Aluminium diethylphosphinate crystals with low fine powder content, their production method and use

By incorporating a phosphorus-containing aluminum salt complex as a seed crystal, the method addresses flowability issues in aluminum diethylphosphinate particles, producing crystals with reduced fine powder content and narrow distribution, enhancing production efficiency and flame retardancy in glass fiber reinforced engineering plastics.

JP2024538313AActive Publication Date: 2024-10-18JIANGSU LISIDE NEW MATERIAL
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024525824
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-03-10
Filing Date
2022-04-18
Publication Date
2024-10-18
Estimated Expiration
2042-04-18

AI Technical Summary

Technical Problem

Conventional aluminum diethylphosphinate particles used in non-halogen flame retardant systems for glass fiber reinforced engineering plastics suffer from flowability issues such as bridging and clogging due to a high content of fine powders, leading to production inefficiencies and material performance inconsistencies.

Method used

A method involving the addition of a phosphorus-containing aluminum salt complex as a seed crystal during the production process to control crystallization, resulting in aluminum diethylphosphinate crystals with a low fine powder content, narrow particle size distribution, and larger particle sizes, thereby reducing bridging and clogging.

Benefits of technology

The produced crystals exhibit improved flowability, eliminating the need for high-concentration masterbatches and ensuring long-term operation in the processing of non-halogen flame-retardant glass fiber reinforced engineering plastics while maintaining high flame retardancy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538313000001_ABST
    Figure 2024538313000001_ABST
Patent Text Reader

Abstract

The present invention discloses a diethylphosphinate aluminum crystal with low content of fine powder, its preparation method, and its use in flame retarding glass fiber reinforced engineering plastics. The present invention uses phosphorus-containing aluminum salt complex as seed crystals to add in the process of preparing diethylphosphinate aluminum crystals, effectively controlling the crystallization process, and obtaining diethylphosphinic acid crystal particles with low content of fine powder, narrow distribution, and large particle size, which can solve the problems of conventional diethylphosphinate aluminum powder such as easy bridging and clogging, and can be applied to the processing process of non-halogen flame retardant glass fiber reinforced engineering plastics. The prepared diethylphosphinate aluminum contains a small amount of phosphorus-containing aluminum salt complex seed crystals, and its flame retardancy is not affected.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of new materials, in particular to an aluminum diethylphosphinate crystal having a low fine powder content, and its preparation method and use. The preparation method uses a phosphorus-containing aluminum salt complex as a seed crystal to obtain an aluminum diethylphosphinate crystal having a low fine powder content that satisfies the powder flowability of a flame retardant required for the production process of halogen-free flame-retardant glass fiber reinforced engineering plastics. [Background technology]

[0002] Glass fiber reinforced engineering plastics (such as various nylons and polyesters) are widely used in the field of electronic devices because of their characteristics such as good rigidity, impact resistance, low warpage, and good appearance. The use in these fields increases the demand for flame retardancy in materials, and although many engineering plastics are flammable materials, when blended with glass fiber, the wick effect of glass fiber makes glass fiber reinforced engineering plastics more flammable. Therefore, when using glass fiber reinforced engineering plastics in these fields, it is necessary to solve the problem of flame retardancy, but the existence of the wick effect makes it even more difficult to make them flame retardant.

[0003] There are two basic types of flame retardant systems for glass fiber reinforced engineering plastics: halogenated flame retardant systems and non-halogenated flame retardant systems. In halogenated flame retardant systems, brominated flame retardants and antimony trioxide are usually used in combination, but many studies have shown that glass fiber reinforced engineering plastics with added brominated flame retardants will produce harmful substances such as thick smoke and hydrogen bromide when burned, which may cause suffocation. Therefore, the development of safe and environmentally friendly non-halogenated flame retardant systems for glass fiber reinforced engineering plastics has become a research hotspot, and new non-halogenated flame retardants or flame retardant systems for glass fiber reinforced engineering plastics have appeared in recent years.

[0004] At present, the mainstream of halogen-free flame retardants applied to glass fiber reinforced engineering plastics is a combination of aluminum diethylphosphinate and a nitrogen-containing compound, for example, a composite system based on aluminum diethylphosphinate, including a composite system of aluminum diethylphosphinate and melamine polyphosphate (MPP), and a composite system of aluminum diethylphosphinate and aluminum phosphite, which does not contain nitrogen. These systems are still widely used because they have high flame retardancy and high temperature resistance and do not have problems such as color. However, in the compounding system based on aluminum diethylphosphinate, the particle size is usually too small, and when used to manufacture flame retardants using a twin-screw extruder, there are usually problems with flowability, and problems such as powder bridging and clogging are easily caused, making it difficult to realize long-term operation. The usual solution to this problem is to manufacture the flame retardant powder into a high-concentration flame retardant masterbatch, but the problems present in this solution are also obvious. (1) Increase the cost of one-time production of the masterbatch. (2) Masterbatches require polymer carriers, and the presence of these carriers can cause insufficient formulation flexibility in downstream materials, and may affect the performance of the materials and prevent them from being used. Therefore, solving the problem of aluminum diethylphosphinate blockage through high-concentration masterbatch solutions is not the best way, and it is necessary to find a way to solve the blockage from aluminum diethylphosphinate itself.

[0005] Research has found that the main cause of bridging and blockage during the use of aluminum diethylphosphinate particles is the fine powder present in the aluminum diethylphosphinate particles, and these fine powders have a very small particle diameter, usually less than 5 μm, and the smaller the particle diameter, the larger the specific surface area and the greater the interparticle force, and when the occupancy rate of the fine powder in this area exceeds a certain value, it is easy to cause bridging and blockage. Therefore, the key to solving blockage is to control the proportion of fine powder in aluminum diethylphosphinate.

[0006] From the perspective of the production process of aluminum diethylphosphinate, the aluminum diethylphosphinate particles are produced by utilizing the low water solubility and crystallization property of aluminum diethylphosphinate, and are obtained by crystallization and precipitation in an aqueous phase through a metathesis reaction, and the actual particle formation process is a crystallization process. According to the electron microscope observation, aluminum diethylphosphinate particles are obtained by stacking a large number of small flake-like small crystal particles, the size of these small crystal particles is very small, and stacking is a random process, so in the natural crystalline state, the size of the crystal particles has a wide distribution, and at the same time, the molecular structure of aluminum diethylphosphinate contains lipophilic ethyl groups and hydrophilic aluminum salt structures, that is, its molecular structure contains both lipophilic and hydrophilic parts, and when small crystal particles are stacked, repulsion occurs, and the action force of the structure formed by stacking small crystal particles is weak, so when shear force such as a stirrer is applied, small particles are easily obtained, so the particle size of aluminum diethylphosphinate particles tends to be small, and in the normal production process, the particle size distribution of the particles obtained is wide, that is, the characteristics of the conventional aluminum diethylphosphinate particles currently produced are small average particle size, wide distribution, and large amount of ultrafine particles. Such particle size characteristics cause the blockage of aluminum diethylphosphinate. Therefore, the key to solving this problem is to control the crystallization process in the production of aluminum diethylphosphinate, reduce the proportion of ultrafine particles, reduce the maximum particle size, appropriately increase the average particle size, distribute the particle size of the particles as close as possible to the average particle size, and narrow the particle size distribution. There have been no relevant reports on the method for effectively reducing the particle size of ultrafine particles. Summary of the Invention [Problem to be solved by the invention]

[0007] In view of the above technical problems and the shortcomings of the present field, the present invention uses phosphorus-containing aluminum salt complex as seed crystals to add in the process of producing aluminum diethylphosphinate crystals, effectively controlling the crystallization process, and obtaining diethylphosphinic acid crystal particles with low fine powder content, narrow distribution and large particle size, which can solve the problems of conventional aluminum diethylphosphinate powder such as easy bridging and clogging, and can be applied to the processing of non-halogen flame-retardant glass fiber reinforced engineering plastics. The produced aluminum diethylphosphinate contains a small amount of phosphorus-containing aluminum salt complex seed crystals, and its flame retardancy is not affected.

[0008] The main object of the present invention is to provide a method for preparing aluminum diethylphosphinate which overcomes the defects of conventional aluminum diethylphosphinate. The method for preparing aluminum diethylphosphinate can obtain aluminum diethylphosphinate crystal particles with low fine powder content, narrow distribution and large particle size, thereby solving flowability problems such as bridging and clogging, eliminating the need to prepare a masterbatch containing a high concentration of carrier, and allowing the powder to be directly applied to the processing of non-halogen flame-retardant glass fiber reinforced engineering plastics while maintaining high flame retardancy.

[0009] The present invention relates to the preparation of aluminum diethylphosphinate with a low content of fine powder, and by adding a small amount of phosphorus-containing aluminum salt complex of aluminum diethylphosphinate and aluminum ethylbutylphosphinate as seed crystals during the preparation of aluminum diethylphosphinate, the crystallization process of aluminum diethylphosphinate can be effectively controlled to obtain aluminum diethylphosphinate crystal powder with a low content of fine powder, narrow distribution and large particle size, which solves the problems of aluminum diethylphosphinate obtained by the conventional preparation method, such as a high content of small particle size powder and wide distribution, and solves the problem of fluidity during use, such as easy formation of bridges and blockages. [Means for solving the problem]

[0010] The specific technical solutions are as follows:

[0011] A method for producing aluminum diethylphosphinate crystals having a low content of fine powder, comprising the steps of: uniformly dispersing a phosphorus-containing aluminum salt complex as seed crystals in an aqueous solution of a soluble diethylphosphinate salt; adding a water-soluble aluminum salt solution containing a strong acid; reacting at 70 to 95°C; and washing and drying the solid product after the reaction to obtain aluminum diethylphosphinate crystals having a low content of fine powder; The phosphorus-containing aluminum salt complex has a structure represented by formula (I): [ka] (In formula (I), a, b, c, d, and e are all molar ratios, a is 0.1 to 0.5, b is 0.5 to 0.9, c, d, and e are 0 to 0.3, and a+b+c+d+e=1; R1 and R2 are each independently selected from H and C1 to C6 alkyl, and when either R1 or R2 is ethyl, the other is not ethyl or butyl, and R3 is C1 to C6 alkyl.)

[0012] The present invention will be described in detail below.

[0013] The present invention aims to solve the flow problems, such as the tendency of bridging and clogging to occur in halogen-free flame retardant systems using aluminum diethylphosphinate, which have been widely used in glass fiber reinforced engineering plastics, and the inventors have conducted extensive research into this matter.

[0014] As a result of the research, it was found that the crystal transition of the phosphorus-containing aluminum salt complex of ethylbutylphosphinate aluminum is different from that of diethylphosphinate aluminum, and that under certain conditions, the crystal transition disappears. This phosphorus-containing aluminum salt complex is, a phosphorus-containing structure of formula (II) and one or more phosphorus-containing structures represented by structural formula (III) and / or structural formula (IV). [ka] In the structural formula (III), R1 and R2 are each independently selected from H or C1-C6 alkyl, and when either R1 or R2 is ethyl, the other is not butyl; In structural formula (IV), R3 is H or C1-C6 alkyl.

[0015] The phosphorus-containing aluminum salt complex exhibits properties different from those of a single aluminum salt or a mixture of a plurality of aluminum salts, and is a compound having a novel structure.

[0016] DSC characterization is performed on phosphorus-containing aluminum salt complexes. Taking the ethylbutylphosphinate aluminum (0.7)-diethylphosphinate aluminum (0.3) complex (numbers represent the molar ratio of aluminum complex salts, same below) with the molecular structure shown in FIG. 1 as an example, its DSC chart is shown in FIG. 2. As can be seen from the DSC chart, this ethylbutylphosphinate aluminum-diethylphosphinate aluminum complex does not have a crystal transition peak. FIG. 3 is a DSC chart of a mixture of ethylbutylphosphinate aluminum and diethylphosphinate aluminum (mixed molar ratio 0.7:0.3), and FIG. 4 and FIG. 5 are DSC charts of ethylbutylphosphinate aluminum and diethylphosphinate aluminum, respectively. As a result, the complex with the novel structure shown in FIG. 1 is different from both mixtures. In the case of both mixtures, DSC shows the characteristics of the mixture, the crystal transition temperature is that of diethylphosphinate aluminum, and the enthalpy value of the crystal transition decreases with the decrease in the ratio. On the other hand, in the case of the complex, at the same ratio, the characteristic crystal transition peak of diethylphosphinate aluminum disappears. Thus, the complex is not a mixture of both but a novel structure.

[0017] As a result of research, it was found that aluminum ethylbutylphosphinate-aluminum diethylphosphinate complex could be obtained regardless of the ratio of aluminum ethylbutylphosphinate and aluminum diethylphosphinate. As a result of further research, it was found that aluminum ethylbutylphosphinate could form aluminum complex salts with aluminum dialkylphosphinate, aluminum monoalkylphosphonite, inorganic aluminum phosphite, or could be complexed with various aluminum dialkylphosphinate, aluminum monoalkylphosphonite, inorganic aluminum phosphite, etc. to obtain phosphorus-containing aluminum salt complexes.

[0018] Surprisingly, when a small amount of phosphorus-containing aluminum salt complex is added to aluminum diethylphosphinate, the crystal transition of aluminum diethylphosphinate is obviously changed, the crystal transition temperature is decreased, the heat absorption / dissipation amount during the crystal transition is decreased, and it is also found that at a certain ratio, the crystal transition of aluminum diethylphosphinate disappears. Figure 6 is a DSC chart of the mixture (weight ratio 8:92) formed by adding the above-prepared aluminum ethylbutylphosphinate-aluminum diethylphosphinate complex to aluminum diethylphosphinate. As can be seen from this chart, when 8wt% of the complex is added, the crystal transition temperature of aluminum diethylphosphinate is decreased from 179°C to 171.3°C, and the crystal transition of aluminum diethylphosphinate is obviously changed and the crystal transition temperature is decreased. In addition, the research results showed that the higher the ratio of phosphorus-containing aluminum salt complex added, the lower the crystal transition temperature. When the content of the phosphorus-containing aluminum salt complex was increased to 30 wt%, the crystal transition of aluminum diethylphosphinate disappeared, that is, no crystal transition occurred within the temperature range under consideration. The DSC chart is shown in FIG. 7.

[0019] From these results, it is clear that the phosphorus-containing aluminum salt complex has a significant effect on the crystal transition process of aluminum diethylphosphinate, and the crystal transition is closely related to crystallization. Therefore, the present inventors proposed that the phosphorus-containing aluminum salt complex affects the crystallization process of producing aluminum diethylphosphinate, and further affects the particle size and distribution of the crystal particles.

[0020] As a result of research, it has been found that by adding phosphorus-containing aluminum salt complex during the preparation of aluminum diethylphosphinate, the phosphorus-containing aluminum salt complex can function as seed crystals, affect the crystallization process, and control the particle size and distribution of crystal particles, and more importantly, the content of fine powder can be reduced, the particle size can be increased, and the particle size distribution can be narrowed, so as to achieve the object of the present invention.As a result of research, it has been found that the phosphorus-containing aluminum salt complex has a molecular structure represented by formula (I).

[0021] Formula (I) shows a complex formed with other phosphorus-containing aluminum salts in the presence of aluminum ethylbutylphosphinate and aluminum diethylphosphinate, and the other phosphorus-containing aluminum salts include aluminum dialkylphosphinate / monoalkyl aluminum hypophosphite other than aluminum ethylbutylphosphinate and aluminum diethylphosphinate, monoalkyl aluminum phosphonite, inorganic aluminum phosphite, etc. Aluminum ethylbutylphosphinate and aluminum diethylphosphinate can form phosphorus-containing aluminum salt complexes with one or more of the other phosphorus-containing aluminum salts mentioned above.

[0022] The present invention also provides Step (1) of dissolving ethylbutylphosphinic acid and / or soluble ethylbutylphosphinic acid salt containing an anion moiety of structural formula (II) and other acids and / or soluble salts containing an anion moiety of structural formula (III) and / or structural formula (IV) involved in complexation (phosphorus-containing complexing anion donor) in water (which may or may not contain a small amount of strong acid), then adding an aluminum-containing compound (aluminum ion donor) and reacting at 80 to 90°C; and (2) a step of, after completion of the reaction, separating the solid from the liquid, washing and drying the solid, and then treating the solid at a high temperature of 180 to 450°C to obtain the phosphorus-containing aluminum salt complex.

[0023] In the above manufacturing method, The soluble salt is typically a sodium or potassium salt, The aluminum-containing compound is preferably at least one of aluminum sulfate, aluminum nitrate, aluminum chloride, aluminum hydroxide, and alumina; The washing is preferably ended when the conductivity of the washing water becomes lower than 500 μs / cm.

[0024] In step (1), the phosphorus-containing complexing anion donor and the aluminum ion donor may be added in an equimolar ratio to ensure complete reaction.

[0025] In step (1), the strong acid may include concentrated sulfuric acid, concentrated nitric acid, concentrated hydrochloric acid, and concentrated phosphoric acid, and the amount of the strong acid added may be 2% to 5% of the mass of the phosphorus-containing complexing anion donor.

[0026] When the aluminum-containing compound is insoluble in water, the aluminum-containing compound may be dispersed in water to form a suspended dispersion, in which case the aluminum-containing compound reacts with the phosphorus-containing complexing anion donor added in the form of an acid, and a high concentration of strong acid may not be present.When the aluminum-containing compound is a water-soluble compound, the reaction is preferably performed in the presence of a high concentration of strong acid, in which case the aluminum-containing compound may react with the phosphorus-containing complexing anion donor added in the form of a salt.

[0027] The concentration of the aluminum-containing compound in the reactants is preferably 15% by mass to 50% by mass.

[0028] In step (1), the reaction time may be from 1 to 5 hours.

[0029] In step (2), After the reaction is completed, a solid precipitate can be obtained by controlling the pH of the liquid phase to less than 4, and the pH control can be achieved by adding an alkali or a metal oxide, etc.

[0030] The drying may be performed using various ovens, drying chambers, dryers, etc., and the drying temperature may be 100-130°C. The high-temperature treatment is an important step in the manufacturing process, and the treatment process is related to the composition and proportion of the phosphorus-containing aluminum salt complex and the treatment amount. The temperature of the high-temperature treatment is an important factor of the high-temperature treatment. Research has shown that if the treatment temperature is less than 180°C, the phosphorus-containing aluminum salt complex of the present application cannot be obtained. The upper limit of the temperature of the high-temperature treatment is the decomposition temperature of the complex, which is usually less than 450°C. The high-temperature treatment process is as follows: the temperature is raised to 180-450°C over 0.5-10 hours, and the high-temperature treatment is performed for 1-300min.

[0031] The high temperature treatment process in step (2) may be carried out under an inert atmosphere (such as a nitrogen atmosphere or a rare gas atmosphere) or under vacuum conditions.

[0032] After step (2), if necessary, the resulting phosphorus-containing aluminum salt complex may be ground to a desired particle size.

[0033] Research has shown that in order to obtain the phosphorus-containing aluminum salt complex of the present invention, both steps of the preparation method are essential, that is, without high-temperature treatment (including a treatment temperature of less than 180°C), or by dry-mixing a part of the phosphorus-containing aluminum salt and then heat-treating it at a high temperature, the phosphorus-containing aluminum salt complex of the present invention cannot be obtained.

[0034] Hereinafter, the parameter conditions for the method for producing aluminum diethylphosphinate crystals having a low fine powder content of the present invention will be described in detail, and preferred embodiments will be described.

[0035] The phosphorus-containing aluminum salt complex has the structure shown in formula (I), and the molecular structure includes at least the complex of aluminum ethylbutylphosphinate and aluminum diethylphosphinate, and in addition, the complex may contain one or more other phosphorus-containing aluminum salts, and the obtained complexes can all affect the crystallization in the preparation of aluminum diethylphosphinate, effectively control the particle size and distribution of crystals, and also greatly reduce the content of fine powder.On the other hand, the phosphorus-containing aluminum salt complex that does not have the structure shown in formula (I) affects the crystallization process, but cannot greatly reduce the content of fine powder, and cannot achieve the object of the present application.

[0036] The water-soluble aluminum salt, soluble diethylphosphinate, may be charged in a stoichiometric molar ratio to the product aluminum diethylphosphinate.

[0037] The soluble diethylphosphinate may be a sodium salt, a potassium salt, or the like, and the concentration in the aqueous solution may be 20% by mass to 60% by mass.

[0038] Taking the theoretical mass of aluminum diethylphosphinate as the product to be 100%, the addition amount of the phosphorus-containing aluminum salt complex is preferably 0.01% to 10%, more preferably 0.1% to 5%. At an appropriate addition amount, it can effectively control the crystallization process and control the content of fine powder without causing a significant change in the crystal properties of aluminum diethylphosphinate. When the phosphorus-containing aluminum salt complex is added in excess, the effective reduction of the fine powder content cannot be further obtained, and it also significantly affects the crystal transition of aluminum diethylphosphinate, resulting in significantly different crystal properties of the obtained substance compared with pure aluminum diethylphosphinate, which is not the purpose of this application. When the addition amount of the phosphorus-containing aluminum salt complex is too low, the control effect of the phosphorus-containing aluminum salt complex is limited, and the purpose of this application to significantly reduce the content of fine powder cannot be achieved.

[0039] The average particle size D50 of the phosphorus-containing aluminum salt complex preferably satisfies 10μm < D50 < 50μm, more preferably 20μm < D50 < 40μm. As a result of research, the particle size of the phosphorus-containing aluminum salt complex affects the control effect on the crystallization process. If the particle size is too small or too large, the content of fine powder cannot be reduced, and the purpose of this application cannot be achieved.

[0040] The phosphorus-containing aluminum salt complex further contains at least one of the following components (A) to (C). (A) One or more non-complex salts of ethylbutylphosphinate, butylbutylphosphinate, ethylhexylphosphinate, butylhexylphosphinate, hexylhexylphosphinate (B) Alkyl phosphonite (C) One or more of sulfate, chloride, phosphate, phosphite, hypophosphite, nitrate, acetate, nitrogen-containing compound, iron-containing compound, calcium-containing compound, magnesium-containing compound, titanium-containing compound, sodium-containing compound, potassium-containing compound.

[0041] The presence of small amounts of the above components (A) to (C) does not affect the effectiveness of the crystallization process by the phosphorus-containing aluminum salt complex, and it is still possible to greatly reduce the content of fine powder.

[0042] The strong acid includes at least one of sulfuric acid, nitric acid, hydrochloric acid, phosphoric acid, and the like.

[0043] The amount of the strong acid added may be 1% to 5%, with the theoretical mass of the product aluminum diethylphosphinate being 100%.

[0044] The aluminum salt in the water-soluble aluminum salt solution preferably includes at least one of aluminum sulfate, aluminum nitrate, and aluminum chloride.

[0045] The concentration of the aluminum salt in the water-soluble aluminum salt solution in the reaction system is preferably 15% by mass to 50% by mass.

[0046] The reaction time may be from 1 to 5 hours.

[0047] After the reaction is completed, a solid precipitate can be obtained by controlling the pH of the liquid phase to less than 4, and the pH control can be achieved by adding an alkali or a metal oxide, etc.

[0048] The washing is preferably ended when the conductivity of the washing water becomes lower than 500 μs / cm.

[0049] The drying may be performed using various ovens, drying chambers, dryers, etc., and the drying temperature may be 100 to 130° C. The drying process in step (4) may be performed under an inert atmosphere (such as a nitrogen atmosphere or a rare gas atmosphere) or under vacuum conditions.

[0050] The aluminum diethylphosphinate crystals with a low content of fine powder produced by the present invention may contain one or more kinds of mixture impurities such as aluminum diethylphosphinate, aluminum ethylbutylphosphinate, aluminum butylbutylphosphinate, aluminum ethylhexylphosphinate, aluminum butylhexylphosphinate, and aluminum hexylhexylphosphinate.

[0051] The aluminum diethylphosphinate crystals with a low content of fine powder contain seed crystals of a phosphorus-containing aluminum salt complex, satisfy 20μm < D50 < 50μm for the average particle size D50, have a bulk density of 500 - 700 g / L, and have a content of fine powder with a particle size of less than 5μm of less than 10 wt%.

[0052] The present invention also provides aluminum diethylphosphinate crystals with a low content of fine powder produced by the above production method.

[0053] The present invention also provides the use of the aluminum diethylphosphinate crystals with a low content of fine powder in the flame retardancy of glass fiber reinforced engineering plastics.

[0054] The glass fiber reinforced engineering plastics may use at least one of polyurethane, thermoplastic elastomer, epoxy resin, thermosetting unsaturated polyester, nylon, thermoplastic polyester, and POK (polyketone) as the polymer matrix.

[0055] The aluminum diethylphosphinate crystals with a low content of fine powder are used as a flame retardant or a flame retardant synergist, in the flame retardancy of varnishes or foaming paints, in the flame retardancy of wood or products containing cellulose, and can be used in the production of flame retardant polymer molding materials, flame retardant polymer films, and flame retardant polymer fibers.

[0056] In the above-mentioned flame-retardant polymer molding material, flame-retardant polymer film, and flame-retardant polymer fiber, the composition of the raw materials, taking the total mass as 100%, is preferably: It comprises 55%-99.9% polymer matrix, 0.1%-45% flame retardant, 0-44.9% filler or reinforcing material, and 0-44.9% additives.

[0057] The flame retardant system comprises: The composition contains 1% by mass to 100% by mass of the aluminum diethylphosphinate crystals having a low content of fine powder, and 0% to 99% by mass of other flame retardant synergists.

[0058] In the flame retardant system, other flame retardants, flame retardant synergists are dialkylphosphinic acids and / or their salts; condensation products of melamine and / or reaction products of melamine with phosphoric acid and / or reaction products of condensation products of melamine with polyphosphoric acid or mixtures thereof; nitrogen-containing phosphates; benzoguanamine, tris(hydroxyethyl)isocyanurate, allantoin, glycoluril, melamine, melamine cyanurate, dicyandiamide and / or guanidine; magnesium oxide, calcium oxide, alumina, zinc oxide, manganese oxide, tin oxide, aluminum hydroxide, boehmite, dihydrotalcite, hydrocalumite, magnesium hydroxide, calcium hydroxide, zinc hydroxide, tin oxide hydrate, manganese hydroxide, zinc borate, alkali zinc silicate and / or zinc stannate; phosphites, hydrogen phosphites or condensates thereof; phosphates and derivatives thereof; Melam, melem, melon, dimelamine pyrophosphate, melamine polyphosphate, melam polyphosphate, melon polyphosphate and / or melem polyphosphate and / or mixed polysalts thereof and / or ammonium hydrogen phosphate, ammonium dihydrogen phosphate and / or ammonium polyphosphate; The phosphinic acid may be selected from aluminum hypophosphite, zinc hypophosphite, calcium hypophosphite, sodium phosphite, monophenylphosphinic acid and its salts, mixtures of dialkylphosphinic acids and their salts with monoalkylphosphinic acids and their salts, 2-carboxyethylalkylphosphinic acids and their salts, 2-carboxyethylmethylphosphinic acid and its salts, 2-carboxyethylarylphosphinic acids and their salts, 2-carboxyethylphenylphosphinic acid and its salts, and an adduct of DOPO and its salts with p-benzoquinone. Effect of the Invention

[0059] Compared with the prior art, the main advantages of the present invention are: The method for preparing aluminum diethylphosphinate according to the present invention overcomes the defects of the conventional methods. The prepared aluminum diethylphosphinate has particle characteristics of low fine powder content, large particle size and narrow distribution, which solves the flowability problems such as easy bridging and blockage, and can be directly applied to the processing of halogen-free flame-retardant glass fiber reinforced engineering plastics, and can realize long-term operation. [Brief description of the drawings]

[0060] [Figure 1] Molecular structure of the aluminum ethylbutylphosphinate(0.7)-aluminum diethylphosphinate(0.3) complex. [Diagram 2] 2 is a DSC chart of the ethylbutylphosphinate aluminum-diethylphosphinate aluminum complex shown in FIG. 1. [Diagram 3] 1 is a DSC chart of a mixture of aluminum ethylbutylphosphinate and aluminum diethylphosphinate (molar ratio 0.7:0.3). [Figure 4] 1 is a DSC chart of aluminum ethylbutylphosphinate. [Diagram 5] 1 is a DSC chart of aluminum diethylphosphinate. [Figure 6]1 is a DSC chart of aluminum diethylphosphinate to which 8% of a phosphorus-containing aluminum salt complex has been added (based on the total mass of the phosphorus-containing aluminum salt complex, aluminum diethylphosphinate being 100%). [Figure 7] 1 is a DSC chart of aluminum diethylphosphinate to which 30% of a phosphorus-containing aluminum salt complex has been added (with the total mass of the phosphorus-containing aluminum salt complex, aluminum diethylphosphinate, being 100%). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0061] The present invention will be further described below with reference to the accompanying drawings and specific examples. It should be understood that these examples are only used to explain the present invention and are not used to limit the scope of the present invention. In the following examples, the operation method without specific conditions is usually according to normal conditions or conditions proposed by the manufacturer. Synthesis of the aluminum ethylbutylphosphinate(0.2)-aluminum diethylphosphinate(0.8) complex

[0062] The molecular structure of the ethylbutylphosphinate aluminum(0.2)-diethylphosphinate aluminum(0.8) complex is shown below. [ka] manufacturing process

[0063] In a 2L reaction kettle, 34.4g (0.2mol) of sodium ethylbutylphosphinate and 115.2g (0.8mol) of sodium diethylphosphinate were dissolved in 381.7g of water, and the mixture was obtained by stirring thoroughly. In a 500mL beaker, 57g of aluminum sulfate was dissolved in 133g of water, and then 4.0g of concentrated sulfuric acid with a concentration of 98wt% was added to the aluminum sulfate solution, and the mixture was stirred thoroughly to mix uniformly, and then transferred to a dripping funnel. The reaction kettle was heated to 90°C, and the sulfuric acid-containing aluminum sulfate solution was dripped over 2 hours, and the reaction was continued for 1 hour while keeping the temperature. The mixture was filtered while hot, and the precipitate was washed several times. When the conductivity of the washing water became less than 200μs / cm, the washing was stopped. The material was transferred to an oven, heated to 120°C, and dried for 60 min. When the moisture content of the solid matter reached 0.1 wt%, the temperature was raised to 180°C at a rate of 2°C / min, held for 60 min, then heated to 320°C at 1°C / min, held for 30 min, cooled to room temperature, and the material was removed to obtain an ethylbutylphosphinate aluminum (0.2)-diethylphosphinate aluminum (0.8) complex, designated as Complex-1. The material was pulverized to an average particle size D50 of 38.0 μm. By referring to the above-mentioned production process, other complexes were obtained by changing the types and molar ratios of raw materials.

[0064] Complex-2: ethylbutylphosphinate aluminum (0.3)-diethylphosphinate aluminum (0.7) complex, average particle size after grinding D50 35.2 μm. Complex-3: aluminum ethylbutylphosphinate (0.2)-aluminum diethylphosphinate (0.7)-aluminum ethylhexylphosphinate (0.1) complex, average particle size after grinding D50 36.1 μm. Complex-4: aluminum ethylbutylphosphinate (0.2)-aluminum diethylphosphinate (0.7)-aluminum phosphite (0.1) complex, average particle size after grinding D50 37.4 μm. Complex-5: aluminum ethylbutylphosphinate (0.2)-aluminum diethylphosphinate (0.7)-aluminum ethylphosphonite (0.1) complex, average particle size after grinding D50 35.8 μm. Complex-6: aluminum ethylbutylphosphinate (0.2)-aluminum diethylphosphinate (0.7)-aluminum ethylhexylphosphinate (0.05)-aluminum phosphite (0.05) complex, average particle size after grinding D50 38.5 μm. Complex-7: aluminum ethylbutylphosphinate (0.2)-aluminum diethylphosphinate (0.7)-aluminum ethylhexylphosphinate (0.05)-aluminum ethylphosphonite (0.05) complex, average particle size after grinding D50 37.6 μm. Complex-8: aluminum ethylbutylphosphinate (0.2)-aluminum diethylphosphinate (0.7)-aluminum ethylphosphonite (0.05)-aluminum phosphite (0.05) complex, average particle size after grinding D50 37.0 μm. Complex-9: aluminum ethylbutylphosphinate (0.2)-aluminum diethylphosphinate (0.65)-aluminum ethylhexylphosphinate (0.05)-aluminum ethylphosphonite (0.05)-aluminum phosphite (0.05) complex, average particle size after grinding D50 38.4 μm. Complex-10: ethylbutylphosphinate aluminum (0.7)-diethylphosphinate aluminum (0.3) complex, average particle size after grinding D50 37.7 μm. Aluminum diethylphosphinate, LFR-8003, average particle size D50 39.2μm, manufactured by Jiangsu Lisit New Materials Co., Ltd. Aluminum ethylbutylphosphinate, average particle size D50 42.6μm, self-made. Example 1 manufacturing process

[0065] In a 2L reaction kettle, 144g (1mol) of sodium diethylphosphinate was dissolved in 336g of water, and the solution was obtained by stirring thoroughly. Next, 12.6g (2wt%) of complex-1 was added, and the complex was uniformly dispersed in the solution. In a 500mL beaker, 57g of aluminum sulfate was dissolved in 133g of water, and then 3.0g of concentrated sulfuric acid with a concentration of 98wt% was added to the aluminum sulfate solution, and the solution was mixed thoroughly and uniformly, and then transferred to a dropping funnel. The reaction kettle was heated to 90°C, and the sulfuric acid-containing aluminum sulfate solution was dropped over 2 hours, and the reaction was continued for 1 hour while keeping the temperature. The solution was filtered while hot, and the precipitate was washed several times. When the conductivity of the washing water became smaller than 200μs / cm, the washing was stopped. The material was transferred to an oven, heated to 120°C, and dried for 60 minutes. When the moisture content of the solid reached 0.1 wt%, the temperature was lowered to room temperature and the material was taken out to obtain aluminum diethylphosphinate. The particle size was tested and the results are shown in Table 1. Particle size test method: Tested using a laser particle size distribution analyzer. The powder was dispersed in a 95 vol% ethanol solution and processed with ultrasonic treatment to obtain the particle size and distribution results, and the content of fine powder less than 5 μm was statistically calculated. Example 2

[0066] The procedure was almost the same as in Example 1, except that the amount of Complex-1 added was changed to 5.2 g (4 wt%), and the remaining conditions were the same. The results are shown in Table 1. Example 3

[0067] The procedure was almost the same as in Example 1, except that the average particle size of the added complex-1 was changed to 25 μm, and the remaining conditions were the same. The results are shown in Table 1. Example 4

[0068] The procedure was almost the same as in Example 1, except that the same mass of Complex-2 was added, and the remaining conditions were the same. The results are shown in Table 1. Comparative Example 1

[0069] The procedure was almost the same as in Example 1, except that no complex was added, and the remaining conditions were the same. The results are shown in Table 1.

[0070] Comparative Example 2 The procedure was almost the same as in Example 1, except that the same mass of aluminum diethylphosphinate was added instead of Complex-1, and the remaining conditions were the same. The results are shown in Table 1.

[0071] Comparative Example 3 The procedure was almost the same as in Example 1, except that the same mass of aluminum ethylbutylphosphinate was added instead of Complex-1, and the remaining conditions were the same. The results are shown in Table 1. Comparative Example 4

[0072] The procedure was almost the same as in Example 1, except that the same mass of a mixture of aluminum ethylbutylphosphinate and aluminum diethylphosphinate (molar ratio 0.2:0.8) was added instead of Complex-1, and the remaining conditions were the same. The results are shown in Table 1. Comparative Example 5

[0073] The procedure was almost the same as in Example 1, except that the average particle size of the added complex-1 was 5 μm, and the remaining conditions were the same. The results are shown in Table 1. Comparative Example 6

[0074] The procedure was almost the same as in Example 1, except that 0.01 g of complex-1 was added, and the remaining conditions were the same. The results are shown in Table 1. Comparative Example 7

[0075] The procedure was almost the same as in Example 1, except that the same mass of Complex-10 was added, and the remaining conditions were the same. The results are shown in Table 1. [Table 1] The results clearly show that the particles obtained using the phosphorus-containing aluminum salt complex of the present application have a larger particle size, a narrower distribution, and a significantly reduced content of fines. Example 5

[0076] The procedure was almost the same as in Example 1, except that the same mass of Complex-3 was added, and the remaining conditions were the same. The results are shown in Table 2. Example 6

[0077] The procedure was almost the same as in Example 1, except that the same mass of Complex-4 was added, and the remaining conditions were the same. The results are shown in Table 2. Example 7

[0078] The procedure was almost the same as in Example 1, except that the same mass of Complex-5 was added, and the remaining conditions were the same. The results are shown in Table 2. Example 8

[0079] The procedure was almost the same as in Example 1, except that the same mass of Complex-6 was added, and the remaining conditions were the same. The results are shown in Table 2. Example 9

[0080] The procedure was almost the same as in Example 1, except that the same mass of Complex-7 was added, and the remaining conditions were the same. The results are shown in Table 2. Example 10

[0081] The procedure was almost the same as in Example 1, except that the same mass of Complex-8 was added, and the remaining conditions were the same. The results are shown in Table 2. Example 11

[0082] The procedure was almost the same as in Example 1, except that the same mass of Complex-9 was added, and the remaining conditions were the same. The results are shown in Table 2. [Table 2] It is clear from the results in Table 2 that the multi-element phosphorus-containing aluminum salt complex of aluminum ethylbutylphosphinate and aluminum diethylphosphinate can have a similar effect on the crystallization process in the preparation of aluminum diethylphosphinate, and can obtain aluminum diethylphosphinate crystals with a low fine powder content, large particle size and narrow particle size distribution. Example 12

[0083] The procedure was almost the same as in Example 1, except that 2.5 g of Complex-1 and 0.1 g of aluminum ethylbutylphosphinate were added, and the remaining conditions were the same. The results are shown in Table 3. Example 13

[0084] The procedure was almost the same as in Example 1, except that 2.5 g of Complex-1 and 0.1 g of aluminum phosphonite were added, and the remaining conditions were the same. The results are shown in Table 3. Example 14

[0085] The procedure was almost the same as in Example 1, except that 2.5 g of Complex-1 and 0.1 g of aluminum phosphate were added, and the remaining conditions were the same. The results are shown in Table 3. [Table 3] It is clear from the results in Table 3 that the phosphorus-containing aluminum salt complex of the present invention does not affect the control of the crystallization process in the production of aluminum diethylphosphinate by the method of the present invention even if a small amount of other non-complex salts are present. Uses of Aluminum Diethylphosphinate Example 15

[0086] Using 50%wt high temperature nylon PPA, 30%wt glass fiber, and 20%wt aluminum diethylphosphinate produced in Example 1, flame retardant glass fiber reinforced PPA was produced according to a prescribed process, and the situation when it was operated continuously for 10 hours was considered. Also, a sample was produced and flame retardancy was tested. As a result, even after 10 hours of operation, it did not stop due to failure such as bridging, and the flame retardancy of the material reached UL94 V0 (0.8mm). Comparative Example 8

[0087] Using 50%wt high temperature nylon PPA, 30%wt glass fiber, and 20%wt aluminum diethylphosphinate produced in Comparative Example 1, flame retardant glass fiber reinforced PPA was produced according to a prescribed process, and the situation when it was operated continuously for 10 hours was considered. Also, samples were produced and flame retardancy was tested. As a result, when it was operated for 10 hours, it stopped three times due to failure such as bridging, and the flame retardancy of the material reached UL94 V0 (0.8mm).

[0088] From the above results, it is clear that the aluminum diethylphosphinate produced by the method of the present invention does not stop due to failure such as bridging, and maintains its flame retardancy.

[0089] Furthermore, it should be understood that, after reading the above description of the invention, one skilled in the art may make various changes or modifications to the invention, and that equivalent forms thereof are also included in the scope defined by the claims of this application.

Claims

1. A method for producing aluminum diethylphosphinate crystals having a low content of fine powder, comprising the steps of: The method includes the steps of: uniformly dispersing a phosphorus-containing aluminum salt complex as seed crystals in an aqueous solution of a soluble diethylphosphinate salt; then adding a water-soluble aluminum salt solution containing a strong acid; reacting at 70-95°C; and washing and drying the solid product after the reaction is completed to obtain the aluminum diethylphosphinate crystals having a low content of fine powder; The phosphorus-containing aluminum salt complex has a structure represented by the following formula (I): The amount of the phosphorus-containing aluminum salt complex added is 0.01% to 10%, based on the theoretical mass of the product aluminum diethylphosphinate being 100%; The method for producing the phosphorus-containing aluminum salt complex, wherein the average particle size of the phosphorus-containing aluminum salt complex satisfies 10 μm<D50<50 μm. 【Chemistry 1】 (In formula (I), a, b, c, d, and e are all molar ratios, a is 0.1 to 0.5, b is 0.5 to 0.9, c, d, and e are 0 to 0.3, and a+b+c+d+e=1; R 1 , R 2 are each independently selected from H and C1-C6 alkyl, and R 1 , R 2 When either one of R is ethyl, the other is not ethyl and butyl. 3 is C1 to C6 alkyl.

2. 2. The method according to claim 1, wherein the amount of the phosphorus-containing aluminum salt complex added is 0.1% to 5%, based on the theoretical mass of the product aluminum diethylphosphinate being 100%.

3. 2. The method according to claim 1, wherein the average particle diameter D50 of the phosphorus-containing aluminum salt complex satisfies 20 μm<D50<40 μm.

4. The method according to claim 1, wherein the phosphorus-containing aluminum salt complex further contains at least one of the following components (A) to (C): (A) one or more non-complex salts of ethylbutylphosphinate, butylbutylphosphinate, ethylhexylphosphinate, butylhexylphosphinate, and hexylhexylphosphinate (B) Alkyl phosphonite (C) one or more of sulfates, chlorides, phosphates, phosphites, hypophosphites, nitrates, acetates, nitrogen-containing compounds, iron-containing compounds, calcium-containing compounds, magnesium-containing compounds, titanium-containing compounds, sodium-containing compounds, and potassium-containing compounds.

5. The strong acid includes at least one of sulfuric acid, nitric acid, hydrochloric acid, and phosphoric acid, 2. The method according to claim 1, wherein the amount of the strong acid added is 1% to 5% of the theoretical mass of the product aluminum diethylphosphinate, which is taken as 100%.

6. 2. The method according to claim 1, wherein the aluminum salt in the water-soluble aluminum salt solution contains at least one of aluminum sulfate, aluminum nitrate, and aluminum chloride.

7. The method according to claim 1, characterized in that the produced aluminum diethylphosphinate crystals with a low content of fine powder contain one or more mixture impurities selected from the group consisting of aluminum diethylphosphinate, aluminum ethylbutylphosphinate, aluminum butylbutylphosphinate, aluminum ethylhexylphosphinate, aluminum butylhexylphosphinate, and aluminum hexylhexylphosphinate.

8. The method according to claim 1, characterized in that the aluminum diethylphosphinate crystals having a low content of fine powder contain seed crystals of a phosphorus-containing aluminum salt complex, have an average particle size D50 that satisfies 20 μm<D50<50 μm, a bulk density of 500-700 g / L, and have a content of fine powder having a particle size of less than 5 μm of less than 10 wt %.

9. 9. Aluminum diethylphosphinate crystals having a low content of fine powder, produced by the method according to any one of claims 1 to 8.

10. 10. Use of the aluminum diethylphosphinate crystal with a low fine powder content as claimed in claim 9 in making glass fiber reinforced engineering plastics flame retardant, characterized in that the glass fiber reinforced engineering plastics have at least one of polyurethane, thermoplastic elastomer, epoxy resin, thermosetting unsaturated polyester, nylon, thermoplastic polyester, and POK as a polymer matrix.

Citation Information

Patent Citations

  • Aluminum diethyl phosphinate material and preparation method thereof

    CN111808133A

  • Polydialkyl phosphinic acid metal composite salt and / or mixture thereof, and uses thereof

    CN111825883A

  • Dialkyl phosphinic acid-aluminum phosphite composite salt and preparation method and application thereof

    CN112876736A

  • Dialkylphosphinic acid-alkylphosphite metal composite salt, and preparation method therefor and use thereof

    WO2020177559A1