ZSM-5 molecular sieve catalyst, its preparation method and its application

JP2024538197A5Active Publication Date: 2024-11-14CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024523449
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-19
Filing Date
2022-10-18
Publication Date
2024-11-14
Estimated Expiration
2042-10-18

AI Technical Summary

Technical Problem

Existing catalysts for olefin catalytic cracking used in producing propylene and ethylene suffer from low selectivity, stability, and rapid deactivation due to factors such as skeletal dealumination, coking, and side reactions, making them unsuitable for long-term industrial use.

Method used

A ZSM-5 molecular sieve catalyst with a specific ratio of skeletal aluminum at the intersection of linear and sinusoidal pore channels and a high silica-alumina ratio, combined with a binder-free structure and controlled pore volume, enhances catalyst stability and selectivity.

Benefits of technology

The catalyst achieves high conversion rates of olefin feedstock with reduced hydrogen transfer index, maintaining activity and selectivity for propylene and ethylene production over extended periods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention relates to a ZSM-5 molecular sieve catalyst, its preparation method and its application, in which the ratio of the amount of framework aluminum at the intersection between the linear pore channels and the sinusoidal pore channels to the amount of framework aluminum in the linear pore channels and the sinusoidal pore channels is 1.4:1-10:1, and the silica-alumina molar ratio SiO 2 / Al 2 O 3 is 80-1500, and the microporous pore volume can account for 70%-92% of the total pore volume. When the catalyst of the present invention is used for producing propylene and ethylene by catalytic cracking of olefins, the catalyst has the characteristics of low reaction hydrogen transfer index, high stability, high conversion of raw olefins, and high selectivity to propylene and ethylene products.
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention

[0001] [Technical field] The present invention relates to the field of catalytic cracking, in particular to a ZSM-5 molecular sieve catalyst and its preparation method, and its application in enhancing the production of propylene and ethylene by olefin catalytic cracking.

[0002] [Background technology] Propylene and ethylene are important basic raw materials in the petrochemical industry. Driven by the rapid growth of demand for polyolefins and their derivatives, the demand for propylene and ethylene has remained strong and has been growing rapidly in recent years. Therefore, they are considered as products with great market potential. C4 and higher mixed olefins are by-products from the FCC units of ethylene plants and refineries, and can usually only be used as low-value-added products such as liquefied gas fuel. Further processing them into propylene and ethylene and making full use of this abundant and valuable olefin resource will undoubtedly contribute greatly to economic and technological development. Olefin-containing raw materials can be converted into ethylene and propylene by olefin catalytic cracking technology. With the continuous innovation and development of development technology, the said olefin catalytic cracking technology has achieved important results, such as increasing the production of propylene and ethylene, greatly improving production efficiency, having a great impact on the development of the petrochemical industry, and helping to promote the subsequent innovation and development of petrochemical production technology. As the core technology of olefin catalytic cracking reaction, catalysts have been widely studied by many scholars with various preparation methods. The research focus is on preparing catalysts with high activity and selectivity, improving the selectivity of molecular sieves by adjusting the acid properties, optimizing and controlling the pore structure of molecular sieves, reducing the formation of by-products and carbon deposits, element modification, loading, and modification method, etc., all of which directly affect the catalyst performance and product distribution.

[0003] Catalysts for olefin cracking using molecular sieves such as hydrogen-type ZSM-5, ZSM-11, or SAPO-34 as active components and inert gas as heat carrier and diluent can greatly contribute to the improvement of various indicators in the reaction. However, the presence of water during the reaction is disadvantageous to the long-term use of the catalyst. Under high-temperature hydrothermal conditions, acidic molecular sieve catalysts usually undergo severe skeletal dealumination, resulting in a rapid decrease in catalytic acid density and irreversible loss of catalytic activity. At the same time, due to the strong acidity of the molecular sieve, side reactions such as olefin oligomerization chain growth, hydrogen transfer and aromatization may occur during the production of propylene and ethylene by olefin cracking, and even coking may occur in the pores of the molecular sieve catalyst, covering the reaction active center and resulting in rapid deactivation of the catalyst. EP0109059A1 describes a method for the preparation of C4-C 12 US6307117 discloses a process for cracking olefins to produce propylene, in which ZSM-5 or ZSM-11 molecular sieves are used as catalysts. 12 It discloses a method for producing propylene and ethylene by cracking olefins, in which the active component of the catalyst used is ZSM-5 molecular sieve containing a group IB metal, without containing protonic acid. The olefin cracking catalysts reported in the above documents all have, to varying degrees, low product selectivity, low catalyst stability, susceptible to coking and deactivation, and inability to operate for long periods, making them difficult to commercialize.

[0004] [Contents of the invention] The technical problem to be solved by the present invention is to provide a ZSM-5 molecular sieve catalyst and its preparation method, and to provide the application of the catalyst to increase the production of propylene and ethylene by olefin catalytic cracking, in the production of propylene and ethylene by olefin catalytic cracking, in response to the problems of poor catalyst stability and low selectivity to propylene and ethylene in the production of propylene and ethylene by olefin catalytic cracking according to the existing technology. When the catalyst of the present invention is used in the production of propylene and ethylene by olefin catalytic cracking, it has the characteristics of low reaction hydrogen transfer index, high stability, high conversion of olefin feedstock, and high selectivity to propylene and ethylene products.

[0005] A first aspect of the present invention provides a ZSM-5 molecular sieve catalyst, wherein the ratio of the amount of framework aluminum located at the intersections of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels is 1.4:1-10:1, and the silica-alumina molar ratio SiO2 / Al2O3 of the ZSM-5 molecular sieve is 80-1500.

[0006] In the above technical solution, the ratio of the amount of framework aluminum located at the intersection of the linear pore flow path and the sinusoidal pore flow path in the catalyst to the amount of framework aluminum inside the linear pore flow path and the sinusoidal pore flow path is preferably 1.4:1 to 4:1, more preferably 1.5:1 to 3:1.

[0007] In the above technical solution, within the range of the ratio of the framework aluminum amount located at the intersection of the straight pore flow path and the sinusoidal pore flow path in the catalyst to the framework aluminum amount inside the straight pore flow path and the sinusoidal pore flow path, the non-limiting value of the specific point can be 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2.0:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.7:1, 2.8:1, 2.9:1, 3.0:1, 3.2:1, 3.5:1, 4.0:1, etc.

[0008] In the above technical solution, the silica-alumina molar ratio SiO2 / Al2O3 of the ZSM-5 molecular sieve in the catalyst is preferably 80-1000, more preferably 96-1000, even more preferably 150-1000, still more preferably 200-1000, and even more preferably 250-1000.

[0009] In the above technical solutions, the microporous pore volume preferably accounts for 70%-92%, more preferably 75%-90%, even more preferably 80%-90% of the total pore volume in the catalyst.

[0010] In the above technical solutions, non-limiting characteristic values ​​of the ratio of microporous pore volume to total pore volume can be 70%, 72%, 73%, 74%, 76%, 78%, 80%, 82%, 84%, 86%, 88%, 90%, 92%, etc.

[0011] In the above technical solution, the total pore volume of the catalyst is preferably 0.01 mL / g to 1.2 mL / g, more preferably 0.1 mL / g to 0.8 mL / g.

[0012] In the above technical solution, the ZSM-5 molecular sieve catalyst preferably comprises the following components in parts by weight: a) 90 parts to 100 parts, preferably 92 parts to 99 parts, of hydrogen-form ZSM-5 molecular sieve; b) 0 to 5 parts, preferably 0.5 to 3.0 parts, of a rare earth element; and c) 0 to 5 parts, preferably 0.5 to 5.0 parts of an alkaline earth metal element.

[0013] In the above technical solution, the silica-alumina molar ratio SiO2 / Al2O3 of the hydrogen type ZSM-5 molecular sieve is preferably 80-1500, more preferably 80-1000, even more preferably 96-1000, still more preferably 150-1000, even more preferably 200-1000, and even more preferably 250-1000.

[0014] In the above technical solution, the rare earth element is preferably at least one selected from La, Ce, Pr and Nd.

[0015] In the above technical solution, the alkaline earth metal element is preferably at least one selected from Mg, Ca, Sr and Ba.

[0016] In the above technical solution, the weight content of the binder in the ZSM-5 molecular sieve catalyst is preferably 5% or less, more preferably 2% or less, and even more preferably 0.5% or less, based on the weight of the catalyst. Furthermore, the ZSM-5 molecular sieve catalyst is preferably a binder-free ZSM-5 molecular sieve catalyst.

[0017] In the above technical solution, the ZSM-5 molecular sieve catalyst is preferably an olefin catalytic cracking catalyst.

[0018] A second aspect of the present invention provides a process for preparing the above ZSM-5 molecular sieve catalyst, comprising the steps of: (1) preparing a ZSM-5 molecular sieve raw material powder; (2) mixing the molecular sieve raw material powder obtained in step (1) with a molding binder, kneading, and drying to form a catalyst precursor; (3) subjecting the catalyst precursor obtained in step (2) to a third hydrothermal crystallization in the presence of a third template agent to perform ammonium exchange to obtain the ZSM-5 molecular sieve catalyst.

[0019] The above technical solution optionally includes step (4): supporting rare earth metals and / or alkaline earth metals on the ZSM-5 molecular sieve obtained in step (3) to obtain a metal-containing ZSM-5 molecular sieve catalyst.

[0020] In the above technical solution, the method for preparing ZSM-5 molecular sieve raw material powder in step (1) preferably includes: (1.1) mixing a first template agent, a first aluminum source, a silicon source, and a first alkali source with water to perform a first hydrothermal crystallization; (1.2) mixing a second aluminum source, a second template agent, and a second alkali source with the mixture obtained after the crystallization in step (1.1) to obtain the ZSM-5 molecular sieve raw material powder after a second hydrothermal crystallization.

[0021] In the above technical solution, the first template agent in step (1.1) is preferably at least one of tetrapropylammonium bromide, tetrapropylammonium hydroxide, tetraethylammonium chloride, and aqueous ammonia; the first aluminum source is preferably at least one of aluminum nitrate, aluminum sulfate, and aluminum phosphate; the silicon source is preferably at least one of water glass, tetraethyl orthosilicate, and silica sol; the first alkali source is preferably at least one of sodium hydroxide and potassium hydroxide. The first hydrothermal crystallization can be carried out in a stainless steel autoclave under autogenous pressure. The water is preferably deionized water. The conditions of the first hydrothermal crystallization are preferably a crystallization temperature of 80°C to 150°C, and a crystallization time of 2 hours to 10 hours. In step (1.1), NH4 + a first template agent based on Al2O3, a first aluminum source based on SiO2, a silicon source based on OH - The molar ratio of the first alkaline source based on NH4 + :Al2O3:SiO2:OH -:H2O=0.2-0.3:0.0005-0.008:1:0.2-0.4:15-20, preferably 0.2-0.3:0.0005-0.001:1:0.2-0.4:15-20.

[0022] In the above technical solution, the second aluminum source in step (1.2) is preferably at least one of potassium aluminum sulfate and sodium metaaluminate. The potassium aluminum sulfate can be a hydrate, such as potassium aluminum sulfate dodecahydrate. The second template agent is preferably at least one of n-butylamine, hexanediamine, and pyridine. The second alkali source is preferably at least one of sodium hydroxide and potassium hydroxide. The molar ratio of the silicon source added in step (1.1) to the total amount of the second aluminum source added in step (1.2) and the first aluminum source added in step (1.1) is preferably 80-1500, more preferably 80-1000, based on SiO2 / Al2O3. The amount of the second aluminum source based on Al2O3 added in step (1.2) preferably accounts for at least 30%, more preferably at least 40%, of the combined weight of the second aluminum source based on Al2O3 in step (1.2) and the first aluminum source based on Al2O3 in step (1.1).

[0023] In the above technical solution, the molar ratio of the second template agent to the second aluminum source in step (1.2) is + / Al2O3, preferably 200-500:1. The second alkali source is used to control the pH value of the system, preferably 8-10. The conditions of the second hydrothermal crystallization are preferably a crystallization temperature of 120°C-200°C and a crystallization time of 10 hours-100 hours. The second hydrothermal crystallization can be carried out in a stainless steel autoclave under autogenous pressure.

[0024] In the above technical solution, the product obtained after the second hydrothermal crystallization can be washed, dried and calcined to obtain ZSM-5 molecular sieve raw material powder. Washing can be performed with deionized water. The drying conditions are preferably a drying temperature of 80°C to 100°C and a drying time of 10 hours to 20 hours. The calcination conditions are preferably a calcination temperature of 500°C to 650°C and a calcination time of 8 hours to 15 hours.

[0025] In step (2) of the above technical solution, the binder is preferably a silicon compound, or a silicon compound and an aluminum compound. The aluminum compound is preferably at least one selected from aluminum oxide and aluminum sol, and the silicon compound is preferably at least one selected from white carbon black and silicon sol. In the binder, the silicon compound is calculated based on silicon dioxide, and the aluminum compound is calculated based on aluminum oxide. The amount of the silicon compound can be 10% by weight to 100% by weight or 50% by weight to 100% by weight. The amount of the binder added is preferably 8% to 45% of the total weight of the molecular sieve raw material powder and the binder, based on the total weight of the aluminum oxide and silicon dioxide, more preferably 10% to 40%. The molding in step (2) can be performed by a conventional molding method such as extrusion molding. In step (2), an appropriate amount of water can be added depending on the molding conditions. The drying conditions are preferably a drying temperature of 80°C to 120°C and a drying time of 5 hours to 10 hours.

[0026] In the above technical solution, the third template agent in step (3) is preferably at least one of aqueous ammonia, ethylamine, ethylenediamine, triethylamine, n-butylamine, hexanediamine, tetrapropylammonium bromide, and tetrapropylammonium hydroxide. The third hydrothermal crystallization is preferably a crystallization carried out by placing the catalyst precursor obtained in step (2) in steam containing the third template agent. The weight ratio of the third template agent to the catalyst precursor is preferably 1-3:1, and the crystallization is preferably carried out at 130°C-200°C for 20 hours-100 hours. The third hydrothermal crystallization is preferably carried out using a gas-solid crystal conversion method (i.e., the catalyst precursor is placed on an intermediate partition net of a crystallization vessel, an aqueous solution containing the third template agent is placed below the intermediate partition net, and water vapor is generated from the aqueous solution containing the third template agent below under crystallization conditions to perform a crystal conversion treatment on the catalyst precursor). The third hydrothermal crystallization can be carried out under self-generated pressure in a stainless steel autoclave. The weight ratio of the third template agent to water in the aqueous solution of the third template agent is preferably 1-2:1.

[0027] In the above technical solution, the product obtained from the third hydrothermal crystallization can be washed, dried and calcined. The drying conditions are preferably a drying temperature of 80°C to 100°C and a drying time of 10 to 20 hours. The calcination conditions are preferably a calcination temperature of 450°C to 600°C and a calcination time of 5 to 10 hours.

[0028] In the above technical solution, the ammonium exchange in step (3) is preferably carried out by placing the product obtained from the crystallization of the catalyst precursor in an aqueous ammonium salt solution for ammonium exchange, washing, and drying. The ammonium salt is preferably one or more selected from the group consisting of ammonium chloride, ammonium nitrate, and ammonium sulfate. The weight content of the ammonium salt in the aqueous ammonium salt solution is preferably 5% to 10%. The ammonium exchange temperature is preferably 80°C to 90°C, and the number of ammonium exchanges is 3 to 6 times. The product obtained after the ammonium exchange is calcined, and the calcination conditions are preferably a calcination temperature of 500°C to 600°C and a calcination time of 4 to 8 hours.

[0029] In the above technical solution, step (4) is an optional step determined based on the catalyst configuration. The method of supporting rare earth metals and / or alkaline earth metals may be an impregnation method. Preferably, the catalyst contains rare earth metals and alkaline earth metals, and the supporting step is to first obtain a ZSM-5 molecular sieve supporting rare earth metals, and then obtain a ZSM-5 molecular sieve supporting rare earth metals and alkaline earth metals, i.e., a metal-containing ZSM-5 molecular sieve catalyst. The impregnation method is preferably an isochoric impregnation method. The molecular sieve is isochoricly impregnated in a solution containing a rare earth metal salt or a solution containing an alkaline earth metal salt for 3 hours to 10 hours, dried at 60°C to 100°C for 10 hours to 20 hours, and calcined at 450°C to 600°C for 8 hours to 10 hours. The weight concentration of the rare earth metal in the rare earth metal salt solution is 0.2% to 5%. The rare earth element is preferably at least one selected from La, Ce, Pr and Nd, and the weight concentration of the alkaline earth metal in the alkaline earth metal salt solution is preferably 0.2% to 5%. The alkaline earth metal element is preferably at least one selected from Mg, Ca, Sr and Ba.

[0030] The third aspect of the present invention provides the application of the above ZSM-5 molecular sieve catalyst in the production of propylene and ethylene by olefin catalytic cracking, or a method for producing propylene and ethylene by using the above ZSM-5 molecular sieve catalyst in olefin catalytic cracking.

[0031] In the above technical solution, the process for producing propylene and ethylene by olefin catalytic cracking may be a process for contacting an olefin feedstock with the above ZSM-5 molecular sieve catalyst to react and obtain propylene and ethylene products.

[0032] In the above technical solution, it is preferable to use at least one of C4-C6 olefins as the raw material, and the reaction conditions are as follows: reaction temperature 400°C to 600°C, more preferably 420°C to 580°C; reaction pressure 0MPa to 0.3MPa, more preferably 0.01MPa to 0.2MPa; weight hourly space velocity 1 h -1 ~50 hours -1 , more preferably 2 hours -1 ~40 hours -1 , preferably.

[0033] In the above technical solution, propylene and ethylene are produced from the raw material through the catalyst layer, and the reaction hydrogen transfer index is preferably less than 9.6%, more preferably less than 7%; in this specification, the reaction hydrogen transfer index is the yield weight ratio of propane and propylene in the product.

[0034] In the prior art, the process of increasing the production of propylene and ethylene by catalytic cracking of olefins has the problems of low selectivity of propylene and ethylene and low stability of catalyst. This is mainly because the olefin cracking reaction network is complex, including one-molecule cracking, two-molecule cracking and three-molecule cracking. The process includes multiple steps such as olefin isomerization, oligomerization, cracking, dehydrogenation aromatization, hydrogen transfer reaction, alkylation, coking, etc., and the degree of hydrogen transfer reaction is an important factor that affects the remaining side reactions and product selectivity. Ordinary low silica-alumina ratio ZSM-5 molecular sieve has more acidic centers, which leads to increased side reactions, reduced product selectivity, and blocking of the pores of the molecular sieve by by-products after being used in the reaction, resulting in reduced catalytic activity and ultimately deactivation of the catalyst. However, ZSM-5 molecular sieve with a high silica-alumina ratio has fewer active centers and uneven activity distribution, resulting in low reaction activity and poor catalytic stability. The inventors have found through their research that when ZSM-5 molecular sieve catalyst is used for the production of propylene and ethylene by catalytic cracking of olefins, it shows good activity and good selectivity, and also improves stability, when the amount of framework aluminum at the intersection of the straight pore channels and the sinusoidal pore channels is significantly greater than the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels, and the silica-alumina ratio of ZSM-5 molecular sieve catalyst is relatively high. Moreover, the appropriate ratio of microporous pore volume helps to improve the performance.

[0035] Compared with the prior art, the present invention has the following technical advantages: 1. The ZSM-5 molecular sieve catalyst of the present invention has the characteristic that the amount of framework aluminum at the intersection of the linear pore channel and the sinusoidal pore channel is significantly larger than the amount of framework aluminum inside the linear pore channel and the sinusoidal pore channel, and the silica-alumina ratio is relatively high, which greatly improves the utilization rate of the catalytic active center, which makes it easier for the products and intermediates generated at the intersection of the pore channel to diffuse, dramatically reduces the occurrence of side reactions and the formation of carbon deposits, dramatically reduces the reaction hydrogen transfer index, greatly improves the catalytic activity and product selectivity, and further improves the stability.

[0036] 2. During the preparation process of the ZSM-5 molecular sieve catalyst of the present invention, especially during the synthesis process of ZSM-5 molecular sieve raw material powder, different aluminum sources and template agents are added stepwise. The prepared molecular sieve catalyst has a composite pore channel structure, and after the crystal conversion treatment, the obtained catalyst basically does not contain binder. The amount of framework aluminum located at the intersection of the linear pore channel and the sinusoidal pore channel is significantly higher than the amount of framework aluminum located inside the linear pore channel and the sinusoidal pore channel, and when the silica-alumina ratio is relatively high, the catalytic activity and product selectivity are significantly improved, and the stability is further improved. The appropriate proportion of microporous pore volume further improves the performance.

[0037] 3. The method for producing ethylene and propylene by olefin catalytic cracking of the present invention effectively improves the drawbacks of the prior art, such as high reaction hydrogen transfer index, low catalytic activity, and low selectivity to propylene and ethylene. By using the catalyst of the present invention, the reaction hydrogen transfer index can be reduced to 9.6% or less, more preferably 7% or less, the conversion rate of the olefin feedstock is 71% or more, and the selectivity to the target products of propylene and ethylene is more than 68%, preferably more than 80%. Even after 75 hours of reaction, there is no significant change in the activity and selectivity of the catalyst, which shows good stability.

[0038] Description of the drawings FIG. 1 shows the skeletal aluminum of the catalyst obtained in Example 1.27 Al nuclear magnetic resonance spectrum. In FIG. 1, line 1 represents framework aluminum species at the intersection of the linear and sinusoidal pore channels, line 2 represents framework aluminum species inside the linear and sinusoidal pore channels, and line 3 represents the original curve before peak separation; FIG. 2 is the XRD spectrum of the catalyst obtained in Example 1; FIG. 3 shows the skeletal aluminum of the catalyst obtained in Comparative Example 5. 27 Al nuclear magnetic resonance spectrum. In FIG. 3, line 1 represents framework aluminum species at the intersection of the linear and sinusoidal pore channels, line 2 represents framework aluminum species inside the linear and sinusoidal pore channels, and line 3 represents the original curve before peak separation; FIG. 4 shows the XRD spectrum of the catalyst obtained in Comparative Example 5.

[0039] [Specific embodiment] The present invention will now be further described with reference to the following examples.

[0040] In the present invention, the determination of the pore volume is carried out using a TriStar 3000 type physical adsorption apparatus. After vacuum treatment at 300°C for 3 hours, the sample is placed in the test apparatus and liquid nitrogen is added to perform the test. The pore distribution of the sample is calculated using the Barret-Joyner-Helenda (BJH) model.

[0041] In the present invention, 27 The instrument used for the Al nuclear magnetic resonance characterization was a Bruker DSX300 nuclear magnetic resonance instrument. 27 For Al chemical shifts, see Al(H2O)6 in saturated aluminum chloride solution. 3+ The nuclear magnetic spectrum was obtained under the condition of a magic angle spinning rate of 4 kHz. In this case, the framework aluminum located at the intersection of the linear pore channel and the sinusoidal pore channel in the catalyst was 27Al nuclear magnetic resonance spectrum, while framework aluminum within the linear and sinusoidal pore channels corresponds to a chemical shift peak at about 54 ppm (e.g., in the range of 54±0.2 ppm). 27 The ratio of the amount of framework aluminum located at the intersection of the linear pore channels and the sinusoidal pore channels to the amount of framework aluminum located inside the linear pore channels and the sinusoidal pore channels is 27 This is the ratio of the corresponding areas of the spectral peaks near 54 ppm and 56 ppm after peak separation by Al nuclear magnetic resonance spectroscopy.

[0042] In the present invention, the XRD analysis was performed using a graphite monochromator, CuKα radiation, a tube voltage of 40 kV, a tube current of 40 mA, and a scanning speed of 15 min. -1 The diffraction pattern was measured using a Rigaku D / MAX-1400X polycrystalline X-ray diffractometer with a scanning range of 2θ 5° to 50°.

[0043] In the present invention, the silica-alumina molar ratio SiO2 / Al2O3 is calculated by analyzing the elemental composition of a solid sample using a Philips Magix X-type fluorescence spectrometer, the operating voltage of which is 40 kV and the operating current of which is 40 mA.

[0044] In the present invention and comparative examples, at least one of C4-C6 olefins is used as a raw material for producing ethylene and propylene by catalytic cracking, and the hydrogen transfer index is the yield weight ratio of propane and propylene in the product; Conversion rate (%) of olefins from feedstock = (1-weight of olefins in product / weight of olefins in feedstock) x 100%; Selectivity (%) of propylene and ethylene = total weight of propylene and ethylene produced in the product / (weight of olefins in the feed - weight of olefins remaining after reaction) x 100%.

[0045] [Example 1] (1) Preparation of ZSM-5 molecular sieve raw powder Tetrapropylammonium bromide was used as the first template agent, aluminum nitrate as the first aluminum source, silica sol as the silicon source, and sodium hydroxide as the first alkali source. + Tetrapropylammonium bromide based on Al2O3, aluminum nitrate based on Al2O3, silica sol based on SiO2, OH - The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH - The mixture was mixed thoroughly and stirred, then transferred to an autoclave and crystallized at 100°C for 8 hours, then cooled for further use. The second aluminum source, potassium aluminum sulfate dodecahydrate, was added after removing the first aluminum source, so that the molar ratio of the silicon source to the total amount of the first aluminum source and the second aluminum source was 300 based on SiO2 / Al2O3. The second template agent, n-butylamine, was added with NH4 + Based on the SiO2 / Al2O3, the second template agent was added to the second aluminum source in a molar ratio of 200:1, and mixed thoroughly with the above crystallization solution. After adjusting the pH to 10 using sodium hydroxide as the second alkali source, the mixture was transferred to a stainless steel autoclave and subjected to a second hydrothermal crystallization at 120°C for 100 hours. The synthesized product was washed with water, dried at 90°C for 15 hours, and calcined at 600°C for 10 hours to obtain ZSM-5 molecular sieve raw material powder.

[0046] (2) Preparation of catalyst precursor 100 g of the above ZSM-5 molecular sieve raw material powder, 25 g of silica sol containing 40 wt % SiO2, and 0.056 g of aluminum oxide were mixed, kneaded, extruded into a strip shape, and dried at 80°C for 10 hours to obtain a catalyst precursor.

[0047] (3) Preparation of hydrogen-type ZSM-5 molecular sieve Ethylamine was used as the third template agent, and a mixture of 30g of ethylamine and 30g of distilled water was added to the reactor in advance, and 20g of the strip catalyst precursor prepared above was placed on a porous stainless steel net in the reactor, sealed, and subjected to gas-solid phase hydrothermal crystallization at 130°C for 100 hours. After recovery, the product was washed with distilled water, dried at 90°C for 15 hours, and then calcined at 550°C for 10 hours in an air atmosphere.

[0048] Thereafter, the mixture was subjected to ammonium exchange three times in a 5 wt % ammonium nitrate solution at 90° C., dried, and then calcined in a muffle furnace at 500° C. for 4 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0049] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of a praseodymium nitrate solution having a Pr content of 1% by weight for 10 hours, dried at 100° C. for 10 hours, and calcined at 550° C. for 8 hours.

[0050] Finally, the above solid was immersed in 20 g of magnesium nitrate solution with a Mg weight content of 2% for 8 hours, dried at 100° C. for 10 hours, and calcined at 550° C. for 8 hours to obtain the catalyst.

[0051] According to the physical adsorption test, the total pore volume of the catalyst was 0.3 mL / g, and the microporous pore volume accounted for 86% of the total pore volume. According to the aluminum nuclear magnetic resonance measurement, the ratio of the amount of framework aluminum located at the intersection of the linear pore channel and the sinusoidal pore channel to the amount of framework aluminum inside the linear pore channel and the sinusoidal pore channel was 2:1, as shown in Figure 1. The molar ratio of the catalyst SiO2 / Al2O3 was 282. Figure 2 shows the XRD spectrum of the catalyst obtained in Example 1, which was found to be a ZSM-5 molecular sieve catalyst with a binder content of less than 0.2%.

[0052] Using a fixed-bed catalytic reactor, the activity of the prepared catalyst was evaluated for the reaction to produce propylene and ethylene by olefin catalytic cracking using a raffinate mixture C4 (butane 40 wt% and butene 60 wt%) from an ethylene plant as the raw material. The process conditions used for the evaluation were catalyst loading of 5 g, reaction temperature of 500°C, reaction pressure of 0.02 MPa, and weight space velocity of 20 h. -1 The reaction results were a C4 olefin conversion of 75%, a hydrogen transfer index of 6.5%, and a selectivity for propylene and ethylene of 80.8%. The catalyst was reacted for 80 hours, but there was no significant change in activity or selectivity, indicating good stability.

[0053] Example 2 (1) Preparation of ZSM-5 molecular sieve raw powder Tetrapropylammonium hydroxide was used as the first template agent, aluminum nitrate as the first aluminum source, tetraethyl orthosilicate as the silicon source, and sodium hydroxide as the first alkali source. + based on tetrapropylammonium hydroxide, based on Al2O3, based on aluminum nitrate, based on SiO2, based on OH - The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH - The mixture was mixed thoroughly and stirred, then transferred to an autoclave and crystallized at 80°C for 10 hours, then cooled for further use. The second aluminum source, sodium aluminate after removing the first aluminum source, was added so that the molar ratio of silicon source to the total amount of the first aluminum source and the second aluminum source was 1000 based on SiO2 / Al2O3. The second template agent, pyridine, was dissolved in NH4 +Based on the SiO2 / Al2O3, the second template agent was added to the second aluminum source in a molar ratio of 300:1, and thoroughly mixed with the above crystallization solution. After adjusting the pH to 8 using sodium hydroxide as the second alkali source, the mixture was transferred to a stainless steel autoclave and subjected to a second hydrothermal crystallization at 200 °C for 10 hours. The synthesized product was washed with water, dried at 80 °C for 20 hours, and calcined at 500 °C for 15 hours to obtain ZSM-5 molecular sieve raw material powder.

[0054] (2) Preparation of catalyst precursor 100 g of the above ZSM-5 molecular sieve raw material powder, 80 g of white carbon black, and 0.68 g of aluminum sol (containing 20% ​​Al2O3 mass fraction) were mixed with 50 g of water, kneaded, extruded into a strip shape, and dried at 120°C for 5 hours to obtain a catalyst precursor.

[0055] 3) Preparation of hydrogen-type ZSM-5 molecular sieve Hexanediamine was used as the third template agent, and a mixture of 60g of hexanediamine and 30g of distilled water was added to the reactor, and 20g of the strip catalyst precursor prepared above was placed on a porous stainless steel net in the reactor, sealed, and crystallized at 150°C for 80 hours. After recovery, it was washed with distilled water, dried at 100°C for 10 hours, and calcined at 600°C for 5 hours in an air atmosphere.

[0056] Thereafter, the ammonium exchange was performed three times in a 10% ammonium nitrate solution at 80°C, and after drying, the ammonium exchange was performed in a muffle furnace at 550°C for 4 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0057] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of a neodymium nitrate solution having a Nd weight content of 2% for 5 hours, dried at 60° C. for 20 hours, and calcined at 600° C. for 8 hours.

[0058] Finally, the above solid was immersed in 20 g of calcium nitrate solution with a Ca weight content of 0.8% for 10 h, dried at 100 °C, and calcined at 500 °C for 10 h to obtain a catalyst. The XRD spectrum of the obtained catalyst was similar to that in Fig. 2, and it was found to be a ZSM-5 molecular sieve catalyst with a binder content of less than 0.2%.

[0059] Physical adsorption tests showed that the total pore volume of the catalyst was 0.4 mL / g, and the microporous pore volume accounted for 90% of the total pore volume. Aluminum nuclear magnetic resonance measurements showed that the ratio of the amount of framework aluminum located at the intersection of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels was 1.5:1. The molar ratio of the catalyst SiO2 / Al2O3 was 925.

[0060] The catalyst was evaluated in the same manner as in Example 1, and the reaction results were a C4 olefin conversion of 73%, a hydrogen transfer index of 4.8%, and a selectivity for propylene and ethylene of 85.6%. This catalyst was reacted for 78 hours, but there was no significant change in activity and selectivity, indicating good stability.

[0061] Example 3 (1) Preparation of ZSM-5 molecular sieve raw powder Tetrapropylammonium bromide was used as the first template agent, aluminum nitrate as the first aluminum source, silica sol as the silicon source, and sodium hydroxide as the first alkali source. + Tetrapropylammonium bromide based on Al2O3, aluminum nitrate based on Al2O3, silica sol based on SiO2, OH - The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH -The mixture was mixed thoroughly and stirred, then transferred to an autoclave and crystallized at 100°C for 8 hours, then cooled for further use. The second aluminum source, potassium aluminum sulfate dodecahydrate, was added after removing the first aluminum source, so that the molar ratio of the silicon source to the total amount of the first aluminum source and the second aluminum source was 300 based on SiO2 / Al2O3. The second template agent, n-butylamine, was added with NH4 + Based on the SiO2 / Al2O3, the second template agent was added to the second aluminum source in a molar ratio of 200:1, and thoroughly mixed with the above crystallization solution. After adjusting the pH to 10 using sodium hydroxide as the second alkali source, the mixture was transferred to a stainless steel autoclave and subjected to a second hydrothermal crystallization at 120°C for 100 hours. The synthesized product was washed with water, dried at 90°C for 15 hours, and calcined at 600°C for 10 hours to obtain ZSM-5 molecular sieve raw material powder.

[0062] (2) Preparation of catalyst precursor 100 g of the above ZSM-5 molecular sieve raw material powder, 25 g of silica sol containing 40 wt % SiO2, and 0.056 g of aluminum oxide were mixed, kneaded, extruded into a strip shape, and dried at 80°C for 10 hours to obtain a catalyst precursor.

[0063] (3) Preparation of hydrogen-type ZSM-5 molecular sieve Ethylamine was used as the third template agent, and a mixture of 30g of ethylamine and 30g of distilled water was added to the reactor in advance, and 20g of the strip catalyst precursor prepared above was placed on a porous stainless steel net in the reactor, sealed, and subjected to gas-solid phase hydrothermal crystallization for 100 hours at 130°C. After recovery, the product was washed with distilled water, dried at 90°C for 15 hours, and then calcined in an air atmosphere at 550°C for 10 hours.

[0064] Then, it was subjected to ammonium exchange three times in a 5 wt% ammonium nitrate solution at 90°C, dried, and then calcined in a muffle furnace at 500°C for 4 hours to obtain a catalyst. The XRD spectrum of the obtained catalyst was the same as that shown in Figure 2, and it was found to be a ZSM-5 molecular sieve catalyst with a binder content of less than 0.2%.

[0065] Physical adsorption tests showed that the total pore volume of the catalyst was 0.5 mL / g, and the microporous pore volume accounted for 87% of the total pore volume. Aluminum nuclear magnetic resonance measurements showed that the ratio of the amount of framework aluminum located at the intersection of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels was 2:1. The molar ratio of the catalyst SiO2 / Al2O3 was 280.

[0066] The catalyst was evaluated in the same manner as in Example 1, and the reaction results were a C4 olefin conversion of 76%, a hydrogen transfer index of 9.6%, and a selectivity for propylene and ethylene of 68.2%. This catalyst was reacted for 82 hours, but there was no significant change in activity and selectivity, indicating good stability.

[0067] Example 4 (1) Preparation of ZSM-5 molecular sieve raw powder Tetrapropylammonium bromide was used as the first template agent, aluminum nitrate as the first aluminum source, silica sol as the silicon source, and sodium hydroxide as the first alkali source. + Tetrapropylammonium bromide based on Al2O3, aluminum nitrate based on Al2O3, silica sol based on SiO2, OH - The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH -The mixture was mixed thoroughly and stirred, then transferred to an autoclave and crystallized at 100°C for 8 hours, then cooled for further use. The second aluminum source, potassium aluminum sulfate dodecahydrate, was added after removing the first aluminum source, so that the molar ratio of the silicon source to the total amount of the first aluminum source and the second aluminum source was 300 based on SiO2 / Al2O3. The second template agent, n-butylamine, was added with NH4 + Based on the SiO2 / Al2O3, the second template agent was added to the second aluminum source in a molar ratio of 200:1, and thoroughly mixed with the above crystallization solution. After adjusting the pH to 10 using sodium hydroxide as the second alkali source, the mixture was transferred to a stainless steel autoclave and subjected to a second hydrothermal crystallization at 120°C for 100 hours. The synthesized product was washed with water, dried at 90°C for 15 hours, and calcined at 600°C for 10 hours to obtain ZSM-5 molecular sieve powder.

[0068] (2) Preparation of catalyst precursor 100 g of the above ZSM-5 molecular sieve raw material powder, 25 g of silica sol containing 40 wt % SiO2, and 0.056 g of aluminum oxide were mixed, kneaded, extruded into a strip shape, and dried at 80°C for 10 hours to obtain a catalyst precursor.

[0069] (3) Preparation of hydrogen-type ZSM-5 molecular sieve Ethylamine was used as the third template agent, and a mixture of 30g of ethylamine and 30g of distilled water was added to the reactor in advance, and 20g of the strip catalyst precursor prepared above was placed on a porous stainless steel net in the reactor, sealed, and then subjected to gas-solid phase hydrothermal crystallization for 100 hours at 130°C. After recovery, the product was washed with distilled water, dried at 90°C for 15 hours, and then calcined in an air atmosphere at 550°C for 10 hours.

[0070] Thereafter, the mixture was subjected to ammonium exchange three times in a 5 wt % ammonium nitrate solution at 90° C., dried, and then calcined in a muffle furnace at 500° C. for 4 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0071] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of a praseodymium nitrate solution with a Pr weight content of 1% for 10 hours, dried at 100°C for 10 hours, and calcined at 550°C for 8 hours to obtain a catalyst. The XRD spectrum of the obtained catalyst was the same as that shown in Figure 2, and it was found to be a ZSM-5 molecular sieve catalyst with a binder content of less than 0.2%.

[0072] Physical adsorption tests showed that the total pore volume of the catalyst was 0.4 mL / g, and the microporous pore volume accounted for 86% of the total pore volume. Aluminum nuclear magnetic resonance measurements showed that the ratio of the amount of framework aluminum located at the intersection of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels was 2:1. The molar ratio of SiO2 / Al2O3 of the catalyst was 285.

[0073] The catalyst was evaluated in the same manner as in Example 1, and the reaction results were a C4 olefin conversion of 77.3%, a hydrogen transfer index of 8.8%, and a selectivity for propylene and ethylene of 70.2%. The catalyst was reacted for 76 hours, but there was no significant change in activity and selectivity, indicating good stability.

[0074] Example 5 (1) Preparation of ZSM-5 molecular sieve raw powder Tetrapropylammonium bromide was used as the first template agent, aluminum nitrate as the first aluminum source, silica sol as the silicon source, and sodium hydroxide as the first alkali source. + Tetrapropylammonium bromide based on Al2O3, aluminum nitrate based on Al2O3, silica sol based on SiO2, OH - The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH -The mixture was mixed thoroughly and stirred, then transferred to an autoclave and crystallized at 100°C for 8 hours, then cooled for further use. The second aluminum source, potassium aluminum sulfate dodecahydrate, was added after removing the first aluminum source, such that the molar ratio of silicon source to the total amount of the first and second aluminum sources was 300 based on SiO2 / Al2O3. The second template agent, n-butylamine, was added with NH4 + Based on the SiO2 / Al2O3, the second template agent was added to the second aluminum source in a molar ratio of 200:1, and thoroughly mixed with the above crystallization solution. After adjusting the pH to 10 using sodium hydroxide as the second alkali source, the mixture was transferred to a stainless steel autoclave and subjected to a second hydrothermal crystallization at 120°C for 100 hours. The synthesized product was washed with water, dried at 90°C for 15 hours, and calcined at 600°C for 10 hours to obtain ZSM-5 molecular sieve powder.

[0075] (2) Preparation of catalyst precursor 100 g of the above ZSM-5 molecular sieve raw material powder, 25 g of silica sol containing 40 wt % SiO2, and 0.056 g of aluminum oxide were mixed, kneaded, extruded into a strip shape, and dried at 80°C for 10 hours to obtain a catalyst precursor.

[0076] (3) Preparation of hydrogen-type ZSM-5 molecular sieve Ethylamine was used as the third template agent, and a mixture of 30g of ethylamine and 30g of distilled water was added to the autoclave in advance. 20g of the strip catalyst precursor prepared above was placed on a porous stainless steel net in the reactor, sealed, and subjected to gas-solid phase hydrothermal crystallization for 100 hours at 130°C. After recovery, the product was washed with distilled water, dried at 90°C for 15 hours, and then calcined at 550°C for 10 hours in an air atmosphere.

[0077] Thereafter, the mixture was subjected to ammonium exchange three times in a 5 wt % ammonium nitrate solution at 90° C., dried, and then calcined in a muffle furnace at 500° C. for 4 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0078] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of magnesium nitrate solution with a Mg weight content of 2% for 8 hours, dried at 100°C for 10 hours, and calcined at 550°C for 8 hours to obtain a catalyst. The XRD spectrum of the obtained catalyst was the same as that shown in Figure 2, and it was found to be a ZSM-5 molecular sieve catalyst with a binder content of less than 0.2%.

[0079] Physical adsorption tests showed that the total pore volume of the catalyst was 0.6 mL / g, and the microporous pore volume accounted for 83% of the total pore volume. Aluminum nuclear magnetic resonance measurements showed that the ratio of the amount of framework aluminum located at the intersection of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels was 1.8:1. The molar ratio of the catalyst SiO2 / Al2O3 was 282.

[0080] The catalyst was evaluated in the same manner as in Example 1, and the reaction results were a C4 olefin conversion of 75.8%, a hydrogen transfer index of 9.3%, and a selectivity for propylene and ethylene of 69.5%. This catalyst was reacted for 75 hours, but there was no significant change in activity and selectivity, indicating good stability.

[0081] Example 6 (1) Preparation of ZSM-5 molecular sieve raw powder Tetrapropylammonium bromide was used as the first template agent, aluminum sulfate as the first aluminum source, silica sol as the silicon source, and sodium hydroxide as the first alkali source. + based on tetrapropylammonium bromide, aluminum sulfate based on Al2O3, silica sol based on SiO2, OH - The molar ratio of sodium hydroxide based on NH4 +:Al2O3:SiO2:OH - The mixture was mixed thoroughly and stirred, then transferred to an autoclave and crystallized at 150°C for 2 hours, then cooled for further use. After removing the first aluminum source, the second aluminum source, potassium aluminum sulfate, was added such that the molar ratio of the silicon source to the total amount of the first aluminum source and the second aluminum source was 100 based on SiO2 / Al2O3. The second template agent, n-butylamine, was added with NH4 + Based on the SiO2 / Al2O3, the second template agent was added to the second aluminum source in a molar ratio of 500:1, and thoroughly mixed with the above crystallization solution. After adjusting the pH to 10 using sodium hydroxide as the second alkali source, the mixture was transferred to a stainless steel autoclave and subjected to a second hydrothermal crystallization at 150 °C for 40 h. The synthesized product was washed with water, dried at 90 °C for 15 h, and calcined at 600 °C for 10 h to obtain ZSM-5 molecular sieve powder.

[0082] (2) Preparation of catalyst precursor 115 g of the above ZSM-5 molecular sieve raw material powder, 10 g of white carbon black, and 0.85 g of aluminum sol (containing 20% ​​Al2O3 by mass fraction) were mixed with 40 g of water, kneaded, extruded into a strip shape, and dried at 120°C for 5 hours to obtain a catalyst precursor.

[0083] (3) Preparation of hydrogen-type ZSM-5 molecular sieve Hexanediamine was used as the third template agent, and a mixture of 60g of hexanediamine and 30g of distilled water was added to the reactor, and 30g of the strip catalyst precursor prepared above was placed on a porous stainless steel net in the reactor, sealed, and crystallized at 200°C for 20 hours. After recovery, the product was washed with distilled water, dried at 100°C for 10 hours, and then calcined at 450°C for 10 hours in an air atmosphere.

[0084] Thereafter, the ammonium exchange was performed six times in a 5% ammonium sulfate solution at 90°C, and after drying, the ammonium exchange was performed in a muffle furnace at 600°C for 4 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0085] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of a neodymium nitrate solution with a Ce weight content of 0.2% for 3 hours, dried at 100°C for 10 hours, and calcined at 450°C for 10 hours.

[0086] Finally, the above solid was immersed in 20 g of magnesium nitrate solution with Mg weight content of 0.2% for 10 h, dried at 100 °C, and calcined at 500 °C for 10 h to obtain a catalyst. The XRD spectrum of the obtained catalyst was similar to that in Figure 2, and it was found to be a ZSM-5 molecular sieve catalyst with a binder content of less than 0.2%.

[0087] Physical adsorption tests showed that the total pore volume of the catalyst was 0.8 mL / g, and the microporous pore volume accounted for 90% of the total pore volume. Aluminum nuclear magnetic resonance measurements showed that the ratio of the amount of framework aluminum located at the intersection of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels was 3:1. The molar ratio of the catalyst SiO2 / Al2O3 was 98.

[0088] The catalyst was evaluated in the same manner as in Example 1, and the reaction results were a C4 olefin conversion of 76.3%, a hydrogen transfer index of 5.3%, and a selectivity for propylene and ethylene of 84.5%. This catalyst was reacted for 77 hours, but there was no significant change in activity and selectivity, indicating good stability.

[0089] Example 7 (1) Preparation of ZSM-5 molecular sieve powder Tetraethylammonium chloride was used as the first template agent, aluminum phosphate as the first aluminum source, water glass as the silicon source, and sodium hydroxide as the first alkali source. +tetraethylammonium chloride based on Al2O3, aluminum phosphate based on Al2O3, water glass based on SiO2, OH - The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH - The mixture was mixed thoroughly and stirred, then transferred to an autoclave and crystallized at 80°C for 10 hours, then cooled for further use. The second aluminum source, sodium metaaluminate, was added after removing the first aluminum source, such that the molar ratio of silicon source to the total amount of the first aluminum source and the second aluminum source was 100 based on SiO2 / Al2O3. The second template agent, hexanediamine, was added with NH4 + Based on the SiO2 / Al2O3, the second template agent was added to the second aluminum source in a molar ratio of 200:1, and thoroughly mixed with the above crystallization solution. After adjusting the pH to 10 using sodium hydroxide as the second alkali source, the mixture was transferred to a stainless steel autoclave and subjected to a second hydrothermal crystallization at 120°C for 100 hours. The synthesized product was washed with water, dried at 100°C for 10 hours, and calcined at 650°C for 8 hours to obtain ZSM-5 molecular sieve raw material powder.

[0090] (2) Preparation of catalyst precursor 112 g of the above ZSM-5 molecular sieve raw material powder, 40 g of white carbon black, and 3.4 g of aluminum sol (containing 20% ​​Al2O3 mass fraction) were mixed with 60 g of water, kneaded, extruded into a strip shape, and dried at 80°C for 10 hours to obtain a catalyst precursor.

[0091] (3) Preparation of hydrogen-type ZSM-5 molecular sieve Triethylamine was used as the third template agent, and a mixture of 50g triethylamine and 50g distilled water was added to the reactor, and 50g of the strip catalyst precursor prepared above was placed on a porous stainless steel net in the reactor, sealed, and crystallized at 130°C for 100 hours. After recovery, the product was washed with distilled water, dried at 80°C for 20 hours, and then calcined at 500°C for 8 hours in air.

[0092] Thereafter, the mixture was subjected to ammonium exchange four times in a 10% ammonium chloride solution at 80°C, dried, and then calcined in a muffle furnace at 500°C for 8 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0093] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of a lanthanum nitrate solution having a La weight content of 5% for 10 hours, dried at 100°C for 12 hours, and calcined at 500°C for 10 hours.

[0094] Finally, the above solid was immersed in 20 g of barium nitrate solution with a Ba weight content of 0.5% for 10 hours, dried at 100°C, and calcined at 500°C for 10 hours to obtain a catalyst. The XRD spectrum of the obtained catalyst was similar to that shown in Figure 2, and it was found to be a ZSM-5 molecular sieve catalyst with a binder content of less than 0.2%.

[0095] Physical adsorption tests showed that the total pore volume of the catalyst was 0.1 mL / g, and the microporous pore volume accounted for 70% of the total pore volume. Aluminum nuclear magnetic resonance measurements showed that the ratio of the amount of framework aluminum located at the intersection of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels was 2:1. The SiO2 / Al2O3 molar ratio of the catalyst was 96.

[0096] The catalyst was evaluated in the same manner as in Example 1, and the reaction results were a C4 olefin conversion of 71%, a hydrogen transfer index of 5.6%, and a selectivity for propylene and ethylene of 80.3%. This catalyst was reacted for 78 hours, but there was no significant change in activity and selectivity, indicating good stability.

[0097] Example 8 (1) Preparation of ZSM-5 molecular sieve raw powder Ammonia water was used as the first template agent, aluminum nitrate as the first aluminum source, tetraethyl orthosilicate as the silicon source, and sodium hydroxide as the first alkali source. + Ammonia water based on Al2O3, aluminum nitrate based on Al2O3, tetraethyl orthosilicate based on SiO2, OH - The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH - The mixture was mixed thoroughly and stirred, then transferred to an autoclave and crystallized at 80°C for 10 hours, then cooled for further use. The second aluminum source, potassium aluminum sulfate, was added after removing the first aluminum source, such that the molar ratio of silicon source to the total amount of the first and second aluminum sources was 500 based on SiO2 / Al2O3. The second template agent, pyridine, was dissolved in NH4 + Based on the SiO2 / Al2O3, the second template agent was added to the second aluminum source in a molar ratio of 400:1, and thoroughly mixed with the above crystallization solution. After adjusting the pH to 8 using sodium hydroxide as the second alkali source, the mixture was transferred to a stainless steel autoclave and subjected to a second hydrothermal crystallization at 180°C for 20 hours. The synthesized product was washed with water, dried at 90°C for 15 hours, and calcined at 600°C for 10 hours to obtain ZSM-5 molecular sieve raw material powder.

[0098] (2) Preparation of catalyst precursor 150 g of the above ZSM-5 molecular sieve raw material powder, 100 g of white carbon black, and 1.7 g of aluminum sol (containing 20% ​​Al2O3 by mass fraction) were mixed with 50 g of water, kneaded, extruded into a strip shape, and dried at 120°C for 5 hours to obtain a catalyst precursor.

[0099] (3) Preparation of hydrogen-type ZSM-5 molecular sieve Hexanediamine was used as the third template agent, and a mixture of 50g of hexanediamine and 30g of distilled water was added to the reactor, and 20g of the strip catalyst precursor prepared above was placed on a porous stainless steel net in the reactor, sealed, and crystallized at 150°C for 80 hours. After recovery, the product was washed with distilled water, dried at 100°C for 10 hours, and then calcined at 600°C for 5 hours in air.

[0100] This was subjected to ammonium exchange three times in a 10% ammonium nitrate solution at 80°C, dried, and then calcined in a muffle furnace at 550°C for 4 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0101] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of a praseodymium nitrate solution having a Pr content of 1% by weight for 5 hours, dried at 60° C. for 20 hours, and calcined at 600° C. for 8 hours.

[0102] Finally, the above solid was immersed in 20 g of strontium nitrate solution with a Sr weight content of 0.3% for 10 h, dried at 100 °C, and calcined at 500 °C for 10 h to obtain a catalyst. The XRD spectrum of the obtained catalyst was similar to that in Figure 2, and it was found to be a ZSM-5 molecular sieve catalyst with a binder content of less than 0.2%.

[0103] Physical adsorption tests showed that the total pore volume of the catalyst was 0.6 mL / g, and the microporous pore volume accounted for 83% of the total pore volume. Aluminum nuclear magnetic resonance measurements showed that the ratio of the amount of framework aluminum located at the intersection of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels was 1.8:1. The molar ratio of the catalyst SiO2 / Al2O3 was 488.

[0104] The catalyst was evaluated in the same manner as in Example 1, and the reaction results were a C4 olefin conversion of 76.5%, a hydrogen transfer index of 5.1%, and a selectivity for propylene and ethylene of 83.9%. This catalyst was reacted for 80 hours, but there was no significant change in activity and selectivity, indicating good stability.

[0105] Example 9 The catalyst of Example 8 was used, and nitrogen-diluted pentene (volume ratio of nitrogen to pentene: 1:1) was used as the raw material to evaluate the reaction activity of the catalyst prepared for the production of propylene and ethylene by olefin catalytic cracking. The process conditions used in the evaluation were catalyst loading of 5 g, reaction temperature of 580° C., reaction pressure of 0.3 MPa, and weight hourly space velocity of 40 h. -1 The reaction results were a C5 olefin conversion of 80%, a hydrogen transfer index of 5.3%, and a selectivity for propylene and ethylene of 82.8%. The catalyst was reacted for 78 hours, but there was no significant change in activity and selectivity, indicating good stability.

[0106] Example 10 Using the catalyst of Example 8 and nitrogen-diluted hexene (volume ratio of nitrogen to hexene 1:1) as a raw material, the reaction activity of the prepared catalyst for the production of propylene and ethylene by olefin catalytic cracking was evaluated. The process conditions used in the evaluation were catalyst loading of 5 g, reaction temperature of 420° C., reaction pressure of 0.01 MPa, weight space velocity of 2 h -1 The reaction results were a C6 olefin conversion of 72%, a hydrogen transfer index of 6.8%, and a selectivity for propylene and ethylene of 80.3%. The catalyst was reacted for 76 hours, but there was no significant change in activity and selectivity, indicating good stability.

[0107] Comparative Example 1 (1) Preparation of ZSM-5 molecular sieve raw powder Tetrapropylammonium bromide was used as the template agent, aluminum nitrate as the aluminum source, silica sol as the silicon source, and sodium hydroxide as the alkali source. +Tetrapropylammonium bromide based on Al2O3, aluminum nitrate based on Al2O3, silica sol based on SiO2, OH - The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH - The mixture was thoroughly mixed and stirred, then transferred to an autoclave and crystallized at 100°C for 8 hours. The synthesized product was washed with water, dried at 90°C for 15 hours, and calcined at 600°C for 10 hours to obtain ZSM-5 molecular sieve powder.

[0108] (2) Preparation of catalyst precursor 100 g of the above ZSM-5 molecular sieve raw material powder, 25 g of silica sol containing 40 wt % SiO2, and 0.056 g of aluminum oxide were mixed, kneaded, extruded into a strip shape, and dried at 80°C for 10 hours to obtain a catalyst precursor.

[0109] (3) Preparation of hydrogen-type ZSM-5 molecular sieve Ethylamine was used as the third template agent, and a mixture of 30g of ethylamine and 30g of distilled water was added to the reactor in advance, and 20g of the strip catalyst precursor prepared above was placed on a porous stainless steel net in the reactor, sealed, and subjected to gas-solid phase hydrothermal crystallization for 100 hours at 130°C. After recovery, the product was washed with distilled water, dried at 90°C for 15 hours, and then calcined in an air atmosphere at 550°C for 10 hours.

[0110] Thereafter, the mixture was subjected to ammonium exchange three times in a 5 wt % ammonium nitrate solution at 90° C., dried, and then calcined in a muffle furnace at 500° C. for 4 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0111] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of a praseodymium nitrate solution having a Pr content of 1% by weight for 10 hours, dried at 100° C. for 10 hours, and calcined at 550° C. for 8 hours.

[0112] Finally, the above solid was immersed in 20 g of magnesium nitrate solution with a Mg weight content of 2% for 8 hours, dried at 100° C. for 10 hours, and calcined at 550° C. for 8 hours to obtain the catalyst.

[0113] Physical adsorption tests showed that the total pore volume of the catalyst was 0.6 mL / g, and the microporous pore volume accounted for 68% of the total pore volume. Aluminum nuclear magnetic resonance measurements showed that the ratio of the amount of framework aluminum located at the intersection of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels was 1:1. The XRD spectrum was similar to Figure 2, and the binder content in the catalyst was less than 0.2%.

[0114] The catalyst evaluation method was the same as in Example 1, and the reaction results were: C4 olefin conversion 76%, hydrogen transfer index 9.2%, and propylene and ethylene selectivity 69.3%. After 65 hours of catalytic reaction, the catalyst activity and selectivity began to decrease.

[0115] Comparative Example 2 (1) Preparation of ZSM-5 molecular sieve raw powder Tetrapropylammonium bromide was used as the first template agent, aluminum nitrate as the first aluminum source, silica sol as the silicon source, and sodium hydroxide as the first alkali source. + Tetrapropylammonium bromide based on Al2O3, aluminum nitrate based on Al2O3, silica sol based on SiO2, OH - The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH -The mixture was mixed thoroughly and stirred, then transferred to an autoclave and crystallized at 100°C for 8 hours, then cooled for further use. The second aluminum source, aluminum nitrate, was added after removing the first aluminum source, such that the molar ratio of silicon source to the total amount of the first and second aluminum sources was 300 based on SiO2 / Al2O3. The second template agent, n-butylamine, was added with NH4 + Based on the SiO2 / Al2O3, the second template agent was added so that the molar ratio of the aluminum source was 200:1, and then thoroughly mixed with the above crystallization solution. After adjusting the pH to 10 using sodium hydroxide as the second alkali source, the mixture was transferred to a stainless steel autoclave and subjected to a second hydrothermal crystallization at 120°C for 100 hours. The synthesized product was washed with water, dried at 90°C for 15 hours, and calcined at 600°C for 10 hours to obtain ZSM-5 molecular sieve raw material powder.

[0116] (2) Preparation of catalyst precursor 50 g of the above ZSM-5 molecular sieve raw material powder, 25 g of silica sol containing 40 wt % SiO2, and 0.056 g of aluminum oxide were mixed, kneaded, extruded into a strip shape, and dried at 80°C for 10 hours to obtain a catalyst precursor.

[0117] (3) Preparation of hydrogen-type ZSM-5 molecular sieve Ethylamine was used as the third template agent, and a mixture of 30g of ethylamine and 30g of distilled water was added to the reactor in advance, and 20g of the strip catalyst precursor prepared above was placed on a porous stainless steel net in the reactor, sealed, and subjected to gas-solid phase hydrothermal crystallization for 100 hours at 130°C. After recovery, the product was washed with distilled water, dried at 90°C for 15 hours, and then calcined in an air atmosphere at 550°C for 10 hours.

[0118] Thereafter, the mixture was subjected to ammonium exchange three times in a 5 wt % ammonium nitrate solution at 90° C., dried, and then calcined in a muffle furnace at 500° C. for 4 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0119] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of a praseodymium nitrate solution having a Pr content of 1% by weight for 10 hours, dried at 100° C. for 10 hours, and calcined at 550° C. for 8 hours.

[0120] Finally, the above solid was immersed in 20 g of magnesium nitrate solution with a Mg weight content of 2% for 8 hours, dried at 100° C. for 10 hours, and calcined at 550° C. for 8 hours to obtain the catalyst.

[0121] Physical adsorption tests showed that the total pore volume of the catalyst was 0.8 mL / g, and the microporous pore volume accounted for 77% of the total pore volume. Aluminum nuclear magnetic resonance measurements showed that the ratio of the amount of framework aluminum located at the intersection of the linear pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the linear pore channels and the sinusoidal pore channels was 0.8:1. The SiO2 / Al2O3 molar ratio of the catalyst was 280. The XRD spectrum was similar to that in Figure 2, and the binder content in the catalyst was less than 0.2%.

[0122] The catalyst evaluation method was the same as in Example 1, and the reaction results were: C4 olefin conversion 72%, hydrogen transfer index 7.3%, and propylene and ethylene selectivity 75.5%. After 70 hours of catalytic reaction, the catalytic activity and selectivity began to decrease.

[0123] Comparative Example 3 (1) Preparation of ZSM-5 molecular sieve raw powder Tetrapropylammonium bromide was used as the first template agent, aluminum nitrate as the first aluminum source, silica sol as the silicon source, and sodium hydroxide as the first alkali source. + Tetrapropylammonium bromide based on Al2O3, aluminum nitrate based on Al2O3, silica sol based on SiO2, OH - The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH -The mixture was mixed thoroughly and stirred, then transferred to an autoclave and crystallized at 100°C for 8 hours, then cooled for further use. The second aluminum source, potassium aluminum sulfate dodecahydrate, was added after removing the first aluminum source, such that the molar ratio of silicon source to the total amount of the first and second aluminum sources was 300 based on SiO2 / Al2O3. The template agent of tetrapropylammonium bromide was added with NH4 + Based on the SiO2 / Al2O3, the template agent was added to the second aluminum source in a molar ratio of 200:1, and thoroughly mixed with the above crystallization solution. After adjusting the pH to 10 using sodium hydroxide as the second alkali source, the mixture was transferred to a stainless steel autoclave and subjected to a second hydrothermal crystallization at 120°C for 100 hours. The synthesized product was washed with water, dried at 90°C for 15 hours, and calcined at 600°C for 10 hours to obtain ZSM-5 molecular sieve raw material powder.

[0124] (2) Preparation of catalyst precursor 100 g of the above ZSM-5 molecular sieve raw material powder, 25 g of silica sol containing 40 wt % SiO2, and 0.056 g of aluminum oxide were mixed, kneaded, extruded into a strip shape, and dried at 80°C for 10 hours to obtain a catalyst precursor.

[0125] (3) Preparation of hydrogen-type ZSM-5 molecular sieve Ethylamine was used as the third template agent, and a mixture of 30g of ethylamine and 30g of distilled water was added to the reactor in advance, and 20g of the strip catalyst precursor prepared above was placed on a porous stainless steel net in the reactor, sealed, and subjected to gas-solid phase hydrothermal crystallization for 100 hours at 130°C. After recovery, the product was washed with distilled water, dried at 90°C for 15 hours, and then calcined in an air atmosphere at 550°C for 10 hours.

[0126] Thereafter, the mixture was subjected to ammonium exchange three times in a 5 wt % ammonium nitrate solution at 90° C., dried, and then calcined in a muffle furnace at 500° C. for 4 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0127] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of a praseodymium nitrate solution having a Pr content of 1% by weight for 10 hours, dried at 100° C. for 10 hours, and calcined at 550° C. for 8 hours.

[0128] Finally, the above solid was immersed in 20 g of magnesium nitrate solution with 2% Mg weight content for 8 hours, dried at 100°C for 10 hours, and calcined at 550°C for 8 hours to obtain a catalyst. The XRD spectrum of the obtained catalyst was the same as that shown in Figure 2, and it was found to be a ZSM-5 molecular sieve catalyst.

[0129] Physical adsorption tests showed that the total pore volume of the catalyst was 0.28 mL / g, and the microporous pore volume accounted for 73% of the total pore volume. Aluminum nuclear magnetic resonance measurements showed that the ratio of the amount of framework aluminum located at the intersection of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels was 1.2:1. The molar ratio of the catalyst SiO2 / Al2O3 was 285. The XRD was similar to Figure 2, and the binder content in the catalyst was less than 0.2%.

[0130] The catalyst evaluation method was the same as in Example 1, and the reaction results were: C4 olefin conversion 69.8%, hydrogen transfer index 7.2%, and propylene and ethylene selectivity 71.8%. After 72 hours of catalytic reaction, the catalytic activity and selectivity began to decrease.

[0131] Comparative Example 4 (1) Preparation of ZSM-5 molecular sieve raw powder Tetrapropylammonium bromide was used as the first template agent, aluminum nitrate as the first aluminum source, silica sol as the silicon source, and sodium hydroxide as the first alkali source. + Tetrapropylammonium bromide based on Al2O3, aluminum nitrate based on Al2O3, silica sol based on SiO2, OH -The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH - The mixture was mixed thoroughly and stirred, then transferred to an autoclave and crystallized at 100°C for 8 hours, then cooled for further use. The second aluminum source, potassium aluminum sulfate dodecahydrate, was added after removing the first aluminum source, such that the molar ratio of silicon source to the total amount of the first and second aluminum sources was 50 based on SiO2 / Al2O3. The second template agent, n-butylamine, was added with NH4 + Based on the SiO2 / Al2O3, the second template agent was added to the second aluminum source in a molar ratio of 200:1, and thoroughly mixed with the above crystallization solution. After adjusting the pH to 10 using sodium hydroxide as the second alkali source, the mixture was transferred to a stainless steel autoclave and subjected to a second hydrothermal crystallization at 120°C for 100 hours. The synthesized product was washed with water, dried at 90°C for 15 hours, and calcined at 600°C for 10 hours to obtain ZSM-5 molecular sieve raw material powder.

[0132] (2) Preparation of catalyst precursor 100 g of the above ZSM-5 molecular sieve raw material powder, 25 g of silica sol containing 40 wt % SiO2, and 0.056 g of aluminum oxide were mixed, kneaded, extruded into a strip shape, and dried at 80°C for 10 hours to obtain a catalyst precursor.

[0133] (3) Preparation of hydrogen-type ZSM-5 molecular sieve Ethylamine was used as the third template agent, and a mixture of 30g of ethylamine and 30g of distilled water was added to the reactor in advance, and 20g of the strip catalyst precursor prepared above was placed on a porous stainless steel net in the reactor, sealed, and subjected to gas-solid phase hydrothermal crystallization for 100 hours at 130°C. After recovery, the product was washed with distilled water, dried at 90°C for 15 hours, and then calcined in an air atmosphere at 550°C for 10 hours.

[0134] Thereafter, the mixture was subjected to ammonium exchange three times in a 5 wt % ammonium nitrate solution at 90° C., dried, and then calcined in a muffle furnace at 500° C. for 4 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0135] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of a praseodymium nitrate solution having a Pr content of 1% by weight for 10 hours, dried at 100° C. for 10 hours, and calcined at 550° C. for 8 hours.

[0136] Finally, the above solid was immersed in 20 g of magnesium nitrate solution with 2% Mg weight content for 8 hours, dried at 100°C for 10 hours, and calcined at 550°C for 8 hours to obtain a catalyst. The XRD spectrum of the obtained catalyst was the same as that shown in Figure 2, and it was found to be a ZSM-5 molecular sieve catalyst.

[0137] Physical adsorption tests showed that the total pore volume of the catalyst was 0.3 mL / g, and the microporous pore volume accounted for 80% of the total pore volume. Aluminum nuclear magnetic resonance measurements showed that the ratio of the amount of framework aluminum located at the intersection of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels was 1.8:1. The molar ratio of SiO2 / Al2O3 in the catalyst was 47. The XRD was similar to Figure 2, and the binder content in the catalyst was less than 0.2%.

[0138] The catalyst evaluation method was the same as in Example 1, and the reaction results were: C4 olefin conversion 68.6%, hydrogen transfer index 12.3%, and propylene and ethylene selectivity 62.5%. After 72 hours of catalytic reaction, the catalytic activity and selectivity began to decrease.

[0139] Comparative Example 5 (1) Preparation of ZSM-5 molecular sieve raw powder Tetrapropylammonium bromide was used as the first template agent, aluminum nitrate as the first aluminum source, silica sol as the silicon source, and sodium hydroxide as the first alkali source. +Tetrapropylammonium bromide based on Al2O3, aluminum nitrate based on Al2O3, silica sol based on SiO2, OH - The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH - The mixture was mixed thoroughly and stirred, then transferred to an autoclave and crystallized at 100°C for 8 hours, then cooled for further use. The second aluminum source, potassium aluminum sulfate dodecahydrate, was added after removing the first aluminum source, such that the molar ratio of silicon source to the total amount of the first and second aluminum sources was 300 based on SiO2 / Al2O3. The second template agent, n-butylamine, was added with NH4 + Based on the SiO2 / Al2O3, the second template agent was added to the second aluminum source in a molar ratio of 200:1, and thoroughly mixed with the above crystallization solution. After adjusting the pH to 10 using sodium hydroxide as the second alkali source, the mixture was transferred to a stainless steel autoclave and subjected to a second hydrothermal crystallization at 120°C for 100 hours. The synthesized product was washed with water, dried at 90°C for 15 hours, and calcined at 600°C for 10 hours to obtain ZSM-5 molecular sieve raw material powder.

[0140] (2) Preparation of catalyst precursor 100 g of the above ZSM-5 molecular sieve raw material powder, 25 g of silica sol containing 40 wt % SiO2, and 0.056 g of aluminum oxide were mixed, kneaded, extruded into a strip shape, and dried at 80°C for 10 hours to obtain a catalyst precursor.

[0141] (3) Preparation of hydrogen-type ZSM-5 molecular sieve 20 g of the strip catalyst precursor prepared above was calcined at 550° C. for 10 hours in an air atmosphere.

[0142] Thereafter, the mixture was subjected to ammonium exchange three times in a 5 wt % ammonium nitrate solution at 90° C., dried, and then calcined in a muffle furnace at 500° C. for 4 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0143] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of a praseodymium nitrate solution having a Pr content of 1% by weight for 10 hours, dried at 100° C. for 10 hours, and calcined at 550° C. for 8 hours.

[0144] Finally, the solid was immersed in 20 g of magnesium nitrate solution with a Mg weight content of 2% for 8 hours, dried at 100°C for 10 hours, and calcined at 550°C for 8 hours to obtain a catalyst. Figure 4 shows the XRD spectrum of the catalyst obtained in Comparative Example 5, which indicates that the catalyst is a ZSM-5 molecular sieve catalyst with a binder content of 10%.

[0145] According to the physical adsorption test, the total pore volume of the catalyst was 0.1 mL / g, and the microporous pore volume accounted for 68% of the total pore volume. According to the aluminum nuclear magnetic resonance measurement, the ratio of the amount of framework aluminum located at the intersection of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels was 0.8:1, as shown in Figure 3. The molar ratio of SiO2 / Al2O3 of the catalyst was 282.

[0146] The catalyst was evaluated in the same manner as in Example 1, and the reaction results were a C4 conversion of 65%, a hydrogen transfer index of 15.8%, and a selectivity for propylene and ethylene of 58.5%.

[0147] Comparative Example 6 (1) Preparation of ZSM-5 molecular sieve raw powder Tetrapropylammonium bromide was used as the template agent, aluminum nitrate as the aluminum source, silica sol as the silicon source, and sodium hydroxide as the alkali source. + Tetrapropylammonium bromide based on Al2O3, aluminum nitrate based on Al2O3, silica sol based on SiO2, OH -The molar ratio of sodium hydroxide based on NH4 + :Al2O3:SiO2:OH - The mixture was thoroughly mixed and stirred, then transferred to an autoclave and crystallized at 100°C for 8 hours. The synthesized product was washed with water, dried at 90°C for 15 hours, and calcined at 600°C for 10 hours to obtain ZSM-5 molecular sieve raw material powder.

[0148] (2) Preparation of catalyst precursor 100 g of the above ZSM-5 molecular sieve raw material powder, 25 g of silica sol containing 40 wt % SiO2, and 0.056 g of aluminum oxide were mixed, kneaded, extruded into a strip shape, and dried at 80°C for 10 hours to obtain a catalyst precursor.

[0149] (3) Preparation of hydrogen-type ZSM-5 molecular sieve 20 g of the strip catalyst precursor prepared above was calcined at 550° C. for 10 hours in an air atmosphere.

[0150] Thereafter, the mixture was subjected to ammonium exchange three times in a 5 wt % ammonium nitrate solution at 90° C., dried, and then calcined in a muffle furnace at 500° C. for 4 hours to obtain a hydrogen-type ZSM-5 molecular sieve.

[0151] (4) Impregnation of metal components The obtained hydrogen-type ZSM-5 molecular sieve solid was immersed in 20 g of a praseodymium nitrate solution having a Pr content of 1% by weight for 10 hours, dried at 100° C. for 10 hours, and calcined at 550° C. for 8 hours.

[0152] Finally, the above solid was immersed in 20 g of magnesium nitrate solution with Mg weight content of 2% for 8 h, dried at 100 °C for 10 h, and calcined at 550 °C for 8 h to obtain a catalyst. The XRD spectrum of the obtained catalyst was similar to that in Figure 4, and it was found to be a ZSM-5 molecular sieve catalyst with a binder content of 10%.

[0153] Physical adsorption tests showed that the total pore volume of the catalyst was 0.13 mL / g, and the microporous pore volume accounted for 62% of the total pore volume. Aluminum nuclear magnetic resonance measurements showed that the ratio of the amount of framework aluminum located at the intersection of the straight pore channels and the sinusoidal pore channels to the amount of framework aluminum inside the straight pore channels and the sinusoidal pore channels was 0.7:1. The SiO2 / Al2O3 molar ratio of the catalyst was 280.

[0154] The catalyst was evaluated in the same manner as in Example 1, and the reaction results were a C4 conversion of 62.5%, a hydrogen transfer index of 16.9%, and a selectivity for propylene and ethylene of 53.5%.

[0155] As can be seen from Figures 1 and 3, the ZSM-5 molecular sieve catalyst of the present invention has a significantly higher ratio of the amount of framework aluminum located at the intersection of the linear pore channels and the sinusoidal pore channels to the amount of framework aluminum located inside the linear pore channels and the sinusoidal pore channels than conventional catalysts.

[0156] As can be seen from Figures 2 and 4, the crystallinity of the catalyst obtained in Example 1 of the present invention is significantly higher than that of the catalyst obtained in Comparative Example 5, and the ZSM-5 molecular sieve catalyst obtained in Comparative Example 5 contains a large amount of binder component.

[0157] Although the specific embodiments of the present invention have been described in detail above, the present invention is not limited thereto. Within the scope of the technical idea of ​​the present invention, the technical solutions of the present invention may be modified in a simple manner, including the combination of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the contents disclosed in the present invention, and all of them belong to the protection scope of the present invention. [Brief description of the drawings]

[0158] [Figure 1]Figure 1 is the framework aluminum 27Al nuclear magnetic resonance spectrum of the catalyst obtained in Example 1. In Figure 1, line 1 represents framework aluminum species at the intersection of the straight and sinusoidal pore channels, line 2 represents framework aluminum species inside the straight and sinusoidal pore channels, and line 3 represents the original curve before peak separation. [Diagram 2] FIG. 2 is an XRD spectrum of the catalyst obtained in Example 1. [Diagram 3] Figure 3 is the framework aluminum 27Al nuclear magnetic resonance spectrum of the catalyst obtained in Comparative Example 5. In Figure 3, line 1 represents framework aluminum species at the intersection of the straight and sinusoidal pore channels, line 2 represents framework aluminum species inside the straight and sinusoidal pore channels, and line 3 represents the original curve before peak separation. [Figure 4] FIG. 4 shows the XRD spectrum of the catalyst obtained in Comparative Example 5.

Claims

1. The ZSM-5 molecular sieve catalyst has a ratio of the amount of framework aluminum located at the intersection of the linear pore channels and the sinusoidal pore channels to the amount of framework aluminum located inside the linear pore channels and the sinusoidal pore channels of 1.4:1 to 10:1, preferably 1.4:1 to 4:1, more preferably 1.5:1 to 3:1, and the silica-alumina molar ratio SiO 2 / Al 2 O 3 is 80 to 1500, preferably 80 to 1000, more preferably 96 to 1000, even more preferably 150 to 1000, still more preferably 200 to 1000, even more preferably 250 to 1000.

2. Catalyst according to claim 1, characterized in that the microporous pore volume of the catalyst accounts for 70% to 92%, preferably 75% to 90%, more preferably 80% to 90% of the total pore volume.

3. Catalyst according to claim 1 or 2, characterized in that the total pore volume of the catalyst is between 0.01 mL / g and 1.2 mL / g, preferably between 0.1 mL / g and 0.8 mL / g.

4. Catalyst according to claim 1 or 2, characterized in that it comprises the following components in parts by weight: a) 90 to 100 parts, preferably 92 to 99 parts, of hydrogen-form ZSM-5 molecular sieve; b) 0 to 5 parts, preferably 0.5 to 3.0 parts, of a rare earth element; and c) 0 to 5 parts, preferably 0.5 to 5.0 parts, of an alkaline earth metal element.

5. The silica-alumina molar ratio of the hydrogen-type ZSM-5 molecular sieve is SiO 2 / Al 2 O 3 is from 80 to 1500, preferably from 80 to 1000, more preferably from 96 to 1000, even more preferably from 150 to 1000, still more preferably from 200 to 1000, even more preferably from 250 to 1000.

6. 5. The catalyst according to claim 4, wherein the rare earth element is at least one selected from La, Ce, Pr, and Nd; and / or the alkaline earth metal element is at least one selected from Mg, Ca, Sr, and Ba.

7. The catalyst according to claim 1 or 2, wherein the weight content of the binder in the ZSM-5 molecular sieve catalyst is 5% or less, preferably 2% or less, more preferably 0.5% or less, based on the weight of the catalyst, and particularly preferably, the ZSM-5 molecular sieve catalyst does not contain a binder.

8. A method for preparing the ZSM-5 molecular sieve catalyst of claim 1, comprising the following steps (1) to (3): (1) preparing ZSM-5 molecular sieve raw material powder; (2) mixing the molecular sieve raw material powder obtained in step (1) with a molding binder, kneading, and drying to form a catalyst precursor; (3) subjecting the catalyst precursor obtained in step (2) to a third hydrothermal crystallization in the presence of a third template agent to perform ammonium exchange to obtain the ZSM-5 molecular sieve catalyst.

9. The preparation method according to claim 8, further comprising step (4): supporting a rare earth metal and / or an alkaline earth metal on the ZSM-5 molecular sieve obtained in step (3) to obtain a metal-containing ZSM-5 molecular sieve catalyst.

10. The method for preparing the ZSM-5 molecular sieve raw material powder in step (1) according to claim 8, characterized in that it comprises the following steps (1.1) and (1.2): (1.1) mixing a first template agent, a first aluminum source, a silicon source, and a first alkali source with water, and performing a first hydrothermal process; (1.2) A step of mixing a second aluminum source, a second template agent, and a second alkali source with the mixture obtained after the crystallization in step (1.1) to obtain the ZSM-5 molecular sieve raw material powder after a second hydrothermal crystallization.

11. The first template agent in step (1.1) is at least one of tetrapropylammonium bromide, tetrapropylammonium hydroxide, tetraethylammonium chloride, and aqueous ammonia; and / or the first aluminum source in step (1.1) is at least one of aluminum nitrate, aluminum sulfate, and aluminum phosphate; and / or the conditions of the first hydrothermal crystallization in step (1.1) are a crystallization temperature of 80°C to 150°C and a crystallization time of 2 hours to 10 hours; and / or in step (1.1), NH 4 + The first template agent based on Al 2 O 3 the first aluminum source based on SiO 2 The silicon source based on OH - the first alkalinity source based on 2 The molar ratio of water based on NH 4 + :Al 2 O 3 : SiO 2 :OH - : H 2 The method according to claim 10, characterized in that the ratio of the % to the % by weight of the mixture was 0.2-0.3:0.0005-0.008:1:0.2-4:15-20, preferably 0.2-0.3:0.0005-0.001:1:0.2-0.4:15-20.

12. the second aluminum source in step (1.2) is at least one of potassium aluminum sulfate and sodium metaaluminate; and / or Al 2 O 3 The amount of the second aluminum source added in step (1.2) is based on Al 2 O 3 accounts for 30% or more, preferably 40% or more, of the total weight of the second aluminum source in step (1.2) and the first aluminum source in step (1.1); and / or the second template agent in step (1.2) is at least one of n-butylamine, hexanediamine, and pyridine; and / or, in step (1.2), using a second alkali source to control the pH value of the system to between 8 and 10; And / or the preparation method according to claim 10, characterized in that the conditions of the second hydrothermal crystallization are a crystallization temperature of 120°C to 200°C and a crystallization time of 10 hours to 100 hours.

13. The third template agent in step (3) is at least one of aqueous ammonia, ethylamine, ethylenediamine, triethylamine, n-butylamine, hexanediamine, tetrapropylammonium bromide, and tetrapropylammonium hydroxide; and / or the third hydrothermal crystallization is performed by placing the catalyst precursor obtained in step (2) in water vapor containing the third template agent, wherein the weight ratio of the third template agent to the catalyst precursor is 1 to 3:1, and the crystallization is performed at 130°C to 200°C for 20 hours to 200 hours.

14. 10. Use of the catalyst according to claim 1 or the catalyst prepared by the preparation method according to claim 8 in the production of propylene and ethylene by olefin catalytic cracking.

15. An olefin feedstock is contacted with a ZSM-5 molecular sieve catalyst to react and obtain propylene and ethylene products. Preferably, at least one of C4 to C6 olefins is used as the feedstock. The reaction conditions are a reaction temperature of 400°C to 600°C, preferably 420°C to 580°C, a reaction pressure of 0 MPa to 0.3 MPa, preferably 0.01 MPa to 0.2 MPa, and a weight hourly space velocity of 1 hour. -1 ~50 hours -1 , preferably 2 hours -1 ~40 hours -1 15. The use according to claim 14, characterized in that: