Nano-sized polyhedral α-alumina particles and their manufacturing method

α-alumina particles with a polyhedral crystal structure address thermal shrinkage and maintain air permeability in secondary battery separation membranes, enhancing thermal stability and ion flow.

JP2024537667AActive Publication Date: 2024-10-16DAEHONG TECHNEW CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024516655
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-28
Filing Date
2022-10-28
Publication Date
2024-10-16
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

Existing secondary battery separation membranes face issues with thermal shrinkage and reduced air permeability due to the use of spherical or amorphous alumina particles, which can lead to safety risks and decreased battery performance.

Method used

The use of α-alumina particles with a polyhedral crystal structure and nano-sized particles (100 to 900 nm) is produced by mixing aluminum salts and a pH regulator, followed by fluorine-based mineralization and calcination, forming a coating that suppresses thermal shrinkage while maintaining high air permeability.

Benefits of technology

The polyhedral α-alumina particles effectively prevent thermal shrinkage and maintain high air permeability, ensuring smooth ion movement and battery performance by forming surface contacts and minimizing interstitial spaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537667000001_ABST
    Figure 2024537667000001_ABST
Patent Text Reader

Abstract

The present invention relates to a polyhedral crystal structure having an average particle size (D 50 The present invention provides a coating agent including α-alumina particles having a particle diameter of 100 to 900 nm. The α-alumina particles are manufactured by mixing pseudoboehmite with a fluoride-based mineralizer and ultrapure water, grinding the mixture, and then sintering the resulting powder to grow into polyhedrons. The polyhedral alumina particles are coated on the surface of a porous polymer substrate while forming surface contact, and the vacant space induced by the interstitial volume between the particles is larger than that of spherical particles, thereby effectively suppressing the thermal shrinkage of the porous polymer substrate and realizing excellent breathability. In addition, the nano-level particle size allows for excellent dispersibility and the formation of a thin coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to α-alumina particles having a polyhedral crystal structure and nano-size and useful as a coating material for components such as secondary battery separators, and a method for producing the same. [Background technology]

[0002] Alumina (Al2O3) has excellent mechanical strength including abrasion resistance, chemical stability, thermal conductivity, and heat resistance, and is used in a wide range of areas such as abrasives, electronic materials, heat dissipation fillers, optical materials, and biomaterials. Such alumina includes α, γ, or η crystalline alumina, and amorphous alumina, but is generally referred to as α-alumina, and its uses can vary depending on the particle size, shape, surface characteristics, and degree of aggregation.

[0003] Recently, alumina has been used as a surface coating to impart thermal stability to separators in secondary batteries used in a variety of electric / electronic devices including mobile devices and electric vehicles.

[0004] In secondary batteries, the separator separates the positive and negative electrodes to prevent electrical shorts, and absorbs the electrolyte required for the battery reaction to maintain high ionic conductivity. To this end, it is generally made of a porous polymer substrate (e.g., polyolefin). When heated, the porous polymer substrate shrinks, which can cause safety issues such as fire and explosion when the positive and negative electrodes come into contact. To overcome this, inorganic particles such as alumina are coated on one or both sides of the porous polymer substrate together with a binder to protect the separator from the risk of breakage and prevent thermal shrinkage.

[0005] Alumina used for coating such separators is mostly spherical or amorphous particles. The spherical alumina is coated on the surface of the separator, and the interstitial volume between the particles creates vacant space, which maintains the separator's breathability and allows smooth movement of ions inside the battery. However, because spherical alumina is coated on the surface of the separator by forming point contacts, it has the disadvantage of being weak in suppressing contraction when the separator is deformed by heat (see Figure 1). In addition, amorphous particles are not uniform in shape, which increases the possibility of causing coating defects on the surface of the separator.

[0006] Meanwhile, in Korean Patent Publication No. 10-2018-0010477 (applicant: CIS), in order to provide alumina for coating the separator of a secondary battery, aluminum hydroxide, ammonium chloride, and sodium polyphosphate are mixed in a solvent, and the mixture is subjected to high-temperature heat treatment, filtration, washing, and dry grinding to produce micro-sized plate-like alumina. This plate-like alumina is excellent in preventing shrinkage due to heat by being in surface contact with the surface of the separator, but since it is laminated and coated in plate form on the surface of the separator through surface contact, it can block the pores of the separator, which can reduce ion movement and cause a decrease in battery performance (see Figure 2). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Republic of Korea Patent Publication No. 10-2018-0010477 Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made to overcome the shortcomings of the prior art by providing a coating agent including α-alumina particles, which can form a surface contact with a surface of a porous substrate such as a separator for a secondary battery, thereby improving heat shrinkage resistance while also realizing excellent breathability, and a method for manufacturing the same. [Means for solving the problem]

[0009] One aspect of the present invention is a polyhedral crystal structure having an average particle size (D 50 The present invention provides a coating agent containing α-alumina particles having a particle diameter of 100 to 900 nm.

[0010] Another aspect of the present invention is a method for producing α-alumina particles contained in the coating agent, comprising the steps of: (Step S1) mixing and reacting an aqueous solution containing one or more aluminum salts with an aqueous solution containing a pH adjuster, filtering and washing the product to obtain pseudoboehmite represented by the following structural formula 1; (Step S2) mixing the pseudoboehmite with a fluorine-based mineralizer and ultrapure water, pulverizing the mixture, filtering and drying the mixture; and (Step S3) filtering and drying the product of Step S2, and calcining the mixture to obtain pseudoboehmite having a polyhedral crystal structure and an average particle size (D 50 obtaining a powder of α-alumina particles having a diameter of 100 to 900 nm.

[0011] [ka] (Structural formula 1)

[0012] Yet another aspect of the present invention provides a member including a porous polymer substrate and a coating layer formed on one or both sides of the substrate, the coating layer including a coating agent including the nano-sized polyhedral α-alumina particles. Effect of the Invention

[0013] The α-alumina particles contained in the coating agent of the present invention are manufactured by mixing pseudoboehmite with a fluoride-based mineralizer and ultrapure water, grinding the mixture, and then sintering the resulting powder to grow it into a polyhedron, and the polyhedral alumina particles are coated on the surface of the porous polymer substrate while forming surface contact, and the vacant space induced by the interstitial volume between the particles is larger than that of spherical particles, so that the thermal shrinkage of the porous polymer substrate is effectively suppressed and excellent breathability is realized. In addition, the nano-level particle size allows for excellent dispersibility and the formation of a thin coating layer. [Brief description of the drawings]

[0014] [Figure 1] 1A and 1B are schematic illustrations of the surface contact morphology when coating a substrate with α-alumina particles. [Diagram 2] 1A and 1B are schematic illustrations of the surface contact morphology when coating a substrate with α-alumina particles. [Diagram 3] 1A and 1B are schematic illustrations of the surface contact morphology when coating a substrate with α-alumina particles. [Figure 4] 2 shows scanning electron microscope (SEM) and transmission electron microscope (TEM) photographs of polyhedral α-alumina particles prepared in Examples 1 and 2 and Comparative Example 1. [Diagram 5] 2 is a SEM photograph of plate-shaped α-alumina particles produced in Comparative Example 2. [Figure 6] In Experimental Example 2, the dimensional change due to thermal shrinkage was observed according to the size and type of alumina particles coated on the circular specimen. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Since the present invention can be modified in various ways and has various embodiments, specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, this is not intended to limit the present invention to the specific embodiment, but should be understood to include any modifications, equivalents, or alternatives within the spirit and technical scope of the present invention. In describing the present invention, if it is determined that a detailed description of related publicly known technology may obscure the gist of the present invention, the detailed description will be omitted.

[0016] The present invention will now be described in more detail.

[0017] One embodiment of the present invention relates to a coating agent comprising α-alumina particles having a polyhedral crystal structure and nano-size.

[0018] The polyhedral crystal structure means that the ratio (D / H) of the diameter (D) perpendicular to the

[0001] plane, which is the crystallographic C-plane, to the height (H) parallel thereto is close to 1.

[0019] In particular, the α-alumina particles according to the present invention may have a tetradecahedral crystal structure in which the <0001> faces occupy 10-20%, specifically 15-20%, of the total crystal face area. If the <0001> face area is less than 10%, the particles will be rod-shaped, and if it exceeds 20%, the particles will be closer to a plate-like shape. Meanwhile, "amorphous" refers to an irregular state in which the outer shape is not constant, and is distinguished from the polyhedral crystal structure of the present invention, which has clear crystal faces.

[0020] When the alumina particles having a polyhedral crystal structure of the present invention are coated on the surface of a porous substrate, void spaces are formed due to the certain angles that the crystal faces of the polyhedrons make as the particles are dispersed and in contact with each other. The void spaces are referred to as pores formed by the interstitial volume between the particles, and when comparing Figures 1 and 3, the void spaces formed by the polyhedral particles are larger than those of spherical particles.

[0021] Referring again to FIG. 3, the particles having the polyhedral crystal structure form surface contact when coated onto the surface of a substrate, and are therefore more effective at preventing thermal shrinkage of the substrate than spherical particles (FIG. 1) which form point contact with the substrate surface.

[0022] On the other hand, referring to FIG. 2, the plate-shaped particles form surface contact with the surface of the substrate, and thus are excellent in preventing thermal shrinkage of the substrate. However, since the particles are stacked in a plate shape, there is little free space, which is disadvantageous in terms of breathability.

[0023] Therefore, the α-alumina particles having a polyhedral crystal structure according to the present invention can be effectively used as a coating agent that not only effectively suppresses thermal shrinkage when coated on a porous polymer substrate such as a separator for a secondary battery, but also enables smooth movement of lithium ions to the porous substrate, thereby not impairing battery performance.

[0024] In addition, the α-alumina particles having a polyhedral crystal structure of the present invention have an average particle size (D 50 ) is in the range of 100 to 900 nm, specifically, 200 to 600 nm.

[0025] D 50 is a median value of the particle size distribution measured by a method commonly used in the art, for example, by using a laser particle size analyzer. In the present invention, D 50 Since the separator has a nano-level structure, it has an advantage in that it improves dispersibility in a coating solution and forms a thinner coating layer than micro-sized particles, thereby reducing the weight and volume of a secondary battery to which the separator is applied.

[0026] Meanwhile, when the polyhedral α-alumina particles are coated on the surface of a porous substrate such as a separator, it is preferable to select the average particle size of the alumina particles to be larger than the pore size of the porous substrate in order to prevent the particles from filling the pores of the porous substrate.

[0027] Another embodiment of the present invention relates to a method for producing an abrasive material containing the α-alumina particles having the polyhedral crystal structure. The method will be described below step by step.

[0028] First, an aqueous solution containing one or more aluminum salts and an aqueous solution containing a pH adjuster are mixed and reacted with each other (Step S1).

[0029] The aluminum salt may include aluminum sulfate (Al2(SO4)3·4~18H2O), aluminum nitrate (Al(NO3)3·9H2O), aluminum acetate (Al(CHCOO)3OH) or a mixture thereof, and is dissolved in heated water (e.g., about 60°C) at a concentration of 5~30% to prepare an aqueous solution for complete dissolution.

[0030] The pH adjuster may include sodium carbonate (Na2CO3), sodium hydroxide (NaOH), potassium hydroxide (KOH), calcium carbonate (CaCO3), or a mixture thereof, and is dissolved in heated water (e.g., about 40°C) at a concentration of 5 to 30% to prepare an aqueous solution for complete dissolution.

[0031] The aluminum salt aqueous solution and the pH adjuster aqueous solution may be mixed at a constant rate (e.g., 25 ml / min) to carry out a sol-gel reaction at a temperature ranging from room temperature to 95° C. The pH of the reactant ranges from 6 to 10.

[0032] Through the above reaction, pseudo-boehmite, which has a chemical composition of AlO(OH) as shown in the following structural formula 1, is produced as a solid.

[0033] [ka] (Structural formula 1)

[0034] Pseudoboehmite of the structural formula 1 has water (H2O) bound to the octahedral unit cell, and therefore has a high water content and a small crystallite size. Therefore, it is formed under a lower pH condition than aluminum hydroxide (Al(OH)3), which is mainly used as a starting material in the conventional alumina production, and when it is transformed into α-Al2O3 through a high-temperature firing process in the subsequent step, it is advantageous to obtain a polyhedral crystal structure because particle aggregation and phase transition occur due to seeds at a relatively low temperature.

[0035] The pseudoboehmite solid is filtered and washed, then mixed with a fluorine-based mineralizer and ultrapure water, and pulverized (step S2).

[0036] The fluoride mineralizer is an additive for growing the crystals of α-alumina particles, and LiF2, AlF3, NaF, NaPF6, K2TiF6, MnF2, or a mixture thereof is used.

[0037] When used in excess, such fluoride-based mineralizers may remain in the final α-alumina or form agglomerates during the firing process. To minimize such drawbacks, it is advantageous to use the precursor powder and the fluoride-based mineralizer in a weight ratio of 100:0.1 to 100:2, more preferably 100:0.5 to 100:1.5.

[0038] The ultrapure water is used in a ratio of 1 to 10 times the weight of the pseudoboehmite to improve the efficiency of grinding while wet-dispersing the pseudoboehmite solid and the fluoride-based mineralizer. The wet dispersion affects the polyhedral crystal structure of the α-alumina particles that are finally produced by uniformly dispersing the fluoride-based mineralizer and minimizing the aggregation of the precursor (pseudoboehmite) particles.

[0039] The pulverization is carried out by a milling method using a number of balls having a diameter of 1 to 20 mm for 1 to 100 hours.

[0040] The pulverized product is filtered and dried, and the resulting powder is then calcined to obtain a powder of α-alumina particles having a nano-sized polyhedral crystal structure (step S3).

[0041] The sintering is a process of melting and synthesizing the dried powder by heat treatment at high temperature, and is carried out in a crucible made of high purity alumina or zirconia.

[0042] Specifically, the firing is performed by increasing the temperature at 3 to 15° C. / min, and then maintaining the temperature at 800 to 1000° C. for 2 to 5 hours. Meanwhile, the firing conditions can be appropriately changed in consideration of the reaction and volatility due to the difference in melting point between each material of the mixture, and the amount of heat required for synthesis.

[0043] The nano-sized polyhedral α-alumina particles prepared as described above are coated on the surface of the porous substrate while forming surface contact, and the void space induced by the interstitial volume between the particles is larger than that of spherical particles, so that the thermal shrinkage of the porous substrate can be effectively suppressed and excellent breathability can be realized.

[0044] Therefore, the present invention further provides a member comprising a porous polymer substrate and a coating layer formed on one or both sides of the substrate, the coating layer being manufactured according to the present invention, having a polyhedral crystal structure, and an average particle size (D 50 The present invention provides a member including α-alumina particles having a particle diameter of 100 to 900 nm.

[0045] In one embodiment of the present invention, the member may include a separator for a secondary battery, the thickness of the porous polymer substrate included in the separator may be in the range of 1 to 100 μm, the diameter of the pores in the porous substrate may be in the range of 10 to 100 nm, 10 to 70 nm, or 10 to 50 nm, and the average particle size of the polyhedral alumina particles may be selected to be larger than the pore size of the porous substrate.

[0046] In addition, the coating layer may contain a binder to provide adhesion of the nano-sized polyhedral α-alumina to the surface of the substrate, and the binder may be selected from polyethylene, polypropylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polystyrene, polyacrylic, and mixtures thereof, each of which has adhesive properties. The thickness of the coating layer is not particularly limited, but is in the range of 0.5 to 50 μm or 1 to 10 μm in consideration of the intended performance of the porous substrate.

[0047] A member having a coating layer containing the nano-sized polyhedral α-alumina particles has a dimensional retention of 50% or more, as defined by the following Equation 1, in a thermal stability test using a circular specimen.

[0048] (Number 1) Dimensional retention rate (%) = (d1 / d0) 2

[0049] In the above formula, d0 is the diameter of the circular specimen before heat treatment, and d1 is the diameter of the circular specimen after heat treatment at 150° C. for 30 minutes.

[0050] Furthermore, the member can satisfy an air permeability of 215 sec / 100 cc or less, for example, 200 to 211 sec / 100 cc, in an air permeability test that measures the time it takes for 100 cc of air to permeate a circular test piece with a diameter of 1 inch.

[0051] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to specific examples so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein. EXAMPLES

[0052] Example 1:

[0053] (Stage 1) Aqueous solution (a) was prepared by completely dissolving 199.8g of Al2(SO4)3·14~18H2O in 982.8g of pure water heated at 60℃, and aqueous solution (b) was prepared by completely dissolving 95.4g of Na2CO3 in 528g of pure water heated at 40℃. Aqueous solution (b) was added to aqueous solution (a) at a rate of 25mL / min and stirred for 10 minutes to react. The reaction product (pH 7.3~7.8) was filtered and washed to obtain pseudoboehmite solids.

[0054] (Stage 2) 40 g of the pseudoboehmite solid and 30.2 g of AlF were mixed with 120 g of ultrapure water, and milled for 48 hours using a ball having a diameter of 5 mm, followed by filtration and drying.

[0055] (Stage 3) The obtained product was filtered and dried, and then heat-treated at 900° C. for 5 hours with a temperature increase rate of 10° C. / min to obtain α-alumina powder.

[0056] Example 2: The same procedure as in Example 1 was carried out, except that in step 2, the grinding by ball milling was carried out for 24 hours.

[0057] Comparative Example 1: The same process as in Example 1 was carried out, except that ball milling was not performed in step 2.

[0058] Comparative Example 2: Aqueous solution (a) was prepared by completely dissolving 199.8g of Al2(SO4)3·14~18H2O in 982.8g of pure water heated at 60℃, and aqueous solution (b) was prepared by completely dissolving 72g of NaOH in 528g of pure water heated at 40℃. Aqueous solution (b) was added to aqueous solution (a) at a rate of 25mL / min and stirred for 10 minutes to react. The reaction product (pH 7.3~7.8) was filtered, washed, dried, and then crushed to obtain pseudoboehmite powder.

[0059] 40 g of the pseudoboehmite powder and 30.8 g of AlF were dry mixed. The mixed powder was heat-treated and fired at 900° C. for 5 hours with a temperature increase rate of 10° C. / min. After the heat treatment, α-alumina particle powder was finally obtained.

[0060] The physical properties of the α-alumina particles prepared in the above examples and comparative examples were measured and are shown in Table 1 below.

[0061] [Table 1]

[0062] As can be seen from Table 1, the α-alumina particles produced by crushing pseudoboehmite, wet mixing it with a fluoride-based mineralizer, and then calcining it according to the embodiment have an average nano-sized diameter (D 50 ) while D 50 The crystal structure exhibited a polyhedral crystal structure with a thickness ratio close to 1.

[0063] Meanwhile, SEM and TEM photographs of the α-alumina particles prepared in Examples 1 and 2 and Comparative Example 1 are shown in FIG.

[0064] From FIG. 4, it can be seen that the α-alumina particles of Examples 1 and 2 have a nano-sized tetradecahedral crystal structure, while the α-alumina particles of Comparative Example 1 have a micro-sized tetradecahedral crystal structure.

[0065] FIG. 5 is an SEM photograph of the α-alumina particles produced in Comparative Example 2, in which the plate-like structure can be seen.

[0066] Experimental example 1: Air permeability test when coating secondary battery separator A coating layer was formed on one side of a separator for a secondary battery using each of the α-alumina particles prepared in the examples and comparative examples. Specifically, the α-alumina particles and an acrylic polymer binder were dispersed in water at a ratio of 95:5 to obtain a slurry, which was then coated on one side of a polyethylene (PE) porous substrate (thickness 11 μm) and dried to form a coating layer with a thickness of 2 μm.

[0067] The porous substrate having the α-alumina particle coating layer formed thereon was cut into a circular specimen having a diameter of 1 inch, and the time required for 100cc of air to permeate through each specimen was measured using an air permeability measuring device (ASAHI SEIKO Co., Ltd.) (measurement condition: 25°C). The results are shown in Table 2 below.

[0068] [Table 2]

[0069] From Table 2, it can be seen that the PE substrate coated with the nano-sized polyhedral α-alumina particles prepared in Examples 1 and 2 has excellent breathability because it takes less time for air to pass through, compared to the substrate coated with the plate-type alumina particles of Comparative Example 2. Meanwhile, the alumina particles of Comparative Example 1 have the best breathability due to their micron size, but are disadvantageous in terms of thermal stability as shown in Experimental Example 2 below.

[0070] Experimental example 2: Thermal stability test for secondary battery separator coating The polyhedral α-alumina particles, which were confirmed to have excellent air permeability in Experimental Example 1, were subjected to a thermal stability test according to size.

[0071] First, four types of polyhedral α-alumina particles with different particle sizes (100 nm, 250 nm, 500 nm, and 2 μm) and general spherical α-alumina particles (average particle size: 500 to 700 nm) were prepared, and each particle was used to form a coating layer with a thickness of 2 μm on a PE porous substrate in the same manner as in Experimental Example 1, and then circular specimens with a diameter of 18 mm were manufactured. Three circular specimens were manufactured for each coated alumina particle.

[0072] Each of the circular specimens was heat-treated at 150° C. for 30 minutes, and then the dimensional change was observed. The results are shown in FIG.

[0073] In addition, after the heat treatment of each specimen, the dimensional retention rate defined by the following Equation 1 was measured, and the results are shown in Table 3 below.

[0074] (Number 1) Dimensional retention rate (%) = (d1 / d0) 2

[0075] In the above formula, d0 is the diameter of the circular specimen before heat treatment, and d1 is the diameter of the circular specimen after heat treatment at 150° C. for 30 minutes.

[0076] [Table 3]

[0077] Referring to Table 3 and FIG. 6, it can be seen that the polyhedral particles have superior thermal stability after being coated on the PE porous substrate compared to the spherical particles.

[0078] Although the specific parts of the present invention have been described in detail above, it is obvious to those skilled in the art that such specific descriptions are merely preferred embodiments and do not limit the scope of the present invention. Therefore, the substantial scope of the present invention is defined by the claims and their equivalents.

Claims

1. It has a polyhedral crystal structure and an average particle size (D 50 ) is 100 to 900 nm.

2. The average particle diameter of the α-alumina particles (D 50 2. The coating agent according to claim 1, wherein the average particle diameter of the first and second particles is 200 to 600 nm.

3. 2. The coating agent of claim 1, wherein the polyhedral crystal structure of the α-alumina particles comprises a tetradecahedral crystal structure.

4. 2. The coating agent according to claim 1, wherein the ratio of [0001] faces in the polyhedral crystal structure of the α-alumina particles is 10 to 20% of the total crystal face area.

5. A method for producing α-alumina particles contained in the coating agent according to claim 1, comprising the steps of: (Step S1) mixing and reacting an aqueous solution containing one or more aluminum salts with an aqueous solution containing a pH adjuster, and filtering and washing the product to obtain pseudoboehmite represented by the following structural formula 1; (Step S2) mixing the pseudoboehmite with a fluorine-based mineralizer and ultrapure water, pulverizing the mixture, filtering and drying the mixture; (Step S3) The product of step S2 is filtered and dried, and then calcined to obtain a polyhedral crystal structure having an average particle size (D 50 obtaining a powder of α-alumina particles having a diameter of 100 to 900 nm. 【Chemistry 1】 (Structural formula 1)

6. The aluminum salt used in step S1 is aluminum sulfate (Al 2 (SO 4 ) 3 ・4 to 18 hours 2 O), aluminum nitrate (Al(NO 3 ) 3 ・9H 2 O), aluminum acetate (Al(CHCOO) 3 6. The method of claim 5, further comprising the step of:

7. The pH adjuster used in step S1 is sodium carbonate (Na 2 CO 3 ), sodium hydroxide (NaOH), potassium hydroxide (KOH), calcium carbonate (CaCO 3 6. The method of claim 5, comprising:

8. The method of claim 5, wherein the ultrapure water is used in step S2 in a ratio of 1 to 10 times the weight of the pseudoboehmite.

9. The method according to claim 5, wherein the pulverization in step S2 is carried out for 1 to 100 hours by a milling method using a plurality of balls having a diameter of 1 to 20 mm.

10. The method of claim 5, wherein in step S2, the pseudoboehmite and the fluoride-based mineralizer are used in a weight ratio of 100:0.1 to 100:

2.

11. The fluoride mineralizer is LiF 2 , AlF 3 , NaF, NaPF 6 , K 2 TiF 6 , MnF 2 or a mixture thereof.

12. The method according to claim 5, wherein the firing in step S3 is performed by increasing the temperature to 3 to 15° C. / min and then maintaining the temperature at 800 to 1000° C. for 2 to 5 hours.

13. A member comprising a porous polymer substrate and a coating layer formed on one or both sides of the substrate, A member, wherein the coating layer comprises the coating agent according to claim 1 .

14. 14. The component of claim 13, wherein the component comprises a separator for a secondary battery.

15. The member according to claim 13, wherein the member has a dimensional retention of 50% or more in a thermal stability test using a circular specimen, the dimensional retention being defined by the following Equation 1: (Equation 1) Dimensional retention rate (%) = (d 1 / d 0 ) 2 In the above formula, d 0 is the diameter of the circular specimen before heat treatment, and d 1 is the diameter of the circular specimen after heat treatment at 150° C. for 30 minutes.

16. The member according to claim 13, wherein the member exhibits an air permeability of 200 to 211 sec / 100 cc in a test measuring the time it takes for 100 cc of air to permeate a circular specimen having a diameter of 1 inch.

Citation Information

Patent Citations

  • Alpha-alumina powder and its production

    JP1995206430A

  • POLYHEDRAL alpha-ALUMINA AND ITS MANUFACTURING METHOD

    JP2008127257A

  • Separator for electrochemical element and electrochemical element

    JP2014056843A

  • Dispersant for forming coated layer of multilayer porous film and manufacturing method of multilayer porous film

    JP2016138288A

  • Thermally conductive silicone composition and thermally conductive silicone material

    JP2021075630A