Nanoflake-shaped spinel oxidation catalyst for anion exchange membrane water electrolysis and its manufacturing method

A spinel-based oxide with a nanoflake structure, produced via controlled coprecipitation, addresses the challenges of agglomeration and non-uniform dispersion in anion exchange membrane water electrolysis systems, improving catalytic activity and conductivity for efficient hydrogen production.

JP2024536827APending Publication Date: 2024-10-08HANWHA SOLUTIONS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024518479
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-24
Filing Date
2022-09-23
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing anion exchange membrane water electrolysis systems face challenges with oxidation catalysts that have high overvoltage, low electrical conductivity, and poor durability due to agglomeration and non-uniform dispersion, leading to increased costs and reduced performance.

Method used

A spinel-based oxide with a nanoflake structure is produced through a controlled coprecipitation method, using a complexing agent and specific pH conditions to form a catalyst with high porosity and uniform dispersion, enhancing catalytic activity and electrical conductivity.

Benefits of technology

The catalyst achieves improved catalytic activity, electrical conductivity, and uniform coating, resulting in enhanced performance and reduced production costs for anion exchange membrane water electrolysis systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536827000001_ABST
    Figure 2024536827000001_ABST
Patent Text Reader

Abstract

The present invention relates to an oxidation catalyst for anion exchange membrane water electrolysis that exhibits excellent catalytic activity, electrical conductivity, and a large surface area, a method for producing the same, and an oxidation electrode for anion exchange membrane water electrolysis and an anion exchange membrane water electrolysis system including the same. The oxidation catalyst for anion exchange membrane water electrolysis of the present invention includes a spinel oxide, and is produced by using a coprecipitation method while precisely controlling the use or absence of a complexing agent and the pH, thereby making it easy to reduce the catalyst particle size and uniformly disperse the catalyst at high viscosity, and has a nano-sized flake structure, which allows uniform coating of ionomer between the flakes, and forms a porous structure to increase the surface area and provide excellent catalytic activity.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Cross-reference to related applications This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0126220 filed on September 24, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to an oxidation catalyst for anion exchange membrane water electrolysis that exhibits excellent catalytic activity, electrical conductivity, and a large surface area, a method for producing the same, and an oxidation electrode for anion exchange membrane water electrolysis and an anion exchange membrane water electrolysis system including the same. [Background technology]

[0003] Water electrolysis is a technology that produces hydrogen by electrically splitting water, which first emerged in the 1800s and has been used for commercial hydrogen production since the 1920s. Recently, as the need for and share of renewable energy has increased significantly, it has been attracting attention as a solution for low-carbon, green hydrogen production.

[0004] The main water electrolysis technologies currently being commercially applied are the alkaline water electrolysis (AWE) system and the proton exchange membrane water electrolysis (PEMWE) system.

[0005] Among these, alkaline water electrolysis is cost-competitive because it uses inexpensive nickel-based electrodes and porous membranes, but it has the disadvantage that it can only operate at low current density because the gap between the porous diaphragm and the electrode is wide, resulting in high internal resistance.Also, alkaline water electrolysis systems have the disadvantages of being large in stack volume, high operating costs, and difficulty in linking with renewable energy sources such as wind or solar power because it is difficult to change the current density suddenly due to the use of porous diaphragms.

[0006] Meanwhile, cation exchange membrane water electrolysis systems are being developed on a megawatt scale. Such cation exchange membrane water electrolysis systems can be operated at high current densities, allowing for a compact system design, and produce high purity hydrogen while maintaining low initial output pressure and minimum load. In addition, they have a fast response speed and are suitable for producing hydrogen in conjunction with renewable energy.

[0007] However, the cation exchange membrane water electrolysis system has a drawback in that the overall manufacturing cost is significantly increased because expensive precious metal catalysts and precious metals must be used as bipolar plates to prevent corrosion.

[0008] Therefore, an anion exchange membrane water electrolysis system has been proposed as a technology to replace the alkaline water electrolysis system and the cation exchange membrane water electrolysis system currently being applied commercially, and interest and research thereon have been greatly increased.

[0009] Such an anion exchange membrane water electrolysis system can be designed compactly and can use non-precious metal materials because it is operated in the same atmosphere as the alkaline water electrolysis system. Therefore, such an anion exchange membrane water electrolysis system can be considered as a system that can utilize the advantages of both the alkaline water electrolysis system and the cation exchange membrane water electrolysis system.

[0010] However, in order to improve the performance of such an anion exchange membrane water electrolysis system, it is necessary to use an oxidation catalyst that exhibits excellent electrical conductivity and catalytic activity at an oxidation electrode (anode) where an oxygen evolution reaction accompanied by a larger overvoltage, for example, the reaction represented by the following reaction formula, occurs, and also has high durability.

[0011] [Reaction Scheme 1] 4OH - →O2+2H2O+4e - Considering that the anion exchange membrane water electrolysis system operates at a low temperature of about 100° C. or more, precious metal catalysts such as IrO2 or RuO2 have been considered as oxidation catalysts that meet the requirements. However, these precious metal catalysts are expensive and difficult to commercialize, making it difficult to utilize the advantages of the anion exchange membrane water electrolysis system.

[0012] Therefore, research has been ongoing recently to apply layered double hydroxides (LDH), perovskite-based compounds, or spinel-based compounds as the oxidation catalyst. However, although the layered double hydroxides and spinel-based compounds have relatively high catalytic activity, they have low electrical conductivity and are therefore unsuitable for use as oxidation catalysts.

[0013] In contrast, spinel structure compounds are oxides represented by the general formula AB2O4 (A and B are alkaline earth metals and transition metals, respectively), and can exhibit excellent catalytic activity and also exhibit excellent electrical conductivity through doping with various metal atoms.

[0014] However, spinel structure compounds synthesized by the existing coprecipitation method are formed into nano-sized particles, but they have high surface energy and tend to solidify, and the particle size increases, which reduces the surface area and reduces catalytic activity, and they have high specific gravity and tend to settle during the slurry production process, making it difficult to disperse well and difficult to produce a uniform coating layer.In addition, spinel structure compounds synthesized by the existing coprecipitation method have high surface energy and tend to solidify, and the ionomer is not uniformly coated, which reduces adhesion, and as the current density increases, bubble generation increases, detachment of the catalyst layer accelerates and durability decreases.

[0015] Therefore, research is being conducted to improve the dispersion process in order to manufacture a highly dispersed and uniform catalyst layer. However, this is not a fundamental solution as it requires additional equipment and energy, which increases the manufacturing cost. In addition, the reality is that an oxidation catalyst that can be applied to an anion exchange membrane water electrolysis system and shows excellent properties has not yet been fully developed.

[0016] In addition, a catalyst layer with high porosity has a wider contact area between the ionomer and the reactant (OH-) and increases the three-phase interface, which allows for excellent cell performance. Therefore, in order to achieve excellent cell performance, the catalyst layer needs to have high porosity.

[0017] Therefore, there is a continuing demand for the development of spinel-based oxidation catalysts that can be manufactured to have improved dispersibility and high porosity by controlling the catalyst particle size and specific gravity. Summary of the Invention [Problem to be solved by the invention]

[0018] Therefore, the present invention provides an oxidation catalyst for anion exchange membrane water electrolysis, which includes a spinel-based oxide that has a large surface area, allows uniform coating of an ionomer, has excellent catalytic activity, and has low cohesive force, allowing uniform dispersion at high viscosity, making it easy to coat on a membrane electrode assembly (MEA), and a manufacturing method thereof.

[0019] The present invention also provides an oxidation electrode for anion exchange membrane water electrolysis, and an anion exchange membrane water electrolysis system, each of which contains the oxidation catalyst. [Means for solving the problem]

[0020] Therefore, the present invention provides an oxidation catalyst for anion exchange membrane water electrolysis, comprising a spinel-based oxide represented by the following Chemical Formula 1, wherein the spinel-based oxide comprises a nanoflake structure: [Chemical formula 1] Nico (2-x) M x O4 In the above chemical formula 1, 0≦x≦0.5.

[0021] The present invention also provides a method for preparing an oxidation catalyst for anion exchange membrane water electrolysis, comprising the steps of: co-precipitating a nickel salt, a cobalt salt, and a metal (M) salt in an aqueous solvent having a pH of 11 or more in the presence of a complexing agent to form a catalyst precursor; and calcining the catalyst precursor at a temperature of 100° C. or more to form a spinel-based oxide of Chemical Formula 1.

[0022] In the spinel structure catalyst of Formula 1, the cobalt (Co) material acts as the active site of the catalyst, so the activity increases as the cobalt (Co) content increases. However, if x exceeds 0.5 and the cobalt content becomes excessive, the catalytic activity decreases rather rapidly.

[0023] The present invention also provides an oxidation electrode for anion exchange membrane water electrolysis, comprising a catalyst layer containing the above-mentioned oxidation catalyst formed on a gas diffusion layer.

[0024] The present invention also provides an anion exchange membrane water electrolysis system, comprising: an anion exchange membrane; a reduction electrode located on one side of the anion exchange membrane; and an oxidation electrode located on the other side of the anion exchange membrane such that a catalyst layer is in contact with the anion exchange membrane. Effect of the Invention

[0025] The oxidation catalyst for anion exchange membrane water electrolysis of the present invention contains a spinel-based metal oxide, and is prepared using a coprecipitation method while precisely controlling the use or absence of a complexing agent and the pH, thereby making it possible to reduce the size of catalyst particles and facilitate uniform dispersion at high viscosity, thereby facilitating MEA coating.

[0026] The oxidation catalyst for anion exchange membrane water electrolysis of the present invention is formed by agglomerating primary particles having a nanoflake structure to form micro-sized secondary particles, which allows for uniform coating of ionomer between the nanoflake structures, and the catalyst layer forms a porous structure, increasing the surface area and providing excellent catalytic activity.

[0027] Due to the excellent overall physical properties of the oxidation catalyst, the anion exchange membrane oxidation catalyst according to the present invention can be very suitably applied to an anion exchange membrane water electrolysis system. [Brief description of the drawings]

[0028] [Figure 1] FIG. 1 is a flowchart showing a process for producing an oxidation catalyst for anion-exchange membrane water electrolysis containing a spinel oxide by a coprecipitation method according to the present invention. [Figure 2a] FIG. 2a is a scanning electron microscope (SEM) photograph of the surface of the oxidation catalysts according to Comparative Examples 1 to 3 and Examples 1 to 5 of the present invention. [Figure 2b] FIG. 2b is a scanning electron microscope (SEM) photograph of the surface of the oxidation catalysts according to Comparative Examples 5 to 7 and Examples 5 to 7 of the present invention. [Figure 2c] FIG. 2c shows a more enlarged SEM and TEM image of the surface of the oxidation catalyst according to Example 4. [Figure 3a] FIG. 3a shows the results of XRD analysis of the oxidation catalyst according to Comparative Example 1 of the present invention. [Figure 3b] FIG. 3b shows the results of XRD analysis of the oxidation catalysts according to Comparative Example 3 and Examples 2 and 4 of the present invention. [Figure 3c] FIG. 3c shows the results of XRD analysis of the oxidation catalysts according to Comparative Examples 5 and 6 and Examples 5, 6, and 7 of the present invention. [Figure 4] FIG. 4 shows the results of comparing the packing density (tab density) of the oxidation catalysts according to Comparative Examples 1, 3 to 7 and Examples 2, 4 to 7 of the present invention. [Diagram 5]FIG. 5 shows photographs of the surface and cross section of the MEA electrode catalyst layer coated with the oxidation catalyst according to Comparative Examples 1 and 3 and Examples 2 and 4 of the present invention, observed with an electron microscope (SEM). [Figure 6] FIG. 6 shows the measured specific surface areas of the oxidation catalysts according to Comparative Examples 1 and 3 and Examples 2 and 4 of the present invention. [Figure 7] FIG. 7 shows a graph of current density (mA / cm2) in the voltage range of 1.4 to 2.2 V for a single cell including oxidation catalysts according to Comparative Examples 1 and 3 and Examples 2 and 4 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] In the present invention, the terms "first", "second", etc. are used to describe various components, and the terms are used only to distinguish one component from another.

[0030] In addition, the terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In this specification, the terms "include", "includes", "has" or "has" are intended to specify the presence of an embodied feature, number, step, component, or combination thereof, and should be understood not to preclude the presence or additional possibility of one or more other features, numbers, steps, components, or combinations thereof.

[0031] In addition, in the present invention, when a layer or element is referred to as being formed "on" or "on" another layer or element, it means that the layer or element is formed directly on the other layer or element, or that other layers or elements can be additionally formed between the layers, on the object, or on the substrate.

[0032] Since the present invention can be modified in various ways and has various forms, the specific embodiments are illustrated and described in detail below, but it is to be understood that the present invention is not limited to the specific disclosed forms, but includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention.

[0033] Hereinafter, an oxidation catalyst for anion exchange membrane water electrolysis and a manufacturing method thereof according to embodiments of the present invention, as well as an oxidation electrode and an anion exchange membrane water electrolysis system including the same will be described in detail.

[0034] First, in the description of the present invention, "particle size Dn" means the particle size at the n% point of the cumulative particle number distribution by particle size. That is, D 50 is the particle size at the 50% point of the cumulative particle number distribution by particle size, and D 90 is the particle size at the 90% point of the cumulative particle number distribution by particle size, D 10 is the particle size at the 10% point of the cumulative particle number distribution by particle size.

[0035] The Dn can be measured using a laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500). When the particles pass through a laser beam, the difference in the diffraction pattern according to the particle size is measured to calculate the particle size distribution. The Dn of the present invention can be calculated by calculating the particle diameter at the 10%, 50%, and 90% points of the cumulative particle number distribution according to the particle size in the measuring device. 10 , D 50 and D. 90 can be measured.

[0036] According to one embodiment of the present invention, there is provided an oxidation catalyst for anion exchange membrane water electrolysis, comprising a spinel-based oxide represented by the following Chemical Formula 1, wherein the spinel-based oxide comprises a nanoflake structure: [Chemical formula 1] Nico (2-x) M x O4 In the above chemical formula 1, 0≦x≦0.5.

[0037] The present inventors have continued their research to develop an oxidation catalyst having excellent general properties suitable for application to an anion exchange membrane water electrolysis system. As a result of such research, it has been confirmed that an oxidation catalyst having a nanoflake structure, which is a spinel oxide represented by Chemical Formula 1, can be provided by controlling the complexing agent and pH range.

[0038] Therefore, the oxidation catalyst produced by the production method of the present invention can be uniformly dispersed at high viscosity during the slurry production process because secondary particles formed by aggregation of primary particles including single or multiple nanoflake structure particles do not grow excessively.In addition, the ionomer can be uniformly coated between the nanoflake structures, and the catalyst layer forms a porous structure to increase the surface area, thereby providing excellent catalytic activity.

[0039] As a result, the oxidation catalyst of one embodiment includes the spinel-based oxide of Formula 1, and can exhibit excellent electrical conductivity, catalytic activity, and MEA coating properties and can be provided with a large surface area, and therefore can be very preferably applied to anion exchange membrane water electrolysis systems and their oxidation electrodes (anodes).

[0040] Meanwhile, in Chemical Formula 1, (2-x) represents the molar ratio of cobalt, and x may represent the molar ratio of metal (M). Specifically, the range of x in Chemical Formula 1 may be 0≦x≦0.5 or 0≦x≦0.2. Preferably, x may be 0.2. The metal molar ratio in the oxidation catalyst for anion exchange membrane water electrolysis may be determined by elemental analysis using a method such as ICP or XRD.

[0041] In addition, in Chemical Formula 1, the metal (M) may be one or more elements selected from the group consisting of Fe, Sc, Ti, V, Cr, Y, Zr, Nb, and Mo. Preferably, the metal (M) may be Fe.

[0042] The Mn3O4 catalyst with spinel structure is stable because it exists as a Mn3O4 phase in 1M KOH (pH 14) electrolyte, but in the oxygen evolution reaction (OER) atmosphere, MnO4 2- It is difficult to use in an alkaline environment because it is transformed into ions and dissolved. This can be confirmed by the Pourbaix diagram, which shows the relationship between pH and voltage.

[0043] In addition, the pure Mn-based spinel catalyst (Mn3O4) has a current of 10 mA / cm 2 It has an overpotential of 370~570mV at current density. Therefore, it shows lower catalytic activity than IrO2, even though it is doped with various materials such as Ni, Co, Pt, etc. to enhance catalytic activity.

[0044] Therefore, Mn-based spinel structure catalysts are not only poor in catalytic activity but also difficult to use due to their unstable structure in an alkaline atmosphere, and are therefore unsuitable for use as oxygen generating catalysts for AEM water electrolysis.

[0045] The spinel oxide contained in the oxidation catalyst for anion exchange membrane water electrolysis may have a form of secondary particles in which primary particles including a single or a plurality of nanoflake structure particles are aggregated.

[0046] The size of primary and secondary particles, including nanoflake structure particles, can be confirmed using a transmission electron microscope (TEM).

[0047] Specifically, the primary particles include single or multiple nanoflake structure particles, and have a particle size (D 50 ) may be 500 nm or less. 50 ) may be 1 to 500 nm, or 100 to 500 nm, or 100 to 400 nm, or 250 to 350 nm. In the present invention, a complexing agent is used in the production method to control the pH range, thereby controlling the degree of aggregation of the secondary particles and preventing the secondary particles from becoming excessively coarse, thereby improving dispersibility.

[0048] In this case, the nanoflake structure is a plate-shaped structure, and the long and short sides may be the same or different. When the long and short sides are the same, the length of one side may be 300 nm or less. Specifically, the long side may be 50 to 300 nm, or 100 to 300 nm, or 100 to 200 nm. When the long and short sides are different, the long side may be 300 nm or less, specifically, the long side may be 50 to 300 nm, or 100 to 300 nm, or 100 to 200 nm, and the short side may be 200 nm or less, specifically, the short side may be 10 to 200 nm, or 10 to 100 nm, or 10 to 50 nm. The thickness of the nanoflakes may be 50 nm or less, specifically, 1 to 50 nm, or 1 to 40 nm, or 1 to 25 nm, or 10 to 15 nm (see Figures 2a to c).

[0049] The oxidation catalyst for anion exchange membrane water electrolysis according to the present invention includes a nano-sized nanoflake structure, so that it can be formed as a porous catalyst layer when the catalyst layer is formed, and ionomer can be coated between the nanoflakes, which is advantageous in showing catalytic activity. However, if the nanoflake structure exceeds the above range, the size of the secondary particles also grows, which makes it difficult to uniformly disperse the high viscosity particles during the slurry preparation process, which makes it difficult to apply the catalyst to MEA coating.

[0050] In addition, the secondary particles have a monodisperse particle size distribution, D 50 The secondary particles may have a particle size of 3 μm or less. 50 The diameter of the secondary particles may be 0.1 to 1 μm, or 0.4 to 0.7 μm. 90may be 10 μm or less, specifically 1-5 μm, or 2-3 μm. It can be seen that the secondary particles of the present invention are formed in a very small size compared to secondary particles produced by the existing coprecipitation method. This is because the oxidation catalyst of the present invention is produced using a complexing agent to form a nanoflake structure, which solidifies during the slurry production process, and the nanoflake structure minimizes aggregation. Therefore, the oxidation catalyst of the present invention minimizes particle aggregation in the slurry state and maintains a small particle size, making it possible to produce a high viscosity slurry and produce a uniform catalyst layer.

[0051] Meanwhile, the spinel oxide according to the present invention may be used as an oxidation catalyst for anion exchange membrane water electrolysis by itself, or may be used in a state where a small amount of a different element is doped. By adding such an additional dopant, the catalytic active sites are increased, and the activity and electrical conductivity of the oxide as an oxidation catalyst can be further improved. The type of the dopant that can be added is not particularly limited, and for example, one or more different elements selected from the group consisting of Ni, Fe, Cu, and Li may be doped.

[0052] The spinel oxide having the above-mentioned excellent catalytic activity, electrical conductivity, and large surface area can be prepared by a method using a coprecipitation method. Therefore, according to another embodiment of the present invention, the method for preparing the oxidation catalyst according to the above-mentioned embodiment is applied.

[0053] In another embodiment of the manufacturing method, the constituent atoms of the catalyst precursor and the spinel oxide can be precisely controlled down to the atomic level using a coprecipitation method, and the spinel oxide particles can be manufactured to have a uniform distribution within a desired particle size range.

[0054] Another embodiment of the manufacturing method includes the steps of co-precipitating a nickel salt, a cobalt salt, and a metal (M) salt in an aqueous solvent having a pH of 11 or more in the presence of a complexing agent to form a catalyst precursor; and calcining the catalyst precursor at a temperature of 100° C. or more to form a spinel-based oxide represented by the following Chemical Formula 1:

[0055] [Chemical formula 1] Nico (2-x) M x O4 In the above chemical formula 1, 0≦x≦0.5.

[0056] The metal (M) of the metal (M) salt may be one or more elements selected from the group consisting of Fe, Sc, Ti, V, Cr, Y, Zr, Nb, and Mo.

[0057] Specifically, the temperature at which the catalyst precursor is calcined may be 100 to 500° C., or 300 to 400° C., and preferably 350° C. In other words, according to the production method according to another embodiment of the present invention, a spinel oxide and an oxidation catalyst can be produced by performing calcination at a low temperature.

[0058] This can prevent the surface area of ​​the oxidation catalyst particles from increasing or the surface defects or oxygen vacancies from being filled in the existing high-temperature solid-phase reaction and heat treatment processes, which can reduce the activity of the catalyst. However, if the heat treatment temperature is too high, the particle size of the oxidation catalyst increases, the surface area decreases, and the number of catalytic active sites decreases, which can have a negative effect on the catalytic activity.

[0059] Meanwhile, the aqueous medium having a pH of 11 or more can be prepared by sequentially adding a first pH adjuster containing ammonium hydroxide or ammonium sulfate and a second pH adjuster containing ammonium oxalate, potassium hydroxide (KOH) or sodium hydroxide (NaOH) to the aqueous medium. That is, the aqueous medium having a pH of 11 or more can be prepared by treating a neutral aqueous medium, for example, distilled water, with a plurality of pH adjusters in multiple steps.

[0060] According to a specific example, the neutral aqueous solvent is treated with a first pH adjuster containing ammonium hydroxide or ammonium sulfate to maintain a pH of 9 to 10.5, and then further treated with a second pH adjuster containing ammonium oxalate, potassium hydroxide or sodium hydroxide to obtain an aqueous solvent having a pH of 11 or more, or 13.5 or more, or 13.5 to 14. Such a multi-step process allows for more precise control of the pH required for the coprecipitation method.

[0061] In addition, in the coprecipitation step, the complexing agent is used to control the reaction rate of the coprecipitation reaction and more effectively obtain a catalyst precursor with a desired structure. A complexing agent is a molecule or ion that forms a coordinate bond around a transition metal ion to generate a complex ion. Without a complexing agent, some intermediate reactions may occur too quickly, making it difficult to suppress particle growth. From this perspective, the use of a complexing agent is necessary to match the stoichiometry in a three-component system or more.

[0062] More specifically, the complexing agent can first coordinate with the cobalt salt to form a cobalt complex compound, which then gradually reacts with the nickel salt and the metal (M) salt to produce a catalyst precursor having a desired atomic composition, uniform particle size distribution, and lattice structure according to a stoichiometric ratio, and an oxidation catalyst using the same.

[0063] The type of the complexing agent is not particularly limited, but an ammonium salt compound may be used taking into consideration appropriate reactivity with the cobalt salt, and specific examples thereof may be one or more selected from the group consisting of ammonium hydroxide (NHOH), ammonium sulfate ((NH)SO), ammonium nitrate (NHNO), and monoammonium phosphate ((NH)HPO).

[0064] For example, when ammonium hydroxide is used as the complexing agent, the reaction between the complexing agent and a cobalt salt can be carried out in two steps as shown in the following reaction scheme 2: [ka] In the above reaction scheme 2, M contains Co.

[0065] In the first step, primary particles having a nano-scale particle size can be formed, and in the second step, the primary particles are aggregated by the Ostwald ripening phenomenon to form secondary particles having a roughly micro-scale particle size. As this cobalt complex compound is formed, it gradually reacts with nickel salts and metal (M) salts, especially iron salts, to produce a catalyst precursor having a desired particle size range, uniform particle size distribution, controlled atomic composition and lattice structure.

[0066] In this coprecipitation step, Co 2+ The ions are in the air. 3+ Or Co 4+ If such oxidation and phase transition occurs, it may be difficult to control the atomic composition, particle size, and particle size distribution according to the stoichiometric ratio of the catalyst precursor. Therefore, it is preferable to carry out the coprecipitation reaction step in an atmosphere that is free of oxygen or air or in an inert atmosphere.

[0067] Meanwhile, in the coprecipitation step, the types of the nickel salt, cobalt salt, and metal (M) salt are not particularly limited, and may have the form of a general salt known to be usable in the coprecipitation reaction. However, in a more specific example, the nickel salt, cobalt salt, and metal (M) salt may have the form of an acid addition salt such as a nitrate salt in which a nitrate ion is bound to each of these metals, or a hydrate thereof.

[0068] In this manner, in the manufacturing method of another embodiment, a catalyst precursor and an oxidation catalyst can be manufactured using an acid addition salt having a relatively low unit price as a reactant, thereby improving the economic efficiency and mass productivity of the overall oxidation catalyst manufacturing process.

[0069] In addition, in the coprecipitation step, the catalyst precursor and the oxidation catalyst can be prepared by controlling the atomic composition according to the stoichiometric ratio while controlling the rate of the coprecipitation reaction as described above. Therefore, in the method according to the other embodiment, the nickel salt, the cobalt salt and the metal (M) salt can be co-precipitated at a molar equivalent ratio of 1:(2-x):x (0≦x≦0.5).

[0070] In addition, in order to form a cobalt complex compound in an appropriate ratio using the above-mentioned complexing agent and to favorably control the reaction rate, it is preferable to use the complexing agent so that the molar ratio of the metal ion of the metal salt to the complexing agent satisfies 1:0.1 to 1:1, 1:0.2 to 1:0.6, or 1:0.2 to 1:0.4.

[0071] The co-precipitation step produces a catalyst precursor containing the metal elements in the desired atomic composition. This catalyst precursor may be in the form of a hydroxide compound containing nickel, cobalt, and the metal (M), specifically iron, in the same molar ratio as the oxidation catalyst formed in the subsequent step. More specifically, the catalyst precursor may be NiCo (2-x) M x It can be produced in the form of particles containing the compound OH2 (0≦x≦0.5).

[0072] Meanwhile, after the coprecipitation reaction step, if necessary, a step of drying the catalyst precursor at a temperature of 50° C. or higher, or 50 to 100° C., or 60 to 90° C. may be further performed, and before the drying step, a step of washing the catalyst precursor at least once, or 1 to 3 times, using water such as distilled water or alcohol such as ethanol may be further performed.

[0073] After the catalyst precursor is prepared through the above-mentioned process, it may be calcined at 100 to 500°C or 300 to 400°C, preferably 350°C, in an air atmosphere to prepare an oxidation catalyst of one embodiment.

[0074] However, as already mentioned above, if the calcination temperature is excessively high, the particle size of the oxidation catalyst may become large, resulting in a small surface area. In addition, the catalytic active sites may become clogged, adversely affecting the activity of the oxidation catalyst, which is undesirable.

[0075] Through the above process, an oxidation catalyst for anion exchange membrane water electrolysis having a large surface area, excellent catalytic activity, and electrical conductivity can be economically and efficiently produced. Due to the above-mentioned excellent physical properties, such an oxidation catalyst can be preferably used as an oxidation electrode in anion exchange membrane water electrolysis system.

[0076] Specifically, it is possible to provide an oxidation electrode for anion exchange membrane water electrolysis, which includes a catalyst layer containing the above-mentioned oxidation catalyst formed on a gas diffusion layer.

[0077] In particular, the oxidation electrode for anion exchange membrane water electrolysis may have the same configuration as an oxidation electrode for a general anion exchange membrane water electrolysis system, except that it contains the oxidation catalyst of the embodiment.

[0078] Specifically, the oxidation electrode of the present invention has a concentration of 0.1 to 5 mg / cm per unit area of ​​the gas diffusion layer. 2 and preferably in an amount of 2 mg / cm 2 In the above range, the higher the content of the oxidation catalyst, the better the performance of the anion exchange membrane water electrolysis system. However, if the content of the oxidation catalyst is excessively increased, the performance of the water electrolysis system may be degraded.

[0079] Moreover, the oxidation catalyst according to one embodiment of the present invention may be formed as an oxidation catalyst layer on a gas diffusion layer, have a porous structure, and have a particle packing density of 1 g / mL or less, specifically 0.5 to 0.9 g / mL.

[0080] The thickness of the catalyst layer containing the oxidation catalyst may be increased in proportion to the content of the oxidation catalyst, and is not particularly limited. For example, the thickness of the catalyst layer may be increased to 2 mg / cm per unit area of ​​the gas diffusion layer. 2When the oxidation catalyst layer is formed with the above content, the thickness of the oxidation catalyst layer may be 4 μm or more, specifically 10 μm or more, and more specifically 10 to 20 μm.

[0081] The above-mentioned oxidation electrode can be manufactured by a general method for manufacturing an oxidation electrode for an anion exchange membrane water electrolysis system, except for the use of an oxidation catalyst according to an embodiment, and therefore, further description thereof will be omitted.

[0082] According to another embodiment of the present invention, there is provided an anion exchange membrane water electrolysis system including the oxidation electrode. Such a water electrolysis system may include an anion exchange membrane; a reduction electrode located on one side of the anion exchange membrane; and an oxidation electrode according to the other embodiment located on the other side of the anion exchange membrane layer such that a catalyst layer is in contact with the anion exchange membrane. Specifically, the anion exchange membrane water electrolysis system according to an embodiment of the present invention may be a membrane electrode assembly (MEA).

[0083] This may result in improved water electrolysis performance by including the oxidation catalyst and oxidation electrode of the previous embodiments.

[0084] Other aspects can be realized by referring to an anion exchange membrane water electrolysis system well known in the art.

[0085] In the following, preferred examples are presented to aid in understanding the invention, but the following examples are merely for the purpose of illustrating the invention and are not intended to limit the invention thereto. EXAMPLES

[0086] Comparative Example 1: Noble metal oxidation catalyst Existing commercially available IrO2 was used as the oxidation catalyst in Comparative Example 1.

[0087] Examples 1 to 7 and Comparative Examples 2 to 7: Production of NiCo(2-x)MxO4 water electrolysis oxidation catalyst The method for producing an oxidation catalyst containing a spinel oxide according to the present invention will be described below.

[0088] First, FIG. 1 shows a spinel oxide (NiCo (2-x) M x This diagram illustrates the synthesis flow of oxidation catalysts containing .

[0089] As shown in FIG. 1, first, the reactor was filled with 1-4 L of distilled water (DIW), and ammonium hydroxide (aqueous ammonia solution) was added as a first pH regulator, followed by stirring at 600 rpm or more to maintain the pH inside the reactor at 10.5. NaOH solution was added as a second pH regulator to maintain the pH inside the reactor at the values ​​shown in Table 1. If the pH is 11 or higher, leaching of the cobalt transition metal may occur, resulting in the production of a catalyst with a different composition, in which case it is difficult to realize a spinel structure and the catalytic activity is reduced.

[0090] Thereafter, an aqueous solution of ammonia (NH4OH) was mixed as a complexing agent according to Table 1 below.

[0091] Next, the molar ratio of nickel salt:cobalt salt:iron salt was controlled to prepare a metal aqueous solution with a molar ratio of 1:2-x:x, which was used as a raw material. At this time, Ni(NO3)3, Co(NO3)2, and Fe(NO3)3 were used as the metal salts and dissolved in distilled water. In Examples 1 to 5 and Comparative Examples 2 to 3, the molar ratio of x was different as shown in the composition in Table 1 below.

[0092] The mixture of the metal aqueous solution thus prepared, NaOH, and NH4OH was fed into the reactor using a metering pump. NaOH was used as a precipitant at the concentration shown in Table 1 below. Next, the reactor was stirred at a speed of 600-1000 rpm to carry out the co-precipitation reaction. The molar ratio of metal ions to ammonium hydroxide as a complexing agent was adjusted to 1:0.2-1:0.4. The co-precipitation reaction was carried out for more than 24 hours. After the reaction was completed, the precipitate was separated and washed with distilled water (DIW). It was then dried in an oven at 80°C for 12 hours.

[0093] Thereafter, the mixture was calcined in an air atmosphere under the conditions shown in Table 1 below, to produce oxidation catalysts containing spinel-based oxides of Examples 1 to 7 and Comparative Examples 2 to 7.

[0094] [Table 1]

[0095] <Experimental Example 1> SEM and TEM image measurement First, the oxidation catalysts of Comparative Examples 1 to 7 and Examples 1 to 7 were analyzed with a scanning electron microscope (SEM) and a transmission electron microscope (TEM), and the photographs are shown in Figs. 2a to 2c, respectively.

[0096] Looking at the particle image of the commercial IrO2 oxidation catalyst of Comparative Example 1 in FIG. 2a, primary particles of a few nanometers in size were agglomerated to form secondary particles of a few μm in size.

[0097] Looking at the images of oxidation catalyst particles for Comparative Examples 2 and 3 in Figure 2a, Comparative Examples 2 and 3 were synthesized using the coprecipitation method without using ammonium hydroxide as a complexing agent, with Comparative Example 2 being an oxide precursor that was not heat-treated and Comparative Example 3 being an oxidation catalyst that was heat-treated. Looking at the SEM images for Comparative Examples 3 and 4, it was confirmed that the primary particles had aggregated to form secondary particles several tens of μm in size. Large particles not only have a low surface area but also a high specific gravity, so they precipitate in the slurry process, making it difficult to uniformly disperse at high viscosity and making MEA coating difficult.

[0098] Looking at the oxidation catalyst particle images of Examples 1 to 7, excluding Comparative Example 4, in Figures 2a and 2b, Examples 2 and 4 are oxidation catalysts containing spinel oxides produced by varying only the concentrations of the complexing agent and precipitant, while Examples 1 and 3 are precursors of Examples 2 and 4, respectively, that were not heat-treated. Also, Figure 2b is a more enlarged image of the oxidation catalyst of Example 4.

[0099] Looking at the images of Examples 2 and 7, it was confirmed that primary particles containing multiple nanoflakes with a size of several hundred nm were formed, and these primary particles were aggregated to form secondary particles with a size of several μm. The catalysts of Examples 2 and 7 have a nanoflake structure and a large surface area, but since the primary particles containing multiple nanoflakes aggregate to form secondary particles with a size of several microns, no aggregation occurs during the slurry production stage. Therefore, the oxidation catalysts of Examples 2 and 7 can form a porous catalyst layer and can demonstrate excellent performance in actual cells, and since they can be uniformly dispersed at high viscosity, an additional dispersion process is not required, which can reduce the cost of MEA production.

[0100] Looking at the oxidation catalyst particle image of Comparative Example 4 in Figure 2a, Comparative Example 4 was prepared by coprecipitation without using NaOH as a precipitant, and it was confirmed that the primary particles were aggregated to form plate-shaped secondary particles of several μm in size. Comparative Example 4 has a small secondary particle size of several μm and a large surface area, and is more reactive than Comparative Examples 2 and 3. It is judged that no aggregation occurs during the slurry preparation stage, and that high viscosity uniform dispersion is possible compared to Comparative Examples 2 and 3. However, since no nanoflake structure is observed, a porous structure is not formed unlike Examples 2 and 7, and the uniform coating of the ionomer between the flakes is inferior to Examples 2 and 7. In addition, when the precipitant NaOH is not used, it is difficult to adjust the composition due to the elution of some cobalt (Co) ions.

[0101] In addition, in the case of Comparative Examples 6 and 7, which were prepared at a low pH, the lower the pH, the smaller the catalyst particles became, making it difficult to realize a nanoplate shape and form a porous structure, and it was thought that the uniform coating of the ionomer between the flakes was inferior.

[0102] FIG. 2c shows Example 4 observed by a transmission electron microscope (TEM), where the nanoflake structure could be observed more clearly.

[0103] <Experimental Example 2> XRD Measurement Figures 3a to 3c show XRD images of the oxidation catalysts. It was confirmed that the XRD peak intensity of the oxidation catalysts of Examples 2 and 4, which were prepared by the coprecipitation method of the present invention, was lower than that of Comparative Example 3. This is because nanoflake-structured particles were formed in the oxidation catalysts of Examples 2 and 4, and it was confirmed from the XRD measurement that nanoflakes were well formed in Examples 2 and 4. Similarly, in the cases of Examples 5, 6, and 7, the XRD peak intensity of the oxidation catalysts was low, confirming that nanoflake-structured particles were well formed.

[0104] <Experimental Example 3> Particle Size Distribution (PDS) Measurement Table 2 below shows the results of measuring the catalyst particle size after preparing slurries by mixing the oxidation catalysts obtained in Comparative Examples 1, 3, and 4 and Examples 2 and 4 with a solvent.

[0105] [Table 2]

[0106] In the IrO2 oxidation catalyst of Comparative Example 1, primary particles of several nm in size were agglomerated during the slurry production process, resulting in D 90 It was confirmed that particles having a standard size of 18.3 μm were formed.

[0107] NiCo synthesized by coprecipitation without using the complexing agent of Comparative Example 3 1.8 Fe 0.2 The O4 catalyst also aggregates during the slurry production process. 90 It was confirmed that particles with a standard size of 12.3 μm were formed, which is considered to be smaller than those in Comparative Example 1, but compared with Examples 2 and 4, 90 It was determined that the particles formed were approximately six times larger than the standard.

[0108] NiCo prepared by coprecipitation using the complexing agents of Examples 2 and 4 1.8 Fe 0.2 The O4 catalyst forms a nanoflake structure and is aggregated during the slurry production process, but the nanoflake structure minimizes aggregation and D 90 It was confirmed that particles with standard sizes of 2.04 μm and 2.24 μm were formed.

[0109] On the other hand, in the case of Comparative Example 4, no precipitant was used in the preparation process, and it was confirmed that aggregation occurred and large particles were formed, similar to the case where no complexing agent was used.

[0110] In the cases of Examples 5 and 6 and Comparative Examples 5 to 7, the particle size distribution was not significantly different from that of Examples 2 and 4. This indicates that the particle size is affected by the concentrations of the complexing agent and precipitant, and is not significantly affected by pH.

[0111] From these results, it can be seen that the oxidation catalyst prepared by the improved coprecipitation method of the present invention has a nanoflake structure, and particle aggregation is minimized in the slurry state, and the particle size is maintained small, making it possible to prepare a high viscosity slurry and produce a uniform catalyst layer.

[0112] <Experimental Example 4> Measurement of particle packing density (Tab Density) Figure 4 shows the tab density of the oxidation catalysts of Comparative Examples 1 and 3 and Examples 2 and 11. Tab density indicates the density at which particles are stacked, and is a value that makes it possible to predict whether the catalyst layer will be formed as porous. The lower the tab density, the more porous the catalyst layer.

[0113] The packing density of the IrO2 oxidation catalyst particles in Comparative Example 1 was 1.16 g / mL, and the NiCo 1.8 Fe 0.2 The packing density of the O4 catalyst was 1.27 g / mL.

[0114] Since there is not much difference in packing density between the oxidation catalysts of Comparative Example 1 and Comparative Example 3, it was expected that when the same weight of oxidation catalyst slurry per unit area was applied to an electrode, a catalyst layer of the same thickness would be formed.

[0115] However, the packing density of the oxidation catalyst of Example 2 was 0.89 g / mL and that of Comparative Example 4 was 0.78 g / mL. The packing density of the oxidation catalyst of Example 4 was 0.55 g / mL, respectively, which was only about 70% or 56% of the packing density of the oxidation catalyst of Comparative Example 3 prepared by the existing coprecipitation method. In other words, it was predicted that the oxidation catalysts of Examples 2 and 7 would form thicker catalyst layers than Comparative Example 3 when the same weight of oxidation catalyst slurry was applied to an electrode.

[0116] <Experimental Example 5> Observation of the surface and cross section of the catalyst coating layer The oxidation catalyst slurries of Comparative Examples 1 and 3 and Examples 2 and 4 were each 0.2 mg / cm 2 The surface and cross section of the catalyst layer coated on the electrode are shown in Figure 5. The particle size distribution of the catalyst coating layer surfaces and cross sections of Examples 6 to 11 was similar to that of Examples 2 and 4.

[0117] The catalytic layer containing the oxidation catalyst of Comparative Example 1 had a thickness of about 4.5 μm. The catalytic layer containing the oxidation catalyst of Comparative Example 3 had a thickness of about 5.6 μm, which was similar to that of Comparative Example 1. In addition, when examining the cross section and surface, the catalytic layer of Comparative Example 3 showed a very dense catalytic layer. When the catalytic layer is dense as in Comparative Example 3, not only is ionomer coating difficult, but the oxidation reaction may occur only on the surface of the catalytic layer, resulting in reduced performance.

[0118] The catalytic layers containing the oxidation catalysts of Examples 2 and 4 had thicknesses of approximately 10 μm and 18 μm, respectively. It can be seen that the catalytic layers were more than twice as thick as those of Comparative Examples 1 and 2, even though the same amount of oxidation catalyst slurry was applied per unit area. Furthermore, by observing the surface and cross section of the catalytic layers containing the oxidation catalysts of Examples 2 and 4, it was found that they were formed as porous catalytic layers. The porous catalytic layer is easy to coat with ionomer, and it is easy to adsorb reactants and desorb products, resulting in good reaction efficiency. In addition, it has excellent performance as the entire inside of the coating layer can participate in the oxidation reaction.

[0119] <Experimental Example 6> Evaluation of catalyst specific surface area Figure 6 shows the results of measuring the specific surface area of ​​the catalyst. The commercial IrO2 catalyst has a specific surface area of ​​25.5 m 2 / g, and in the case of Comparative Example 3 where no complexing agent was used, the measured value was 107.8 m 2 On the other hand, the catalyst of Example 4 synthesized by the coprecipitation method of the present invention was measured to have a value of 225.8 m 2 / g. This is 8.8 times higher than that of existing commercial catalysts and approximately 2 times higher than that of Comparative Example 3. Since the larger the surface area, the more catalytic active sites there are, the higher the efficiency of water electrolysis can be expected when using the catalyst of the present embodiment.

[0120] <Experimental Example 7> Single cell evaluation Single cells containing the oxidation catalysts of Comparative Examples 1 and 3 and Examples 2 and 4 were fabricated, and their electrochemical performance was evaluated and shown in FIG.

[0121] The single cell structure was based on the fabricated MEA, with the cathode and anode parts each having a gas diffusion layer (GDL), bipolar plate, current collector, and end plate formed symmetrically. The gas diffusion layer of the cathode was made of 300μm thick carbon paper coated with MPL, and the gas diffusion layer of the anode was made of 370μm thick Ti felt. The bipolar plate was made of Ni plate, the flow channel was formed in a serpentine shape with a depth of 1mm, and the bipolar plate was 3mm thick. The end plate was 3mm thick and made of Ni. The gasket was made of 250μm thick Teflon sheet.

[0122] The catalyst coating ink was made of a mixed solvent of 90wt% IPA and 10wt% DIW, and the catalyst for evaluation was prepared using the sonication method at a content of about 1wt%, and the ionomer was a Fumatech product added at a content of 30% relative to the catalyst.

[0123] The MEA was manufactured using a Sono spray coater at a substrate temperature of 50° C. and an oxidation catalyst loading of 2 mg / cm for Comparative Examples 1 and 3 or Examples 2 and 4. 2The reduction electrode catalyst was TKK Pt / C (Pt 40wt%) prepared in the same manner and the loading amount was 0.4mg / cm 2 was adjusted to.

[0124] The membrane used is Fumatech FAA-3-50, with an effective active area of ​​5cm 2 It was.

[0125] The fabricated MEA was dried at 70℃ for about 2 minutes and then used for assembling a single cell. The clamping pressure was set to 70 IN.LB during assembling the single cell.

[0126] The assembled single cell was installed in the electrolysis station and preheated for 30 minutes, after which electrolysis was evaluated with a linear sweep scenario at intervals of 0.01V / 10sec from 1.45V to 2.1V. The electrolyte used was KOH 1M, the flow rate was 90ml / min, the cell temperature was 60℃, and the pressure was normal pressure. The results are shown in Figure 9.

[0127] The oxidation catalyst of Comparative Example 1 had a current of 0.52 A / cm at 1.7 V. 2 , 1.34A / cm at 1.9V 2 , 2.25A / cm at 2.1V 2 The oxidation catalyst of Comparative Example 3 showed 0.71 A / cm at 1.7 V. 2 , 1.89A / cm at 1.9V 2 , 3.31A / cm at 2.1V 2 showed.

[0128] As mentioned above, Comparative Example 1 showed a similar degree of catalyst layer density and thickness to Comparative Example 3, but still showed inferior catalytic performance.

[0129] Examples 2 and 4 showed better electrochemical performance than Comparative Examples 1 and 3.

[0130] Specifically, Example 4 has a current of 0.96 A / cm at 1.7 V. 2 , 2.4A / cm at 1.9V2 , 4.0A / cm at 2.1V 2 Compared with Comparative Example 1, Example 4 showed an improvement of 84% at 1.7 V, 79% at 1.9 V, and 78% at 2.1 V, showing an overall improvement of 78 to 84%.

[0131] From the above results, NiCo 1.8 Fe 0.2 Not only is the activity of the O4 oxidation catalyst itself superior to that of commercial IrO2 oxidation catalysts, but when manufactured by the improved manufacturing method of the present invention, secondary particles having a nanoflake structure are formed to form a porous catalyst layer, resulting in even better catalytic performance.In addition, the oxidation catalyst manufactured by the improved manufacturing method of the present invention has suppressed particle aggregation in a slurry state, allowing for uniform catalyst dispersion at high viscosity, eliminating the need for a subsequent process for dispersion and reducing manufacturing costs.

Claims

1. The spinel-based oxide has the following formula 1: The spinel-based oxide has a nanoflake structure, and is an oxidation catalyst for anion exchange membrane water electrolysis: [Chemical formula 1] NiCo (2-x) M x O 4 In the above formula 1, 0≦x≦0.

5.

2. 2. The oxidation catalyst for anion exchange membrane water electrolysis according to claim 1, wherein in Formula 1, M is one or more elements selected from the group consisting of Fe, Sc, Ti, V, Cr, Y, Zr, Nb, and Mo.

3. The nanoflake structure is a plate-shaped structure, The length of the long side is 300 nm or less, and the surface area is 150 m 2 The oxidation catalyst for anion exchange membrane water electrolysis according to claim 1, wherein the oxidation catalyst has a molecular weight of 1.0 to 1.0 mol / g or more.

4. The spinel oxide is The secondary particles are formed by agglomeration of primary particles. The primary particles include single or multiple nanoflake structured particles, and have a particle size (D 50 2. The oxidation catalyst for anion exchange membrane water electrolysis according to claim 1, wherein the average particle diameter is 500 nm or less.

5. The secondary particles are D 50 The oxidation catalyst for anion exchange membrane water electrolysis according to claim 4, wherein the catalyst has a particle size of 3 μm or less and a monodisperse particle size distribution.

6. co-precipitation of a nickel salt, a cobalt salt and a metal (M) salt in the presence of a complexing agent in an aqueous medium having a pH of 11 or greater to form a catalyst precursor; and A method for preparing an oxidation catalyst for anion exchange membrane water electrolysis, comprising calcining the catalyst precursor at a temperature of 100° C. or more to form a spinel-based oxide represented by Chemical Formula 1: [Chemical formula 1] NiCo (2-x) M x O 4 In the above formula 1, 0≦x≦0.

5.

7. The aqueous medium having a pH of 11 or more is a first pH adjuster comprising ammonium hydroxide or ammonium sulfate; 7. The method for producing an oxidation catalyst for anion exchange membrane water electrolysis according to claim 6, wherein the oxidation catalyst is formed by sequentially adding a second pH adjuster containing ammonium oxalate, potassium hydroxide (KOH) or sodium hydroxide (NaOH) to an aqueous solvent.

8. The complexing agent is ammonium hydroxide (NH 4 OH), ammonium sulfate (NH 4 ) 2 SO 4 ), Ammonium nitrate (NH 4 NO 3 ) and ammonium phosphate monobasic ((NH 4 ) 2 H.P.O. 4 The method for producing an oxidation catalyst for anion exchange membrane water electrolysis according to claim 6, wherein the oxidation catalyst comprises at least one selected from the group consisting of:

9. 7. The method for producing an oxidation catalyst for anion exchange membrane water electrolysis according to claim 6, wherein the nickel salt, the cobalt salt and the metal (M) salt are co-precipitated in a molar equivalent ratio of 1:(2-x):x (0≦x≦0.5).

10. 7. The method for producing an oxidation catalyst for anion exchange membrane water electrolysis according to claim 6, wherein in Chemical Formula 1, the metal (M) of the metal (M) salt is one or more elements selected from the group consisting of Fe, Sc, Ti, V, Cr, Y, Zr, Nb, and Mo.

11. The method for producing an oxidation catalyst for anion exchange membrane water electrolysis according to claim 6, wherein the nickel salt, the cobalt salt and the metal (M) salt are each in the form of an acid addition salt of a metal or a hydrate thereof.

12. 13. An oxidation electrode for anion exchange membrane water electrolysis, comprising a catalyst layer comprising the oxidation catalyst of claim 1 formed on a gas diffusion layer.

13. The oxidation catalyst is present in an amount of 0.1 to 5 mg / cm per unit area of ​​the gas diffusion layer. 2 The oxidation electrode for anion exchange membrane water electrolysis according to claim 12, wherein the anion exchange membrane water electrolysis oxidation electrode comprises:

14. Polyelectrolyte layer; a reduction electrode located on one side of the polyelectrolyte layer; and 13. An anion exchange membrane water electrolysis system comprising the oxidation electrode of claim 12 located on the other side of the polymer electrolyte layer such that a catalyst layer is in contact with the polymer electrolyte layer.

Citation Information

Patent Citations

  • Method for preparing Ni / NiCo2O4 porous composite electrode for alkaline medium oxygen evolution

    CN102605386A

  • Electrode clad with catalyst, showing weak overvoltage to release oxygen and useful for water electrolysis particularly in alkaline medium

    JP1983136789A

  • Plate single crystal composed of metal oxide, thin film of the metal oxide, production methods for the single crystal and the film and variable-resistance element using the single crystal or the film

    JP2012188315A

  • Alkaline water electrolysis method

    JP2017119895A

  • Cathode for metal-air battery, method of manufacturing the same, and metal-air battery comprising the same

    US20170271684A1