Manufacturing method of copper alloy sheet material for automobiles or electric / electronic parts having excellent strength, electrical conductivity and bending workability, and copper alloy sheet material manufactured therefrom
A copper alloy sheet material with optimized nickel, cobalt, silicon, and chromium composition, along with controlled processing, addresses the limitations of existing alloys by achieving high strength, conductivity, and bending workability, suitable for automotive and electronic parts.
Patent Information
- Application Number
- JP2024521208
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-29
- Filing Date
- 2022-10-11
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2042-10-11
AI Technical Summary
Existing copper-nickel-silicon alloys used in automobiles and electronic parts lack sufficient strength, electrical conductivity, and bending workability due to issues with the addition of elements like nickel and cobalt, which increase strength but decrease conductivity, and the formation of coarse inclusions during casting and rolling.
A manufacturing method for a copper alloy sheet material using specific compositions of nickel, cobalt, silicon, tin, chromium, and other impurities, combined with controlled processing steps such as hot rolling, intermediate heat treatment, and two-stage aging treatment, to achieve optimal grain size and texture for improved strength, conductivity, and bending workability.
The method produces a copper alloy sheet material with tensile strength of 850 MPa or more, electrical conductivity of 40% IACS or more, and bending workability of R/t≦1.0, ensuring reliability and performance in automotive and electronic applications.
Smart Images

Figure 2024538740000001 
Figure 2024538740000002 
Figure 2024538740000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a copper alloy sheet material for automobiles or electric / electronic parts having excellent strength, electrical conductivity and bending workability, and the copper alloy sheet material produced therefrom, and in particular to a method for producing a copper-nickel-cobalt-silicon (Cu-Ni-Co-Si)-based copper alloy sheet material and the copper alloy sheet material produced therefrom. [Background technology]
[0002] Copper alloy materials used in automobiles or electrical / electronic parts require good electrical conductivity to suppress Joule heat generation caused by current flow, and high strength to withstand stresses applied during device assembly or operation. In addition, automobiles or electrical / electronic parts are usually manufactured in the form of copper alloy sheets and shaped by bending, so excellent bendability is also required.
[0003] From the viewpoint of high strength and high electrical conductivity, the use of precipitation hardened copper alloys has been increasing as copper alloys for automobiles or electrical / electronic parts, instead of conventional solid solution hardened copper alloys such as phosphor bronze and brass. In precipitation hardened copper alloys, the fine precipitates are uniformly dispersed by aging the solution-treated supersaturated solid solution, which increases the strength of the alloy and reduces the amount of solid solution elements in the copper, improving the electrical conductivity. As a result, a material with excellent mechanical properties such as strength and elasticity and good electrical conductivity, i.e., thermal conductivity, can be obtained.
[0004] Among precipitation hardened copper alloys, Cu-Ni-Si copper alloys, commonly known as Corson alloys, are representative copper alloys with relatively high electrical conductivity, strength and bending workability, with a tensile strength of 700MPa and an electrical conductivity of 40%IACS, and are currently being actively developed in the industry. Corson alloys can improve strength and electrical conductivity by precipitating fine Ni-Si intermetallic compounds in the copper matrix. However, since the strength is insufficient when applied to automobiles or electrical and electronic parts, measures such as increasing the content of nickel (Ni) and silicon (Si) or adding magnesium (Mg) have been taken, but the addition of additional elements increases the strength but reduces the conductivity. Recently, copper-nickel-cobalt-silicon (Cu-Ni-Co-Si) alloys, in which part of the Ni in Corson alloys is replaced with Co, have been actively developed. However, the physical properties required for materials for electrical and electronic parts are significantly insufficient.
[0005] In Korean Patent Publication No. 10-2009-0122303, the size and distribution of the second phase of a copper-nickel-cobalt-silicon (Cu-Ni-Co-Si) alloy is controlled to improve bendability, but the final physical properties are only tensile strength of 800 MPa and electrical conductivity of 40% IACS.
[0006] In Korean Patent Publication No. 10-2014-0056003, the content of nickel (Ni), cobalt (Co) and silicon (Si) was increased to ensure strength, and the distribution of precipitates and the orientation of crystals were controlled to ensure physical properties of a yield strength of 950 MPa and electrical conductivity of 40% IACS. However, in actual alloy production, if the total content of nickel (Ni) and cobalt (Co) exceeds 3.5% by weight, there is a high probability of cracks occurring during hot rolling due to the coarse inclusions formed inside the ingot during casting. In addition, while the nickel (Ni) and cobalt (Co) content is increased to ensure strength, the bending workability is significantly low, making it highly likely that cracks will occur during part processing, making it unsuitable as a material for electrical and electronic parts. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention provides a method for producing a copper alloy sheet material for automobiles or electric / electronic parts, which has excellent strength, electrical conductivity and bending workability, and a copper alloy sheet material produced by the method. [Means for solving the problem]
[0008] The present invention is directed to a sintered body comprising, by weight percent, 1.5-3.4% nickel (Ni), 0.1-1.5% cobalt (Co), 0.3-1.2% silicon (Si), 0.1-0.8% tin (Sn), 0.01-0.45% chromium (Cr), the balance being copper (Cu), and unavoidable impurities of a total amount of 0.4% or less, the unavoidable impurities being selected from the group consisting of Mg, Al, P, Ca, Ti, V, Zn, Fe, Zr, and Mn. A method for producing one or more copper alloy sheet materials for automobiles or electric / electronic parts, the method comprising the steps of: melting and casting 1.5-3.4% nickel (Ni), 0.1-1.5% cobalt (Co), 0.3-1.2% silicon (Si), 0.1-0.8% tin (Sn), 0.01-0.45% chromium (Cr), the balance being copper (Cu) and a total of 0.4% or less of unavoidable impurities to obtain an ingot; The method for producing a copper alloy sheet material for automobiles and electric / electronic parts includes the steps of hot rolling the obtained ingot in a temperature range of 900°C to 1040°C; first cold rolling the sheet material obtained in the previous step with a rolling reduction of 50% or more; intermediate heat treating the sheet material obtained in the previous step at 400°C to 800°C for 1 to 300 minutes; second cold rolling the sheet material obtained in the previous step with a rolling reduction of 70% to 90%; solution treating the sheet material obtained in the previous step at a temperature of 820°C to 1000°C for 20 to 300 seconds; finish cold rolling the sheet material obtained in the previous step with a rolling reduction of 10% to 50%; and two-stage aging treatment of aging the product obtained in the previous step at a temperature of 440°C to 600°C for 5 minutes to 300 minutes, and then aging treatment at a temperature of 350°C to 440°C for 1 hour to 30 hours.
[0009] In the above-mentioned preparation method, the contents of Ni, Co and Si satisfy 3.5≦(Ni+Co) / Si≦4.5.
[0010] In the above preparation method, the Ni and Co contents satisfy Ni+Co≦3.5.
[0011] The solution heat treated plate material simultaneously satisfies the following formulas:
[0012] 5 ≦ Grain size (μm) XI{200} / (I{111}+I{220}+I{311}) ≦ 60
[0013] 2 ≦ Grain size (μm) - I{200} / (I{111}+I{220}+I{311}) ≦ 19
[0014] Here, I{111}, I{200}, I{220}, and I{311} are the diffraction integrated intensities of the diffraction peaks of each crystal plane measured by X-ray diffraction.
[0015] In the above manufacturing method, the plate material obtained in the previous step is cooled at a rate of 20 to 40° C. / s after the solution treatment.
[0016] In the above manufacturing method, the number of passes during the second cold rolling is 5 to 10.
[0017] The present invention provides a copper alloy sheet material for automobiles and electric / electronic parts, which is produced by the above-mentioned method for producing a copper alloy material of the present invention.
[0018] The copper alloy sheet has a tensile strength of 850 MPa or more, bending workability of R / t≦1.0 (180° bending) in both the rolling method and the right-angle method, and an electrical conductivity of 40% IACS or more. Effect of the Invention
[0019] The present invention provides a method for producing a copper alloy sheet material for automobiles or electric / electronic parts, which has excellent strength, electrical conductivity and bending workability, and a copper alloy sheet material produced by the method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] In this specification, when a content is indicated as %, it means % by weight unless otherwise specified.
[0021] The present invention provides a method for producing a copper alloy sheet for automobiles or electric / electronic parts, which has improved strength, electrical conductivity, and bending workability, and a copper alloy sheet for automobiles or electric / electronic parts produced therefrom. Hereinafter, the method for producing a copper alloy sheet for electric / electronic parts according to the present invention and the copper alloy sheet for electric / electronic parts produced therefrom will be described in order.
[0022] The method for producing a copper alloy sheet material according to the present invention comprises, by weight percent, 1.5 to 3.4% nickel (Ni), 0.1 to 1.5% cobalt (Co), 0.3 to 1.2% silicon (Si), 0.1 to 0.8% tin (Sn), 0.01 to 0.45% chromium (Cr), the balance being copper (Cu), and unavoidable impurities of a total amount of 0.4% or less, the unavoidable impurities being Mg, Al, P, Ca, Ti, V, Zn, Fe, Zr, and Mn. A method for producing a copper alloy sheet material for automobiles or electric / electronic parts, which is one or more selected from the group consisting of nickel (Ni), cobalt (Co), silicon (Si), tin (Sn), tin (Sn), chromium (Cr), copper (Cu), and unavoidable impurities of a total amount of 0.4% or less, by melting and casting the material to obtain an ingot; The method includes the steps of hot rolling the obtained ingot in the temperature range of 900°C to 1040°C; primary cold rolling the plate material obtained in the previous step with a rolling reduction of 50% or more; intermediate heat treatment of the plate material obtained in the previous step at 400°C to 800°C for 1 minute to 300 minutes; secondary cold rolling of the plate material obtained in the previous step with a rolling reduction of 70% to 90%; solution treatment of the plate material obtained in the previous step at a temperature of 820°C to 1000°C for 20 seconds to 300 seconds; finish cold rolling the plate material obtained in the previous step with a rolling reduction of 10% to 50%; and a two-stage aging treatment step of aging the product obtained in the previous step at a temperature of 440°C to 600°C for 5 minutes to 300 minutes, and then aging treatment at a temperature of 350°C to 440°C for 1 hour to 30 hours.
[0023] First, the composition ranges of the component elements of the copper alloy sheet material according to the present invention are as follows:
[0024] (a) Nickel (Ni): 1.5-3.4%
[0025] Ni is an element that forms (Co, Ni)2Si precipitates and improves the strength and electrical conductivity properties of copper alloy sheet materials. To fully exert this effect, the Ni content is set to 1.5% or more. On the other hand, excessive Ni content forms precipitates, and Ni remaining in solid solution in the matrix can cause a decrease in electrical conductivity or the formation of coarse precipitates that can cause collapse during bending, so the Ni content is limited to a range of 3.4% or less.
[0026] (b) Cobalt (Co): 0.1-1.5%
[0027] Co is an element that forms (Co,Ni)2Si-based precipitates, improves the strength and electrical conductivity of the copper alloy sheet material, has a high precipitation temperature, and improves the precipitation driving force at high temperatures. In order to fully exert this effect, it is preferable to ensure a Co content of 0.1% or more. However, if the amount is excessive, Co that cannot form precipitates with Si becomes an impurity that exists in a solid solution state in the copper matrix, or forms coarse precipitates at high temperatures, which has the effect of reducing the strength and electrical conductivity, so it is preferable to control it to 1.5% or less.
[0028] (c) Silicon (Si): 0.3~1.2%
[0029] Si is an element necessary for the formation of (Co, Ni)2Si-based precipitates. In the copper alloy sheet material according to the present invention, Ni, Co and Si in the alloy do not all become precipitates by aging treatment, but exist in a solid solution state in the parent phase to some extent. Ni, Co and Si in the solid solution state improve the strength of the copper alloy slightly, but the effect is smaller than that in the precipitated state, and they also cause a decrease in electrical conductivity. Therefore, the Si content is preferably in the range of 0.3 to 1.2%.
[0030] (d) Tin (Sn): 0.1-0.8%
[0031] The present inventors have found that Sn has the effect of increasing the strength during the final aging treatment by decreasing the temperature at which the supersaturated solid solution of the alloy is formed. The precipitation hardening alloy is an alloy that ensures strength and electrical conductivity by forming a supersaturated solid solution by cooling after solution treatment in which the additive elements are dissolved in the copper matrix, and then precipitating the dissolved elements in fine size with a uniform distribution by proceeding with aging treatment. Therefore, the more additive elements are dissolved in the copper matrix, the more the distribution of precipitates increases during aging treatment, and the effect of precipitation increases. In the copper alloy sheet material according to the present invention, the tin content of 0.1 to 0.8% reduces the temperature at which the supersaturated solid solution is formed by about 20°C compared to a copper-nickel-cobalt-silicon (Cu-Ni-Co-Si) alloy without tin. In other words, when solution treatment is performed at the same temperature, an alloy to which Sn is added can dissolve more elements, which results in a higher strength after aging treatment. If tin is added in an amount less than 0.1%, the effect of increasing the solid solubility is not obtained, and if it exceeds 0.8%, a large amount of tin remains in the matrix, making it impossible to ensure sufficient electrical conductivity.
[0032] (e) Chromium (Cr): 0.01-0.45%
[0033] The present inventors have found that chromium (Cr) has an excellent effect of increasing electrical conductivity. In the case of precipitation hardening alloys such as copper-nickel-silicon (Cu-Ni-Si) and copper-nickel-cobalt-silicon (Cu-Ni-Co-Si) alloys, elements dissolved in the matrix are expelled from the matrix by long-term aging treatment after solution treatment to form precipitates, thereby increasing electrical conductivity. At this time, since the precipitates are formed at an equilibrium fraction for a given aging treatment temperature, it is necessary to reduce the equilibrium temperature of copper in order to further increase electrical conductivity.
[0034] When chromium (Cr) is added at 0.01 to 0.45%, Cr reacts with Si even at low temperatures to form Cr-Si precipitates, which can expel even more Si remaining in the matrix. In other words, the addition of Cr can further reduce the solid solubility of copper in the temperature range of aging treatment, and has the effect of increasing electrical conductivity. When Cr is added at less than 0.01%, the effect of reducing the solid solubility of copper in the temperature range of aging treatment cannot be obtained, and when added at more than 0.45%, the intrinsic property of Cr elements solidifying with each other causes them to grow as coarse inclusions, and the desired strength cannot be obtained.
[0035] (f) Weight ratio of Ni, Co, and Si: 3.5≦(Ni+Co) / Si≦4.5
[0036] Even if the Ni, Co, and Si are controlled within the above-mentioned ranges, unless the optimum weight ratio for forming intermetallic compounds is provided, the precipitates cannot be formed sufficiently, and therefore the maximum strength and electrical conductivity cannot be obtained. The best strength and electrical conductivity can be obtained when the ratio of Ni, Co, and Si satisfies the following relational formula.
[0037] 3.5≦(Ni+Co) / Si≦4.5
[0038] Even if the above-mentioned ranges of the contents of the elements Ni, Co, and Si are satisfied, if the above-mentioned relational expressions are not satisfied, it is not possible to simultaneously obtain a tensile strength of 850 MPa or more, an electrical conductivity of 40% IACS or more, and a bending workability of R / t≦1.0. If the ratio of (Ni+Co) / Si is less than 3.5, Si is over-dissolved in the matrix, resulting in a decrease in strength, electrical conductivity, and bending workability, and conversely, if it exceeds 4.5, Ni and Co are over-dissolved, preventing a high fraction of precipitates from being obtained.
[0039] (g) Ni+Co≦3.5
[0040] Even if the above-mentioned (Ni+Co) / Si ratio is satisfied, if the above-mentioned relational expression is not satisfied, it is not possible to ensure a tensile strength of 850 MPa or more and an electrical conductivity of 40% IACS or more. If the Ni+Co content exceeds 3.5, coarse crystals are formed during casting, and cracks are likely to occur during hot rolling, and excessive Ni and Co are over-dissolved in the matrix, resulting in a decrease in electrical conductivity.
[0041] (h) Inevitable impurities
[0042] In the copper alloy sheet according to the present invention, the unavoidable impurities are elements that can be selectively contained. The copper alloy sheet according to the present invention can contain one or more elements selected from the group consisting of Mg, Al, P, Ca, Ti, V, Zn, Fe, Zr and Mn as impurities in a total amount of 0.4% by weight or less. Specifically, Ti has the effect of preventing the aggregation of crystallized particles that are inevitably generated during casting and solidification, thereby suppressing the formation of coarse crystallized particles, Mg has the effect of improving the stress relaxation resistance, and Zn and Fe have the effect of improving the solderability and castability of the copper alloy sheet. Al, V and Zr have the effect of improving the strength. P and Ca have a deoxidizing effect and are advantageous in improving hot workability.
[0043] However, if the total amount of the above-mentioned impurities in the copper alloy sheet material of the present invention exceeds 0.4% by weight, side cracks are caused during hot working, so it is necessary to control the amount to 0.4% by weight or less.
[0044] As described above, the method for producing a copper alloy sheet material according to the present invention includes the steps of: (1) melting and casting 1.5-3.4% nickel (Ni), 0.1-1.5% cobalt (Co), 0.3-1.2% silicon (Si), 0.1-0.8% tin (Sn), 0.01-0.45% chromium (Cr), the balance copper (Cu), and unavoidable impurities in a total amount of 0.4% or less to obtain an ingot (=melting and casting step); (2) hot rolling the obtained ingot at a temperature range of 900°C to 1040°C (=hot rolling step); (3) performing a first cold rolling on the sheet material obtained in the previous step at a rolling reduction of 50% or more (=first cold rolling step); and (4) intermediately heat treating the sheet material obtained in the previous step at 400°C to 800°C for 1 to 300 minutes. (5) a step of subjecting the plate material obtained in the previous step to a second cold rolling at a rolling reduction of 70% to 90% (= a second cold rolling step); (6) a step of subjecting the plate material obtained in the previous step to a solution treatment at a temperature of 820°C to 1000°C for 20 to 300 seconds (= a solution treatment step); (7) a step of subjecting the plate material obtained in the previous step to a finish cold rolling at a rolling reduction of 10% to 50% (= a finish cold rolling step); and (8) a two-stage aging treatment step (= a two-stage aging treatment step) of aging the product obtained in the previous step at a temperature of 440°C to 600°C for 5 minutes to 300 minutes and then aging at a temperature of 350°C to 440°C for 1 hour to 30 hours.
[0045] Although not described in detail in this specification, in the above-mentioned manufacturing method, a person skilled in the art may perform facing after hot rolling, if necessary, and may perform acid-washing, polishing, or degreasing after each heat treatment, if necessary.
[0046] Each of the main process steps is described in more detail below.
[0047] (1) Melting and casting step
[0048] The components of the composition described above are mixed and melted. The melting is performed at 1250°C to 1350°C so that all the raw materials are melted. If the melting temperature is lower than 1250°C, the fluidity of the molten metal decreases, and if the melting temperature is higher than 1350°C, the solubility of oxygen and hydrogen in the molten metal increases, impairing the quality of the ingot.
[0049] After the melting is completed, the molten metal is stabilized by holding the molten metal at 1180° C. to 1230° C. for 30 to 120 minutes. The conditions for stabilizing the molten metal can be appropriately determined by a person skilled in the art based on the knowledge in the field.
[0050] Once the molten metal stabilization process is complete, the ingots are cast. The cooling rate for the ingots during casting is 100°C / min to 200°C / min. A cooling rate of less than 100°C / min is not practical in terms of cost, and a rate of more than 200°C / min will cause thermal stress inside the ingot due to rapid cooling, resulting in cracks.
[0051] The melting and casting steps are carried out in a general atmospheric melting furnace, for example, a high-frequency atmospheric melting furnace, but may be more preferably carried out in an inert gas atmosphere or a vacuum melting furnace to prevent oxidation of some components such as Cr, Si, etc.
[0052] (2) Hot rolling step
[0053] The ingot obtained as described above is rolled in the temperature range of 900° C. to 1040° C. In the hot rolling of the copper alloy of the present invention, rapid cooling is performed after the rolling is completed so as not to generate precipitates during the rolling.
[0054] (3) First cold rolling step
[0055] The plate material obtained in the previous step is subjected to a first cold rolling with a reduction of 50% or more. In order to increase the driving force for the formation of cube structure seeds in the intermediate heat treatment step described below, it is preferable to set the reduction to 50% or more. If the reduction is less than 50%, sufficient cube structure seeds will not be formed as desired in the subsequent intermediate heat treatment step. These seeds are fine recrystallized grains formed in the intermediate heat treatment step.
[0056] (4) Intermediate heat treatment step
[0057] The plate material obtained in the previous step is subjected to intermediate heat treatment at 400 to 800°C for 1 to 300 minutes. When intermediate heat treatment is performed within this range, recrystallized grains are partially formed and seeds of a cube structure are formed.
[0058] The intermediate heat treatment step in the typical copper alloy manufacturing process is a step to relieve stresses generated by electric potentials and the like that have accumulated in the material so that the material can be more easily (with less force) rolled to the desired thickness in the subsequent cold rolling process.
[0059] However, the purpose of the intermediate heat treatment in the present invention is different from the usual purpose, and is to partially recrystallize the rolled structure formed by cold rolling after hot rolling, thereby generating recrystallized grains.
[0060] The intermediate heat treatment is performed at 400°C to 800°C for 1 minute to 300 minutes. If the heat treatment temperature is less than 400°C or the heat treatment time is less than 1 minute, recrystallization is not sufficiently performed, and the ratio defined in the relational expression between the crystal grain size and the diffraction integrated intensity of the {200}, {111}, {220} and {311} crystal planes described later cannot be obtained. If the heat treatment temperature is more than 800°C or the heat treatment time is more than 300 minutes, the alloy components are dissolved simultaneously with the growth of the crystal grains, resulting in random orientation, and this also makes it impossible to obtain the ratio defined in the relational expression between the crystal grain size and the diffraction integrated intensity of the {200}, {111}, {220} and {311} crystal planes described later. Specific details are disclosed in the section on texture control below.
[0061] (5) Secondary cold rolling step
[0062] The plate material obtained in the previous step is subjected to secondary cold rolling with 5 to 10 passes and a reduction rate of 70% or more. After hot rolling, a high solution temperature and a long solution time are required to sufficiently dissolve the coarse (Co, Ni)2Si crystals and precipitates generated by cooling and intermediate heat treatment. In particular, Co has high precipitation and solution temperatures, making it difficult to dissolve it sufficiently to ensure strength.
[0063] The present inventors have found that by introducing appropriate rolling conditions and refining the generated coarse (Co, Ni)2Si crystals and precipitates and stretching them, sufficient solid solubility can be obtained in the solution treatment described below. In a normal rolling process, the number of rolling times is set to 2 to 3 times to achieve the desired thickness, but in the present invention, the number of rolling times is set to 5 to 10 times. If the number of rolling times is less than 5, the coarse (Co, Ni)2Si crystals and precipitates cannot be refined, and sufficient solid solution is not achieved in the solution treatment described below. On the other hand, if the number of rolling times is 10 or more, the productivity decreases rapidly, making it difficult to apply to actual mass production. In addition, even if rolling is performed 5 to 10 times, if the reduction rate is less than 70%, the (Co, Ni)2Si crystals and precipitates are not refined, and the driving force for recrystallization in the solution treatment described below decreases, making it difficult to obtain the desired diffraction integrated intensity.
[0064] (6) Solution treatment step
[0065] The sheet material obtained in the previous step is solution treated for 20 to 300 seconds at a temperature of 820°C to 1000°C. The main objectives of conventional solution treatment are to redissolve the solute elements in the matrix and to recrystallize, but the objective of the solution treatment in the present invention also includes the formation of a recrystallized texture with cubes as the main orientation component.
[0066] The solution treatment is carried out in a temperature range of 820°C to 1000°C. If the temperature is too low, recrystallization is incomplete and the solid solution of the solute elements is insufficient, so that sufficient strength and electrical conductivity cannot be obtained during the aging treatment described below. On the other hand, if the temperature is too high, the crystal grains become coarse, so that it is difficult to finally obtain a high-strength copper alloy sheet material with excellent bending workability. In addition, if the heat treatment is performed for less than 20 seconds in the above-mentioned temperature range, recrystallization is not formed and a cube structure cannot be formed. On the other hand, if the heat treatment is performed for more than 300 seconds, the crystal grains become coarse, so that excellent bending workability cannot be obtained.
[0067] After solution treatment, the plate material is cooled at a rate of 20 to 40°C / s. Since Co has a high precipitation temperature, if it is cooled at a rate of less than 20°C / s after solution treatment, the dissolved Co solute is quickly re-extracted from the matrix, making it impossible to ensure sufficient strength in the aging treatment described below. If the cooling rate exceeds 40°C / s, stress is generated inside the plate material, causing deterioration of the plate shape, such as plate bending.
[0068] (7) Finish cold rolling step
[0069] The plate material obtained in the previous step is finish cold-rolled at a rolling ratio of 10% to 50%. The strength level can be improved by the finish cold rolling. The rolling ratio of the finish cold rolling is in the range of 10% to 50%. If the rolling ratio is less than 10%, the precipitation driving force is insufficient, so sufficient strength cannot be ensured in the aging treatment step described later. If the rolling ratio exceeds 50%, the strength level is improved, but the cube structure is reduced and bending workability is significantly reduced.
[0070] (8) Two-step aging treatment step
[0071] The product obtained in the previous step is subjected to a first aging treatment at a temperature range of 440°C to 600°C for 5 to 300 minutes, and then a second aging treatment at a temperature range of 350°C to 440°C for 1 to 30 hours.
[0072] Generally, the aging treatment of Cu-Ni-Si based copper alloys is often carried out by a single heat treatment in the range of 400°C to 450°C, where the effect of increasing strength due to the formation of intermetallic compounds is most prominent.
[0073] However, in the present invention, the primary aging treatment is carried out in the range of 440°C to 600°C, and the secondary aging treatment is carried out in the range of 350°C to 440°C.
[0074] The primary aging treatment, which is performed at a temperature between 440°C and 600°C, is intended to increase Co-Si precipitation at high temperatures and provide the sheet material with an appropriate thermal history. If the aging temperature is less than 440°C, Co-Si precipitates are not formed, but if it exceeds 600°C, re-dissolution of the precipitates occurs. Co-Si precipitates refer to (Co,Ni)2Si precipitates with a high specific gravity of Co.
[0075] The subsequent secondary aging treatment in the range of 350°C to 440°C increases the precipitation of Ni-Si that was not sufficiently precipitated in the primary aging, thereby further improving the strength and electrical conductivity. If the aging temperature is less than 350°C, the aging time becomes long and the productivity is significantly reduced, and if it exceeds 440°C, Ni-Si precipitates are not formed and strength and electrical conductivity cannot be sufficiently secured. Ni-Si precipitates refer to (Co,Ni)2Si precipitates with a high specific gravity of Ni.
[0076] Copper alloy sheet material obtained by the manufacturing method according to the present invention
[0077] (1) Recrystallization fraction
[0078] When a crystalline structure processed by rolling is heated at a certain temperature, the internal stress accumulated by processing gradually decreases, and new crystal nuclei without internal deformation are generated from the original crystal grains with residual deformation, which gradually grow and confront the original crystal grains. This phenomenon is called recrystallization, and the grains generated by this phenomenon are called recrystallized grains. Unless otherwise defined, in the present invention, the grains formed by recrystallization in the intermediate heat treatment step are called recrystallized grains.
[0079] The present inventors have discovered that the size and fraction of recrystallized grains formed in the intermediate heat treatment step increases the cube fraction in the solution treatment described below.
[0080] According to the present invention, when the end faces parallel to the rolling direction of a test piece that has been subjected to intermediate heat treatment are etched and the structure is observed using a SEM, if the area ratio of the recrystallized structure is 60% to 90%, the crystal plane fraction of the cube structure grows to a high level in the solution treatment described below, improving bending workability.
[0081] If the ratio of recrystallized structure after the intermediate heat treatment is less than 60%, the crystal grains will grow as a random structure without preferential orientation in the solution treatment described below. If the ratio of recrystallized structure exceeds 90%, the driving force for the growth of the cube structure will decrease and the desired texture will not be obtained.
[0082] (2) Control of grain size and texture
[0083] The X-ray diffraction pattern from the sheet surface (rolled surface) of a Cu-Ni-Co-Si-based copper alloy sheet material is generally composed of diffraction peaks of four crystal planes: {111}, {200}, {220}, and {311}. The X-ray diffraction intensity of other crystal planes is relatively very small, so that it can be ignored from the viewpoint of controlling the texture. Among these crystal planes, {200} is a so-called cube texture crystal plane. When the fraction of the cube texture crystal plane is high and the fraction of other crystal planes is low, non-uniform deformation is suppressed and bending workability is improved. In this specification, unless otherwise specified, the crystal grains related to the intensity of the X-ray diffraction integral refer to the crystal grains generated in the sheet material after the solution treatment.
[0084] According to the method for producing the copper alloy sheet of the present invention, the size of the crystal grains generated in the sheet after the solution treatment is in the range of 5 to 20 μm. When the crystal grain size is within this range, the strength is not reduced and the bending workability can be improved. When the crystal grain size is less than 5 μm, the elasticity of the material is reduced and the spring characteristics are poor, making it difficult to apply to parts, and when the crystal grain size exceeds 20 μm, the strength is reduced and the bending workability is also reduced.
[0085] However, in copper alloy sheet materials, it is difficult to have an appropriate crystal grain size and increase the fraction of cube structure as described above, as it is difficult to simultaneously increase strength and electrical conductivity, which are mutually opposing properties. More specifically, since the method of forming cube structure seeds differs for each alloy composition, it is necessary to find an appropriate method of forming cube structure seeds, and even if the cube structure seeds are successfully formed, it is necessary to find the growth conditions of the structure in order to grow them into a cube structure with a high fraction. This is a challenge that must be tackled after comprehensively understanding all components, contents, and intermediate formation processes. That is, since the growth of the cube structure is performed at high temperatures, the crystal grain size is likely to become coarse, and even if it is successfully manufactured up to this point, it is difficult to ensure the physical properties of strength, high electrical conductivity, and bending workability, which are the objective of the present invention, without work hardening by rolling. This is because if the rolling rate is increased to ensure the physical properties, the fraction of the cube structure decreases and bending workability is significantly reduced, and on the other hand, if rolling is not introduced or the rolling rate is reduced to ensure bending workability, the strength cannot be increased.
[0086] Nevertheless, the present inventors have surprisingly found that in the case of the copper alloy sheet material according to the present invention, when the crystal grain size after solution treatment and the crystal plane fraction of the cube structure simultaneously satisfy the following two formulas, non-uniform changes are suppressed and bending workability is improved.
[0087] 5 ≦ Grain size (μm) Х I{200} / (I{111}+I{220}+I{311}) ≦ 60
[0088] 2 ≦ Grain size (μm) - I{200} / (I{111}+I{220}+I{311}) ≦ 19
[0089] Here, I{111}, I{200}, I{220}, and I{311} are the diffraction integrated intensities of the diffraction peaks of each crystal plane measured by X-ray diffraction.
[0090] If the grain size and the ratio of the X-ray diffraction integrated intensity, I{200} / (I{111}+I{220}+I{311}), do not simultaneously satisfy the above formula after solution treatment, bending workability will rapidly deteriorate.
[0091] The above-mentioned relationship is satisfied when the copper alloy sheet is manufactured by the above-mentioned manufacturing method of the present invention. In particular, the conditions of the intermediate heat treatment, the second cold rolling and the solution treatment must be included in the conditions presented in the manufacturing method of the copper alloy sheet of the present invention.
[0092] (3) Physical properties of the copper alloy sheet material produced by the production method of the present invention
[0093] The copper alloy material of the present invention has a tensile strength of 850 MPa or more, an electrical conductivity of 40% IACS or more, and bending workability of R / t≦1.0 or less in a 180 degree bending test in both the rolling direction and the direction perpendicular to the rolling direction.
[0094] The strength of the copper alloy material of the present invention is represented by tensile strength. The tensile strength of the copper alloy material of the present invention is 850 MPa or more. If the tensile strength is less than 850 MPa, the material cannot withstand the stress applied during assembly or operation of automobile parts or electric / electronic parts, and the contact pressure between parts is reduced, resulting in reduced reliability, so a tensile strength of 850 MPa or more is necessary.
[0095] The electrical conductivity of the copper alloy material of the present invention is 40% IACS or more. In the case of automotive connectors, the number of pins has increased from 50 to 70 in the past to 120 or more, and heat generation control is also an important issue to be solved. In this regard, in the case of copper alloy materials used as automotive connectors, if the electrical conductivity is less than 40% IACS, it becomes difficult to perform appropriate heat generation control. If the heat generation control is insufficient, the life of the equipment will be reduced due to the high temperature generated from the parts. Therefore, the electrical conductivity of copper alloy materials used for automobiles or electronic and electrical parts is required to be 40% IACS or more. The copper alloy material of the present invention ensures electrical conductivity of 40% IACS or more by reducing the solid solubility of the additive elements in the base by Cr, optimizing the content ratio of Ni, Co, and Si, and performing a two-stage aging treatment that can maximize the precipitation of (Co, Ni)2Si.
[0096] The bending workability of the copper alloy material of the present invention is R / t≦1.0 (180° bending) in both the rolling direction and the direction perpendicular to the rolling direction. If the R / t value of the bending workability exceeds 1.0, bending cracks occur during bending of narrow-width processed products, making it difficult to apply the material to small or complex-shaped processed products, and therefore bending workability of R / t≦1.0 is necessary. The copper alloy material of the present invention has excellent strength and electrical conductivity and ensures bending workability of R / t≦1.0 by controlling the grain size and texture described above through condition control of the steps of intermediate heat treatment, secondary cold rolling, and solution treatment in the manufacturing method of the present invention. The relational expression for controlling the grain size and texture may be found in the above content. EXAMPLES
[0097] Examples 1 to 10 Test pieces of Examples 1 to 10 were produced with the compositions shown in Table 1. The method for producing the test pieces is described below.
[0098] According to each example, alloy elements including copper were mixed based on 10 kg and melted in a high-frequency atmospheric melting furnace with the composition shown in Table 1. After melting was completed, the molten metal was stabilized by holding at 1210°C for 40 minutes, and an ingot having a thickness of 35 mm, a width of 140 mm, and a length of 200 to 250 mm was cast.
[0099] The obtained ingot was cut into 30 mm portions at the bottom and top for rapid cooling and to remove defects such as shrinkage holes, and the middle ingot was hot rolled and quenched under the conditions shown in Table 2. After hot rolling, the ingot was faced to a thickness of 0.5 mm to remove the oxide scale formed on both surfaces.
[0100] Next, under the conditions shown in Table 2, first cold rolling, intermediate heat treatment, second cold rolling, solution treatment, finish rolling and final two-step aging treatment were performed.
[0101] Finally, plate test pieces with a thickness of 0.1 t were produced.
[0102] Comparative Examples 1 to 26 For each of the comparative examples, a test piece was produced using the composition shown in Table 1 by the method shown in Table 2, and evaluation tests were carried out in the same manner as for the test pieces obtained in Examples 1-10.
[0103] [Table 1]
[0104] [Table 2]
[0105] Meanwhile, in the process of manufacturing each test piece according to Tables 1 and 2, the recrystallization ratio in the intermediate heat treatment step was calculated using EBSD (Electron Backscatter Diffraction) from EDAX, and the size of the recrystallized grains after the solution treatment was measured using Quanta650FEG (FE-SEM) from FEI. Typically, the size of the recrystallized grains measured in the solution treatment step of Example 1 is 8 μm.
[0106] In addition, an X-ray diffractometer was used to measure the integrated intensity of X-ray diffraction peaks of {200}, {220}, {111}, and {311} crystal planes relative to the sample sheet surface (rolled surface) were determined using a characteristic X-ray of Cu-Kα1 at a tube voltage of 40 kV and a tube current of 30 mA. For example, in the solution treatment step of Example 1 obtained by the above-mentioned method, the integrated intensity ratio of the I{200} / (I{111}+I{220}+I{311}) diffraction peaks was 1.5.
[0107] Using the previously determined recrystallized grain size and the ratio of the integrated intensity of the I{200} / (I{111}+I{220}+I{311}) diffraction peak, the value of the recrystallized grain size -I{200} / (I{111}+I{220}+I{311}) and the value of the recrystallized grain size xI{200} / (I{111}+I{220}+I{311}) were determined in the solution treatment step. In the solution treatment step of Example 1, the value of the recrystallized grain size -I{200} / (I{111}+I{220}+I{311}) was 6.5, and the value of the recrystallized grain size xI{200} / (I{111}+I{220}+I{311}) was 12. Values calculated in the same manner for the other examples and comparative examples are shown in Table 3.
[0108] In the cases where test pieces were successfully produced from Examples 1 to 10 and Comparative Examples 1 to 25, the tensile strength, electrical conductivity and bending workability of the obtained samples were evaluated by the following methods.
[0109] Test Example (Tensile strength) The tensile strength in the rolling direction was measured using a tensile tester in accordance with JIS Z 2241. The results are shown in Table 3.
[0110] (Bending workability) For bending workability, a complete contact bending test (180° complete contact U-bend test) was performed in the direction parallel to the rolling direction (bad way) and perpendicular to the rolling direction (good way). With the bending radius R and material thickness t, a complete contact bending test (180° complete contact U-bend test, R / t≦1.0 condition) was performed in the direction parallel to the rolling direction (bad way) and perpendicular to the rolling direction (good way). If no cracks were observed with an optical microscope, the material was rated as O, and if cracks were observed, the material was rated as X. The results are shown in Table 3.
[0111] (Electrical Conductivity) The electrical conductivity was measured using a FOERSTER SIGMATEST after polishing the surface of the test piece and removing all oxide scale at a frequency of 240 kHz. The results are shown in Table 3.
[0112] [Table 3]
[0113] As can be seen from Table 3, it can be confirmed that Examples 1 to 10 have a tensile strength of 850 MPa or more, an electrical conductivity of 40% IACS or more, and R / t≦1.0 or less in a 180° fully contacted U-bend test in the direction parallel to the rolling direction (bad way) and in the direction perpendicular to the rolling direction (good way). That is, the test pieces of Examples 1 to 10 have high strength, high conductivity, and excellent bending workability.
[0114] On the other hand, in Comparative Example 1, since the Ni content was as low as 1.2%, both the strength and electrical conductivity were reduced due to the effect of Si dissolved in the matrix.
[0115] In Comparative Example 2, the sum of the Ni and Co contents was too high at 4.19%, and Ni and Co were over-dissolved in the copper matrix, failing to form a high proportion of precipitates, so high strength and electrical conductivity were not obtained.
[0116] In Comparative Example 3, the impurities Al and Mn were excessively added at 0.7% or more, and side cracks occurred during hot rolling, making it impossible to manufacture a finished test piece.
[0117] In Comparative Example 4, the (Ni+Co) / Si ratio was too high at 5.35, and the Ni and Co remaining after forming precipitates with Si were over-dissolved, failing to form a high fraction of precipitates and remaining in the matrix, making it impossible to ensure strength and electrical conductivity.
[0118] In Comparative Example 5, the Cr content was excessively added at 0.75%, and coarse inclusions were formed, resulting in low strength and cracks during bending tests.
[0119] In Comparative Example 6, the intermediate heat treatment was performed at a temperature of 310°C for 275 minutes, which was too low, and the recrystallization ratio was not sufficient to form a cube structure, and the desired texture was not obtained in the solution treatment. As a result, cracks occurred at the bent part at R / t=1.0 during the 180° bending test in the bad-way direction parallel to the rolling direction.
[0120] In Comparative Example 7, the secondary cold rolling reduction was 50%, which was too low for rolling, and the precipitates that had become coarse after intermediate heat treatment were not sufficiently refined, the solid solubility decreased during solution treatment, and finally sufficient strength could not be secured. Since a sufficient driving force for recrystallization was not obtained, the fraction of cube structure was low during solution treatment, and as a result, cracks occurred in the bent part during bending test.
[0121] In Comparative Example 8, the secondary cold rolling was performed with two passes. As a result, rolling was performed with an excessively small number of passes, and the precipitates that had become coarse after the intermediate heat treatment were not sufficiently refined, the solid solubility decreased during the solution treatment, and finally sufficient strength could not be secured.
[0122] In Comparative Example 9, the test piece was produced by carrying out the heat treatment at a too low temperature, i.e., the solution treatment condition was 700°C x 250 seconds. Because the heat treatment was carried out at a low temperature, the alloy components such as Ni, Co, Si, and Cr were not completely dissolved in the matrix, and as a result, the strength could not be ensured in the final aging treatment.
[0123] In Comparative Example 10, the cooling condition after the solution treatment was 10° C. / sec, which was an excessively slow cooling rate, and as a result, the solute that had been dissolved in the matrix during the solution treatment was quickly re-extracted from the matrix during cooling due to the slow cooling rate, and as a result, sufficient strength could not be secured during the aging treatment.
[0124] In Comparative Example 11, the reduction ratio of the finish rolling was increased to 70% to produce a test piece. Because the reduction ratio of the finish rolling was too high, the strength increased significantly, but the electrical conductivity and bending workability decreased. During the bending test, cracks occurred at the bent portion.
[0125] In Comparative Example 12, a test piece was produced by performing aging treatment solely under the secondary aging conditions without performing the primary aging treatment, and as a result, precipitation was not sufficiently performed, and sufficient strength and electrical conductivity were not obtained.
[0126] In Comparative Example 13, the secondary aging treatment was performed at a high temperature of 480°C for 5 hours to produce a test piece. As a result, Ni-Si precipitates were not sufficiently formed due to the high temperature, and both the strength and electrical conductivity were low.
[0127] In Comparative Example 14, the Sn content was 1.2%, which was too high. As a result, the Sn content remaining in the matrix even after the precipitation treatment was high, resulting in a low electrical conductivity value.
[0128] In Comparative Example 15, the Cr content was added at an excessively low level of 0.01%, so that the effect of reducing the solid solubility during aging treatment was not obtained, and sufficient electrical conductivity could not be secured.
[0129] In Comparative Example 16, the Si content was excessively added at 1.3%, and sufficient precipitates were not obtained, so that sufficient strength and electrical conductivity could not be ensured.
[0130] In Comparative Example 17, the Ni content was excessively added at 4.2%, so that precipitates could not be formed, and sufficient electrical conductivity could not be secured due to the influence of Ni remaining in the matrix, and bending workability was reduced due to the formation of coarse precipitates.
[0131] In Comparative Example 18, the Co content was excessively added at 1.7%, and the (Ni+Co) / Si ratio was high, so sufficient strength and electrical conductivity could not be ensured.
[0132] In Comparative Example 19, since the Si content was extremely low at 0.2%, sufficient precipitates were not formed, and strength and electrical conductivity could not be ensured.
[0133] In Comparative Example 20, the Sn content was added at an excessively low level of 0.03%, which resulted in the effect of increasing the solid solubility during solution treatment not being obtained, and therefore sufficient strength was not obtained.
[0134] In Comparative Example 21, the reduction rate of the first cold rolling was low at 30%, and a sufficient area percentage of recrystallized grains was not obtained during intermediate heat treatment. As a result, the recrystallized grain size xI{200} / (I{111}+I{220}+I{311}) was not obtained during solution treatment, and bending workability was significantly reduced.
[0135] In Comparative Example 22, the temperature of the intermediate heat treatment was too high at 900°C, and complete recrystallization occurred during the intermediate heat treatment. As a result, the recrystallized grain size -I{200} / (I{111}+I{220}+I{311}) was not obtained during the solution treatment, and bending workability could not be ensured.
[0136] In Comparative Example 23, the solution treatment temperature was 1030°C, which was too high, causing rapid growth of crystal grains and failing to obtain a value that satisfied the recrystallized grain size -I{200} / (I{111}+I{220}+I{311}). As a result, sufficient bending workability could not be ensured.
[0137] In Comparative Example 24, the solution treatment time was short, Ni, Co, Si, and Cr were not sufficiently dissolved, and strength could not be ensured. In addition, the fine recrystallized grain size did not satisfy the recrystallized grain size xI{200} / (I{111}+I{220}+I{311}), and bending workability could not be ensured.
[0138] In Comparative Example 25, the solution treatment time was too long, causing the crystal grains to grow coarse, and as a result, sufficient bending workability could not be ensured.
Claims
1. The alloy is composed of, by weight, 1.5 to 3.4% nickel (Ni), 0.1 to 1.5% cobalt (Co), 0.3 to 1.2% silicon (Si), 0.1 to 0.8% tin (Sn), 0.01 to 0.45% chromium (Cr), the balance being copper (Cu), and unavoidable impurities of a total amount of 0.4% or less, the unavoidable impurities being one or more selected from the group consisting of Mg, Al, P, Ca, Ti, V, Zn, Fe, Zr, and Mn.
1. A method for producing a copper alloy sheet material for automobiles or electric / electronic parts, the method comprising the steps of: melting and casting 1.5-3.4% nickel (Ni), 0.1-1.5% cobalt (Co), 0.3-1.2% silicon (Si), 0.1-0.8% tin (Sn), 0.01-0.45% chromium (Cr), the balance copper (Cu) and unavoidable impurities in a total amount of 0.4% or less to obtain an ingot; hot rolling the obtained ingot at a temperature range of 900°C to 1040°C; A step of subjecting the plate material obtained in the previous step to a first cold rolling at a rolling reduction of 50% or more; intermediate heat treatment of the plate material obtained in the previous step at 400°C to 800°C for 1 to 300 minutes; A step of subjecting the plate material obtained in the previous step to a second cold rolling with a rolling reduction of 70% to 90%; subjecting the plate material obtained in the previous step to solution treatment at a temperature of 820°C to 1000°C for 20 seconds to 300 seconds; Finish cold rolling the plate material obtained in the previous step with a rolling reduction of 10% to 50%; and A method for producing a copper alloy sheet material for automobiles and electric / electronic parts, comprising a two-stage aging treatment in which the product obtained in the previous step is aged at a temperature of 440°C to 600°C for 5 minutes to 300 minutes, and then aged at a temperature of 350°C to 440°C for 1 hour to 30 hours.
2. The method for producing a copper alloy sheet according to claim 1, wherein the contents of Ni, Co and Si satisfy 3.5≦(Ni+Co) / Si≦4.
5.
3. The method for producing a copper alloy sheet according to claim 1, wherein the contents of Ni and Co satisfy Ni+Co≦3.
5.
4. The manufacturing method according to claim 1, wherein the solution heat treated plate material simultaneously satisfies the following formulas: 5≦grain size (μm) XI{200} / (I{111}+I{220}+I{311})≦60 2≦grain size (μm) − I{200} / (I{111}+I{220}+I{311})≦19 Here, I{111}, I{200}, I{220}, and I{311} are the diffraction integrated intensities of the diffraction peaks of the respective crystal planes measured by X-ray diffraction.
5. The method according to claim 1, wherein after the solution treatment, the steel is cooled at a rate of 20 to 40° C. / s.
6. The method according to claim 1, wherein the number of passes in the second cold rolling is 5 to 10.
7. A copper alloy sheet material for automobiles and electric / electronic parts, produced according to any one of claims 1 to 6.
8. The copper alloy sheet according to claim 7, wherein the copper alloy sheet has a tensile strength of 850 MPa or more, bending workability of R / t≦1.0 (180° bending) in both the rolling direction and the direction perpendicular to the rolling direction, and an electrical conductivity of 40% IACS or more.
Citation Information
Patent Citations
High-performance copper alloy strip and preparation method thereof
CN112501472A
Copper alloy containing cobalt, nickel and silicon
JP2005532477A
Copper alloy for electrical and electronic equipment
JP2009007666A
Copper alloy sheet material and manufacturing method therefor
JP2010275622A
Cu-Ni-Si-Co-BASED COPPER ALLOY FOR ELECTRONIC MATERIAL
JP2016183418A