Polyolefin separator for electrochemical device and electrochemical device having the same
A polyolefin separation membrane with controlled PDI and pore size enhances compression resistance and dielectric breakdown voltage, addressing deformation issues in electrochemical devices and improving manufacturing efficiency.
Patent Information
- Application Number
- JP2024521859
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-06-14
- Filing Date
- 2023-02-14
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-02-14
AI Technical Summary
Existing polyolefin-based separation membranes for electrochemical devices face issues with deformation and thickness reduction during high-pressure lamination, leading to reduced battery performance and dielectric breakdown voltage.
A polyolefin separation membrane with controlled polydispersity index (PDI) of 2.5 to 4.2, average pore size of 20 to 40 nm, and maximum pore size of 50 nm or less, along with a deformation rate of 25% or less under specific tensile forces, is developed to enhance compression resistance and maintain dielectric breakdown voltage.
The membrane exhibits improved compression resistance and maintains high dielectric breakdown voltage, allowing for faster process speeds and increased efficiency in electrochemical device manufacturing.
Smart Images

Figure 2024537301000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention claims the benefit of the filing date of Korean Patent Application No. 10-2022-0072072, filed with the Korean Intellectual Property Office on June 14, 2022, the entire contents of which are incorporated herein by reference. The present invention relates to a separator for electrochemical devices based on a polyolefin resin and an electrochemical device including the same. [Background technology]
[0002] A film substrate having a large number of pores and based on a polymer resin such as polyolefin is used as a separator for electrochemical devices such as secondary batteries. In general, an electrode assembly is manufactured through a lamination process in which a separator and an electrode are bonded by heat and pressure. The higher the heat and pressure applied in this process, the stronger the adhesion between the electrode and the separator. Recently, in order to improve productivity, the process speed has been increased, and the time during which heat is applied to the separator has been shortened, so that the adhesive strength is ensured by increasing the pressure, but there is a concern about deformation due to high pressure. In addition, the thickness of the polymer film substrate is significantly reduced during the lamination process, and the damage to the pores is significant, which reduces not only the performance of the battery but also the dielectric breakdown voltage of the separator, resulting in problems such as high-pot failure and low voltage failure. Therefore, it is necessary to develop a porous polymer film substrate for a separator that is less deformed even under high-pressure lamination conditions. Summary of the Invention [Problem to be solved by the invention]
[0003] An object of the present invention is to provide a polyolefin separator for electrochemical devices that has improved compression resistance, low thickness change rate and deformation rate during a lamination process for manufacturing an electrode assembly, and high breakdown voltage.
[0004] Another object of the present invention is to provide an electrochemical device including a separator having the above-mentioned properties.
[0005] It will be readily apparent that the objects and advantages of the present invention may be realized by means of the instrumentalities or methods, and combinations thereof, as recited in the appended claims. [Means for solving the problem]
[0006] A first aspect of the present invention is a separator for an electrochemical device having a large number of pores and comprising a polyolefin resin,
[0007] The polydispersity index (PDI) of the polyolefin resin is 2.5 to 4.2;
[0008] The average size of the pores is 20 nm to 40 nm, and the maximum size of the pores is 50 nm or less;
[0009] The separator for an electrochemical device comprises:
[0010] When a tensile force of 15 MPa is applied at 60°C for 60 seconds, the deformation rate is 25% or less;
[0011] Provided is a polyolefin separator for electrochemical devices, which takes 200 seconds or less to reach a recovery rate of 70% when a tensile force of 2 MPa at 70°C is applied for 180 seconds and then removed.
[0012] A second aspect of the present invention relates to the first aspect,
[0013] The polydispersity index (PDI) of the polyolefin resin is 2.5 to 4.0;
[0014] The average size of the pores is 20 nm to 39 nm, and the maximum size of the pores is 48 nm or less;
[0015] The separator for an electrochemical device comprises:
[0016] The deformation rate is 23% or less when a tensile force of 15 MPa is applied at 60°C for 60 seconds;
[0017] Provided is a polyolefin separator for electrochemical devices, which takes 190 seconds or less to reach a recovery rate of 70% when a tensile force of 2 MPa at 70°C is applied for 180 seconds and then removed.
[0018] A third aspect of the present invention relates to the first or second aspect,
[0019] The polydispersity index (PDI) of the polyolefin resin is 2.6 to 3.9;
[0020] The average size of the pores is 21 nm to 38 nm, and the maximum size of the pores is 46 nm or less;
[0021] The separator for an electrochemical device comprises:
[0022] When a tensile force of 15 MPa is applied at 60°C for 60 seconds, the deformation rate is 21% or less;
[0023] Provided is a polyolefin separator for electrochemical devices, which takes 180 seconds or less to reach a recovery rate of 70% when a tensile deformation force of 2 MPa at 70°C is applied for 180 seconds and then removed.
[0024] A fourth aspect of the present invention relates to the third aspect,
[0025] The average size of the pores is 22.2 nm to 36.1 nm;
[0026] The separator for an electrochemical device comprises:
[0027] The deformation rate is 20.1% or less when a tensile force of 15 MPa is applied for 60 seconds at 60°C;
[0028] Provided is a polyolefin separator for electrochemical devices, which takes 178 seconds or less to reach a recovery rate of 70% when a tensile force of 2 MPa at 70°C is applied for 180 seconds and then removed.
[0029] A fifth aspect of the present invention is any one of the first to fourth aspects,
[0030] The polyolefin resin has a weight average molecular weight of 500,000 to 1,500,000, and the polyolefin separation membrane for electrochemical devices is provided.
[0031] In a sixth aspect of the present invention, in any one of the first to fifth aspects,
[0032] The polyolefin separation membrane for electrochemical devices includes a core portion made of a mixture of polyethylene and polypropylene, and polyethylene skin portions laminated on both sides of the core portion.
[0033] A seventh aspect of the present invention is any one of the first to sixth aspects,
[0034] The polyolefin separator provides a polyolefin separator for an electrochemical device, which is manufactured by a wet manufacturing method in which a pore-forming agent is extracted to form pores.
[0035] An eighth aspect of the present invention provides an electrochemical device including an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator is a polyolefin separator according to any one of the first to seventh aspects.
[0036] A ninth aspect of the present invention relates to the eighth aspect,
[0037] The electrochemical device is a lithium secondary battery. Effect of the Invention
[0038] The polyolefin separation membrane according to the present invention has a polydispersity index of the polyolefin resin, an average pore size and a maximum pore size formed in the separation membrane, which are controlled within a predetermined range, and the deformation rate and recovery rate of the separation membrane are controlled to be below a certain value under a predetermined condition, thereby improving the compression resistance of the separation membrane.
[0039] As a result, the separator has a low thickness reduction rate due to pressure applied during the lamination process for manufacturing the electrode assembly. As a result, the separator of the present invention has high insulation properties without a decrease in dielectric breakdown voltage. In addition, even if high pressure is applied during the lamination process, the separator is less damaged and the process speed can be increased, improving processability.
[0040] The accompanying drawings illustrate preferred embodiments of the invention and, together with the detailed description, are intended to explain the principles of the invention, and are not intended to limit the scope of the invention. Meanwhile, the shape, size, scale, ratio, etc. of elements in the drawings described in this specification may be exaggerated in order to emphasize a clearer description. [Brief description of the drawings]
[0041] [Figure 1] 1 shows an SEM image of a cross section of the separation membrane of Example 1;
[0042] [Diagram 2] 1 shows an SEM image of a cross section of the separation membrane of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0043] The present invention will be described in detail below. Prior to that, the terms or words used in the present specification and claims should not be interpreted limited to their ordinary or dictionary meanings, but should be interpreted with a meaning and concept that matches the technical idea of the present invention based on the principle that the inventor can appropriately define the concept of the term to best describe his / her invention. Therefore, it should be understood that the embodiment described in this specification and the configuration illustrated in the drawings are only the most preferred embodiment of the present invention and do not fully represent the technical idea of the present invention, and therefore there may be various equivalents and modifications that can replace them at the time of this application.
[0044] Throughout the specification of this application, when a part is said to "comprise" certain elements, this means that it can further include other elements, rather than excluding other elements, unless specifically stated to the contrary.
[0045] In this specification, the characteristic of having pores means that an object contains a plurality of pores and the pores are interconnected in a structure that allows gas and / or liquid fluids to pass from one side of the object to the other side.
[0046] The present invention relates to a separator for an electrochemical device, which may be applied to the separator itself or one component of the separator. Therefore, the separator of the present invention may have another layer disposed on at least one surface of the separator substrate, if necessary, in terms of material or function. In one embodiment of the present invention, the separator may have an organic / inorganic composite coating layer including inorganic particles and / or a binder resin formed on at least one or both surfaces of the porous substrate.
[0047] The present invention also relates to an electrochemical device including the separator. In the present invention, the electrochemical device is a device that converts chemical energy into electrical energy by an electrochemical reaction, and is a concept that encompasses primary and secondary batteries. In the present specification, the secondary battery is capable of being charged and discharged, and refers to a lithium secondary battery, a nickel-cadmium battery, a nickel-hydrogen battery, etc. The lithium secondary battery uses lithium ions as an ion conductor, and examples thereof include, but are not limited to, a non-aqueous electrolyte secondary battery including a liquid electrolyte, an all-solid-state battery including a solid electrolyte, a lithium polymer battery including a gel polymer electrolyte, and a lithium metal battery using lithium metal as an anode.
[0048] In the present specification, the separator has a porous property including a large number of pores, and serves as a porous ion-conducting barrier that allows ions to pass while blocking electrical contact between the negative electrode and the positive electrode in the electrochemical device.
[0049] The polyolefin separator for electrochemical devices according to the present invention will be described in detail below.
[0050] The polyolefin separator for electrochemical devices of the present invention is a separator for electrochemical devices having a large number of pores and containing a polyolefin resin,
[0051] The polydispersity index (PDI) of the polyolefin resin is 2.5 to 4.2;
[0052] The average size of the pores is 20 nm to 40 nm, and the maximum size of the pores is 50 nm or less;
[0053] The separator for an electrochemical device comprises:
[0054] When a tensile force of 15 MPa is applied at 60°C for 60 seconds, the deformation rate is 25% or less;
[0055] When a tensile force of 2 MPa is applied for 180 seconds at 70° C. and then removed, the time required for the recovery rate to reach 70% is 200 seconds or less.
[0056] In the present invention, the polyolefin separation membrane is manufactured using a polyolefin resin as a base resin. Examples of polyolefin resins include polyethylene, polypropylene, polypentene, etc., and may contain one or more of these. A separation membrane having porosity, i.e., a large number of pores, manufactured using such a polyolefin resin as a base resin is advantageous in terms of imparting a shutdown function at an appropriate temperature. In particular, when polyethylene and polypropylene are simultaneously contained as polyolefin resins, the shutdown property and physical properties such as mechanical strength can be simultaneously improved.
[0057] Generally, the higher the molecular weight of the resin, the more advantageous it is for compression resistance, and therefore the weight average molecular weight of the polyolefin resin may be higher than conventionally, 500,000 to 1,500,000. When different types of polyolefin resins are mixed and used, or when a separator is formed with a multi-layer structure made of different types of polyolefin resins, the weight average molecular weight of the polyolefin resin is calculated by adding the weight average molecular weights according to the content ratio of each polyolefin resin.
[0058] In addition to the polyolefin-based resin, other resin components may be mixed as necessary, and in addition to the resin components, for example, filler particles may be included. The filler particles may be introduced for the purpose of a pressure barrier to prevent the thickness, pore size, and porosity of the separation membrane substrate from being excessively reduced due to the high pressure applied in the lamination process described below. The filler particles may include organic fillers or inorganic fillers having a predetermined particle size, and are not limited to a specific component as long as they have a strength equal to or greater than that of the polyolefin resin.
[0059] In the present invention, the polyolefin resin has a polydispersity index (PDI) of 2.5 to 4.2, an average pore size of 20 nm to 40 nm, and a maximum pore size of 50 nm or less. That is, in the present invention, the polyolefin resin has a low polydispersity index, and the average pore size and the maximum pore size are small. When these ranges are satisfied at the same time, the compression resistance is improved. If the polydispersity index is less than 2.5, there is a problem that the processability is reduced and the uniformity of the film is reduced, and if it exceeds 4.2, there is a problem that the compression resistance is reduced. In addition, if the average pore size is less than 20 nm, there is a problem that the air permeability is reduced and a phenomenon occurs in which by-products block small pores during charging and discharging of the battery, and if it exceeds 40 nm, there is a problem that the thickness of the separator is not uniform, thickness deformation occurs, and compression resistance is reduced due to local thickness deformation. In addition, if the maximum pore size exceeds 50 nm, there is also a problem that compression resistance is reduced.
[0060] The pore size can be calculated from the pore size distribution measured using a capillary flow porometer. For example, the separator to be measured is first wetted with a wetting agent such as Galwick solution, and then the air pressure on one side of the substrate is gradually increased. When the applied air pressure exceeds the capillary attraction of the wetting agent present in the pores, the wetting agent blocking the pores is expelled, and the pore size and distribution are measured based on the pressure and flow rate at the moment of expulsion, from which the average pore size and maximum size can be determined.
[0061] In this aspect, the polydispersity index (PDI) of the polyolefin resin may be 2.5 to 4.0, more specifically 2.6 to 3.9. The average pore size may be 20 nm to 39 nm, more specifically 21 nm to 38 nm, and most specifically 22.2 nm to 36.1 nm. The maximum pore size may be 48 nm or less, more specifically 46 nm or less.
[0062] Meanwhile, in the present invention, the separator for electrochemical devices has a deformation rate of 25% or less when a tensile force of 15 MPa at 60° C. is applied for 60 seconds, and at the same time, when a tensile force of 2 MPa at 70° C. is applied for 180 seconds and then removed, the time it takes for the recovery rate to reach 70% is 200 seconds or less.
[0063] If the deformation rate exceeds 25% under the above conditions, or the time required for the recovery rate to reach 70% exceeds 200 seconds, the compression resistance decreases after the lamination process with the electrodes.
[0064] In this aspect, the separator for an electrochemical device is
[0065] When a tensile deformation force of 15 MPa at 60° C. is applied for 60 seconds, the deformation rate may be 23% or less, and when a tensile deformation force of 2 MPa at 70° C. is applied for 180 seconds and then removed, the time required for the recovery rate to reach 70% may be 190 seconds or less;
[0066] More specifically, when a tensile deformation force of 15 MPa is applied at 60° C. for 60 seconds, the deformation rate may be 21% or less, and when a tensile deformation force of 2 MPa is applied at 70° C. for 180 seconds and then removed, the time required for the recovery rate to reach 70% may be 180 seconds or less.
[0067] Most specifically, when a tensile deformation force of 15 MPa at 60°C is applied for 60 seconds, the deformation rate may be 20.1% or less, and when a tensile deformation force of 2 MPa at 70°C is applied for 180 seconds and then removed, the time it takes for the recovery rate to reach 70% may be 178 seconds or less.
[0068] The polyolefin separation membrane may be prepared as follows, but is not limited thereto.
[0069] In one embodiment of the present invention, the separation membrane may be manufactured by a method (wet method) in which a polyolefin resin is mixed with a plasticizer (diluents) at a high temperature to form a single phase, the polymer material and the plasticizer are phase-separated during cooling, the plasticizer is extracted to form pores, and then the membrane is stretched and heat-set. In particular, the polyolefin separation membrane may include a core portion made of a mixture of polyethylene and polypropylene, and a polyethylene skin portion laminated on both sides of the core portion, but is not limited thereto.
[0070] The average pore size and maximum pore size of the separator can be easily prepared by those skilled in the art by adjusting the mixing ratio of the plasticizer, the stretching ratio, the heat setting temperature, etc., so as to conform to the scope of the present invention.
[0071] In the present invention, the polyolefin separation membrane substrate prepared by the above-mentioned method may have a thickness of 5 μm to 30 μm.
[0072] Meanwhile, in one embodiment of the present invention, the separator may further include an organic / inorganic composite coating layer formed on at least one surface of the polyolefin separator substrate.
[0073] The organic / inorganic composite coating layer includes a binder resin and inorganic particles and has a porous property. In one embodiment of the present invention, the organic / inorganic composite coating layer may include the binder resin and the inorganic particles in a weight ratio of 1:99 to 30:70. The ratio may be appropriately adjusted within the range, and for example, the binder resin may be 1 wt% or more, 5 wt% or more, or 10 wt% or more, and the inorganic particles may be 80 wt% or more, 85 wt% or more, 90 wt% or more, or 95 wt% or more, out of a total of 100 wt% of the binder resin and the inorganic particles.
[0074] The organic / inorganic composite coating layer may be formed by binding inorganic particles with a binder resin and accumulating them inside, and the pores in the organic / inorganic composite coating layer may be caused by interstitial volumes, which are void spaces between the inorganic particles.
[0075] In one embodiment of the present invention, the porosity of the organic / inorganic composite coating layer may be 30vol% to 70vol%. If the porosity is 70vol% or less, it is possible to ensure mechanical properties that can withstand the pressing process for bonding with the electrode, and since the surface opening ratio is not too high, it is suitable for ensuring adhesive strength. On the other hand, if the porosity is 30vol% or more, it is advantageous from the viewpoint of ion permeability.
[0076] The organic / inorganic composite coating layer may have a thickness of 1 μm to 20 μm on either side of the separator substrate, but is not limited thereto. The thickness can be adjusted to an appropriate range by those skilled in the art in terms of heat resistance or electrical resistance.
[0077] Non-limiting examples of binder resins that can be used in the organic / inorganic composite coating layer of the present invention include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene-vinyl acetate copolymer, polyethylene oxide, and the like. The polymer resin may be any one selected from the group consisting of polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, and carboxyl methyl cellulose, or a mixture of two or more of these polymer resins, but is not limited thereto.
[0078] In a specific embodiment of the present invention, the inorganic particles usable in the organic / inorganic composite coating layer are not particularly limited as long as they are electrochemically stable. That is, the inorganic particles usable in the present invention are within the operating voltage range (e.g., Li / Li + There are no particular limitations as long as the oxidation and / or reduction reaction does not occur at a voltage of 0 V to 5 V relative to the reference voltage.
[0079] Non-limiting examples of the inorganic particles include BaTiO3, Pb(Zr,Ti)O3 (PZT), 1-x La x Zr 1-y Ti y O3(PLZT, 0 <x<1、0<y<1)、Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, SiC, Al(OH)3, TiO2, aluminum peroxide, zinc tin hydroxide (ZnSn(OH)6), tin-zinc oxide (Zn2SnO4, ZnSnO3), antimony trioxide (Sb2O3), antimony tetroxide (Sb2O4), antimony pentoxide (Sb2O5), etc., and one or more of these may be included.
[0080] In addition, the average diameter of inorganic particles (D 50 ) is not particularly limited, but is preferably in the range of 0.3 μm to 1 μm in order to form a coating layer of uniform thickness and to have a suitable porosity. If it is less than 0.3 μm, the dispersibility of inorganic particles in the slurry prepared for producing the coating layer may decrease, and if it exceeds 1 μm, the thickness of the coating layer formed may increase.
[0081] In one embodiment of the present invention, the organic / inorganic composite coating layer may be formed, for example, as follows. First, a binder resin is dissolved in a suitable organic solvent to prepare a polymer solution. The solvent preferably has a solubility index similar to that of the binder polymer to be used and a low boiling point. This is to facilitate uniform mixing and subsequent solvent removal. Non-limiting examples of usable solvents include acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or a mixture thereof.
[0082] Next, inorganic particles are added and dispersed in the prepared polymer solution. In the present invention, the content ratio of the inorganic particles to the binder is as described above, and is appropriately adjusted in consideration of the thickness, pore size, and porosity of the coating layer of the present invention to be finally prepared.
[0083] Next, the inorganic particle slurry prepared as above is applied to at least one surface of the prepared separation membrane substrate and dried. The method of applying the slurry to the surface of the separation membrane substrate is not limited to any particular method, and any common method known in the art can be used. For example, various methods such as dip coating, die coating, roll coating, comma coating, or a combination thereof can be used.
[0084] The drying process is performed by appropriately setting temperature and time conditions to minimize the occurrence of surface defects in the organic / inorganic composite coating layer, and drying auxiliary devices such as a drying oven or hot air may be used within an appropriate range.
[0085] When the separator includes an organic / inorganic composite porous layer, damage caused by pressure of inorganic particles on the surface of the separator substrate facing the organic / inorganic composite porous layer during the lamination process may be reduced.
[0086] The separator prepared by the above method is interposed between the negative electrode and the positive electrode, and is manufactured into an electrode assembly by a lamination process in which heat and / or pressure are applied to bond them. In one embodiment of the present invention, the lamination process may be performed by a roll press device including a pair of pressure rollers. That is, the negative electrode, the separator, and the positive electrode may be sequentially stacked and then inserted between the pressure rollers to achieve interlayer bonding. At this time, the lamination process may be performed by a hot pressing method.
[0087] The present invention also provides an electrochemical device, particularly a lithium secondary battery, including the separator. The battery includes an anode, a cathode, and a separator interposed between the anode and the cathode, and the separator includes a separator substrate having the above-described characteristics.
[0088] The positive electrode comprises a positive electrode current collector and a positive electrode active material layer on at least one surface of the current collector, the positive electrode active material layer including a positive electrode active material, a conductive material, and a binder resin. The positive electrode active material may be a layered compound such as lithium manganese oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; 1+x Mn 2-x Lithium manganese oxides such as LiMnO4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, and Cu2V2O7; and the chemical formula LiNi 1-x M x Lithium nickel oxide with Ni site represented by the chemical formula LiMnO2 (where M=Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x=0.01 to 0.3); 1-x M xLithium manganese composite oxides represented by O2 (where M = Co, Ni, Fe, Cr, Zn or Ta and x = 0.01 to 0.1) or Li2Mn3MO8 (where M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which part of Li in the chemical formula is substituted with alkaline earth metal ions; disulfide compounds; It can contain one or a mixture of two or more of Fe2(MoO4)3.
[0089] In the present invention, the negative electrode includes a negative electrode current collector and a negative electrode active material layer containing a negative electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. As the negative electrode active material, the negative electrode includes carbon such as lithium metal oxide, graphitized carbon, and graphite-based carbon; Li x Fe2O3(0 ≦ x ≦ 1), Li x WO2(0 ≦ x ≦ 1), Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Group 1, Group 2, Group 3 elements of the periodic table, halogen; 0 < x ≦ 1; 1 ≦ y ≦ 3; 1 ≦ z ≦ 8) and other metal composite oxides; lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, and Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials; It can contain one or a mixture of two or more selected from titanium oxides.
[0090] In a specific embodiment of the present invention, the conductive material may be, for example, any one selected from the group consisting of graphite, carbon black, carbon or metal fiber, metal powder, conductive whisker, conductive metal oxide, activated carbon, and polyphenylene derivatives, or a mixture of two or more of these conductive materials. More specifically, the conductive material may be any one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more of these conductive materials.
[0091] The current collector is not particularly limited as long as it has high conductivity without inducing a chemical change in the battery. For example, stainless steel, copper, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, or the like may be used.
[0092] The binder resin may be a polymer commonly used in electrodes in the art. Non-limiting examples of such binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene-vinyl acetate copolymer, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. Examples of the dispersant include, but are not limited to, cyanoethyl acetatepropionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, and carboxyl methyl cellulose. In the present invention, the positive electrode slurry for preparing the positive electrode active material layer may include a dispersant, and the dispersant may be a pyrrolidone-based compound. Specifically, the dispersant may be N-methylpyrrolidone (ADC-01, LG Chemicals).
[0093] In the present invention, the content of the dispersant contained in the positive electrode slurry may be more than 0 parts by weight and not more than 0.5 parts by weight, based on 100 parts by weight of the positive electrode slurry. Specifically, the content of the dispersant contained in the positive electrode slurry may be more than 0.05 parts by weight and not more than 0.4 parts by weight, based on 100 parts by weight of the positive electrode slurry.
[0094] In the present invention, the negative electrode slurry for preparing the negative electrode active material layer may include a dispersant, and the dispersant may be a polypyrrolidone-based compound. Specifically, the dispersant may be polyvinylpyrrolidone (manufactured by Junsei Corporation).
[0095] In the present invention, the content of the dispersant contained in the negative electrode slurry may be more than 0 parts by weight and not more than 0.5 parts by weight, based on 100 parts by weight of the negative electrode slurry. Specifically, the content of the dispersant contained in the negative electrode slurry may be more than 0.05 parts by weight and not more than 0.4 parts by weight, based on 100 parts by weight of the negative electrode slurry.
[0096] The electrode assembly prepared as above can be placed in a suitable case and an electrolyte can be injected to manufacture a battery.
[0097] In the present invention, the electrolyte is + B - A salt having the structure: + Li + , Na + , K + or a combination thereof, - PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2)2 - , C(CF2SO2)3- or a combination thereof, dissolved or dissociated in an organic solvent such as, but not limited to, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma butyrolactone (γ-butyrolactone), or a mixture thereof.
[0098] The present invention also provides a battery module including a battery having the electrode assembly as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source. Specific examples of the device include, but are not limited to, a power tool powered by a battery-type motor, electric vehicles including electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), and the like, electric two-wheeled vehicles including electric bicycles (E-bikes) and electric scooters (E-scooters), electric golf carts, and power storage systems.
[0099] Hereinafter, the present invention will be described in detail with reference to examples in order to specifically explain the present invention. However, the examples according to the present invention may be modified in various different forms, and the scope of the present invention should not be construed as being limited to the examples detailed below. The examples of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.
[0100] [Example 1]
[0101] A resin made by mixing polyethylene (weight average molecular weight 900,000) and polypropylene (weight average molecular weight 350,000) in a weight ratio of 93:7 was used as the core, and polyethylene (weight average molecular weight 900,000) resin was placed on both sides of the core and co-extruded into the skins, and a polyolefin separation membrane substrate (total thickness about 9 μm, core thickness: 7 μm, total thickness of both skins 2 μm) was produced by a wet method at a stretching temperature of 105° C. and a heat setting temperature of 130° C. The PDI of the resin used to produce the separation membrane was calculated according to the following formula 1.
[0102] The PDI, average pore size, maximum pore size, deformation rate when a tensile force of 15 MPa at 60°C is applied for 60 seconds (referred to as recovery deformation rate), and the time required for the recovery rate to reach 70% when a tensile force of 2 MPa at 70°C is applied for 180 seconds and then removed (referred to as recovery time) of the prepared polyolefin separator are shown in Table 1 below.
[0103] [Example 2]
[0104] A separator was prepared in the same manner as in Example 1, except that the stretching temperature was 120°C and the heat setting temperature was 115°C.
[0105] [Example 3]
[0106] A separator was prepared in the same manner as in Example 1, except that the heat setting temperature was adjusted to 115°C.
[0107] [Comparative Example 1]
[0108] A separation membrane was manufactured in the same manner as in Example 1, except that a resin made by mixing polyethylene (weight average molecular weight 900,000) and polypropylene (weight average molecular weight 350,000) in a weight ratio of 97:3 was used as the skin portion, and the stretching temperature was adjusted to 120°C.
[0109] [Comparative Example 2]
[0110] A separation membrane was manufactured in the same manner as in Example 1, except that a resin made by mixing polyethylene (weight average molecular weight 900,000) and polypropylene (weight average molecular weight 350,000) in a weight ratio of 97:3 was used as the skin portion, and the heat setting temperature was adjusted to 115°C.
[0111] [Comparative Example 3]
[0112] A separation membrane was manufactured in the same manner as in Example 1, except that a resin in which polyethylene (weight average molecular weight 900,000) and polypropylene (weight average molecular weight 350,000) were mixed in a weight ratio of 97:3 was used as the skin portion.
[0113] [Comparative Example 4]
[0114] A separation membrane was manufactured in the same manner as in Example 1, except that a resin made by mixing polyethylene (weight average molecular weight 900,000) and polypropylene (weight average molecular weight 350,000) in a weight ratio of 97:3 was used as the skin portion, and the stretching temperature was set to 120°C and the heat setting temperature was set to 115°C.
[0115] [PDI measurement]
[0116] (Formula 1) PDI = (weight average molecular weight) / (number average molecular weight)
[0117] At this time, the weight average molecular weight and number average molecular weight were determined by cutting the separation membrane to a predetermined size and analyzing it through gel permeation chromatography (GPC).
[0118] [Measurement of average and maximum pore size]
[0119] The pore size distribution was measured using a capillary flow porometer (CFP method).
[0120] [Measurement of deformation rate when a tensile force of 15 MPa is applied for 60 seconds at 60°C]
[0121] Through Dynamic Mechanical Analysis creep evaluation (DMA850, TA Instruments), a stress of 15 MPa was applied at 60°C for 60 seconds to measure the deformation rate.
[0122] [Measurement of the time it takes for the recovery rate to reach 70% after applying a tensile force of 2 MPa at 70°C for 180 seconds and then removing the force]
[0123] Using Dynamic Mechanical Analysis (DMA850, TA Instruments), the time it took for the recovery rate to reach 70% after applying a stress of 2 MPa at 70°C for 180 seconds was measured.
[0124] [Table 1]
[0125] [Manufacturing of electrode assemblies]
[0126] 1) Manufacturing of positive electrodes
[0127] Cathode active material (LiNi 0.8 Mn 0.1 Co 0.1 O2), conductive material (carbon black), dispersant (N-methylpyrrolidone, ADC-01, LG Chemicals), and binder resin (mixture of PVDF-HFP and PVDF) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for a positive electrode active material layer with a concentration of 50 wt% for the remaining components excluding water. Next, the slurry was applied to the surface of an aluminum thin film (thickness 10 μm) and dried to prepare a positive electrode having a positive electrode active material layer (thickness 120 μm).
[0128] 2) Manufacturing of negative electrodes
[0129] Graphite (a blend of natural graphite and artificial graphite), conductive material (carbon black), dispersant (Polyvinylpyrrolidone, Junsei), and binder resin (a mixture of PVDF-HFP and PVDF) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for the negative electrode active material layer, with the remaining components excluding water being 50 wt% in concentration. The slurry was then applied to the surface of a copper thin film (thickness 10 μm) and dried to prepare a negative electrode having a negative electrode active material layer (thickness 120 μm).
[0130] 3) Lamination process
[0131] The prepared negative and positive electrodes were laminated with the separators of the Examples and Comparative Examples interposed therebetween to obtain an electrode assembly by performing a lamination process at 70° C. and 5.2 MPa for 10 seconds using a hot press.
[0132] [Pores size reduction rate]
[0133] The reduction rate of the pore size was calculated based on the following formula 2.
[0134] (Formula 2) Pore size reduction rate (%) = (CD / C)*100
[0135] In the above formula 2, C represents the average pore size of the separation membrane substrate before lamination, and D represents the average pore size of the separation membrane substrate obtained after lamination.
[0136] [Resistance measurement]
[0137] Resistance was measured by placing each separator substrate between SUS and injecting an electrolyte solution to prepare a coin cell, and measuring the resistance (ER) by EIS. The frequency was set to 100,000 to 10,000 Hz. The electrolyte solution was a mixture of ethylene carbonate and ethyl methyl carbonate in a non-aqueous solvent at a ratio of 3:7, and LiPF6 at a concentration of 1M.
[0138] [Breakdown voltage]
[0139] The SUS mesh and separator substrate were hot-pressed at 90°C, 4 MPa, and 1 s, and the voltage was increased at a rate of 100 V / s to determine the voltage at which the fail condition (>0.5 mA, 3 s) was reached. After measuring the breakdown voltage of 30 samples for each example and comparative example, the bottom 1% voltage was derived through a Weibull distribution analysis.
[0140] [Capacity maintenance rate]
[0141] The produced battery was repeatedly charged and discharged in the range of 2.5 V to 4.25 V at a rate of 1 C, and the ratio of the discharge capacity after each cycle to the initial discharge capacity was calculated. The capacity retention rate was evaluated at room temperature.
[0142] The results of the above measurements are shown in Table 2 below.
[0143] [Table 2]
Claims
1. A separator for an electrochemical device having a large number of pores and comprising a polyolefin resin, The polydispersity index (PDI) of the polyolefin resin is 2.5 to 4.2; The average size of the pores is 20 nm to 40 nm, and the maximum size of the pores is 50 nm or less; Polyolefin separation membrane for electrochemical elements.
2. The separator for an electrochemical device comprises: The deformation rate is 25% or less when a tensile deformation force of 15 MPa is applied at 60° C. for 60 seconds; When a tensile deformation force of 2 MPa is applied for 180 seconds at 70° C. and then removed, the time required for the recovery rate to reach 70% is 200 seconds or less. The polyolefin separator for an electrochemical device according to claim 1 .
3. The polydispersity index (PDI) of the polyolefin resin is 2.5 to 4.0; the average pore size is between 20 nm and 39 nm, and the maximum pore size is less than or equal to 48 nm; The separator for an electrochemical device comprises: The deformation rate is 23% or less when a tensile deformation force of 15 MPa is applied at 60° C. for 60 seconds; When a tensile force of 2 MPa is applied at 70° C. for 180 seconds and then removed, the time required for the recovery rate to reach 70% is 190 seconds or less. The polyolefin separator for an electrochemical device according to claim 2 .
4. The polydispersity index (PDI) of the polyolefin resin is 2.6 to 3.9; the average pore size is between 21 nm and 38 nm, and the maximum pore size is less than or equal to 46 nm; The separator for an electrochemical device comprises: The deformation rate is 21% or less when a tensile deformation force of 15 MPa is applied at 60° C. for 60 seconds; When a tensile force of 2 MPa is applied to the material at 70° C. for 180 seconds and then removed, the time required for the recovery rate to reach 70% is 180 seconds or less. The polyolefin separator for an electrochemical device according to claim 2 .
5. The average size of the pores is between 22.2 nm and 36.1 nm; The separator for an electrochemical device comprises: The deformation rate is 20.1% or less when a tensile deformation force of 15 MPa is applied at 60° C. for 60 seconds; When a tensile force of 2 MPa is applied at 70° C. for 180 seconds and then removed, the time required for the recovery rate to reach 70% is 178 seconds or less. The polyolefin separator for an electrochemical device according to claim 4 .
6. The polyolefin separator for electrochemical devices according to claim 1, wherein the polyolefin resin has a weight average molecular weight of 500,000 to 1,500,000.
7. 2. The polyolefin separation membrane for electrochemical devices according to claim 1, comprising a core portion made of a mixture of polyethylene and polypropylene, and polyethylene skin portions laminated on both sides of the core portion.
8. 2. The polyolefin separator for an electrochemical device according to claim 1, wherein the polyolefin separator is manufactured by a wet manufacturing method in which pores are formed by extracting a pore-forming agent.
9. An electrochemical device comprising an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, 9. An electrochemical element, wherein the separation membrane is the separation membrane according to claim 1.
10. The electrochemical device according to claim 9, wherein the electrochemical device is a lithium secondary battery.
Citation Information
Patent Citations
Multi-layer microporous membrane and forming method thereof, and battery separator and battery
JP2013035293A
Laminated porous film, separator for battery and battery
JP2014124780A
Microporous film and separator using the same
JP2015120786A
Polyolefin multilayer microporous membrane and battery separator
WO2015182689A1