Compositions and methods for preparing microencapsulated phase change materials - Patents.com

A solvent-free and surfactant-free method for PCM microencapsulation using isocyanates and amine compounds with inorganic fillers addresses leakage and efficiency issues, achieving stable and efficient PCM encapsulation with recyclable filtrate.

JP2024537147AActive Publication Date: 2024-10-10DOW GLOBAL TECHNOLOGIES LLC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024520739
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-10-28
Publication Date
2024-10-10
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

Existing methods for microencapsulating phase change materials (PCMs) face challenges such as solvent use, complex reaction control, and inefficient heat transfer, leading to leakage and low heat transfer coefficients, which are not environmentally friendly and hinder process efficiency.

Method used

A solvent-free and surfactant-free method using a composition comprising an oil phase with phase change material, aliphatic and aromatic isocyanates, and an aqueous phase with a water-soluble amine compound, allowing for rapid shell formation and encapsulation without emulsification, facilitated by inorganic fillers for stability and filtration.

Benefits of technology

The method achieves robust microencapsulation with high heat transfer efficiency, environmental sustainability, and recyclable filtrate, ensuring stable PCM performance through controlled shell thickness and prevention of leakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537147000001_ABST
    Figure 2024537147000001_ABST
Patent Text Reader

Abstract

The present disclosure relates to compositions and methods for preparing microencapsulated phase change materials, the compositions including an oil phase component and an aqueous phase component, the oil phase component having, based on the total weight of the oil phase component, 40% to 99% by weight of a phase change material; - 0.5% to 30% by weight of an aliphatic isocyanate having at least two NCO-functional groups, - 0.5% to 30% by weight of an aromatic isocyanate having at least two NCO-functional groups, (2) the aqueous phase component comprises water in an amount at least three times the total weight of the oil phase ingredients; - a water-soluble amine compound having at least two NH-functional groups, the molar ratio of NH- ​​to NCO- being between 0.5:1 and 3:1; The method is a robust and efficient process that does not require organic solvents or surfactants.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to compositions and methods for preparing microencapsulated phase change materials, which are robust and efficient processes that do not require solvents or surfactants. [Background technology]

[0002] Phase change materials (PCMs) have been widely studied and used in various kinds of applications. In building systems, many studies have proven the performance of PCMs in reducing energy consumption. Solid-liquid PCMs are the most commonly used materials and have been widely studied. Solid-liquid PCMs melt after absorbing heat, so they need to be encapsulated before being applied to building structures to prevent leakage. In general, PCMs can be stabilized by impregnation, marco-encapsulation, and microencapsulation methods. The two main characteristics are their stabilization and heat transfer coefficient. Well-encapsulated PCMs should have good stability and high heat transfer coefficient.

[0003] Impregnation is a method in which a porous matrix is ​​used to absorb the PCM. There is still a risk of leakage during the melting and solidification cycles. Usually, organic PCMs exhibit lower heat transfer coefficients. Therefore, the heat transfer coefficient of the material being impregnated depends heavily on the thermal conductivity of the matrix skeleton. Macroencapsulation (less than 1 mm) is also a simple and cheap method. However, the heat transfer coefficient is usually low. Simulation work revealed that it takes as much as 169.2 minutes to melt a 50 mm macrocapsule of wax. While the core portion may remain solid, the edge portion melts and becomes liquid form, thus preventing effective heat transfer. Microencapsulation (1-1000 μm) has proven to be an effective method to obtain high heat transfer coefficients due to its large surface area. Simulations showed that only 2.2 seconds were required when the capsule diameter was 500 μm.

[0004] To prepare PCM microcapsules, various kinds of encapsulation methods have been developed in recent decades. In situ polymerization, interfacial polymerization and emulsion polymerization are the three main methods. During interfacial polymerization, the organic PCM is emulsified in the water phase by a surfactant together with an isocyanate. Sometimes, a solvent is added to the oil phase. A curing agent such as an alcohol or an amine is slowly added to react with the NCO groups to obtain a polyurea or polyurethane shell.

[0005] However, interfacial polymerization requires carefully controlled polymerization parameters, such as stirring speed and curing agent addition rate. Furthermore, the use of a solvent is often required because phase change materials are usually immiscible with reactive aromatic isocyanates, which preferentially react quickly to form a stable shell. Solvents may be added to aid in the dissolution of other isocyanates in the organic PCM. For regulatory, environmental, and process efficiency reasons, solvents are not preferred. Another important and less obvious reason for removing the solvent is wastewater treatment considerations if the system must be filtered to recover the microcapsule powder. Such solvent-free reactor systems allow both easy separation of the encapsulated material and easy reuse of the reactor effluent water. Aqueous surfactants or colloidal stabilizers may not be preferred in processes that recycle the reactor effluent, as concentrations must be monitored and corrected to ensure that the microcapsules maintain the desired particle size.

[0006] Therefore, there is still an urgent need for a unique method for preparing microencapsulated phase change materials that can overcome the above-mentioned shortcomings and meet all requirements regarding PCM microcapsules, environmental regulations and process efficiency.

[0007] After persistent research, the present inventors have surprisingly developed a unique composition for preparing microencapsulated phase change materials by using a specially designed formulation that can overcome the above-mentioned drawbacks in the manufacture of PCM microcapsules. Summary of the Invention

[0008] The present disclosure provides a unique composition for preparing microencapsulated phase change materials and a method for preparing microencapsulated phase change materials using the composition.

[0009] In a first aspect of the present disclosure, the present disclosure provides a composition for preparing a microencapsulated phase change material, the composition comprising an oil phase component and an aqueous phase component; (1) The oil phase components are, based on the total weight of the oil phase components, 40% to 99% by weight of a phase change material; - 0.5% to 30% by weight of an aliphatic isocyanate having at least two NCO-functional groups, - 0.5% to 30% by weight of an aromatic isocyanate having at least two NCO-functional groups, Including, (2) The aqueous phase component is water in an amount at least three times the total weight of the oil phase ingredients; - a water-soluble amine compound having at least two NH-functional groups, the molar ratio of NH- ​​to NCO- being between 0.5:1 and 3:1; The present invention provides a composition comprising:

[0010] In a second aspect of the present disclosure, the present disclosure provides a composition for preparing a microencapsulated phase change material, wherein the oil phase component further comprises 5 wt % to 25 wt % of an inorganic filler, based on the total weight of the oil phase component.

[0011] In a third aspect of the present disclosure, the present disclosure provides a method for preparing a microencapsulated phase change material, the method comprising: (1) blending a mixture of an aliphatic isocyanate having at least two NCO-functional groups and an aromatic isocyanate having at least two NCO-functional groups with a phase change material to form an oil phase component, the oil phase component having, based on the total weight of the oil phase component, 40% to 99% by weight of a phase change material; - 0.5% to 30% by weight of an aliphatic isocyanate having at least two NCO-functional groups, - 0.5% to 30% by weight of an aromatic isocyanate having at least two NCO-functional groups, blending, (2) dissolving an amine compound having at least two NH-functional groups in water to form an aqueous phase component, the aqueous phase component comprising: water in an amount at least three times the total weight of the oil phase ingredients; - a water-soluble amine compound having at least two NH-functional groups, the molar ratio of NH- ​​to NCO- being between 0.5:1 and 3:1; and (3) adding, under agitation, the oil phase component to the water phase component to form a microencapsulated phase change material.

[0012] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention, as claimed. [Brief description of the drawings]

[0013] [Figure 1] 1 is an optical microscope photograph of a comparative example in the present disclosure. [Diagram 2] 1 is an optical microscope photograph of an embodiment of the present invention in the present disclosure. [Diagram 3] 1A is an optical micrograph of inventive Example 1 of the present disclosure at room temperature (a), a polarized light micrograph at room temperature (b), and a polarized light micrograph at 50° C. (c). [Figure 4] 1 is a DSC curve of 20 freeze-thaw cycles in the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs, and all publications, patent applications, patents, and other references mentioned herein are incorporated by reference.

[0015] As disclosed herein, "and / or" means "and, or alternatively" or "in addition, or alternatively." All ranges are inclusive of the endpoints unless otherwise indicated.

[0016] In certain embodiments of the present disclosure, the composition for preparing the microencapsulated phase change material comprises an oil phase component and a water phase component (ie, a two-component system). The oil phase component contains 40 wt% to 99 wt%, 40 wt% to 90 wt%, 40 wt% to 80 wt%, 40 wt% to 70 wt%, 40 wt% to 60 wt%, 40 wt% to 50 wt%, 50 wt% to 99 wt%, 50 wt% to 90 wt%, 50 wt% to 80 wt%, 50 wt% to 70 wt%, 50 wt% to 60 wt%, 60 wt% to 99 wt%, 60 wt% to 90 wt%, 60 wt% to 80 wt%, 60 wt% to 70 wt%, 70 wt% to 99 wt%, 470 wt% to 90 wt%, 70 wt% to 80 wt%, 80 wt% to 99 wt%, 80 wt% to 90 wt%, or 90 wt% to 99 wt% of the phase change material based on the total weight of the oil phase component. The oil phase component comprises 0.5 wt% to 30 wt%, 0.5 wt% to 25 wt%, 0.5 wt% to 20 wt%, 0.5 wt% to 15 wt%, 0.5 wt% to 10 wt%, 0.5 wt% to 5 wt%, 5 wt% to 30 wt%, 5 wt% to 25 wt%, 5 wt% to 20 wt%, 5 wt% to 15 wt%, 5 wt% to 10 wt%, 10 wt% to 30 wt%, 10 wt% to 25 wt%, 1.0 wt% to 20 wt%, 1.0 wt% to 15 wt%, 15 wt% to 30 wt%, 15 wt% to 25 wt%, 15 wt% to 20 wt%, 20 wt% to 30 wt%, 20 wt% to 25 wt%, or 25 wt% to 30 wt%, based on the total weight of the oil phase component. The oil phase component comprises 0.5 wt% to 30 wt%, 0.5 wt% to 25 wt%, 0.5 wt% to 20 wt%, 0.5 wt% to 15 wt%, 0.5 wt% to 10 wt%, 0.5 wt% to 5 wt%, 5 wt% to 30 wt%, 5 wt% to 25 wt%, 5 wt% to 20 wt%, 5 wt% to 15 wt%, 5 wt% to 10 wt%, 10 wt% to 30 wt%, 10 wt% to 25 wt%, 1.0 wt% to 20 wt%, 1.0 wt% to 15 wt%, 15 wt% to 30 wt%, 15 wt% to 25 wt%, 15 wt% to 20 wt%, 20 wt% to 30 wt%, 20 wt% to 25 wt%, or 25 wt% to 30 wt%, based on the total weight of the oil phase component.

[0017] In some embodiments of the present disclosure, the aqueous phase component comprises water in an amount at least 3 times, at least 4 times, or at least 5 times the total weight of the oil phase component, and the amine compound having at least two NH-functional groups is used in a molar ratio of NH- ​​to NCO- of 0.5:1 to 3:1, 0.5:1 to 2:1, 0.5:1 to 1:1, 0.5:1 to 0.7:1, 0.7:1 to 3:1, 0.7:1 to 2:1, 0.7:1 to 1:1, 1:1 to 3:1, 1:1 to 2:1, or 2:1 to 3:1.

[0018] In some embodiments of the present disclosure, the phase change material may include an organic PCM or a eutectic PCM. Examples of phase change materials include paraffin hydrocarbons (e.g., C14-C45 paraffin hydrocarbons, e.g., paraffin wax, C14, C18, C22-C45 hydrocarbons, e.g., tetradecane, pentadecane, hexadecane, heptadecane, octadecane), carboxylic acid esters (e.g., fatty acid esters, methyl laurate, ethyl laurate, methyl stearate, ethyl stearate, methyl behenate, and ethyl behenate), carboxylic acids (e.g., fatty acids, capric acid, lauric acid, tetradecanoic acid, pentadecanoic acid, hexadecanoic acid, octadecanoic acid), polyalcohols (e.g., polyethylene glycol (PEG)), and the like.

[0019] In certain embodiments of the present disclosure, the aliphatic isocyanates having at least two NCO-functional groups include aliphatic diisocyanates and their dimers and trimers, C2-C8 alkylene diisocyanates, such as tetramethylene diisocyanate and hexamethylene diisocyanate (HDI), 1,12-dodecane diisocyanate, 2,2,4-trimethyl-hexamethylene diisocyanate, 2,4,4-trimethyl-hexamethylene diisocyanate, 2-methyl-1,5-pentamethylene diisocyanate; alicyclic diisocyanates and their dimers and trimers, such as isophorone diisocyanate (IPDI) and dicyclohexyl methane diisocyanate. diisocyanate (HMDI), 1,4-cyclohexane diisocyanate, and 1,3-bis-(isocyanatomethyl)cyclohexane; aromatic diisocyanates and their dimers and trimers, such as toluene diisocyanate (TDI) and diphenyl methane diisocyanate (MDI). Preferably, the aliphatic isocyanate is a hexamethylene diisocyanate homopolymer, a hexamethylene diisocyanate adduct, an isophorone diisocyanate homopolymer, an isophorone diisocyanate adduct, or a mixture thereof. Most preferably, the aliphatic isocyanate having at least two NCO-functional groups is selected from the group consisting of methylene-bis(cyclohexylisocyanate) (HMDI), hexamethylene-diisocyanate (HDI), tetramethylene-diisocyanate, cyclohexane-diisocyanate, hexahydrotoluene diisocyanate, isophorone diisocyanate (IPDI), and any mixture thereof.

[0020] In one embodiment of the present disclosure, the aromatic isocyanate compound is a C6-C aryl isocyanate having at least two isocyanate (NCO-) groups. 15 Aromatic isocyanate compound. C6~C15 The aromatic isocyanate compound may be selected from the group consisting of diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), naphthalene diisocyanate (NDI), phenylene diisocyanate, any isomer thereof, and any combination thereof. Isomers of MDI include 4,4'-MDI, 2,4'-MDI, 2,2'-MDI, etc. Isomers of TDI include 2,3-TDI, 2,4-TDI, 2,5-TDI, 2,6-TDI, 3,4-TDI, 3,5-TDI, etc. Isomers of NDI include 1,5-NDI, 1,2-NDI, 1,3-NDI, 1,4-NDI, 1,6-NDI, 1,7-NDI, 1,8-NDI, 2,3-NDI, 2,6-NDI, 2,7-NDI, etc. The isomers of phenylene diisocyanate include 1,2-phenylene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, etc. The aromatic isocyanate compound may include any one or more of the isomers shown above. According to an embodiment of the present invention, the aromatic isocyanate compound is MDI, for example, a mixture of 4,4'-MDI and 2,4'-MDI, specifically, a mixture of 50-99% by weight of 4,4'-MDI and 1-50% by weight of 2,4'-MDI, or a mixture of 98% by weight of 4,4'-MDI and 2% by weight of 2,4'-MDI. Preferably, the aromatic isocyanate compound is selected from the group consisting of polymethylene polyphenylisocyanate, diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), naphthalene diisocyanate (NDI), phenylene diisocyanate, and any combination thereof.

[0021] In some embodiments of the present disclosure, the amine compound is water-soluble and comprises aromatic polyamines having at least two NH-functional groups, with primary amino groups directly bonded to the carbon atoms of the aromatic ring. Examples of such aromatic polyamines include 2,4- and / or 2,6-toluene diamine (TDA), 4,4'-, 2,4'- and 2,2'-diphenylmethane diamine (MDA), or mixtures of any two or more thereof. The water-soluble amine compound having at least two NH-functional groups can include alicyclic polyamines such as hydrogenated MDA, 1-methyl-2,4-diaminocyclohexane, 1-methyl-2,6-diaminocyclohexane, etc. The amine compounds are water-soluble and have at least two NH-functional groups, which may include aliphatic polyamines such as tetramethylene-1,4-diamine, hexamethylene-1,6-diamine, trimethylhexanediamine, tetramethylhexanediamine, isophoronediamine, 1,3- and / or 1,4-bis(aminomethyl)cyclohexane, and 2,4- or 2,6-diamine-1-methylecyclohexane. Preferably, the amine compound is selected from the group consisting of diethylenetriamine (DETA), triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, ethylenediamine (EDA), propylenediamine and triethylenediamine, 2,4- and / or 2,6-toluenediamine (TDA), 4,4'-, 2,4'- and 2,2'-diphenylmethanediamine (MDA), 1-methyl-2,4-diaminocyclohexane, 1-methyl-2,6-diaminocyclohexane, tetramethylene-1,4-diamine, hexamethylene-1,6-diamine, trimethylhexanediamine, tetramethylhexanediamine, isophoronediamine, 1,3- and / or 1,4-bis(aminomethyl)cyclohexane and 2,4- or 2,6-diamine-1-methylecyclohexane, and any combination thereof.

[0022] In certain embodiments of the present disclosure, the oil phase component further comprises 5% to 25%, 5% to 20%, 5% to 15%, 5% to 10%, 10% to 25%, 10% to 20%, 10% to 15%, 15% to 25%, 15% to 20%, or 20% to 25% by weight of an inorganic filler, based on the total weight of the oil phase component. Exemplary inorganic fillers include, but are not limited to, natural calcium carbonates including chalk, calcite, and marble, synthetic carbonates, magnesium and calcium salts, dolomite, magnesium carbonate, zinc carbonate, lime, magnesia, barium sulfate, barite, calcium sulfate, silica, magnesium silicate, talc, wollastonite, clay, and aluminum silicate, kaolin, mica, metal or alkaline earth oxides or hydroxides, magnesium hydroxide, iron oxide, zinc oxide, glass or carbon fibers or powders, or powders or mixtures of these compounds. Preferably, the inorganic filler is selected from the group consisting of CaCO3, talc, mica, SiO2, TiO2, kaolin, coal gangue powder, sepiolite powder, attapulgite powder, montmorillonite, and any combination thereof.

[0023] In some embodiments of the present disclosure, there is no need to add surfactant to the composition, so there is no emulsification process. The amine compound as the curing agent is added first and dissolved in the water phase. Then the oil phase component is added to the water phase component. During the addition, the isocyanate in the oil phase component reacts quickly with the curing agent to form a thin film and maintain the shape of the microcapsule. The oil phase dispersion and shell formation occur almost simultaneously. This process is straightforward and robust. The composition for preparing the microencapsulated phase change material is substantially free of any surfactant (e.g., sulfate surfactant, sulfonate surfactant, nonionic surfactant, etc.), stabilizer, organic solvent, and emulsifier (e.g., sodium salt of styrene maleic anhydride copolymer, sodium dodecylbenzene sulfonate, alkylphenol polyoxyethylene ether (OP-10), etc.). In general, surfactants include anionic surfactants, cationic surfactants, amphoteric surfactants or nonionic surfactants, such as sulfate salts of ethoxylated phenols, such as poly(oxy-1,2-ethanediyl) α-sulfo-ω(nonylphenoxy) salts; alkali metal fatty acid salts, such as alkali metal oleates and stearates; alkali metal C 12 ~C 16 Alkyl sulfates, such as alkali metal lauryl sulfates; amine C 12 ~C 16 Alkyl sulfates, such as amine lauryl sulfate, or triethanolamine lauryl sulfate; alkali metal C 12 ~C 16 Alkylbenzene sulfonates, e.g., sodium branched and linear dodecylbenzene sulfonate; amines such as triethanolamine dodecylbenzene sulfonate; 12 ~C 16 Alkylbenzene sulfonates; Fluorinated C4-C 16 Alkyl esters and alkali metals C4-C 16 Anionic and nonionic fluorocarbon emulsifiers, such as perfluoroalkylsulfonates; organosilicon emulsifiers, such as modified polydimethylsiloxanes.

[0024] In certain embodiments of the invention, the microcapsule structure comprises one or a combination of a core-shell structure, a single-shell structure, a multi-shell structure, a single cavity-single core structure, a single cavity-multicore structure, a multi-cavity-multicore structure, a porous structure, a skeletal structure, and a three-dimensional network structure.

[0025] The present disclosure provides an exemplary composition for preparing a microencapsulated phase change material, the composition comprising an oil phase component and an aqueous phase component, (1) The oil phase components are, based on the total weight of the oil phase components, 40% to 99% by weight of paraffin wax; - 0.5% to 30% by weight of isophorone diisocyanate (IPDI) and / or dicyclohexylmethane-4,4'-diisocyanate (HMDI), 0.5% by weight to 30% by weight of polymethylene polyphenylisocyanate; -5% by weight to 25% by weight of CaCO3 and / or talc; Including, (2) The aqueous phase component is water in an amount at least three times the total weight of the oil phase ingredients; diethylenetriamine (DETA) in which the molar ratio of NH- ​​to NCO- is from 0.5:1 to 3:1; A composition comprising:

[0026] In one embodiment of the present disclosure, there is provided a method for preparing a microencapsulated phase change material, comprising the steps of: (1) blending a mixture of an aliphatic isocyanate having at least two NCO-functional groups and an aromatic isocyanate having at least two NCO-functional groups with a phase change material to form an oil phase component; (2) dissolving an amine compound having at least two NH-functional groups in water to form an aqueous phase component; (3) adding, under agitation, the oil phase component to the water phase component to form a dispersion of microencapsulated phase change material.

[0027] In a further embodiment of the present disclosure, step (1) further comprises blending the mixture of an aliphatic isocyanate having at least two NCO-functional groups and an aromatic isocyanate having at least two NCO-functional groups, and the phase change material with an inorganic filler. In an alternative embodiment of the present disclosure, step (3) further comprises adding an inorganic filler to the water phase component separately from or together with the oil phase component.

[0028] In a further embodiment of the present disclosure, the method for preparing a microencapsulated phase change material further comprises, after step (3), step (4) of filtering the dispersion to provide a microencapsulated phase change material powder, which step (4) also produces a filtrate.

[0029] In a further embodiment of the present disclosure, the method for preparing a microencapsulated phase change material further comprises, after step (4), recycling the filtrate to step (3).

[0030] In the present disclosure, an exemplary method for preparing a microencapsulated phase change material includes: 1) blending a mixture of an aliphatic isocyanate having at least two NCO-functional groups and an aromatic isocyanate having at least two NCO-functional groups with paraffin wax and inorganic fillers (e.g., anti-caking agents, e.g., CaCO3 and / or talc) to form an oil phase; 2) dissolving an amine compound having at least two NH-functional groups (as a curing agent) in water to provide an aqueous phase; 3) Pour the oil phase into the water phase while stirring, alternatively do not use surfactants, colloidal stabilizers and internal stabilizers (such as DMPA); 4) curing the mixture obtained in 3) for several hours (e.g., 8 hours) to provide a microcapsule dispersion; 5) filtering the dispersion to form a microcapsule powder and a filtrate; 6) recycling the filtrate to 3) for polymerization.

[0031] The present disclosure provides a feasible microencapsulation method for obtaining organic PCM microcapsules, which has the following advantages: a) Robust and efficient processes; b) does not use solvents or surfactants; c) the filtrate is reusable, and d) The shell thickness can be controlled to balance cost and leak protection. EXAMPLES

[0032] Some embodiments of the present invention are now described in the following examples, in which all parts and percentages are by weight unless otherwise specified.

[0033] Information on the raw materials used in the examples is listed in Table 1 below.

[0034] [Table 1]

[0035] Examples 1 to 5 of the present invention and Comparative Examples 1 to 4 In the following Inventive Examples (IE) 1-5 and Comparative Examples (CE) 1-4, microencapsulated phase change materials were prepared according to the compositions and processes set forth in Table 2.

[0036] A. Preparation of the Oil Phase For IE1-4 and CE1-4, the wax was heated to about 50° C. to obtain a hot liquid wax. The aliphatic and aromatic isocyanate mixture and filler (if present) were added to the hot liquid wax according to the composition set forth in Table 2.

[0037] In IE5, the wax was heated to about 50° C. to obtain a hot liquid wax. An aliphatic and aromatic isocyanate mixture was added to the hot liquid wax according to the composition set forth in Table 2.

[0038] B. Preparation of the Aqueous Phase For IE1-5 and CE1-4, the water was heated to about 50° C. and then the curing agent was added according to the composition listed in Table 2.

[0039] C. Mixing the Oil and Water Phases In IE1-5 and CE1-4, the hot oil phase was poured into the water phase while stirring at approximately 500 rpm.

[0040] D. Curing by interfacial polymerization For IE1-4 and CE1-4, aliphatic and aromatic isocyanate mixtures were cured with a curing agent via interfacial polymerization at about 50° C. for 6 hours to obtain dispersions of microencapsulated phase change materials.

[0041] In IE5, the aliphatic and aromatic isocyanate mixture was cured with a curing agent via interfacial polymerization for 6 hours at about 50° C. to obtain a dispersion of microencapsulated phase change material. After 6 hours of interfacial polymerization, 10 g of 800 mesh mica powder was added.

[0042] E. Filtration of the Dispersion The dispersions of the microencapsulated phase change materials (IE1-4) or the microcapsule agglomerates (CE3-4) were filtered to obtain microcapsule powders.

[0043] [Table 2]

[0044] Testing and Evaluation The morphology of the microencapsulated phase change materials obtained in IE1-5 and CE1-4 was examined by optical microscopy. In IE1-5 and CE1-4, a droplet of the cured PCM dispersion was taken and placed on a glass slide. The droplet of the dispersion was then dried at room temperature and then placed under an optical microscope for observation.

[0045] FIG. 1 shows optical micrographs of comparative examples CE1-4. FIG. 2 shows optical micrographs of inventive examples IE1-5. FIG. 3(a) shows an optical micrograph of IE1 at room temperature. FIG. 3(b) shows a polarized light micrograph of IE1 at room temperature. FIG. 3(c) shows a polarized light micrograph of IE1 at 50° C. (c). FIG. 4 shows the DSC curves of 20 freeze-melt cycles.

[0046] Comparing CE1 in Figure 1 with IE1 in Figure 2, it can be seen that microcapsules cannot be obtained if the water phase does not contain an amine hardener. The isocyanate mixture in CE1 is reacted with water, but the reaction rate is not fast enough to form a solid shell to protect the microcapsules, even when the temperature is increased to about 50°C. The amine in the water phase is an essential component to immediately react with the isocyanate to form a solid shell when the oil phase is dispersed in the water phase.

[0047] Microcapsules can also be formed when the oil phase does not contain fillers (CE2 in Figure 1). However, the dispersion becomes thick after the reaction, which means that the polymer from the reaction between the isocyanate in the water phase and the amine or water thickens the dispersion. Furthermore, the resulting microcapsules cannot be filtered due to their weak shell. The added inorganic filler not only helps the precipitation of the polyurea polymer on the microcapsule surface, but also plays an important role in preventing caking of the filtered microcapsules. Different kinds of inorganic fillers can be used, such as CaCO3, mica powder, talcum powder, etc.

[0048] Aliphatic isocyanates such as IPDI, HMDI and HDI are miscible with wax liquids, while aromatic isocyanates usually have relatively low solubility in wax liquids. Therefore, a mixture of aliphatic and aromatic isocyanates was used to balance solubility, reaction rate and crosslink density. Microcapsules were obtained using these compositions and are shown in Figure 2. The size of the microcapsules ranges from 1 to 200 mm.

[0049] IPDI was used to prepare microcapsules. The product morphology is shown in CE3 in Figure 1. Only microcapsule aggregates could be obtained. This is believed to be due to the fact that the hydrophilic IPDI-DETA prepolymer formed diffused into the aqueous phase and the microdroplets aggregated with each other. PAPI27 was also used in the product form shown in CE4 in Figure 1. Due to its low solubility in the wax liquid and too fast reaction rate, aggregation of the microcapsules also occurred.

[0050] IE1 to IE3 in FIG. 2 indicate the following. -Mixtures of aliphatic and aromatic isocyanates can provide a good balance between solubility and reaction rate to produce microcapsules rather than agglomeration of microcapsules (CE3-4 in Figure 1 vs. IE1-3 in Figure 2). - An amine hardener in the water phase is an essential component (CE1 in Figure 1 vs. IE1-3 in Figure 2). With the aid and reinforcement of inorganic fillers, the microcapsules can be filtered to form a powder or slurry (IE1-3 in Fig. 2 versus CE2 in Fig. 1). - Different types of fillers can be used (IE2 in Fig. 1 vs. IE1 in Fig. 2). - PCMs with different melting points can be used (IE3 in Fig. 1 vs. IE1 and IE2 in Fig. 2).

[0051] As shown in IE4 of Figure 2, the filtrate can be recycled and used in the aqueous phase so that the inventive method of preparing microencapsulated PCM is environmentally friendly. As shown in IE5, the filler cake prevention aid may be added after the reaction, which may provide more latitude in the manufacturing process.

[0052] The obtained microcapsules can achieve good solidification-melting stability, as shown in Figure 3. Figure 3(a) shows an optical microscope photograph of IE1 in Figure 2 at room temperature. When the wax is in a crystalline phase, it shows bright crystalline domains under a polarized microscope, as shown in Figure 3(b). When the wax in the microcapsules melts after heating, the bright crystalline domains disappear, as shown in Figure 3c. The stability is also evidenced by DSC tests. As shown in IE3 in Figure 2, after 20 cycles of heating and cooling of the microcapsules, no latent heat reduction occurs, as shown in Figure 4.

Claims

1. A composition for preparing a microencapsulated phase change material, the composition comprising an oil phase component and an aqueous phase component, (1) The oil phase component contains, based on the total weight of the oil phase component, - 40% to 99% by weight of a phase change material; - 0.5% to 30% by weight of an aliphatic isocyanate having at least two NCO-functional groups, - 0.5% to 30% by weight of an aromatic isocyanate having at least two NCO-functional groups, Including, (2) The aqueous phase component is - water in an amount of at least three times the total weight of the oil phase components; - a water-soluble amine compound having at least two NH-functional groups, the molar ratio of NH- ​​to NCO- being between 0.5:1 and 3:1, A composition comprising:

2. The oil phase component is, based on the total weight of the oil phase component, - 50% to 90% by weight of a phase change material; - 5% to 25% by weight of an aliphatic isocyanate having at least two NCO-functional groups; - 5% to 25% by weight of an aromatic isocyanate having at least two NCO-functional groups, The composition of claim 1 , comprising:

3. The aqueous phase component is - water in an amount of at least 4 times the total weight of the oil phase components; - an amine compound having at least two NH-functional groups, the molar ratio of NH- ​​to NCO- being from 0.7:1 to 2:

1.

4. the aliphatic isocyanate is selected from the group consisting of methylene-bis(cyclohexylisocyanate) (HMDI), hexamethylene-diisocyanate (HDI), tetramethylene-diisocyanate, cyclohexane-diisocyanate, hexahydrotoluene diisocyanate, isophorone diisocyanate (IPDI), and any mixture thereof; the aromatic isocyanate compound is selected from the group consisting of polymethylene polyphenylisocyanate, diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), naphthalene diisocyanate (NDI), phenylene diisocyanate, and any combination thereof; and / or The composition according to any one of claims 1 to 3, wherein the amine compound is selected from the group consisting of diethylenetriamine (DETA), triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, ethylenediamine (EDA), propylenediamine and triethylenediamine, 2,4- and / or 2,6-toluenediamine (TDA), 4,4'-, 2,4'- and 2,2'-diphenylmethanediamine (MDA), 1-methyl-2,4-diaminocyclohexane, 1-methyl-2,6-diaminocyclohexane, tetramethylene-1,4-diamine, hexamethylene-1,6-diamine, trimethylhexanediamine, tetramethylhexanediamine, isophoronediamine, 1,3- and / or 1,4-bis(aminomethyl)cyclohexane and 2,4- or 2,6-diamine-1-methylecyclohexane, and any combination thereof.

5. The oil phase component further comprises 5% by weight to 25% by weight of an inorganic filler based on the total weight of the oil phase component, and the inorganic filler is CaCO 3 , talc, mica, SiO 2 , TiO 2 4. The composition of claim 1, wherein the inorganic filler is selected from the group consisting of: kaolin, coal gangue powder, sepiolite powder, attapulgite powder, montmorillonite, and any combination thereof.

6. The composition according to any one of claims 1 to 3, wherein the composition is free of surfactants, stabilizers, organic solvents and emulsifiers.

7. 1. A method for preparing a microencapsulated phase change material, comprising: (1) blending a mixture of an aliphatic isocyanate having at least two NCO-functional groups and an aromatic isocyanate having at least two NCO-functional groups with a phase change material to form an oil phase component, the oil phase component having, based on the total weight of the oil phase component, - 40% to 99% by weight of a phase change material; - 0.5% to 30% by weight of an aliphatic isocyanate having at least two NCO-functional groups, - 0.5% to 30% by weight of an aromatic isocyanate having at least two NCO-functional groups, blending, (2) dissolving an amine compound having at least two NH-functional groups in water to form an aqueous phase component, the aqueous phase component comprising: - water in an amount of at least three times the total weight of the oil phase components; an amine compound having at least two NH-functional groups, the molar ratio of NH- ​​to NCO- being from 0.5:1 to 3:1, and (3) adding, under stirring, the oil phase component to the water phase component to form a dispersion of microencapsulated phase change material; A method comprising:

8. The oil phase component is, based on the total weight of the oil phase component, - 50% to 90% by weight of a phase change material; - 5% to 25% by weight of an aliphatic isocyanate having at least two NCO-functional groups; - 5% to 25% by weight of an aromatic isocyanate having at least two NCO-functional groups, The method of claim 7, comprising:

9. The aqueous phase component is - water in an amount of at least 4 times the total weight of the oil phase components; an amine compound having at least two NH-functional groups, the molar ratio of NH- ​​to NCO- being from 0.7:1 to 2:1, The method of claim 7, comprising:

10. the aliphatic isocyanate is selected from the group consisting of methylenebis(cyclohexylisocyanate) (HMDI), hexamethylene-diisocyanate (HDI), tetramethylene-diisocyanate, cyclohexane-diisocyanate, hexahydrotoluene diisocyanate, isophorone diisocyanate (IPDI), and any mixture thereof; the aromatic isocyanate compound is selected from the group consisting of polymethylene polyphenylisocyanate, diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), naphthalene diisocyanate (NDI), phenylene diisocyanate, and any combination thereof; and / or 10. The method of any one of claims 7 to 9, wherein the amine compound is selected from the group consisting of diethylenetriamine (DETA), triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, ethylenediamine (EDA), propylenediamine and triethylenediamine, 2,4- and / or 2,6-toluenediamine (TDA), 4,4'-, 2,4'- and 2,2'-diphenylmethanediamine (MDA), 1-methyl-2,4-diaminocyclohexane, 1-methyl-2,6-diaminocyclohexane, tetramethylene-1,4-diamine, hexamethylene-1,6-diamine, trimethylhexanediamine, tetramethylhexanediamine, isophoronediamine, 1,3- and / or 1,4-bis(aminomethyl)cyclohexane and 2,4- or 2,6-diamine-1-methylecyclohexane, and any combination thereof.

11. 10. The method of any one of claims 7 to 9, wherein step (1) further comprises blending the mixture, phase change material, with an inorganic filler such that the oil phase component further comprises 5 wt% to 25 wt% of an inorganic filler, based on the total weight of the oil phase component.

12. Step (3) further comprises adding an inorganic filler in an amount of 5% to 25% by weight based on the total weight of the oil phase components, the inorganic filler being CaCO 3 , talc, mica, SiO 2 , TiO 2 10. The method of any one of claims 7 to 9, wherein the inorganic fine particles are selected from the group consisting of: kaolin, coal gangue powder, sepiolite powder, attapulgite powder, montmorillonite, and any combination thereof.

13. The method according to any one of claims 7 to 9, wherein the method is free of surfactants, stabilizers, organic solvents and emulsifiers.

14. 10. The method of claim 7, further comprising, after step (3), a step (4) of filtering the dispersion to provide a microencapsulated phase change material powder, the step (4) also producing a filtrate.

15. 15. The method of claim 14, wherein the method further comprises, after step (4), recycling the filtrate to step (3).

Citation Information

Patent Citations

  • Method for preparing paraffin phase change microcapsules from lignin emulsification particles

    CN110079279A

  • Thermal storage medium microcapsule and building materials or fabrics using the same

    JP2003003158A

  • Micro capsule for heat storage and micro capsule sheet

    JP2018076485A

  • Heat storage sheet

    JP2018154663A

  • Encapsulates

    US20180215983A1