Fuel cell separator plate with metal coating layer and manufacturing method thereof
A platinum-based coating on fuel cell separators addresses corrosion and conductivity issues by forming a discontinuous film through electrolytic plating and heat treatment, ensuring durability and efficiency in humid conditions.
Patent Information
- Application Number
- JP2024523788
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-04
- Filing Date
- 2022-11-03
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2042-11-03
AI Technical Summary
Existing fuel cell separators face issues with corrosion and reduced conductivity due to metal oxide formation in humid environments, leading to performance degradation, and there is a need for alternative coating materials that provide both corrosion resistance and conductivity, especially with the rising cost of gold.
A method involving the application of a discontinuous platinum coating on the base material using electrolytic or electroless plating, combined with heat treatment, to form a platinum-based coating film on stainless steel or titanium alloy surfaces, enhancing corrosion resistance and conductivity.
The method results in a fuel cell separator with improved corrosion resistance and conductivity, maintaining performance in harsh environments, and offers efficient production processes.
Smart Images

Figure 2024538807000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a separator plate for a fuel cell with a metal coating layer and a manufacturing method thereof, and more particularly to a separator plate for a fuel cell with a discontinuous coating layer using platinum and precious metals and a manufacturing method thereof. [Background technology]
[0002] Fuel cells used for hydrogen electricity are used as a power source that generates electricity through an electrochemical reaction between reactant gas and catalyst. The stack of a fuel cell has a structure in which components such as a membrane electrode assembly (MEA), separator (bipolar plate), gasket, current collector, and end plate are connected, and the membrane electrode assembly (MEA) has a structure in which gas diffusion electrodes (GDEs) consisting of a catalyst layer and a gas diffusion layer (GDL) are in contact with both sides of the MEA via a polymer electrolyte membrane.
[0003] The metal separator for fuel cells is one of the components that constitute the main body of a fuel cell, and is in electrical contact with the hydrogen electrode of a unit cell and the air electrode of an adjacent cell, and hydrogen and air are supplied to the inside of each electrode through the fluid flow channels on both sides of the separator. Thus, the metal separator of a fuel cell plays a key role in collecting and transferring electricity generated in an electrochemical reaction, conducting electricity, discharging water formed in the electric reaction, and managing heat inside the cell.
[0004] The base material of the separator plate is made of a material that has excellent electrical conductivity, such as stainless steel, titanium alloy, aluminum alloy, or polymer composite material. However, due to the characteristics of metals, when the separator plate is exposed to the high temperature and high humidity operating environment of a vehicle fuel cell for a long period of time, corrosion is accelerated and the metal oxide formed on the surface acts as an electrical insulator, resulting in a decrease in conductivity or catalyst contamination, thereby reducing the overall performance of the fuel cell.
[0005] In order to prevent such inconveniences, research has been ongoing to ensure corrosion resistance and improve conductivity by forming discontinuous coating films containing various precious metal materials, including polymers, carbon, gold (Au), platinum (Pt), ruthenium (Ru), iridium (Ir), etc., on the surface of the base material of the metal separator, but in practice, coating films using gold (Au) nano-coating films are mainstream. However, the need for development of alternative coating films is emerging due to the continuous rise in the price of gold (Au).
[0006] Furthermore, although there have been experiments and studies that have shown that a discontinuous platinum (Pt) coating film can be formed on the surface of a base material, the reality is that there are insufficient results that demonstrate the efficiency of the process and the notable significance of the application of the coating film using platinum.
[0007] When a discontinuous coating film is applied, part of the surface of the separator base material will be directly exposed to the outside. However, for future fuel cell stacks that require high output and long durability, a coating technology that has excellent conductivity and chemical stability even when used in harsh environments is required, even though a large amount of financial resources will be required to ensure performance through the coating uniformity of the new coating material and to verify the stability of the plated electrode body.
[0008] Related technology includes Korean Patent Publication No. 10-2015-0138105 (Publication date: 2017.04.07., Title of invention: Coating composition for metal separator of solid oxide fuel cell and manufacturing method thereof). Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide a metal separator for a vehicle fuel cell that has excellent corrosion resistance and contact resistance, and that can be produced efficiently, and a method for producing the same. [Means for solving the problem]
[0010] A method for manufacturing a metal separator for a vehicle fuel cell according to one aspect of the present invention may include the steps of: preparing a base material; applying a coating agent containing platinum (Pt) and further containing at least one selected from the group consisting of gold (Au), ruthenium (Ru), iridium (Ir), ruthenium oxide (RuO2), and iridium oxide (IrO2), and an electrolyte solution to the base material to form a discontinuous coating film; and heat-treating the base material with the coating film.
[0011] In one embodiment, the base material may be stainless steel plate, titanium or aluminum.
[0012] In an embodiment, the coating film forming step may be any one of electrolytic plating, electroless plating, and PVD processes.
[0013] In one embodiment, the platinum (Pt) contained in the coating agent may include chloroplatinic acid (H2PtCl6) or potassium chloroplatinate (K2PtCl6).
[0014] In one embodiment, the heat treatment step can be performed at a temperature in the range of 80 to 600° C. and for a time in the range of 10 to 180 minutes.
[0015] In one embodiment, the heat treatment step can be performed in one of a vacuum, air, and an oxygen atmosphere.
[0016] A metal separator for a fuel cell for vehicles according to another aspect of the present invention may be a metal separator for a fuel cell for vehicles manufactured by the method according to any of the above embodiments. Effect of the Invention
[0017] According to the present invention, it is possible to provide a metal separator for a fuel cell which has excellent corrosion resistance and contact resistance, and which can be produced with excellent production efficiency, and a method for producing the same. [Brief description of the drawings]
[0018] [Figure 1] 2 is a process flow diagram illustrating a method for manufacturing a separator for a fuel cell according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing a platinum coating step according to an embodiment of the present invention and a comparative example. [Diagram 3] 2A to 2C are diagrams illustrating heat treatment steps according to an embodiment of the present invention and a comparative example. [Figure 4] FIG. 2 is a schematic diagram illustrating test pieces and measurement positions for measuring contact resistance in examples and comparative examples of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings so that a person having ordinary skill in the art to which the present invention belongs can easily carry out the present invention. The present invention may be embodied in various different forms and is not limited to the embodiments described in the present specification. Throughout the present specification, the same or similar components are denoted by the same reference numerals. In addition, detailed descriptions of known functions and configurations that may unnecessarily obscure the gist of the present invention will be omitted.
[0020] 1 is a flow chart of a method for manufacturing a metal separator for a vehicle fuel cell according to an embodiment of the present invention. The method includes a base material forming step S110, a coating layer forming step S120 on the surface of the base material, and a heat treatment step S130.
[0021] Base material formation step S110
[0022] The steel material for the metal separator of a vehicle fuel cell is not particularly limited as long as it is a metal or non-ferrous metal used for a metal separator, but stainless steel, titanium, aluminum, etc. can be used. For example, SUS300 and 400 series stainless steel and Grade 1 titanium are preferred in terms of elongation and durability.
[0023] Step S120: Forming a coating layer on the base material surface
[0024] FIG. 2 is a diagram that illustrates a step of forming a discontinuous coating film containing platinum on the surface of the base material.
[0025] When a vehicle fuel cell is exposed to a high temperature and humidity operating environment for a long period of time, metal oxides that gradually have a negative effect on the conductivity of the fuel cell are formed on the surface of the base material. Therefore, in the present invention, a discontinuous coating layer is formed on the surface of the base material to provide a fuel cell that is excellent in both corrosion resistance and conductivity.
[0026] In order to form a coating layer having both excellent corrosion resistance and conductivity, various precious metals including gold (Au), platinum (Pt), ruthenium (Ru), and iridium (Ir) are typically used. In the present invention, a coating layer including platinum (Pt) is formed on the surface of a base material according to the purpose, thereby forming a coating layer for a metal separator of a vehicle fuel cell having excellent corrosion resistance and conductivity.
[0027] Specifically, in the coating layer forming step, a coating film is formed by applying a current at a constant coating temperature using a coating material and an electrolyte. Any coating material that contains platinum (Pt) and can be used as a coating material can be used without any particular restrictions, but chloroplatinic acid (H2PtCl6) or potassium chloroplatinate (K2PtCl6) is particularly desirable for a stable and efficient process.
[0028] The platinum (Pt) and additional precious metal-based coating materials used in the coating material may be nanoparticles having a size of 10 nm to 1 μm, and within the above range, the surface of the base material may be provided with a discontinuous coating film form that reduces density.
[0029] As the electrolyte, an acid electrolyte may be used, for example, a sulfuric acid-based or hydrochloric acid-based electrolyte. In particular, H2SO4 or HClO4 is preferred from the viewpoint of efficient chemical reaction in the platinum coating layer formation process.
[0030] The content of the coating material and the electrolyte can be varied depending on the desired Pt deposition amount and coating density according to the specific embodiment. For example, chloroplatinic acid (H2PtCl6) or potassium chloroplatinate (K2PtCl6) is added at 1×10 -4 ~1) M and perchloric acid (HClO4) or sulfuric acid (H2SO4) (1 × 10 -2 In particular, when chloroplatinic acid (H2PtCl6) or potassium chloroplatinate (K2PtCl6) is used in a range of 2 mM to 0.1 M with perchloric acid (HClO4) or sulfuric acid (H2SO4) in a range of 0.1 M to 0.5 M, excellent corrosion performance and contact resistance can be achieved, and more preferably, chloroplatinic acid (H2PtCl6) or potassium chloroplatinate (K2PtCl6) can be used in a range of 10 mM to 0.05 M with perchloric acid (HClO4) or sulfuric acid (H2SO4) in a range of 0.2 M to 0.3 M.
[0031] Within the above range, the relative content of the coating material and the electrolyte is within the range of 1 to 10 times the unit molar content of the electrolyte, whereby a coating film having excellent corrosion performance and contact resistance can be formed. If the content is below the above range, sufficient platinum (Pt) coating may not be achieved, and if the content exceeds the above range, the process efficiency decreases.
[0032] As a coating material, chloroplatinic acid (H2PtCl6) or potassium chloroplatinate (K2PtCl6) is used at 5×10 -3If used at less than 5×10, it will be difficult to secure a sufficient amount of platinum (Pt) deposition, and the electrolyte will -3 If less than this amount is used, it will be difficult to ensure sufficient reduction.
[0033] In addition to the platinum-containing chloroplatinic acid or potassium chloroplatinate, a coating material composed of a precious metal component such as gold (Au), ruthenium (Ru), iridium (Ir), ruthenium oxide (RuO2), and iridium oxide (IrO2) may be used as the coating material. When a further coating material is used, a hydrofluoric acid-based or sulfuric acid-based electrolyte may be used in addition to the sulfuric acid-based or hydrochloric acid-based electrolyte depending on the chemical properties of the added substance.
[0034] The coating step can be performed at room temperature, but since heating improves reactivity, it is performed at a temperature in the range of, for example, 25 to 80°C. In particular, when the coating step is performed in the range of 40 to 60°C, the efficiency of the process is reconsidered and the corrosion performance and contact resistance are excellent, and in particular, the corrosion performance and contact resistance are excellent in the range of 50 to 60°C.
[0035] When coating, the applied current is 5 to 60 mA / cm 2 In order to prevent the platinum (Pt) deposition from being insufficiently or excessively coated, while preventing surface oxidation due to an overcurrent, it is preferable to carry out the deposition within the range of 10 to 20 mA / cm. 2 It is preferable to perform the treatment within this range in terms of the surface stability of the base material and excellent performance of the coating film.
[0036] The method of coating the surface of the base material is not particularly limited as long as it is a commonly used method, and may be selected from, for example, electrolytic plating, electroless plating, or PVD methods, and the efficiency of the process may be increased when using these methods. In particular, electrolytic plating is preferable in terms of uniform coating properties and mass production in coating and manufacturing both electrodes of the separator.
[0037] Heat treatment step S130
[0038] FIG. 3 is a diagram showing a schematic diagram of a step of heat treating the base material with the coating film.
[0039] In the base material surface coating step, a discontinuous coating layer of platinum (Pt) and other materials is formed on the surface of the base material, and part of the surface of the base material is exposed to the outside. Therefore, in order to ensure excellent corrosion current and contact resistance throughout the separator, an oxide film formation step S130 is performed through a heat treatment process.
[0040] Specifically, the temperature of the heat treatment process varies depending on the characteristics of the oxide film formation of the base material, but may be, for example, in the temperature range of 80 to 600°C. In particular, in the case of a stainless steel base material, a temperature range of 170 to 230°C, and in the case of a titanium base material, a temperature range of 300 to 500°C, are excellent in terms of the oxide film formation speed and efficiency.
[0041] The time for the heat treatment process varies depending on the characteristics of the base material, but may be, for example, 10 to 180 minutes. In particular, when the heat treatment process is performed for 30 to 60 minutes, the corrosion current of the oxide film and the contact resistance are excellent.
[0042] The heat treatment process can be carried out in the atmosphere, but when it is carried out in a low-oxygen, vacuum or nitrogen atmosphere, the efficiency of oxide film formation and the performance of the oxide film formed are improved. In particular, when the heat treatment process is carried out in a low-oxygen atmosphere, it is preferable in terms of preventing excessive generation of oxide film, providing excellent contact resistance performance, and maintaining coating adhesion performance.
[0043] Metal separator for vehicle fuel cells
[0044] According to the method for manufacturing the metal separator of the fuel cell for vehicles, the metal separator of the fuel cell can have excellent corrosion resistance and electrical conductivity for a long period of time even in a high temperature and high humidity operating environment.
[0045] Therefore, as described above, a metal separator for a vehicle fuel cell having excellent corrosion resistance and electrical conductivity can be completed by going through a base material coating step using a coating material containing platinum (Pt) and an electrolyte, and a heat treatment step, to form a metal separator for a vehicle fuel cell in which a base material, a discontinuous coating film on its surface, and an oxide film are formed in the areas where the coating film is not formed. EXAMPLES
[0046] Examples and Comparative Examples
[0047] The base material formation step and coating step were performed using the base material, coating material and electrolyte composition, applied current and temperature in Table 1 below, and the base material with the discontinuous coating layer was subjected to a heat treatment step under the conditions in Table 2 to produce specimens for the examples and comparative examples, respectively.
[0048] Specifically, in comparison with the examples according to the present invention, in the coating material formation step, the amount of coating material in Comparative Example 1 was different, the amount of electrolyte in Comparative Example 5 was different, and the applied current in Comparative Examples 2 and 6 was different, as shown in Table 1. In the heat treatment step, the heat treatment time in Comparative Examples 3 and 6 was different, and the heat treatment temperature in Comparative Examples 4 and 8 was different, as shown in Table 2, to produce metal separator specimens.
[0049] [Table 1]
[0050] [Table 2]
[0051] Contact resistance measurement
[0052] The interfacial contact resistance (ICR) was measured for the examples and comparative examples. FIG. 4 is a schematic diagram showing the structure of a specimen for measuring the contact resistance of a metal separator of a fuel cell for vehicles according to the present invention and the measurement position of a comparative specimen (dummy). Prior to the actual measurement, two gas diffusion layers (GDL) 120 and one current collector 130 were formed on both sides of a metal separator (bipolar plate, bp) 110 of each of the comparative examples and examples to prepare specimens, and the contact resistance between the separator and the gas diffusion layer (GDL) was measured at two points R1 and R2 and calculated according to the following formula: To measure R2, three gas diffusion layers 120 were stacked without the metal separator, and current collectors 130 were stacked on both sides of the stack to prepare a dummy specimen. When measuring the contact resistance, a pressure of 50 to 100 N / cm was applied to the dummy specimen using a pressure device (Instron 68SC5). 2 pressure was applied.
[0053]
number
[0054]
number
[0055]
number
[0056]
number
[0057] In the above formula, bp represents the metal separator, GDL represents the gas diffusion layer, cc represents the current collector, and S represents the separator-GDL reaction area.
[0058] Corrosion performance measurements
[0059] Specimens were prepared from the metal separators of the above examples and comparative examples, and short-term corrosion resistance evaluations were performed on the base material and surface treatment layer of each specimen. Potentiodynamic polarization method was performed under the test conditions shown in Table 3 below. HIOKI's 3541 precision resistance measurement equipment was used for current application and resistance measurement.
[0060] [Table 3]
[0061] The results of the interfacial contact resistance and corrosion performance measured as described above are shown in Table 4 below.
[0062] [Table 4]
[0063] For the comparative example and the working example, steering rack bars were manufactured and subjected to a cold drawing test, and the products were visually observed to see whether cracks occurred or not. The results are shown in Table 4.
[0064] Referring to Tables 1 to 4, in Examples 1 to 5 and Comparative Examples 1 to 4 in which a stainless steel base material was used, and Examples 6 to 10 and Comparative Examples 5 to 8 in which a titanium base material was used, it was found that each of the Examples was superior in terms of corrosion performance and interfacial contact resistance when compared to the Comparative Examples.
[0065] Specifically, when the amount of electrolyte or coating material is outside the range of the present invention, a noticeable decrease in performance was observed in both interfacial contact resistance and corrosion performance compared to other examples using the same base material, and it was confirmed that the interfacial contact resistance performance decreased when the applied current and coating temperature were outside a certain range. This means that appropriate coating process conditions have a significant impact on achieving the objectives of the present invention.
[0066] In the heat treatment step, it was found that the heat treatment temperature and heat treatment time each affect the interfacial contact resistance and the corrosion performance. In particular, it was confirmed that the heat treatment time has a significant effect on the interfacial contact resistance, and the heat treatment temperature has a significant effect on the corrosion performance.
[0067] Although the present invention has been described with reference to the preferred embodiment, various modifications and variations can be made by those skilled in the art. As long as such modifications and variations do not deviate from the scope of the present invention, they can be said to belong to the present invention. Therefore, the scope of the present invention should be determined by the claims set forth below. [Industrial Applicability]
[0068] INDUSTRIAL APPLICABILITY The present invention can be applied in the field of fuel cells and the field of separators for fuel cells, and can improve the reliability and competitiveness of products in the relevant fields.
Claims
1. Preparing a base material; The base material is applying a coating agent containing platinum (Pt) and an electrolyte to form a discontinuous coating film; and A step of heat treating the base material with the coating film; 2. A method for manufacturing a metal separator for a vehicle fuel cell, comprising:
2. The coating agent is selected from the group consisting of gold (Au), ruthenium (Ru), iridium (Ir), and ruthenium oxide (RuO 2 ), and iridium oxide (IrO 2 2. The method of claim 1, further comprising at least one selected from the group consisting of:
3. 2. The method for manufacturing a metal separator for a vehicle fuel cell according to claim 1, wherein the base material is a stainless steel plate, titanium or aluminum plate.
4. 2. The method of claim 1, wherein the coating film forming step is any one of electrolytic plating, electroless plating, and PVD.
5. The platinum (Pt) contained in the coating agent is chloroplatinic acid (H 2 PtCl 6 ) or potassium chloroplatinate (K 2 PtCl 6 2. The method for manufacturing a metal separator plate for a vehicle fuel cell according to claim 1, further comprising:
6. 2. The method of claim 1, wherein the heat treatment is performed at a temperature in the range of 80 to 600.degree. C. for a time in the range of 10 to 180 minutes.
7. 2. The method of claim 1, wherein the heat treatment is performed under any one of a vacuum, air, and an oxygen atmosphere.
8. A metal separator plate for a vehicle fuel cell manufactured by the method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Metal separation plate for fuel cells with a coating film formed on its surface and method for manufacturing the same
JP2013501340A
Conductive member, manufacturing method thereof and fuel cell separator using the same, and polymer electrolyte fuel cell
JP2016143596A
Bipolar plate for fuel cell and method for production thereof
WO2003026052A1
Separator for fuel cell and method for producing same
WO2006126613A1