Compound, patterning material, semiconductor device, terminal, and patterning method

Organic mixed metal-oxygen cluster compounds enhance patterning material sensitivity and resolution, addressing low sensitivity and high energy issues in semiconductor manufacturing with short wavelength light sources.

JP2024538266AActive Publication Date: 2024-10-18HUAWEI TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024525272
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-31
Filing Date
2022-09-02
Publication Date
2024-10-18
Estimated Expiration
2042-09-02

AI Technical Summary

Technical Problem

Existing patterning materials struggle with low sensitivity and high exposure energy requirements when using light sources with wavelengths below 15 nm, leading to inadequate resolution and edge roughness in semiconductor manufacturing.

Method used

Development of organic mixed metal-oxygen cluster compounds with specific chemical formulas, incorporating metals like Ti, Bi, and Co, and organic ligands with functional groups, enhancing sensitivity and resolution under soft X-ray exposure.

Benefits of technology

The compounds achieve high sensitivity, high etching resistance, and low outgassing, enabling patterns with improved resolution and reduced edge roughness using short wavelength light sources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538266000001_ABST
    Figure 2024538266000001_ABST
Patent Text Reader

Abstract

The present application provides organic mixed metal-oxygen cluster compounds having the general chemical formula: (M1): a (M2) b (M3) c O g (L1) x (L2) y (L3) z where M1 is selected from at least one of Ti, Zr, and Hf; M2 is selected from at least one of Bi, Te, Sn, Pt, Ag, and Au; M3 is selected from at least one of Fe, Ni, Co, and Cu; L1, L2, and L3 are each selected from organic ligands, which can be coordinated to a metal and contain at least one of O, S, Se, N, and P functioning as a coordination atom; a, b, g, x, y, and z are all natural numbers equal to or greater than 1, and c is a natural number equal to or greater than 0. The present application further provides a patterning material containing the organic mixed metal-oxygen cluster compound, a semiconductor device containing the patterning material, a terminal, and a method for patterning a substrate surface. In the method for patterning a substrate surface in the present application, a pattern with small edge roughness can be realized at high resolution using a simple material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to China Patent Application No. 202111281644.9, entitled "Compound, Patterning Material, Semiconductor Device, Terminal, and Patterning Method," filed with the State Intellectual Property Office of China on October 31, 2021, the entire contents of which are incorporated herein by reference.

[0002] The present application relates to an organic mixed metal-oxygen cluster compound, a patterning material containing the organic mixed metal-oxygen cluster compound, and a semiconductor device, terminal, and substrate surface patterning method using the patterning material. [Background technology]

[0003] With the rapid development of integrated circuit industry, especially when the computation power of chips per unit area is improved, in other words, when the key size corresponding to chips is smaller, the development of patterning technology is essential. The patterning process generally includes the following steps: using a predetermined pattern as a template, irradiating a film layer coated on the surface of a substrate through the template, forming an irradiated structure having an irradiated area and a non-irradiated area on the film layer; selectively dissolving and washing the irradiated structure or the non-irradiated structure, the pattern formed by the residual material is the same as the pattern of the template, and the residual patterning material can have etching resistance in the etching step; selectively protecting the substrate from being etched or slowly etched, forming a graph for transferring to the substrate, forming a pattern on the substrate such as a silicon wafer, the pattern being the pattern that was first selectively exposed. Summary of the Invention [Problem to be solved by the invention]

[0004] In advanced processes for realizing graphics using short wavelength (less than 15 nm) light, the light source transmission efficiency of the patterning technology is low, so the patterning material is required to show high sensitivity, and the exposure energy is usually 30 mJ / cm 2 The following are the current patterning material systems, including organic polymer material systems, organic silicon material systems, etc. Organic polymer material systems are traditional patterning materials. Before short wavelengths of less than 15 nm were applied, organic polymer material systems were used. However, as the wavelength of the patterning light source decreases to less than 15 nm, the resolution of the formed pattern needs to be improved. Organic silicon material systems have high resolution and small molecular size. However, silicon has low sensitivity to light sources with wavelengths of less than 15 nm, and extremely high exposure energy is required. [Means for solving the problem]

[0005] In a first aspect of the present embodiment, there is provided an organic mixed metal-oxygen cluster compound, The general chemical formula is: (M1) a (M2) b (M3) c O g (L1) x (L2) y (L3) z where M1 is selected from at least one of Ti, Zr, and Hf; M2 is selected from at least one of Bi, Te, Sn, Pt, Ag, and Au; M3 is selected from at least one of Fe, Ni, Co, and Cu; L1, L2, and L3 are each selected from organic ligands, which can be coordinated to a metal and contain at least one of O, S, Se, N, and P that function as a ligating atom; An organic mixed metal-oxygen cluster compound is provided, wherein a, b, g, x, y and z are all natural numbers greater than or equal to 1, and c is a natural number greater than or equal to 0.

[0006] In this application, under exposure to soft X-rays with wavelengths ranging from 1 nm to 15 nm, the organic mixed metal-oxygen cluster compound has high sensitivity and can be fine-tuned. The organic mixed metal-oxygen cluster compound has metals and organic ligands. The types and ratios of different metals can be adjusted and / or photosensitive functional groups can be introduced into the organic ligands, so that the photosensitivity of the patterning material can be enhanced, the line edge roughness can be improved, and the resolution can be improved from 10 nm to 40 nm.

[0007] In one embodiment of the present application, 2≦a+b+c≦60.

[0008] In one embodiment of the present application, g+x+y+z≦8(a+b+c).

[0009] g+x+y+z≦8(a+b+c) is determined based on the atomic coordination number.

[0010] In one embodiment of the present invention, 5≧b / (a+c)≧0.1.

[0011] In one implementation of the present application, the ratio of a:b:c is 5:9:1.

[0012] In one embodiment of the present application, M1 is Ti, M2 is Bi, and M3 is at least one of Co and Ni.

[0013] In one embodiment of the present application, at least one of L1, L2, and L3 comprises a functional group, and the functional group is selected from at least one of a carboxylic acid, an alcohol, a phenol, a nitrile, an alkyne, an alcoholamine, a pyridine, a pyrazole, an imidazole, a piperazine, and a pyrazine.

[0014] Functional groups are introduced into the organic ligands L1, L2, and L3 to adjust properties such as the solubility of the organic mixed metal-oxygen cluster compounds, which in turn affect the thickness, film layer roughness, resolution, film layer adhesion, and corrosion resistance of the film layers comprising the organic mixed metal-oxygen cluster compounds.

[0015] In one embodiment of the present application, at least one of L1, L2, and L3 comprises a radiation-sensitive functional group, the radiation-sensitive functional group comprising at least one of a double bond, a triple bond, and an epoxypropane.

[0016] The radiation-sensitive functional groups may further enhance the photosensitivity of the organic mixed metal-oxygen cluster compounds, resulting in improved line edge roughness and improved resolution.

[0017] In one embodiment of the present application, one or more of L1 and L2 coexist in the same organic ligand.

[0018] In one embodiment of the present application, at least a portion of the metal ions in the organic mixed metal-oxygen cluster compound are replaced with a radiation sensitive element, the radiation sensitive element including at least one of Na, Mg, Al, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Rb, Sr, Y, Ga, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, Sn, Sb, Te, Cs, Ba, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Pb, Bi, and Po, and the replacing radiation sensitive element is different from the metal element originally contained in the organic mixed metal-oxygen cluster compound.

[0019] The radiation-sensitive element can substitute for the metal element of the organic mixed metal-oxygen cluster compound to increase the photosensitivity of the organic mixed metal-oxygen cluster compound.

[0020] In a second aspect of the present embodiment, there is provided a patterning material comprising an organic mixed metal-oxygen cluster compound, the general chemical formula of which is: (M1) a (M2) b (M3) c Og(L1) x (L2) y (L3) z where: M1 is selected from at least one of Ti, Zr, and Hf; M2 is selected from at least one of Bi, Te, Sn, Pt, Ag, and Au; M3 is selected from at least one of Fe, Ni, Co, and Cu; L1, L2, and L3 are each selected from organic ligands, which directly coordinate to the metal and contain at least one of O, S, Se, N, and P that function as a coordination atom; a, b, g, x, y, and z are all natural numbers greater than or equal to 1, and c is a natural number greater than or equal to 0.

[0021] The organic mixed metal-oxygen cluster compounds are used as the main materials of the patterning materials, which can meet the requirements of high sensitivity, high etching resistance, high resolution, low outgassing (meaning less gas is released in the exposure process), small molecular size, and the material properties can be fine-tuned by using mixed metals.

[0022] In one embodiment of the present application, 2≦a+b+c≦60, g+x+y+z≦8(a+b+c), and 5≧b / (a+c)≧0.1.

[0023] In one embodiment of the present application, the ratio of a:b:c is 5:9:1, M1 is Ti, M2 is Bi, and M3 is at least one of Co and Ni.

[0024] In one embodiment of the present application, at least one of L1, L2, and L3 comprises a functional group, and the functional group is selected from at least one of a carboxylic acid, an alcohol, a phenol, a nitrile, an alkyne, an alcoholamine, a pyridine, a pyrazole, an imidazole, a piperazine, and a pyrazine.

[0025] In one embodiment of the present application, at least one of L1, L2, and L3 comprises a radiation-sensitive functional group, the radiation-sensitive functional group comprising at least one of a double bond, a triple bond, and an epoxypropane.

[0026] In one embodiment of the present application, one or more of L1 and L2 coexist in the same organic ligand.

[0027] In one embodiment of the present application, at least a portion of the metal ions in the organic mixed metal-oxygen cluster compound are replaced by a radiation sensitive element, the radiation sensitive element including at least one of Na, Mg, Al, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Rb, Sr, Y, Ga, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, Sn, Sb, Te, Cs, Ba, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Pb, Bi, and Po, and the radiation sensitive element for replacement is different from the metal element originally contained in the organic mixed metal-oxygen cluster compound.

[0028] In a third aspect of the present embodiment, there is provided a semiconductor device, A substrate; a functional layer disposed on a surface of the substrate, the functional layer comprising a patterning material according to a second aspect of an embodiment of the present application; A semiconductor device having the following structure is provided.

[0029] The functional layer pattern has high resolution and low pattern edge roughness.

[0030] In a fourth aspect of an embodiment of the present application, there is provided a terminal having a housing and a semiconductor device housed in the housing, the semiconductor device having a semiconductor device according to the third aspect of an embodiment of the present application.

[0031] In a fifth aspect of the present embodiment, there is provided a method for patterning a surface of a substrate, comprising the steps of: Providing a substrate; Forming a patterning material layer on a surface of the substrate, the patterning material layer comprising an organic mixed metal-oxygen cluster compound, the organic mixed metal-oxygen cluster compound having a general chemical formula: (M1) a (M2) b (M3) c O g (L1) x (L2) y (L3) z where M1 is selected from at least one of Ti, Zr, and Hf; M2 is selected from at least one of Bi, Te, Sn, Pt, Ag, and Au; M3 is selected from at least one of Fe, Ni, Co, and Cu; L1, L2, and L3 are each selected from organic ligands, and the organic ligands directly coordinate to a metal and contain at least one of O, S, Se, N, and P that function as a coordination atom; a, b, g, x, y, and z are all natural numbers greater than or equal to 1, and c is a natural number greater than or equal to 0; performing a localized exposure to the patterning material layer; removing portions of the patterning material layer using a developer; A method for patterning a substrate surface is provided, comprising:

[0032] The method of patterning a substrate surface herein can provide a patterned layer of patterning material with high resolution and low edge roughness, facilitating processing performed with semiconductor devices.

[0033] In one embodiment of the present application, in the general chemical formula of the organic mixed metal-oxygen cluster compound, 2≦a+b+c≦60, g+x+y+z≦8(a+b+c), and 5≧b / (a+c)≧0.1.

[0034] In one embodiment of the present application, in the general chemical formula of the organic mixed metal-oxygen cluster compound, at least one of L1, L2, and L3 comprises a functional group, and the functional group is selected from at least one of carboxylic acid, alcohol, phenol, nitrile, alkyne, alcoholamine, pyridine, pyrazole, imidazole, piperazine, and pyrazine.

[0035] In one embodiment of the present application, at least one of L1, L2, and L3 comprises a radiation-sensitive functional group, the radiation-sensitive functional group comprising at least one of a double bond, a triple bond, and an epoxypropane.

[0036] In one embodiment of the present application, at least a portion of the metal ions in the organic mixed metal-oxygen cluster compound are replaced by a radiation sensitive element, the radiation sensitive element including at least one of Na, Mg, Al, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Rb, Sr, Y, Ga, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, Sn, Sb, Te, Cs, Ba, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Pb, Bi, and Po, and the radiation sensitive element for replacement is different from the metal element originally contained in the organic mixed metal-oxygen cluster compound.

[0037] In one embodiment of the present application, in the general chemical formula of the organic mixed metal-oxygen cluster compound, the ratio of a:b:c is 5:9:1, M1 is Ti, M2 is Bi, and M3 is at least one of Co and Ni.

[0038] In one embodiment of the present application, the step of performing localized exposure of the patterning material layer uses any single wavelength or mixed wavelength light of soft X-rays in the wavelength range of 1 nm to 15 nm, or uses an electron beam, or uses extreme ultraviolet radiation.

[0039] In one embodiment of the present application, a mask is used in the step of performing localized exposure on the patterning material layer using soft X-rays, and soft X-rays carrying pattern information reach the patterning material layer through the mask, thereby locally exposing the patterning material layer.

[0040] In one embodiment of the present application, the developer is at least one of isopropanol, N,N-dimethylformamide, 2-acetoxy-1-methoxypropane, ethyl lactate, and water.

[0041] In one embodiment of the present application, the method for patterning a substrate surface further comprises etching the substrate using the patterning material film layer remaining on the substrate as a protection layer. [Brief description of the drawings]

[0042] [Figure 1] 1 is a schematic diagram of the patterning process. [Diagram 2] 1 is a diagram illustrating a schematic cross-sectional structure of a semiconductor device according to an embodiment of the present application. [Diagram 3] FIG. 2 is a schematic diagram of the structure of an organic mixed metal-oxygen cluster compound according to Example 1 of the present application. [Figure 4] 1 is an infrared spectrum of an organic mixed metal-oxygen cluster compound according to Example 1 of the present application. [Figure 5A]FIG. 2 is a scanning electron microscope view of an exposed and developed patterned material coating. [Figure 5B] FIG. 2 is a scanning electron microscope view of an exposed and developed patterned material coating. [Figure 6] FIG. 2 is a schematic diagram of the structure of an organic mixed metal-oxygen cluster compound according to Example 2 of the present application. [Figure 7] 1 is an infrared spectrum of an organic mixed metal-oxygen cluster compound according to Example 1 of the present application. [Figure 8A] FIG. 2 is a scanning electron microscope view of an exposed and developed patterned material coating. [Figure 8B] FIG. 2 is a scanning electron microscope view of an exposed and developed patterned material coating. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings.

[0044] In the patterning process, a high-precision pattern can be formed by using soft X-rays with a wavelength in the range of 1 nm to 15 nm as an exposure light source or by using electron beam etching. As shown in Fig. 1, the patterning process includes the steps of (1) forming a patterning material film layer 20 on a substrate 10, (2) selectively exposing the patterning material film layer 20, (3) developing the exposed patterning material film layer 20 to remove a part of the patterning material film layer 20, and (4) etching the substrate 10 using the remaining part of the patterning material film layer 20 as a protective layer.

[0045] In step (1), forming a patterning material film layer on a substrate includes: mixing a patterning material with a suitable solvent to form a solution with a certain concentration, the solution concentration can be adjusted according to the film thickness requirement, generally, a higher solution concentration corresponds to a thicker film layer; taking a certain volume of the solution based on the size of the substrate, and coating it on the substrate by spin-coating, the substrate can be a silicon wafer; and forming a patterning material film layer with a thickness of less than 100 nm on the silicon wafer covered by another coating, or on any other coating using the silicon wafer as the final substrate. Before selective exposure, the solvent remaining in the film layer is usually removed by baking.

[0046] In the selective exposure process in step (2), a mask (not shown) may be used. Any single wavelength or mixed wavelength light in soft X-rays with a wavelength ranging from 1 nm to 15 nm is selectively irradiated onto the patterning material film layer through the mask, and the pattern on the mask is transferred onto the patterning material film layer. After the patterning material is selectively irradiated, the chemical properties and solubility of the irradiated part of the patterning material are changed.

[0047] In the step (3), the irradiated patterning material is cleaned using a developer (which may be selected from organic solution, inorganic solution, pure solvent, mixed solvent, solvent with additive, etc.). The cleaning is performed for 10 seconds to 300 seconds, and may be a single-step cleaning or a multi-step cleaning. If the patterning material is a positive-type patterning material, the irradiated portion of the cleaned patterning material layer is washed away, forming a positive-type pattern. If the patterning material is a negative-type patterning material, the irradiated portion of the cleaned patterning material layer is not washed away, forming a negative-type pattern.

[0048] In step (4), the pattern formed by the patterning material selectively protects the substrate in the etching step. After performing the etching under certain conditions, the patterning material and the unprotected parts of the substrate are etched. However, the etching rate of the parts of the substrate protected by the patterning material is slower than the etching rate of the unprotected parts, so that a pattern is finally formed on the substrate.

[0049] In the above-mentioned patterning process, soft X-rays with wavelengths ranging from 1 nm to 15 nm or electron beams without a mask are used for exposure. Under these conditions, the resulting pattern is required to have high resolution, low pattern edge roughness, and low exposure energy consumption. However, it is difficult to meet these requirements with existing patterning materials.

[0050] Thus, the present application provides a patterning material that can be used in a process in which patterning is performed by exposure to short wavelength (less than 15 nm) soft X-rays or electron beams. The patterning material has high sensitivity to short wavelength (less than 15 nm) soft X-rays, thereby improving the pattern resolution and improving the pattern edge roughness.

[0051] The patterning material includes an organic mixed metal-oxygen cluster compound. In addition to the organic mixed metal-oxygen cluster compound, the patterning material may further include additives, such as a stabilizer, a dispersant, or a solvent.

[0052] The general chemical formula for organic mixed metal-oxygen cluster compounds is (M1) a (M2) b (M3) c O g (L1) x (L2) y (L3) z where M1 is selected from at least one of highly reactive metals / highly resolvable metals Ti, Zr, and Hf; M2 is selected from at least one of highly sensitive metals Bi, Te, Sn, Pt, Ag, and Au; M3 is selected from at least one of bridging metals Fe, Ni, Co, and Cu; L1, L2, and L3 are each selected from organic ligands that directly coordinate to a metal, including, but not limited to, O, S, Se, N, and P that function as coordinating atoms; a, b, g, x, y, and z are all natural numbers of 1 or more; and c is a natural number of 0 or more.

[0053] In some embodiments, when c=0, this represents that the organic mixed metal-oxygen cluster compound contains only two metals, M1 and M2.

[0054] In some embodiments, 2≦a+b+c≦60.

[0055] In some embodiments, g+x+y+z≦8(a+b+c), where g+x+y+z≦8(a+b+c) is determined based on the atomic coordination numbers.

[0056] In some embodiments, 5≧b / (a+c)≧0.1.

[0057] In one embodiment, the molar ratio of M1 to M2 to M3 is 5:9:1, i.e., the ratio of a to b to c is 5:9:1, and M1 is Ti, M2 is Bi, and M3 is at least one of Co and Ni.

[0058] In some embodiments, L1 and L2 may be organic ligands independent of each other. In some other embodiments, one or more of L1 and L2 (because there may be multiple organic ligands L1 and L2) coexist in the same organic ligand. For example, L1 and L2 coexist in a salicylic acid ligand. In this case, L1 may be an alcohol-based organic ligand and L2 may be a carboxylic acid-based organic ligand.

[0059] In some embodiments, at least a portion of the metal ions in the organic mixed metal-oxygen cluster compound may be replaced with a radiation sensitive element to enhance the photosensitivity of the organic mixed metal-oxygen cluster compound. The radiation sensitive element includes at least one of Na, Mg, Al, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Rb, Sr, Y, Ga, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, Sn, Sb, Te, Cs, Ba, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Pb, Bi, and Po. Since M1, M2, and M3 of the organic mixed metal-oxygen cluster compound may contain at least one of the above-mentioned radiation-sensitive elements Ti, Fe, Co, Ni, Cu, Ag, Sn, Te, Hf, Pt, Au, and Bi, the radiation-sensitive element replacing the metal ion in the organic mixed metal-oxygen cluster compound is different from the metal element originally contained in the organic mixed metal-oxygen cluster compound in the present application. That is, for example, when the organic mixed metal-oxygen cluster compound contains metal Ti, Ti is not selected as the radiation-sensitive element for replacement.

[0060] In some embodiments, a radiation-sensitive functional group may be introduced into at least one of L1, L2, and L3 to further enhance the photosensitivity of the organic mixed metal-oxygen cluster compound, improve line edge roughness, and improve resolution. The radiation-sensitive functional group includes at least one of a double bond, a triple bond, and an epoxypropane.

[0061] In some embodiments, a radiation-sensitive functional group may be introduced into at least one of the organic ligands L1, L2, and L3. For example, the functional group may be at least one of additionally accessible reactive groups such as carboxylic acids, alcohols, phenols, nitriles, alkynes, alcoholamines, pyridines, pyrazoles, imidazoles, piperazines, and pyrazines, to adjust properties such as the solubility of the organic mixed metal-oxygen cluster compound, thereby affecting the film layer thickness, film layer roughness, resolution, film layer adhesion, and corrosion resistance.

[0062] It can be appreciated that the ratio of coordination atoms of the organic ligand to the metal ion may be adjusted to improve the sensitivity, line edge roughness, and resolution of the organic mixed metal-oxygen cluster compounds.

[0063] In this application, the organic mixed metal-oxygen cluster compound includes metals and organic ligands. By adjusting the types and ratios of different metals and / or introducing photosensitive functional groups into the organic ligands, the photosensitivity of the patterning material may be further enhanced, the line edge roughness may be improved, and the resolution may be improved.

[0064] In this application, under exposure to soft X-rays with wavelengths ranging from 1 nm to 15 nm, the organic mixed metal-oxygen cluster compound has high sensitivity and can be fine-tuned. The organic mixed metal-oxygen cluster compound is used as the main material of the patterning material, which can solve the problem that the patterning material needs to meet high sensitivity, high etching resistance, high resolution, low outgassing (meaning less gas is released in the exposure process), small molecular size, and material properties that can be fine-tuned by using mixed metals.

[0065] In this application, the patterning method implemented using the aforementioned patterning material includes the following steps.

[0066] (a) Substrate surface treatment Hydrophilization treatment: Cleaning is performed in piranha solution (H2O: 30% ammonia hydroxide: 30% H2O2 = 5:1:1) for 15 to 20 minutes, followed by rinsing with deionized water and then isopropanol. Before use, the liquid on the substrate surface is dried using an air gun.

[0067] Hydrophobization treatment: After the substrate is subjected to hydrophilization treatment, hexamethyldisilazane (HMDS) is uniformly coated on the surface of the substrate by vapor plating or spin coating.

[0068] Anti-reflective layer treatment: An anti-reflective layer is added on the bottom layer, or a silicide layer or a carbon compound layer is coated on the bottom layer by spin coating method.

[0069] (b) Solution preparation The prepared organic mixed metal-oxygen cluster compound (white powder) is dissolved in a solvent to form a clear solution. If there is obvious insolubility, the solvent is reselected to dissolve the organic mixed metal-oxygen cluster compound and obtain a clear solution. The solution is then filtered to obtain a patterning material formulation mixture. The solvent includes, but is not limited to, N,N-dimethylformamide, ethyl lactate, 2-acetoxy-1-methoxypropane, isopropanol, toluene, dichloromethane, etc. The concentration of the organic mixed metal-oxygen cluster compound in the solvent is about 5 mg / mL to 30 mg / mL.

[0070] (c) Preparation of membrane layer Based on the size of the substrate, an appropriate amount of the patterning material blend mixture is used for spin coating. For example, typically, 1 mL to 5 mL of the patterning material blend mixture is spin coated on a 4-inch silicon wafer to obtain a patterning material film layer with a uniform thickness of 5 nm to 200 nm and a surface roughness of less than 2 nm. After spin coating, an optional baking step may be added. The baking temperature to remove the residual solvent ranges from 60° C. to 200° C., and the baking time ranges from 20 seconds to 120 seconds.

[0071] (d) Film layer exposure The patterning material layer is selectively irradiated with electron beams, extreme ultraviolet light, or soft X-rays with wavelengths ranging from 1 nm to 15 nm. A chemical reaction occurs in the irradiated portions of the patterning material layer, changing the solubility of the irradiated portions. A mask is used in the step of locally exposing the patterning material layer with soft X-rays. The soft X-rays carrying the pattern information reach the patterning material layer through the mask, and the patterning material layer is locally exposed.

[0072] After exposure, an optional baking step may be added to accelerate any pending chemical reactions in the film layer, with baking temperatures ranging from 60° C. to 200° C. and baking times ranging from 20 seconds to 120 seconds.

[0073] (e) Development process In the development process, a developer is used to contact the exposed film layer, and a portion of the patterning material film layer is dissolved and removed. For example, the film layer may be immersed in the developer. The contact time between the developer and the film layer is usually not more than 10 minutes.

[0074] In some embodiments, the developer includes solvents such as isopropanol, N,N-dimethylformamide, 2-acetoxy-1-methoxypropane, ethyl lactate, and water, or combinations thereof, as well as other solvents that allow the material to exhibit different dissolution rates before and after irradiation.

[0075] In an embodiment, the developer may be a developer comprising the following solvents or a mixture of two or more of the following solvents: Aqueous solutions of tetramethylammonium hydroxide (TMAH) with concentrations ranging from 0.5% to 5%; Organic solvents such as ketones, e.g., cyclohexanone, methyl-2-n-pentyl ketone; Alcohols, such as 3-methoxy-1-butanol, 3-methyl-3-methoxy-1-butanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, diacetone alcohol; ethers, such as propylene glycol monomethyl ether, 2-methoxyethanol, propylene glycol monoethyl ether, 2-ethoxyethanol, 1,2-dimethoxypropane, and diethylene glycol dimethyl ether; Esters, such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, ethyl pyruvate, butyl acetate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, and propylene glycol mono-tert-butyl ether acetate; Lactones, such as gamma-butyrolactone; High boiling alcohol solvents, such as diethylene glycol, propylene glycol, glycerol, 1,4-butanediol, or 1,3-butanediol.

[0076] The development time of contact between the developer and the exposed film layer ranges from 10 seconds to 120 seconds. After the development process, a water washing rinsing process may be optionally added, and the washing rinsing time may be from 10 s to 120 s. After the rinsing process, a baking process may be optionally added, and the baking temperature may be in the range of 60° C. to 200° C., and the baking time may be in the range of 20 s to 120 s.

[0077] (f) Pattern description The resulting patterns are observed and measured using an electron microscope or an atomic force microscope. The resulting pattern resolution is 3 nm to 100 nm, and the edge roughness is 2% to 30% of the pattern resolution.

[0078] (g) Etching process (selective) The patterning material film layer may be used as a protective layer to etch the substrate, and the pattern may be transferred to the substrate under etching conditions such as oxygen ions or in an ion implantation process.

[0079] It may be understood that step (a) is selectively performed. In some embodiments, step (a) may be omitted, or a hydrophilic or hydrophobic treatment may be performed in step (a).

[0080] It may be understood that step (g) is selectively performed. In some embodiments, step (g) may be omitted instead. This may leave an unetched patterned film layer on the substrate as a functional layer.

[0081] The present application further provides an electronic device (not shown) having the semiconductor device. In some embodiments, the semiconductor device may be part of an integrated circuit (not shown). As shown in FIG. 2, the semiconductor device 100 has a substrate 10 and a patterned functional layer 30 (e.g., a dielectric material layer) formed on the substrate 10. The functional layer 30 includes an organic mixed metal-oxygen cluster compound. The pattern resolution of the functional layer 30 is high, reaching 10 nm to 40 nm. The edge roughness of the pattern is low, within 10% of the resolution.

[0082] The following further illustrates the technical solutions in the embodiments of the present application by using specific embodiments.

[0083] Example 1 An organic mixed metal-oxygen cluster compound is synthesized: Ti5CoBi9O9(C7H4O3)9(C2OO)(C7H4O3). In particular, the aforementioned molecular formula is [Ti(C7H4O3)3]3@Ti2Co II It may be represented as Bi9O8(μ2-O)(μ2-C2OO)(C7H4O3)8, where @ represents [Ti(C7H4O3)3]3 connected to two central Ti atoms, one O atom connected to two atoms in a μ2 bridging manner, and (C2OO) groups connected to two atoms in a μ2 bridging manner.

[0084] 0.05 mmol of bismuth salicylate, 0.1 mol of cobalt acetate, 0.1 mmol of salicylic acid, and 0.5 ml of titanium tetraisopropoxide are mixed in 8 ml of acetonitrile, heated to 80°C, and cooled to room temperature after 3 days. The precipitated crystals are organic mixed metal-oxygen cluster compounds.

[0085] Figure 3 shows [Ti(C7H4O3)3]3@Ti2Co II A schematic diagram of the structure of Bi9O8(μ2-O)(μ2-C2OO)(C7H4O3)8 is shown. In Fig. 3, some atoms such as oxygen, carbon, nitrogen, and hydrogen are omitted to clarify the structure.

[0086] Figure 4 shows the infrared spectrogram of an organic mixed metal-oxygen cluster compound. -1 The characteristic peaks at 1032 to 1242 cm are in the region of the expansion vibration of metal-oxygen bonds, suggesting the presence of Bi-O, Ti-O, and Co-O. -1 The characteristic peak at 1349 to 1595 cm is the expansion vibration region of CO. -1 The characteristic peak at 3000 to 3500 cm represents the skeletal vibration of the benzene ring and indicates the presence of a benzene ring. -1 The characteristic peak at the position is the OH / NH expansion vibration region and the H2O peak, suggesting that the organic mixed metal-oxygen cluster compound contains a trace amount of water molecules.

[0087] Patterning process Hydrophilization treatment: Cleaning treatment is carried out in piranha solution (H2O: 30% ammonia hydroxide: 30% H2O2 = 5:1:1) for 15 to 20 minutes, treated with deionized water, and then washed with isopropanol. Before use, the liquid on the surface is dried by using an air gun. Hydrophobization treatment: After carrying out hydrophilization treatment on the silicon wafer, HMDS is uniformly coated on the surface of the silicon wafer by vapor plating or spin coating.

[0088] Preparation of the membrane layer: 5 mg to 20 mg of organic mixed metal-oxygen cluster compound is dissolved in 1 mL of N,N-dimethylformamide (DMF), the solution is filtered, and an appropriate amount of the filtered solution is taken and spin-coated onto the surface of a hydrophilic or hydrophobic silicon wafer to form a metal-organic cluster patterning material coating.

[0089] Radiation exposure: Exposure is carried out on the patterned material coating using electron beam etching techniques (EBL).

[0090] Development: The developer combinations used include mixtures of DMF and propylene glycol monomethyl ether acetate (PGMEA) in a volume ratio of 10:1 to 1:10, and mixtures of isopropanol (IPA) and PGMEA in a volume ratio of 10:1 to 1:10. Development times range from 15 to 60 seconds.

[0091] Graphical Delineation: A scanning electron microscope (SEM) is used to delineate a pattern onto an exposed and developed patterning material coating.

[0092] As shown in Figures 5A and 5B, the exposed and developed patterning material coating is a plurality of lines extending in the same direction. The line width in Figure 5(a) is 100 nm, and the line width in Figure 5(b) is 50 nm. The resolution of the exposed and developed patterning material coating can reach 100 nm or even 50 nm.

[0093] In this embodiment, a new kind of Ti, Co, and Bi mixed metal-oxygen cluster compound can be used as a high-performance patterning material for exposure using a light source with a wavelength of less than 15 nm and an electron beam. High-resolution patterns can be formed after exposure. Also, the properties of the patterning material can be fine-tuned through the proportion of mixed metals.

[0094] Example 2 An organic mixed metal-oxygen cluster compound is synthesized: Ti5NiBi9O9(C7H4O3)9(C2OO)(C7H4O3). In particular, the aforementioned molecular formula is [Ti(C7H4O3)3]3@Ti2Ni II It can be represented as Bi9O8(μ2-O)(μ2-C2OO)(C7H4O3)8, where @ represents [Ti(C7H4O3)3]3 bonded to two central Ti atoms, one O atom bonded to two atoms in μ2-bridging manner, and (C2OO) groups bonded to two atoms in μ2-bridging manner.

[0095] 0.05 mmol of bismuth salicylate, 0.1 mol of nickel acetate, 0.1 mmol of salicylic acid, and 0.5 ml of titanium tetraisopropoxide are mixed in 8 ml of acetonitrile, heated to 80°C, and cooled to room temperature after 3 days. The precipitated crystals are organic mixed metal-oxygen cluster compounds.

[0096] Figure 6 shows [Ti(C7H4O3)3]3@Ti2Ni II A schematic diagram of the structure of Bi9O8(μ2-O)(μ2-C2OO)(C7H4O3)8 is shown in Figure 6. Note that in Figure 6, some atoms such as oxygen, carbon, nitrogen, and hydrogen are omitted to clarify the structure.

[0097] Figure 7 shows the infrared spectrogram of an organic mixed metal-oxygen cluster compound. -1 The characteristic peaks at 1030 to 1240 cm are in the region of the expansion vibration of metal-oxygen bonds, suggesting the presence of Bi-O, Ti-O, and Ni-O. -1The characteristic peak at 1464 to 1608 cm is the expansion vibration region of CO. -1 The characteristic peak at position indicates the skeletal vibration of the benzene ring, suggesting the presence of a benzene ring.

[0098] Patterning Method Silicon wafer processing: Hydrophilization treatment: Cleaning treatment is carried out in piranha solution (H2O: 30% ammonium hydroxide: 30% H2O2 = 5:1:1) for 15 to 20 minutes, followed by treatment with deionized water and rinsing with isopropanol. Before use, the liquid on the surface of the silicon wafer is dried by using an air gun.

[0099] Hydrophobization treatment: After the silicon wafer is subjected to hydrophilization treatment, the surface of the silicon wafer is uniformly coated with HMDS by vapor plating or spin coating.

[0100] Preparation of membrane layer: 5 mg to 30 mg of solid sample is dissolved in 1 mL of ethyl lactate solvent, the solution is filtered, and an appropriate amount of the filtered solution is taken and spin-coated onto the surface of a hydrophilic or hydrophobic silicon substrate to form a mixed metal-organic cluster patterning material coating.

[0101] Radiation Exposure: In the present invention, exposure is performed on the patterning material layer using an electron beam etching technique (EBL).

[0102] Development: The developer combination used in the present invention includes isopropanol. Development times range from 15 to 60 seconds.

[0103] Patterning: A scanning electron microscope (SEM) is used to pattern the exposed and developed layer material.

[0104] As shown in Figures 8A and 8B, the exposed and developed patterning material coating is a plurality of lines extending in the same direction. The width of the lines in Figure 8(a) is 100 nm, and the width of the lines in Figure 8(b) is 50 nm. The resolution of the exposed and developed patterning material coating may reach 100 nm or 50 nm.

[0105] It should be noted that the above description is merely a specific embodiment of the present application, and the scope of protection of the present application is not limited thereto. Any modifications or replacements that can be easily found by those skilled in the art within the technical scope described in the present application should be within the scope of protection of the present application. If not inconsistent, the features in the embodiments and embodiments of the present application may be combined with each other. Therefore, the scope of protection of the present application is subject to the scope of protection of the claims. [Explanation of symbols]

[0106] 100 Semiconductor device 10 Substrate 20 Patterning material film layer 30 Functional Layers

Claims

1. 1. An organic mixed metal-oxygen cluster compound comprising: The general chemical formula is: <h2 style=";text-align:left;direction:ltr">(M1)<h2 style=";text-align:left;direction:ltr"> a <h2 style=";text-align:left;direction:ltr"> (M2)<h2 style=";text-align:left;direction:ltr"> b <h2 style=";text-align:left;direction:ltr"> (M3)<h2 style=";text-align:left;direction:ltr"> c <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> g <h2 style=";text-align:left;direction:ltr"> (L1)<h2 style=";text-align:left;direction:ltr"> x <h2 style=";text-align:left;direction:ltr"> (L2)<h2 style=";text-align:left;direction:ltr"> y <h2 style=";text-align:left;direction:ltr"> (L3)<h2 style=";text-align:left;direction:ltr"> z where M1 is selected from at least one of Ti, Zr, and Hf; M2 is selected from at least one of Bi, Te, Sn, Pt, Ag, and Au; M3 is selected from at least one of Fe, Ni, Co, and Cu; L1, L2, and L3 are each selected from organic ligands, which can be coordinated to a metal and contain at least one of O, S, Se, N, and P that function as a ligating atom; an organic mixed metal-oxygen cluster compound, wherein a, b, g, x, y and z are all natural numbers equal to or greater than 1, and c is a natural number equal to or greater than 0;

2. 2. The organic mixed metal-oxygen cluster compound of claim 1, wherein 2≦a+b+c≦60.

3. 3. The organic mixed metal-oxygen cluster compound of claim 1 or 2, wherein g+x+y+z≦8(a+b+c).

4. 4. The organic mixed metal-oxygen cluster compound of claim 1, wherein 5 > b / (a+c) > 0.

1.

5. 5. The organic mixed metal-oxygen cluster compound of claim 1, wherein the ratio of a:b:c is 5:9:

1.

6. 6. The organic mixed metal-oxygen cluster compound of claim 5, wherein M1 is Ti, M2 is Bi, and M3 is at least one of Co and Ni.

7. At least one of L1, L2, and L3 comprises a functional group; 7. The organic mixed metal-oxygen cluster compound of claim 1, wherein the functional group is selected from at least one of carboxylic acids, alcohols, phenols, nitriles, alkynes, alcoholamines, pyridines, pyrazoles, imidazoles, piperazines, and pyrazines.

8. At least one of L1, L2, and L3 comprises a radiation-sensitive functional group; 8. The organic mixed metal-oxygen cluster compound of claim 1, wherein the radiation sensitive functional group comprises at least one of a double bond, a triple bond, and an epoxypropane.

9. 9. The organic mixed metal-oxygen cluster compound of claim 1, wherein one or more of L1 and L2 coexist in the same organic ligand.

10. At least a portion of the metal ions in the organic mixed metal-oxygen cluster compound are replaced with a radiation sensitive element; the radiation sensitive element comprises at least one of Na, Mg, Al, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Rb, Sr, Y, Ga, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, Sn, Sb, Te, Cs, Ba, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Pb, Bi, and Po; 10. The organic mixed metal-oxygen cluster compound of claim 1, wherein the radiation sensitive element for substitution is different from the metal element originally contained in the organic mixed metal-oxygen cluster compound.

11. 1. A patterning material comprising an organic mixed metal-oxygen cluster compound, The general chemical formula of the organic mixed metal-oxygen cluster compound is: <h2 style=";text-align:left;direction:ltr">(M1)<h2 style=";text-align:left;direction:ltr"> a <h2 style=";text-align:left;direction:ltr"> (M2)<h2 style=";text-align:left;direction:ltr"> b <h2 style=";text-align:left;direction:ltr"> (M3)<h2 style=";text-align:left;direction:ltr"> c <h2 style=";text-align:left;direction:ltr"> Og(L1)<h2 style=";text-align:left;direction:ltr"> x <h2 style=";text-align:left;direction:ltr"> (L2)<h2 style=";text-align:left;direction:ltr"> y <h2 style=";text-align:left;direction:ltr"> (L3)<h2 style=";text-align:left;direction:ltr"> z where: M1 is selected from at least one of Ti, Zr, and Hf; M2 is selected from at least one of Bi, Te, Sn, Pt, Ag, and Au; M3 is selected from at least one of Fe, Ni, Co, and Cu; L1, L2, and L3 are each selected from organic ligands, which directly coordinate to the metal and contain at least one of O, S, Se, N, and P that function as a coordination atom; wherein b, g, x, y, and z are all natural numbers equal to or greater than 1, and c is a natural number equal to or greater than 0.

12. 12. The patterning material of claim 11, wherein 2≦a+b+c≦60, g+x+y+z≦8(a+b+c), and 5≧b / (a+c)≧0.

1.

13. The ratio of a:b:c is 5:9:1, 13. The patterning material of claim 11 or 12, wherein M1 is Ti, M2 is Bi, and M3 is at least one of Co and Ni.

14. 14. The patterning material of claim 11, wherein at least one of L1, L2, and L3 comprises a functional group selected from at least one of a carboxylic acid, an alcohol, a phenol, a nitrile, an alkyne, an alcoholamine, a pyridine, a pyrazole, an imidazole, a piperazine, and a pyrazine.

15. 15. The patterning material of claim 11, wherein at least one of L1, L2, and L3 comprises a radiation-sensitive functional group, the radiation-sensitive functional group comprising at least one of a double bond, a triple bond, and an epoxypropane.

16. 16. The patterning material of claim 11, wherein one or more of L1 and L2 coexist in the same organic ligand.

17. At least a portion of the metal ions in the organic mixed metal-oxygen cluster compound are replaced by a radiation sensitive element; the radiation sensitive element comprises at least one of Na, Mg, Al, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Rb, Sr, Y, Ga, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, Sn, Sb, Te, Cs, Ba, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Pb, Bi, and Po; 17. The patterning material of claim 11, wherein the substitution radiation-sensitive element is different from the metal element originally contained in the organic mixed metal-oxygen cluster compound.

18. A semiconductor device comprising: A substrate; a functional layer disposed on a surface of the substrate, the functional layer comprising a patterning material according to any one of claims 11 to 17; The semiconductor device has

19. A terminal, A housing and A semiconductor device accommodated in the housing; having A terminal comprising the semiconductor device according to claim 18.

20. 1. A method for patterning a surface of a substrate, comprising the steps of: Providing a substrate; Forming a patterning material layer on a surface of the substrate, the patterning material layer comprising an organic mixed metal-oxygen cluster compound, the organic mixed metal-oxygen cluster compound having a general chemical formula: <h2 style=";text-align:left;direction:ltr">(M1)<h2 style=";text-align:left;direction:ltr"> a <h2 style=";text-align:left;direction:ltr"> (M2)<h2 style=";text-align:left;direction:ltr"> b <h2 style=";text-align:left;direction:ltr"> (M3)<h2 style=";text-align:left;direction:ltr"> c <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> g <h2 style=";text-align:left;direction:ltr"> (L1)<h2 style=";text-align:left;direction:ltr"> x <h2 style=";text-align:left;direction:ltr"> (L2)<h2 style=";text-align:left;direction:ltr"> y <h2 style=";text-align:left;direction:ltr"> (L3)<h2 style=";text-align:left;direction:ltr"> z where M1 is selected from at least one of Ti, Zr, and Hf; M2 is selected from at least one of Bi, Te, Sn, Pt, Ag, and Au; M3 is selected from at least one of Fe, Ni, Co, and Cu; L1, L2, and L3 are each selected from organic ligands, and the organic ligands directly coordinate to a metal and contain at least one of O, S, Se, N, and P that function as a coordination atom; a, b, g, x, y, and z are all natural numbers greater than or equal to 1, and c is a natural number greater than or equal to 0; performing a localized exposure to the patterning material layer; removing portions of the patterning material layer using a developer; A method for patterning a substrate surface comprising the steps of:

21. 21. The method of patterning a substrate surface according to claim 20, wherein in the general chemical formula of the organic mixed metal-oxygen cluster compound, 2≦a+b+c≦60, g+x+y+z≦8(a+b+c), and 5≧b / (a+c)≧0.

1.

22. In the general chemical formula of the organic mixed metal-oxygen cluster compound, at least one of L1, L2, and L3 contains a functional group; 22. The method of patterning a substrate surface according to claim 20 or 21, wherein the functional group is selected from at least one of carboxylic acids, alcohols, phenols, nitriles, alkynes, alcoholamines, pyridines, pyrazoles, imidazoles, piperazines, and pyrazines.

23. 23. The method for patterning a substrate surface according to any one of claims 20 to 22, wherein at least one of L1, L2, and L3 comprises a radiation-sensitive functional group, the radiation-sensitive functional group comprising at least one of a double bond, a triple bond, and an epoxypropane.

24. At least a portion of the metal ions in the organic mixed metal-oxygen cluster compound are replaced by a radiation sensitive element; the radiation sensitive element comprises at least one of Na, Mg, Al, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Rb, Sr, Y, Ga, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, Sn, Sb, Te, Cs, Ba, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Pb, Bi, and Po; 24. The method for patterning a substrate surface according to claim 20, wherein the substitutional radiation sensitive element is different from the metal element originally contained in the organic mixed metal-oxygen cluster compound.

25. 25. The method of claim 20, wherein in the general chemical formula of the organic mixed metal-oxygen cluster compound, the ratio of a:b:c is 5:9:1, M1 is Ti, M2 is Bi, and M3 is at least one of Co and Ni.

26. 26. The method for patterning a substrate surface according to any one of claims 20 to 25, wherein in the step of performing localized exposure on the patterning material layer, any single wavelength or mixed wavelength light of soft X-rays in the wavelength range of 1 nm to 15 nm is used, or an electron beam is used, or extreme ultraviolet radiation is used.

27. 27. The method for patterning a substrate surface according to claim 26, wherein in the step of performing localized exposure on the patterning material layer using soft X-rays, a mask is used, and soft X-rays carrying pattern information reach the patterning material layer through the mask, thereby locally exposing the patterning material layer.

28. 28. The method of claim 20, wherein the developer is at least one of isopropanol, N,N-dimethylformamide, 2-acetoxy-1-methoxypropane, ethyl lactate, and water.

29. 29. The method for patterning a substrate surface according to claim 20, further comprising the step of etching the substrate using the patterning material film layer remaining on the substrate as a protection layer.

Citation Information

Patent Citations

  • Organically modified metal oxide nanoparticle, solution containing organically modified metal oxide nanoparticle, resist composition containing organically modified metal oxide nanoparticle and resist pattern formation method

    JP2021102604A

  • Pattern forming method and radiation sensitive composition

    WO2019220835A1