Electrochemical Devices
Incorporating tin chloride in the electrolyte of lithium metal secondary batteries forms a protective layer on the lithium metal negative electrode, addressing the depletion of salts and additives, enhancing efficiency and extending the battery's lifespan by suppressing dendrite growth and improving charging/discharging efficiency.
Patent Information
- Application Number
- JP2024521032
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-01-11
- Filing Date
- 2023-01-11
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-01-11
AI Technical Summary
Lithium metal secondary batteries, such as lithium-sulfur batteries, suffer from depletion of salts and additives in the electrolyte due to side reactions, leading to decreased charging/discharging efficiency and shortened battery life due to dendrite growth and instability of the lithium metal negative electrode.
Incorporating tin chloride into the non-aqueous electrolyte with a content of 0.5% to 5% by weight, which forms a Li-Cl and Li-Sn alloy protective layer on the lithium metal negative electrode during the initial charging/discharging process, preventing depletion of salts and additives and suppressing dendrite growth.
Improves lithium charging/discharging efficiency, enhances lithium usage efficiency, and extends the lifespan of the electrochemical device by forming a stable protective layer that prevents side reactions and maintains electrolyte integrity.
Smart Images

Figure 2024537211000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrochemical device, and more particularly to an electrochemical device having improved life characteristics by preventing depletion of salts and additives in an electrolyte.
[0002] This application claims priority to Korean Patent Application No. 10-2022-0004176, filed on January 11, 2022, the entire contents of which are incorporated herein by reference in their entirety in the specification and drawings. [Background technology]
[0003] As interest in energy storage technology grows, the fields of application are expanding to include energy in mobile phones, tablets, laptops, and video cameras, as well as electric vehicles (EVs) and hybrid electric vehicles (HEVs), and research and development on electrochemical devices is gradually increasing. Electrochemical devices are the field that has attracted the most attention in this regard, and recently, the development of such batteries has led to research and development on new electrode and battery designs to improve capacity density and specific energy.
[0004] Among these electrochemical devices, lithium metal secondary batteries that use lithium metal as the anode, such as lithium-sulfur batteries (Li-S batteries), have a theoretical capacity of 3,862mAh / g, making them the next generation high capacity batteries, as they use lightweight lithium metal as the anode active material. In lithium-sulfur batteries, a reduction reaction of sulfur and an oxidation reaction of lithium metal occur during discharge, at which time sulfur changes from a ring structure of S8 to a linear structure of lithium polysulfide (LiPS), and such lithium-sulfur batteries are characterized by a stepwise discharge voltage until the polysulfide is completely reduced to Li2S.
[0005] However, in lithium metal secondary batteries such as lithium-sulfur batteries, the charge / discharge efficiency decreases during the charge / discharge process due to side reactions of the electrolyte (accumulation of by-products due to the decomposition of the electrolyte) and instability of lithium metal (occurrence of short circuits due to the growth of dendrites on the lithium metal anode), shortening the battery life.
[0006] In particular, lithium metal, which is the negative electrode active material, easily forms large-area dendrites and reacts with salts and additives in the electrolyte to form a solid electrolyte interphase (SEI), which continuously consumes the salts and additives in the electrolyte and ultimately accelerates battery degradation.
[0007] Therefore, the use of lithium metal as the negative electrode necessitates the development of technology to prevent the depletion of salts and additives in the electrolyte. Summary of the Invention [Problem to be solved by the invention]
[0008] Therefore, an object of the present invention is to provide an electrochemical device capable of preventing depletion of salts and additives in an electrolyte. [Means for solving the problem]
[0009] In order to solve the above problems, according to one aspect of the present invention, there is provided an electrochemical device according to the following embodiment.
[0010] The first embodiment relates to an electrochemical element including a positive electrode, a lithium metal negative electrode, a separator interposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte solution including tin chloride (SnCl2).
[0011] In the second embodiment, in the first embodiment, the content of the tin chloride may be 0.5% by weight to 5% by weight with respect to 100% by weight of the entire non-aqueous electrolyte solution.
[0012] In the third embodiment, in the first or second embodiment, the content of the tin chloride may be 1 wt % to 4 wt % with respect to 100 wt % of the total non-aqueous electrolyte solution.
[0013] A fourth embodiment is any one of the first to third embodiments, and may further include a Li-Cl and Li-Sn alloy protective layer on the surface of the lithium metal negative electrode.
[0014] In the fifth embodiment, in any one of the first to fourth embodiments, the nonaqueous electrolyte solution may further include a first solvent including a heterocyclic compound that may or may not include one or more double bonds and that includes one or more oxygen atoms and sulfur atoms, a second solvent including one or more of an ether compound, an ester compound, an amide compound, and a carbonate compound, a lithium salt, and lithium nitrate.
[0015] The sixth embodiment is the fifth embodiment, wherein the lithium salt is LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiC4BO8, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (C2F5SO2)2NLi, (SO2F)2NLi, (CF3SO2)2NLi, (CF3SO2)3CLi, lithium chloroborane, lithium aliphatic carboxylates having 4 or less carbon atoms, lithium 4-phenylborate, lithium imide, or two or more of these.
[0016] In the seventh embodiment, in the fifth or sixth embodiment, the concentration of the lithium salt may be 0.2 to 2.0M.
[0017] In the eighth embodiment, in any one of the fifth to seventh embodiments, the heterocyclic compound may be a 3- to 15-membered heterocyclic compound substituted or unsubstituted with one or more selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, a cyclic alkyl group having 3 to 8 carbon atoms, an aryl group having 6 to 10 carbon atoms, a halogen group, a nitro group, an amine group, and a sulfonyl group, or may be a polycyclic compound of a heterocyclic compound and one or more of a cyclic alkyl group having 3 to 8 carbon atoms and an aryl group having 6 to 10 carbon atoms.
[0018] In the ninth embodiment, in any one of the fifth to eighth embodiments, the heterocyclic compound is 1,3-dioxolane, 4,5-diethyl-1,3-dioxolane, 4,5-dimethyl-1,3-dioxolane, 4-methyl-1,3-dioxolane, 4-ethyl-1,3-dioxolane, 1,3-dioxane, 1,4-dioxane, 4-methyl-1,3-dioxane, and 2-methyl-1,3-dioxane, furan, 2-methylfuran, 3-methylfuran, 2-ethylfuran, 2-propyl The thiophene may include furan, 2-butylfuran, 2,3-dimethylfuran, 2,4-dimethylfuran, 2,5-dimethylfuran, pyran, 2-methylpyran, 3-methylpyran, 4-methylpyran, benzofuran, 2-(2-nitrovinyl)furan, thiophene, 2-methylthiophene, 2-ethylthiophene, 2-propylthiophene, 2-butylthiophene, 2,3-dimethylthiophene, 2,4-dimethylthiophene, 2,5-dimethylthiophene, or two or more thereof.
[0019] A tenth embodiment is any one of the fifth to ninth embodiments, wherein the ether compound of the second solvent is dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, dimethoxyethane, diethoxyethane, methoxyethoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, triethylene glycol methyl ethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol methyl ethyl ether, polyethylene glycol dimethyl ether, polyethylene glycol diethyl ether, polyethylene glycol methyl ethyl ether, or two or more of these.
[0020] In an eleventh embodiment, in any one of the first to tenth embodiments, the nonaqueous electrolyte may further include lanthanum nitrate, potassium nitrate, cesium nitrate, magnesium nitrate, barium nitrate, lithium nitrite, potassium nitrite, cesium nitrite, or two or more of these.
[0021] In a twelfth embodiment, in any one of the first to eleventh embodiments, the nonaqueous electrolyte may further include 1,3-dioxolane as a first solvent, dimethoxyethane as a second solvent, (CF3SO2)2NLi as a lithium salt, and lithium nitrate.
[0022] A thirteenth embodiment is any one of the first to twelfth embodiments, in which the electrochemical device can be a lithium-sulfur battery.
[0023] In a fourteenth embodiment, in any one of the first to twelfth embodiments, the electrochemical device may be a lithium-lithium symmetric cell. Effect of the Invention
[0024] The electrochemical device according to an embodiment of the present invention includes tin chloride in the non-aqueous electrolyte, which can improve lithium charge / discharge efficiency and suppress the growth of dendrites.
[0025] In addition, the electrochemical device according to an embodiment of the present invention includes tin chloride in the non-aqueous electrolyte, thereby improving the lithium usage efficiency, thereby increasing the capacity and lifespan of the electrochemical device.
[0026] In an electrochemical device according to an embodiment of the present invention, the content of tin chloride in the non-aqueous electrolyte is 0.5 wt % to 4 wt % based on 100 wt % of the total non-aqueous electrolyte, thereby preventing a side reaction between tin chloride and a positive electrode active material and more easily improving the life of the electrochemical device.
[0027] In the electrochemical device according to an embodiment of the present invention, tin chloride contained in the non-aqueous electrolyte reacts with the lithium metal anode during an initial charge / discharge process to form a lithophilic / high ion conductive Li-Cl and Li-Sn alloy protective layer on the surface of the lithium metal anode, thereby making it easier to improve the life span of the electrochemical device.
[0028] The following drawings attached to this specification illustrate preferred embodiments of the present invention and, together with the detailed description of the invention, serve to further understand the technical ideas of the present invention. Therefore, the present invention should not be interpreted as being limited only to the matters described in the drawings. [Brief description of the drawings]
[0029] [Figure 1] FIG. 2 shows the interface resistance of the lithium-lithium symmetric cell produced in Example 2-1. [Diagram 2] FIG. 2 shows the interface resistance of the lithium-lithium symmetric cell produced in Example 2-2. [Diagram 3] FIG. 13 shows the interface resistance of the lithium-lithium symmetric cell produced in Example 2-3. [Figure 4]FIG. 13 shows the interface resistance of the lithium-lithium symmetric cell produced in Example 2-4. [Diagram 5] FIG. 13 shows the interface resistance of the lithium-lithium symmetric cell produced in Example 2-5. [Figure 6] FIG. 13 shows the interface resistance of the lithium-lithium symmetric cell produced in Example 2-6. [Figure 7] FIG. 13 is a graph showing the interface resistance of a lithium-lithium symmetric cell produced in Comparative Example 2-1. [Figure 8] FIG. 2 shows the cycle life performance of the lithium-lithium symmetric cell prepared in Example 2-1. [Figure 9] FIG. 2 shows the cycle life performance of the lithium-lithium symmetric cell prepared in Example 2-2. [Figure 10] FIG. 13 shows the cycle life performance of the lithium-lithium symmetric cell prepared in Example 2-3. [Figure 11] FIG. 13 shows the cycle life performance of the lithium-lithium symmetric cells prepared in Example 2-4. [Figure 12] FIG. 13 shows the cycle life performance of the lithium-lithium symmetric cells prepared in Example 2-5. [Figure 13] FIG. 13 shows the cycle life performance of the lithium-lithium symmetric cells prepared in Example 2-6. [Figure 14] FIG. 13 shows the cycle life performance of the lithium-lithium symmetric cell prepared in Comparative Example 2-1. [Figure 15] FIG. 2 shows the cycle life performance of the lithium-sulfur batteries produced in Examples 3-1 to 3-6 and Comparative Example 3-1. [Figure 16] FIG. 3 is a photograph showing the surface of the lithium metal negative electrode of the lithium-sulfur battery produced in Example 3-3 after 100 cycles of operation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the attached drawings. Prior to this, the terms and words used in the present specification and claims are not to be construed as being limited to their ordinary and dictionary meanings, but are to be construed as having meanings and concepts according to the technical ideas of the present invention, in accordance with the principle that the inventors themselves can appropriately define the concepts of terms in order to best describe the invention.
[0031] Therefore, it should be understood that the configurations shown in the embodiments described in this specification are merely the most preferred embodiments of the present invention and do not represent the entire technical idea of the present invention, and therefore there may be various equivalents and modifications that can be substituted therefor at the time of this application.
[0032] An electrochemical device according to an embodiment of the present invention includes a positive electrode, a lithium metal negative electrode, a separator interposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte solution including tin chloride (SnCl2).
[0033] The positive electrode includes a positive electrode active material, a binder, and a conductive material. The positive electrode active material is applied to a general electrochemical element and may include, for example, a lithium nickel cobalt manganese-based compound (lithium NCM-based compound), elemental sulfur (S8), a sulfur-based compound, or a mixture thereof. Specifically, the sulfur-based compound may be Li2Sn (n≧1), an organic sulfur compound, or a carbon-sulfur complex (C2S x ) n(x=2.5 to 50, n≧2). The positive electrode active material may include a sulfur-carbon composite, and since the sulfur material alone does not have electrical conductivity, it may be used in combination with a conductive material. The carbon material (or carbon source) constituting the sulfur-carbon composite may be any material commonly used in the art that has a porous structure or a high specific surface area. For example, the porous carbon material may be, but is not limited to, graphite, graphene, carbon black such as denka black, acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black, carbon nanotubes (CNT) such as single-walled carbon nanotubes (SWCNT) or multi-walled carbon nanotubes (MWCNT), carbon fibers such as graphite nanofibers (GNF), carbon nanofibers (CNF), or activated carbon fibers (ACF), or activated carbon, or two or more of these. The shape of the porous carbon material is not particularly limited as long as it is spherical, rod-like, needle-like, plate-like, tubular, or bulk-like and applicable to an electrochemical device.
[0034] In addition, the carbon material has pores, and the porosity of the pores may be 40 to 90%, or 60 to 80%. When the porosity of the pores is within the above range, lithium ions are easily transferred normally, and the problem of a decrease in mechanical strength is easily prevented. The pore size of the carbon material may be 10 nm to 5 μm, or 50 nm to 5 μm. When the pore size of the carbon material is within the above range, lithium ions are easily transmitted, and the short circuit and safety problems of the battery due to contact between electrodes are easily prevented.
[0035] The binder is a component for binding the positive electrode active material and the conductive material and binding to the current collector, and examples of the binder include polyvinylidene fluoride (PVdF), polyvinylidene fluoride-polyhexafluoropropylene copolymer (PVdF / HFP), polyvinyl acetate, polyvinyl alcohol, polyvinyl ether, polyethylene, polyethylene oxide, alkylated polyethylene oxide, polypropylene, polymethyl (meth)acrylate, polyethyl (meth)acrylate, polytetrafluoroethylene (PTFE), polyvinyl chloride, polyacrylonitrile, polyvinylpyridine, polyvinylpyrrolidone, styrene-butadiene rubber, acrylonitrile-butadiene rubber, ethylene-propylene-diene monomer (EPDM) rubber, sulfonated EPDM rubber, styrene-butylene rubber, fluororubber, carboxymethylcellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, and two or more of these may be used, but are not necessarily limited thereto.
[0036] The binder may be added in an amount of 1 to 50 parts by weight, or 3 to 15 parts by weight, based on 100 parts by weight of the total weight of the positive electrode. When the content of the binder satisfies the above-mentioned range, it is easy to ensure the adhesive strength between the positive electrode active material and the current collector, and it is easy to ensure the battery capacity.
[0037] The conductive material contained in the positive electrode is not particularly limited as long as it does not cause side reactions in the internal environment of the electrochemical element, does not cause chemical changes in the battery, and has excellent electrical conductivity. Representative examples include graphite or conductive carbon. For example, graphite such as natural graphite and artificial graphite, carbon black, acetylene black, ketjen black, denka black, thermal black, channel black, furnace black, lamp black, and thermal black, carbon-based substances having a graphene or graphite crystal structure, conductive fibers such as carbon fibers and metal fibers, fluorine carbon, metal powders such as aluminum powder and nickel powder, conductive whiskey such as zinc oxide and potassium titanate, conductive oxides such as titanium oxide, and conductive polymers such as polyphenylene derivatives, or two or more of these can be used, but are not necessarily limited to these.
[0038] The conductive material may be added in an amount of 0.5 to 50 parts by weight, or 1 to 30 parts by weight, based on 100 parts by weight of the total weight of the positive electrode. When the content of the conductive material satisfies the above-mentioned range, it is easy to improve electrical conductivity, easy to prevent deterioration of electrochemical properties, and easy to ensure the capacity and energy density of the positive electrode.
[0039] The method of including a conductive material in the positive electrode is not particularly limited, and a conventional method known in the art, such as coating the positive electrode active material, can be used. In addition, if necessary, a conductive second coating layer can be added to the positive electrode active material instead of adding the conductive material as described above.
[0040] In addition, a filler can be selectively added to the positive electrode of the present invention as a component for suppressing the expansion of the electrode. Such a filler is not particularly limited as long as it can suppress the expansion of the electrode without causing a chemical change in the battery, and for example, olefin polymers such as polyethylene and polypropylene, and fibrous materials such as glass fiber and carbon fiber can be used.
[0041] The positive electrode can be manufactured by dispersing and mixing the positive electrode active material, binder, conductive material, etc. in a dispersion medium (solvent) to prepare a slurry, applying the slurry onto a positive electrode current collector, and then drying and rolling the slurry. The dispersion medium can be, but is not necessarily limited to, NMP (N-methyl-2-pyrrolidone), DMF (dimethyl formamide), DMSO (dimethyl sulfoxide), ethanol, isopropanol, water, and mixtures thereof.
[0042] The positive electrode current collector may be, but is not limited to, platinum (Pt), gold (Au), palladium (Pd), iridium (Ir), silver (Ag), ruthenium (Ru), nickel (Ni), stainless steel (STS), aluminum (Al), molybdenum (Mo), chromium (Cr), carbon (C), titanium (Ti), tungsten (W), ITO (In doped SnO2), FTO (F doped SnO2), and alloys thereof, and aluminum (Al) or stainless steel surface-treated with carbon (C), nickel (Ni), titanium (Ti), or silver (Ag). The positive electrode current collector may be in the form of a foil, a film, a sheet, a punched one, a porous body, a foam, or the like.
[0043] The negative electrode is lithium metal, and may further include a current collector on one side of the lithium metal. The current collector may be a negative electrode current collector. The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be selected from the group consisting of copper, aluminum, stainless steel, zinc, titanium, silver, palladium, nickel, iron, chromium, alloys thereof, and combinations thereof. The stainless steel may be surface-treated with carbon, nickel, titanium, or silver, and the alloy may be an aluminum-cadmium alloy. In addition to these, calcined carbon, a non-conductive polymer or a conductive polymer surface-treated with a conductive material, etc. may also be used. In general, a copper thin plate is used as the negative electrode current collector.
[0044] In addition, the negative electrode current collector may be in various forms, such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc., with or without microscopic irregularities on the surface. In addition, the negative electrode current collector may have a thickness in the range of 3 to 500 μm. When the thickness of the negative electrode current collector satisfies the above range, it is easy to ensure processability even when the cell is folded and assembled while ensuring the current collecting effect.
[0045] The lithium metal may be lithium or a lithium alloy, which may include an element capable of being alloyed with lithium, specifically an alloy of lithium with at least one element selected from the group consisting of Si, Sn, C, Pt, Ir, Ni, Cu, Ti, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Sb, Pb, In, Zn, Ba, Ra, Ge, and Al.
[0046] The lithium metal may be in the form of a sheet or foil, and in some cases, may be in the form of lithium or a lithium alloy deposited or coated on a current collector by a dry process, or may be in the form of metals and alloys on particles deposited or coated by a wet process, etc.
[0047] A conventional separator may be interposed between the positive electrode and the negative electrode. The separator is a physical separator having a function of physically separating the electrodes, and may be any type of separator that is used as a conventional separator, and is particularly preferred to have low resistance to ion transfer in the electrolyte and excellent electrolyte humidification. The separator separates or insulates the positive electrode and the negative electrode from each other, and allows lithium ions to be transported between the positive electrode and the negative electrode. Such a separator may be made of a porous, non-conductive or insulating material. The separator may be an independent member such as a film, or a coating layer added to the positive electrode and / or the negative electrode.
[0048] Examples of polyolefin-based porous membranes that can be used as the separation membrane include membranes formed from polyolefin-based polymers such as polyethylene (e.g., high density polyethylene, linear low density polyethylene, low density polyethylene, and ultra-high molecular weight polyethylene), polypropylene, polybutylene, and polypentene, either alone or in combination. Examples of nonwoven fabrics that can be used as the separator include nonwoven fabrics made of polymers such as polyphenylene oxide, polyimide, polyamide, polycarbonate, polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyphenylene sulfide, polyacetal, polyethersulfone, polyether ether ketone, and polyester, either alone or in combination. Such nonwoven fabrics are in the form of fibers forming a porous web, and may be in the form of spunbond or meltblown made of long fibers.
[0049] The thickness of the separator is not particularly limited, but may be 1 to 100 μm, or 5 to 50 μm. When the thickness of the separator is within the above range, the mechanical properties can be maintained and the problem of the separator acting as a resistance layer and the deterioration of the battery performance can be easily prevented. The pore size and porosity of the separator are not particularly limited, but the pore size may be 0.1 to 50 μm, and the porosity may be 10 to 95%. When the pore size of the separator is within the above range, the separator is easily prevented from acting as a resistance layer and the mechanical properties of the separator can be easily maintained.
[0050] The tin chloride improves the lithium charge / discharge efficiency and inhibits the growth of dendrites, and contributes to increasing the capacity and lifespan of the battery by improving the lithium utilization efficiency.
[0051] Conventionally, lithium metal is supported in a solvent in which metal chloride is dissolved, and a lithium alloy / Li-Cl protective layer is formed on the surface of the lithium metal anode.
[0052] However, such an ex-situ protective layer formation method has limitations such as low reactivity of metal chlorides due to non-uniformity of the lithium metal surface and the presence of a native oxide layer on the lithium metal surface, and destruction of the protective layer during the initial charge / discharge process.
[0053] The inventors of the present invention have found that the life of a battery can be improved by using tin chloride as an electrolyte additive, and have completed the present invention.
[0054] When tin chloride is included in the non-aqueous electrolyte as an electrolyte additive, it is possible to overcome the low reactivity between lithium and tin chloride caused by the native oxide layer on the surface of the lithium metal negative electrode.
[0055] In one embodiment of the present invention, tin chloride can form Li-Cl and Li-Sn alloy protective layers in-situ on the surface of the lithium metal negative electrode during the initial charge / discharge process when the natural oxide film on the surface of the lithium metal negative electrode is destroyed, and thus the Li-Cl and Li-Sn alloy protective layers can be included on the surface of the lithium metal negative electrode.
[0056] The tin chloride contained in the non-aqueous electrolyte can etch the natural oxide film, which has high interfacial resistance on the surface of lithium during the initial charge and discharge process, and can reduce the interfacial resistance between lithium and the electrolyte. At the same time, the tin chloride can react with the lithium metal negative electrode to form a lithophilic Li-Cl and Li-Sn alloy protective layer on the surface of the lithium metal negative electrode, which improves the lithium charge and discharge efficiency and makes it easier to suppress the growth of dendrites. The Li-Cl and Li-Sn alloy protective layer functions as a stable electrode protective layer that prevents the depletion of salts and additives in the electrolyte. By including the Li-Cl and Li-Sn alloy protective layer on the surface of the lithium metal negative electrode, the life of the electrochemical device can be more easily improved.
[0057] In one embodiment of the present invention, the content of the tin chloride may be 0.5% to 5% by weight, 0.7% to 5% by weight, 1% to 5% by weight, 0.7% to 4% by weight, 1% to 4% by weight, 1% to 3% by weight, or 1% to 2% by weight, based on 100% by weight of the entire non-aqueous electrolyte. When the content of the tin chloride satisfies the above-mentioned range, the problem of the deterioration of the battery being promoted due to the side reaction between the tin chloride and the positive electrode active material is prevented, and the life improvement effect is more easily exhibited. In particular, when the content of the tin chloride is 1% to 2% by weight based on 100% by weight of the entire non-aqueous electrolyte, the life of the electrochemical element can be most improved.
[0058] In one embodiment of the present invention, the non-aqueous electrolyte may further include a first solvent including a heterocyclic compound having one or more double bonds and including at least one oxygen atom and at least one sulfur atom; a second solvent including at least one of an ether-based compound, an ester-based compound, an amide-based compound, and a carbonate-based compound; a lithium salt; and lithium nitrate.
[0059] Hereinafter, the first solvent, the second solvent, the lithium salt, and the lithium nitrate contained in the nonaqueous electrolyte according to one embodiment of the present invention will be specifically described.
[0060] First Solvent The first solvent includes a heterocyclic compound containing one or more double bonds and one or more oxygen atoms and sulfur atoms. The first solvent has a property of making it difficult to dissolve salt due to delocalization of lone pair electrons of the heteroatom (oxygen atom or sulfur atom). Therefore, a polymer protective film (solid electrolyte interphase, SEI layer) is formed on the surface of lithium metal through a ring opening polymerization reaction of the heterocyclic compound in the initial discharge stage of the battery, thereby suppressing the generation of lithium dendrites. Furthermore, decomposition of the electrolyte on the surface of lithium metal and the resulting side reactions are reduced, thereby improving the life characteristics of the electrochemical device.
[0061] That is, the heterocyclic compound of the present invention may contain one or more double bonds in order to form a polymer protective film on the surface of lithium metal, and must contain one or more heteroatoms (oxygen atoms or sulfur atoms) in order to exert effects such as having polarity and increasing affinity with other solvents in the electrolyte.
[0062] The heterocyclic compound may be a 3- to 15-membered, 3- to 7-membered, or 5- to 6-membered heterocyclic compound. The heterocyclic compound may be a heterocyclic compound substituted or unsubstituted with one or more selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, a cyclic alkyl group having 3 to 8 carbon atoms, an aryl group having 6 to 10 carbon atoms, a halogen group, a nitro group (-NO2), an amine group (-NH2), and a sulfonyl group (-SO2). The heterocyclic compound may be a polycyclic compound of a heterocyclic compound and one or more of a cyclic alkyl group having 3 to 8 carbon atoms and an aryl group having 6 to 10 carbon atoms.
[0063] When the heterocyclic compound is substituted with an alkyl group having 1 to 4 carbon atoms, the radicals are stabilized, and side reactions of the electrolyte gun can be suppressed. When the heterocyclic compound is substituted with a halogen group or a nitro group, a functional protective film can be formed on the surface of lithium metal, and the formed functional protective film can be stabilized as a compact protective film. In addition, uniform deposition of lithium metal is possible. In particular, when the electrochemical device is a lithium-sulfur battery, side reactions between polysulfide and lithium metal can be suppressed.
[0064] Specific examples of the heterocyclic compound include 1,3-dioxolane, 4,5-diethyl-1,3-dioxolane, 4,5-dimethyl-1,3-dioxolane, 4-methyl-1,3-dioxolane, 4-ethyl-1,3-dioxolane, and 1,3-dioxane. ane, 1,4-dioxane, 4-methyl-1,3-dioxane, 2-methyl-1,3-dioxane, furan, 2-methylfuran, 3-methylfuran, 2-ethylfuran, 2-propylfuran, 2-butylfuran, 2,3-dimethylfuran Examples of thiophene include 2,3-dimethylfuran, 2,4-dimethylfuran, 2,5-dimethylfuran, pyran, 2-methylpyran, 3-methylpyran, 4-methylpyran, benzofuran, 2-(2-nitrovinyl)furan, thiophene, 2-methylthiophene, 2-ethylthiophene, 2-propylthiophene, 2-butylthiophene, 2,3-dimethylthiophene, 2,4-dimethylthiophene, and 2,5-dimethylthiophene.The first solvent containing such a heterocyclic compound may be included in a volume ratio of 5 to 50 with respect to a volume ratio of 100 of the total organic solvent (i.e., first solvent + second solvent) included in the nonaqueous electrolyte according to one embodiment of the present invention (the remainder corresponds to the second solvent). When the content of the first solvent satisfies the above-mentioned range, it is easy to prevent the problem that a protective film is not completely formed on the lithium metal surface, and it is easy to prevent the problem that the capacity and life of the battery are reduced due to an increase in the surface resistance of the electrolyte and lithium metal.
[0065] In particular, when the positive electrode active material is sulfur, the ability to reduce the amount of polysulfide eluted decreases, making it difficult to suppress an increase in the resistance of the electrolyte, which is a problem that can be easily prevented.
[0066] Second Solvent The second solvent includes at least one of an ether-based compound, an ester-based compound, an amide-based compound, and a carbonate-based compound, and not only dissolves a lithium salt to impart lithium ion conductivity to the electrolyte, but also dissolves a positive electrode active material to facilitate an electrochemical reaction with lithium. In particular, when the positive electrode active material is sulfur, the second solvent dissolves the positive electrode active material sulfur to facilitate an electrochemical reaction with lithium.
[0067] The carbonate-based compound may be a linear carbonate-based compound or a cyclic carbonate-based compound.
[0068] Specific examples of the ether-based compound include dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, dimethoxyethane, diethoxyethane, methoxyethoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, triethylene glycol methyl ethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol methyl ethyl ether, polyethylene glycol dimethyl ether, polyethylene glycol diethyl ether, polyethylene glycol methyl ethyl ether, or two or more of these, but are not limited thereto.
[0069] Examples of the ester compound include, but are not limited to, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, ε-caprolactone, or two or more of these.
[0070] The amide-based compound may be any conventional amide-based compound used in the art.
[0071] Examples of the linear carbonate compound include, but are not limited to, dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), ethylmethyl carbonate (EMC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), or two or more of these.
[0072] Examples of the cyclic carbonate compound include, but are not limited to, ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, vinylethylene carbonate, halides thereof (such as fluoroethylene carbonate (FEC)), or two or more of these.
[0073] The second solvent may be included in a volume ratio of 50 to 95 with respect to a volume ratio of 100 of the total organic solvent (i.e., first solvent + second solvent) included in the nonaqueous electrolyte according to an embodiment of the present invention. When the content of the second solvent satisfies the above-mentioned range, the lithium salt can be sufficiently dissolved, and the problem of the lithium ion conductivity decreasing can be easily prevented, and the problem of the positive electrode active material being precipitated beyond the concentration at which it dissolves can be easily prevented. In particular, when the positive electrode active material is sulfur, the problem of the sulfur of the positive electrode active material being precipitated beyond the concentration at which it dissolves can be easily prevented, and the problem of the shuttle phenomenon between lithium polysulfide and lithium metal anode being aggravated due to the excessive dissolution of sulfur, resulting in a shortened lifespan, can be easily prevented.
[0074] Meanwhile, the organic solvent including the first solvent and the second solvent may be included in an amount of 60 to 99.5 wt%, or 60 to 99 wt%, or 60 to 98 wt%, or 60 to 95 wt%, based on 100 wt% of the total nonaqueous electrolyte according to an embodiment of the present invention. When the content of the organic solvent satisfies the above range, it is easy to prevent a problem in which the viscosity of the electrolyte increases and the ionic conductivity decreases, or a problem in which the lithium salt or additives are not completely dissolved in the electrolyte, and it is easy to prevent a problem in which the concentration of the lithium salt in the electrolyte decreases and the ionic conductivity decreases.
[0075] Lithium salts The lithium salt is an electrolyte salt used to increase ionic conductivity, and examples thereof include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiC4BO8, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (C2F5SO2)2NLi, (SO2F)2NLi (i.e., LiFSI), (CF3SO2)2NLi (i.e., LiTFSI), (CF3SO2)3CLi, lithium chloroborane, lithium aliphatic carboxylate having 4 or less carbon atoms, lithium 4-phenylborate, lithium imide, or two or more of these. In particular, using (CF3SO2)2Nli or (SO2F2)Nli as the lithium salt may be advantageous in that it has high solubility in the first solvent and / or second solvent and high lithium ion conductivity.
[0076] The concentration of the lithium salt may be determined in consideration of ion conductivity, and may be, for example, 0.2 to 2 M, or 0.5 to 1 M. When the concentration of the lithium salt satisfies the above-mentioned range, it is easy to ensure ion conductivity suitable for driving the battery, and it is possible to prevent the viscosity of the electrolyte from increasing, which reduces the mobility of lithium ions, or prevents an increase in the decomposition reaction of the lithium salt itself.
[0077] Lithium nitrate The non-aqueous electrolyte according to an embodiment of the present invention may include lithium nitrate (LiNO3). Lithium nitrate reacts with the lithium metal negative electrode to form a lithophilic protective film, such as lithium nitride (Li3N) or lithium oxynitride (LiON), on the surface of the lithium metal negative electrode, thereby suppressing the growth of lithium dendrites and preventing decomposition of electrolyte components, thereby improving battery life and efficiency.
[0078] If necessary, the non-aqueous electrolyte may further contain lanthanum nitrate (La(NO3)3), potassium nitrate (KNO3), cesium nitrate (CsNO3), magnesium (MgNO3), barium nitrate (BaNO3), lithium nitrite (LiNO2), potassium nitrite (KNO2), cesium nitrite (CsNO2), or two or more of these.
[0079] The lithium nitrate may be contained in an amount of 0.1 to 7 wt%, or 0.5 to 5 wt%, or 0.5 to 1.5 wt%, based on 100 wt% of the total non-aqueous electrolyte. When the lithium nitrate content is within the above range, it is easy to prevent the problem of a sudden decrease in coulombic efficiency and the phenomenon of an increase in the viscosity of the electrolyte.
[0080] The non-aqueous electrolyte according to an embodiment of the present invention may include 1,3-dioxolane as a first solvent, dimethoxyethane as a second solvent, (CF3SO2)2NLi as a lithium salt, lithium nitrate, and tin chloride. The 1,3-dioxolane and dimethoxyethane have high lithium polysulfide solubility and can stabilize the lithium metal negative electrode. Therefore, when the non-aqueous electrolyte includes the above-mentioned materials, optimal electrochemical device characteristics can be exhibited.
[0081] The electrochemical device of the present invention includes all devices that perform electrochemical reactions, and specific examples thereof include all kinds of primary and secondary batteries, fuel cells, solar cells, and capacitors such as supercapacitor devices.
[0082] In one embodiment of the present invention, the electrochemical device is any lithium secondary battery commonly used in the art that uses lithium metal as a negative electrode, and may be a lithium-sulfur battery or a lithium-lithium symmetric cell.
[0083] The electrochemical device according to an embodiment of the present invention including the above-mentioned positive electrode, negative electrode, separator, and electrolyte may be manufactured by a process of placing a positive electrode opposite to a negative electrode, interposing a separator therebetween, and then injecting a nonaqueous electrolyte according to an embodiment of the present invention.
[0084] Meanwhile, the lithium secondary battery according to an embodiment of the present invention can be applied to a battery cell used as a power source for a small device, and can be particularly suitably used as a unit battery of a battery module that is a power source for a medium-sized or large device. In view of this, the present invention further provides a battery module including two or more electrochemical devices electrically connected (series or parallel). The number of electrochemical devices included in the battery module can be variously adjusted in consideration of the use and capacity of the battery module. The present invention further provides a battery pack in which the battery modules are electrically connected according to a conventional technique in the art. The battery module and the battery pack can be used as a power source for one or more medium-sized or large devices including a power tool, an electric vehicle (EV), a hybrid electric vehicle (HEV), and an electric vehicle (PHEV), an electric truck, an electric commercial vehicle, or a power storage system, but are not necessarily limited thereto.
[0085] The present invention will be described in detail below with reference to examples for better understanding. However, the examples according to the present invention may be modified into various other forms, and the scope of the present invention should not be construed as being limited to the following examples. The embodiments of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.
[0086] Example 1-1 First, 1 wt% lithium nitrate and 0.5 wt% tin chloride were added to an organic solvent made by mixing 1,3-dioxolane (first solvent) and dimethoxyethane (second solvent) in a 1:1 volume ratio (v / v) based on the total weight of the electrolyte, and dissolved to a concentration of 1M (CF3SO2)2NLi(LiTFSI) (lithium salt) to prepare a non-aqueous electrolyte.
[0087] Example 1-2 A non-aqueous electrolyte solution was prepared in the same manner as in Example 1-1, except that 1 wt % tin chloride was added instead of 0.5 wt % tin chloride.
[0088] Examples 1-3 A non-aqueous electrolyte solution was prepared in the same manner as in Example 1-1, except that 2 wt % tin chloride was added instead of 0.5 wt % tin chloride.
[0089] Examples 1-4 A non-aqueous electrolyte solution was prepared in the same manner as in Example 1-1, except that 3 wt % tin chloride was added instead of 0.5 wt % tin chloride.
[0090] Examples 1-5 A non-aqueous electrolyte solution was prepared in the same manner as in Example 1-1, except that 4 wt % tin chloride was added instead of 0.5 wt % tin chloride.
[0091] Examples 1-6 A non-aqueous electrolyte solution was prepared in the same manner as in Example 1-1, except that 5 wt % tin chloride was added instead of 0.5 wt % tin chloride.
[0092] Comparative Example 1-1 A non-aqueous electrolyte solution was prepared in the same manner as in Example 1-1, except that tin chloride was not added.
[0093] Examples 2-1 to 2-6 and Comparative Example 2-1: Preparation of Lithium-Lithium Symmetric Cell Lithium was cross-rolled to a thickness of 35 μm onto a copper current collector to prepare two electrodes, one for each of the positive and negative electrodes, with the lithium facing each other. A porous polyethylene (PE) separator having a thickness of 16 μm was then interposed between the positive and negative electrodes, and the non-aqueous electrolytes prepared in Examples 1-1 to 1-6 and Comparative Example 1-1 were then injected and sealed to prepare a coin cell type lithium-lithium symmetric cell.
[0094] Examples 3-1 to 3-6 and Comparative Example 3-1: Manufacture of lithium-sulfur batteries First, 87.5 parts by weight of a sulfur-carbon (CNT) composite (S / C 75:25 weight ratio) as a positive electrode active material, 5 parts by weight of Denka Black as a conductive material, and 7.5 parts by weight of styrene butadiene rubber / carboxymethyl cellulose (SBR / CMC 7:3) as a binder were mixed to prepare a positive electrode slurry composition, which was then applied to one side of a current collector (Al foil), dried at 80°C, and rolled using a roll press device to prepare a positive electrode (at this time, the loading amount was 4 mg / cm). 2 (I did.)
[0095] Next, the prepared positive electrode and a negative electrode in which lithium was cross-rolled to a thickness of 35 μm on a copper current collector were disposed opposite each other, and a porous polyethylene (PE) separator was interposed between them. Then, the nonaqueous electrolytes prepared in Examples 1-1 to 1-6 and Comparative Example 1-1 were injected and sealed to prepare coin cell type lithium-sulfur batteries.
[0096] Evaluation example 1: Evaluation of interface resistance and cycle life of lithium-lithium symmetric cell The interface resistance and cycle life of the lithium-lithium symmetric cells prepared in Examples 2-1 to 2-6 and Comparative Example 2-1 were evaluated and are shown in Table 1 and FIGS. 1 to 14.
[0097] The interfacial resistance of the lithium-lithium symmetric cell was determined by measuring the impedance of the lithium-lithium symmetric cells prepared in Examples 2-1 to 2-6 and Comparative Example 2-1 at a temperature of 25° C. in a frequency range of 0.1 Hz to 1 MHz using electrochemical impedance spectroscopy (EIS), and defining the radius of the first semicircle as the interfacial resistance (R).
[0098] The cycle life of the lithium-lithium symmetric cells was 1.5 mA / cm at 25° C. for the lithium-lithium symmetric cells prepared in Examples 2-1 to 2-6 and Comparative Example 2-1. 2 The discharge (lower limit -1V) and charge (upper limit +1V) cycles were repeated at a current density of 100 mA, and the potential was measured over time (cycles).
[0099] [Table 1]
[0100] As can be seen from Table 1 and Figures 1 to 7, the lithium-lithium symmetric cells prepared in Examples 2-1 to 2-6 containing tin chloride in the electrolyte were found to have reduced interfacial resistance compared to the lithium-lithium symmetric cell prepared in Comparative Example 2-1 containing no tin chloride in the electrolyte. This is because the native oxide film on the surface of the lithium metal negative electrode, which has high interfacial resistance, is etched by tin chloride, and a lithophilic Li-Cl and Li-Sn alloy protective layer is formed on the surface of the lithium metal negative electrode.
[0101] In addition, as can be seen from Table 1 and Figures 8 to 14, the lithium-lithium symmetric cells prepared in Examples 2-1 to 2-6 containing tin chloride in the electrolyte were confirmed to have improved life spans compared to the lithium-lithium symmetric cell prepared in Comparative Example 2-1 containing no tin chloride in the electrolyte. In particular, the lithium-lithium symmetric cells prepared in Examples 2-1 to 2-5, in which the tin chloride content was 0.5 wt % to 4 wt % relative to 100 wt % of the total electrolyte, were confirmed to have further improved life spans.
[0102] Evaluation example 2: Evaluation of cycle life of lithium-sulfur battery The lithium-sulfur batteries prepared in Examples 3-1 to 3-6 and Comparative Example 3-1 were subjected to 0.2C charge / 0.3C discharge cycles in the voltage range of 1.8V to 2.5V in CC mode at a temperature of 25°C to measure the capacity-potential according to the charge-discharge cycles (after a stabilization process of initial 0.1C / 0.1C 2.5 cycles and 0.2C / 0.2C 3 cycles, the batteries were driven at 0.3C / 0.5C from the 7th cycle). The results are shown in Table 2 and FIG. 15.
[0103] [Table 2]
[0104] As can be seen from Table 2 and FIG. 15, it was confirmed that the lithium-sulfur batteries prepared in Examples 3-1 to 3-6 containing tin chloride in the electrolyte had improved life spans compared to the lithium-sulfur battery prepared in Comparative Example 3-1 containing no tin chloride in the electrolyte. In particular, it was confirmed that the lithium-sulfur batteries prepared in Examples 3-1 to 3-5, in which the tin chloride content was 0.5 wt% to 4 wt% based on 100 wt% of the total electrolyte, had further improved life spans. Among them, it was confirmed that the lithium-sulfur battery prepared in Example 3-2, in which the tin chloride content was 1 wt% based on 100 wt% of the total electrolyte, had a significantly improved life span, and the lithium-sulfur battery prepared in Example 3-3, in which the tin chloride content was 2 wt% based on 100 wt% of the total electrolyte, had the longest life span.
[0105] Evaluation example 3: Analysis of the surface of the lithium metal negative electrode of a lithium-sulfur battery After the lithium-sulfur battery prepared in Example 3-3 was operated for 100 cycles, the surface of the lithium metal anode of the lithium-sulfur battery was analyzed using a transmission electron microscope (SEM) EDS (energy dispersive spectroscopy) and the results are shown in FIG. 16.
[0106] As can be seen in Figure 16, Sn and Cl were detected on the surface of the lithium metal negative electrode even after the battery was operated. This confirmed that Li-Cl and Li-Sn alloy protective layers were present on the surface of the lithium metal negative electrode even after the battery was operated.
Claims
1. A positive electrode, a lithium metal negative electrode, a separator interposed between the positive electrode and the negative electrode, and tin chloride (SnCl 2 and a non-aqueous electrolyte solution containing the same.
2. 2. The electrochemical element according to claim 1, wherein the content of said tin chloride is 0.5% by weight to 5% by weight with respect to 100% by weight of the total non-aqueous electrolyte.
3. 2. The electrochemical element according to claim 1, wherein the content of said tin chloride is 1% by weight to 4% by weight with respect to 100% by weight of the total amount of said non-aqueous electrolyte.
4. 4. The electrochemical element according to claim 1, further comprising a Li-Cl and Li-Sn alloy protective layer on the surface of the lithium metal negative electrode.
5. The nonaqueous electrolyte solution includes a first solvent including a heterocyclic compound having one or more double bonds or not and having one or more oxygen atoms and sulfur atoms; a second solvent including at least one of an ether-based compound, an ester-based compound, an amide-based compound, and a carbonate-based compound; A lithium salt; 4. The electrochemical element according to claim 1 , further comprising lithium nitrate.
6. The lithium salts are LiCl, LiBr, LiI, LiClO 4 , LiBF 4 , LiB 10 C 10 , LiPF 6 , LiCF 3 SO 3 , LiCF 3 CO 2 , LiC 4 B.O. 8 , LiAsF 6 , LiSbF 6 , LiAlCl 4 , C.H. 3 SO 3 Li, C.F. 3 SO 3 Li, (C 2 F 5 SO 2 ) 2 NLi, (SO 2 F) 2 NLi, (CF 3 SO 2 ) 2 NLi, (CF 3 SO 2 ) 3 6. The electrochemical element according to claim 5, comprising CLi, lithium chloroborane, lithium aliphatic carboxylate having 4 or less carbon atoms, lithium 4-phenylborate, lithium imide, or two or more of these.
7. 6. The electrochemical device according to claim 5, wherein the concentration of the lithium salt is from 0.2 to 2.0M.
8. 6. The electrochemical element according to claim 5, wherein the heterocyclic compound is a 3- to 15-membered heterocyclic compound unsubstituted or substituted with one or more selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, a cyclic alkyl group having 3 to 8 carbon atoms, an aryl group having 6 to 10 carbon atoms, a halogen group, a nitro group, an amine group, and a sulfonyl group, or a polycyclic compound of a heterocyclic compound and one or more of a cyclic alkyl group having 3 to 8 carbon atoms and an aryl group having 6 to 10 carbon atoms.
9. The heterocyclic compounds include 1,3-dioxolane, 4,5-diethyl-1,3-dioxolane, 4,5-dimethyl-1,3-dioxolane, 4-methyl-1,3-dioxolane, 4-ethyl-1,3-dioxolane, 1,3-dioxane, 1,4-dioxane, 4-methyl-1,3-dioxane, and 2-methyl-1,3-dioxane, furan, 2-methylfuran, 3-methylfuran, 2-ethylfuran, 2-propylfuran, 2-butylfuran, and 2,3-dimethylfuran. 2,4-dimethylfuran, 2,5-dimethylfuran, pyran, 2-methylpyran, 3-methylpyran, 4-methylpyran, benzofuran, 2-(2-nitrovinyl)furan, thiophene, 2-methylthiophene, 2-ethylthiophene, 2-propylthiophene, 2-butylthiophene, 2,3-dimethylthiophene, 2,4-dimethylthiophene, 2,5-dimethylthiophene, or two or more of these. The electrochemical element according to claim 5.
10. 6. The electrochemical element according to claim 5, wherein the ether-based compound of the second solvent includes dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, dimethoxyethane, diethoxyethane, methoxyethoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, triethylene glycol methyl ethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol methyl ethyl ether, polyethylene glycol dimethyl ether, polyethylene glycol diethyl ether, polyethylene glycol methyl ethyl ether, or two or more of these.
11. 4. The electrochemical element according to claim 1, wherein the non-aqueous electrolyte further contains lanthanum nitrate, potassium nitrate, cesium nitrate, magnesium nitrate, barium nitrate, lithium nitrite, potassium nitrite, cesium nitrite, or two or more of these.
12. The non-aqueous electrolyte contains 1,3-dioxolane as a first solvent, dimethoxyethane as a second solvent, and a lithium salt (CF 3 SO 2 ) 2 4. The electrochemical element according to claim 1, further comprising NLi and lithium nitrate.
13. 4. The electrochemical device according to claim 1, wherein the electrochemical device is a lithium-sulfur battery.
14. 4. An electrochemical element according to claim 1, characterized in that the electrochemical element is a lithium-lithium symmetric cell.
Citation Information
Patent Citations
Nonaqueous electrolyte cell
JP1983161263A
Nonaqueous electrolyte secondary battery
JP2005251516A
Electrolyte for lithium-sulfur battery and lithium-sulfur battery containing the same
JP2019507482A
ELECTROLYTE CONTAINING LiBF4 AND LITHIUM ION SECONDARY BATTERY
JP2021068534A
Electrolyte for aluminum electrode and lithium secondary battery including same
KR1020140060891A