Solid Electrolyte
A zeolite-polymer binder-ionic conductor composition addresses leakage and stability issues in solid electrolytes, providing enhanced conductivity and safety for all-solid-state batteries.
Patent Information
- Application Number
- JP2024519618
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-01
- Filing Date
- 2022-09-30
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2042-09-30
AI Technical Summary
Existing solid electrolytes in all-solid-state batteries face challenges such as leakage risk, mechanical instability, low conductivity at low temperatures, limited electrochemical stability, and flammability, which compromise safety and performance.
A solid electrolyte composition combining zeolite crystals with a polymeric binder and an ionic conductor, where zeolite crystals are agglomerated by a polymer binder to form a solid reservoir for ionic conductors, enhancing mechanical strength, flexibility, and conductivity.
The composition achieves electrical conductivity comparable to liquid electrolytes, with improved mechanical stability, safety, and resistance to dendrite growth, enabling high electrochemical stability and reduced flammability, suitable for use in all-solid-state batteries.
Smart Images

Figure 2024537072000001 
Figure 2024537072000002 
Figure 2024537072000003
Abstract
Description
[Technical field]
[0001] The present patent application relates to the field of electrical energy storage in batteries, more particularly secondary batteries, more particularly secondary batteries of the Li-ion type, in particular lithium batteries with solid electrolyte, also known as all-solid-state batteries. [Background technology]
[0002] Research in the field of batteries, especially secondary batteries, and developments in this field over the past decades have been and remain very significant in terms of the number of players and the amounts of money involved.
[0003] Rechargeable or secondary batteries have an advantage over primary (non-rechargeable) batteries because the relevant chemical reactions that occur at the positive and negative electrodes of the battery are reversible. The electrodes of a secondary cell can be regenerated several times by applying an electric charge. This is why many electrode systems have been developed to store the electric charge. In parallel, a great deal of effort has been put into the development of electrolytes that can improve the capacity of electrochemical cells.
[0004] Typically, a battery includes at least one negative electrode (or anode) bonded to a copper current collector, a positive electrode (or cathode) bonded to an aluminum current collector, a separator, and an electrolyte. The electrolyte consists, for example, of a lithium salt, which in the case of Li-ion batteries is typically lithium hexafluorophosphate, mixed with a solvent, typically a mixture of organic carbonates, selected to optimize ion transport and dissociation. A high dielectric constant favors ion dissociation and thus the number of ions available in a given volume, and a low viscosity favors ion diffusion, which, among other parameters, plays an important role in the charge and discharge rates of electrochemical systems.
[0005] A typical Li-ion battery therefore comprises a liquid electrolyte, most often based on a solvent, a lithium salt and an additive. Considering the increasing use of this type of battery in the field of electronic consumer products in general, such as computers, tablets or mobile phones (smartphones), but also in the field of transportation, especially with electric vehicles, it is a major challenge to improve the safety of these lithium batteries and to reduce their manufacturing costs.
[0006] In particular, liquid electrolytes offer the advantage of good ionic conductivity, but have the drawback of leaking (spilling) of the fluid in case of mechanical and / or chemical damage to the battery, which is usually harmful since it not only leads to malfunction or even failure of the battery, but also to contamination and degradation, especially due to corrosion or even fire and / or explosion of the battery.
[0007] To solve this problem, in recent years, "all-solid-state" batteries containing solid polymer electrolytes (the most common being SPE, short for Solid Polymer Electrolytes) have been considered as an alternative to flammable liquid electrolytes. SPE, which is a solid polymer electrolyte, does not contain a liquid solvent and therefore avoids the use of flammable liquid components as in conventional Li-ion batteries, making it possible to manufacture thinner and more flexible batteries.
[0008] Besides SPEs, there are also solid-state batteries mainly composed of oxides or phosphates, which show great potential for both small-scale applications, e.g., 3D microbatteries, and large-scale energy storage applications, e.g., for electric vehicles.
[0009] Also, to provide the expected performance, the ionic conductivity of the solid electrolyte present in such solid-state batteries must be at least comparable to that of the liquid electrolyte, i.e., 10 at 25 °C as measured by electrochemical impedance spectroscopy. -3 S.cm -1The electrochemical stability must allow the electrolyte to be used in areas where high energy density is required, such as in the automotive industry, with cathode materials that can function at high voltages, especially voltages above 4.4 V. Finally, the solid electrolyte must have a certain resistance to fire or cell runaway, i.e. it must be able to function without any serious problems up to at least 80 ° C and must not ignite below 130 ° C.
[0010] Solid electrolytes therefore remain the subject of intensive research to overcome the drawbacks listed above. Inorganic materials such as oxides, phosphates and ceramics have a thermal conductivity of 10 -3 S.cm -1 Although they have electrical conductivity up to 1000 Å (order of magnitude of that of liquid electrolytes), they can be very hard or even brittle. As a result, they do not cope well with the volume changes that electrodes undergo during cycling, which can lead to loss of contact between the electrode and the solid electrolyte.
[0011] Other inorganic materials, thiophosphates (see ACS Energy Lett., (2020), 5(10), 3221-3223), have better electrical conductivity (10 -2 S.cm -1 up to 10000 kPa), which can exceed the conductivity of liquid electrolytes. However, thiophosphates are also relatively rigid and have a low electrochemical stability window, but above all they are very unstable with respect to water and release hydrogen sulfide (H2S) in case of accidental opening of the cell, which is unacceptable not only for obvious reasons of environmental protection but above all in terms of user safety.
[0012] Another possible solution is to use polymers, which, due to their high flexibility, would most likely be able to cope with the variations in electrode volume during cycling and avoid the risk of fracture at the electrode / electrolyte interface. However, in certain cases, polymers suffer from somewhat limited electrochemical stability, notably a low electrical conductivity, which is less than 10 at 25 °C. -4 S.cm -1 It is often less than that.
[0013] To overcome this low ionic conductivity at room temperature, as well as to further improve the mechanical properties, it has been proposed to add mineral filler type materials, such as zeolites (LZ Fan, H. He, CW Nan, "Tailoring inorganic-polymer composites for the mass production of solid-state batteries", Nat. Rev. Mater., (2021), https: / / doi.org / 10.1038 / s41578-021-00320-0). The term "active filler" is used when the filler is a lithium ion conductor (e.g. LATP - lithium aluminum titanium phosphate, LLZO - lithium lanthanum zirconium oxide, lithium zeolite, etc.), and "inactive filler" is used when it is not an ion conductor (SiO2, Al2O3, etc.). Solid electrolytes consisting of polymer / mineral filler composites are called hybrid solid electrolytes.
[0014] At the moment, the most commonly used polymers as solid polymer electrolytes are polyethers, such as poly(ethylene oxide), also known as PEO. However, these polymers have the drawback of easily crystallizing, especially at temperatures close to room temperature, which has the effect of very significantly reducing the ionic conductivity of the polymer. This is why these polymers allow the use of batteries that are inserted only at a minimum temperature above their glass transition temperature, for example above 60°C. However, it would be convenient to be able to use such batteries at room temperature and even at negative temperatures, typically -20°C or even lower. Furthermore, these PEOs are highly hydrophilic and have a tendency to plasticize, especially in the presence of lithium salts, which reduces their mechanical stability. Finally, poly(ethylene oxide) monomers are known to be lethal by inhalation, making the use of this product harmful to health.
[0015] Polymer electrolytes make it possible to guarantee mechanical stability during the charge / discharge cycles of the battery, to preserve the cohesion between the electrolyte and the electrodes, without compromising the ionic conductivity by excessively long chains, and to guarantee electrical insulation between the two electrodes during the volume changes related to the insertion / deinsertion of lithium. Until now, to solve this problem of size stability, especially with PEO, it was necessary to produce polymers with very long chains in order to obtain chain entanglements and ensure the mechanical stability of the electrodes. However, this increase in the molecular weight of the polymer impairs its chain mobility, its glass transition temperature and its ionic conductivity.
[0016] Thus, in order to obtain a highly efficient battery, in order to obtain a polymer that is a good ionic conductor even at room temperature or at low temperatures, typically between -20°C and +80°C, it is firstly necessary to minimize its crystallinity, so that it cannot crystallize at the operating temperature of the battery, which would weaken the ionic conductivity, and secondly, it is necessary to have a glass transition temperature that is as low as possible, lower than the operating temperature of the battery, so that the polymer does not have a glassy state at the operating temperature of the battery, which would itself tend to weaken the ionic conductivity.
[0017] As mentioned above, another component of a conventional Li-ion battery (with liquid electrolyte) is the separator, which is located between the two electrodes and acts first as a mechanical and electronic barrier and second as an ionic conductor. There are several categories of separators that can be referred to by the collective term separator: dry polymer membranes, gelled polymer membranes, and microporous or macroporous separators soaked in liquid electrolyte.
[0018] The separator market is currently dominated by the use of polyolefins (e.g., those sold under the most common names by Celgard, Asahi Kasei, Toray, Sumitomo Chemical and SK Innovation), generally produced by extrusion and / or stretching. The separator must simultaneously have a low thickness, an optimal affinity for the electrolyte, and sufficient mechanical strength. Among the most advantageous alternatives to polyolefins, polymers with a better affinity for standard electrolytes have been proposed to reduce the internal resistance of the system, such as poly(vinylidene fluoride) (PVDF) and poly(vinylidene fluoride-hexafluoropropene) (P(VDF-co-HFP)).
[0019] Dry polymer membranes, free from liquid solvents, avoid the use of flammable liquid components as in conventional Li-ion batteries and allow the production of thinner and more flexible batteries. However, they have properties significantly inferior to those of liquid electrolytes, especially with regard to ionic conductivity. To function in the high regime, for example for mobile phones, for fast charging, especially for electric vehicles, or for power applications, for example for power tools, good electrical conductivity is required.
[0020] Gelled dense membranes also constitute an alternative to separators soaked with liquid electrolyte. The term "dense membrane" refers to membranes that no longer have free porosity. They are swollen with solvents, which are strongly chemically bound to the membrane material and have lost all of their solvation properties. The solute then passes through the membrane without entraining any solvent. In the case of these membranes, the free spaces correspond to those left between the membranes by the polymer chains and have the size of simple organic molecules or hydrated ions. The main drawback of these gelled membranes is that they contain large amounts of flammable solvents. Another drawback that can be mentioned is that they lose their mechanical properties after swelling, which impairs the easy handling of the separators for cell manufacture and their good resistance to mechanical stresses during the charge / discharge cycles of the battery.
[0021] US5296318 describes a separator based on a VDF-HFP copolymer swollen in an electrolyte consisting of a mixture of lithium salts (LiPF6) and carbonates as solvents. The examples described use Kynar Flex® 2801 and Kynar Flex® 2750, which contain 12% and 15% by weight of HFP, respectively. More generally, the patent describes an optimum HFP content of 8% to 25% by weight of HFP. Below 8% HFP, the authors mention difficulties associated with the use of the membrane. Above 25%, the mechanical strength after swelling is insufficient. The process for producing the separator is a solvent-based process, which involves the use of tetrahydrofuran, a very volatile solvent. The ionic conductivities reported in examples 1 and 2 are 0.3 mS.cm, respectively. -1 and 0.4 mS.cm -1 It is.
[0022] The document describes the need to use an additional crosslinking step for separators based on VDF-HFP copolymers with an HFP content of more than 25% by weight in order to enhance the mechanical strength after swelling. These copolymers give satisfactory results even after heating up to 70° C. However, the copolymers swollen under the influence of a solvent are soluble in liquid electrolytes at temperatures above 80° C. If the electrolyte membrane melts under certain stress, the electrolyte can flow and cause a short circuit inside the battery, leading to rapid discharge and heating.
[0023] To solve this problem, US2019 / 0088916 proposes a non-porous separator that contains a polymeric material that can be gelled with an organic solvent in an electrolyte solution, forming a polymeric gel electrolyte by the addition of the electrolyte solution. This non-porous separator contains at least one synthetic polymeric compound or one natural polymeric compound, and also contains, as a matrix, at least one polymeric material that cannot be gelled with an organic solvent. The examples show that the non-gelling polymer is used in the form of a porous membrane impregnated with a solution of a gellable polymer. This approach therefore imposes complex steps for producing a porous membrane of a non-gellable polymer, which makes it possible to control the porosity and the nature of the porosity (pore size and open porosity). Furthermore, this manufacturing process requires the use of a solvent-based step to impregnate the pores of the porous membrane, which has the disadvantage of using a solvent and requires an evaporation step.
[0024] International patent application WO2020 / 0127454 relates to the aqueous dispersion polymerization of monomers containing VF2 using RAFT / MADIX technology. More specifically, said document describes a composition containing a non-electroactive mineral filler, which may be zeolite or silica, for producing a separator after a drying step of the dispersion.
[0025] A study by X. Chi et al. (Nature, Vol. 592, (2021), 551-571), in the context of batteries based on Li-air technology, proposes a continuous membrane obtained by grafting carbon nanotubes (CNTs) onto a steel mesh followed by seed growth of LiX zeolite on the CNTs. The zeolite is preferentially produced in situ by crystal growth directly on the CNTs. It is therefore a hybrid system combining steel, carbon nanotubes and zeolite, the manufacture of which on an industrial scale seems relatively difficult and therefore expensive. Moreover, the mechanical strength of this hybrid system may prove to be insufficient or even inadequate, taking into account that cracks may lead to lithium dendrites, which may cause a short circuit in the battery.
[0026] Other documents in the scientific and patent literature describe the presence of zeolites in Li-ion batteries, for example as a component of the separator, usually as an adsorbent for undesirable molecules such as water or acids, but also as a coating on the separator itself to enhance its mechanical properties. In this configuration, it is thus a porous separator for lithium-ion batteries with liquid or gel electrolyte, consisting of a film of a porous polymer (for example polypropylene) with a surface layer of zeolite, the adhesion between the porous polymer and the zeolite being usually ensured by another polymer, for example PVDF.
[0027] Patent US5728489 describes a liquid electrolyte comprising a polymer matrix whose structural integrity can be reinforced with a lithiated zeolite present in an amount between 1% and 30% by weight of the liquid electrolyte. As mentioned above, liquid electrolyte batteries are unsatisfactory in that they can be subject to leakage of said liquid electrolyte.
[0028] CN104277423 describes a material for reducing the operating temperature of a battery, which is thermally conductive and flame retardant, and includes a mixture of a mineral filler with a small amount of zeolite, and the mixture is subjected to sintering with a ceramic filler.CN201210209283 describes a solid electrolyte including polyoxyethylene or a derivative thereof, a lithium salt, and an organic / mineral hybrid framework selected from a metal / organic framework (MOF), a covalent / organic framework (COF), and a zeolite / imidazole framework (ZIF).
[0029] Thus, there remains a need for solid-state batteries that do not suffer from the drawbacks previously envisioned and known today. [Prior art documents] [Patent documents]
[0030] [Patent Document 1] U.S. Pat. No. 5,296,318 [Patent Document 2] US Patent Application Publication No. 2019 / 0088916 [Patent Document 3] International Publication No. 2020 / 0127454 [Patent Document 4] U.S. Pat. No. 5,728,489 [Patent Document 5] China Patent Publication No. 104277423 [Patent Document 6] China Patent Application Publication No. 201210209283 [Non-patent literature]
[0031] [Non-Patent Document 1] ACS Energy Lett., (2020), 5(10), 3221-3223 [Non-Patent Document 2] LZFan, H.He, CWNan, "Tailoring inorganic-polymer composites for the mass production of solid-state batteries", Nat.Rev.Mater., (2021), https: / / doi.org / 10.1038 / s41578-021-00320-0 [Non-Patent Document 3] X. Chi et al., Nature, Vol. 592, (2021), 551-571 Summary of the Invention [Problem to be solved by the invention]
[0032] It is therefore a first object of the present invention to propose a solid electrolyte for producing all-solid-state batteries that are free from the risk of leakage in case of mechanical damage to the battery. As a further subject, the present invention proposes a solid electrolyte for producing electrodes that have a satisfactory mechanical stability, and more particularly a satisfactory size stability, in order to avoid loss of cohesion and loss of adhesion to the metal current collector.
[0033] Another object of the present invention is to provide a thermoplastic polymer having a satisfactory conductivity even at low temperatures, typically below 80° C., which may go down to −20° C. or even −30° C., and in particular a conductivity comparable to or even higher than that of liquid electrolytes, e.g. -3 S.cm -1 Another objective is to propose a solid electrolyte with a high chemical stability (electrochemical stability) at voltages typically above 4.4 V.
[0034] Another object of the invention is to propose a process for the manufacture of a solid electrolyte that is fast, easy and cheap to carry out, makes it possible to avoid the formation of dendrites, is anhydrous, makes it possible to eliminate the risk of degradation, and allows the manufacture of systems with the lowest possible amount of volatile compounds, so as to eliminate the risk of fire. Another object is to propose a solid electrolyte that has good fire resistance, in particular with limited or no risk of fire at temperatures below 120° C. Another object is to propose a solid electrolyte that maintains good resistance to runaway, in particular electrical properties, in particular electrical conductivity properties, under operating conditions, for example at temperatures up to about 80° C. Further objects will become clear in the light of the description of the invention presented below. [Means for solving the problem]
[0035] The present invention therefore relates to the field of electrochemical devices, in particular lithium ion batteries, and more particularly all-solid-state lithium batteries. More particularly, the present invention relates to a solid electrolyte composition for use in such batteries, in particular in the separator and / or in the cathode (catholyte) and / or in the anode (anolyte). The present invention also relates to a process for the manufacture of such a composition, in particular intended for the manufacture of an all-solid-state lithium battery. More particularly, this composition is intended for the manufacture of a separator for such batteries. The present invention also relates to a battery separator comprising such a solid electrolyte composition and a process for its manufacture.
[0036] The inventors have now discovered that it is possible to achieve at least some, if not all, of the above objectives by means of the present invention, which is detailed below and which notably makes it possible to combine both the advantages of liquid electrolytes, in particular with regard to electrical conductivity, and the advantages offered by solid electrolytes, in particular with regard to stability and the absence of any risk of leakage.
[0037] Thus, according to a first aspect, the present invention provides a method for producing a method for treating a cancer cell comprising: A / one or more zeolite crystals; B / at least one polymer binder, the amount of which is between 0.5% and 20% by weight, preferably between 1% and 10% by weight, relative to the total weight of the zeolite crystals and the binder; and C / at least one ionic conductor containing at least one lithium salt The present invention relates to a composition comprising: DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] Unless otherwise indicated in this disclosure, ranges of values are understood to be inclusive of the limits.
[0039] The present invention therefore relates to a solid electrolyte in which immobilized zeolite crystals are combined with a polymer binder to provide cohesion to the solid electrolyte, as well as mechanical strength and flexibility, making it perfectly suitable for use in batteries. Furthermore, the zeolite crystals bound by the polymer binder act as a reservoir for the ionic conductor, thus ensuring electrical conductivity perfectly suitable for use in batteries, especially secondary batteries. In other words, the ionic conductor of the composition according to the invention is contained in the solid combination of zeolite crystals + polymer binder (inside and on the surface).
[0040] In prior art solid electrolytes, when zeolites are present, they are used to trap undesirable elements such as water (moisture) rather than forming a solid three-dimensional network capable of supporting ionic conductors. Moreover, in the prior art, the proportion of zeolites in the solid electrolyte is always low or even very low.
[0041] The zeolite crystals that can be used in the present invention can be crystals of one or more zeolites, either the same or different. The term "zeolite" refers to a specific negatively charged ceramic with an aluminosilicate framework, whose electrical neutrality is ensured by one or more counter cations.
[0042] Examples of zeolite crystals that are perfectly suitable for use in the present invention include crystals of one or more zeolites selected from natural or synthetic zeolites, more specifically natural zeolites. More specifically, the zeolites are selected from faujasite (FAU), MFI zeolite, chabazite (CHA), heulandite (HEU), Linde A-type (LTA) zeolite, EMT zeolite, beta zeolite (BEA), mordenite (MOR), and mixtures thereof. These different types of zeolites are clearly defined, for example, in the "Atlas of Zeolite Framework Types", 5th Edition, (2001), Elsevier, and are readily commercially available to those skilled in the art or are easily synthesized by known procedures available in the scientific and patent literature.
[0043] For the purposes of the present invention, it is also possible to use hierarchically porous homologues of the abovementioned zeolites (known as "HPZ"), which are generally obtained by direct synthesis, as described for example in patent applications WO2015 / 019013 or WO2007 / 043731, in particular by using sacrificial agents, or by post-treatment, as described for example in WO2013 / 106816.
[0044] Preferably, the zeolite crystals are crystals of one or more zeolites selected from faujasites, preferably Y, X, MSX or LSX type faujasites, entirely preferably X, MSX or LSX type faujasites, more preferably MSX or LSX type faujasites, and entirely preferably LSX type faujasites. These different types of faujasites are characterized by their silicon / aluminium (Si / Al) molar ratio, which is well known to the skilled person and can be measured according to the indications given in the characterization techniques described later in this specification. LSX type faujasites are characterized by a Si / Al molar ratio equal to about 1.00±0.05. MSX type faujasites are characterized by a Si / Al molar ratio between 1.05 and 1.15, X type faujasites are characterized by a Si / Al molar ratio between 1.15 and 1.50, and Y type faujasites are characterized by a Si / Al molar ratio greater than 1.50. For reasons of homogeneity it is preferred to use only one type of zeolite, preferably a faujasite type zeolite.
[0045] The countercation used to neutralize the zeolite may be any cation known to those skilled in the art, for example a hydronium ion, an organic cation (imidazolium, pyridinium, pyrrolidinium, etc.), an alkali metal cation, an alkaline earth metal cation, a transition metal cation, a rare earth metal cation, in particular a lanthanum cation, a praseodymium cation, a neodymium cation, and also a cation selected from a mixture of two or more of the cations listed above. For the purposes of the present invention, when the solid electrolyte is particularly suitable for the preparation of lithium ion batteries, preferred zeolites are those in which the countercation is a lithium cation, optionally with a hydronium cation and / or one or more other alkali metal or alkaline earth metal cations, such as a sodium cation, a potassium cation, a rubidium cation, a cesium cation, a magnesium cation, a calcium cation, a strontium cation or a barium cation, and mixtures thereof, which cations are preferably present in a negligible amount relative to the lithium cation, for example less than 5% of the exchangeable sites according to the indications given in the characterization techniques described below.
[0046] According to a preferred embodiment of the invention, the countercation of the zeolite is lithium in an amount of more than 95%, preferably more than 98%, more preferably more than 99% of the exchangeable sites, as shown below, and other countercations necessary for the neutrality of the zeolite are advantageously alkali and alkaline earth metal cations, rare earth metal cations, and transition metal cations, such as titanium, zirconium, hafnium, rutherfordium, and hydronium cations, as well as mixtures of the abovementioned cations.
[0047] According to a most particularly advantageous embodiment, the composition of the invention comprises an LSX-type faujasite zeolite, the countercation of which is lithium in an amount greater than 95% of the exchangeable sites, this zeolite being commonly designated "LiLSX".
[0048] The size and size distribution of the zeolite crystals present in the composition according to the invention can vary in wide proportions. However, it is preferred that the size of the crystals, evaluated by scanning electron microscope (SEM) observations as shown later in the characterization technique, is between 0.02 μm and 20.00 μm, more preferably between 0.02 μm and 10.00 μm, more preferably between 0.03 μm and 5.00 μm, and advantageously between 0.05 μm and 1.00 μm. According to a most particularly preferred embodiment, the size distribution of the crystal sizes is monomodal, bimodal or polymodal, preferably bimodal.
[0049] The composition according to the invention is a solid composition and is advantageously anhydrous, i.e. free of water or having only trace amounts of water, i.e. less than 1000 ppm by volume, preferably less than 100 ppm and better still less than 50 ppm.
[0050] In the composition according to the invention, which is a solid composition, the polymeric binder ensures the aggregation of the zeolite crystals. The polymeric binder is very advantageously electrochemically stable, i.e. it does not decompose or otherwise degrade under voltage, so that the physical integrity and electrochemical properties of the battery components are maintained, especially when exposed to the battery operating temperatures and voltages, typically ranging from -20°C to +80°C, typically voltages above 4.4V. Examples of polymers most suitable for the purposes of the present invention include, but are not limited to, fluoropolymers (PVDF, PTFE), carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), polyacrylic acid (PAA) and its esters, polyimides, etc., preferably fluoropolymers including optionally functionalized fluorinated homopolymers and optionally functionalized fluorinated copolymers.
[0051] Among the fluoropolymers, poly(vinylidene fluoride), better known by the abbreviation PVDF, is preferred. Also preferred are copolymers of vinylidene fluoride (VDF) with at least one VDF-compatible comonomer. The term "VDF-compatible comonomer" means a comonomer that may be halogenated (fluorinated and / or chlorinated and / or brominated) or not, and that is polymerizable with VDF.
[0052] Non-limiting examples of suitable comonomers include vinyl fluoride, 1,2-difluoroethylene, trifluoroethylene, tetrafluoroethylene, hexafluoropropylene, trifluoropropene, in particular 3,3,3-trifluoropropene, tetrafluoropropene, in particular 2,3,3,3-tetrafluoropropene or 1,3,3,3-tetrafluoropropene, hexafluoroisobutylene, perfluorobutylethylene, pentafluoropropene, in particular 1,1,3,3,3-pentafluoropropene or 1,2,3,3,3-pentafluoropropene, perfluoroalkyl vinyl ethers, in particular those of the general formula Rf-O-CF=CF2, where Rf is an alkyl group preferably containing 1 to 4 carbon atoms (preferred examples are perfluoropropyl vinyl ether and perfluoromethyl vinyl ether). The comonomers may contain, in addition to fluorine, one or more chlorine and / or bromine atoms. Such comonomers may be selected in particular from bromotrifluoroethylene, chlorofluoroethylene, chlorotrifluoroethylene and chlorotrifluoropropene. Chlorofluoroethylene can represent either 1-chloro-1-fluoroethylene or 1-chloro-2-fluoroethylene. The 1-chloro-1-fluoroethylene isomer is preferred. The chlorotrifluoropropene is preferably selected from 1-chloro-3,3,3-trifluoropropene and 2-chloro-3,3,3-trifluoropropene, and mixtures thereof.
[0053] According to a preferred embodiment, the comonomer is selected from vinyl fluoride, trifluoroethylene, chlorotrifluoroethylene (CTFE), 1,2-difluoroethylene, tetrafluoroethylene (TFE), hexafluoropropylene (HFP), perfluoro(alkyl vinyl) ethers, such as perfluoro(methyl vinyl) ether (PMVE), perfluoro(ethyl vinyl) ether (PEVE), perfluoro(propyl vinyl) ether (PPVE), and mixtures thereof.
[0054] According to one embodiment, the VDF copolymer is a terpolymer. According to one embodiment, the polymer binder is a copolymer of vinylidene fluoride (VDF) and hexafluoropropylene (HFP), more commonly known as P(VDF-co-HFP). Advantageously, said P(VDF-co-HFP) copolymer has a mass content of HFP of 5% to 45%.
[0055] According to a preferred embodiment of the present invention, the polymer binder is not soluble in the ion conductor. According to another preferred embodiment, the polymer binder is a fluoropolymer, preferably the polymer is selected from PVDF, which may be functionalized, and PVDF-based copolymers, which may be functionalized. It is clearly understood that two or more different polymer binders may be used in the composition of the present invention.
[0056] As mentioned above, the polymer binder used in a minimal proportion relative to the amount of zeolite crystals allows the cohesion between said zeolite crystals, which behaves like a solid reservoir for the ionic conductor of the composition of the invention. The mass of zeolite crystals present in the composition according to the invention is reduced in air at 25°C to 450°C, +5°C.min -1 This can be measured by thermogravimetric analysis (TGA) at a heating rate of 100 .mu.m.
[0057] The ionic conductor present in the composition according to the invention is preferably, and very advantageously, anhydrous, i.e. it does not contain any water or contains only traces of water, i.e. it contains only amounts of water less than 1000 ppm by volume, preferably less than 100 ppm and better still less than 50 ppm.
[0058] According to one embodiment, the ionic conductor comprises, and preferably consists of, at least one lithium salt. The lithium salts that may be used in the context of the present invention are preferably selected from lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium 2-trifluoromethyl-4,5-dicyanoimidazole (LiTDI), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium nitrate (LiNO3), lithium bis(oxalato)borate (LiBOB), and mixtures of two or more of these in any proportion. Particularly preferred lithium salts for the purposes of the present invention are LiTFSI sold by Solvay, or LiFSI and / or LiTDI sold by the company Arkema. LiFSI is most particularly preferred, optionally in a mixture with LiTDI from Arkema.
[0059] If present, the solvent used is a solvent for the lithium salt. Among completely suitable solvents, mention may be made of ionic liquids, in particular ionic liquids formed by the combination of organic cations and anions.
[0060] Non-limiting examples of organic cations include ammonium cations, sulfonium cations, pyridinium cations, pyrrolidinium cations, imidazolium cations, imidazolinium cations, phosphonium cations, guanidinium cations, piperidinium cations, thiazolium cations, triazolium cations, oxazolium cations and pyrazolium cations, and mixtures thereof. According to one embodiment, the cation is selected from the group consisting of C1-C 30It may contain alkyl groups, for example 1-butyl-1-methylpyrrolidinium (BMPYR), 1-ethyl-3-methylimidazolium (EMIM), tributylmethylphosphonium (TBMPHO), N-methyl-N-propylpyrrolidinium or N-methyl-N-butylpiperidinium.
[0061] According to one embodiment, the anions associated therewith include, by way of non-limiting example, imides, in particular bis(fluorosulfonyl)imides and bis(trifluoromethanesulfonyl)imides, borates, phosphates, phosphinates and phosphonates, in particular alkylphosphonates, amides (in particular dicyanamide), aluminates (in particular tetrachloroaluminate), halides (e.g. bromide, chloride and iodide anions), cyanates and acetates (CHCOO - ), and in particular trifluoroacetate (CF3COO - ), sulfonates, especially methanesulfonate (CH3SO3 - ) or trifluoromethanesulfonate (CF3SO3 - ), and sulfates, in particular hydrogen sulfates.
[0062] According to a preferred embodiment, the anion is tetrafluoroborate (BF4 - ), bis(oxalato)borate (BOB - ), hexafluorophosphate (PF6 - ), hexafluoroarsenate (AsF6 - ), triflate or trifluoromethylsulfonate (CF3SO3 - ), bis(fluorosulfonyl)imide (FSI - ), bis(trifluoromethanesulfonyl)imide (TFSI - ), nitrates (NO3 - ) and 4,5-dicyano-2-(trifluoromethyl)imidazole (TDI - According to one embodiment, the anion is selected from TDI - , F.S.I. - , TFSI - , PF6 -, BF4 - , NO3 - and B.O.B. - Preferably, the anion is selected from FSI - It is.
[0063] Non-limiting examples that may be mentioned among preferred ionic liquids include EMIM-FSI, EMIM-TFSI, BMPYR-FSI, BMPYR-TFSI, TBMPHO-FSI, TBMPHO-TFSI, and mixtures thereof.
[0064] Other possible solvents may include, in a non-limiting manner: - carbonates, such as vinylene carbonate (VC) (CAS: 872-36-6), fluoroethylene carbonate or 4-fluoro-1,3-dioxolan-2-one (F1EC) (CAS: 114435-02-8), trans-4,5-difluoro-1,3-dioxolan-2-one (F2EC) (CAS: 171730-81-7), ethylene carbonate (EC) (CAS: 96-49-1), propylene carbonate (PC) (CAS: 108-32-7), - nitriles such as succinonitrile (SN), 3-methoxypropionitrile (CAS: 110-67-8), (2-cyanoethyl)triethoxysilane (CAS: 919-31-3), ethers, such as 1,3-dioxolane (DOL), dimethoxyethane (DME), dibutyl ether (DBE), poly(ethylene glycol dimethyl ether), in particular diethylene glycol dimethyl ether (EG2DME), triethylene glycol dimethyl ether (EG3DME) and tetraethylene glycol dimethyl ether (EG4DME); - Sulfolane (CAS: 126-33-0), and - Triethyl phosphate (TEP) (CAS: 78-40-0).
[0065] Among the solvents listed above, EG4DME, DOL, DME, SN and F1EC are preferred. Mixtures of two or more of the solvents defined above can be used, optionally in combination with one or more ionic liquids defined above. The amount of solvent(s) can vary in wide proportions, for example from 1% to 99% by weight.
[0066] Non-limiting and purely illustrative examples of ionic conductors include LiFSI, LiTFSI or mixtures of LiFSI and LiTFSI, in combination with one or more solvents advantageously selected from SN, DOL, DME, F1EC and EG4DME, optionally in combination with one or more ionic liquids, such as EMIM-FSI or TBMPHO-FSI.
[0067] More particularly preferred examples include the following mixtures: (LiFSI and SN), (LiTFSI and SN), (LiFSI and TEP), (LiFSI and EG4DME), (LiFSI, EC and F1EC), (LiFSI, EG4DME and EMIM-FSI), (LiFSI, EG4DME and TBMPHO-FSI), (LiFSI, EC, F1EC and EMIM-FSI), (LiFSI, DOL and DME), and (LiFSI, DOL, DME and SN).
[0068] Examples of ionic conductors which are perfectly suitable for the purposes of the present invention include: LiFSI (14% by weight) and succinonitrile (86% by weight), LiTFSI (20% by weight) and succinonitrile (80% by weight), LiFSI (14% by weight) and TEP (86% by weight), LiFSI (14% by weight) and EG4DME (86% by weight), LiFSI (14% by weight), EC (80% by weight) and F1EC (6% by weight), LiFSI (14% by weight), EG4DME (43% by weight) and EMIM-FSI (43% by weight), LiFSI (14% by weight), EG4DME (43% by weight) and TBMPHO-FSI (43% by weight), - LiFSI (14% by weight), EC (37% by weight), F1EC (6% by weight) and EMIM-FSI (43% by weight), LiFSI (14% by weight), DOL (43% by weight) and DME (43% by weight), LiFSI (14 wt%), DOL (21.5 wt%), DME (21.5 wt%) and SN (43 wt%).
[0069] The ionic conductor is impregnated into the solid (zeolite crystals + polymer binder) as shown below. The amount of ionic conductor that can be impregnated into the solid can vary in wide proportions, without limitation, depending, inter alia, on the nature of the zeolite and the size of the zeolite crystals, the zeolite / binder weight ratio, the nature and amount of each component of the ionic conductor. This amount is generally between 5% and 400% by weight, preferably between 5% and 300% by weight, more preferably between 10% and 200% by weight, relative to the solid (zeolite crystals + polymer binder).
[0070] The composition according to the invention is therefore a solid electrolyte characterised by the presence of a (liquid) ionic conductor interspersed in a set of crystals of one or more zeolites bound together by at least one polymer binder. According to one embodiment of the invention, the amount of crystals of one or more zeolites represents at least 55% by weight, preferably at least 60% by weight, more preferably at least 80% by weight, advantageously at least 90% by weight and more preferentially at least 95% by weight of the solid (zeolites + binder) without ionic conductor.
[0071] A non-limiting example of a composition according to the present invention is a composition comprising: A / crystals of FAU type zeolite(s), advantageously LSX zeolite crystals, preferably exchanged with lithium; B / at least one fluorinated polymer binder, preferably PVDF, in an amount between 0.5% and 20% by weight, preferably between 1% and 10% by weight, relative to the total weight of the crystals of one or more zeolites and the binder; C / at least one ionic conductor comprising at least one lithium salt, advantageously LiFSI, at least one solvent advantageously selected from SN, DOL, DME, F1EC and EG4DME, and optionally at least one ionic liquid, for example EMIM-FSI.
[0072] As non-limiting examples of compositions according to the invention there may be mentioned: - zeolite LiLSX (45% by weight), PVDF (5% by weight) and an ionic conductor [50% by weight, composed of LiFSI (14% by weight) and succinonitrile (86% by weight)], - LiLSX zeolite (58.5% by weight), PVDF (6.5% by weight) and an ionic conductor (35% by weight, composed of LiFSI (14% by weight) and succinonitrile (86% by weight)); - LiLSX zeolite (61.7% by weight), PVDF (3.3% by weight) and an ionic conductor (35% by weight, composed of LiFSI (14% by weight) and succinonitrile (86% by weight)); - LiLSX zeolite (61.7% by weight), PVDF (3.3% by weight) and an ionic conductor (35% by weight, composed of LiTFSI (20% by weight) and succinonitrile (80% by weight)); - LiLSX zeolite (61.7 wt%), PVDF (3.3 wt%) and ionic conductor (35 wt%, composed of LiFSI (14 wt%) and TEP (86 wt%); - LiLSX zeolite (61.7% by weight), PVDF (3.3% by weight) and ionic conductor (35% by weight, composed of LiFSI (14% by weight) and EG4DME (86% by weight)); - LiLSX zeolite (61.7% by weight), PVDF (3.3% by weight) and ionic conductor (35% by weight, composed of LiFSI (14% by weight), EC (80% by weight) and F1EC (6% by weight) - LiLSX zeolite (61.7 wt%), PVDF (3.3 wt%) and ionic conductor (35 wt%, composed of LiFSI (14 wt%), EMIM-FSI (43 wt%) and EG4DME (43 wt%); - LiLSX zeolite (61.7% by weight), PVDF (3.3% by weight) and ionic conductor (35% by weight, composed of LiFSI (14% by weight), TBMPHO-FSI (43% by weight) and EG4DME (43% by weight)); - LiLSX zeolite (61.7% by weight), PVDF (3.3% by weight) and an ionic conductor [35% by weight, composed of LiFSI (14% by weight), EMIM-FSI (43% by weight), EC (37% by weight) and F1EC (6% by weight)], - zeolite LiLSX (61.7 wt%), PVDF (3.3 wt%) and ionic conductor [35 wt%, composed of LiFSI (14 wt%), DOL (21.5 wt%), DME (21.5 wt%) and SN (43 wt%)].
[0073] The composition of the present invention has the advantage that it is a solid electrolyte and at the same time has good flexibility, providing mechanical strength perfectly suitable for use in batteries, especially lithium-ion batteries. Quite surprisingly, it has been discovered that the electrical conductivity of the composition of the present invention is comparable or even identical to that of the ionic conductors impregnated in the solid [zeolite + binder]. Thus, the composition according to the present invention provides an excellent compromise between optimized mechanical properties (solid and flexible electrolyte) and maximum ionic conductivity.
[0074] The compositions of the present invention can be prepared by imbibing the ionic conductor into the system (zeolite crystals + polymer binder) or by imbibing the ionic conductor into the zeolite crystals followed by the addition of the polymer binder.
[0075] According to one embodiment, the process for preparing the composition according to the invention comprises: a) mixing zeolite crystals in the solid state with at least one polymer binder; b) forming it into the desired appearance and size; c) applying heat and pressure to the homogenized, molded assembly to soften the polymeric binder; d) maintaining the temperature and pressure until cohesion occurs between the zeolite crystals and the binder; e) Cool until the binder hardens.
[0076] The mixing in step a) can be carried out according to any conventional technique known to those skilled in the art for mixing solids. The shaping to the desired appearance and size in step b) can be carried out, for example, by extrusion or any other technique known to those skilled in the art.
[0077] The heating in step c) must be at a temperature sufficient to soften the polymer binder and adhere to the zeolite crystals. The heating temperature is typically about 5°C to 10°C above the melting or softening point of the polymer binder. The pressure applied depends on many factors including the amount of crystals relative to the binder, the size of the zeolite crystals, the nature of the binder, etc., and is typically between 10 MPa and 2000 MPa, generally between 100 MPa and 1500 MPa.
[0078] The imbibing step, whether carried out on the zeolite crystals or on the article obtained after cooling in step e) of the above process, can be carried out by any means known per se, for example by partial or total, preferably total, immersion in an ion conductor, for a period which depends on the nature and amounts of the various components of the composition of the invention, typically a period which can range from a few minutes to a few hours.
[0079] The composition of the present invention may be in the form of a film or various forms of weak aggregates in some embodiments and sizes, for example and purely for illustrative purposes, for example, when the composition is used as a separator in an all-solid-state battery, the composition is in the form of a film.
[0080] Thus, the composition of the present invention is in the form of a solid containing zeolite crystals soaked in a solid electrolyte, the crystals being immobilized by a polymer binder. The composition of the present invention behaves like a reservoir containing a liquid electrolyte, and leakage of the electrolyte is not possible. This greatly reduces the flammability of the electrolyte.
[0081] The polymer binder which immobilizes the zeolite crystals therefore gives the solid composition of the invention mechanical strength and flexibility which makes it perfectly suitable for use as a solid electrolyte, for example in lithium-ion type batteries.
[0082] Thus, the solid composition according to the invention behaves like a solid electrolyte in which the pores and interstitial spaces of the zeolite are at least partially or totally filled with a liquid ionic conductor, and ions can circulate freely within the pores and interstitial spaces without the solid electrolyte leaking out of the electrolyte.
[0083] The composition according to the present invention, being a solid electrolyte, exhibits performance qualities at least equal to those of liquid electrolytes in terms of ionic conductivity and electrochemical stability.In particular, it has been observed that the composition according to the present invention provides a completely satisfactory and adequate electrochemical stability, in that it has a very good resistance to oxidation and reduction when voltage is applied.Therefore, one of the further advantages of the composition according to the present invention is that it provides electrochemical performance at least equal to that of liquid electrolytes, while improving safety.
[0084] The compositions according to the invention also surprisingly show resistance to the growth of dendrites, typically lithium dendrites, which may be detrimental to the correct functioning of the battery by causing short circuits.The compositions according to the invention can therefore be used not only in batteries with anodes made of graphite, graphite / silicon or silicon, but also in batteries with metal anodes, for example lithium metal, which allows the gain of energy density, especially compared to conventional Li-ion technology.
[0085] Due to the numerous advantages offered by the compositions of the invention, the compositions according to the invention can be very advantageously used as solid electrolytes in many electrochemical devices, such as, as non-limiting examples, membrane electrode assemblies (MEAs) for batteries, capacitors, electrochemical double layer capacitors, fuel cells or electrochromic devices. More specifically, as mentioned above, the solid electrolytes of the invention can be used as separators and / or in the cathode (catholyte) and / or in the anode (anolyte), especially in batteries, more specifically in secondary batteries, typically all-solid-state batteries, and even more specifically in all-solid-state lithium-ion batteries.
[0086] According to yet another aspect, the present invention relates to the use of the aforementioned composition as a separator in an all-solid-state battery. According to yet another aspect, the present invention relates to a separator, in particular for a Li-ion secondary battery, comprising a composition according to the present invention. In a preferred embodiment, the composition according to the present invention constitutes the separator of an all-solid-state battery. The composition according to the present invention may also be used as an anolyte or catholyte in a battery, for example a Li-ion secondary battery, more particularly in an all-solid-state battery.
[0087] According to one embodiment of the separator of the present invention, it is in the form of a film, which advantageously has a thickness, measured with a Palmer micrometer, between 5 μm and 500 μm, preferably between 5 μm and 100 μm, more preferably between 5 μm and 50 μm, and even more preferably between 5 μm and 20 μm.
[0088] Finally, the present invention relates to providing a rechargeable Li-ion battery including such a separator.
[0089] The present invention also relates to a battery comprising at least one composition comprising crystals of one or more zeolites as defined above, the battery being an all-solid-state battery or a Li-ion secondary battery, in which said at least one composition comprising crystals of one or more zeolites in a battery according to the invention constitutes the separator and / or the anolyte and / or the catholyte, preferably the separator, of said battery.
[0090] <Characterization techniques> The physical properties of zeolites may be evaluated by methods known to those skilled in the art, the main ones being described below.
[0091] <Zeolite crystal particle size> The number-average diameter of zeolite crystals is estimated by observation with a scanning electron microscope (SEM). To estimate the size of the zeolite crystals on the sample, a set of images is taken at a magnification of at least 5000. The diameters of at least 200 crystals are then measured using dedicated software, for example the Smile View software published by LoGraMi. The accuracy is on the order of 3%.
[0092] <Chemical analysis of zeolite - Si / Al ratio and exchange degree> The elemental chemical analysis of the zeolites is carried out on a wavelength dispersive spectrometer (WDXRF), for example a Tiger S8 instrument from the company Brüker, according to the technique of chemical analysis by X-ray fluorescence as described in the standard NF EN ISO 12677:2011.
[0093] X-ray fluorescence is a non-destructive spectral technique that utilizes the photoluminescence of atoms in the X-ray range to establish the elemental composition of a sample. Excitation of atoms, typically by an X-ray beam or by electron bombardment, produces specific radiation after the atoms return to their ground state. Measurement uncertainties of less than 0.4% by weight are conventionally obtained after calibration for each oxide.
[0094] Other methods of analysis are exemplified by atomic absorption spectrometry (AAS) and inductively coupled plasma atomic emission spectrometry (ICP-AES) methods described in standards NF EN ISO 21587-3 or NF EN ISO 21079-3 for machines such as the Agilent 5110.
[0095] After calibration for each oxide SiO2 and Al2O3, and for various oxides (e.g. those derived from exchangeable cations, e.g. sodium), measurement uncertainties of less than 0.4% by weight are conventionally obtained. The ICP-AES method is particularly suitable for the measurement of lithium content.
[0096] The elemental chemical analysis described above therefore makes it possible to check the Si / Al molar ratio of the zeolite used. In the present description, the measurement uncertainty of the Si / Al ratio is ±5%. The measurement of the Si / Al ratio of the zeolite present in the adsorption material can also be carried out by solid-state silicon nuclear magnetic resonance (NMR) spectroscopy.
[0097] The quality of the ion exchange is related to the number of moles of the cation under consideration in the zeolite crystal after the exchange. More precisely, the proportion of cations relative to the number of exchangeable sites is estimated by evaluating the ratio between the equimolar number of said cations (to reach electron neutrality) and the total number of exchangeable sites equal to the total number of aluminum atoms present in the zeolite framework. The respective amount of each cation is evaluated by chemical analysis of the corresponding cation. EXAMPLES
[0098] The following examples illustrate, but do not limit, the scope of the invention.
[0099] [Example 1: Preparation of solid electrolyte for separator of Li-ion battery] A mixture is prepared containing 5% by weight of PVDF (Kynar® from Arkema) with a melting point below 175°C and 95% by weight of lithium zeolite LiLSX (NaLSX crystals are prepared according to EP 2244976 and then exchanged with lithium by exchanging the sodium cations in a lithium chloride solution according to conventional techniques). The number average diameter of the LiLSX crystals is 5.5 μm. The binder + zeolite crystal mixture is ground in a mortar and then pelletized in a pelletizer at 3000 kg.cm. -2 and compressed at 160°C for 15 minutes. A 250 μm thick film is then obtained, which is soaked at room temperature by immersion in a solution of ionic conductor A, which is composed of 80% by weight of succinonitrile and 20% by weight of LiTFSI (Gotion). The film is then discharged and weighed to determine the increase in mass after absorption, which is about 55%. The final solid electrolyte is then composed of LiLSX zeolite (61.7% by weight), PVDF (3.3% by weight) and ionic conductor A (35% by weight). It is named SE1.
[0100] [Example 2: Preparation of PEO-based solid electrolyte for Li-ion battery separator] For comparison, a PEO (poly(ethylene oxide))-based solid electrolyte composed of 80% by weight PEO and 20% by weight LiTFSI is prepared. PEO is dissolved in acetonitrile, and then LiTFSI is added. The resulting solution is deposited on a glass plate by solvent casting, and then dried under vacuum at 60° C. to evaporate the acetonitrile. A self-supporting film, named SE2, is then obtained.
[0101] [Example 3: Measurement of electrical conductivity of all-solid separator] The conductivity (σ) is evaluated by electrochemical impedance spectroscopy by placing the solid electrolyte between two gold electrodes in a leak-proof conductivity cell and under inert atmosphere (CESH, BioLogic). The results are shown in Table 1. Electrolyte SE1 has a much higher conductivity at 25 °C than the reference PEO (SE2).
[0102] [Table 1]
[0103] [Example 4: Measurement of thermal stability of all-solid separator] The conductivity (σ) is evaluated by electrochemical impedance spectroscopy by placing the solid electrolyte between two gold electrodes in a leak-proof conductivity cell and under inert atmosphere (CESH, BioLogic). The results are shown in Table 2. Electrolyte SE1 has a much higher conductivity at 25 °C than the reference PEO (SE2).
[0104] [Table 2]
[0105] [Example 5: Measurement of electrochemical stability of all-solid separator] The electrochemical stability of various solid electrolytes is evaluated by cyclic voltammetry at 60 °C (under an inert atmosphere) by placing the solid electrolyte in a button cell between a stainless steel electrode and a lithium metal electrode. Cyclic voltammetry is performed between 2 V and 6 V at 1 mV / s. The results are shown in Table 3. Electrolyte SE1 has a much higher electrochemical stability than the reference PEO (SE2).
[0106] [Table 3]
Claims
1. A / one or more zeolite crystals; B / at least one polymer binder, the amount of said polymer binder being between 0.5% and 20% by weight, preferably between 1% and 10% by weight, relative to the total weight of the zeolite crystals and the binder; and C / at least one ionic conductor containing at least one lithium salt A composition comprising:
2. 2. The composition of claim 1, wherein the zeolite crystals are crystals of one or more zeolites selected from faujasite (FAU), MFI zeolite, chabazite (CHA), heulandite (HEU), Linde type A (LTA) zeolite, EMT zeolite, beta zeolite (BEA), mordenite (MOR), and mixtures thereof.
3. 3. A composition according to claim 1 or claim 2, wherein the zeolite crystals are crystals of one or more zeolites selected from Y-type, X-type, MSX-type or LSX-type faujasite, preferably entirely X-type, MSX-type or LSX-type faujasite, more preferably MSX-type or LSX-type faujasite, and preferably entirely LSX-type faujasite.
4. The composition according to any one of claims 1 to 3, wherein the zeolite crystals are crystals of one or more zeolites whose counter cations are selected from hydronium ions, organic cations, alkali metal cations, alkaline earth metal cations, transition metal cations, rare earth metal cations, and mixtures of two or more of these.
5. 5. The composition according to any one of claims 1 to 4, wherein the zeolite crystals are crystals of one or more zeolites whose countercations are lithium cations, and optionally hydronium cations and / or one or more other alkali metal or alkaline earth metal cations, such as sodium cations, potassium cations, rubidium cations, cesium cations, magnesium cations, calcium cations, strontium cations, or barium cations, and mixtures thereof.
6. 6. The composition according to any one of claims 1 to 5, wherein the size of the zeolite crystals is between 0.02 μm and 20.00 μm, more preferably between 0.02 μm and 10.00 μm, more preferably between 0.03 μm and 5.00 μm, and advantageously between 0.05 μm and 1.00 μm.
7. The composition according to any one of claims 1 to 6, wherein the at least one polymeric binder is selected from fluoropolymers, carboxymethylcellulose, styrene-butadiene rubber, polyacrylic acid and its esters, and polyimides, preferably from fluoropolymers including optionally functionalized fluorinated homopolymers and optionally functionalized fluorinated copolymers.
8. 8. The composition according to claim 1, wherein the at least one polymeric binder is selected from polyvinylidene fluoride and copolymers of vinylidene fluoride and at least one comonomer compatible with vinylidene fluoride.
9. 9. The composition according to any one of claims 1 to 8, wherein the lithium salt is selected from lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium 2-trifluoromethyl-4,5-dicyanoimidazole, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium nitrate, lithium bis(oxalato)borate, and mixtures of two or more thereof in any proportion, preferably selected from mixtures with lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium 2-trifluoromethyl-4,5-dicyanoimidazole.
10. 10. The composition according to any one of claims 1 to 9, wherein the amount of ionic conductor is generally between 5% and 400% by weight, preferably between 5% and 300% by weight, and more preferably between 10% and 200% by weight, based on the solids (zeolite crystals + polymer binder).
11. A composition according to any one of the preceding claims, wherein the ionic conductor comprises LiFSI, LiTFSI or a mixture of LiFSI and LiTFSI in combination with one or more solvents advantageously selected from SN, DOL, DME, F1EC and EG4DME, and optionally one or more ionic liquids.
12. A / crystals of FAU type zeolite, advantageously LSX zeolite crystals, preferably exchanged with lithium; B / at least one fluorinated polymer binder, preferably PVDF, in an amount between 0.5% and 20% by weight, preferably between 1% and 10% by weight, relative to the total weight of the crystals of one or more zeolites and the binder; C / at least one ionic conductor comprising at least one lithium salt, preferably LiFSI, at least one solvent preferably selected from SN, DOL, DME, F1EC and EG4DME, and optionally at least one ionic liquid; The composition according to any one of claims 1 to 11, comprising:
13. Use of a composition according to any one of claims 1 to 12 as a separator and / or in a cathode (catholyte) and / or in an anode (anolyte), in particular in a battery, more particularly in a secondary battery, typically an all-solid-state battery, and even more particularly in an all-solid-state lithium-ion battery.
14. 15. The use according to claim 14 as a separator for an all-solid-state battery in the form of a film having a thickness between 5 μm and 500 μm, preferably between 5 μm and 100 μm, more preferably between 5 μm and 50 μm, and even more preferably between 5 μm and 20 μm.
Citation Information
Patent Citations
Rechargeable Lithium Insertion Batteries Using Hybrid Polymer Electrolytes
JP1996507407A
Agglomerated zeolite adsorbent, its production and use in separation of industrial gas at not extermely low temperature
JP1999076810A
Low-silica faujasite-type zeolite and its production
JP1999217212A
Low-silica faujasite-type zeolite and its production
JP1999217213A
Fine low silica faujasite type zeolite and its production
JP1999343112A
Cited By
Solid electrolyte, method for producing same, and power storage device
WO2026121260A1