Stable ion-exchange membranes with radical scavengers.

By integrating cerium oxide nanoparticles into ion exchange membranes with fluorinated ionomers, the membranes' resistance to radical-induced degradation is enhanced, ensuring prolonged operational life and durability in heavy-duty applications.

JP2024537326APending Publication Date: 2024-10-10THE CHEMOURS CO FC LLC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024522082
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-06-14
Filing Date
2022-10-11
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing ion exchange membranes in fuel cells and water electrolyzers are prone to degradation due to hydrogen peroxide and peroxide radicals, leading to premature failure, especially in heavy-duty applications like trucks, despite the use of cerium compounds which do not provide sufficient stability and durability.

Method used

Incorporating cerium oxide nanoparticles into the ion exchange membrane composition, along with fluorinated ionomers and optional additives, enhances the membrane's resistance to chemical attack, resulting in longer operational lifetimes.

Benefits of technology

The modified ion exchange membranes demonstrate significantly improved durability, withstanding at least 400 hours without voltage drop in unreinforced membranes and up to 1500 hours with reinforcement, surpassing the performance of previous solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537326000001_ABST
    Figure 2024537326000001_ABST
Patent Text Reader

Abstract

Fluorinated ionomer and Ce x M 1-x O y A long-lasting, highly durable ion exchange membrane is described, comprising nanoparticles and optional additives, where x is 0.2-0.9, y is 1-3, and M is Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni. The optional additives may include a reinforcing layer that may be embedded in the ion exchange membrane. Such membranes are formed from ion exchange polymer dispersions and are useful for forming membrane assemblies for fuel cell or water electrolysis applications. The membranes and membrane assemblies have improved chemical stability and durability in such applications.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The ion exchange dispersions and ion exchange membranes are doped with Ce to improve the chemical stability and durability of the membranes in fuel cell or water electrolysis applications. x M 1-x O y The compound is directly incorporated into the composition. [Background technology]

[0002] Polymer electrolyte membranes in fuel cells, water electrolyzers, or other applications are exposed to chemical stressors that cause membrane thinning and premature failure. Reactions and ion transport in fuel cells or water electrolyzers occur in ion exchange membranes, for example ion exchange membranes made from perfluorinated sulfonic acid ionomers, across a membrane electrode assembly including an anode and a cathode. In fuel cells, hydrogen ions generated by the electrochemical reaction of hydrogen introduced at the anode migrate through the membrane to the cathode as a reducing electrode, and electrons migrate through an external circuit to the cathode to generate electricity. At the cathode, oxygen molecules, hydrogen ions, and electrons react with each other to generate heat and water. In water electrolyzers, protons driven by the oxygen evolution electrochemical reaction of water introduced at the anode migrate through the membrane to the cathode as a reducing electrode, and electrons migrate through an external circuit to the cathode. At the cathode, the combination of protons and electrons generates hydrogen gas. However, hydrogen peroxide and peroxide radicals may also be formed during the ion exchange process in either application, which can attack and decompose the membrane polymer.

[0003] One solution that has been used previously is to add cerium compounds, such as cerium oxide, cerium(III) hexahydrate, to the membrane to scavenge the radical species that would initiate decomposition. Other relevant references, such as U.S. Patent No. 11,038,189, recommend the addition of Ce as an antioxidant during membrane assembly. x Zr 1-xO4 nanofibers. Still other references suggest adding antioxidant compounds to the anode or cathode layers that would help prevent the migration of harmful radicals through the ion exchange membrane. However, these compounds, while improving chemical stability, have not demonstrated the necessary stability and durability suitable for heavy duty applications such as heavy duty trucks that may operate for at least 5,000 hours of service. Summary of the Invention [Means for solving the problem]

[0004] The compositions and products of the present invention provide much greater resistance to chemical attack, thereby enabling longer expected life for applications such as heavy duty trucks. x M 1-x O y Certain Ce nanoparticles x M 1-x O y The use of compounds makes this possible.

[0005] In one embodiment, the present invention is an ion exchange membrane comprising about 70-99.99 wt. % of a fluorinated ionomer and about 0.01-1.0 wt. % of Ce, all based on the total dry weight of the membrane. x M 1-x O y ion exchange membrane comprising nanoparticles and about 0-29.99 wt. % of an optional additive, wherein x is 0.6-0.9, y is 1-3, and M is selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni.

[0006] The present invention provides an ion exchange dispersion comprising a liquid carrier, about 70-99.99 wt. % of a fluorinated ionomer, and about 0.01-1.0 wt. % of Ce, all based on the total solids weight of the dispersion. x M 1-x O yThe present invention further relates to an ion exchange dispersion comprising nanoparticles and about 0-29.99 wt. % of an optional additive, wherein x is 0.6-0.9, y is 1-3, and M is selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni.

[0007] In another embodiment, the present invention is an ion exchange membrane comprising about 70-97.99 wt. % of a fluorinated ionomer and about 0.01-1.0 wt. % of Ce, all based on the total dry weight of the membrane. x M 1-x O y The present invention relates to an ion exchange membrane comprising nanoparticles and about 2-29.99 wt. % of an additive comprising a reinforcing layer, wherein x is 0.2-0.9, y is 1-3, and M is selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni, and the reinforcing layer is embedded in the ion exchange membrane.

[0008] In yet another embodiment, the present invention is an ion exchange membrane comprising about 70-99.99 wt. % of a fluorinated ionomer and about 0.01-1.0 wt. % of Ce, all based on the total dry weight of the membrane. x M 1-x O y and about 0-29.99 wt % of an optional additive, wherein x is 0.6-0.9, y is 1-3, and M is selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni, with the proviso that if the membrane is unreinforced, the membrane lasts for at least 400 hours before dropping below 0.8 V following an accelerated open circuit voltage stress test, or with the proviso that if the membrane is reinforced, the membrane lasts for at least 1500 hours before dropping below 0.8 V following an accelerated open circuit voltage stress test. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a cross-sectional view of a membrane assembly representing one embodiment. [Diagram 2]1 is a graph showing the Open Circuit Voltage (OCV) Accelerated Stress Test (AST) performance of Comparative Example A. [Diagram 3] 13 is a graph showing the OCV AST performance of Comparative Example B. [Figure 4] 13 is a graph showing the OCV AST performance of Comparative Example C. [Diagram 5] 1 is a graph showing the OCV AST performance of Example 1. [Figure 6] 1 is a graph showing the OCV AST performance of Example 2. [Figure 7] 1 is a graph showing the OCV AST performance of Example 3. [Figure 8] 1 is a graph showing the OCV AST performance of Example 4. [Figure 9] 13 is a graph showing the composite AST performance of Comparative Example B. [Figure 10] 1 is a graph showing the composite AST performance of Example 1. [Figure 11] 1 is a graph showing the composite AST performance of Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The features of the embodiments of the invention described in the Detailed Description may be combined in any manner.

[0011] In one embodiment, the present invention is an ion exchange membrane comprising about 70-99.99 wt. % of a fluorinated ionomer and about 0.01-1.0 wt. % of Ce, all based on the total dry weight of the membrane. x M 1-x O y% of an optional additive, and about 0-29.99 wt. % of an optional additive, where x is 0.6-0.9, y is 1-3, and M is selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni. In another embodiment, the present invention relates to an ion exchange membrane comprising about 70-97.99 wt. % of a fluorinated ionomer and about 0.01-1.0 wt. % of Ce, all based on the total dry weight of the membrane. x M 1-x O y % of an additive comprising nanoparticles and a reinforcing layer, wherein x is 0.2-0.9, y is 1-3, and M is selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni, and the reinforcing layer is embedded in the ion exchange membrane. In another embodiment, the invention relates to an ion exchange membrane comprising about 70-99.99 wt. % of a fluorinated ionomer and about 0.01-1.0 wt. % of Ce, all based on the total dry weight of the membrane. x M 1-x O y and about 0-29.99 wt % of an optional additive, wherein x is 0.6-0.9, y is 1-3, and M is selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni, with the proviso that if the membrane is unreinforced, the membrane lasts for at least 400 hours before dropping below 0.8 V following an accelerated open circuit voltage stress test, or with the proviso that if the membrane is reinforced, the membrane lasts for at least 1500 hours before dropping below 0.8 V following an accelerated open circuit voltage stress test.

[0012] Ce used in the ion exchange membrane or ion exchange dispersion of the present invention x M 1-x O y The compound may be any compound that provides durability and stability performance to ion exchange polymers and ion exchange membranes. The molar ratio of Ce to M is important to provide such durability and stability. In one embodiment, the compound has the formula Ce x M 1-x O yIn one embodiment, the molar amount of Ce is greater than the molar amount of M such that x is greater than (1-x). In one embodiment, x is between 0.2 and 0.9, and the compound Ce 0.2-0.9 M 0.8-0.1 O y or x is between 0.6 and 0.9, and the compound Ce 0.6-0.9 M 0.4-0.1 O y or x is between 0.7 and 0.9, and the compound Ce 0.7-0.9 M 0.3-0.1 O y or x is between 0.75 and 0.85, and the compound Ce 0.75-0.85 M 0.25-0.15 O y For oxygen, y is typically 1 to 3, alternatively 2 to 3, alternatively 2.

[0013] Compound Ce x M 1-x O y where M is the surface oxygen vacancy and / or surface Ce in the lattice structure of CeO2. 3+ M may be any element that promotes ions. For example, M may be an element selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni. The compound may have more than one M element present, provided that the ratio of Ce to total M remains the same. Blends of compounds using different M elements may also be included. In one embodiment, M is Zr.

[0014] Ce x M 1-x O yThe compounds may be in any form, including but not limited to, particulate or nanoparticle form. The compounds may typically have an average particle size of about 1-25 nm, alternatively about 1-20 nm, alternatively about 1-15 nm, alternatively about 5-10 nm, or any range of particle sizes within the aforementioned ranges, as measured by transmission electron microscopy (TEM). The aspect ratio of the compounds as measured by TEM may typically be 1:1 or greater, alternatively 1:1 to 1:10, alternatively 1:1 to 1:3, or any range of aspect ratios within the aforementioned ranges.

[0015] The fluorinated ionomer used in the ion exchange membrane or ion exchange dispersion of the present invention may be any ionomer suitable for ion exchange membranes and may include one or more different fluorinated ionomers. In one aspect, the fluorinated ionomer is a fluorinated polymer that includes a sulfonate group. The term "sulfonate group" is intended to refer to either a sulfonic acid group or a salt of a sulfonic acid, including but not limited to alkali metal or ammonium salts. A preferred functional group is represented by the formula -SO3X, where X is H, Li, Na, K, or N(R 1 )(R 2 )(R 3 )(R 4 )(wherein, R 1 , R 2 , R 3 , and R 4 are the same or different and are H, CH, or CH. Fluorinated ionomers containing sulfonate groups are available from The Chemours Company (Wilmington, Del.) under the trade name Nafion™.

[0016] For example, the fluorinated ionomer may include the following repeat unit: -[CF2-CF((CF2) b -(O-(CF2CFR f ) c ) a -O-(CF2CFR' f )d SO3X)] _ In the formula, b is 0 or 1, c is an integer from 2 to 8, a is 0, 1, or 2, d is an integer from 1 to 8, and R f and R' f is independently selected from F, Cl, or a perfluorinated alkyl group having 1 to 10 carbon atoms, a is 0, 1, or 2, and X is H, Li, Na, K, or N(R 1 )(R 2 )(R 3 )(R 4 )(wherein, R 1 , R 2 , R 3 , and R 4 are the same or different and are H, CH3, or C2H5). For clarity, the subdivision ((CF2) b -(O-(CF2CFR f ) c ) a -O-(CF2CFR' f ) d SO3X) are pendant chains derived from a perfluorinated polymer backbone. Branched pendant chains with multiple sulfonic acid groups are also included.

[0017] In one embodiment, the fluorinated ionomer is a copolymer made of two or more monomers. For example, it is a copolymer of a sulfonic acid-containing monomer with tetrafluoroethylene (TFE) (resulting in the repeat unit -[CF2-CF2]-) or with other comonomers. For example, a monomer with pendant phosphonic acid groups can be incorporated into the fluorinated ionomer to obtain a fluorinated ionomer containing both sulfonic acid and phosphonic acid groups. The fluorinated ionomers, and the resulting ion exchange membranes, typically have an equivalent weight (EW) of less than about 1000 g / mol, alternatively less than about 900 g / mol, alternatively less than about 850 g / mol, alternatively between about 400 and 1000 g / mol, alternatively between about 400 and 900 g / mol, alternatively between about 400 and 850 g / mol. EW can be measured by acid-base titration, where the unit g / mol refers to the amount in grams of fluorinated ionomer required to neutralize 1 mole of NaOH representing 1 mole of sulfonic acid groups.

[0018] A preferred class of fluorinated ionomers containing sulfonate groups is represented by the formula -(O-CF2CFR f ) a -O-CF2CFR' f SO3X (in the formula, R f and R' f is independently selected from F, Cl, or a perfluorinated alkyl group having 1 to 10 carbon atoms, a is 0, 1, or 2, and X is H, Li, Na, K, or N(R 1 )(R 2 )(R 3 )(R 4 )(wherein, R 1 , R 2 , R 3 , and R 4The ionomers preferably contain a highly fluorinated, most preferably perfluorinated, carbon backbone with pendant chains represented by X, X, XH, and XH, which may be the same or different and are H, CH3, or C2H5. Preferred fluorinated ionomers containing sulfonate groups include, for example, the polymers disclosed in U.S. Pat. No. 3,282,875, U.S. Pat. No. 4,358,545, or U.S. Pat. No. 4,940,525. For vanadium redox flow battery, water electrolysis, and fuel cell applications, the fluorinated ionomers in the ion exchange membranes are typically used in the proton form, i.e., X is H.

[0019] One preferred fluorinated ionomer containing sulfonic acid groups comprises a perfluorocarbon backbone and a pendant chain represented by the formula -O-CF2CF(CF3)-O-CF2CF2SO3X, where X is as defined above. When X is H, the side chain is -O-CF2CF(CF3)-O-CF2CF2SO3H. This type of fluorinated ionomer containing sulfonate groups is disclosed in U.S. Pat. No. 3,282,875 and can be made by copolymerization of TFE with a perfluorinated vinyl ether, CF2=CF-O-CF2CF(CF3)-O-CF2CF2SO2F, perfluoro(3,6-dioxa-4-methyl-7-octene sulfonyl fluoride) (PSEPVE), followed by hydrolysis of the sulfonyl fluoride groups to sulfonate groups, and conversion to the proton form if desired for a particular application.

[0020] One preferred fluorinated ionomer containing this type of sulfonate group, disclosed in US Patent No. 4,358,545 and US Patent No. 4,940,525, has a pendant chain -O-CF2CF2SO3X, where X is as defined above. This fluorinated ionomer containing sulfonic acid groups can be made by copolymerization of tetrafluoroethylene (TFE) with the perfluorinated vinyl ether CF2=CF-O-CF2CF2SO2F, perfluoro(3-oxa-4-pentenesulfonyl fluoride) (PFSVE), followed by hydrolysis and conversion to the proton form if required for a particular application. When X is H, the pendant chain is -O-CF2CF2SO3H.

[0021] The ion exchange membrane or the ion exchange dispersion may also include optional additives, including, but not limited to, reinforcing materials, fillers, surfactants, dispersing aids, or other materials. In one aspect, the ion exchange membrane does not include catalytic materials such as metals. In one embodiment, a reinforcing layer is embedded in the ion exchange membrane. In this case, the reinforcing layer may be, for example, polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkylvinylether copolymer, polyether ether ketone (PEEK), polyphenylene sulfide (PPS), polyether sulfone (PES), or liquid crystal polymer (LCP). The reinforcing layer may be in the form of a porous support layer, such as a woven fabric, an expanded or expanded film, or a net. The term "polytetrafluoroethylene" refers to the chemical makeup of the layer and may include woven PTFE, expanded PTFE (ePTFE), non-woven PTFE, and the like. When present, the reinforcing layer may comprise about 2-29.99 wt.%, alternatively about 5-24.90 wt.%, alternatively about 10-19.90 wt.%, or any range of wt.% within the aforementioned ranges, based on the total dry weight of the ion exchange membrane. The remainder of the amount of optional additive in wt.% of the total dry weight thickness is comprised of other types of additives. The reinforcing layer may have a thickness of about 1-100 μm, alternatively about 2-75 μm, alternatively about 3-60 μm, or any range of thickness within the aforementioned ranges, as measured by contact micrometer.

[0022] The ion exchange membrane is formed, for example, by casting a dispersion of an ion exchange polymer. The ion exchange dispersion can be cast on a substrate, dried, and annealed to form a dry membrane, which can then be peeled off from the substrate. If a reinforcing layer is used, the reinforcing material can be coated, immersed, or otherwise embedded in the ion exchange dispersion, and the product can then be applied onto a substrate, dried, annealed, and peeled off from the substrate to form a dry reinforced membrane. Other methods of coating the reinforcing layer include, but are not limited to, brushing, spraying, notch bar coating, fluid die coating, rod coating, slot-fed knife coating, three-roll coating, or decal transfer.

[0023] In one aspect, the present invention provides an ion exchange dispersion comprising a liquid carrier, a fluorinated ionomer, and Ce. x M 1-x O y The present invention relates to an ion exchange dispersion comprising a compound or nanoparticles and an optional additive, wherein x is 0.6-0.9, y is 1-3, and M is selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni. x M 1-x O yThe compounds and optional additives are described above. The liquid carrier may include water, an organic solvent, or a mixture thereof. Examples of suitable organic solvents include, but are not limited to, lower alcohols (methanol, ethanol, isopropanol, n-propanol, etc.), polyols (e.g., ethylene glycol, propylene glycol, glycerol, etc.), ethers (e.g., tetrahydrofuran and dioxane, etc.), diglyme, polyglycol ethers, ether acetates, acetonitrile, acetone, dimethylsulfoxide, N,N-dimethylacetamide, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, N,N-dimethylformamide, N-methylpyrrolidinone, dimethylimidazolidinone, butyrolactone, hexamethylphosphoric triamide, isobutyl methyl ketone, sulfolane, and combinations thereof. The solids content of the dispersion may range from about 5 to 40% by weight, alternatively from about 10 to 35% by weight, alternatively from about 15 to 30% by weight. When mixed with organic solvent, water typically comprises about 15-90% by weight, alternatively about 20-70% by weight, alternatively about 25-50% by weight of the total liquid carrier weight, with the remainder being made up of organic solvent.

[0024] The fluorinated ionomer comprises about 70-99.99 weight percent of the ion exchange membrane or ion exchange dispersion, alternatively about 70-97.99 weight percent, alternatively about 75-99.90 weight percent, alternatively about 75-94.90 weight percent, alternatively about 80-99.90 weight percent, alternatively about 80-89.90 weight percent, or any range of weight percents within the aforementioned ranges, based on the total dry weight of the ion exchange membrane or based on the total solids weight of the ion exchange dispersion. x M 1-x O yThe compound or nanoparticles comprise about 0.01-1.0 weight percent of the ion exchange membrane or ion exchange dispersion, alternatively about 0.1-1.0 weight percent, alternatively about 0.1-0.5 weight percent, or any range of weight percent within the aforementioned ranges, based on the total dry weight of the ion exchange membrane or based on the total solids weight of the ion exchange dispersion. The optional additives comprise about 0-29.99 weight percent (inclusive), alternatively about 0-24.90 weight percent, alternatively about 2-29.99 weight percent, alternatively about 5-24.90 weight percent, alternatively about 0-19.90 weight percent, alternatively about 10-19.90 weight percent, or any range of weight percent within the aforementioned ranges, based on the total dry weight of the ion exchange membrane or based on the total solids weight of the ion exchange dispersion.

[0025] The dry thickness of the ion exchange membrane depends on the needs of the end use application. For example, for fuel cell applications, the ion exchange membrane may have a dry thickness of less than about 20 μm, alternatively less than about 18 μm, alternatively about 8-18 μm, alternatively about 10-15 μm, as measured by a Mitutoyo thickness gauge. For water electrolyzer applications, the ion exchange membrane may have a dry thickness of less than about 40-120 μm, alternatively about 50-95 μm, alternatively about 45-85 μm, as measured by a Mitutoyo thickness gauge.

[0026] The ion exchange membrane is used in a membrane assembly having multiple layers of functional material. The membrane assembly, or membrane electrode assembly (MEA), may include a cathode catalyst layer (CCL) on one side of the ion exchange membrane and an anode catalyst layer (ACL) on the other side of the ion exchange membrane. For example, in one embodiment shown in FIG. 1, a cathode catalyst layer 4 is in direct contact with an ion exchange membrane 1, which is further in direct contact with an anode catalyst layer 2 to create an ion exchange membrane assembly 5. The ion exchange membrane 1 may have a reinforcing layer 3 embedded within the ion exchange membrane. The membrane assembly may include multiple layers of the same material and may include additional layers of functional material such as gas diffusion layers or bipolar plates.

[0027] The CCL and ACL may be applied to the ion exchange membrane in the form of a catalyst ink. The catalyst ink composition often includes a catalyst component and a polymeric binder, which often includes a fluorinated ionomer, such as the fluorinated ionomers described above. The polymer used in the CCL and ACL may be the same or different from the polymer used as the fluorinated ionomer in the ion exchange membrane. The catalyst component may include, but is not limited to, metal particles or carbon-supported metal particles. Specific metals may include, but are not limited to, platinum, ruthenium, gold, silver, palladium, iridium, rhodium, iron, cobalt, nickel, chromium, tungsten, manganese, vanadium, and alloys thereof. Solvents, such as those mentioned for use in the ion exchange dispersions, may be used to aid in the application of the catalyst ink to the ion exchange membrane. The CCL and ACL materials may be applied to the ion exchange membrane by any suitable means, including brushing, spraying, notch bar coating, fluid die coating, rod coating, slot-fed knife coating, three-roll coating, or decal transfer.

[0028] In one embodiment, the ion exchange membrane is unreinforced and lasts at least 400 hours before dropping below 0.8 V according to an open circuit voltage accelerated stress test (Fuel Cell Technical Team Roadmap, November 2017, Table P.3). In another embodiment, the ion exchange membrane is unreinforced and lasts at least 500 hours, in another embodiment, the ion exchange membrane is unreinforced and lasts at least 800 hours, and in another embodiment, the ion exchange membrane is unreinforced and lasts at least 1000 hours. In one embodiment, the ion exchange membrane is reinforced and lasts at least 1500 hours before dropping below 0.8 V according to an open circuit voltage accelerated stress test (Fuel Cell Technical Team Roadmap, November 2017, Table P.3), in another embodiment, the ion exchange membrane is reinforced and lasts at least 1800 hours, in another embodiment, the ion exchange membrane or the membrane electrode assembly is reinforced and lasts at least 2000 hours, and in another embodiment, the ion exchange membrane is reinforced and lasts at least 2300 hours. In one embodiment, the ion exchange membrane is reinforced and has a hydrogen crossover of 15 mA / cm according to a composite AST (Fuel Cell Technical Team Roadmap, November 2017, Table P.5). 2 and in another embodiment, the ion exchange membrane is reinforced and has a hydrogen crossover of 15 mA / cm. 2 and in another embodiment, the ion exchange membrane is reinforced and has a hydrogen crossover of 15 mA / cm. 2 It will last at least 100,000 combined cycles before exceeding EXAMPLES

[0029] The invention is illustrated in the following examples, which do not limit the scope of the invention described in the claims.

[0030] All solvents and reagents were obtained from Sigma-Aldrich (St. Louis, Mo.) unless otherwise indicated.

[0031] W813 is a Ce-based composite with a solid content of 13% by weight. 0.82 Zr 0.18 Dispersion of O2 (Ce 0.82 Zr 0.18 O2 has an average particle size of 5 nm) and Ce 0.75 Zr 0.25 The O2 dispersion contained 19.2 wt% solids. 0.75 Zr 0.25 Dispersion of O2 (Ce 0.75 Zr 0.25 CeO2 Dispersion 1 is a dispersion with 9.5 wt% solids (CeO2 has an average particle size of less than 25 nm), CeO2 Dispersion 2 is a dispersion with 20 wt% solids (CeO2 has an average particle size of 5 nm), all available from Cerion Nanomaterials (Rochester, NY).

[0032] Nafion™ D2020 is a perfluorosulfonic acid polymer dispersion having 20-22 wt. % solids and an EW of about 920 available from The Chemours Company (Wilmington, Del.).

[0033] The expanded PTFE reinforcing layer was a nonwoven fabric having a thickness of 8 μm available from Donaldson Company, Inc. (Minneapolis, MN).

[0034] Platinum-on-carbon black electrocatalyst (46.3% Pt) is available from Tanaka Kikinkzoku Koygo KK (Marunouchi, Japan).

[0035] Test Method The following test methods and materials were used in the examples herein.

[0036] 2. Preparation of Membrane Assembly Platinum-on-carbon black electrocatalyst (510.5 mg), deionized water (68.00 g), n-propanol (41.76 g), and Nafion™ D2020 dispersion (1194 μL) were stirred together to form a catalyst ink solution, which was then chilled on ice for 30 min. The catalyst ink was sonicated with a horn sonicator at 50% power for 10 s, followed by bath sonication in cold water (0-5 °C) for 30 min.

[0037] The catalyst ink was sprayed on both sides of the ion exchange membrane by ultrasonic spray coating (Sonotek ExactaCoat) at 90 °C with the vacuum turned on. The membrane was coated with 0.1 mg Pt / cm on the anode side. 2 , 0.4 mg Pt / cm on the cathode side 2 has a final loading of

[0038] Test Method 1 - Open Circuit Voltage (OCV) Accelerated Stress Test (AST) This test measures chemical stability and is known as OCV AST, a test standard established by the U.S. Department of Energy's Fuel Cell Technical Team Recommendations (Fuel Cell Technical Team Roadmap, November 2017, Table P.3). The membrane assemblies were tested according to this standard test method, except that these conditions were cycled for the times indicated rather than the standard 500 hours. The test was run until the cell voltage dropped below 0.8 V.

[0039] Test Method 2 - Complex AST This test measures the combined chemical and mechanical stability, known as Combined AST, a test standard established by the U.S. Department of Energy's Fuel Cell Technical Team Recommendation (Fuel Cell Technical Team Roadmap, November 2017, Table P.5). Membrane assemblies were tested according to this standard test method and demonstrated a hydrogen crossover of 15 mA / cm. 2 These conditions were repeated until the reaction temperature exceeded 100°C.

[0040] Comparative example A Nafion™ D2020 dispersion (15.0 g) was added to a 20 mL glass vial equipped with a stir bar and placed on a stir plate at medium rotation. CeO2 Dispersion 1 (124.1 mg) was added to the stirred dispersion until the CeO2 was fully incorporated to form a milky white liquid composite dispersion. The dispersion was cast onto a polyethylene terephthalate (PET) substrate fixed to a glass plate and coated to a wet thickness of 200 μm using a doctor blade. The dispersion layer was dried in a dry box at 10% relative humidity for 1 hour to form a dry film with a thickness of 17 μm across the membrane. The dried film was then heated at 160° C. for 3 minutes in a convection oven to thermally cure the polymer. After removal from the oven, the film was peeled off from the PET substrate to obtain a free-standing film. A membrane assembly was formed and tested according to the test method described above. The results are shown in Figure 2. The cell voltage dropped below 0.8 V at 166 hours.

[0041] Comparative example B Comparative Example A was repeated on a larger scale to form a membrane dispersion. Approximately 0.4 wt. % of CeO2 Dispersion 1 was added to the Nafion™ D2020 dispersion. The resulting mixture was then diluted to 16% solids while maintaining the same ratio of 1.29 parts by weight of n-propanol to 1 part by weight of water. A roll-to-roll slot die membrane coater was used to embed an expanded PTFE reinforcing layer into the resulting composite dispersion. This process resulted in a wet intermediate with a thickness of approximately 150 microns. The wet intermediate was then dried by successively heating to a series of increasing drying temperatures, the first of which was between 120 and 150°F, and the last of which was between 140 and 160°F. The dried intermediate membrane was then heat cured by a subsequent heating step, the temperature of which was between 320 and 340°F. Finally, the heat cured dry membrane was subjected to a final heating step, the temperature of which was between 110 and 130°F. The dry thickness of the membrane was 15 μm. A membrane assembly was formed and tested according to the test method described above. The results are shown in Figures 3 and 9. The cell voltage dropped to 0.802 V at 1,235 hours. Hydrogen crossover was 15 mA / cm for 38,016 cycles. 2 exceeded.

[0042] Comparative example C Comparative Example A was repeated using CeO2 Dispersion 2 instead of CeO2 Dispersion 1. In this example, stirred Nafion™ D2020 dispersion (15.0 g) was combined with CeO2 Dispersion 2 (58.9 mg) and the dry thickness of the membrane was 20 μm. A membrane assembly was formed and tested according to the test method described above. The results are shown in Figure 4. The cell voltage dropped to below 0.8 V at 180 hours.

[0043] Example 1 A dispersion of a copolymer of TFE and perfluoro(4-methyl-3,6-dioxa-7-octene-1-sulfonic acid) was formed by the procedure of U.S. Patent No. 4,433,082. The final polymer dispersion contained 27.5 wt.% ion exchange polymer, 27.6 wt.% water, and 44.9 wt.% ethanol and had an EW value of 814.

[0044] Separately, water and ethanol were combined in a vessel equipped with stirring. The W813 dispersion was slowly added to the mixture to obtain Ce with a W813 dispersion / water / ethanol weight ratio of 1 / 2 / 2. 0.82 Zr 0.18 The resulting CeO2 dispersion was 0.82 Zr 0.18 The O2 mixture (234.28 g) was mixed with the fluorinated ion exchange polymer dispersion (3 kg) under high mixing to form a composite dispersion. A roll-to-roll slot die membrane coater was used to embed the expanded PTFE reinforcing layer into the composite dispersion. This resulted in a wet intermediate with a thickness of approximately 130 microns. The resulting wet intermediate was then dried by successively heating to a series of increasing drying temperatures, the first of which was between 40 and 70°C, and the last of which was between 140 and 170°C. The dried intermediate membrane was then heat cured by a final heating step, the temperature of which was between 180 and 200°C. The dry thickness of the membrane was 15 μm.

[0045] A membrane assembly was formed and tested according to the test method described above, and the results are shown in Figures 5 and 10. The cell voltage dropped below 0.8 V at 3,346 hours, and the hydrogen crossover was 15 mA / cm for 112,878 cycles. 2 Compared with Comparative Example B and Comparative Example C, Ce 0.82 Zr 0.18 It can be seen that the membrane containing O2 has unexpectedly superior durability to a similarly reinforced membrane containing CeO2.

[0046] Example 2 Example 1 was repeated on a smaller scale using Nafion™ D2020 dispersion as the polymer dispersion. The composite dispersion was made up of 15.0 g of Nafion™ D2020 dispersion and 155.6 mg of Ce. 0.82 Zr 0.18The composite dispersion was cast onto a polyethylene terephthalate (PET) substrate fixed on a glass plate and coated to a wet thickness of 200 μm using a doctor blade. The dispersion layer was dried in a dry box at 10% relative humidity for 1 hour to form a dry film with a thickness of 18 μm across the membrane. The dried film was then heated at 160° C. for 3 minutes in a convection oven to thermally cure the polymer. After removal from the oven, the film was peeled off from the PET substrate to obtain a free-standing film with a dry thickness of 18 μm. The membrane assembly was formed and tested according to the test method described above. The results are shown in FIG. 6. The cell voltage dropped to below 0.8 V at 1,108 hours. Compared to Comparative Example A, the Ce 0.82 Zr 0.18 It can be seen that the membrane containing O2 lasts about six times longer than a similar unreinforced membrane containing CeO2.

[0047] Example 3 Example 1 was repeated, except that the wet thickness was 75 μm and the dry membrane thickness was 10 μm. A membrane assembly was formed and tested according to the test method described above. The results are shown in Figures 7 and 11. The cell voltage dropped to 0.805 V at 1,384 hours. Hydrogen crossover was 15 mA / cm for 107,550 cycles. 2 Even at a thinner thickness, this film has superior chemical and mechanical stability compared to the film using the CeO2 radical scavenger.

[0048] Example 4 Radical scavenger dispersion contains Ce 0.75 Zr 0.25 Example 2 was repeated, except that the CeO2 dispersion was O2. A membrane assembly was formed and tested according to the test method described above. The results are shown in Figure 8. The cell voltage dropped to below 0.8 V at 2,330 hours. Compared to Comparative Example A, the CeO2 dispersion was O2. 0.75 Zr 0.25 The membrane containing O2 is found to last about 14 times longer than a similar unreinforced membrane containing CeO2.

Claims

1. 1. An ion exchange membrane comprising about 70-99.99 wt. % of a fluorinated ionomer and about 0.01-1.0 wt. % of Ce, all based on the total dry weight of the membrane. x M 1-x O y 1. An ion exchange membrane comprising nanoparticles and about 0-29.99 wt. % of an optional additive, wherein x is 0.6-0.9, y is 1-3, and M is selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni.

2. The ion exchange membrane of claim 1 , wherein the optional additive is present and comprises a reinforcing layer embedded in the ion exchange membrane.

3. The ion exchange membrane according to claim 2, wherein the reinforcing layer is selected from polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkylvinylether copolymer, polyetheretherketone, polyphenylene sulfide, polyethersulfone, or liquid crystal polymer.

4. The ion exchange membrane of claim 3 , wherein the reinforcing layer is expanded PTFE (ePTFE).

5. The ion exchange membrane according to claims 1 to 4, wherein M is Zr.

6. The Ce x M 1-x O y The ion exchange membrane according to claims 1 to 5, wherein the nanoparticles have an aspect ratio of 1:1 to 1:

10.

7. The Ce x M 1-x O y The ion exchange membrane of claim 6, wherein the nanoparticles have an aspect ratio of 1:1 to 1:

3.

8. The Ce x M 1-x O y The ion exchange membrane according to any one of claims 1 to 7, wherein the nanoparticles have an average particle size of about 1 to 25 nm.

9. The Ce x M 1-x O y The ion exchange membrane of claim 8, wherein the nanoparticles have an average particle size of about 1 to 15 nm.

10. The ion exchange membrane of claims 1 to 9 having an equivalent weight (EW) of less than about 1000 g / mol.

11. 11. The ion exchange membrane of claim 10 having an EW of less than about 900 g / mol.

12. The ion exchange membrane of claims 1 to 11 having a dry thickness of less than about 20 μm.

13. The ion exchange membrane according to claims 1 to 11, having a dry thickness of about 40 to 120 μm.

14. About 75-99.90 wt. % fluorinated ionomer and about 0.1-1.0 wt. % Ce, all based on the total dry weight of the membrane. x M 1-x O y The ion exchange membrane of claims 1 to 13, comprising nanoparticles and about 0 to 24.90 wt % of optional additives.

15. The ion exchange membrane according to claims 1 to 14, wherein the fluorinated ionomer is a fluorinated polymer having a sulfonate group.

16. 1. An ion exchange dispersion comprising a liquid carrier, about 70-99.99 wt. % of a fluorinated ionomer, and about 0.01-1.0 wt. % of Ce, all based on the total solids weight of the dispersion. x M 1-x O y 1. An ion-exchange dispersion comprising nanoparticles and about 0-29.99 wt. % of an optional additive, wherein x is 0.6-0.9, y is 1-3, and M is selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni.

17. 17. The ion-exchanged dispersion of claim 16, wherein M is Zr.

18. The Ce x M 1-x O y 18. An ion exchange dispersion according to claims 16 to 17, wherein the nanoparticles have an aspect ratio of from 1:1 to 1:

10.

19. The Ce x M 1-x O y The ion exchange dispersion of claims 16 to 18, wherein the nanoparticles have an average particle size of about 1 to 25 nm.

20. 20. The ion exchange dispersion of claims 16-19 having an equivalent weight (EW) of less than about 1000 g / mol.

21. About 75-99.90 wt. % fluorinated ionomer and about 0.1-1.0 wt. % Ce, all based on the total solids weight of the dispersion. x M 1-x O y 21. The ion exchange dispersion of claims 16-20 comprising nanoparticles and about 0-24.90 wt. % of optional additives.

22. The ion exchange dispersion of claims 16 to 21, wherein the fluorinated ionomer is a fluorinated polymer having sulfonate groups.

23. A membrane assembly comprising the ion exchange membrane of claims 1 to 15, wherein the membrane assembly comprises a cathode catalyst layer on one side of the ion exchange membrane and an anode catalyst layer on the other side of the ion exchange membrane.

24. 1. An ion exchange membrane comprising about 70-97.99 wt. % of a fluorinated ionomer and about 0.01-1.0 wt. % of Ce, all based on the total dry weight of the membrane. x M 1-x O y 1. An ion exchange membrane comprising nanoparticles and about 2-29.99 wt. % of an additive comprising a reinforcing layer, wherein x is 0.2-0.9, y is 1-3, and M is selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni, and wherein the reinforcing layer is embedded in the ion exchange membrane.

25. 25. The ion exchange membrane of claim 24, wherein the reinforcing layer is selected from polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkylvinylether copolymer, polyetheretherketone, polyphenylene sulfide, polyethersulfone, or liquid crystal polymer.

26. 26. The ion exchange membrane of claim 25, wherein the reinforcing layer is expanded PTFE (ePTFE).

27. The ion exchange membrane according to claims 24 to 26, wherein M is Zr.

28. The Ce x M 1-x O y The ion exchange membrane according to claims 24 to 27, wherein the nanoparticles have an aspect ratio of 1:1 to 1:

10.

29. The Ce x M 1-x O y 29. The ion exchange membrane of claim 28, wherein the nanoparticles have an aspect ratio of 1:1 to 1:

3.

30. The Ce x M 1-x O y The ion exchange membrane according to claims 24 to 29, wherein the nanoparticles have an average particle size of about 1 to 25 nm.

31. The Ce x M 1-x O y The ion exchange membrane of claim 30, wherein the nanoparticles have an average particle size of about 1 to 15 nm.

32. The ion exchange membrane of claims 24 to 31 having an equivalent weight (EW) of less than about 1000 g / mol.

33. 33. The ion exchange membrane of claim 32 having an EW of less than about 900 g / mol.

34. The ion exchange membrane of claims 24 to 33 having a dry thickness of less than about 20 μm.

35. The ion exchange membrane of claims 24 to 33 having a dry thickness of about 40 to 120 μm.

36. About 75-94.90 wt. % fluorinated ionomer and about 0.1-1.0 wt. % Ce, all based on the total dry weight of the membrane. x M 1-x O y 36. The ion exchange membrane of claims 24-35, comprising nanoparticles and about 5-24.90% of optional additives.

37. The ion exchange membrane according to claims 24 to 36, wherein the fluorinated ionomer is a fluorinated polymer having a sulfonate group.

38. A membrane assembly comprising the ion exchange membrane of claims 24 to 37, wherein the membrane assembly comprises a cathode catalyst layer on one side of the ion exchange membrane and an anode catalyst layer on the other side of the ion exchange membrane.

39. 1. An ion exchange membrane comprising about 70-99.99 wt. % of a fluorinated ionomer and about 0.01-1.0 wt. % of Ce, all based on the total dry weight of the membrane. x M 1-x O y and about 0-29.99 wt. % of an optional additive, wherein x is 0.6-0.9, y is 1-3, and M is selected from Zr, Gd, Pr, Eu, Nd, La, Hf, Tb, Pd, Pt, or Ni; If the membrane is unreinforced, it will last at least 400 hours before dropping below 0.8 V according to an accelerated open circuit voltage stress test; or An ion exchange membrane, provided that when said membrane is reinforced, said membrane will last at least 1500 hours before dropping below 0.8 V according to an open circuit voltage accelerated stress test.

40. 40. The ion exchange membrane of claim 39, wherein the membrane, when unreinforced, lasts for at least 500 hours before dropping below 0.8 V following an accelerated open circuit voltage stress test, or the membrane, when reinforced, lasts for at least 1800 hours before dropping below 0.8 V following an accelerated open circuit voltage stress test.

41. The ion exchange membrane of claims 39-40, wherein the optional additive is present and comprises a reinforcing layer embedded in the ion exchange membrane.

42. About 70-97.99 wt. % fluorinated ionomer and about 0.01-1.0 wt. % Ce, all based on the total dry weight of the membrane. x M 1-x O y 42. The ion exchange membrane of claim 41 comprising nanoparticles and about 2-29.99 wt. % of the additive comprising the reinforcing layer.

43. The ion exchange membrane according to claims 41 to 42, wherein the reinforcing layer is selected from polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkylvinylether copolymer, polyetheretherketone, polyphenylene sulfide, polyethersulfone, or liquid crystal polymer.

44. 44. The ion exchange membrane of claim 43, wherein the reinforcing layer is expanded PTFE (ePTFE).

45. The ion exchange membrane according to claims 39 to 44, wherein M is Zr.

46. The Ce x M 1-x O y The ion exchange membrane according to claims 39 to 45, wherein the compound has an aspect ratio of 1:1 to 1:

10.

47. The Ce x M 1-x O y 47. The ion exchange membrane of claim 46, wherein the compound has an aspect ratio of 1:1 to 1:

3.

48. The Ce x M 1-x O y The ion exchange membrane according to claims 39 to 47, wherein the compound has an average particle size of about 1 to 25 nm.

49. The Ce x M 1-x O y The ion exchange membrane of claim 48, wherein the compound has an average particle size of about 1 to 15 nm.

50. The ion exchange membrane of claims 39 to 49 having an equivalent weight (EW) of less than about 1000 g / mol.

51. 51. The ion exchange membrane of claim 50 having an EW of less than about 900 g / mol.

52. The ion exchange membrane of claims 39 to 51 having a dry thickness of less than about 20 μm.

53. The ion exchange membrane of claims 39 to 51 having a dry thickness of about 40 to 120 μm.

54. About 75-99.90 wt. % fluorinated ionomer and about 0.1-1.0 wt. % Ce, all based on the total dry weight of the membrane. x M 1-x O y 54. The ion exchange membrane of claims 39-53, comprising the compound and about 0-24.90 wt. % of optional additives.

55. The ion exchange membrane according to claims 39 to 54, wherein the fluorinated ionomer is a fluorinated polymer having sulfonate groups.

56. 56. A membrane assembly comprising the ion exchange membrane of claims 39-55, wherein the membrane assembly comprises a cathode catalyst layer on one side of the ion exchange membrane and an anode catalyst layer on the other side of the ion exchange membrane.

Citation Information

Patent Citations

  • Solid polyelectrolyte film and polymer electrolyte fuel cell using the same, and their manufacturing method

    JP2006059756A

  • Additive for layer of fuel cell