Surface treatment composition for ternary hot-dip zinc alloy plated steel sheet, ternary hot-dip zinc alloy plated steel sheet surface-treated with the same and method for producing the same

A resin-based surface treatment composition for hot-dip zinc alloy coated steel sheets addresses corrosion and blackening issues, offering enhanced resistance and unique colors, while being environmentally friendly and stable.

JP2024538107AActive Publication Date: 2024-10-18POHANG IRON & STEEL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024522325
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-10-14
Publication Date
2024-10-18
Estimated Expiration
2041-10-14

AI Technical Summary

Technical Problem

Existing surface treatment agents for hot-dip zinc alloy coated steel sheets suffer from poor corrosion resistance, blackening resistance, and environmental pollution due to the use of heavy metals like chromium, and lack unique surface color properties suitable for construction materials.

Method used

A surface treatment composition comprising a resin mixture of high molecular weight polysilicon-modified polyurethane base resin, low molecular weight polysilicon-modified polyurethane auxiliary resin, and epoxy auxiliary resin, along with anti-tarnish agents, adhesion promoters, rust and corrosion-resistant agents, colored pigments, and pigment stabilizers, which form a film layer on the steel sheet to enhance corrosion resistance, blackening resistance, and provide unique surface colors.

Benefits of technology

The composition provides excellent corrosion resistance, blackening resistance, alkali resistance, and unique surface color characteristics without using harmful heavy metals, ensuring environmental safety and improved surface gloss, while maintaining solution stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538107000001
    Figure 2024538107000001
  • Figure 2024538107000002
    Figure 2024538107000002
  • Figure 2024538107000003
    Figure 2024538107000003
Patent Text Reader

Abstract

The present invention provides a surface treatment composition capable of imparting excellent corrosion resistance, blackening resistance, alkali resistance and unique surface color properties to ternary hot-dip zinc alloy plated steel sheet. The present invention provides a surface treatment composition comprising, relative to 100% by weight of the solid content of the composition, 70-90% by weight of a resin mixture containing a high molecular weight polysilicon-modified polyurethane main resin, a low molecular weight polysilicon-modified polyurethane auxiliary resin and an epoxy auxiliary resin; 0.5-10% by weight of a discoloration inhibitor; 0.5-10% by weight of an adhesion promoter; 0.5-10% by weight of a rust and corrosion inhibitor; 0.1-2% by weight of a color pigment; and 0.1-1% by weight of a pigment stabilizer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a surface treatment composition for a ternary hot-dip zinc alloy-plated steel sheet, a ternary hot-dip zinc alloy-plated steel sheet surface-treated with the same, and a method for producing the same. [Background technology]

[0002] Generally, steel sheets having a hot-dip zinc alloy plating layer containing magnesium (Mg) and aluminum (Al), which is a steel material with superior corrosion resistance against red rust compared to pure galvanized steel sheets, have most of their exposed surfaces composed of zinc (Zn) or zinc alloy (Zn alloy), and when exposed to general living environments, especially humid atmospheres, the surface develops white rust. In addition, magnesium and aluminum contained in the plating layer have a higher affinity for oxygen than zinc, so blackening is likely to occur when there is a shortage of oxygen to bind to zinc.

[0003] Conventionally, metal surfaces were coated with 5 to 100 mg / m as part of anti-rust treatment. 2 In the past, the pretreatment agent was pretreated with chromate, followed by the formation of an organic film. However, due to the heavy metals contained in the pretreatment agent, such as chromium (Cr), additional pretreatment equipment and processes were required, and the heavy metal wastewater posed a safety issue for workers. In addition, the hexavalent chromium-containing solution generated in the washing water and wastewater must be treated according to a special treatment process, which increases the manufacturing cost, and chromate-treated plated steel sheets also have the problem of eluting chromium ions during use or disposal, which causes serious environmental pollution problems.

[0004] In order to solve these problems while ensuring corrosion resistance, conventional techniques have developed surface treatment agents such as corrosion-resistant metal coating agents that do not contain chromium. For example, Patent Documents 1 and 2 disclose a technique for forming a coating material by containing aluminum biphosphate or by combining tannic acid with sodium acetate, sodium borate, aromatic carboxylic acids such as imidazole, and surfactants, but these have the problem of poor corrosion resistance. Patent Document 3 discloses a surface treatment agent composed of zirconium carbonate, vanadyl ions, zirconium compounds, etc., but although it has good corrosion resistance, it has the problem of being vulnerable to blackening.

[0005] On the other hand, Patent Document 4 discloses a surface treatment agent composed of titanium-based, zirconium-based, phosphoric acid-based, molybdenum-based compounds, etc., but has a problem in that it cannot suppress blackening phenomenon in hot-dip zinc alloy-plated steel sheets using magnesium (Mg), aluminum (Al), etc. Patent Document 5 discloses a surface treatment agent composed of ammonium molybdate, water-dispersed urethane resin, isopropylamine, ammonium zirconium carbonate, epoxy-based silane coupling agent, and silica sol, but has a problem in that it cannot impart sufficient corrosion resistance.

[0006] Meanwhile, in order to use steel materials as building materials, the surface characteristics must be beautiful, and it is necessary to impart a unique color to the steel material so that the surface of the steel material can be distinguished from existing hot-dip galvanized steel materials and hot-dip zinc alloy plated steel materials when customers use the steel material. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 53-28857 [Patent Document 2] Japanese Patent Application Publication No. 51-71233 [Patent Document 3] JP 2002-332574 A [Patent Document 4] Japanese Patent Application Publication No. 7-096699 [Patent Document 5] JP 2005-146340 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been devised in view of the above-mentioned circumstances, and aims to provide a surface treatment composition which can impart excellent corrosion resistance, blackening resistance, alkali resistance and unique surface color characteristics to ternary hot-dip zinc alloy plated steel sheets used as building materials.

[0009] Another object of the present invention is to provide a surface treatment composition which has excellent pigment dispersion stability, does not cause precipitation or aggregation even when used after long-term storage, and can impart excellent corrosion resistance and discoloration resistance, particularly to hot-dip zinc alloy-plated steel sheets under high-temperature and high-humidity environments.

[0010] Another object of the present invention is to provide a surface treatment composition which is completely free of heavy metal components such as chromium, which are environmental pollutants, and is therefore harmless to the human body and does not cause problems due to environmental pollution.

[0011] Another object of the present invention is to provide a hot-dip zinc alloy plated steel sheet having excellent corrosion resistance, blackening resistance, alkali resistance and unique surface color characteristics, and a manufacturing method thereof. [Means for solving the problem]

[0012] According to one embodiment of the present invention, there is provided a surface treatment composition comprising, relative to 100% by weight of the solids content of the composition, 70 to 90% by weight of a resin mixture containing a high molecular weight polysilicon-modified polyurethane main resin, a low molecular weight polysilicon-modified polyurethane auxiliary resin, and an epoxy auxiliary resin; 0.5 to 10% by weight of a discoloration inhibitor; 0.5 to 10% by weight of an adhesion promoter; 0.5 to 10% by weight of a rust and corrosion inhibitor; 0.1 to 2% by weight of a coloring pigment; and 0.1 to 1% by weight of a pigment stabilizer.

[0013] According to one embodiment of the present invention, there is provided a surface-treated ternary hot-dip zinc alloy plated steel sheet, comprising: a steel sheet; a ternary hot-dip zinc alloy plating layer formed on at least one surface of the steel sheet; and a surface treatment film layer formed on the ternary hot-dip zinc alloy plating layer, wherein the surface treatment film layer is formed from the surface treatment composition.

[0014] According to one embodiment of the present invention, there is provided a method for producing a surface-treated ternary hot-dip zinc alloy-plated steel sheet, the method including: coating the surface treatment composition on a ternary hot-dip zinc alloy-plated steel sheet having a ternary hot-dip zinc alloy plating layer formed thereon; and drying the surface treatment composition to form a surface treatment film layer. Effect of the Invention

[0015] The surface treatment composition according to the present invention is coated on a hot-dip zinc alloy-plated steel sheet to form a surface treatment film layer, thereby providing a hot-dip zinc alloy-plated steel sheet having excellent corrosion resistance, blackening resistance, alkali resistance and unique surface color characteristics.

[0016] In addition, the surface treatment composition according to the present invention has excellent pigment dispersion stability, does not cause precipitation or aggregation even when used after long-term storage, and can impart excellent surface gloss to hot-dip zinc alloy plated steel sheets.

[0017] Furthermore, since the surface treatment composition according to the present invention does not contain any heavy metal components such as chromium, which are environmental pollutants, it is harmless to the human body and does not cause problems due to environmental pollution. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, preferred embodiments of the present invention will be described. However, the present invention can be modified in various other forms, and the scope of the present invention is not limited to the following embodiments.

[0019] The present invention relates to a surface treatment composition for ternary hot-dip zinc alloy plated steel sheets, which has excellent solution stability, and when applied to ternary hot-dip zinc alloy plated steel sheets, has excellent flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, alkali resistance, and excellent surface properties. The present invention also relates to a ternary hot-dip zinc alloy plated steel sheet surface-treated with the surface treatment composition, and a method for producing the same.

[0020] A surface treatment composition according to one embodiment of the present invention can contain, relative to 100% by weight of the solids content of the composition, 70 to 90% by weight of a resin mixture containing a high molecular weight polysilicon-modified polyurethane main resin, a low molecular weight polysilicon-modified polyurethane auxiliary resin, and an epoxy auxiliary resin; 0.5 to 10% by weight of a discoloration inhibitor; 0.5 to 10% by weight of an adhesion promoter; 0.5 to 10% by weight of a rust and corrosion inhibitor; 0.1 to 2% by weight of a coloring pigment; and 0.1 to 1% by weight of a pigment stabilizer.

[0021] In one embodiment, the high molecular weight polysilicon modified polyurethane base resin is a component that can impart excellent corrosion resistance, water resistance, and solvent resistance to ternary hot-dip zinc alloy plated steel sheet. The high molecular weight polysilicon modified polyurethane base resin can be synthesized from, but is not limited to, a silicone polymer and a polycarbonate polyol, and has self-crosslinking properties by using a trimer isocyanate polymer during synthesis.

[0022] The weight-average molecular weight (Mw) of the high molecular weight polysilicon-modified polyurethane base resin may be 100,000 to 200,000. If the weight-average molecular weight is less than 100,000, it is difficult to ensure sufficient corrosion resistance. On the other hand, if the weight-average molecular weight is more than 200,000, the solution stability decreases, the hardness of the film increases, and the processability may decrease.

[0023] The glass transition temperature (Tg) of the high molecular weight polysilicon modified polyurethane base resin may be -20°C to -10°C. If the glass transition temperature is less than -20°C, it is difficult to ensure sufficient corrosion resistance. On the other hand, if the glass transition temperature is more than -10°C, the solution stability decreases, the hardness of the film increases, and there is a possibility that problems such as reduced processability may occur.

[0024] In one embodiment, the low molecular weight polysilicon-modified polyurethane auxiliary resin is a component that can impart softness to the ternary hot-dip zinc alloy plated steel sheet to improve processability and adhesion.The low molecular weight polysilicon-modified polyurethane auxiliary resin can be synthesized from, but is not limited to, a silicone polymer and a polycarbonate polyol.Unlike the high molecular weight polysilicon-modified polyurethane main resin, the low molecular weight polysilicon-modified polyurethane auxiliary resin does not have self-crosslinking properties.

[0025] The weight-average molecular weight of the low-molecular-weight polysilicon-modified polyurethane auxiliary resin may be 30,000 to 70,000. If the weight-average molecular weight is less than 30,000, it is difficult to ensure sufficient corrosion resistance due to a decrease in the density of the coating. On the other hand, if the weight-average molecular weight is more than 70,000, the effect of imparting softness to the coating is insufficient, which may cause problems such as reduced processability and adhesion.

[0026] The glass transition temperature (Tg) of the low molecular weight polysilicon modified polyurethane auxiliary resin may be -30°C to -20°C. If the glass transition temperature is less than -30°C, it is difficult to ensure sufficient corrosion resistance due to a decrease in density of the coating. On the other hand, if the glass transition temperature is more than -20°C, the effect of imparting soft properties to the coating is insufficient, which may cause problems such as reduced processability and adhesion.

[0027] In one embodiment, the auxiliary epoxy resin is a component for forming a dense coating on a ternary hot-dip zinc alloy plated steel sheet and improving the corrosion resistance of the sheet.

[0028] The epoxide equivalent ratio of the epoxy auxiliary resin may be 450 to 550 g / eq. If the epoxide equivalent ratio is less than 450 g / eq, the effect of improving the density of the coating and the corrosion resistance of the plate is insufficient. On the other hand, if the epoxide equivalent ratio exceeds 550 g / eq, the coating becomes too hard, which may cause a problem of reduced processability.

[0029] The weight average molecular weight (Mw) of the epoxy auxiliary resin may be 450 to 4,000. If the weight average molecular weight (Mw) is less than 450, the effect of improving the density of the coating and the corrosion resistance of the plate is insufficient. On the other hand, if the weight average molecular weight (Mw) is more than 4,000, the coating becomes too hard, which may cause a problem of reduced processability.

[0030] The resin mixture may be a mixture of high molecular weight polysilicon modified polyurethane main resin: low molecular weight polysilicon modified polyurethane auxiliary resin: epoxy auxiliary resin in a weight ratio of 1:4.5:4.5-9:0.5:0.5, preferably 1:0.5:0.5-9:0.5:0.5, more preferably 2:0.5:0.5-9:0.5:0.5. For example, high molecular weight polysilicon modified polyurethane main resin: low molecular weight polysilicon modified polyurethane auxiliary resin: epoxy auxiliary resin can be mixed and used in a weight ratio of 2:0.5:0.5, more preferably 1:0.5:0.5.

[0031] If the content of the high molecular weight polysilicon-modified polyurethane base resin in the resin mixture is too low, the flat corrosion resistance, processed part corrosion resistance, and alkali resistance of the steel plate may be reduced. On the other hand, if the content of the high molecular weight polysilicon-modified polyurethane base resin in the resin mixture is too high, the processed part corrosion resistance and blackening resistance of the steel plate may be reduced.

[0032] In one embodiment, the content of the resin mixture may be 70 to 90% by weight based on 100% by weight of the solid content of the surface treatment composition. If the content of the resin mixture is less than 70% by weight, it is difficult to ensure sufficient corrosion resistance and alkali resistance, and if the content of the resin mixture is more than 90% by weight, the content of additives for improving the physical properties in the surface treatment composition becomes relatively small, which may cause problems such as reduced corrosion resistance and reduced solution stability.

[0033] In one embodiment, the discoloration inhibitor is a component contained in order to prevent discoloration of the ternary hot-dip zinc alloy plated steel sheet in a high-temperature and high-humidity environment. The discoloration inhibitor may be one or more compounds selected from the group consisting of ammonium molybdate and sodium molybdate.

[0034] The content of the discoloration inhibitor may be 0.5 to 10% by weight based on 100% by weight of the solid content of the surface treatment composition. If the content of the discoloration inhibitor is less than 0.5% by weight, sufficient discoloration resistance cannot be expected, and if the content of the discoloration inhibitor is more than 10% by weight, although the effect of improving discoloration resistance is slight, a problem of reduced corrosion resistance may occur.

[0035] In one embodiment, the adhesion promoter is a component for improving the adhesion between the steel sheet and the resin to prevent peeling of the coating and to prevent moisture from penetrating into the plating layer in a high humidity environment. As the adhesion promoter, one or more selected from the group consisting of ester phosphate, ammonium phosphate, and ammonium zirconium carbonate (AZC) can be used.

[0036] The content of the adhesion promoter may be 0.5 to 10 wt% based on 100 wt% of the solid content of the surface treatment composition. If the content of the adhesion promoter is less than 0.5 wt%, the effect of improving adhesion and preventing moisture penetration may be insufficient, and if the content of the adhesion promoter is more than 10 wt%, the solution stability of the surface treatment composition may decrease.

[0037] In one embodiment, the rust and corrosion inhibitor is a component contained in order to improve the corrosion resistance of the ternary hot-dip zinc alloy plated steel sheet, and may be one or more selected from the group consisting of phosphate-based rust inhibitors, fluorine-based rust inhibitors, vanadium-based rust inhibitors, cerium salt-based rust inhibitors, and selenium salt-based rust inhibitors.

[0038] The content of the rust and corrosion inhibitor may be 0.5 to 10% by weight based on 100% by weight of the solid content of the surface treatment composition. If the content of the rust and corrosion inhibitor is less than 0.5% by weight, it may be difficult to ensure blackening resistance and alkali resistance, and if the content of the rust and corrosion inhibitor is more than 10% by weight, it may be difficult to ensure corrosion resistance.

[0039] In one embodiment, the color pigment is a component for imparting color to the ternary hot-dip zinc alloy plated steel sheet to impart beautiful surface properties. As the color pigment, one or more types selected from the group consisting of one or more inorganic pigments selected from the group consisting of titanium, lead, iron, copper, and chromium; and azo-based organic pigments; can be used.

[0040] The content of the color pigment may be 0.1 to 2% by weight based on 100% by weight of the solid content of the surface treatment composition. If the content of the color pigment is less than 0.1% by weight, it is difficult to achieve sufficient color expression, and if the content of the color pigment is more than 2% by weight, problems such as reduced solution stability and corrosion resistance may occur.

[0041] In one embodiment, the pigment stabilizer is a component for capping the color pigment to uniformly disperse the color pigment in the coating, thereby improving the gloss of the coating. The pigment stabilizer may be, but is not limited to, a carboxyl polymer.

[0042] The content of the pigment stabilizer may be 0.1 to 1 wt% based on 100 wt% of the solid content of the surface treatment composition. If the content of the pigment stabilizer is less than 0.1 wt%, it is difficult to ensure sufficient solution stability, and if the content of the pigment stabilizer is more than 1 wt%, there is a possibility that a problem will arise in that the gloss of the film is rather reduced due to excessive residual components in the film.

[0043] In one embodiment, the surface treatment composition includes water as a solvent to dilute each component, and the water may be deionized water or distilled water. The solvent is included as the balance other than each component of the present invention, and the content thereof may be 60 to 80 wt %. Furthermore, the surface treatment composition according to one embodiment may further include N-Ethyl-2-pyrrolidone (NEP) as an auxiliary solvent to ensure solution stability, and the N-Ethyl-2-pyrrolidone may be included in an amount of 20 to 40 wt % of the total solvent.

[0044] A ternary hot-dip zinc alloy plated steel sheet surface-treated with a surface treatment composition containing a water-soluble organic resin and an inorganic compound according to one embodiment of the present invention has excellent corrosion resistance and blackening resistance as well as excellent surface color and gloss. In addition, the surface treatment composition according to one embodiment of the present invention does not contain hexavalent chromium, which is a harmful environmental substance, and contains water-soluble organic resin and inorganic compound that are harmless to the human body as main components, thereby preventing damage to the human body and environmental pollution problems.

[0045] According to one embodiment of the present invention, there is provided a ternary hot-dip zinc alloy plated steel sheet which has been surface-treated with the above-mentioned surface treatment composition.

[0046] Specifically, the surface-treated ternary hot-dip zinc alloy plated steel sheet may include a steel sheet, a ternary hot-dip zinc alloy plated layer formed on at least one surface of the steel sheet, and a surface treatment coating layer containing an organic resin and an inorganic compound formed on the ternary hot-dip zinc alloy plated layer.

[0047] The base steel sheet and the ternary hot-dip zinc alloy plating layer may include an Al-enriched layer formed at the interface, and the Al-enriched layer may have an area ratio of 70% to 100%. The ternary hot-dip zinc alloy plating layer may include 0.2 to 15% by weight of Al, 0.5 to 3.5% by weight of Mg, and the balance being Zn and unavoidable impurities.

[0048] In one embodiment, the ternary hot-dip zinc alloy plated steel sheet includes an Al-enriched layer formed at the interface between the base iron and the Zn-Al-Mg alloy plated layer, and the occupied area ratio of the Al-enriched layer may be 70% to 100%, more preferably 73% to 100%. Here, the occupied area ratio means the ratio of the area of ​​the Al-enriched layer to the area of ​​the base iron when projected from the surface of the plated steel sheet in the thickness direction of the base iron and assuming a flat surface without considering three-dimensional bending, etc. When the occupied area ratio of the Al-enriched layer is ensured to be 70% or more, the Al-enriched layer has a form in which fine particles are continuously formed, and the platability and plating adhesion can be significantly improved.

[0049] In the ternary hot-dip zinc alloy plated steel sheet according to one embodiment of the present invention, Mg plays an extremely important role in improving the corrosion resistance of the ternary hot-dip zinc alloy plated steel sheet, and effectively prevents the corrosion of the ternary hot-dip zinc alloy plated steel sheet by forming a dense zinc hydroxide-based corrosion product on the surface of the plated layer in a corrosive environment. In the present invention, in order to ensure the intended corrosion resistance effect, the plated layer needs to contain 0.5 wt% or more of Mg, and more preferably, 0.9 wt% or more. However, if the content is excessive, Mg oxidized dross will rapidly increase on the surface of the plated bath, and the oxidation prevention effect of the addition of trace elements will be offset. From the viewpoint of preventing this, the plated layer should contain 3.5 wt% or less of Mg, and more preferably, 3.2 wt% or less of Mg.

[0050] In a ternary hot-dip zinc alloy coated steel sheet according to an embodiment of the present invention, Al suppresses the formation of Mg oxide dross in the coating bath and reacts with Zn and Mg in the coating bath to form a Zn-Al-Mg intermetallic compound, thereby improving the corrosion resistance of the coated steel sheet. To obtain the above effects, the coating layer must contain 0.2 wt% or more of Al, and more preferably, 0.9 wt% or more. However, if the content is excessive, the weldability and phosphating property of the coated steel may deteriorate. From the viewpoint of preventing this, the coating layer should contain 15 wt% or less of Al, and more preferably, 12 wt% or less of Al.

[0051] The surface treatment film layer containing the organic resin and inorganic compound can be formed from a surface treatment composition containing 70-90% by weight of a resin mixture containing a high molecular weight polysilicon-modified polyurethane main resin, a low molecular weight polysilicon-modified polyurethane auxiliary resin and an epoxy auxiliary resin, 0.5-10% by weight of a discoloration inhibitor, 0.5-10% by weight of an adhesion promoter, 0.5-10% by weight of a rust and corrosion inhibitor, 0.1-2% by weight of a color pigment, and 0.1-1% by weight of a pigment stabilizer, based on 100% by weight of the solid content of the composition. The surface treatment composition has the same technical features as those described above, so a redundant description will not be given.

[0052] In one embodiment, the surface treatment film layer is a coating layer formed by drying the above-mentioned surface treatment composition, and corresponds to the components remaining after all the volatile substances contained in the surface treatment film layer containing the organic resin and inorganic compound have evaporated. Therefore, the surface treatment film layer containing the organic resin and inorganic compound does not contain the solvent water or N-ethyl-2-pyrrolidone, and also does not contain the solvent contained in the surface treatment composition containing the organic resin and inorganic compound. Therefore, the components contained in the surface treatment film layer containing the organic resin and inorganic compound correspond to the content based on 100 wt% of the total solid content.

[0053] According to one embodiment of the present invention, there is provided a method for producing a surface-treated ternary hot-dip zinc alloy-plated steel sheet, the method including: coating the above-mentioned surface treatment composition on a ternary hot-dip zinc alloy-plated steel sheet having a ternary hot-dip zinc alloy plating layer formed thereon; and drying the surface treatment composition to form a surface treatment film layer.

[0054] In one embodiment, the surface treatment composition may be coated to a thickness of 2.5 to 50 μm. The coated surface treatment composition may be dried to form a dry coating layer, and the dry coating layer may have a thickness of 1 to 10 μm. If the coating thickness of the surface treatment composition is less than 2.5 μm, the surface treatment composition may be applied too thinly to the convex parts of the steel sheet roughness, which may cause a problem of reduced corrosion resistance, and if the thickness exceeds 50 μm, the coating layer may be formed too thick, which may cause deterioration of workability and economic problems due to increased solution treatment costs.

[0055] The method for coating the surface treatment composition is not particularly limited as long as it is a commonly used coating method. For example, it is preferable to coat the surface treatment composition by any one of a roll coating method, a spray method, a deposition method, a spray squeegee method, and a deposition squeegee method.

[0056] The process of drying the surface treatment composition coated on the ternary hot-dip zinc alloy plated steel sheet is preferably carried out at a temperature of 70 to 250°C based on the PMT of the base steel sheet. If the drying temperature is less than 70°C based on the PMT of the base steel sheet, the curing reaction of the organic resin does not proceed completely, so that a strong film structure is not formed, and corrosion resistance and alkali resistance may be poor. On the other hand, if the drying temperature exceeds 250°C based on the PMT of the base steel sheet, work productivity may decrease due to the generation of water vapor and fumes during the water cooling process, and the surface quality of the product may decrease due to the condensation phenomenon in which evaporated water vapor condenses on the top of the drying equipment.

[0057] Meanwhile, the drying process is preferably carried out in a hot air drying oven or an induction heating oven. When the surface treatment composition is dried using a hot air drying oven, the internal temperature of the hot air drying oven is preferably 100 to 300°C. When the surface treatment composition is dried using an induction heating oven, the current applied to the induction heating oven is preferably 1000 to 5000A, more preferably 1500 to 3500A. When the internal temperature of the hot air drying oven is less than 100°C or the current applied to the induction heating oven is less than 1000A, the curing reaction of the surface treatment composition may not be complete, and the corrosion resistance and alkali resistance may be poor. In addition, when the internal temperature of the hot air drying oven exceeds 300°C or the current applied to the induction heating oven exceeds 5000A, the work productivity may be deteriorated due to the generation of water vapor and fumes during the water cooling process, and the surface quality of the product may be deteriorated due to the condensation phenomenon in which evaporated water vapor is condensed on the upper part of the drying equipment.

[0058] In addition, the surface treatment composition is dried to form a surface treatment film layer, and then the surface treatment film layer is water-cooled to provide a finally surface-treated ternary hot-dip zinc alloy plated steel sheet.

[0059] The method for producing a ternary hot-dip zinc alloy plated steel sheet according to one embodiment of the present invention may be carried out in a continuous process, and the speed of the continuous process is preferably 80 to 120 mpm. If the speed of the continuous process is less than 80 mpm, there is a possibility that a problem of reduced productivity may occur, and if it exceeds 120 mpm, there is a possibility that the solution may be scattered during the process of drying the surface treatment composition, resulting in surface defects. EXAMPLES

[0060] The present invention will be described in detail below with reference to examples. The following examples are provided to help understand the present invention and are not intended to limit the present invention.

[0061] Preparation of test specimens The ternary hot-dip zinc alloy-coated steel sheet (coating amount on one side: 0.5 to 2.0 g / m2) is made of ternary hot-dip zinc alloy coating layer consisting of, by weight, 1.5% Mg, 1.5% Al, and the balance Zn. 2 After cutting the specimens to a size of 7cm x 15cm (horizontal x vertical) and removing the oil, the resulting compositions were applied to hot-dip zinc alloy plated steel sheets using a bar coater. Then, the specimens were cured at a PMT (Peak Metal Temperature (temperature of the substrate surface)) of 180±20°C to prepare test specimens.

[0062] Testing and Evaluation Methods The methods and criteria for evaluating the physical properties of the surface-treated steel sheets in the present examples are as follows.

[0063] <Corrosion resistance of flat plates> After treating the test pieces according to the method specified in ASTM B117, the rate of white rust formation on the steel sheets over time was measured, with the following evaluation criteria:

[0064] ◎: It took more than 144 hours for white rust to appear ○: Time taken for white rust to appear was 96 hours or more but less than 144 hours △: Time taken for white rust to appear was between 55 and 96 hours. X: Time taken for white rust to appear is less than 55 hours

[0065] <Corrosion resistance of processed parts> The test piece was pushed up to a height of 6 mm using an Erichsen tester, and the degree of white rust was measured after 24 hours. The evaluation criteria were as follows:

[0066] ◎: Less than 5% of the area has white rust after 48 hours ○: White rust area after 48 hours is 5% or more and less than 7% X: White rust occurs on 7% or more of the surface area after 48 hours

[0067] <Blackening resistance> The test piece was left in a thermohygrostat maintaining the temperature at 50°C and the relative humidity at 95% for 120 hours, and the color change (color difference: ΔE) of the test piece before and after the test was observed. The evaluation criteria were as follows:

[0068] ◎: ΔE≦2 ○:2<ΔE≦3 △:3<ΔE≦4 X:ΔE>4

[0069] <Alkaline resistance> The test piece was immersed in an alkaline degreasing solution at 60℃ for 2 minutes, then washed with water and air-blowing, after which the color difference (ΔE) before and after was measured. The alkaline degreasing solution used was Finecleaner L 4460 A: 20g / 2.4L + L 4460 B 12g / 2.4L (pH=12) from Daehan Parkerizing Co., Ltd. The evaluation criteria were as follows:

[0070] ◎: ΔE≦2 ○:2<ΔE≦3 △:3<ΔE≦4 X:ΔE>4

[0071] <Solution stability> The surface treatment composition was placed in a container and placed in a thermostatic oven at 50° C. for 7 days, after which the occurrence of precipitation was visually observed and the change in viscosity was measured. The evaluation criteria were as follows:

[0072] ○: No precipitation, viscosity change less than 1 cP △: No precipitation, viscosity change is 1cP or more but less than 5cP X: Precipitation occurs or viscosity change is 5cP or more

[0073] <Glossiness> The gloss of the test piece was measured at an incident angle of 60° using a gloss meter, and the evaluation criteria were as follows:

[0074] ○: Good, gloss value 80 or more X: Poor, gloss value less than 80

[0075] Components of the surface treatment composition The components of the surface treatment compositions used in the examples are as follows:

[0076] - High molecular weight polysilicon modified polyurethane base resin: polyurethane resin with a weight average molecular weight of 150,000 - Low molecular weight polysilicon modified polyurethane auxiliary resin (auxiliary resin 1): polyurethane resin with a weight average molecular weight of 50,000 - Epoxy auxiliary resin (auxiliary resin 2): Epoxy resin with an equivalent ratio of 500g / eq and a weight average molecular weight of 2,000 - Anti-tarnish agent: Ammonium molybdate - Adhesion promoter: Ammonium zirconium carbonate - Anti-rust and anti-corrosion agent: Fluorine-based anti-rust agent - Color pigment: Azo organic pigment - Pigment stabilizer: Carboxyl polymer - Solvent: A mixture of water and N-Ethyl-2-pyrrolidone (NEP)

[0077] Example 1: Changes in physical properties depending on resin mixture content A surface treatment composition was prepared by mixing the above-mentioned main resin, auxiliary resin 1, and auxiliary resin 2 in a weight ratio of 1:0.5:0.5, a discoloration inhibitor, an adhesion promoter, a rust and corrosion inhibitor, a color pigment, and a pigment stabilizer in the amounts shown in Table 1. The surface treatment composition contains a mixed solvent of 49 wt % water and 21 wt % N-ethyl-2-pyrrolidone (70 wt % based on the total weight of the composition).

[0078] The solution stability of the surface treatment composition prepared above was evaluated. In addition, after the surface treatment composition was applied to the above-mentioned test specimen, the flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and alkali resistance of the test specimen were evaluated. The evaluation results are shown in Table 1 below.

[0079] [Table 1]

[0080] Referring to Table 1 above, inventive examples 1 to 3, in which the resin mixture content satisfies the content proposed by the present invention, showed good (◯) or better results in all physical properties. However, comparative example 1, which contained an excessively small amount of resin mixture, showed poor results in flat plate corrosion resistance, processed part corrosion resistance, and alkali resistance, and comparative example 2, which contained an excessively large amount of resin mixture, showed poor results in flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and solution stability.

[0081] Example 2: Changes in physical properties depending on the content ratio of main resin and auxiliary resin A surface treatment composition was prepared containing 80% by weight of a resin mixture containing the above-mentioned main resin, auxiliary resin 1, and auxiliary resin 2, 5% by weight of a discoloration inhibitor, 5.5% by weight of an adhesion promoter, 8% by weight of a rust and corrosion inhibitor, 1% by weight of a color pigment, and 0.5% by weight of a pigment stabilizer. The surface treatment composition contains a mixed solvent of 49% by weight of water and 21% by weight of N-ethyl-2-pyrrolidone (70% by weight based on the total weight of the composition).

[0082] In the above resin mixture, the main resin, auxiliary resin 1, and auxiliary resin 2 were mixed in the weight ratio shown in Table 2 below.

[0083] After the above surface treatment composition was applied to the above-mentioned test specimen, the flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and alkali resistance of the test specimen were evaluated, and the evaluation results are shown in Table 2 below.

[0084] [Table 2]

[0085] Referring to Table 2, inventive examples 4 to 7, in which the weight ratio of the main resin to the auxiliary resin satisfies the content ratio proposed by the present invention, all physical properties were good (◯) or better. On the other hand, comparative example 3, which contained an excessively small amount of water-soluble main resin, showed poor results in flat plate corrosion resistance, processed part corrosion resistance, and alkali resistance, and comparative example 4, which contained excessively small amounts of auxiliary resin 1 and auxiliary resin 2, showed poor results in processed part corrosion resistance and blackening resistance.

[0086] Example 3: Changes in physical properties depending on the content of discoloration inhibitor A surface treatment composition was prepared by mixing the above-mentioned main resin, auxiliary resin 1, and auxiliary resin 2 in a weight ratio of 1:0.5:0.5, a discoloration inhibitor, an adhesion promoter, a rust and corrosion inhibitor, a color pigment, and a pigment stabilizer in the amounts shown in Table 3. The surface treatment composition contains a mixed solvent of 49 wt % water and 21 wt % N-ethyl-2-pyrrolidone (70 wt % based on the total weight of the composition).

[0087] The solution stability of the surface treatment composition prepared above was evaluated. In addition, after the surface treatment composition was applied to the above-mentioned test specimen, the flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and alkali resistance of the test specimen were evaluated. The evaluation results are shown in Table 3 below.

[0088] [Table 3]

[0089] Referring to Table 3 above, inventive examples 8 to 10, in which the content of the discoloration inhibitor satisfies the content proposed by the present invention, showed good (◯) or better results in all physical properties. On the other hand, comparative example 5, which contained an excessively small amount of discoloration inhibitor, showed poor results in blackening resistance and alkali resistance, and comparative example 6, which contained an excessively large amount of discoloration inhibitor, showed poor results in plate corrosion resistance, processed part corrosion resistance, and solution stability.

[0090] Example 4: Changes in physical properties depending on the content of adhesion promoter A surface treatment composition was prepared by mixing the above-mentioned main resin, auxiliary resin 1, and auxiliary resin 2 in a weight ratio of 1:0.5:0.5 with a resin mixture, a discoloration inhibitor, an adhesion promoter, a rust and corrosion inhibitor, a color pigment, and a pigment stabilizer in the amounts shown in Table 4. The surface treatment composition contains a mixed solvent of 49 wt % water and 21 wt % N-ethyl-2-pyrrolidone (70 wt % based on the total weight of the composition).

[0091] The solution stability of the surface treatment composition prepared above was evaluated. In addition, after the surface treatment composition was applied to the above-mentioned test specimen, the flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and alkali resistance of the test specimen were evaluated. The evaluation results are shown in Table 4 below.

[0092] [Table 4]

[0093] Referring to Table 4, inventive examples 11 to 13, in which the adhesion promoter content satisfies the content proposed by the present invention, showed good (◯) or better results in all physical properties. However, comparative example 7, which contained an excessively small amount of adhesion promoter, showed poor results in plate corrosion resistance, processed part corrosion resistance, and alkali resistance, and comparative example 8, which contained an excessively large amount of adhesion promoter, showed poor results in solution stability.

[0094] Example 5: Changes in physical properties depending on the content of rust and corrosion inhibitors A surface treatment composition was prepared by mixing the above-mentioned main resin, auxiliary resin 1, and auxiliary resin 2 in a weight ratio of 1:0.5:0.5, a discoloration inhibitor, an adhesion promoter, a rust and corrosion inhibitor, a color pigment, and a pigment stabilizer in the amounts shown in Table 5. The surface treatment composition contains a mixed solvent of 49 wt % water and 21 wt % N-ethyl-2-pyrrolidone (70 wt % based on the total weight of the composition).

[0095] The solution stability of the surface treatment composition prepared above was evaluated. In addition, after the surface treatment composition was applied to the above-mentioned test specimen, the flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, and alkali resistance of the test specimen were evaluated. The evaluation results are shown in Table 5 below.

[0096] [Table 5]

[0097] Referring to Table 5, inventive examples 14 to 16, in which the rust and corrosion inhibitor content satisfies the content proposed by the present invention, showed good (◯) or better results in all physical properties. However, comparative example 9, which contained an excessively small amount of rust and corrosion inhibitor, showed poor results in flat plate corrosion resistance and processed part corrosion resistance, and comparative example 10, which contained an excessively large amount of rust and corrosion inhibitor, showed poor results in blackening resistance and alkali resistance.

[0098] Example 6: Changes in physical properties depending on the content of color pigments A surface treatment composition was prepared by mixing the above-mentioned main resin, auxiliary resin 1, and auxiliary resin 2 in a weight ratio of 1:0.5:0.5 with a resin mixture, a discoloration inhibitor, an adhesion promoter, a rust and corrosion inhibitor, a color pigment, and a pigment stabilizer in the amounts shown in Table 6. The surface treatment composition contains a mixed solvent of 49 wt % water and 21 wt % N-ethyl-2-pyrrolidone (70 wt % based on the total weight of the composition).

[0099] The solution stability of the surface treatment composition produced above was evaluated. In addition, after the surface treatment composition was applied to the above-mentioned test specimen, the test specimen was evaluated for flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, alkali resistance, and degree of surface color development. The degree of surface color development was evaluated by visually observing the test specimen treated with the surface treatment composition, and the degree of color development was classified into good (○) and poor (X). The evaluation results are shown in Table 6 below.

[0100] [Table 6]

[0101] Referring to Table 6, Examples 17 to 19, which contain the color pigment content as proposed by the present invention, showed good (◯) or better results in all physical properties. However, Comparative Example 11, which contains an excessively small amount of color pigment, showed poor results in surface color expression, and Comparative Example 12, which contains an excessively large amount of color pigment, showed poor results in plate corrosion resistance, processed part corrosion resistance, and solution stability.

[0102] Example 7: Changes in physical properties depending on the content of pigment stabilizer A surface treatment composition was prepared by mixing the above-mentioned main resin, auxiliary resin 1, and auxiliary resin 2 in a weight ratio of 1:0.5:0.5 with a resin mixture, a discoloration inhibitor, an adhesion promoter, a rust and corrosion inhibitor, a color pigment, and a pigment stabilizer in the amounts shown in Table 7. The surface treatment composition contains a mixed solvent of 49 wt % water and 21 wt % N-ethyl-2-pyrrolidone (70 wt % based on the total weight of the composition).

[0103] The solution stability of the surface treatment composition prepared above was evaluated. In addition, after the surface treatment composition was applied to the above-mentioned test specimen, the flat plate corrosion resistance, processed part corrosion resistance, blackening resistance, alkali resistance, and gloss of the test specimen were evaluated. The evaluation results are shown in Table 7 below.

[0104] [Table 7]

[0105] Referring to Table 7, Examples 20 to 22, which contain the pigment stabilizer content as proposed by the present invention, showed good (◯) or better results in all physical properties. However, Comparative Example 13, which contains too little pigment stabilizer, showed poor solution stability, and Comparative Example 14, which contains too much pigment stabilizer, showed poor gloss.

[0106] Example 8: Changes in physical properties depending on the thickness of the coating layer and drying temperature The surface treatment composition according to Example 2 was bar-coated on a test specimen, and dried in a hot air drying oven. The thickness of the coating layer and the PMT temperature were controlled as shown in Table 8 below, and the flat corrosion resistance, processed part corrosion resistance, blackening resistance, and alkali resistance of the test specimen were evaluated.

[0107] [Table 8]

[0108] As shown in Table 8 above, inventive examples 23 to 26 in which a coating layer having a thickness of 1 to 10 μm was formed, all physical properties were good (◯) or better. On the other hand, comparative example 15 in which the formed coating was excessively thin showed average (△) results in flat plate corrosion resistance, blackening resistance, and alkali resistance, and showed a poor result in processed part corrosion resistance. On the other hand, comparative example 16 in which an excessively thick coating was formed showed a poor result in processed part corrosion resistance, and did not have improved physical properties compared to inventive example 26, so from an economical point of view, a coating thickness of more than 10 μm is not required. On the other hand, as shown in Table 8 above, inventive examples 27 to 29 in which a coating layer was formed by drying the coating at 70 to 250 ° C. showed good (◯) or better results in all physical properties. On the other hand, comparative example 17 in which the drying temperature was excessively low showed poor results in all physical properties because the coating was not sufficiently dried. On the other hand, Comparative Example 18, in which the drying temperature was excessively high, showed poor resistance to blackening due to fume drops on the steel sheet caused by condensation of water vapor generated on the steel sheet during the air cooling process (water cooling). As described above, the examples of the present invention have been described in detail, but the scope of the present invention is not limited thereto, and it is obvious to a person skilled in the art that various modifications and variations are possible within the scope of the technical idea of ​​the present invention described in the claims.

Claims

1. Based on 100% by weight of the solid content of the composition, 70-90% by weight of a resin mixture containing a high molecular weight polysilicon-modified polyurethane base resin, a low molecular weight polysilicon-modified polyurethane auxiliary resin, and an epoxy auxiliary resin; 0.5 to 10% by weight of anti-tarnish agent; Adhesion promoter 0.5-10% by weight; Rust and corrosion inhibitor 0.5 to 10% by weight; 0.1 to 2% by weight of a color pigment; and A surface treatment composition comprising 0.1 to 1 weight percent of a pigment stabilizer.

2. The surface treatment composition according to claim 1, wherein the high molecular weight polysilicon modified polyurethane main resin, the low molecular weight polysilicon modified polyurethane auxiliary resin and the epoxy auxiliary resin are mixed in a weight ratio of 1:4.5:4.5 to 9:0.5:0.

5.

3. The surface treatment composition according to claim 1, wherein the high molecular weight polysilicon modified polyurethane base resin has a glass transition temperature (Tg) of -20°C to -10°C and a weight average molecular weight (Mw) of 100,000 to 200,000.

4. The surface treatment composition according to claim 1, wherein the low molecular weight polysilicon modified polyurethane auxiliary resin has a glass transition temperature (Tg) of -30°C to -20°C and a weight average molecular weight (Mw) of 30,000 to 70,000.

5. 2. The surface treatment composition of claim 1, wherein the epoxy co-resin has an epoxide equivalent ratio of 450 to 550 g / eq and a weight average molecular weight (Mw) of 450 to 4,000.

6. 2. The surface treatment solution composition according to claim 1, wherein the discoloration inhibitor is at least one selected from the group consisting of ammonium molybdate and sodium molybdate.

7. 2. The surface treatment composition according to claim 1, wherein the adhesion promoter is at least one selected from the group consisting of phosphate esters, ammonium phosphates, and ammonium zirconium carbonate.

8. 2. The surface treatment solution composition according to claim 1, wherein the rust-preventing and corrosion-resistant agent is at least one selected from the group consisting of phosphoric acid-based rust inhibitors, fluorine-based rust inhibitors, vanadium-based rust inhibitors, cerium salt-based rust inhibitors, and selenium salt-based rust inhibitors.

9. 2. The surface treatment composition according to claim 1, wherein the coloring pigment comprises at least one selected from the group consisting of: at least one inorganic pigment selected from the group consisting of titanium, lead, iron, copper, and chromium; and at least one azo-based organic pigment.

10. The surface treatment composition according to claim 1 , wherein the pigment stabilizer is a carboxyl-based polymer.

11. The surface treatment composition further comprises a solvent; 11. The surface treatment composition according to any one of claims 1 to 10, having a solids content of 20 to 40% by weight, the remainder being solvent, based on the total weight of the surface treatment composition.

12. The surface treatment composition according to claim 11, wherein the solvent comprises 20 to 40% by weight of N-ethyl-2-pyrrolidone (NEP) based on the total weight of the solvent, with the balance being water.

13. Steel plate; A ternary hot-dip zinc alloy plating layer formed on at least one surface of the steel sheet; and A surface treatment coating layer is formed on the ternary hot-dip zinc alloy plating layer, A surface-treated ternary hot-dip zinc alloy plated steel sheet, wherein the surface treatment film layer is formed from the surface treatment composition according to any one of claims 1 to 10.

14. The ternary hot-dip zinc alloy plating layer includes an Al-enriched layer formed at the interface, The surface-treated ternary hot-dip zinc alloy plated steel sheet according to claim 13, wherein an occupation area ratio of the Al-enriched layer is 70% to 100%.

15. The ternary hot-dip zinc alloy plated steel sheet according to claim 13, wherein the ternary hot-dip zinc alloy plated layer contains Al: 0.2 to 15 wt %, Mg: 0.5 to 3.5 wt %, the balance being Zn and inevitable impurities.

16. The surface-treated ternary hot-dip zinc alloy plated steel sheet according to claim 13, wherein the surface treatment coating layer has a thickness of 1 μm to 10 μm.

17. A step of coating the surface treatment composition according to any one of claims 1 to 10 on a ternary hot-dip zinc alloy plated steel sheet having a ternary hot-dip zinc alloy plated layer formed thereon; and The method for producing a surface-treated ternary hot-dip zinc alloy plated steel sheet includes a step of drying the surface treatment composition to form a surface treatment film layer.

18. The method for producing a surface-treated ternary hot-dip zinc alloy plated steel sheet according to claim 17, wherein the surface treatment composition is coated to a thickness of 2.5 μm to 50 μm.

19. The method for producing a surface-treated ternary hot-dip zinc alloy plated steel sheet according to claim 17, wherein the surface treatment composition is dried by increasing the temperature to 70 to 250°C in the step of forming the surface treatment film layer.

Citation Information

Patent Citations

  • Waterproof anti-ageing ground paint for roof and preparation method

    CN107216790A

  • Surface-treated metal material

    JP2007038652A

  • Coating agent for metal

    JP2010090367A

  • Surface treatment composition for ternary hot-dip galvannealed steel sheet, providing excellent corrosion resistance and surface color, ternary hot-dip galvannealed steel sheet surface-treated using same, and manufacturing method therefor

    WO2021112392A1

  • Aenmetsukikozaino boseishitajishoriho

    JP1976071233A