain a concentration of TiC particles that can be very high in the ceramic-metal composite granules (52 to 95% by volume) without the risk of defects (gas holes, cracks, inhomogeneities, etc.) inside the casting structure or of uncontrolled and dangerous reactions and extrusions during the in-situ formation of TiC of self-propagating exothermic reactions (SHS, see above) of large amounts of reactive materials during conventional casting processes. In the present invention, a high average concentration of TiC can be achieved in the reinforcement volume of the wear parts via the low porosity of the ceramic-metal composite granules. Values ​​reaching about 62% by volume can be reached depending on the shaping / piling of the ceramic-metal composite granules in the reinforcement volume.

[0042] The use of additional metal powder in conjunction with the ceramic-metal particulate allows for a supplemental increase in the carbide concentration within the interstices once filled by the cast metal, which complements the high concentration of TiC in the ceramic-metal composite particulate, but is not too high in order to maintain the alternating hard and ductile structural properties.

[0043] The hierarchical wear parts of the present invention are substantially free of porosity and cracks, resulting in better mechanical and wear properties.

[0044] The particle size of the titanium carbide and ceramic-metal composite particulates (TiC + binder) of the present invention can be largely controlled during the manufacturing process (choice of raw materials, crushing, shaping process and sintering conditions). The use of sintered millimeter-level TiC-based ceramic-metal composite particulates produced by known powder metallurgy methods allows for control of grain size and porosity, use of various compositions of metal alloys as the first metal matrix, high concentration of TiC, easy shaping of inserts without many manual operations, and good internal integrity of the grains after the casting process even under high thermal shock conditions.

[0045] Production of ceramic-metal composite granules: The grinding and / or mixing of the inorganic TiC powder (52 to 95% by volume, preferably 61 to 90% by volume, more preferably 70 to 90% by volume) and the metal powder as the first metal matrix (5 to 48% by volume, preferably 10 to 39% by volume, more preferably 10 to 30% by volume) is carried out in a ball mill with a liquid, which may be water or alcohol, depending on the oxidation sensitivity of the metal binder, as described above. Various additives (antioxidants, dispersants, binders, plasticizers, lubricants, waxes for pressing, etc.) can also be added for various purposes.

[0046] Once the desired average particle size is reached (usually less than 20 μm, preferably less than 10 μm, more preferably less than 5 μm), the slurry is dried (by vacuum drying or spray drying) to obtain a weak agglomerate of powder containing the organic coagent.

[0047] The weakly cohesive powder is introduced into the granulator through a hopper. This machine comprises two rolls through which the powder passes under reduced pressure and is compacted. At the outlet, a continuous strip (sheet) of compacted material is obtained, which is then crushed to obtain ceramic-metal composite granules. These granules are then sieved to obtain the desired grain size. The undesired grain size group is optionally recycled. The relative density of the resulting granules (depending on the powder properties and the blend composition at the compaction level) is typically between 40 and 70%.

[0048] Depending on the grinding method (impact grinding can result in more solid granules, whereas compression grinding can give more flat granules), it is also possible to adjust the particle size distribution of the granules, as well as their shape to be more or less solid or flat. The granules obtained have a diameter that can result in granules that are generally between 0.5 and 10 mm, preferably between 0.8 and 6 mm, more preferably between 1 and 4 mm, and even more preferably between 1 and 3 mm, after sintering. The granules can also be classically obtained directly as grains or much larger, by uniaxial pressing or granulation of powder blends, and can be further ground into granules before or after sintering.

[0049] Finally, the liquid phase sintering process can be carried out in a furnace at a temperature of 1000 to 1600° C. under vacuum, N2, Ar, H2 or mixtures for a few minutes or hours depending on the metal phase (type and amount of binder) until the desired porosity is reached, preferably less than 5%, more preferably less than 3%, most preferably less than 2%.

[0050] The resulting sintered granules are then mixed with an organic binder and with a carbide-forming metal powder selected from the group consisting of tungsten, vanadium, molybdenum, titanium, niobium, hafnium and zirconium or mixtures thereof, the carbide-forming powder having an average particle size d 50between 20 and 500 μm. The admixture contains 3 to 20%, preferably 5 to 15% by volume of the carbide-forming metal powder and 80 to 97%, preferably 85 to 95% by volume of the resulting ceramic-metal composite particles.

[0051] Reproduction of 3D reinforcement structure (core) As mentioned above, the ceramic-metal composite granules coated with carbide-forming metal powder are weakly cohered either by an adhesive or by containing them in a container or by any other means. The proportion of adhesive does not exceed 10% by weight, preferably between 2 and 7% by weight, relative to the total weight of the granules. This adhesive is preferably an organic adhesive based on polyurethane or phenolic resin.

[0052] The ceramic-metal composite particulates with low porosity can be mixed with an organic binder, preferably before hardening and stamping the core. Depending on the particulate shape, particle size distribution, particulate placement during core creation or vibration during tapping of the particulate bed, the core typically contains 30 to 70% by volume, preferably 40 to 60% by volume of dense particulates and 70 to 30% by volume, preferably 60 to 40% by volume of voids (millimeter-level gaps) in a 3D interconnected network.

[0053] Wear parts casting process The core (a three-dimensional interconnected network reinforcing structure) is placed into the mold section of the wear part to be reinforced and secured with screws or any other available means. Hot liquid iron-based alloy, preferably high chromium white cast iron or steel, is then poured into the mold.

[0054] Thus, at high temperature, the liquid, iron-based alloy fills only the millimeter-level gaps between the grains of the core.

[0055] Due to the limited amount of metal carbide forming metal powder, there is no excessive SHS reaction (exothermic reaction or gas emission) during the casting process, the casting metal may penetrate the interstices (millimeter level spaces between the grains), but may barely penetrate it because the ceramic-metal composite grains are not porous, but the metal powder may form micrometer level carbide particles in the interstices where the second metal matrix exists until the wear part is completely cooled.

[0056] Measurement method For porosity, graininess or particle size measurements, samples are prepared for metallographic examination free of crushing and polishing marks. Care must be taken to avoid particle leakage which may lead to a false evaluation of porosity. Sample preparation guidelines can be found in ISO 4499-1:2020 and ISO 4499-3:2016, 8.1 and 8.2.

[0057] Porosity measurement: The volume fraction of the voids in the free granules can be calculated from the measured density and theoretical density of the granules.

[0058] The porosity volume fraction of grains embedded in a metal matrix is ​​measured according to ISO 13383-2:2012. This standard applies specifically to fine ceramics, but the described method for measuring the porosity volume fraction can be applied to other materials as well. As the samples here are hard metal composites and not pure fine ceramics, the sample preparation should be done according to ISO 4499-1:2020 and ISO 4499-3:2016, 8.1 and 8.2. Etching is not necessary for the porosity measurement, but can be performed anyway, as it is not said to change the results of the measurement.

[0059] Titanium carbide average particle size: The average particle size of the embedded titanium carbide particles is calculated by the linear intercept method according to ISO 4499-3:2016. Five images are taken from five different grain microstructures using an optical or electron microscope at known magnification such that there are 10 to 20 titanium carbide particles across the field of view. Four linear intercept lines are drawn across each calibrated image such that no single particle is crossed more than once by a line.

[0060] If the wire cuts a particle of titanium carbide, the length of the wire (l i ) are counted using a calibrated rule (i=1, 2, 3…n corresponds to the 1st, 2nd, 3rd, …, nth grain). Incomplete grains touching the edge of the image must be ignored. At least 200 grains must be counted.

[0061] The average linear cut particle size is defined as:

[0062]

number

[0063] Average particle size of ceramic-metallic particles: A panoramic image of the photomicrograph is created by adjusting the presence of at least 250 ceramic-metal grains across the entire field of view of the polished surface of the sample. The process of combining a series of digital images of different parts of the object into a panoramic image of the entire object that retains good resolution using a computer program and an optical microscope (e.g. a typical image area panorama obtained with an Alicona Infinite Focus) is part of the prior art. A suitable thresholding allows segmenting the grayscale image into features of the object (grains) and the background (see FIG. 11). If the thresholding is not consistent due to insufficient image quality, a manual stage is used, which involves manually drawing on tracing paper the grains, the scale bar if present, and the image borders, followed by scanning the tracing paper.

[0064] The Feret diameter, which is the distance between two tangents placed perpendicular to the measurement direction, is measured in all directions for each grain by image analysis software (e.g. ImageJ). An example is shown in Figure 12.

[0065] The minimum and maximum Feret diameters of each granule in the image are measured. The minimum Feret diameter is the shortest Feret diameter in the measured set of Feret diameters. The maximum Feret diameter is the longest Feret diameter in the measured set of Feret diameters. Granules in contact with the edge of the image must be ignored. The average of the minimum and maximum Feret diameters of each granule is taken as the equivalent diameter x. The volumetric size distribution q3(x) of the granules is then calculated based on a sphere with diameter x. The D 50 is the volume mass mean diameter x according to ISO 9276-2:2014 - 1,3 It is understood that.

[0066] Average particle size of ceramic-metal granules during granule manufacturing process: Particle size is measured by dynamic image analysis using a Retsch Camsizer according to ISO 13322-2:2006. The particle size used for the particle size distribution is X c min , which is the shortest code measured for the set of largest codes of particle projections (due to the closeness of the screening / sieving results).

[0067] particulate matter d 50 X c min is the volume mass mean diameter of the volume distribution based on

[0068] Particle size measurement of powders during the crushing process: The particle size of the powder during the grinding process is measured by laser diffraction using MIE theory according to the guidelines published in ISO 13320:2020 using a Malvern Mastersizer 2000. The refractive index of TiC is set to 3 and the absorptivity to 1. The absorbance should be within the range of 10 to 15% and the weighted residual should be less than 1%.

[0069] Density measurement of sintered granules Density measurements of sintered granules are carried out using water according to ISO 3369:2006. A gas displacement pycnometer (such as Micromeritics' AccuPyc II 1345 Pycnometer) can also be used for granules without open porosity, giving substantially identical density values.

[0070] Measurement of additional char concentration in the interstices between grains The concentration of additional carbides in the interstitial spaces is measured according to ISO 13383-2:2012, which specifies a manual method of measurement for the determination of volume fractions in fine ceramics, using photomicrographs of polished and etched cross sections, by overlaying squares and counting the number of intersections that lie in each ceramic phase.

[0071] Implementation - Anvil Wear Parts Anvil wear parts for use in longitudinal impact members were made according to the present invention, with the reinforcement volume of the wear part having different average volume percentages of TiC ranging from about 30 to 50 volume % (FIGS. 1 to 3).

[0072] They were compared to wear parts made according to U.S. Patent No. 8,999,518, invention Example 4 (where the total volume percentage of TiC in the reinforcement volume is about 32 volume %). The reason for this comparison is that Example 4 is a typical "in situ" composition (Ti+C and moderator in a self-propagating reaction) that can be handled with care in a plant, despite the fact that it still causes flames, gases and some hot liquid metal ejection during the casting process.

[0073] The anvil wear parts of the present invention were also compared to wear parts made with different ceramic reinforcements but the same metal matrix.

[0074] Preparation of two different types of TiC granules: TiC powder with a size less than 325 mesh (44 μm) is mixed with one or more alloyed elements or pure single elements to the composition shown in Table 1. The powder is then crushed in a ball mill for 24 hours with a processing aid such as alcohol to avoid oxidation of the metal to an average particle size of 3 μm.

[0075] [Table 1]

[0076] After the antioxidant solvent is removed by a vacuum dryer with a rotary blade, about 2% by weight of paraffin wax is added and mixed with the powder blend. The resulting weakly agglomerated powder is then sieved through a 100 μm sieve. A strip of 70% theoretical density of the inorganic / metallic powder mixture is produced by rolling between the rotating rolls of a roller compactor granulator at about 200 bar pressure. The strip is then crushed into irregular granules by passing through a sieve with a suitable mesh size. After crushing, the granules are sieved to have dimensions between 1.4 and 4 mm. These irregular porous granules are then sintered at high temperatures of about 1300°C to 1500°C for 2 hours in a vacuum furnace with a partial pressure of argon at about 20 mbar until a minimal porosity (<0,5% by volume) is reached.

[0077] The low porosity sintered granules type 2 are then mixed with about 2% by weight of an organic two-component polyurethane adhesive, and a carbide-forming elemental metal powder is then added to the admixture containing the granules type 2, the niobium powder having a size less than 325 mesh of Example 1, and the zirconium powder less than 325 mesh of Example 2. The fine metal powder particles adhere to the polyurethane on the surface of the millimeter-level granules and form a coating on the surface.

[0078] The blend is cast into a silicone mold (vibration may be applied to facilitate filling and ensure all particles are filled correctly) with the desired shape of 100×30×150 mm. After drying at 100° C. in a stove for several hours or gas curing with amine gas for polyurethane binder, the core is hard enough to be demolded.

[0079] This interconnected network of metal coated granules contains approximately 55% by volume of fine powder coated dense granules (45% by volume of voids / millimeter level gaps between coated granules) as shown in Figures 5 and 6. Each core / 3D reinforcing structure is placed into a mold in the wear part section and reinforced (as shown in Figure 4). Hot liquid high chromium white cast iron or carbon steel of the composition shown in Table 2 is then poured into the mold.

[0080] [Table 2]

[0081] During the casting process, the hot liquid metal fills all the millimeter-level gaps between the grains of the interconnected network, said gaps representing 45% of the total volume of the reinforced part. During the casting process, the polyurethane adhesive is carbonized and the metal powder additive reacts with the carbon of the melt as a carbon source and / or with the carbon of the carbonized polyurethane to form additional carbide particles. After the casting process, in the reinforced part, a composite is formed from a high concentration of about 86% by volume of titanium carbide particles bonded by 55% by volume of a first metal matrix and 45% by volume of a second metal matrix with an average additional concentration of niobium or zirconium additional carbide particles of about 8% by volume (see Table 3 below). The total volume content of carbides, other than the chromium carbides naturally present in the chromium steel, obtained in the reinforced macro-microstructure of the wear part is then about 47% by volume. EXAMPLES

[0082] In the following examples, the dimensions of the reinforced area are 150 x 100 x 30 mm, and the 3 The filling rate of the reinforcement is 55% by volume, so the volume of the metal-ceramic particulate is 248 cm 3 is equivalent to.

[0083] The following discloses the composition and properties of a three-dimensional interconnected network of periodically alternating millimeter-scale ceramic-metal composite grains.

[0084] [Table 3]

[0085] Reinforcement volume is 450cm 3 (V 補強された ) and 1314 g of granules (W 粒状物 ) to evaluate the concentration of additional carbides in the second metal matrix (volume %). The theoretical density of the granules is 5,33 g / cm 3 The porosity is 0.4% by volume and the total granule volume is 247 cm 3 and the volume of the gap is 202.5 cm 3 It is.

[0086] [Table 4]

[0087] Comparison with prior art The wear parts according to the invention are compared with the wear parts obtained in Example 4 of U.S. Patent No. 8,999,518 (see Inventive Comparative Example 2). The anvil wear parts according to the invention are also compared with wear parts made from ceramic-metal particulates in which the binder is the same as the casting alloy (see Inventive Comparative Example 3). The anvil ring of the milling machine on which these tests were performed is shown in FIG.

[0088] In this machine, the inventors alternated anvils containing inserts according to the invention (as depicted in Figures 2 and 3) surrounded on either side by anvils reinforced according to the prior art, Comparative Example 2 and Comparative Example 3, in order to evaluate wear under identical conditions. The material to be crushed is projected at high speed onto the working surface of the anvil (a single anvil before wear is depicted in Figure 2). During the crushing process, the working surface is worn. The worn anvils are depicted in Figure 3.

[0089] Calculation of the evaluation index For each anvil, the mass loss is measured by weighing each anvil before and after use. Mass loss = (final mass - initial mass) / initial mass The rating index is defined as follows, where the reference mass loss is the average mass loss of Example 4 of US Pat. No. 8,999,518, the anvils on either side of the test anvil (of Comparative Example 2 herein). PI = mass loss of reference anvil / mass loss of test anvil

[0090] A rating index greater than 1 means that the test anvil is not worn compared to the reference anvil, and a rating index less than 1 means that the test anvil is worn compared to the reference anvil.

[0091] - The performance index (PI) of the anvil reinforced according to the comparative example 3 of the present invention (using ceramic-metal composite particulates containing 86% by volume (80% by mass) of titanium carbide bonded by a similar metal matrix as the casting alloy) is 1.10. The higher performance than the comparative example 2 (example 4 of US Pat. No. 8,999,518) can be explained by the lower defects such as cracks and porosity of the parts, as well as the much higher local and total volume concentration of titanium carbide in the particulates and reinforcement. - The performance index (PI) of the anvil reinforced according to the inventive comparative example 1 (using ceramic-metal composite granules containing 86% by volume (80% by mass) of titanium carbide bonded by a different metal matrix (steel) as the casting alloy) is 1.20. The higher performance compared to comparative example 3 can be explained by the higher toughness of the granules due to the tough steel matrix against the relatively brittle high chromium white cast iron matrix. - The performance index (PI) of the anvil reinforced according to Example 1 of the invention (using ceramic-metal composite particulates containing 86% by volume (80% by mass) of titanium carbide) and 8% by volume of additional carbides in the casting alloy formed by additional niobium metal powder in the insert before the casting process is 1.30. The higher performance than Example 2 can be explained by the presence of niobium carbide in the second metal matrix, which outperforms zirconium carbide in this particular condition. The performance index (PI) of the anvil reinforced according to Example 2 of the invention (using ceramic-metal composite particulates containing 86% by volume (80% by mass) of titanium carbide) and 8% by volume of additional carbides in the casting alloy formed by additional zirconium metal powder in the insert before the casting process is 1.25. The higher performance than Comparative Example 1 can be explained by the additional carbides in the second metal matrix.

[0092] Density of composites relative to density of compounds (titanium carbide and alloys) The table below illustrates the density of the composites as a function of volume percent TiC and volume percent porosity (for iron-based alloys).

[0093] [Table 5]

[0094] [Table 6]

[0095] Advantages of the Invention Compared with the prior art, the present invention has the following advantages: - Better wear performance due to a locally high volume % of TiC in the granules (which is practically impossible to achieve with SHS technology using large amounts of reactants as in the prior art). - Better wear performance or mechanical properties of the wear parts by adjusting the size and volume content of titanium carbide and the use of a metal phase binder (first metal matrix) such as manganese steel with high mechanical properties in TiC ceramic-metal composite particulates in combination with a cast alloy (second metal matrix) such as high chromium white iron, the first metal matrix being different from the second metal matrix. - Better wear performance or mechanical properties of the wear parts by adjusting the size and volume content of the additional carbides in the second metal matrix. - Better wear performance or mechanical properties of the wear parts due to lower porosity and / or fewer crack defects as little or no gas is evolved during the casting process.

Claims

1. 1. A hierarchical composite wear part comprising reinforced and non-reinforced portions, the reinforced portions comprising a three-dimensionally interconnected network of millimeter-sized ceramic-metal composite particulates periodically arranged with millimeter-sized gaps, the ceramic-metal composite particulates containing at least 52 vol.%, preferably at least 61 vol.%, more preferably at least 70 vol.% micrometer-sized titanium carbide particles embedded in a first metal matrix, the ceramic-metal composite particulates having a porosity of less than 5 vol.%, preferably less than 3 vol.%, most preferably less than 2 vol.%, the volume fraction of porosity of the particulates embedded in the first metal matrix being measured according to ISO 13383-2:2012; the three-dimensionally interconnected network of ceramic-metal composite particles having millimeter-level interstices is embedded in a second metal matrix, the volume content of the ceramic-metal composite particles in the reinforcement portion being comprised between 45 and 65 volume percent, preferably between 50 and 60 volume percent; the composition of the first metal matrix is ​​substantially different from the composition of the second metal matrix; The second metal matrix contains an iron-based casting alloy present in the millimeter-level interstices of the reinforcement portion, and the millimeter-level interstices further contain at least 1 vol. %, preferably at least 3 vol. %, of micrometer-level carbide particles selected from the group consisting of tungsten carbide, vanadium carbide, molybdenum carbide, titanium carbide, niobium carbide, hafnium carbide and zirconium carbide or mixtures thereof, the volume percentage of additional carbides in the second metal matrix being measured according to ISO 13383-2:2012; Hierarchical composite wear parts.

2. The average particle size d of the embedded ceramic-metal composite particles 50 between 0.5 and 10 mm, preferably between 1 and 5 mm, and said average particle size is as follows: - taking a photomicrograph image of a polished cross-section of the sample capturing at least 250 ceramic-metal grains across the field of view; - measuring the Feret diameter of the granular material; - calculating the volumetric particle size distribution of the granular material; - d of said granules 50 Calculating in accordance with ISO 9276-2:2014; The hierarchical composite wear part of claim 1 , wherein the wear resistance is measured by

3. The average particle size d of the titanium carbide particles embedded in the first metal matrix 50 3. The hierarchical composite wear part according to claim 1 or 2, wherein the average particle size of the embedded titanium carbide particles is between 0.1 and 50 μm, preferably between 1 and 20 μm, as measured by the linear intercept method according to ISO 4499-3:2016.

4. The average particle size d of micrometer-level carbide particles selected from the group consisting of tungsten carbide, vanadium carbide, molybdenum carbide, titanium carbide, niobium carbide, hafnium carbide, chromium carbide and zirconium carbide or mixtures thereof embedded in the second metal matrix. 50 4. The hierarchical composite wear part according to claim 1, wherein the average grain size of the carbide particles embedded in the second metal matrix is ​​between 0.1 and 50 μm, preferably between 1 and 20 μm, as measured by a linear intercept method according to ISO 4499-3:2016.

5. 5. The hierarchical composite wear part of claim 1, wherein the first metal matrix is ​​selected from the group consisting of a ferro-based alloy, a ferromanganese-based alloy, a ferrochromium-based alloy, and a nickel-based alloy, the composition of the ferro-based alloy being substantially different from the composition of the iron-based cast alloy of claim 1.

6. The hierarchical composite wear part of any one of claims 1 to 5, wherein the second metal matrix comprises high chromium white iron or steel.

7. - crushing a powder composition containing titanium carbide particles, titanium nitride particles, titanium carbonitride particles, or a mixture thereof and metal particles of the first metal matrix to obtain an average particle size d 50 between 1 and 20 μm, preferably between 1 and 10 μm; - mixing 1 to 10%, preferably 1 to 6%, of a weakly cohesive wax into the powder composition; - forming the weakly cohesive powder into a strip, sheet or rod; - Average particle diameter d 50 grinding the strip, sheet or rod into ceramic-metal composite particles until the diameter is between 0.05 and 10 mm, preferably between 0.1 and 5 mm; - sintering the particles of said ceramic-metal composite into millimetre-sized granules until the porosity is less than 5%, more preferably less than 3% and most preferably less than 2%; - mixing said sintered ceramic-metal composite particulates with about 1 to 8% by weight, preferably 2 to 6% by weight, of an organic binder; - mixing 1 to 20%, preferably 5 to 15% by volume of a carbide-forming metal powder with 80 to 97%, preferably 85 to 95% by volume of the ceramic-metal composite particles obtained in the previous step, said carbide-forming metal powder being selected from the group consisting of tungsten, vanadium, molybdenum, titanium, niobium, hafnium and zirconium or mixtures thereof, said carbide-forming powder having an average particle size d 50 is 20 to 500 μm; - forming the admixture in a first mould; - drying the mixture at a suitable temperature to harden or dry the adhesive; - stamping the dried mixture to obtain a three-dimensional interconnected network of millimeter-sized ceramic-metal composite grains periodically interleaved with millimeter-sized gaps; - placing said three-dimensionally interconnected network in a second mold volume of a reinforced hierarchical composite cast wear part; - casting a second metal matrix into a second mold and simultaneously penetrating the millimeter-level interstices of said three-dimensionally interconnected network to form additional carbides in the millimeter-level interstices selected from the group consisting of tungsten carbide, vanadium carbide, molybdenum carbide, titanium carbide, niobium carbide, hafnium carbide and zirconium carbide, or mixtures thereof; - stamping the hierarchical composite cast wear part; A method for producing the ceramic-metal composite particulate according to any one of claims 1 to 6, comprising:

8. The density of the sintered ceramic-metal composite particulates is 4.8 g / cm 3 to 6 g / cm 3 between 5 g / cm and 6 g / cm 3 to 5.6 g / cm 3 and more preferably 5.2 g / cm 3 to 5.4 g / cm 3 and said density is measured before the casting step of the second metal matrix according to ISO 3369:2006.

9. The ceramic-metal composite particles are heated in vacuum, N 2 , Ar, H 2 or mixture thereof, in a furnace at a temperature of 1000 to 1600°C, until the porosity is less than 5%, more preferably less than 3%, and most preferably less than 2%.

10. 8. The method according to claim 7, wherein the ceramic-metal composite particulates sintered by liquid phase sintering are sintered in a vacuum furnace with a partial pressure of argon of about 20 mbar at a temperature of 1300°C to 1500°C for 2 hours until the porosity is <0.5% by volume.

Citation Information

Patent Citations

  • JP1982500788A

  • Layered composite materials

    JP2012502802A

  • Powder composition for producing casting inserts, casting inserts and method for obtaining local composite zones in castings - Patents.com

    JP2019501026A

  • Hierarchical composite material

    US20110229715A1

  • Powder Composition For The Manufacture Of Casting Inserts, Casting Insert And Method Of Obtaining Local Composite Zones In Castings

    US20180369905A1