Glass substrate, its manufacturing method, and electronic device

Asymmetric compressive stress distribution on glass substrates enhances impact resistance and durability, addressing the issue of breakage in electronic devices by improving both impact and bending strength.

JP2024537082AActive Publication Date: 2024-10-10BYD CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024519782
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-12
Filing Date
2022-09-22
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Glass substrates used in electronic devices suffer from low impact resistance and easy breakage, leading to aesthetic damage and functional impairment when subjected to accidental drops or external forces.

Method used

The glass substrate features asymmetric compressive stress distributions on opposite surfaces, with one side having higher surface compressive stress and deeper depth than the other, enhancing impact resistance and bending strength.

Benefits of technology

The asymmetric compressive stress distribution significantly improves the impact resistance and durability of electronic devices, protecting them from external impacts and bending deformations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A glass substrate, a manufacturing method thereof, and an electronic device are disclosed. The glass substrate has a first surface compressive stress layer and a second surface compressive stress layer on opposite sides thereof. The surface compressive stress of the first surface compressive stress layer is greater than the surface compressive stress of the second surface compressive stress layer, and the depth of the first surface compressive stress layer is less than the depth of the second surface compressive stress layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to a Chinese patent application filed with the State Intellectual Property Office of the People's Republic of China on October 12, 2021, bearing application number 202111189979.8 and title "Glass Substrate and Electronic Device," the entire contents of which are incorporated herein by reference.

[0002] The present application relates to the technical field of glass products, and in particular to glass substrates and manufacturing methods thereof, as well as electronic devices. [Background technology]

[0003] At present, glass is often used as a screen cover or a back cover in electronic devices, but glass has a problem of low impact resistance and easy breakage. When an electronic device is carelessly dropped or subjected to an external force, the glass will bend and deform, causing breakage, which will damage the aesthetics of the electronic device and affect the normal use of the electronic device. Therefore, it is necessary to provide a new glass that can improve the impact resistance of electronic devices and ensure a long service life of electronic devices. Summary of the Invention [Problem to be solved by the invention]

[0004] In view of this, the glass substrate according to the present application has different compressive stress distributions on both surfaces located opposite each other, so that one side can withstand the impact of a hard object and the other side can withstand the tension of bending deformation. When the glass substrate is applied to an electronic device, the impact resistance of the electronic device can be improved, and the durability of the electronic device can be increased. [Means for solving the problem]

[0005] In a first aspect, the glass substrate according to the present application has a first surface compressive stress layer and a second surface compressive stress layer on opposite sides, the surface compressive stress of the first surface compressive stress layer being greater than the surface compressive stress of the second surface compressive stress layer, and the depth of the first surface compressive stress layer being smaller than the depth of the second surface compressive stress layer.

[0006] In the present application, the compressive stresses on the surfaces on both sides of the glass substrate are distributed asymmetrically, the first surface compressive stress layer has high surface compressive stress and can withstand impact from a hard object, and the second surface compressive stress layer has a deep depth and can withstand higher bending tension. When the glass substrate is applied to an electronic device, the first surface of the glass substrate functions as the outer surface of the electronic device and the second surface of the glass substrate is adjacent to an electronic component. When the electronic device is impacted by an external object, the glass substrate can better protect the electronic device and improve the reliability of the electronic device.

[0007] Preferably, a ratio of an absolute value of a difference between the compressive stress integral of the first surface compressive stress layer and the compressive stress integral of the second surface compressive stress layer to the compressive stress integral of either surface compressive stress layer is 5% or less.

[0008] Preferably, when the compressive stress integral of the obtained first surface compressive stress layer is equal to the compressive stress integral of the second surface compressive stress layer, the ratio of the absolute value of the difference between the compressive stress integral of the first surface compressive stress layer and the compressive stress integral of the second surface compressive stress layer to the compressive stress integral of the first surface compressive stress layer or the compressive stress integral of the second surface compressive stress layer is 5% or less; when the compressive stress integral of the first surface compressive stress layer is larger than the compressive stress integral of the second surface compressive stress layer, the ratio of the absolute value of the difference between the compressive stress integral of the first surface compressive stress layer and the compressive stress integral of the second surface compressive stress layer to the compressive stress integral of the second surface compressive stress layer is 5% or less; and when the compressive stress integral of the first surface compressive stress layer is smaller than the compressive stress integral of the second surface compressive stress layer, the ratio of the absolute value of the difference between the compressive stress integral of the first surface compressive stress layer and the compressive stress integral of the second surface compressive stress layer to the compressive stress integral of the first surface compressive stress layer is 5% or less.

[0009] Preferably, the surface compressive stress of the first surface compressive stress layer is 700 MPa to 1200 MPa, and the surface compressive stress of the second surface compressive stress layer is 300 MPa to 850 MPa.

[0010] Preferably, the ratio of the surface compressive stress of the first surface compressive stress layer to the surface compressive stress of the second surface compressive stress layer is 1.2 or more.

[0011] Preferably, when the thickness of the glass substrate is t, the depth of the first surface compressive stress layer is 0.004 mm or more and 0.1t or less, and the depth of the second surface compressive stress layer is 0.085 mm or more and 0.6t or less.

[0012] Preferably, the thickness t of the glass substrate is 0.1 mm to 5 mm.

[0013] Preferably, the material of the glass substrate includes one or more of lithium aluminosilicate glass, soda lime silicate glass, and soda lime glass.

[0014] Preferably, the first surface compressive stress layer and / or the second surface compressive stress layer is obtained by chemically strengthening or physically strengthening a glass substrate.

[0015] Preferably, the glass substrate has a bending strength of 1000 MPa to 2100 MPa.

[0016] The glass substrate according to the first aspect of the present application has high mechanical strength, high impact resistance and drop resistance, and can be applied to in-vehicle displays, mobile phone covers and related daily home appliances and consumer electronic products, thereby providing electronic devices with high strength, impact resistance and drop resistance, improving the reliability and safety of the products.

[0017] In a second aspect, a method for producing a glass substrate according to the first aspect of the present application includes the steps of: providing a glass substrate precursor, the glass substrate precursor including both surfaces opposite to each other, and providing a first protective layer on one surface to obtain the glass substrate precursor having the first protective layer; placing the glass substrate precursor having the first protective layer in molten salt to perform a first tempering, thereby forming a compressive stress layer on a side of the glass substrate precursor on which the first protective layer is not provided; removing the first protective layer and providing a second protective layer on a surface of the glass substrate precursor on which the compressive stress layer is provided; and placing the glass substrate precursor having the second protective layer in the molten salt to perform a second tempering, thereby forming a compressive stress layer on the side of the glass substrate precursor on which the second protective layer is not provided, and removing the second protective layer to obtain the glass substrate.

[0018] Preferably, the molten salt is a sodium salt or a potassium salt.

[0019] Preferably, the molten salt comprises one or more of potassium nitrate, sodium nitrate.

[0020] Preferably, the temperature of the molten salt is 360°C to 450°C.

[0021] Preferably, the time for the first strengthening and / or the second strengthening is 60 minutes to 200 minutes.

[0022] Preferably, the first reinforcement and / or the second reinforcement is a stepwise reinforcement using a plurality of types of molten salts.

[0023] Preferably, the first protective layer and the second protective layer are heat resistant protective coatings.

[0024] In a third aspect, an electronic device according to the present application includes an electronic component and a glass cover covering the electronic component, the glass cover including the glass substrate according to the first aspect of the present application.

[0025] Preferably, in the glass substrate, the second surface compressive stress layer is close to the electronic component, and the first surface compressive stress layer is away from the electronic component.

[0026] Preferably, the glass cover comprises a screen cover and / or a back cover of an electronic device. [Brief description of the drawings]

[0027] [Figure 1] FIG. 2 is a stress distribution curve diagram along the thickness direction of a glass substrate according to an embodiment of the present application. [Diagram 2] FIG. 11 is a stress distribution curve diagram along the thickness direction of a glass substrate according to another embodiment of the present application. [Diagram 3] 1 is a flowchart of a method for manufacturing a glass substrate according to an embodiment of the present application. [Figure 4] 1 is a schematic configuration diagram of an electronic device according to an embodiment of the present application. [Diagram 5] FIG. 2 is a stress distribution curve diagram along the thickness direction of the glass plate of Example A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Hereinafter, the technical means in the embodiments of the present application will be described clearly and completely with reference to the drawings in the embodiments of the present application, and obviously, the described embodiments are only a part of the embodiments of the present application, but not all of them, and all other embodiments that a person skilled in the art can obtain based on the embodiments of the present application without creative labor are all within the scope of protection of the present application.

[0029] For ease of understanding, some terms related to the present application are explained as follows: Depth of compressive stress (DOL) refers to the distance from the point where the compressive stress inside the glass is 0 to the glass surface, in this specification, the depth of the compressive stress layer is the same concept as the compressive stress depth, and the compressive stress integral refers to the integral of the compressive stress and the compressive stress depth, that is, the area between the compressive stress and the compressive stress depth, and as shown in Fig. 5, the compressive stress integral of the first surface compressive stress layer is S1, and the compressive stress integral of the second surface compressive stress layer is S2.

[0030] Glass has excellent aesthetics and is widely used in electronic products. However, glass has low impact resistance and is easily broken, so it needs to be tempered to strengthen its mechanical properties. After tempering, compressive stress occurs on the surface of the glass, and tensile stress against the compressive stress occurs inside the glass. When the internal tensile stress exceeds the limit that the glass can withstand, the glass will self-explode. In order to obtain glass with strong impact resistance and high stability, the glass substrate of the present application has different compressive stress distributions on both surfaces located opposite each other, so that one side can withstand the impact of a hard object and the other side can withstand the tension of bending deformation. The compressive stress distribution allows the properties of both sides of the glass substrate to be optimized without the glass self-exploding, so that both surfaces of the glass substrate have their own advantages, and is suitable for the application of the glass substrate in electronic devices. When the glass substrate is applied to an electronic device, the impact resistance of the electronic device can be improved and the durability of the electronic device can be increased.

[0031] For electronic devices, the outer surface generally receives impact, and when glass is applied to electronic devices, only one surface of the glass becomes the impact surface. Based on the above scenario, the present application redesigns the compressive stress distribution on both sides of the glass on the premise that the tensile stress inside the glass does not change, and optimizes the properties of the surfaces on both sides of the glass. FIG. 1 is a stress distribution curve diagram along the thickness direction of a glass substrate according to an embodiment of the present application. As shown in FIG. 1, the glass substrate of the present application includes a first surface and a second surface located on opposite sides to each other, the first surface side of the glass substrate has a first surface compressive stress layer, and the second surface side of the glass substrate has a second surface compressive stress layer, the surface compressive stress of the first surface compressive stress layer is greater than the surface compressive stress of the second surface compressive stress layer, and the depth of the first surface compressive stress layer is smaller than the depth of the second surface compressive stress layer. When glass is impacted by a hard object, it receives compressive stress on the impact surface, but receives tensile stress due to bending on the back side of the impact surface. The first surface of the glass substrate of the present application has a higher surface compressive stress and can withstand the impact of a hard object and avoid direct penetration of the glass, and the second surface of the glass substrate has a greater depth and can withstand a higher bending tension and inhibit the glass from cracking, thereby greatly improving the comprehensive properties of the glass substrate and making the glass substrate more suitable for application scenarios.

[0032] In the embodiment of the present application, the ratio of the absolute value of the difference between the compressive stress integral of the first surface compressive stress layer and the compressive stress integral of the second surface compressive stress layer to the compressive stress integral of either surface compressive stress layer is 5% or less. That is, the absolute value of the difference between the compressive stress integral S1 of the first surface compressive stress layer of the glass substrate and the compressive stress integral S2 of the second surface compressive stress layer is |S1-S2|, and S x In S1 and S2, the value (S x may represent S1 or S2) or a smaller value, |S1-S2| and S x and S2 is 5% or less. Specifically, when S1 is equal to S2, the ratio of |S1-S2| to S2 or the ratio of |S1-S2| to S1 is 5% or less, when S1 is greater than S2, the ratio of |S1-S2| to S2 is 5% or less, when S2 is greater than S1, the ratio of |S1-S2| to S1 is 5% or less, and when |S2 is greater than S1, the ratio of |S1-S2| to S1 is 5% or less.x The ratio of the compressive stress integral difference between the compressive stress layers on both sides of the glass may be, but is not limited to, 5%, 3%, 2%, 1%, 0.5% or 0%. If the absolute value |S1-S2| of the compressive stress integral difference between the compressive stress layers on both sides of the glass is too large, the stress balance on both sides of the glass is lost and the glass is easily deformed, which reduces the structural stability of the glass substrate. Preferably, the compressive stress integral of the first surface compressive stress layer of the glass substrate is equal to the compressive stress integral of the second surface compressive stress layer, that is, the absolute value of the difference between the compressive stress integral of the first surface compressive stress layer of the glass substrate and the compressive stress integral of the second surface compressive stress layer of the glass substrate is equal to 0, and the compressive stress integrals on both sides of the glass substrate are equal, the stress on both sides of the glass substrate are balanced, the flatness of the glass substrate is high, and the structural stability is high. In some embodiments of the present application, the compressive stress integral of the first surface compressive stress layer of the glass substrate is greater than the compressive stress integral of the second surface compressive stress layer. Since the first surface of the glass substrate is an impact surface and receives a large external force, on the premise that the ratio of the surface compressive stress integral difference |S1-S2| on both sides of the glass substrate to the compressive stress integral of one of the surface compressive stress layers is 5% or less, the larger the compressive stress integral of the first surface compressive stress layer, the greater the impact of a larger external force it can withstand, and the better the impact resistance of the glass substrate can be.

[0033] In the glass substrate of the present application, the compressive stress distribution curve of one side surface may be a single parabola or a function curve with an inflection point. Figure 2 is a stress distribution curve diagram along the thickness direction of a glass substrate according to another embodiment of the present application. As shown in Figure 2, the compressive stress distribution curve in Figure 2 is a function curve with an inflection point. When the glass is tempered multiple times, an inflection point appears on the compressive stress distribution curve of its surface, and the slope of the function curve before and after the inflection point is different. When the compressive stress distribution curve of the surface of the glass substrate is a function curve with an inflection point, the compressive stress is reduced, so the compressive stress depth can be further deepened, and the glass does not self-explode.

[0034] In some embodiments of the present application, the thickness t of the glass substrate is 0.1 mm to 5 mm, and the thickness of the glass substrate may be specifically, but not limited to, 0.1 mm, 0.5 mm, 1 mm, 2 mm, or 5 mm. The asymmetric compressive stress distribution on the surface of the glass substrate of the present application has a significant improvement effect on glass of the above thickness, and if the thickness of the glass substrate is too thin, the central stress of the glass substrate is too high, making it easy to self-explode, and if the thickness of the glass substrate is too thick, it does not meet the trend of lightness and thinness required by the electronics industry. In some embodiments of the present application, the depth of the first surface compressive stress layer is 0.004 mm or more and 0.1t or less, and the depth of the second surface compressive stress layer is 0.085 mm or more and 0.6t or less, where 0.1t refers to the product of the thickness t of the glass substrate and 0.1, and 0.6t refers to the product of the thickness t of the glass substrate and 0.6. For example, when the thickness of the glass substrate is 0.5 mm, the depth of the first surface compressive stress layer is 0.004 mm to 0.05 mm, and the depth of the second surface compressive stress layer is 0.085 mm to 0.3 mm. By controlling the depth of the compressive stress layer within the above range, it is possible to ensure that the glass substrate has high bending resistance without self-explosion.

[0035] In the embodiment of the present application, the surface compressive stress of the first surface compressive stress layer is 700 MPa to 1200 MPa. The surface compressive stress of the first surface compressive stress layer may be specifically, but is not limited to, 700 MPa, 800 MPa, 1000 MPa, or 1200 MPa. In the embodiment of the present application, the surface compressive stress of the second surface compressive stress layer is 300 MPa to 850 MPa. The surface compressive stress of the second surface compressive stress layer may be specifically, but is not limited to, 300 MPa, 400 MPa, 500 MPa, 700 MPa, or 850 MPa. In the embodiment of the present application, the ratio of the surface compressive stress of the first surface compressive stress layer to the surface compressive stress of the second surface compressive stress layer is 1.2 or more. By controlling the ratio of the surface compressive stresses on both sides of the glass substrate within the above range, the mechanical properties of the glass substrate can be effectively improved.

[0036] In the embodiment of the present application, the material of the glass substrate includes one or more of lithium aluminosilicate glass, soda lime silicate glass, and soda lime glass. In the embodiment of the present application, the bending strength of the glass substrate is 1000 MPa to 2100 MPa, and the bending strength refers to the bending strength of the second surface of the glass substrate. In the embodiment of the present application, the size of the glass substrate can be adjusted as needed, and the size of the glass substrate does not affect the stress distribution. In some embodiments of the present application, the area of ​​the glass substrate is 0.5 cm 2 ~1m 2 It is.

[0037] The glass substrate of the present application has a first surface with high compressive stress and can withstand damage caused by sharp objects, and a second surface with deep compressive stress depth and can withstand a higher degree of fracture caused by bending. By adjusting the compressive stress distribution on both sides of the glass substrate, the advantages of one side of the glass substrate are more prominent, and the glass substrate can be adapted for application in electronic devices.

[0038] In the present application, the compressive stress layers on both sides of the glass substrate may be formed by chemical strengthening or physical strengthening.

[0039] Further, the method for manufacturing a glass substrate according to the present application manufactures the above-mentioned glass substrate. Fig. 3 is a flow chart of the method for manufacturing a glass substrate according to an embodiment of the present application. As shown in Fig. 3, strengthening the glass by the above-mentioned method means forming different stress distributions on both sides of the glass and strengthening the surfaces on both sides of the glass respectively. Specifically, the above-mentioned method includes: Step 100 of providing a glass substrate precursor, the glass substrate precursor including two surfaces opposite to each other, and providing a first protective layer on one surface of the glass substrate precursor to obtain the glass substrate precursor having the first protective layer; Step 200: forming a compressive stress layer on a side of the glass substrate precursor on which the first protective layer is not provided by placing the glass substrate precursor having the first protective layer in a molten salt for a first tempering process; Step 300: removing the first protective layer and providing a second protective layer on the surface of the glass substrate precursor having the compressive stress layer; and step 400 of performing a second strengthening by putting the glass substrate precursor having the second protective layer into the molten salt to form a compressive stress layer on the side of the glass substrate precursor on which the second protective layer is not provided, and removing the second protective layer to obtain the glass substrate.

[0040] In the present application, a glass substrate having a desired compressive stress distribution can be formed by controlling the type, temperature and tempering time of the molten salt. In the present application, the molten salt may be a sodium salt or a potassium salt. In some embodiments of the present application, the molten salt includes one or more of potassium nitrate and sodium nitrate. When the glass substrate precursor is tempered using potassium nitrate, a single parabolic compressive stress distribution curve can be formed, and when a mixed salt, for example a mixture of sodium nitrate and potassium nitrate, or sodium nitrate and potassium nitrate, respectively, is used for tempering, a compressive stress distribution curve having an inflection point can be formed. In the present application, the temperature of the molten salt is 360°C to 450°C, and the temperature of the molten salt may be specifically, but is not limited to, 360°C, 380°C, 400°C, 430°C or 450°C, and when the temperature of the molten salt is high, the tempering time required to reach a predetermined stress layer depth is shorter. In the present application, the time of the first tempering and / or the second tempering is 60min to 200min, and the longer the tempering time, the deeper the depth of the stress layer tempered at a predetermined temperature. In an embodiment of the present application, the first and / or second tempering may be stepwise tempering using multiple kinds of molten salts, for example, the first tempering may be tempered with molten sodium nitrate for 10 minutes and then tempered with molten potassium nitrate for 90 minutes, where the first tempering time is 100 minutes. In an embodiment of the present application, the first and second protective layers are heat-resistant protective coatings, which can protect the glass surface and prevent ion exchange from occurring on the glass surface.

[0041] In the embodiment of the present application, in order to make the surface compressive stress of the first surface compressive stress layer larger than that of the second surface compressive stress layer, a higher purity potassium nitrate is used when strengthening the first surface, and the strengthening time is appropriately shortened. In the embodiment of the present application, in order to make the depth of the second surface compressive stress layer deeper than that of the first surface compressive stress layer, a certain proportion of mixed molten salt is used when strengthening the second surface, and the strengthening time is appropriately extended.

[0042] In the present embodiment, physical strengthening may be used to strengthen the glass to obtain the present glass substrate.

[0043] Further, the glass cover according to the present application includes the above-mentioned glass substrate, and the outer surface of the glass cover is the first surface of the glass substrate, and the inner surface is the second surface of the glass substrate. The glass cover has high mechanical strength and is not easily broken in daily use scenes. In the embodiment of the present application, the glass cover may be partially made of a glass substrate and partially made of other materials such as plastics and metals, or may be entirely made of a glass substrate. The specific size of the glass cover can be adjusted or processed based on actual needs, and the description is omitted in the present embodiment. In some embodiments of the present application, the glass cover can be applied to the housing or display of a communication device, and has the characteristics of good texture, easy heat dissipation, and high impact resistance, and does not affect the signal of the communication device, so that it can be widely applied in the communication field, especially the 5G communication field.

[0044] The present application further provides an electronic device. FIG. 4 is a schematic diagram of an electronic device 100 according to an embodiment of the present application. As shown in FIG. 4, the electronic device 100 includes a screen cover 10, an electronic component 20, and a rear cover 30, and the screen cover 10 and the rear cover 30 cover the electronic component 20. In the embodiment of the present application, the screen cover or the rear cover is a glass cover according to the present application, or the screen cover and the rear cover are both glass covers according to the present application. When the glass cover is applied to an electronic device, the outer surface of the glass cover is a surface away from the electronic component, and the inner surface is a surface close to the electronic component. Since the first surface of the glass substrate has a high compressive stress, the outer surface of the glass cover can withstand external impact, and since the second surface of the glass substrate has a deep compressive stress depth, the inner surface of the glass cover can withstand a higher bending tension, thereby effectively protecting the electronic component and extending the service life of the electronic device. In an embodiment of the present application, electronic devices include, but are not limited to, mobile terminals such as mobile phones, tablet computers, laptops, palmtop computers, wearable devices, smart bracelets, smart watches, pedometers, and fixed terminals such as digital TVs and desktop computers.

[0045] The technical solutions of the present application will be further described below with reference to several examples. EXAMPLES

[0046] The manufacturing method of the glass substrate includes:

[0047] A glass substrate precursor of grade Corning GG5 and size 145 mm×70 mm×0.7 mm was provided, and the second surface of the glass substrate precursor was protected by a heat-resistant coating.

[0048] The first surface of the glass substrate precursor was chemically strengthened in two stages in a strengthening molten salt. The glass substrate precursor was placed in a NaNO3 molten salt to perform a first chemical strengthening on the first surface, with the molten salt temperature being 380°C and the first chemical strengthening time being 25 min. The glass substrate precursor was then placed in a KNO3 molten salt to perform a second chemical strengthening, with the molten salt temperature being 380°C and the second chemical strengthening time being 90 min. A first surface compressive stress layer with large surface compressive stress and shallow stress depth was formed on the first surface.

[0049] The heat-resistant protective coating on the second surface was removed, and the first surface of the glass substrate precursor was protected by a heat-resistant coating.

[0050] The second surface of the glass substrate precursor was chemically strengthened in two separate steps in a strengthening molten salt, the glass substrate precursor was placed in a NaNO3 molten salt to perform the first chemical strengthening on the second surface, the temperature of the molten salt was 380°C, and the time for the first chemical strengthening was 147 min, and the glass substrate precursor was placed in a mixed molten salt of KNO3 with a mass fraction of 62% and NaNO3 with a mass fraction of 38% to perform the second chemical strengthening, the temperature of the molten salt was 380°C, and the time for the second chemical strengthening was 20 min. A second surface compressive stress layer with small surface compressive stress and deep stress depth was formed on the second surface.

[0051] The heat-resistant protective coating on the first surface was removed to obtain a glass substrate.

[0052] The glass substrate and the electronic components are assembled to obtain a mobile phone, with the glass substrate having a first surface that is the exterior surface of the mobile phone and a second surface that is disposed inside the mobile phone (adjacent to the electronic components). EXAMPLES

[0053] The manufacturing method of the glass substrate includes:

[0054] A glass substrate precursor of grade Corning GG5 and size 145 mm×70 mm×0.7 mm was provided, and the second surface of the glass substrate precursor was protected by a heat-resistant coating.

[0055] The glass substrate precursor was placed in a KNO3 molten salt to perform chemical strengthening on the first surface of the glass substrate precursor. The temperature of the molten salt was 380°C, and the chemical strengthening time was 120 min. A first surface compressive stress layer with large surface compressive stress and shallow stress depth was formed on the first surface.

[0056] The heat-resistant protective coating on the second surface was removed, and the first surface of the glass substrate precursor was protected by a heat-resistant coating.

[0057] The second surface of the glass substrate precursor was chemically strengthened in two separate steps in a strengthening molten salt, the glass substrate precursor was placed in a NaNO3 molten salt to perform the first chemical strengthening on the second surface, the temperature of the molten salt was 380°C, and the time for the first chemical strengthening was 122 min, and the glass substrate precursor was placed in a mixed molten salt of 94% KNO3 and 6% NaNO3 by mass fraction to perform the second chemical strengthening, the temperature of the molten salt was 380°C, and the time for the second chemical strengthening was 10 min. A second surface compressive stress layer with small surface compressive stress and deep stress depth was formed on the second surface.

[0058] The heat-resistant protective coating on the first surface was removed to obtain a glass substrate.

[0059] The glass substrate and the electronic components are assembled to obtain a mobile phone, with the glass substrate having a first surface that is the exterior surface of the mobile phone and a second surface that is disposed inside the mobile phone (adjacent to the electronic components). EXAMPLES

[0060] The manufacturing method of the glass substrate includes:

[0061] A glass substrate precursor of Corning GG5 grade and 145 mm×70 mm×0.7 mm in size was provided, and the second surface of the glass substrate precursor was protected by a heat-resistant coating.

[0062] The glass substrate precursor was placed in a mixed molten salt of 94% KNO3 by mass fraction and 6% NaNO3 by mass fraction to perform chemical strengthening on the first surface of the glass substrate precursor. The temperature of the molten salt was 380°C, and the chemical strengthening time was 32 minutes. A first surface compressive stress layer with large surface compressive stress and shallow stress depth was formed on the first surface.

[0063] The heat-resistant protective coating on the second surface was removed, and the first surface of the glass substrate precursor was protected by a heat-resistant coating.

[0064] The second surface of the glass substrate precursor was chemically strengthened in two separate steps in a strengthening molten salt, the glass substrate precursor was placed in a NaNO3 molten salt to perform the first chemical strengthening on the second surface, the temperature of the molten salt was 380°C, and the time for the first chemical strengthening was 97 min, and the glass substrate precursor was placed in a mixed molten salt of KNO3 with a mass fraction of 62% and NaNO3 with a mass fraction of 38% to perform the second chemical strengthening, the temperature of the molten salt was 380°C, and the time for the second chemical strengthening was 10 min. A second surface compressive stress layer with small surface compressive stress and deep stress depth was formed on the second surface.

[0065] The heat-resistant protective coating on the first surface was removed to obtain a glass substrate.

[0066] The glass substrate and the electronic components are assembled to obtain a mobile phone, with the glass substrate having a first surface that is the exterior surface of the mobile phone and a second surface that is disposed inside the mobile phone (adjacent to the electronic components). EXAMPLES

[0067] The manufacturing method of the glass substrate includes:

[0068] A glass substrate precursor of grade Corning GG5 and size 145 mm×70 mm×0.7 mm was provided, and the second surface of the glass substrate precursor was protected by a heat-resistant coating.

[0069] The first surface of the glass substrate precursor was chemically strengthened in two stages in a strengthening molten salt. The glass substrate precursor was placed in a NaNO3 molten salt to perform a first chemical strengthening on the first surface, the molten salt temperature was 380°C, and the first chemical strengthening time was 30 min. The glass substrate precursor was further placed in a KNO3 molten salt to perform a second chemical strengthening, the molten salt temperature was 380°C, and the second chemical strengthening time was 20 min. A first surface compressive stress layer with large surface compressive stress and shallow stress depth was formed on the first surface.

[0070] The heat-resistant protective coating on the second surface was removed, and the first surface of the glass substrate precursor was protected by a heat-resistant coating.

[0071] The second surface of the glass substrate precursor was chemically strengthened in two separate steps in a strengthening molten salt, the glass substrate precursor was placed in a NaNO3 molten salt to perform the first chemical strengthening on the second surface, the temperature of the molten salt was 380°C, and the time for the first chemical strengthening was 65 min, and the glass substrate precursor was placed in a mixed molten salt of KNO3 with a mass fraction of 62% and NaNO3 with a mass fraction of 38% to perform the second chemical strengthening, the temperature of the molten salt was 380°C, and the time for the second chemical strengthening was 20 min. A second surface compressive stress layer with small surface compressive stress and deep stress depth was formed on the second surface.

[0072] The heat-resistant protective coating on the first surface was removed to obtain a glass substrate.

[0073] The glass substrate and the electronic components are assembled to obtain a mobile phone, with the glass substrate having a first surface that is the exterior surface of the mobile phone and a second surface that is disposed inside the mobile phone (adjacent to the electronic components). EXAMPLES

[0074] The manufacturing method of the glass substrate includes:

[0075] A glass substrate precursor of grade Corning GG5 and size 145 mm×70 mm×0.7 mm was provided, and the second surface of the glass substrate precursor was protected by a heat-resistant coating.

[0076] The first surface of the glass substrate precursor was chemically strengthened in two stages in a strengthening molten salt. The glass substrate precursor was placed in a NaNO3 molten salt to perform a first chemical strengthening on the first surface, with the molten salt temperature being 380°C and the first chemical strengthening time being 30 min. The glass substrate precursor was then placed in a KNO3 molten salt to perform a second chemical strengthening, with the molten salt temperature being 380°C and the second chemical strengthening time being 125 min. A first surface compressive stress layer with large surface compressive stress and shallow stress depth was formed on the first surface.

[0077] The heat-resistant protective coating on the second surface was removed, and the first surface of the glass substrate precursor was protected by a heat-resistant coating.

[0078] The second surface of the glass substrate precursor was chemically strengthened in two separate steps in a strengthening molten salt, the glass substrate precursor was placed in a NaNO3 molten salt to perform the first chemical strengthening on the second surface, the temperature of the molten salt was 380°C, and the time for the first chemical strengthening was 210 min, and the glass substrate precursor was placed in a mixed molten salt of KNO3 with a mass fraction of 62% and NaNO3 with a mass fraction of 38% to perform the second chemical strengthening, the temperature of the molten salt was 380°C, and the time for the second chemical strengthening was 10 min. A second surface compressive stress layer with small surface compressive stress and deep stress depth was formed on the second surface.

[0079] The heat-resistant protective coating on the first surface was removed to obtain a glass substrate.

[0080] The glass substrate and the electronic components are assembled to obtain a mobile phone, with the glass substrate having a first surface that is the exterior surface of the mobile phone and a second surface that is disposed inside the mobile phone (adjacent to the electronic components). EXAMPLES

[0081] The manufacturing method of the glass substrate includes:

[0082] A glass substrate precursor of grade Corning GG5 and size 145 mm×70 mm×0.7 mm was provided, and the second surface of the glass substrate precursor was protected by a heat-resistant coating.

[0083] The first surface of the glass substrate precursor was chemically strengthened in two stages in a strengthening molten salt. The glass substrate precursor was placed in a NaNO3 molten salt to perform a first chemical strengthening on the first surface, the molten salt temperature was 380°C, and the first chemical strengthening time was 30 min. The glass substrate precursor was further placed in a KNO3 molten salt to perform a second chemical strengthening, the molten salt temperature was 380°C, and the second chemical strengthening time was 60 min. A first surface compressive stress layer with large surface compressive stress and shallow stress depth was formed on the first surface.

[0084] The heat-resistant protective coating on the second surface was removed, and the first surface of the glass substrate precursor was protected by a heat-resistant coating.

[0085] The second surface of the glass substrate precursor was chemically strengthened in two separate steps in a strengthening molten salt, the glass substrate precursor was placed in a NaNO3 molten salt to perform the first chemical strengthening on the second surface, the temperature of the molten salt was 380°C, and the time for the first chemical strengthening was 90 min, and the glass substrate precursor was placed in a mixed molten salt of KNO3 with a mass fraction of 62% and NaNO3 with a mass fraction of 38% to perform the second chemical strengthening, the temperature of the molten salt was 380°C, and the time for the second chemical strengthening was 60 min. A second surface compressive stress layer with small surface compressive stress and deep stress depth was formed on the second surface.

[0086] The heat-resistant protective coating on the first surface was removed to obtain a glass substrate.

[0087] The glass substrate and the electronic components are assembled to obtain a mobile phone, with the glass substrate having a first surface that is the exterior surface of the mobile phone and a second surface that is disposed inside the mobile phone (adjacent to the electronic components).

[0088] Example A The method for producing a glass sheet includes the following:

[0089] A glass plate precursor was provided, Corning GG5 grade, 145 mm x 70 mm x 0.7 mm in size.

[0090] The glass plate precursor was placed in KNO3 molten salt for chemical strengthening, the temperature of the molten salt was 380°C, and the chemical strengthening time was 120 min. A symmetrical compressive stress distribution was formed on both sides of the glass plate. FIG. 5 is a stress distribution curve diagram along the thickness direction of the glass plate of Example A.

[0091] The glass plate and electronic components were assembled to obtain a mobile phone.

[0092] Example B The difference between Example B and Example A is that chemical strengthening was performed twice, and the chemical strengthening specifically includes the following:

[0093] The glass plate precursor was placed in NaNO3 molten salt for the first chemical strengthening, the temperature of the molten salt was 380°C, and the first chemical strengthening time was 8 min. The glass plate precursor was then placed in KNO3 molten salt for the second chemical strengthening, the temperature of the molten salt was 380°C, and the second chemical strengthening time was 90 min. A symmetrical compressive stress distribution was formed on the surfaces on both sides of the glass plate.

[0094] The glass plate and electronic components were assembled to obtain a mobile phone.

[0095] Example C The method for producing a glass sheet includes the following:

[0096] A glass plate precursor of Corning GG5 grade and measuring 145 mm×70 mm×0.7 mm was provided, and a second surface of the glass plate precursor was protected by a heat resistant coating.

[0097] The first surface of the glass plate precursor was chemically strengthened in two separate steps in a strengthening molten salt, and the glass plate precursor was placed in a KNO3 molten salt to chemically strengthen the first surface. The temperature of the molten salt was 380°C, and the first chemical strengthening time was 65 min.

[0098] The heat-resistant protective coating on the second surface was removed, and the first surface of the glass plate precursor was protected by a heat-resistant coating.

[0099] The second surface of the glass plate was chemically strengthened in two separate steps in a strengthening molten salt, the glass plate precursor was placed in a NaNO3 molten salt to perform the first chemical strengthening on the second surface, the molten salt temperature was 380°C, and the first chemical strengthening time was 8 minutes, and the glass plate precursor was placed in a KNO3 molten salt to perform the second chemical strengthening, the molten salt temperature was 380°C, and the second chemical strengthening time was 20 minutes. A second surface compressive stress layer with small surface compressive stress and deep stress depth was formed on the second surface.

[0100] The heat-resistant protective coating on the first surface was removed to obtain a glass plate.

[0101] The glass sheet and the electronic components are assembled to obtain a mobile phone, with the glass sheet having a first surface that is an exterior surface of the mobile phone and a second surface that is disposed within the mobile phone (adjacent to the electronic components).

[0102] (Example of comparison) In order to verify the properties of the ceramic appearance member manufactured in the present application, the present application further provides effect examples.

[0103] 1) Using FSM-6000LEUV Plus from Shenzhen Tano Instrument Co., Ltd., stress tests were performed on the glass substrates of Examples 1 to 6 and the glass plates of Examples A to C to obtain compressive stress distribution curves. The stress parameters of the glass substrates of Examples 1 to 6 and the glass plates of Examples A to C are shown in Table 1, where DOL represents the compressive stress depth, CS represents the surface compressive stress, and |S1-S2| / S x represents the ratio of the difference between the surface compressive stress integrals on both sides to the surface compressive stress integral on one side, and S xis the small compressive stress integral in the compressive stress layers on the first and second surfaces.

[0104] Table 1. Compressive stress distribution of glass substrates of Examples 1 to 6 and glass plates of Examples A to C [Table 1]

[0105] 2) Using a drop impact tester, a sandpaper drop test was performed on the products of Examples 1-6 and Examples A-C to test their impact resistance. The test method specifically includes the following: Adjust the vacuum suction nozzle of the tester to a horizontal state, suck up the electronic product, place the glass substrate or glass plate facing downward, and place the 80 mesh sandpaper horizontally on the test table surface (the test table surface is a marble plane) below the suction nozzle to ensure that the sandpaper is flat and unwarped. After the product is raised to the test height, it releases gas and begins to fall. The drop height starts from 50 cm and gradually increases by 5 cm each time until the glass surface is broken, and the height before the glass is broken (the maximum height at which the glass surface is not broken) is recorded, and the experimental results of the sandpaper drop test are shown in Table 2.

[0106] 3) A bending strength tester is used to perform bending strength tests on the glass substrates of Examples 1 to 6 and the glass plates of Examples A to C. Based on the product usage (the first surface of the glass substrate is the impact surface, and the second surface is subjected to bending tension), the bending tension of the second surface of the glass substrate and the glass plate is tested. The test process specifically includes the following: The second surface of the glass cover is placed downward and the first surface is placed upward to perform the strength test, the distance between the upper support plates is 20 mm, the distance between the lower support plates is 40 mm, the drop speed is 3 mm / min, a force is applied downward until the glass breaks, and the maximum force P at the time of breaking is recorded; The bending strength was calculated using the formula: bending strength = 3P x (40 - 20) x 0.001 / (2 x glass width x glass thickness x glass thickness).

[0107] The experimental results of the bending strength test are shown in Table 2.

[0108] Table 2: Characteristic parameters of the glass substrates of Examples 1 to 6 and the glass plates of Examples A to C [Table 2]

[0109] As can be seen from Table 2, compared with the symmetrically distributed glass plate, the glass substrate according to the embodiment of the present application has higher impact resistance and bending strength in certain application scenarios, and when applied to electronic devices, it can effectively protect the electronic devices and extend the service life of the electronic devices.

[0110] The above description is the preferred embodiment of the present application, but should not be understood as limiting the scope of the present application. However, those skilled in the art can make some improvements and modifications without departing from the principle of the present application, and these improvements and modifications are also considered to be within the protection scope of the present application.

Claims

1. A glass substrate comprising a first surface compressive stress layer and a second surface compressive stress layer on opposite sides, the surface compressive stress of the first surface compressive stress layer being greater than the surface compressive stress of the second surface compressive stress layer, and the depth of the first surface compressive stress layer being smaller than the depth of the second surface compressive stress layer.

2. 2. The glass substrate according to claim 1, wherein a ratio of an absolute value of a difference between the compressive stress integral of the first surface compressive stress layer and the compressive stress integral of the second surface compressive stress layer to the compressive stress integral of either surface compressive stress layer is 5% or less.

3. when the obtained compressive stress integral of the first surface compressive stress layer is equal to the compressive stress integral of the second surface compressive stress layer, a ratio of an absolute value of a difference between the compressive stress integral of the first surface compressive stress layer and the compressive stress integral of the second surface compressive stress layer to the compressive stress integral of the first surface compressive stress layer or the compressive stress integral of the second surface compressive stress layer is 5% or less, when the compressive stress integral of the first surface compressive stress layer is larger than the compressive stress integral of the second surface compressive stress layer, a ratio of an absolute value of a difference between the compressive stress integral of the first surface compressive stress layer and the compressive stress integral of the second surface compressive stress layer to the compressive stress integral of the second surface compressive stress layer is 5% or less; 3. The glass substrate according to claim 2, wherein when the compressive stress integral of the first surface compressive stress layer is smaller than the compressive stress integral of the second surface compressive stress layer, a ratio of an absolute value of a difference between the compressive stress integral of the first surface compressive stress layer and the compressive stress integral of the second surface compressive stress layer to the compressive stress integral of the first surface compressive stress layer is 5% or less.

4. 4. The glass substrate according to claim 1, wherein the first surface compressive stress layer has a surface compressive stress of 700 MPa to 1200 MPa, and the second surface compressive stress layer has a surface compressive stress of 300 MPa to 850 MPa.

5. 5. The glass substrate according to claim 1, wherein a ratio of a surface compressive stress of the first surface compressive stress layer to a surface compressive stress of the second surface compressive stress layer is 1.2 or more.

6. 6. The glass substrate according to claim 1, wherein, when a thickness of the glass substrate is t, a depth of the first surface compressive stress layer is 0.004 mm or more and 0.1t or less, and a depth of the second surface compressive stress layer is 0.085 mm or more and 0.6t or less.

7. 7. The glass substrate according to claim 1, wherein the glass substrate has a thickness t of 0.1 mm to 5 mm.

8. 8. The glass substrate according to claim 1, wherein the material of the glass substrate includes one or more of lithium aluminosilicate glass, soda lime silicate glass, and soda lime glass.

9. The glass substrate according to any one of claims 1 to 8, wherein the first surface compressive stress layer and / or the second surface compressive stress layer is obtained by chemically strengthening or physically strengthening a glass plate.

10. 10. The glass substrate according to claim 1, wherein the bending strength of the glass substrate is from 1000 MPa to 2100 MPa.

11. A method for producing a glass substrate according to any one of claims 1 to 10, comprising the steps of: providing a glass substrate precursor, the glass substrate precursor including two surfaces opposite to each other, and providing a first protective layer on one surface of the glass substrate precursor to obtain the glass substrate precursor having the first protective layer; A step of forming a compressive stress layer on a side of the glass substrate precursor on which the first protective layer is not provided by placing the glass substrate precursor having the first protective layer in a molten salt to perform a first tempering process; removing the first protective layer and providing a second protective layer on a surface of the glass substrate precursor having a compressive stress layer; and putting the glass substrate precursor having the second protective layer into the molten salt to perform a second strengthening on the precursor, thereby forming a compressive stress layer on a side of the glass substrate precursor on which the second protective layer is not provided, and removing the second protective layer to obtain the glass substrate.

12. 12. The method according to claim 11, wherein the molten salt is a sodium salt or a potassium salt.

13. 13. The method of claim 11 or 12, wherein the molten salt comprises one or more of potassium nitrate, sodium nitrate.

14. 14. The method according to claim 10, wherein the temperature of the molten salt is between 360°C and 450°C.

15. 15. The method according to any one of claims 10 to 14, characterized in that the duration of the first intensification and / or the second intensification is between 60 min and 200 min.

16. The method according to any one of claims 10 to 15, wherein the first strengthening and / or the second strengthening is stepwise strengthening using a plurality of types of molten salts.

17. The method according to any one of claims 10 to 16, characterized in that the first and second protective layers are heat resistant protective coatings.

18. An electronic device (100) comprising: an electronic component (20); and a glass cover covering the electronic component (20), the glass cover comprising the glass substrate according to any one of claims 1 to 10.

19. 20. The electronic device (100) of claim 18, wherein, in the glass substrate, the second surface compressive stress layer is adjacent to the electronic component (20) and the first surface compressive stress layer is away from the electronic component (20).

20. 20. The electronic device (100) according to claim 18 or 19, characterized in that the glass cover is a screen cover (10) and / or a back cover (30) of the electronic device (100).

Citation Information

Patent Citations

  • Single-sided dominant compressive stress glass

    CN209259943U

  • Chemically strengthened glass

    JP2016169143A

  • Ion exchange process and chemically strengthened glass substrate obtained thereby

    JP2016538233A

  • Glasses and glass-ceramics with metal oxide concentration gradients

    JP2017537862A

  • Window substrate and display device including the same

    JP2018024567A