High-hardness optical windows with anti-reflection coatings that have low reflectance and transmittance in the visible range for use in infrared sensing systems
A high-hardness optical window with a multilayer film structure addresses the vulnerability of LIDAR systems to collisions by ensuring high transmittance and low reflectance in the infrared range, enhancing durability and performance while maintaining signal integrity and appearance.
Patent Information
- Application Number
- JP2024519296
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-27
- Filing Date
- 2022-10-07
- Publication Date
- 2024-10-28
AI Technical Summary
Infrared sensing systems, such as LIDAR systems, are vulnerable to damage from collisions with objects like stones, causing scattering of electromagnetic beams and degrading system performance.
A high-hardness optical window with a multilayer film structure comprising alternating layers of high and low refractive index materials, designed to provide high transmittance and low reflectance in the infrared range, while incorporating a scratch-resistant layer to minimize damage from impacts.
The window enhances the durability and performance of LIDAR systems by preventing beam scattering and maintaining signal integrity, while also offering a dark, aesthetically pleasing appearance.
Smart Images

Figure 2024538944000001_ABST
Abstract
Description
Priority
[0001] This application claims the benefit of priority under 35 U.S.C. § 120 of U.S. patent application Ser. No. 63 / 257,814, filed October 20, 2021, Ser. No. 63 / 344,147, filed May 20, 2022, and Ser. No. 63 / 410,320, filed September 27, 2022, the disclosures of all of which are incorporated herein by reference. [Technical field]
[0002] The present disclosure relates to high hardness optical windows for infrared sensing systems having anti-reflective coatings with low reflectance and transmittance in the visible range. [Background technology]
[0003] A light detection and ranging (LIDAR) system includes an electromagnetic wave emitter and a detector. The electromagnetic wave emitter emits an electromagnetic wave emitter beam. The emitted electromagnetic wave emitter beam may be reflected by an object, and the reflected electromagnetic wave emitter beam is detected by a detector. The electromagnetic wave emitter beam is radially extended, such as in a pulsed manner, to detect objects throughout the field of view. Information about the object can then be deciphered from the characteristics of the detected reflected electromagnetic wave emitter beam. The distance from the electromagnetic wave emitter to the object can be determined from the time of flight of the electromagnetic wave emitter beam from when the electromagnetic wave emitter beam is emitted until the reflected electromagnetic wave emitter beam is detected. If the object is moving, the path and speed of the object can be determined by determining the radial shift of the position where the emitted electromagnetic wave emitter beam is detected as a reflected beam as a function of time, or by measuring the Doppler frequency.
[0004] Infrared detection systems mounted in exposed environments, such as LIDAR systems mounted on automobiles (e.g., infrared detection systems for aerospace and home security applications), need to be protected from the environment and various damage factors, for example by cover lenses or cover glass windows. In addition, other applications are also possible, in which the LIDAR system is mounted on a vehicle to realize assisted driving, semi-autonomous driving, or fully autonomous driving due to the spatial mapping function provided by the LIDAR system. In such applications, the electromagnetic radiation detector is mounted on the roof of the vehicle or on a low part of the front part of the vehicle. In vehicle LIDAR applications, electromagnetic wave emitters that emit electromagnetic waves with wavelengths outside the visible light range, such as 905 nm and 1550 nm, are being considered. In addition, to protect the electromagnetic radiation detector from collisions with objects such as stones, a window is installed at a position in the line of sight of the electromagnetic radiation detector between the electromagnetic radiation detector and the outside world. Similarly, in other LIDAR system applications, such as aerospace and home security applications, a window is installed between the electromagnetic wave emitter / detector and the outside world. Summary of the Invention [Problem to be solved by the invention]
[0005] However, when an object such as a stone hits a window, the window is scratched or otherwise damaged, causing the emitted electromagnetic wave emitter beam and the reflected electromagnetic wave emitter beam to be scattered by the window, thereby reducing the effectiveness of the LIDAR system. [Means for solving the problem]
[0006] The present disclosure provides a solution to the above problems with a window including a first multilayer and a second multilayer. When the window is mounted in a LIDAR system, the first multilayer can be oriented away from the electromagnetic wave emitter / detector, and the first multilayer can incorporate a scratch-resistant layer to provide damage resistance to the window. Thus, when an object such as a stone strikes the window, the window is less likely to develop defects that would scatter the emitted or reflected electromagnetic wave emitter beam, improving performance. Additionally, the first multilayer and the second multilayer include alternating layers of materials having different refractive indices, including materials that provide hardness and scratch resistance. The number and thickness of the alternating layers can be configured to provide the window with high transmission and low reflectance in a desired wavelength range (e.g., a 50 nm wide wavelength range within the range of 1400 nm to 1600 nm). Additionally, the alternating layers of materials can be selected to provide a relatively low transmission and reflection of waves in the visible spectrum. This reduces signal noise due to visible light impinging on the LIDAR system's detector, while also giving the window an aesthetically pleasing dark appearance.
[0007] According to one embodiment of the present disclosure, a window for a sensing system is disclosed. The window comprises a substrate, the substrate having a first surface and a second surface, the first surface and the second surface being major surfaces of the substrate. The window also comprises a first multilayer film. The first multilayer film is disposed on the first surface of the substrate. The first multilayer film includes alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the first multilayer film being higher than the refractive index of the one or more low refractive index materials of the first multilayer film. The window also comprises a second multilayer film. The second multilayer film is disposed on the second surface of the substrate. The second multilayer film includes alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the second multilayer film being higher than the refractive index of the one or more low refractive index materials of the second multilayer film. The first multilayer has a maximum window hardness of at least 8 GPa as measured by Berkovich hardness testing. The number, thickness, number of layers, and materials of the alternating layers in the first and second multilayers are configured such that the average transmittance of the window measured in a 50 nm wide target wavelength range within a range of 1400 nm to 1600 nm is greater than 90% for light incident on the first and second faces at an angle of incidence of 15° or less, the average reflectance of the window measured in a 50 nm wide target wavelength range within a range of 1400 nm to 1600 nm is less than 1% for light incident on the first and second faces at an angle of incidence of 15° or less, and the average transmittance of the window measured in a range of 400 nm to 700 nm is less than 5% for light incident on the first and second faces at an angle of incidence of 15° or less.
[0008] According to another embodiment of the present disclosure, a window for a sensing system is disclosed. The window comprises a substrate, the substrate having a first surface and a second surface, the first surface and the second surface being major surfaces of the substrate. The window also comprises a first multilayer film. The first multilayer film is disposed on the first surface of the substrate. The first multilayer film includes alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the first multilayer film being higher than the refractive index of the one or more low refractive index materials of the first multilayer film. The window also comprises a second multilayer film. The second multilayer film is disposed on the second surface of the substrate. The second multilayer film includes alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the second multilayer film being higher than the refractive index of the one or more low refractive index materials of the second multilayer film. The first multilayer film has a maximum hardness of at least 8 GPa as measured by Berkovich hardness testing. The number, thickness, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the average reflectance of the window measured in a 50 nm wide target wavelength range within a range of 1400 nm to 1600 nm is less than 0.5% for light incident on the first and second faces at an angle of 15° or less, the CIELAB L* value of the window for an incident angle of 60° or less on the first multilayer film is 45 or less, and the CIELAB a* and b* values of the window as viewed from the first multilayer film are -6.0 or more and 6.0 or less.
[0009] According to another embodiment of the present disclosure, a window for a sensing system is disclosed. The window comprises a substrate, the substrate having a first surface and a second surface, the first surface and the second surface being major surfaces of the substrate. The window also comprises a first multilayer film. The first multilayer film is disposed on the first surface of the substrate. The first multilayer film includes alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the first multilayer film being higher than the refractive index of the one or more low refractive index materials of the first multilayer film. The window also comprises a second multilayer film. The second multilayer film is disposed on the second surface of the substrate. The second multilayer film includes alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the second multilayer film being higher than the refractive index of the one or more low refractive index materials of the second multilayer film, the one or more high refractive index materials of the second multilayer film including silicon. The first multilayer film has a maximum hardness of at least 8 GPa as measured by Berkovich hardness testing. The number, thickness, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the average reflectance of the window measured in a 50 nm wide target wavelength range within 1400 nm to 1600 nm for light incident on the first and second faces at an angle of 15° or less is less than 1%, and the average transmittance of the window measured in a 50 nm wide target wavelength range within 1400 nm to 1600 nm for light incident on the first and second faces at an angle of 15° or less is greater than 90%.
[0010] Additional features and advantages are described in the detailed description that follows, and in part will become apparent to those skilled in the art from the description, or may be learned by practice of the embodiments described herein, including the following detailed description, claims, and accompanying drawings.
[0011] It should be understood that both the foregoing general description and the following detailed description are merely exemplary and are intended to provide an overview or framework for understanding the nature and features of the claimed invention. The accompanying drawings are included to provide a further understanding, and are incorporated in and constitute a part of this specification. The drawings illustrate one or more embodiments and, together with the following detailed description, serve to explain the principles and operation of various embodiments. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a side view of a vehicle in an external environment, illustrating a LIDAR system on the roof of the vehicle and another LIDAR system on the front of the vehicle, in accordance with one or more embodiments of the present disclosure. [Diagram 2] FIG. 2 is a schematic diagram of one of the LIDAR systems of FIG. 1 , illustrating an electromagnetic radiation detector within a housing emitting electromagnetic waves that exit the housing through a window and return through the window as a reflected wave, in accordance with one or more embodiments of the present disclosure. [Diagram 3] FIG. 3 is a cross-sectional view of the window shown in FIG. 2 in region III of FIG. 2, illustrating that the window comprises a substrate, a multilayer film on a first side of the substrate, and a second multilayer film on a second side of the substrate, in accordance with one or more embodiments of the present disclosure. [Figure 4] FIG. 4 is a cross-sectional view of the window shown in FIG. 3 in region IV of FIG. 3 , in accordance with one or more embodiments of the present disclosure, illustrating a multilayer film including alternating layers of one or more high refractive index materials and one or more low refractive index materials, where an edge of the multilayer film closest to the external environment is provided by one of the layers of the one or more low refractive index materials. [Diagram 5] FIG. 4 is a cross-sectional view of the window shown in FIG. 3 at region V of FIG. 3 , illustrating a second multilayer including alternating layers of one or more high refractive index materials and one or more low refractive index materials, where an end surface of the second multilayer closest to the electromagnetic radiation detector is provided by one of the layers of the one or more low refractive index materials, in accordance with one or more embodiments of the present disclosure. [Figure 6]1 is a graph showing the refractive index and extinction coefficient as a function of wavelength for a silicon material used in a second multilayer film in a window of Example 1, which is configured by disposing a first multilayer film and a second multilayer film on a glass substrate, in accordance with one or more embodiments of the present disclosure; [Figure 7] 1 is a graph showing the visible-to-infrared performance, as determined by modeling, of the two-sided reflectance and transmittance across the wavelength range of 400 nm to 1600 nm for light normally incident on the window of Example 1 in accordance with one or more embodiments of the present disclosure. [Figure 8] 1 is a graph showing modeled two-sided transmission for light normally incident on the first multilayer coating of the window of Example 1 in the infrared wavelength range of interest, 1500 nm to 1600 nm, according to one or more embodiments of the present disclosure. [Figure 9] 1 is a graph showing the P-polarized light transmittance and the S-polarized light transmittance of two surfaces in the infrared wavelength range of interest, 1500 nm to 1600 nm, for light incident at an angle of incidence of 60 degrees on the first multilayer coating of the window of Example 1, as obtained by modeling, in accordance with one or more embodiments of the present disclosure. [Figure 10] 1 is a graph showing modeled two-sided reflectance for light perpendicularly incident on the first and second multilayers of the window of Example 1 in the infrared wavelength range of interest, 1500 nm to 1600 nm, according to one or more embodiments of the present disclosure. [Figure 11] FIG. 13 is a graph showing modeled two-sided transmission for light in the visible spectrum normally incident on the first multilayer film of the window of Example 1, in accordance with one or more embodiments of the present disclosure. [Figure 12A] FIG. 1 is a graph showing CIELAB color space a* and b* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 1 in accordance with one or more embodiments of the present disclosure. [Figure 12B] FIG. 13 is a graph showing CIELAB lightness L* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 1, in accordance with one or more embodiments of the present disclosure. [Figure 13]1 is a graph showing nanoindentation hardness as a function of depth into a first multilayer for two samples constructed according to the window of Example 1, in accordance with one or more embodiments of the present disclosure. [Figure 14] 1 is a graph showing the refractive index and extinction coefficient as a function of wavelength for a silicon material used in a second multilayer film in a window of Example 2, which is configured by disposing a first multilayer film and a second multilayer film on a glass substrate, in accordance with one or more embodiments of the present disclosure; [Figure 15] 1 is a graph showing the visible-to-infrared performance, as obtained by modeling, of the two-sided reflectance and transmittance across the wavelength range of 400 nm to 1600 nm for light normally incident on the window of Example 2 in accordance with one or more embodiments of the present disclosure. [Figure 16] 1 is a graph showing modeled two-sided transmission for light normally incident on the first multilayer coating of the window of Example 2 in the infrared wavelength range of interest, 1500 nm to 1600 nm, according to one or more embodiments of the present disclosure. [Figure 17] 1 is a graph showing the P-polarized light transmittance and S-polarized light transmittance of two surfaces in the infrared wavelength range of interest, 1500 nm to 1600 nm, for light incident at an angle of incidence of 60 degrees on the first multilayer coating of the window of Example 2, as obtained by modeling, in accordance with one or more embodiments of the present disclosure. [Figure 18] 1 is a graph showing modeled two-sided reflectance for light perpendicularly incident on the first and second multilayers of a window of Example 2 in the infrared wavelength range of interest, 1500 nm to 1600 nm, according to one or more embodiments of the present disclosure. [Figure 19] FIG. 13 is a graph showing modeled two-sided transmission for light in the visible spectrum normally incident on the first multilayer film of the window of Example 2, in accordance with one or more embodiments of the present disclosure; [Figure 20A] FIG. 13 is a graph showing CIELAB color space a* and b* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 2, in accordance with one or more embodiments of the present disclosure. [Figure 20B]FIG. 13 is a graph showing CIELAB lightness L* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 2, in accordance with one or more embodiments of the present disclosure. [Figure 21] 1 is a graph showing the visible-to-infrared performance, obtained by modeling, of Example 3 including a first multilayer and a second multilayer for light normally incident across the wavelength range of 400 nm to 1600 nm for two-sided reflectance and transmittance; [Figure 22] 1 is a graph showing modeled two-sided transmission for light normally incident on the first multilayer coating of the window of Example 3 in the infrared wavelength range of interest, 1500 nm to 1600 nm, according to one or more embodiments of the present disclosure. [Figure 23] 1 is a graph showing the P-polarized light transmittance and S-polarized light transmittance of two surfaces in the infrared wavelength range of interest, 1500 nm to 1600 nm, for light incident at an angle of incidence of 60 degrees on the first multilayer coating of the window of Example 3, as obtained by modeling, in accordance with one or more embodiments of the present disclosure. [Figure 24] 1 is a graph showing modeled two-sided reflectance for light normally incident on the first and second multilayers of a window of Example 3 in the infrared wavelength range of interest, 1500 nm to 1600 nm, according to one or more embodiments of the present disclosure. [Diagram 25] FIG. 13 is a graph showing modeled two-sided transmission for light in the visible spectrum normally incident on the first multilayer film of the window of Example 3, in accordance with one or more embodiments of the present disclosure. [Figure 26A] FIG. 13 is a graph showing CIELAB color space a* and b* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 3 in accordance with one or more embodiments of the present disclosure. [Figure 26B] FIG. 13 is a graph showing CIELAB lightness L* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 3, in accordance with one or more embodiments of the present disclosure. [Figure 27]1 is a graph showing the visible-to-infrared performance of Example 4, including a first multilayer and a second multilayer, for normally incident light across the wavelength range of 400 nm to 1600 nm in terms of two-sided reflectance and transmittance, as determined by modeling, in accordance with one or more embodiments of the present disclosure. [Figure 28] 1 is a graph showing modeled two-sided transmission for light normally incident on the first multilayer of the window of Example 4 in the infrared wavelength range of interest, 1500 nm to 1600 nm, according to one or more embodiments of the present disclosure. [Figure 29] 1 is a graph showing the P-polarized light transmittance and the S-polarized light transmittance of two surfaces in the infrared wavelength range of interest, 1500 nm to 1600 nm, for light incident at an angle of incidence of 60 degrees on the first multilayer coating of the window of Example 4, as obtained by modeling, in accordance with one or more embodiments of the present disclosure. [Diagram 30] 1 is a graph showing modeled two-sided reflectance for light normally incident on the first and second multilayers of the window of Example 4 in the infrared wavelength range of interest, 1500 nm to 1600 nm, according to one or more embodiments of the present disclosure. [Diagram 31] FIG. 13 is a graph showing modeled two-sided transmission for light in the visible spectrum normally incident on the first multilayer film of the window of Example 4, in accordance with one or more embodiments of the present disclosure. [Figure 32A] FIG. 13 is a graph showing CIELAB color space a* and b* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 4 in accordance with one or more embodiments of the present disclosure. [Figure 32B] FIG. 13 is a graph showing CIELAB lightness L* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 4 in accordance with one or more embodiments of the present disclosure. [Diagram 33] 1 is a graph showing the visible-to-infrared performance, as determined by modeling, of Example 5, including a first multilayer and a second multilayer, for light normally incident across the wavelength range of 400 nm to 1600 nm, in terms of two-sided reflectance and transmittance. [Diagram 34]1 is a graph showing modeled two-sided transmission for light normally incident on the first multilayer coating of the window of Example 5 in the infrared wavelength range of interest, 1500 nm to 1600 nm, according to one or more embodiments of the present disclosure. [Diagram 35] 1 is a graph showing the P-polarized light transmittance and the S-polarized light transmittance of two surfaces in the infrared wavelength range of interest, 1500 nm to 1600 nm, for light incident at an angle of incidence of 60 degrees on the first multilayer coating of the window of Example 5, as obtained by modeling, in accordance with one or more embodiments of the present disclosure. [Diagram 36] 1 is a graph showing modeled two-sided reflectance for light normally incident on the first and second multilayers of the window of Example 5 in the infrared wavelength range of interest, 1500 nm to 1600 nm, according to one or more embodiments of the present disclosure. [Figure 37] FIG. 13 is a graph showing modeled two-sided transmission for light in the visible spectrum normally incident on the first multilayer film of the window of Example 5, according to one or more embodiments of the present disclosure. [Figure 38A] FIG. 13 is a graph showing CIELAB color space a* and b* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 5, in accordance with one or more embodiments of the present disclosure. [Figure 38B] FIG. 13 is a graph showing CIELAB lightness L* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 5 in accordance with one or more embodiments of the present disclosure. [Figure 39] 1 is a graph showing the refractive index and extinction coefficient as a function of wavelength for a silicon material used in a second multilayer film in a window of Example 6, which is configured by disposing a first multilayer film and a second multilayer film on a glass substrate, in accordance with one or more embodiments of the present disclosure; [Diagram 40] 1 is a graph showing modeled visible-to-infrared performance for two-sided transmission across the wavelength range of 400 nm to 1600 nm for light incident on a window of Example 6 including a first multilayer film and a second multilayer film according to one or more embodiments of the present disclosure. [Diagram 41]1 is a graph showing the visible-to-infrared performance, obtained by modeling, of Example 6 window including a first multilayer and a second multilayer across the wavelength range of 400 nm to 1600 nm for light incident thereon; [Diagram 42] FIG. 13 is a graph showing CIELAB color space a* and b* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 6, in accordance with one or more embodiments of the present disclosure. [Diagram 43] 1 is a graph showing infrared performance obtained by modeling for two-sided transmission across the wavelength range of 1500 nm to 1600 nm for light incident on a window of Example 7 including a first multilayer film and a second multilayer film according to one or more embodiments of the present disclosure. [Diagram 44] 1 is a graph showing infrared performance, as obtained by modeling, for two-sided reflectance across the wavelength range of 1500 nm to 1600 nm for light incident on a window of Example 7 including a first multilayer and a second multilayer according to one or more embodiments of the present disclosure. [Diagram 45] 1 is a graph showing modeled visible-to-infrared performance for two-sided transmission across the wavelength range of 350 nm to 1600 nm for light incident on a window of Example 7 including a first multilayer film and a second multilayer film according to one or more embodiments of the present disclosure. [Figure 46] 1 is a graph showing the visible-to-infrared performance, as determined by modeling, of Example 7 window including a first multilayer and a second multilayer across the wavelength range of 350 nm to 1600 nm for light incident thereon; [Figure 47] 1 is a graph showing modeled visible performance for two-sided transmission across the wavelength range of 400 nm to 700 nm for light incident on a window of Example 7 including a first multilayer film and a second multilayer film according to one or more embodiments of the present disclosure. [Figure 48] FIG. 13 is a graph showing CIELAB color space a* and b* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 7, in accordance with one or more embodiments of the present disclosure. [Figure 49]FIG. 13 is a graph showing CIELAB lightness L* values for light incident at multiple angles of incidence on the first multilayer coating of the window of Example 7, in accordance with one or more embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Next, an embodiment of a window for use in a LIDAR detector will be described in detail. It should be noted that the same or similar parts are designated with the same reference numerals throughout the drawings whenever possible. The windows described herein can include a first multilayer and a second multilayer composed of alternating layers of high and low refractive index materials. The first and second multilayers are configured to provide relatively high transmission and low reflectance in the desired infrared wavelength range of interest. The window can be mounted in a LIDAR system with the first multilayer facing away from the detector / radiation emitter, which is the side exposed to the outside world, and the second multilayer facing the detector / radiation emitter. That is, the first multilayer can be mounted such that it is the first multilayer that is seen by an outside observer of the LIDAR system. Light emitted from the radiation emitter can first enter the second multilayer and then propagate through the substrate. According to the present disclosure, the first multilayer of the windows described herein can include one or more relatively thick (e.g., 500 nm or more) scratch-resistant layers of high refractive index material. The scratch-resistant layers can be embedded in the first multilayer such that the maximum nanoindentation hardness of the window is 8 GPa or more (e.g., 10 GPa or more, 12 GPa or more, 14 GPa or more) as measured by performing a Berkovich hardness test on the first multilayer. Such nanoindentation hardness has the advantage of providing scratch resistance and improving the performance of the LIDAR system.
[0014] Also, in some aspects, the alternating layers in the first and second multilayers of the windows described herein are configured to provide desirable optical performance attributes in the infrared spectrum for operation of LIDAR systems. In some embodiments, the number, thickness, number of layers, and materials of the alternating layers in the first and second multilayers are configured to provide an average transmittance of the window over a 50 nm wide wavelength range of interest within the range of 1400 nm to 1600 nm for light incident on the first and second faces at an angle of incidence of 15° or less, greater than 90% (e.g., 95% or more). Also, the number, thickness, number of layers, and materials of the alternating layers in the first and second multilayers are configured to provide an average P-polarized transmittance and an average S-polarized transmittance of the window over a 50 nm wide wavelength range of interest within the range of 1400 nm to 1600 nm for light incident on the first and second faces at an angle of incidence of 60° or less, greater than 85% (e.g., 90% or more, 93% or more).
[0015] In yet further aspects, the first and second multilayers of the windows described herein can be constructed to have relatively low visible light reflectance and transmittance. This can provide an aesthetically pleasing dark appearance to the window while eliminating signal noise. In some embodiments, for example, the number, thickness, number of layers, and materials of alternating layers in the first and second multilayers are configured to provide an average transmittance of the window below 5% for light incident on the first multilayer at an angle of incidence of 15° or less, measured in the range of 400 nm to 700 nm. Such low visible light transmittance can be achieved by incorporating a silicon layer in the amount described herein into the second multilayer. This can provide the windows described herein with a CIELAB lightness L* value of 45 or less (e.g., 40 or less, 35 or less, 30 or less) when viewed at an angle of 60° or less from the first multilayer (i.e., from outside the LIDAR detector). Additionally, the windows described herein can exhibit CIELAB color space a* and b* values when viewed through the first multilayer film of from -6 to 6 (e.g., from -5 to 5, from -4 to 4, from -3 to 3, from -2.5 to 2.5). The color of the window when viewed from the first multilayer film side can be black or a relatively dark color so that the window is not noticeable to an outside viewer.
[0016] Thus, the windows described herein provide durable anti-reflective performance for the desired wavelength range of 1400 nm to 1600 nm while providing a black or dark appearance that is aesthetically pleasing and provides performance enhancement. The windows described herein can improve the performance of LIDAR detectors over existing detectors by preventing visible light from entering the detector, improving the signal to noise ratio. Additionally, the windows described herein can reduce unpleasant glare to the eyes of an outside viewer.
[0017] Unless otherwise noted, the total reflectance, specular reflectance, and average reflectance values given herein are two-sided reflectance values that represent the total reflectance of the entire window, including the reflectance associated with each material interface of the window (e.g., air-multilayer interface, multilayer-substrate interface, etc.) Also, unless otherwise noted, reflectance values in the infrared are measured from the side of the second multilayer described herein (e.g., the side facing the detector / emitter of a LIDAR system) and reflectance values in the visible are measured from the side of the first multilayer described herein (e.g., the side facing the outside world of a LIDAR system).
[0018] Unless otherwise specified in this specification, the average transmittance and average reflectance values are determined using the reflectance values (%) and transmittance values (%) at various wavelengths within a specified wavelength range. The average transmittance and average reflectance values can be determined by measuring at least three reflectance values or transmittance values within a desired wavelength range and averaging the values.
[0019] Unless otherwise specified in this specification, the CIELAB color space a* value, b* value and lightness L* value are measured / simulated under the conditions of a standard observer with a 10-degree field of view using a D65 light source.
[0020] As used herein, the terms "dark appearance" or "black appearance" refer to the reflective appearance of a window when viewed from the exterior surface. Windows having a dark or black appearance according to the present disclosure have a CIELAB lightness L* value below 45 when viewed at an angle of 60° or less.
[0021] It is to be noted that, unless expressly stated otherwise, no method described herein is intended to be construed as requiring that the steps be performed in a particular order. Thus, unless a method claim actually recites the order of the steps, or unless otherwise expressly stated in the claims or detailed description of the invention that the steps are limited to a particular order, no order of steps is intended to be inferred in any respect. This applies to all non-express matters that may be the basis of interpretation, such as matters of reasoning about the sequence or sequence of steps, common meanings derived from grammatical constructions or punctuation, the number or type of embodiments described herein, etc.
[0022] As used herein, the term "and / or" when used in conjunction with a list of two or more items means that any one of the listed items may be used alone, or any combination of two or more of the listed items may be used. For example, if a composition is described as containing components A, B, and / or C, the composition may contain A alone, B alone, C alone, a combination of A and B, a combination of A and C, a combination of B and C, or a combination of A, B, and C.
[0023] Modifications of the present disclosure will occur to those skilled in the art and those who make or use the present disclosure. Therefore, it should be understood that the above-described embodiments shown in the drawings are for illustrative purposes only and are not intended to limit the scope of the present disclosure. The scope of the present disclosure is defined by the following claims, which are to be construed in accordance with patent law principles, including the doctrine of equivalents.
[0024] As used herein, relational terms such as first and second, top and bottom, etc., are used only to distinguish one entity or operation from another and do not necessarily require or imply any actual relationship or order between these entities or operations. The terms "comprise", "including", "having" and other variations thereof have a non-exclusive inclusion meaning. Thus, when a process, method, article, or apparatus "comprises" ("includes" or "has") a recited element, it does not include only the recited elements, but may also include other elements not expressly recited, or elements inherent to such process, method, article, or apparatus. When an element preceded by the article "a" is described as "comprising" ("including" or "having"), it does not exclude the presence of additional elements identical to the recited element in the process, method, article, or apparatus that includes the element, unless a further limiting condition is provided.
[0025] In this specification, the term "about" means that a quantity or characteristic, such as an amount, size, composition, parameter, etc., is not necessarily exact or does not have to be exactly the value, but rather can be an approximation and / or a value around that quantity or characteristic, incorporating tolerances, conversion factors, rounding, measurement error, and other factors known to those skilled in the art, as necessary. Thus, when the term "about" is used to describe a value or an endpoint of a range, it is to be understood that the particular value or endpoint is included in the disclosure. In this specification, regardless of whether a value or an endpoint of a range is introduced with "about", the endpoint of the value or range is intended to include two embodiments, that is, an embodiment modified by "about" and an embodiment not modified by "about". It will also be understood that the meanings of the endpoints of each range are both relative to each other and independent of each other.
[0026] Additionally, the term "formed from" can mean one or more of "comprise," "consist essentially of," or "consist of." For example, when a component is "formed from" a particular material, the component may comprise, consist essentially of, or consist of the particular material.
[0027] Additionally, as used herein, the terms "article," "glass-article," "ceramic-article," "glass-ceramic," "glass element," and "glass-ceramic article(s)" are used interchangeably in their broadest sense and include any object made in whole or in part from glass and / or glass-ceramic materials.
[0028] As used herein, the term "disposed" is used to refer to a layer or sublayer that is provided on a surface by methods such as coating, deposition, forming, etc. The term "disposed" can include providing a layer / sublayer directly on an adjacent layer / sublayer, or providing a layer / sublayer separated by an intervening material that may or may not form a layer.
[0029] Unless otherwise specified herein, the refractive index of materials described herein is measured at 1550 nm.
[0030] 1, a vehicle 10 is equipped with one or more LIDAR systems 12. The one or more LIDAR systems 12 may be located anywhere on or within the vehicle 10. For example, the one or more LIDAR systems 12 may be located on a roof 14 of the vehicle 10, a front portion 16 of the vehicle 10, or both.
[0031] 2, each of the one or more LIDAR systems 12 includes an electromagnetic radiation detector 18 as known in the art. The electromagnetic radiation detector 18 may be housed within a housing 20. The electromagnetic radiation detector 18 emits an electromagnetic wave 22 having a wavelength or range of wavelengths. The emitted electromagnetic wave 22 exits the housing 20 through a window 24 that is on the path of the electromagnetic wave. If an object (not shown) in an external world 26 is on the path of the electromagnetic wave 22, the emitted electromagnetic wave 22 will reflect off the object and return to the electromagnetic radiation detector 18 as a reflected wave 28. The reflected wave 28 also passes through the window 24 to reach the electromagnetic radiation detector 18. In various embodiments, the emitted wave 22 and the reflected wave 28 may include light within a suitable wavelength range of interest. For example, in embodiments, emitted wave 22 and reflected wave 28 can be between 1400 nm and 1600 nm (e.g., between 1500 nm and 1600 nm, between 1525 nm and 1575 nm, about 1550 nm, 1550 nm). It is contemplated that electromagnetic waves other than reflected wave 28 (e.g., electromagnetic waves having wavelengths in the visible spectrum, some ultraviolet range, etc.) may also interact with window 24. As described herein, window 24 may include a multi-layer coating having a layer structure designed to absorb visible spectrum light and reflect a relatively small amount of visible spectrum light, thereby giving the window a dark or black appearance when viewed from outside housing 20.
[0032] The "visible spectrum" is the portion of the electromagnetic spectrum visible to the human eye, and generally refers to electromagnetic waves with wavelengths within the range of about 380 nm or 400 nm to about 700 nm. The "ultraviolet range" is the portion of the electromagnetic spectrum with wavelengths from about 10 nm to about 400 nm. The "infrared range" of the electromagnetic spectrum is the region of long wavelengths above about 700 nm. The sun produces solar electromagnetic waves, commonly called "sunlight," whose wavelengths fall within these three ranges.
[0033] 3, each window 24 of the one or more LIDAR systems 12 includes a substrate 30. The substrate 30 has a first surface 32 and a second surface 34. The first surface 32 and the second surface 34 are the major surfaces of the substrate 30. The first surface 32 is the surface closest to the external world 26. The second surface 34 is the surface closest to the electromagnetic radiation detector 18. The outgoing wave 22 encounters the second surface 34 before encountering the first surface 32. Meanwhile, the reflected wave 28 encounters the first surface 32 before encountering the second surface 34. The substrate 30 further includes a first multilayer film 36 disposed on the first surface 32 of the substrate 30 and a second multilayer film 38 disposed on the second surface 34 of the substrate 30. It should be understood that the window 24 described herein is not limited to vehicle applications, but may be utilized in any application in which the window 24 would benefit from the improved crashworthiness and optical performance described in detail herein.
[0034] Substrate 30 can be constructed from a variety of different materials consistent with the teachings of this disclosure. In embodiments, substrate 30 can be constructed from any type of glass, glass-ceramic, ceramic, or suitable polymer-based material. Various examples of the structure and composition of substrate 30 are now described in detail.
[0035] In embodiments, substrate 30 comprises a glass composition or is a glass article. Substrate 30 can comprise, for example, borosilicate glass, aluminosilicate glass, soda-lime glass, chemically strengthened borosilicate glass, chemically strengthened aluminosilicate glass, or chemically strengthened soda-lime glass. In embodiments, the glass composition of substrate 30 is a composition that can be chemically strengthened by an ion exchange process. In embodiments, this composition can be a lithium ion-free composition.
[0036] An alkali aluminosilicate glass composition suitable for substrate 30 includes alumina, at least one alkali metal, and SiO. In some embodiments, the glass composition includes more than 50 mol% SiO, in other embodiments at least 58 mol% SiO, and in still other embodiments at least 60 mol% SiO, and has a ratio (Al2O3+B2O3) / Σ 修飾物質 (i.e., the sum of modifiers) is greater than 1, the component ratios are expressed in mole percent, and the modifiers in the formula are alkali metal oxides. In a particular embodiment, the composition comprises 58-72 mole percent SiO2, 9-17 mole percent Al2O3, 2-12 mole percent B2O3, 8-16 mole percent Na2O, and 0-4 mole percent K2O, and the ratio (Al2O3+B2O3) / Σ 修飾物質 is greater than 1.
[0037] Other alkali aluminosilicate glass compositions suitable for substrate 30 include 64-68 mol% SiO2, 12-16 mol% Na2O, 8-12 mol% Al2O3, 0-3 mol% B2O3, 2-5 mol% K2O, 4-6 mol% MgO, and 0-5 mol% CaO, where 66 mol%≦SiO2+B2O3+CaO≦69 mol%, Na2O+K2O+B2O3+MgO+CaO+SrO>10 mol%, 5 mol%≦MgO+CaO+SrO≦8 mol%, (Na2O+B2O3)-Al2O3≦2 mol%, 2 mol%≦Na2O-Al2O3≦6 mol%, and 4 mol%≦(Na2O+K2O)-Al2O3≦10 mol%.
[0038] Other alkali aluminosilicate glass compositions suitable for substrate 30 include 2 mol % or more of Al2O3 and / or ZrO2, or 4 mol % or more of Al2O3 and / or ZrO2.
[0039] An example of a glass composition includes SiO2, B2O3, and Na2O, where (SiO2+B2O3)≧66 mol% and Na2O≧9 mol%. In one embodiment, the composition includes at least 6 wt% aluminum oxide. In a further embodiment, the composition of one or more alkaline earth oxides, for example the content of alkaline earth oxides, is at least 5 wt%. In some embodiments, a suitable composition further includes at least one of K2O, MgO, and CaO. In a particular embodiment, the composition of the substrate 30 includes 61-75 mol% SiO2, 7-15 mol% Al2O3, 0-12 mol% B2O3, 9-21 mol% Na2O, 0-4 mol% K2O, 0-7 mol% MgO, and 0-3 mol% CaO.
[0040] Yet another exemplary composition suitable for substrate 30 includes 60-70 mol% SiO2, 6-14 mol% Al2O3, 0-15 mol% B2O3, 0-15 mol% Li2O, 0-20 mol% Na2O, 0-10 mol% K2O, 0-8 mol% MgO, 0-10 mol% CaO, 0-5 mol% ZrO2, 0-1 mol% SnO2, 0-1 mol% CeO2, less than 50 ppm As2O3, and less than 50 ppm Sb2O3, where 12 mol%≦(Li2O+Na2O+K2O)≦20 mol%, and 0 mol%≦(MgO+CaO)≦10 mol%.
[0041] Yet another exemplary glass composition suitable for substrate 30 includes 63.5-66.5 mol% SiO2, 8-12 mol% Al2O3, 0-3 mol% B2O3, 0-5 mol% Li2O, 8-18 mol% Na2O, 0-5 mol% K2O, 1-7 mol% MgO, 0-2.5 mol% CaO, 0-3 mol% ZrO2, 0.05-0.25 mol% SnO2, 0.05-0.5 mol% CeO2, less than 50 ppm As2O3, and less than 50 ppm Sb2O3, where 14 mol%≦(Li2O+Na2O+K2O)≦18 mol%, and 2 mol%≦(MgO+CaO)≦7 mol%.
[0042] The substrate 30 can be a substantially flat or sheet-like substrate, although other embodiments can utilize substrates that are formed or shaped into other shapes, such as curved shapes. The length and width of the substrate 30 can vary depending on the desired dimensions of the window 24. The substrate 30 can be formed using a variety of methods, such as float glass processes or down-draw processes (e.g., fusion draw, slot draw). The substrate 30 can be used in an untempered state. A commercially available example of an untempered substrate 30 suitable for the window 24 is Corning® Glass Code 2320, a sodium aluminosilicate glass substrate.
[0043] The glass forming the substrate 30 can be modified so that the region continuous with the first surface 32 and / or the region continuous with the second surface 34 is subjected to compressive stress ("CS"). In such a case, the region subjected to compressive stress extends from the first surface 32 and / or the second surface 34 to the compression depth. Furthermore, due to the occurrence of compressive stress in this manner, a region subjected to tensile stress is formed in the center. The tensile stress has a maximum value at the center of this central region, and this value is called the central tension (CT). The central region extends between the compression depths and is subjected to tensile stress. The tensile stress in the central region is balanced with the compressive stress in the region subjected to compressive stress (works to counteract the compressive stress). In this specification, "depth of compression" and "DOC" refer to the depth within the substrate 30 where the stress changes from compressive stress to tensile stress. The compression depth is the depth where the stress changes from positive (compressive) to negative (tensile), and thus the stress value is zero at the compression depth. The compression depth protects the substrate 30 from cracks caused by a sharp impact on the first side 32 and / or second side 34 of the substrate 30 from propagating beyond the compression depth, and the compressive stress minimizes the likelihood of a grown crack breaking through the compression depth. In some embodiments, each compression depth is at least 20 μm. In some embodiments, the absolute value of the maximum compressive stress Cs in the region subjected to compressive stress is at least 200 MPa, at least about 400 MPa, at least 600 MPa, or up to about 1000 MPa.
[0044] Two methods for extracting a detailed and accurate stress profile (stress as a function of depth) of a substrate 30 having regions under compressive stress are disclosed in U.S. Patent No. 9,140,543, entitled "Systems and Methods for Measuring Stress Profile of Ion-Exchanged Glass," filed May 3, 2012 by Douglas Clippinger Alan et al., which claims the benefit of priority from U.S. Provisional Patent Application No. 61 / 489,800, filed May 25, 2011, the entire disclosure of which is incorporated herein by reference.
[0045] In some embodiments, creating regions of compressive stress in substrate 30 includes subjecting substrate 30 to an ion-exchange chemical tempering process (chemical tempering is often referred to as "chemical strengthening"). In an ion-exchange chemical tempering process, ions at or near first side 32 and second side 34 of substrate 30 are replaced with larger ions, typically of the same valence or oxidation state. In embodiments in which substrate 30 comprises (or consists essentially of, or consists of) alkali aluminosilicate glass, alkali borosilicate glass, alkali aluminoborosilicate glass, or alkali silicate glass, the ions in the surface layer of the glass and the larger ions are selected from the group consisting of Na, ... + (Li + is present in the glass), K + , Rb + , Cs + Alternatively, the monovalent cations in or near the first surface 32 and the second surface 34 may be replaced with a monovalent cation other than an alkali metal cation, such as Ag + etc.) can also be substituted.
[0046] In some embodiments, the ion-exchange process is performed by immersing the substrate 30 in a molten salt bath containing larger ions that will replace the smaller ions in the substrate 30. Parameters of the ion-exchange process include, but are not limited to, bath composition and temperature, immersion time, number of times the glass is immersed in the salt bath(s), use of multiple salt baths, and additional steps such as annealing and washing steps. Those skilled in the art will appreciate that such ion-exchange process parameters are typically determined by the composition of the substrate 30 and the desired compression depth and compressive stress of the substrate 30 as a result of the strengthening process. By way of example, ion-exchange of an alkali metal-containing glass substrate can be performed by immersing the substrate in at least one molten bath containing salts of larger alkali metal ions (such as, but not limited to, nitrates, sulfates, chlorides, etc.). In some embodiments, the molten salt bath includes potassium nitrate (0-100% by weight), sodium nitrate (0-100% by weight), and lithium nitrate (0-12% by weight), with the combined weight percent of potassium nitrate and sodium nitrate being in the range of 88% to 100% by weight. In embodiments, the temperature of the molten salt bath typically ranges from about 350° C. to about 500° C., and the immersion time ranges from about 15 minutes to about 40 hours, such as from about 20 minutes to about 10 hours, although other temperatures and immersion times can be used. Substrate 30 can be treated, such as by acid polishing, to remove or reduce the effects of surface defects.
[0047] In some embodiments, the substrate 30 includes a glass-ceramic material having both a glass phase and a ceramic phase. Exemplary glass-ceramics include materials in which the glass phase is formed from silicates, borosilicates, aluminosilicates, or aluminoborosilicates, and the ceramic phase is formed from β-spodumene, β-quartz, nepheline, kalsilite, or carnegiete. "Glass-ceramic" includes materials that are produced using controlled glass crystallization. Examples of suitable glass-ceramics include Li2O-Al2O3-SiO2-based (i.e., LAS-based) glass ceramics, MgO-Al2O3-SiO2-based (i.e., MAS-based) glass ceramics, ZnOxAl2O3xnSiO2 (i.e., ZAS-based), and / or glass ceramics that include β-quartz solid solution, β-spodumene, cordierite, lithium disilicate, or the like, as the predominant crystalline phase. The glass-ceramic substrate can be strengthened using a chemical strengthening process.
[0048] In embodiments, substrate 30 comprises a ceramic material, such as an inorganic crystal, such as an oxide, nitride, carbide, oxynitride, and / or carbonitride, etc. Exemplary ceramics include materials having an alumina phase, an aluminum titanate phase, a mullite phase, a cordierite phase, a zircon phase, a spinel phase, a perovskite phase, a zirconia phase, a ceria phase, a silicon carbide phase, a silicon nitride phase, a silicon aluminum oxynitride phase, or a zeolite phase.
[0049] In some embodiments, the substrate 30 comprises an organic or suitable polymeric material. Examples of suitable polymers include, but are not limited to, thermoplastics such as polystyrene (PS) (including styrene copolymers and blends), polycarbonate (PC) (including copolymers and blends), polyester (including copolymers and blends such as polyethylene terephthalate copolymers and polyethylene terephthalate copolymers), polyolefins (PO) and cyclic polyolefins (cyclic PO), polyvinyl chloride (PVC), acrylic polymers (including copolymers and blends) including polymethyl methacrylate (PMMA), thermoplastic urethanes (TPU), polyetherimides (PEI), and blends of these polymers. Other exemplary polymers include epoxy resins, styrene resins, phenolic resins, melamine resins, and silicone resins.
[0050] In some embodiments, the substrate 30 includes multiple layers or sublayers. The layers or sublayers of the substrate 30 may be the same or different from each other. In some embodiments, for example, the substrate 30 includes a glass laminate. In some embodiments, the glass laminate includes a first glass sheet and a second glass sheet, which are bonded to each other via a suitable interlayer (e.g., a polymer interlayer) disposed between the first glass sheet and the second glass sheet. In some embodiments, the glass laminate includes a glass-on-glass laminate (e.g., a laminate formed by a fusion draw process). Glass-polymer laminates are also within the scope of the present disclosure. Any material may be used for the substrate 30 as long as it can meet the optical requirements described herein.
[0051] In embodiments, substrate 30 exhibits a modulus of elasticity (Young's modulus) in the range of about 30 GPa to about 120 GPa. In some examples, the modulus of elasticity of the substrate can be in the range of about 30 GPa to about 110 GPa, about 30 GPa to about 100 GPa, about 30 GPa to about 90 GPa, about 30 GPa to about 80 GPa, about 30 GPa to about 70 GPa, about 40 GPa to about 120 GPa, about 50 GPa to about 120 GPa, about 60 GPa to about 120 GPa, about 70 GPa to about 120 GPa, and all ranges and sub-ranges therebetween.
[0052] In embodiments, substrate 30 exhibits an average transmittance in the visible wavelength range of about 85% or more, about 86% or more, about 87% or more, about 88% or more, about 89% or more, about 90% or more, about 91% or more, or about 92% or more. In embodiments, substrate 30 includes a color component (e.g., a color layer or colorant) and can optionally exhibit a color, such as white, black, red, blue, green, yellow, orange, etc.
[0053] As shown in FIG. 3, the substrate 30 has a thickness 35 defined as the shortest linear distance between the first surface 32 and the second surface 34. In some embodiments, the thickness 35 of the substrate 30 is about 100 μm to about 5 mm. In some embodiments, the physical thickness 35 of the substrate 30 can be in the range of about 100 μm to about 500 μm (e.g., 100 μm, 200 μm, 300 μm, 400 μm, or 500 μm). In other embodiments, the thickness 35 is in the range of about 500 μm to about 1000 μm (e.g., 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, or 1000 μm). The thickness 35 can also be greater than about 1 mm (e.g., about 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, or 7 mm). In one or more specific embodiments, the thickness 35 is 2 mm or less or 1 mm or less.
[0054] In embodiments, thickness 35 is uniform enough that substrate 30 has a planar shape (e.g., thickness 35 varies less than 1% across the substrate). In embodiments, thickness 35 is a non-uniform thickness, having a value that varies as a function of position on substrate 30. For aesthetic and / or functional reasons, thickness 35 can vary along one or more of its dimensions. For example, the edges of substrate 30 can be thicker than the center of substrate 30. The length, width, and physical thickness dimensions of substrate 30 can also vary depending on the application of article 30.
[0055] In some embodiments, the substrate 30 includes a layer of a material that absorbs visible light and transmits infrared light. Examples of such materials include acrylic sheets that transmit infrared light and absorb visible light, such as those available from ePlastics under the tradenames Plexiglas® IR acrylic 3143 and CYRO under the tradename ACRYLITE® IR acrylic 1146. "Plexiglas" IR acrylic 3143 has a transmittance of about 0% (at least less than 10%, or less than 1%) for electromagnetic waves with wavelengths of about 700 nm or less, but has a transmittance of about 90% (greater than 85%) for wavelengths within the range of 800 nm to about 1100 nm (including 905 nm).
[0056] In embodiments, substrate 30 exhibits a refractive index in the range of about 1.45 to about 1.55. In embodiments, the average transmittance of the substrate across the entire spectral range of 1400 nm to 1600 nm is 95% or greater (e.g., 96% or greater, 97% or greater, 98% or greater, 99% or greater, 99.5% or greater).
[0057] 4 and 5, both the first multilayer film 36 and the second multilayer film 38 have a certain number of alternating layers of one or more high refractive index materials 40 and one or more low refractive index materials 42. Although the layers of the one or more high refractive index materials 40 and the one or more low refractive index materials 42 are identified by the same reference numbers, it should be understood that the use of the same reference numbers does not imply that the layers are made of the same material or have the same structure. In both the first multilayer film 36 and the second multilayer film 38, the different layers of the high refractive index materials 40 and the different layers of the low refractive index materials 42 can have different compositional or structural properties.
[0058] As used herein, the terms "higher refractive index" and "lower refractive index" refer to refractive index values relative to one another and mean that the refractive index of one or more high refractive index materials 40 is higher than the refractive index of one or more low refractive index materials 42. In some embodiments, the refractive index of one or more high refractive index materials 40 is about 1.7 to about 4.0. In some embodiments, the refractive index of one or more low refractive index materials 42 is about 1.3 to about 1.6. In some embodiments, the refractive index of one or more low refractive index materials 42 is about 1.3 to about 1.7, and the refractive index of one or more high refractive index materials 40 is about 1.9 to about 3.8. The difference in refractive index between any one of the one or more high refractive index materials 40 and any one of the one or more low refractive index materials 42 can be about 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more, 1.0 or more, 1.5 or more, 2.0 or more, 2.1 or more, 2.2 or more, or even 2.3 or more. Due to the difference in refractive index between the one or more high refractive index materials 40 and the one or more low refractive index materials 42, by manipulating the number (number of layers) of alternating layers and their thicknesses, electromagnetic waves within a certain wavelength range can be selectively transmitted through the window 24 and, independently, electromagnetic waves within a certain wavelength range can be selectively reflected by the first multilayer film 36. Thus, the first multilayer film 36 (and, if utilized, the second multilayer film 38) is a thin-film optical filter having predetermined optical properties configured as a function of the quantity, thickness, number of layers, and materials selected for the one or more high refractive index materials 40 and the one or more low refractive index materials 42.
[0059] Some examples of materials suitable for use as the one or more low refractive index materials 42 are SiO2, Al2O3, GeO2, SiO, AlO x N y , SiO x N y , Si u Al v O x N y, MgO, MgAl2O4, MgF2, BaF2, CaF2, DyF3, YbF3, YF3, CeF3, etc. The material used as the one or more low refractive index materials 42 (e.g., AlO x N y , SiO x N y , Si u Al v O x N y The nitrogen content (in materials such as Cr, Cu, Ni, and Fe) can be minimized.
[0060] Some examples of materials suitable for use as the one or more high refractive index materials 40 include Si, amorphous silicon (a-Si), SiN x , SiN x :H y , AlN x , Si u Al v O x N y , Ta2O5, Nb2O5, AlN, Si3N4, AlO x N y , SiO x N y , HfO2, TiO2, ZrO2, Y2O3, Al2O3, MoO3, diamond-like carbon, etc. x Material or AlN x The oxygen content in the material can be minimized. x N y The material is oxygen-doped AlN. x In other words, AlN x The high refractive index material(s) 40 may have a crystal structure of AlON (e.g., a wurtzite structure), but need not have a crystal structure of AlON. x N y The material may include about 0 atomic % to about 20 atomic % oxygen, or about 5 atomic % to about 15 atomic % oxygen and 30 atomic % to about 50 atomic % nitrogen. u Alv O x N y can contain about 10 atomic % to about 30 atomic % or about 15 atomic % to about 25 atomic % silicon, about 20 atomic % to about 40 atomic % or about 25 atomic % to about 35 atomic % aluminum, about 0 atomic % to about 20 atomic % or about 1 atomic % to about 20 atomic % oxygen, and about 30 atomic % to about 50 atomic % nitrogen. In addition, hydrogen can be added to the above material up to about 30 mass %. Note that the refractive indexes of the one or more high refractive index materials 40 and the one or more low refractive index materials 42 are relative to each other, so the same material (e.g., Al2O3) may be considered suitable for one or more high refractive index materials 40 based on the refractive index of the material selected as the one or more low refractive index materials 42, or may be considered suitable for one or more low refractive index materials 42 based on the refractive index of the material selected for the one or more high refractive index materials 40.
[0061] In some embodiments, the one or more low refractive index materials 42 of the first multilayer 36 are comprised of SiO layers, and the one or more high refractive index materials 40 of the first multilayer 36 are comprised of SiO layers. x N y layer or SiN x In some embodiments, the one or more low index materials 42 of the first multilayer 36 are comprised of SiO2 layers and the one or more high index materials 40 of the first multilayer 36 are comprised of SiN x layer or SiO x N y In one embodiment, the one or more low refractive index materials 42 of the first multilayer 36 are SiO2 layers and the one or more high refractive index materials 40 of the second multilayer 38 include silicon layers (e.g., a-Si layers). In some embodiments, the one or more low refractive index materials 42 of the first multilayer 36 are SiO2 layers and the one or more high refractive index materials 40 of the first multilayer 36 include SiN x layer or SiO x N y The one or more low refractive index materials 42 of the second multilayer film 38 are made of SiO2 layers, and the one or more high refractive index materials 40 of the second multilayer film 38 are made of amorphous silicon layers (a-Si layers) and SiN xlayer or SiO x N y and a layer.
[0062] In either the first multilayer film 36 or the second multilayer film 38, the number of alternating layers of the high refractive index material 40 and the low refractive index material 42 is not particularly limited. In some embodiments, the number of such alternating layers in the first multilayer film 36 is 7 or more, 9 or more, 11 or more, 13 or more, 15 or more, 17 or more, 19 or more, 21 or more, 23 or more, 25 or more, 51 or more, or 81 or more. In some embodiments, the number of alternating layers in the second multilayer film 38 is 7 or more, 9 or more, 11 or more, 13 or more, 15 or more, 17 or more, 19 or more, 21 or more, 23 or more, 25 or more, 51 or more, or 81 or more. In various embodiments, the number of alternating layers in the first and second multilayer films 36 and 38 making up the window 24 (excluding the substrate 30) is 14 or more, 20 or more, 26 or more, 32 or more, 38 or more, 44 or more, 50 or more, 72 or more, or 100 or more. In general, the greater the number of layers in the first and second multilayer films 36 and 38, the narrower the range of transmittance and reflectance properties of the window 24 to one or more particular wavelengths or wavelength ranges.
[0063] The alternating layers of the first multilayer 36 and the alternating layers of the second multilayer 38 have a thickness. The thickness selected for each alternating layer determines the optical path length of light propagating through the window 24 and determines the amplification or attenuation due to interference between the various light rays reflected at each material interface of the window 24. Thus, the thickness of each alternating layer in combination with the refractive indices of the one or more high index materials 40 and the one or more low index materials 42 determine the reflectance and transmittance spectra of the window 24.
[0064] 3, 4 and 5, when the reflected wave 28 interacts with the window 24, it first encounters an end surface 44 of the first multilayer film 36. The end surface 44 may be open to the outside world 26. In one embodiment, the end surface 44 is made of one of the layers of the one or more low refractive index materials 42, which makes the refractive index of the end surface 44 closer to the refractive index of the air of the outside world 26, thereby reducing the reflection of the electromagnetic wave (whether the electromagnetic wave is the reflected wave 28 or not) incident on the end surface 44 at the end surface 44. The layer of the one or more layers of the low refractive index materials 42 that makes up the end surface 44 is the layer of the first multilayer film 36 that is located farthest from the substrate 30. Similarly, in some embodiments, when the one or more low refractive index materials 42 are SiO2, the one or more layers of the low refractive index materials 42, the SiO2 layer, are disposed directly on the first surface 32 of the substrate 30 (which typically has a large mole % of SiO2 in the substrate 30). Without wishing to be bound by theory, it is believed that the substrate 30 and the one or more adjacent layers of low index material 42 both comprise SiO2, which may enhance bond strength.
[0065] On the other hand, when the outgoing wave 22 interacts with the window 24, it first encounters the end surface 48 of the second multilayer film 38. In one embodiment, the end surface 48 is constructed from one of the layers of the one or more low index materials 42, which makes the index of refraction of the end surface 48 closer to the index of refraction of the air in the housing 20, thereby reducing the reflection of the outgoing wave 22 incident on the end surface 48 at the end surface 48. The layer of the one or more layers of the low index material 42 that constitutes the end surface 48 is the layer of the second multilayer film 38 that is furthest from the substrate 30. Similarly, in some embodiments, when the one or more low index materials 42 are SiO2, the one or more layers of the low index material 42, the SiO2 layer, are disposed directly on the second surface 34 of the substrate 30.
[0066] A material having a relatively high refractive index may also have a relatively high hardness, providing scratch resistance and impact resistance. An example of a high hardness material that may be one of the one or more high refractive index materials 40 is SiO. x N y Another example of a high hardness material that can be one of the one or more high refractive index materials 40 is SiN.x , SiN x :H y , Si3N4. Relatively thick (e.g., 500 nm or more) SiO x N y It has been found that employing a layer (or other suitable high refractive index material layer) can enhance the scratch resistance, damage resistance, or both of the window 24. Such enhanced scratch and damage resistance may be particularly beneficial in the first multilayer 36, which is more likely to encounter debris impact from the external environment 26. Thus, in some embodiments, a layer of the one or more high refractive index materials 40 in the first multilayer 36 has a thickness of 500 nm or more (e.g., 1000 nm or more, 1500 nm or more, 2000 nm or more). Such a high refractive index layer having a thickness of 500 nm or more is referred to herein as a "scratch resistant layer."
[0067] In some embodiments, the thickness and location of the scratch-resistant layer within the first multilayer film 36 can be optimized to provide a desired level of hardness and scratch resistance to the first multilayer film 36, and thus the entire window 24. The desired thickness of the scratch-resistant layer of the high refractive index material 40 that functions as a layer that provides hardness and scratch resistance to the window 24 can vary depending on the application of the window 24. For example, the thickness of the scratch-resistant layer of the high refractive index material 40 required for a window 24 protecting a LIDAR system 12 on a vehicle 10 can be different from the thickness required for a window 24 protecting a LIDAR system 12 in an office building. In some embodiments, the thickness of the scratch-resistant layer of the high refractive index material 40 that functions as a layer that provides hardness and scratch resistance to the window 24 can be 500 nm to 50,000 nm, such as 500 nm to 10,000 nm, such as 2,000 nm to 5,000 nm. In embodiments, the thickness of the scratch-resistant layer of high refractive index material 40 is 30% or more, 40% or more, 50% or more, 65% or more, or 85% or more, or 86% or more of the thickness of the first multilayer 36. Note that the scratch-resistant layer of high refractive index material 40, which functions as the layer that provides hardness and scratch resistance to window 24, is typically, but not necessarily, part of the first multilayer 36 that faces the outside world 26, rather than the second multilayer 38 that is protected by the housing 20.
[0068] As will be described in more detail below, the quantity, thickness, number of layers, and materials of the remaining layers of the first multilayer 36 and the second multilayer 38 can be selected to provide the window 24 with the desired optical properties (desired transmittance and reflectance at the desired wavelengths). This can be done largely independent of the thickness of the scratch-resistant layer of the high refractive index material 40 that serves as the layer that provides hardness and scratch resistance to the window 24. The optical properties of the overall window 24 are less sensitive to the thickness of the scratch-resistant layer of the high refractive index material 40 that serves as the layer that provides hardness and scratch resistance to the window 24 when the scratch-resistant layer material has relatively low or negligible optical absorption for electromagnetic radiation at the targeted wavelength or wavelength range (e.g., 1400 nm to 1600 nm, 1550 nm). For example, Si3N4 has negligible absorption of electromagnetic radiation at wavelengths of 700 nm to 2000 nm.
[0069] In this way, since the overall optical characteristics are not easily affected by the thickness of the scratch-resistant layer of the high refractive index material 40 in the first multilayer film 36, it is possible to set the thickness of the scratch-resistant layer in advance so as to satisfy a predetermined hardness requirement or scratch resistance requirement. For example, the hardness requirement and scratch resistance requirement are considered to be different between the first multilayer film 36 for the window 24 used in the roof 14 of the vehicle 10 and the first multilayer film 36 for the window 24 used in the front part 16 of the vehicle 10, and therefore the thickness required for the scratch-resistant layer of the high refractive index material 40 is considered to be different. The thickness of the scratch-resistant layer can be set in accordance with such requirements without significantly changing the transmittance and reflectance characteristics of the first multilayer film 36 as a whole.
[0070] The hardness of the first multilayer 36 having a scratch resistant layer of high refractive index material 40, and therefore the window 24, can be quantified. In some embodiments, the maximum hardness of the window 24 measured by performing a Berkovich indenter hardness test on the first multilayer 36 having a scratch resistant layer of high refractive index material 40 at one or more indentation depths ranging from 50 nm to 2000 nm (measured from the end face 44), or even 2000 nm to 5000 nm, can be about 8 GPa or more, about 10 GPa or more, about 12 GPa or more, about 14 GPa or more, about 15 GPa or more, about 16 GPa or more, or about 18 GPa or more. As used herein, the term "Berkovich Indenter Hardness Test" includes measuring the hardness of a material at a surface by indenting a diamond Berkovich indenter into the surface of the material. The Berkovich indentation hardness test includes a step of indenting the end surface 44 of the first multilayer film 36 with a diamond Berkovich indenter to a depth ranging from about 50 nm to about 2000 nm (or the entire thickness of the first multilayer film 36) and a step of measuring the maximum hardness from the indentation over the entire indentation depth range or a portion of the indentation depth range (e.g., a range from about 100 nm to about 600 nm). The hardness test is typically described in Oliver, WC, Pharr, GM, "An improved technique for determining hardness and elastic modulus using load and displacement sensing indentation experiments," J. Mater. Res., Vol. 7, No. 6, 1992, pp. 1564-1583, and Oliver, WC, Pharr, GM, "Measurement of Hardness and Elastic Modulus by Instrument Indentation: Advances in Understanding and Refinements to Methodology," J. Mater. Res., Vol. 19, No. 1, 2004, pp. 3-20.The above levels of hardness improve the window 24's resistance to damage when struck by objects such as sand, pebbles, and debris that may be encountered while using the LIDAR system 12 for its intended purpose (e.g., installation in the vehicle 10 (see FIG. 1 )). Thus, the above levels of hardness reduce or prevent the LIDAR system 12 from scattering light due to impact damage and degrading performance that would occur if the LIDAR system did not have the above levels of hardness.
[0071] In some embodiments, at least a portion of the first multilayer 36 is disposed between the scratch-resistant layer of high refractive index material 40 and the end face 44. In some embodiments, the first multilayer 36 includes multiple alternating layers of one or more low refractive index materials 42 and one or more high refractive index materials 40 between the end face 44 and the scratch-resistant layer. Such alternating layer stacks disposed between the scratch-resistant layer and the end face 44 are referred to herein as "optical control layers." In some embodiments, the optical control layers disposed between the scratch-resistant layer and the end face 44 have a total thickness of 500 nm or more (e.g., 600 nm or more, 700 nm or more, 800 nm or more, 900 nm or more, 1000 nm or more, 1100 nm or more, 1200 nm or more, 1300 nm or more). The quantity, composition, and thickness of the optical control layers can be selected to provide the desired anti-reflective performance attributes described herein at the operating wavelength of the LIDAR system 12, which is in the range of 1400 nm to 1600 nm, such that the first multilayer film 36 can be designed to provide desirable optical performance characteristics, as described herein, in the visible and / or UV spectrum.
[0072] In some embodiments, at least 25% (e.g., at least 26%, at least 27%, at least 28%, at least 29%, at least 30%) of the thickness 46 of the first multilayer film 36 is disposed between the scratch-resistant layer and the end surface 44. By positioning the scratch-resistant layer in the first multilayer film 36 at such a depth, it is believed that the nanoindentation hardness (measured by a Berkovich indenter hardness test) of the first multilayer film 36 is promoted to be relatively high over a relatively long depth range in the first multilayer film 36. In some embodiments, the nanoindentation hardness of the first multilayer film 36 in the depth range of 250 nm to 2000 nm is 8 GPa or more. In some embodiments, the nanoindentation hardness of the first multilayer film 36 in the depth range of 1000 nm to 2000 nm is 8.5 GPa or more. By setting the hardness value in this range, it becomes easier to obtain scratch resistance and damage resistance against cracks of a relatively wide range of depths.
[0073] 4 and 5, the first multilayer 36 has a thickness 46 and the second multilayer 38 has a thickness 50. The thickness 46 of the first multilayer 36, which is assumed to include one or more scratch-resistant layers of high refractive index material 40, can be about 1 μm or more to provide the transmittance and reflectance characteristics described herein. In some embodiments, the thickness 46 is in the range of 1 μm to slightly more than 50 μm, such as about 1 μm to about 10 μm, about 2800 nm to about 5900 nm. The lower limit of about 1 μm is approximately the minimum thickness 46 that can provide hardness and scratch resistance to the window 24. On the other hand, the upper limit of the thickness 46 is limited by the cost and time required to place the layers of the first multilayer 36 on the substrate 30. In addition, the upper limit of the thickness 46 is also limited to prevent the first multilayer 36 from causing warping of the substrate 30. This limit depends on the thickness of the substrate 30. The thickness 50 of the second multilayer film 38 may be any thickness deemed necessary to impart the desired transmittance and reflectance characteristics to the window 24. In some embodiments, the thickness 50 of the second multilayer film 38 is within a range of about 800 nm to about 7000 nm.
[0074] The number, thickness, number of layers, and materials of the layers in the first multilayer film 36 and the second multilayer film are configured to solve the problem described in the above section "Problems to be Solved by the Invention" by maximizing the thickness of the high refractive index material 40 to impart hardness, impact resistance, and scratch resistance to the window 24, and to provide a relatively high infrared transmittance of the window 24 at 1400 nm to 1600 nm. In several embodiments, the thickness, number, and materials of the alternating layers in the first multilayer film 36 and the second multilayer film 38 are configured to provide an average transmittance of the window 24 of 90% or more (e.g., 91% or more, 92% or more, 93% or more, 94% or more, 95% or more) for light incident on the first surface 32 and the second surface 34 at an angle of 15° or less with respect to the normal to the first surface 32 and the second surface 34, in a target wavelength range of 50 nm in width within the range of 1400 nm to 1600 nm.
[0075] In several embodiments, the thicknesses, number of layers, and materials of the alternating layers in the first multilayer film 36 and the second multilayer film 38 are configured so that the average reflectance of the window 24 determined in a 50 nm wide target wavelength range within the range of 1400 nm to 1600 nm is 0.5% or less (e.g., 0.4% or less, 0.3% or less, 0.2% or less, 0.1% or less, 0.08% or less) for light incident on the first surface 32 and the second surface 34 at an angle of 15° or less relative to the normal to the first surface 32 and the second surface 34. In several embodiments, the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film 36 and the second multilayer film 38 are configured so that the average P-polarized light transmittance and average S-polarized light transmittance of the window determined in a 50 nm wide target wavelength range within the range of 1400 nm to 1600 nm are greater than 85% (e.g., 86% or more, 87% or more, 88% or more, 89% or more, 90% or more, 91% or more, 92% or more) for light incident on the first surface 32 and the second surface 34 at an angle of 60° or less relative to the normal to the first surface 32 and the second surface 34 (e.g., an incident angle of 0° to 60°, 0° to 50°, 0° to 40°, 0° to 30°). As used herein, the term "reflectance" is defined as the percentage of optical power of incident light, of wavelengths within a given wavelength range, that is reflected by a material (e.g., window 24, substrate 30, first multilayer 36, second multilayer 38, or portions thereof).
[0076] In some embodiments, the thicknesses, number of layers, and materials of the alternating layers in the first multilayer film 36 and the second multilayer film 38 are configured to provide an average transmittance of the window 24 of 95% or more (e.g., 95.5% or more, 96% or more, 96.5% or more, 97.5% or more, 98% or more) for light perpendicularly incident on the first face 32 and the second face 34 in a 50 nm wide target wavelength range within the range of 1400 nm to 1600 nm. In this specification, the terms "transmittance" and "percentage transmission" are used synonymously to refer to the percentage of optical power that is transmitted through a material (e.g., the window 24, the substrate 30, the first multilayer film 36, the second multilayer film 38, or a portion thereof) of incident light having a wavelength within a predetermined wavelength range.
[0077] Additionally, in various embodiments, the thicknesses, number of layers, and materials of the alternating layers of the first multilayer film 36 and the second multilayer film 38 are further configured (as well as configured to meet the infrared optical performance requirements described herein) to provide a desired dark appearance to the window 24. For example, the window 24 may exhibit a CIELAB color space a* value for light incident on the first surface 32 at an angle of incidence between 0° and 90° when viewed from the outside world 26 (see FIG. 1) of −6.0 to 6.0. The window 24 may exhibit a CIELAB color space b* value for light incident on the first surface 32 at an angle of incidence between 0° and 90° of −6.0 to 6.0 (e.g., −5.0 to 5.0, −4.0 to 4.0, −3.0 to 3.0, −2.5 to 2.5, −2.5 to 0.0). Such color space values may be achieved even in embodiments in which substrate 30 has a relatively high transmittance (eg, 90% or greater) and a relatively low reflectance (eg, 22% or less) across the visible spectrum.
[0078] In some embodiments, the thicknesses, number of layers, and materials of the alternating layers in the first multilayer film 36 and the second multilayer film 38 are configured to provide a CIELAB lightness L* value of 45 or less (e.g., 40 or less, 35 or less, 30 or less) for the window 24 when viewed at an incidence angle of 60° or less. In some embodiments, the thicknesses, number of layers, and materials of the alternating layers in the first multilayer film 36 and the second multilayer film 38 are configured to provide a CIELAB lightness L* value of less than 20 for the window 24 reflecting light normally incident on the first multilayer film 36. The set of CIELAB color space values and lightness values listed above represent a relatively dark appearance for the window 24 when viewed at various incidence angles.
[0079] The window 24 may have a dark appearance by including silicon (e.g., in the form of a-Si) in the second multilayer 38 as one of the one or more high refractive index materials 40. In addition to having a relatively high refractive index (approximately 3.8 at 1550 nm), amorphous silicon (a-Si) has a relatively high optical absorption in the ultraviolet and visible regions, while having an acceptably low optical absorption in the 900-1800 nm region. Thus, the thickness and number of amorphous silicon layers (a-Si layers) in addition to the other layers in the first multilayer 36 and second multilayer 38 can provide a window 24 that has low electromagnetic transmission in the ultraviolet and visible regions (due in part to the absorbance of amorphous silicon in both wavelength regions), but high transmission in the desired range of the infrared region. In some embodiments, the second multilayer 38 includes one or more layers of amorphous silicon (a-Si layers) as one of the one or more high refractive index materials 40, while the first multilayer 36 does not include an amorphous silicon layer (a-Si layer). Such a structure has the advantage that the silicon is protected from the external environment 26 since it is located only on the back side of the substrate 30. Thus, the nanoindentation hardness values described herein can be achieved by incorporating a scratch resistant layer in the first multilayer 36, and the dark appearance can be achieved by including silicon in the second multilayer 38.
[0080] In some embodiments, the alternating layers in the second multilayer film 38 made of silicon have a total thickness of 250 nm or more (e.g., 300 nm or more, 325 nm or more, 350 nm or more, 375 nm or more, 400 nm or more, 500 nm or more). In some embodiments, the layers in the second multilayer film 38 made of silicon may have a total thickness of 250 nm or more. In some embodiments, the thickness of the silicon layers in the second multilayer film 38 totals at least 35% (e.g., at least 40%, at least 45%, at least 50%) of the thickness 50 of the second multilayer film 38. Applicant has found that such a silicon thickness sufficiently absorbs visible light such that the average transmittance of window 24 measured in the range of 400 nm to 700 nm for light incident on first and second faces 32, 34 at angles of 15° or less relative to the normal to first and second faces 32, 34 is less than 5% (e.g., 4.5% or less, 4.0% or less, 3.5% or less, 3.0% or less, 2.5% or less, 2.0% or less, 1.5% or less, 1.0% or less, 0.9% or less, 0.8% or less, 0.7% or less, 0.6% or less, 0.5% or less, 0.4% or less, 0.3% or less, 0.2% or less, 0.1% or less). This improves the signal-to-noise ratio of LIDAR system 12 by preventing the portion of reflected wave 28 (see FIG. 2) that contains visible light from reaching radiation detector 18.
[0081] In some embodiments, the second multilayer film 38 includes two or more layers formed from silicon. In some embodiments, at least one of the two or more layers formed from silicon has a thickness of 150 nm or more (e.g., 160 nm or more, 170 nm or more, 180 nm or more, 190 nm or more, 200 nm or more). In some embodiments, at least two of the two or more layers formed from silicon in the second multilayer film 38 (but fewer than the total number of layers) have a thickness of 150 nm or more. In some embodiments, at least seven of the alternating layers in the second multilayer film 38 are disposed between one of the silicon layers having a thickness of 150 nm or more and the second surface 34. In some embodiments, the thickness of each of the less than 150 nm silicon layers on the second surface side of the second multilayer film 38 is 70 nm or less (e.g., 65 nm or less, 60 nm or less, 55 nm or less, 50 nm or less, 30 nm or less, 25 nm or less, 20 nm or less). It is believed that spacing the relatively thick silicon layers from the substrate 30 in this manner helps reduce reflectance in the visible spectrum.
[0082] In embodiments, the alternating layers in the first multilayer 36 and second multilayer 38 are constructed to have a relatively low average reflectance in the visible spectrum. For example, in embodiments, the average reflectance of the window measured in the wavelength range of 400 nm to 700 nm is 10% or less (e.g., 9% or less, 8% or less, 7% or less). This low reflectance has the advantage of preventing the window 24 from appearing colored when viewed from the outside world 26 (see FIG. 1 ) and facilitating the realization of the CIE color space a* and b* values and lightness L* values described herein.
[0083] In some embodiments, to suppress the reflectance of the window in the visible spectrum, the silicon layer in the second multilayer 38 closest to the substrate 30 is the thinnest silicon layer in the second multilayer 38. That is, the layer in the second multilayer 38 in which the one or more high refractive index materials 40 are silicon is the thinnest layer closest to the substrate 30. In some embodiments, the silicon layer in the second multilayer 38 closest to the substrate 30 is 10 nm or less (e.g., 8 nm or less, 7 nm or less, 6 nm or less, 5 nm or less, 4 nm or less, 3 nm or less, 2 nm or less). Applicants have found that such a structure has the advantage of preventing colored reflectance from the silicon-containing layer in the second multilayer 38 while contributing to the relatively low visible transmittance described herein.
[0084] In some embodiments, the layer of the one or more layers of high index material 40 in the second multilayer 38 closest to the substrate 30 is not a layer of silicon. In some embodiments, for example, the layer of the one or more layers of high index material 40 closest to the substrate 30 is made of the same high index material (e.g., SiN) as the high index material used in the first multilayer. x , SiO x N y , Si3N4). In embodiments, the layer of one or more layers of high refractive index material 40 in second multilayer 38 closest to substrate 30 is the only layer of high refractive index layers in second multilayer 38 that is not composed of silicon. Without wishing to be bound by theory, applicants believe that such a structure can contribute to reduced reflectance in the visible spectrum when second multilayer 38 includes silicon, particularly when second multilayer 38 has silicon layers each having a thickness of 8 nm or greater.
[0085] Each layer in the first multilayer film 36 and the second multilayer film 38 (i.e., the layers of high refractive index material 40 and the layers of low refractive index material 42) can be formed by any method known in the art, such as a discontinuous deposition process or a continuous deposition process. In one or more embodiments, the layers can be formed exclusively by a continuous deposition process or an exclusively discontinuous deposition process. EXAMPLES
[0086] All of the following examples are modeling examples that utilize computer-aided modeling to demonstrate how the quantity, thickness, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 can be set to produce desired average transmittance and average reflectance of window 24 as a function of wavelength and angle of incidence of incident electromagnetic radiation.
[0087] The refractive index and extinction coefficient of each material were measured as a function of wavelength over the entire spectral range from 400 nm to 1600 nm. x N y , SiN x The refractive indices and absorbances of SiO, Si, and an aluminosilicate glass substrate (Corning Code 2320) are shown below in Table A. In some of the examples below, these materials were utilized for the high refractive index material 40, the low refractive index material 42, and the substrate 30. TIFF2024538944000002.tif126166
[0088] TIFF2024538944000003.tif126166
[0089] TIFF2024538944000004.tif122170
[0090] These refractive indices were then used to calculate the transmittance and reflectance spectra. Note that, for convenience, in each table showing the modeling examples, only the refractive index value corresponding to a wavelength of about 1550 nm was selected from the refractive index dispersion curve and used as the refractive index.
[0091] Example 1 - The window 24 of Example 1 had a first multilayer 36 on a first side 32 of a substrate 30 of aluminosilicate glass (Corning Code 2320). The window 24 of Example 1 also had a second multilayer 38 on a second side 34 of the substrate 30. The first multilayer 36 was made up of SiO2 (the SiO2(1) material in Table A above) as the low refractive index material 42 and SiO2 (the SiO2(2) material in Table A above) as the high refractive index material 40. x N y The structure was such that 25 layers were alternately stacked. The 18th layer was a scratch-resistant layer made of a high refractive index material 40 having a thickness of 2000 nm. The 1st to 17th layers were light control layers that spaced the scratch-resistant layer from the end face 44. The total thickness of the 1st to 17th layers was 1398.6 nm. The 19th to 25th layers were refractive index matching layers that spaced the scratch-resistant layer from the first surface 32. The total thickness of the 19th to 25th layers was 252.1 nm. In this example, the scratch-resistant layer accounted for 54.78% of the thickness of the first multilayer film 36.
[0092] The second multilayer film 38 is configured by alternately stacking 15 layers of low refractive index material 42 and high refractive index material 40. In this embodiment, the low refractive index material 42 is SiO2, and the high refractive index material 40 is SiO x N y As shown in the table, the 28th layer (the layer of the high refractive index material 40 closest to the substrate 30 (the 26th layer in this embodiment)) was made of SiO x N y and the other layers of high refractive index material 40 were Si. Layer 30 (the Si layer closest to substrate 30) was the thinnest Si layer with a thickness of 8.1 nm. The total thickness of the silicon layers was 595 nm, accounting for 46.2% of the total thickness of second multilayer 38.
[0093] The values of the refractive index and extinction coefficient of the Si material used in Example 1 are shown in FIG. 6. As shown in the figure, the extinction coefficient of the Si material used in this example is 0.23 at 700 nm. This corresponds to an internal transmittance (transmittance of silicon only) of the total thickness of the silicon layer in Example 1 being about 1.37%. Also, the extinction coefficient at 400 nm is 2.2. Therefore, it is expected that the total transmittance of multiple silicon layers is significantly lower at 400 nm than at 700 nm.
[0094] The thicknesses of each layer in the first multilayer film 36 and the second multilayer film 38 were set as shown in Table 1 below, and were used to calculate the transmittance, reflectance, CIELAB color space values, lightness values, and nanoindentation hardness values shown in Figures 7 to 13.
[0095] [Table 1]
[0096] 7 shows a graph including a first curve 702, a second curve 704, and a third curve 706 for the window 24 according to Example 1. The first curve 702 shows the transmittance of the window 24 over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the window 24, as obtained by modeling. The second curve 704 shows the reflectance over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the second multilayer film 38, as obtained by modeling. The third curve 706 shows the reflectance over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the first multilayer film 36, as obtained by modeling. As shown, the quantity, thickness, number of layers, and materials of the first and second multilayer films 36, 38 of the window 24 of Example 1 are configured such that the window 24 has a transmittance of greater than 90% for light perpendicularly incident on the window 24 at wavelengths greater than 1420 nm. However, the transmittance is less than 2% throughout the visible spectrum. As shown by curves 704 and 706, the window 24 of Example 1 has a reflectance of less than 1% for wavelengths greater than 1500 nm when viewed from either the first or second multilayer film 36, respectively. The window of Example 1 has a reflectance of less than 9% when viewed from the first multilayer film 36 throughout the visible spectrum. Thus, the results shown in FIG. 7 demonstrate that the window 24 of Example 1 has the effect of effectively preventing transmission and reflection in the visible spectrum, while effectively exhibiting the anti-reflection performance described herein at infrared wavelengths.
[0097] As is clear from Fig. 8, the quantities, thicknesses, numbers of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 1 are configured so that the transmittance of the window 24 for light perpendicularly incident on the first surface 32 or the second surface 34 exceeds 92.25% over the entire wavelength range of 1500 nm to 1600 nm. Also, as is clear from Fig. 9, the quantities, thicknesses, numbers of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 1 are configured so that the average P-polarized light transmittance and the average S-polarized light transmittance of the window 24 obtained in the target wavelength range of 1500 nm to 1600 nm exceeds 87% for light incident on the first surface and the second surface at an angle of 60° or less with respect to the normal to the first surface and the second surface.
[0098] 10, the quantity, thickness, number of layers, and material of the first multilayer film 36 and the second multilayer film 38 of the window 24 in Example 1 are configured so that the reflectance at the end face 44 of the first multilayer film 36 and the reflectance at the end face 48 of the second multilayer film 38 of the window 24 for light perpendicularly incident on the substrate 30 are less than 0.8% in the wavelength range of approximately 1500 nm to 1600 nm. The reason why the reflectance at the end face 44 is approximately the same as the reflectance at the end face 48 is because the first multilayer film 36 and the second multilayer film 38 are made of materials having relatively low absorbance in the above-mentioned wavelength range. As shown in the figure, the reflectance obtained by modeling reached a minimum value of approximately 0.1% at approximately 1550 nm, and was less than 0.25% throughout the wavelength range of 1525 nm to 1575 nm.
[0099] As is apparent from FIG. 11, the quantities, thicknesses, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 1 are configured such that the transmittance of the window 24 is substantially below 1.0% across the entire visible spectrum. The transmittance in the visible spectrum from 400 nm to 650 nm is below 0.2%. Furthermore, the transmittance in the visible spectrum for wavelengths shorter than 600 nm is below 0.1%. It is believed that the absorption of visible light by the silicon layer of the second multilayer film 38 contributes to some extent to these low transmittance values.
[0100] As is apparent from FIG. 12A and FIG. 12B, the quantity, thickness, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 1 are configured to give the window 24 a dark appearance when viewed from the end face 44 of the first multilayer film. FIG. 12A shows CIELAB single-sided reflected color data for light reflected from the end face 44 of Example 1 obtained by simulation. The color of the single-sided reflected light can be characterized using CIELAB color coordinates. The a* axis in the color space represents the green to red color component, with negative a* values corresponding to green and positive a* values corresponding to red. The b* axis in the color space represents the blue to yellow color component, with negative b* values corresponding to blue and positive b* values corresponding to yellow. The closer the a* and b* values are to the origin, the lower the color saturation perceived by a person viewing the reflected light. The CIELA a* and b* values were generated by performing simulations at a number of different light source incidence angles ranging from 0° to 90°. As shown, the a* values range from about -2.25 to about 0.4, and the b* values range from about -2.2 to about 1.25, indicating that the window 24 according to Example 1 has a desaturated appearance when viewed from the outside world 26 (see FIG. 1).
[0101] 12B is a graph showing the CIELAB lightness L* values obtained by modeling as a function of the angle of incidence on the end face 44. As shown, the lightness L* value for angles of incidence of 60° or less is 30 or less. This indicates that the window 24 according to Example 1 has a dark appearance when viewed from the outside world 26 (see FIG. 1).
[0102] FIG. 13 shows the nanoindentation hardness measured as a function of depth for two samples constructed according to Example 1 herein. The hardness values are simulated results from performing Berkovich indenter hardness testing as described herein. The first sample was measured at a depth range of 50 nm to 1000 nm, and the second sample was measured at a depth range of 50 nm to 2000 nm. As shown in FIG. 13, both samples exhibited a first maximum hardness 1104 of greater than 8 GPa at a depth of about 250 nm. Additionally, the second sample exhibited a second maximum hardness 1102 of greater than 10 GPa at a depth of about 1050 nm. Without wishing to be bound by theory, it is believed that the maximum hardness is located above the scratch resistant layer because the stress field from the indenter propagates below the scratch resistant layer at a depth of 1050 nm. 11, the window 24 according to Example 1 exhibits a nanoindentation hardness of more than 8 GPa over the entire depth range of 250 nm to 2000 nm. Also, the window 24 according to Example 1 exhibits a nanoindentation hardness of more than 9 GPa over the entire depth range of 750 nm to 2000 nm. This indicates that the present example provides scratch resistance / damage resistance suitable for a variety of applications.
[0103] Example 2 - The window 24 of Example 2 had a first multilayer 36 on a first side 32 of a substrate 30 of aluminosilicate glass (Corning Code 2320). The window 24 of Example 2 also had a second multilayer 38 on a second side 34 of the substrate 30. The first multilayer 36 was a multilayer of SiO2 (SiO2(2) material in Table A) as the low refractive index material 42 and SiN as the high refractive index material 40. x (Table A SiN x (1) material) were alternately stacked in 21 layers. The 14th layer was a scratch-resistant layer made of high refractive index material 40 with a thickness of 2000 nm. The scratch-resistant layer was made of SiN x(2) material. The first to thirteenth layers were light control layers that spaced the scratch-resistant layer from the end face 44. The total thickness of the first to thirteenth layers was 1063.9 nm. The fifteenth to twenty-first layers were refractive index matching layers that spaced the scratch-resistant layer from the first surface 32. The total thickness of the fifteenth to twenty-first layers was 241.8 nm. In this example, the scratch-resistant layer accounted for 60.5% of the thickness of the first multilayer film 36.
[0104] The second multilayer film 38 is configured by alternately stacking 13 layers of low refractive index material 42 and high refractive index material 40. In this embodiment, the low refractive index material 42 is SiO2 (SiO2(2) material in Table A), and the high refractive index material 40 is SiN x (Table A SiN x As shown in the table, the 24th layer (the layer of the high refractive index material 40 closest to the substrate 30 (the 20th layer in this embodiment)) was made of SiN x and the other layers of high refractive index material 40 were Si. Layer 26 (the Si layer closest to substrate 30) was the thinnest Si layer with a thickness of 8.0 nm. The total thickness of the silicon layers was 414.6 nm, accounting for 39.49% of the total thickness of second multilayer 38.
[0105] The refractive index and extinction coefficient values of the Si material used in Example 2 are shown in FIG. 14. As shown in the figure, the extinction coefficient at 700 nm of the Si material used in this example is 0.29. This corresponds to an internal transmittance (transmittance of silicon only) of the total thickness of the silicon layer in Example 2 being about 2.29%. Also, the extinction coefficient at 400 nm is 2.2. Therefore, it is expected that the total transmittance of multiple silicon layers is significantly lower at 400 nm than at 700 nm.
[0106] The thickness of each layer in the first multilayer film 36 and the second multilayer film 38 was set as shown in Table 2 below, and this was used to calculate the transmittance, reflectance, CIELAB color space values and lightness values, and nanoindentation hardness shown in Figures 15 to 20B.
[0107] [Table 2]
[0108] 15 shows a graph including a first curve 1502, a second curve 1504, and a third curve 1506 for the window 24 according to Example 2. The first curve 1502 shows the transmittance of the window 24 over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the window 24, as obtained by modeling. The second curve 1504 shows the reflectance over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the first multilayer film 36, as obtained by modeling. The third curve 1506 shows the reflectance over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the second multilayer film 38, as obtained by modeling. As shown, the quantity, thickness, number of layers, and materials of the first and second multilayer films 36, 38 of the window 24 of Example 2 are configured to provide a transmittance of the window 24 of greater than 90% for light perpendicularly incident on the window 24 at wavelengths greater than 1380 nm. However, the transmittance is less than 2% throughout the visible spectrum. As shown by curves 1504 and 1506, the reflectance of the window 24 of Example 2 for wavelengths greater than 1500 nm is less than 1% when viewed from the first and second multilayer films 36, 38. The reflectance of the window of Example 2 when viewed from the first multilayer film 36 is less than 22% throughout the visible spectrum. Thus, the results shown in FIG. 15 demonstrate that the window 24 of Example 2 effectively prevents transmission and reflection in the visible spectrum while effectively providing the anti-reflection performance described herein at infrared wavelengths.
[0109] As is apparent from Fig. 16, the quantities, thicknesses, numbers of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 2 are configured so that the transmittance of the window 24 for light perpendicularly incident on the first surface 32 or the second surface 34 exceeds 99.6% over the entire wavelength range of 1500 nm to 1600 nm. Also, as is apparent from Fig. 17, the quantities, thicknesses, numbers of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 2 are configured so that the average P-polarized light transmittance and the average S-polarized light transmittance of the window 24 obtained in the target wavelength range of 1500 nm to 1600 nm exceeds 91.75% for light incident on the first surface and the second surface at an angle of 60° or less with respect to the normal to the first surface and the second surface.
[0110] 18, the quantity, thickness, number of layers, and material of the first multilayer film 36 and the second multilayer film 38 of the window 24 in Example 2 are configured so that the reflectance at the end face 44 of the first multilayer film 36 (and each layer in the window 24) of the window 24 and the reflectance at the end face 48 of the second multilayer film 38 for light perpendicularly incident on the substrate 30 are less than 0.4% in the wavelength range of approximately 1500 nm to 1600 nm. The reason why the reflectance at the end face 44 is approximately the same as the reflectance at the end face 48 is because the first multilayer film 36 and the second multilayer film 38 are made of materials having relatively low absorbance in the above-mentioned wavelength range. As shown in the figure, the reflectance obtained by modeling reached a minimum value of approximately 0.1% at approximately 1550 nm, and was less than 0.25% throughout the wavelength range of 1510 nm to 1600 nm.
[0111] As is apparent from FIG. 19, the quantities, thicknesses, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 2 are configured such that the transmittance of the window 24 is substantially below 1.0% across the entire visible spectrum. The transmittance in the visible spectrum from 400 nm to 650 nm is below 0.2%. Furthermore, the transmittance in the visible spectrum for wavelengths shorter than 550 nm is below 0.1%. It is believed that these low transmittance values are at least in part due to the absorption of visible light by the silicon layer of the second multilayer film 38.
[0112] As is apparent from FIG. 20A and FIG. 20B, the quantity, thickness, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 2 are configured to give the window 24 a dark appearance when viewed from the end face 44 of the first multilayer film. FIG. 20A shows CIELAB single-sided reflection color data for light reflected from the end face 44 of Example 2 obtained by simulation. The color of the single-sided reflected light can be characterized using CIELAB color coordinates. The a* axis in the color space represents the green to red color component, with negative a* values corresponding to green and positive a* values corresponding to red. The b* axis in the color space represents the blue to yellow color component, with negative b* values corresponding to blue and positive b* values corresponding to yellow. The closer the a* and b* values are to the origin, the lower the color saturation perceived by a person viewing the reflected light. The CIELA a* and b* values were generated by performing simulations at a number of different light source incidence angles ranging from 0° to 90°. As shown, the a* values range from about -2.0 to about 0.75, and the b* values range from about -2.1 to about 1.3, indicating that the window 24 of Example 2 has a desaturated appearance when viewed from the outside world 26 (see FIG. 1).
[0113] 20B is a graph showing the CIELAB lightness L* values obtained by modeling as a function of the angle of incidence on the end face 44. As shown, the lightness L* value for angles of incidence of 60° or less is 35 or less. This indicates that the window 24 according to Example 2 has a dark appearance when viewed from the outside world 26 (see FIG. 1).
[0114] Example 3 - The window 24 of Example 3 had a first multilayer 36 on a first side 32 of a substrate 30 of aluminosilicate glass (Corning Code 2320). The window 24 of Example 3 also had a second multilayer 38 on a second side 34 of the substrate 30. The first multilayer 36 was a multilayer of SiO2 (SiO2(1) material in Table A) as the low refractive index material 42 and SiN as the high refractive index material 40. x (Table A SiN x (1) material) was alternately stacked in 25 layers. The 18th layer was made of high refractive index material 40 (SiN in Table A) with a thickness of 2000 nm. x (2) Material) was used as the scratch-resistant layer. The first to seventeenth layers were used as light control layers that spaced the scratch-resistant layer from the end face 44. The total thickness of the first to seventeenth layers was 1387.5 nm. The nineteenth to twenty-fifth layers were used as refractive index matching layers that spaced the scratch-resistant layer from the first surface 32. The total thickness of the nineteenth to twenty-fifth layers was 249.5 nm. In this example, the scratch-resistant layer accounted for 54.99% of the thickness of the first multilayer film 36.
[0115] The second multilayer film 38 is configured by alternately stacking 15 layers of low refractive index material 42 and high refractive index material 40. In this embodiment, the low refractive index material 42 is SiO2 (SiO2(2) material in Table A), and the high refractive index material 40 is SiN x (Table A SiN x As shown in the table, the 28th layer (the layer of the high refractive index material 40 closest to the substrate 30 (the 20th layer in this embodiment)) was made of SiN x and the other layers of high refractive index material 40 were Si. Layer 30 (the Si layer closest to substrate 30) was the thinnest Si layer with a thickness of 8.0 nm. The total thickness of the silicon layers was 584.28 nm, accounting for 46.62% of the total thickness of second multilayer film 38. The silicon material used in Example 3 was the same as that described in the description of Example 2 above (the silicon material having the properties shown in FIG. 14).
[0116] The thickness of each layer in the first multilayer film 36 and the second multilayer film 38 was set as shown in Table 3 below, and this was used to calculate the transmittance, reflectance, CIELAB color space values and lightness values, and nanoindentation hardness shown in Figures 21 to 26B.
[0117] [Table 3]
[0118] 21 shows a graph including a first curve 2102, a second curve 2104, and a third curve 2106 for the window 24 according to Example 3. The first curve 2102 shows the transmittance of the window 24 over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the window 24, as obtained by modeling. The second curve 2104 shows the reflectance over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the first multilayer film 36, as obtained by modeling. The third curve 2106 shows the reflectance over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the second multilayer film 38, as obtained by modeling. As shown, the quantity, thickness, number of layers, and materials of the first and second multilayer films 36, 38 of the window 24 of Example 3 are configured such that the window 24 has a transmittance of greater than 90% for light perpendicularly incident on the window 24 at wavelengths greater than 1420 nm. However, the transmittance is less than 2% throughout the visible spectrum. As shown by curves 2104 and 2106, the window 24 of Example 3 has a reflectance of less than 1% for wavelengths greater than 1500 nm when viewed from either the first or second multilayer film 36, respectively. The window of Example 3 has a reflectance of less than 10% when viewed from the first multilayer film 36 throughout the visible spectrum. Thus, the results shown in FIG. 21 demonstrate that the window 24 of Example 3 has the effect of effectively preventing transmission and reflection in the visible spectrum, while effectively exhibiting the anti-reflection performance described herein at infrared wavelengths.
[0119] As is apparent from Fig. 22, the quantities, thicknesses, numbers of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 3 are configured so that the transmittance of the window 24 for light perpendicularly incident on the first surface 32 or the second surface 34 exceeds 99.0% over the entire wavelength range of 1500 nm to 1600 nm. Also, as is apparent from Fig. 23, the quantities, thicknesses, numbers of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 3 are configured so that the average P-polarized light transmittance and the average S-polarized light transmittance of the window 24 obtained in the target wavelength range of 1500 nm to 1600 nm exceeds 88% for light incident on the first surface 32 or the second surface at an angle of 60° or less with respect to the normal to the first surface and the second surface.
[0120] Furthermore, as is clear from FIG. 24, the quantity, thickness, number of layers, and material of the first multilayer film 36 and the second multilayer film 38 of the window 24 in Example 3 are configured so that the reflectance at the end face 44 of the first multilayer film 36 (and each layer in the window 24) of the window 24 and the reflectance at the end face 48 of the second multilayer film 38 for light perpendicularly incident on the substrate 30 are less than 1.0% in the wavelength range of approximately 1500 nm to 1600 nm. The reason why the reflectance at the end face 44 is approximately the same as the reflectance at the end face 48 is because the first multilayer film 36 and the second multilayer film 38 are made of materials having relatively low absorbance in the above-mentioned wavelength range. As shown in the figure, the reflectance obtained by modeling reached a minimum value of approximately 0.1% at approximately 1540 nm, and was less than 0.2% throughout the wavelength range of 1530 nm to 1600 nm.
[0121] As is apparent from Figure 25, the quantities, thicknesses, number of layers, and materials of the first multilayer 36 and second multilayer 38 of the window 24 of Example 3 are configured such that the transmittance of the window 24 is substantially below 0.5% across the entire visible spectrum. Also, the transmittance in the visible spectrum from 400 nm to 600 nm is below 0.1%. It is believed that the absorption of visible light by the silicon layer of the second multilayer 38 contributes in part to these low transmittance values.
[0122] As is apparent from FIG. 26A and FIG. 26B, the quantity, thickness, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 3 are configured to give the window 24 a dark appearance when viewed from the end face 44 of the first multilayer film. FIG. 26A shows CIELAB single-sided reflection color data for light reflected from the end face 44 of Example 3 obtained by simulation. The color of the single-sided reflected light can be characterized using CIELAB color coordinates. The a* axis in the color space represents the green to red color component, with negative a* values corresponding to green and positive a* values corresponding to red. The b* axis in the color space represents the blue to yellow color component, with negative b* values corresponding to blue and positive b* values corresponding to yellow. The closer the a* and b* values are to the origin, the lower the saturation of the color perceived by the person viewing the reflected light. The CIELA a* and b* values were generated by performing simulations at a number of different light source incidence angles ranging from 0° to 90°. As shown in curve 2602, the a* value ranges from about -2.25 to about 0.4, and the b* value ranges from about -2.0 to about 0.5, indicating that window 24 according to Example 3 has a desaturated appearance when viewed from outside 26 (see FIG. 1).
[0123] 26B is a graph showing the CIELAB lightness L* values obtained by modeling as a function of the angle of incidence on the end face 44. As shown, the lightness L* value for angles of incidence of 60° or less is 30 or less. This indicates that the window 24 according to Example 3 has a dark appearance when viewed from the outside world 26 (see FIG. 1).
[0124] Example 4 - The window 24 of Example 4 had a first multilayer 36 on a first side 32 of a substrate 30 of aluminosilicate glass (Corning Code 2320). The window 24 of Example 4 also had a second multilayer 38 on a second side 34 of the substrate 30. The first multilayer 36 was a multilayer of SiO2 (SiO2(2) material in Table A) as the low refractive index material 42 and SiN as the high refractive index material 40. x (Table A SiN xThe 20th layer was made of a 2000 nm thick high refractive index material 40 (SiN in Table A). x (2) Material) was used as the scratch-resistant layer. The first to nineteenth layers were used as light control layers that spaced the scratch-resistant layer from the end face 44. The total thickness of the first to nineteenth layers was 1361.8 nm. The twenty-first to twenty-ninth layers were used as refractive index matching layers that spaced the scratch-resistant layer from the first surface 32. The total thickness of the twenty-first to twenty-ninth layers was 326.0 nm. In this example, the scratch-resistant layer accounted for 54.23% of the thickness of the first multilayer film 36.
[0125] The second multilayer film 38 is configured by alternately stacking 15 layers of low refractive index material 42 and high refractive index material 40. In this embodiment, the low refractive index material 42 is SiO2 (SiO2(2) material in Table A), and the high refractive index material 40 is SiN x (Table A SiN x As shown in the table, the 32nd layer (the layer of the high refractive index material 40 closest to the substrate 30 (the 30th layer in this embodiment)) was made of SiN x and the other layers of high refractive index material 40 were Si. Layer 34 (the Si layer closest to substrate 30) was the thinnest Si layer with a thickness of 8.23 nm. The total thickness of the silicon layers was 585 nm, accounting for 45.41% of the total thickness of second multilayer film 38. The silicon material used in Example 4 was the same as that described in the description of Example 2 above (the silicon material having the properties shown in FIG. 14).
[0126] The thickness of each layer in the first multilayer film 36 and the second multilayer film 38 was set as shown in Table 4 below, and this was used to calculate the transmittance, reflectance, CIELAB color space values and lightness values, and nanoindentation hardness shown in Figures 27 to 32B.
[0127] [Table 4]
[0128] 27 shows a graph including a first curve 2702, a second curve 2704, and a third curve 2706 for the window 24 according to Example 4. The first curve 2702 shows the transmittance of the window 24 over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the window 24, as obtained by modeling. The second curve 2704 shows the reflectance over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the first multilayer film 36, as obtained by modeling. The third curve 2706 shows the reflectance over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the second multilayer film 38, as obtained by modeling. As shown, the quantity, thickness, number of layers, and materials of the first and second multilayer films 36, 38 of the window 24 of Example 4 are configured such that the transmittance of the window 24 for light perpendicularly incident on the window 24 at wavelengths greater than 1400 nm is greater than 90%, whereas the transmittance is less than 1% throughout the visible spectrum. Additionally, as shown by curves 2704 and 2706, the reflectance of the window 24 of Example 4 for wavelengths greater than 1500 nm is less than 1% when viewed from both the first and second multilayer films 36, 38. Additionally, the reflectance of the window of Example 4 when viewed from the first multilayer film 36 is less than 22% throughout the visible spectrum (and the reflectance is less than 10% for wavelengths greater than about 420 nm). Thus, the results shown in FIG. 27 demonstrate that the window 24 of Example 4 effectively prevents transmission and reflection in the visible spectrum while effectively exhibiting the anti-reflection performance described herein at infrared wavelengths.
[0129] As is clear from Fig. 28, the quantities, thicknesses, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 4 are configured so that the transmittance of the window 24 for light perpendicularly incident on the first surface 32 or the second surface 34 exceeds 99.4% over the entire wavelength range of 1500 nm to 1600 nm. Also, as is clear from Fig. 29, the quantities, thicknesses, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 4 are configured so that the average P-polarized light transmittance and the average S-polarized light transmittance of the window 24 obtained in the target wavelength range of 1500 nm to 1600 nm exceeds 92.2% for light incident on the first surface and the second surface at an angle of 60° or less with respect to the normal to the first surface and the second surface. The S-polarized light transmittance and the P-polarized light transmittance exceed 93.5% over the entire wavelength range of 1530 nm to 1600 nm. Example 4 appears to have the highest anti-reflection performance at high angles of incidence of all the examples, regardless of polarization.
[0130] Furthermore, as is clear from Fig. 30, the quantity, thickness, number of layers, and material of the first multilayer film 36 and the second multilayer film 38 of the window 24 in Example 4 are configured so that the reflectance at the end face 44 of the first multilayer film 36 (and each layer in the window 24) of the window 24 and the reflectance at the end face 48 of the second multilayer film 38 for light perpendicularly incident on the substrate 30 are less than 0.6% in the wavelength range of approximately 1500 nm to 1600 nm. The reason why the reflectance at the end face 44 is approximately the same as the reflectance at the end face 48 is because the first multilayer film 36 and the second multilayer film 38 are made of materials having relatively low absorbance in the above-mentioned wavelength range. As shown in the figure, the reflectance obtained by modeling reached a minimum value of approximately 0.08% at approximately 1550 nm, and was less than 0.1% throughout the wavelength range of 1535 nm to 1565 nm.
[0131] As is apparent from Figure 31, the quantities, thicknesses, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 in Example 4 are configured so that the transmittance of the window 24 for light perpendicularly incident on the substrate 30 is substantially below 0.3% across the entire visible spectrum. Also, the transmittance in the visible spectrum from 400 nm to 650 nm is below 0.1%. It is believed that the absorption of visible light by the silicon layer of the second multilayer film 38 contributes to these low transmittance values.
[0132] As is apparent from FIG. 32A and FIG. 32B, the quantity, thickness, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 4 are configured to give the window 24 a dark appearance when viewed from the end face 44 of the first multilayer film. FIG. 32A shows CIELAB single-sided reflection color data for light reflected from the end face 44 of Example 4 obtained by simulation. The color of the single-sided reflected light can be characterized using CIELAB color coordinates. The a* axis in the color space represents the green to red color component, with negative a* values corresponding to green and positive a* values corresponding to red. The b* axis in the color space represents the blue to yellow color component, with negative b* values corresponding to blue and positive b* values corresponding to yellow. The closer the a* and b* values are to the origin, the lower the saturation of the color perceived by the person viewing the reflected light. The CIELA a* and b* values were generated by performing simulations at a number of different light source incidence angles ranging from 0° to 90°. As shown in curve 3202, the a* value ranges from about -3.15 to about 1.5, and the b* value ranges from about -4.0 to 5.6, indicating that window 24 according to Example 4 has a low-saturation appearance when viewed from outside 26 (see FIG. 1).
[0133] 32B is a graph showing the CIELAB lightness L* values obtained by modeling as a function of the angle of incidence on the end face 44. As shown, the lightness L* value for angles of incidence of 60° or less is 42 or less. This indicates that the window 24 according to Example 4 has a dark appearance when viewed from the outside world 26 (see FIG. 1).
[0134] Example 5 - The window 24 of Example 5 had a first multilayer 36 on a first side 32 of a substrate 30 of aluminosilicate glass (Corning Code 2320). The window 24 of Example 5 also had a second multilayer 38 on a second side 34 of the substrate 30. The first multilayer 36 was a multilayer of SiO2 (SiO2(2) material in Table A) as the low refractive index material 42 and SiN as the high refractive index material 40. x (Table A SiN x (1) Material) was alternately stacked in 27 layers. The 18th layer was made of high refractive index material 40 (SiN in Table A) with a thickness of 2000 nm. x (2) Material) was used as the scratch-resistant layer. The first to seventeenth layers were used as light control layers that spaced the scratch-resistant layer from the end face 44. The total thickness of the first to seventeenth layers was 1300 nm. The nineteenth to twenty-seventh layers were used as refractive index matching layers that spaced the scratch-resistant layer from the first surface 32. The total thickness of the nineteenth to twenty-seventh layers was 376.2 nm. In this example, the scratch-resistant layer accounted for 54.40% of the thickness of the first multilayer film 36.
[0135] The second multilayer film 38 is configured by alternately stacking 15 layers of low refractive index material 42 and high refractive index material 40. In this embodiment, the low refractive index material 42 is SiO2 (SiO2(2) material in Table A), and the high refractive index material 40 is SiN x (Table A SiN x As shown in the table, the 30th layer (the layer of the high refractive index material 40 closest to the substrate 30 (the 28th layer in this embodiment)) was made of SiN x and the other layers of high refractive index material 40 were Si. Layer 32 (the Si layer closest to substrate 30) was the thinnest Si layer with a thickness of 8.03 nm. The total thickness of the silicon layers was 518.35 nm, accounting for 36.67% of the total thickness of second multilayer film 38. The silicon material used in Example 5 was the same as that described in the description of Example 2 above (the silicon material having the properties shown in FIG. 14).
[0136] The thickness of each layer in the first multilayer film 36 and the second multilayer film 38 was set as shown in Table 5 below, and this was used to calculate the transmittance, reflectance, CIELAB color space values and lightness values, and nanoindentation hardness shown in Figures 33 to 38B.
[0137] [Table 5]
[0138] 33 shows a graph including a first curve 3302, a second curve 3304, and a third curve 3306 for the window 24 according to Example 5. The first curve 3302 shows the transmittance of the window 24 over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the window 24, as obtained by modeling. The second curve 3304 shows the reflectance over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the first multilayer film 36, as obtained by modeling. The third curve 3306 shows the reflectance over the entire spectral range of 400 nm to 1600 nm for light perpendicularly incident on the second multilayer film 38, as obtained by modeling. As shown, the quantity, thickness, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 5 are configured such that the transmittance of the window 24 for light perpendicularly incident on the window 24 at wavelengths greater than 1400 nm is greater than 90%. However, the transmittance is less than 5% throughout the visible spectrum (and less than 1% for wavelengths between 400 nm and 630 nm). As shown by curves 3304 and 3306, the reflectance of the window 24 of Example 5 for wavelengths greater than 1500 nm is less than 1% when viewed from the first multilayer film 36 and when viewed from the second multilayer film 38. The reflectance of the window of Example 5 when viewed from the first multilayer film 36 is less than 22% throughout the visible spectrum. Thus, the results shown in FIG. 33 demonstrate that the window 24 of Example 5 effectively prevents transmission and reflection in the visible spectrum while effectively exhibiting the anti-reflection performance described herein at infrared wavelengths.
[0139] As is clear from Fig. 34, the quantities, thicknesses, numbers of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 5 are configured so that the transmittance of the window 24 for light perpendicularly incident on the first surface 32 or the second surface 34 exceeds 99.1% over the entire wavelength range of 1500 nm to 1600 nm. Also, as is clear from Fig. 35, the quantities, thicknesses, numbers of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 5 are configured so that the average P-polarized light transmittance and the average S-polarized light transmittance of the window 24 obtained in the target wavelength range of 1500 nm to 1600 nm exceeds 91.8% for light incident on the first surface and the second surface at an angle of 60° or less with respect to the normal to the first surface and the second surface.
[0140] Furthermore, as is clear from FIG. 36, the quantity, thickness, number of layers, and material of the first multilayer film 36 and the second multilayer film 38 of the window 24 in Example 5 are configured so that the reflectance at the end face 44 of the first multilayer film 36 (and each layer in the window 24) of the window 24 and the reflectance at the end face 48 of the second multilayer film 38 for light perpendicularly incident on the substrate 30 are less than 1.0% in the wavelength range of approximately 1500 nm to 1600 nm. The reason why the reflectance at the end face 44 is similar to the reflectance at the end face 48 is because the first multilayer film 36 and the second multilayer film 38 are made of materials having relatively low absorbance in the above-mentioned wavelength range. As shown in the figure, the reflectance obtained by modeling reached a minimum value of less than 0.05% at about 1545 nm, and was less than 0.1% throughout the wavelength range of 1530 nm to 1565 nm.
[0141] As is apparent from Figure 37, the quantities, thicknesses, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 in Example 5 are configured so that the transmittance of the window 24 for light perpendicularly incident on the substrate 30 is substantially below 3% across the entire visible spectrum. Also, the transmittance in the visible spectrum from 400 nm to 650 nm is below 0.3%. It is believed that the absorption of visible light by the silicon layer of the second multilayer film 38 contributes to these low transmittance values.
[0142] As is apparent from FIG. 38A and FIG. 38B, the quantity, thickness, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 5 are configured to give the window 24 a dark appearance when viewed from the end face 44 of the first multilayer film. FIG. 38A shows CIELAB single-sided reflection color data for light reflected from the end face 44 of Example 5 obtained by simulation. The color of the single-sided reflected light can be characterized using CIELAB color coordinates. The a* axis in the color space represents the green to red color component, with negative a* values corresponding to green and positive a* values corresponding to red. The b* axis in the color space represents the blue to yellow color component, with negative b* values corresponding to blue and positive b* values corresponding to yellow. The closer the a* and b* values are to the origin, the lower the color saturation perceived by a person viewing the reflected light. The CIELA a* and b* values were generated by performing simulations at a number of different light source incidence angles ranging from 0° to 90°. As shown in curve 3802, the a* value ranges from about -3.1 to about 0.5, and the b* value ranges from about -4.5 to 2.6, indicating that window 24 according to Example 5 has a low-saturation appearance when viewed from outside 26 (see FIG. 1).
[0143] 32B is a graph showing the CIELAB lightness L* values obtained by modeling as a function of the angle of incidence on the end face 44. As shown, the lightness L* value for angles of incidence of 60° or less is 45 or less. This indicates that the window 24 according to Example 5 has a dark appearance when viewed from the outside world 26 (see FIG. 1).
[0144] Example 6 - The window 24 of Example 6 had a first multilayer 36 on a first side 32 of a substrate 30 of aluminosilicate glass (Corning Code 2320). The window 24 of Example 6 also had a second multilayer 38 on a second side 34 of the substrate 30. The first multilayer 36 was a multilayer of SiO2 as the low index material 42 and SiN as the high index material 40. xThe structure was such that 27 layers were alternately stacked. The 18th layer was a scratch-resistant layer made of a high refractive index material 40 having a thickness of 2000 nm. The 1st to 17th layers were light control layers that spaced the scratch-resistant layer from the end face 44. The total thickness of the 1st to 17th layers was 1818.92 nm. The 19th to 27th layers were refractive index matching layers that spaced the scratch-resistant layer from the first surface 32. The total thickness of the 19th to 27th layers was 328.77 nm. In this example, the scratch-resistant layer accounted for 48.21% of the thickness of the first multilayer film 36.
[0145] The second multilayer film 38 is configured by alternately stacking 19 layers of low refractive index material 42 and high refractive index material 40. In this embodiment, the low refractive index material 42 is SiO2, and the high refractive index material 40 is SiN x As shown in the table, the 30th layer, the 32nd layer, and the 34th layer (the three layers of the high refractive index material 40 closest to the substrate 30 (in this embodiment, the 28th layer)) were made of SiN. x and the other layers of high refractive index material 40 were Si. Layer 36 (the Si layer closest to substrate 30) was the thinnest Si layer with a thickness of 12.02 nm. The total thickness of the silicon layers was 708.03 nm, accounting for 27.52% of the total thickness of second multilayer 38.
[0146] The values of the refractive index and extinction coefficient of the Si material used in Example 6 are shown in FIG. 39. As shown in the figure, the extinction coefficient of the Si material used in this example at 700 nm is about 0.37. This corresponds to the internal transmittance (transmittance of silicon only) of the total thickness of the silicon layer in Example 6 being low. Also, the extinction coefficient at 400 nm is about 3.2. Therefore, it is expected that the total transmittance of multiple silicon layers is particularly low at 400 nm compared to the transmittance at 700 nm.
[0147] The thicknesses of each layer in the first multilayer film 36 and the second multilayer film 38 were set as shown in Table 6 below, and were used to calculate the transmittance, reflectance, and CIELAB color space values shown in Figures 40, 41, and 42.
[0148] [Table 6]
[0149] FIG. 40 shows a graph including a first curve 4000, a second curve 4002, and a third curve 4004 for the window 24 according to Example 6. The first curve 4000 shows the transmittance (average transmittance of both polarizations) of the window 24 over the entire spectral range of 400 nm to 1600 nm for light incident on the window 24 at an angle of incidence of 15°, obtained by modeling. The second curve 4002 shows the transmittance (S-polarized transmittance) over the entire spectral range of 400 nm to 1600 nm for light incident on the window 24 at an angle of incidence of 60°, obtained by modeling. The third curve 4004 shows the transmittance (P-polarized transmittance) over the entire spectral range of 400 nm to 1600 nm for light incident on the window 24 at an angle of incidence of 60°, obtained by modeling. As shown, the quantities, thicknesses, layers, and materials of the first and second multilayer films 36 and 38 of the window 24 of Example 6 are configured such that the average transmittance of the window 24 exceeds 99.5% for light in the wavelength range of 1500 nm to 1575 nm that is incident on the window 24 at an angle of incidence of 15°. Meanwhile, the transmittance is below 5% throughout the visible spectrum (and the transmittance is below 1% for wavelengths of 400 nm to 750 nm). Also, as is clear from curves 4002 and 4004, the quantities, thicknesses, layers, and materials of the first and second multilayer films 36 and 38 of the window 24 of Example 6 are configured such that the average P-polarized transmittance and average S-polarized transmittance of the window 24 in the target wavelength range of 1500 nm to 1575 nm exceeds 90% for light that is incident on the first and second surfaces at an angle of 60° or less relative to the normal to the first and second surfaces.
[0150] 41, the quantities, thicknesses, numbers of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 in Example 6 are configured so that the reflectance at the end face 44 of the first multilayer film 36 of the window 24 (and each layer in the window 24) for light incident on the substrate 30 at an incident angle of 15° is less than 0.5% in the wavelength range of approximately 1500 nm to 1575 nm. Also, as is clear from the curve 4102 in FIG. 41, the quantities, thicknesses, numbers of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 in Example 6 are configured so that the reflectance at the end face 48 of the second multilayer film 38 of the window 24 (and each layer in the window 24) for light incident on the substrate 30 at an incident angle of 15° is less than 0.5% in the wavelength range of approximately 1500 nm to 1575 nm. The reflectance at facet 44 is comparable to the reflectance at facet 48 because first and second multilayers 36, 38 are constructed from materials that have relatively low absorbance in the wavelength ranges discussed above. As further shown in curve 4100 of FIG. 41, the quantity, thickness, number of layers, and materials of first and second multilayers 36, 38 of window 24 of Example 6 are configured to provide an average transmittance of window 24 of less than 3% across the visible spectrum for light incident on first multilayer 36 at an angle of incidence of 15°. These low reflectance values are believed to be due to the absorption of visible light by the silicon layer of second multilayer 38.
[0151] As can be seen from FIG. 42, the quantity, thickness, number of layers, and materials of the first and second multilayers 36, 38 of the window 24 of Example 6 are configured to provide a desaturated appearance of the window 24 when viewed from the edge 44 of the first multilayer. FIG. 42 shows CIELAB single-sided reflected color data for light reflected from the edge 44 of Example 6, obtained by simulation under D65 illuminant and 1964 standard observer conditions (the conditions under which all CIELAB color measurements described herein are expressed). The color of the single-sided reflected light can be characterized using CIELAB color coordinates. The a* axis in the color space represents the green to red color component, with negative a* values corresponding to green and positive a* values corresponding to red. The b* axis in the color space represents the blue to yellow color component, with negative b* values corresponding to blue and positive b* values corresponding to yellow. The closer the a* and b* values are to the origin, the less saturated the color will be perceived by a viewer of the reflected light. The CIELA Ba* and b* values were generated by simulating a number of different angles of incidence for a D65 illuminant, ranging from 0° to 90°. As shown by the curves in Figure 42, the b* values range from about -0.7 to about 1.25, and the a* values range from about -1.1 to 3.1. Example 6 also exhibited an L* value of 30.5 or less over the entire target angle range of 0° to 55°.
[0152] In Examples 1 to 6, the number of layers of the alternating layers in which the low refractive index material 42 and the high refractive index material 40 are alternately stacked in the first multilayer film 36 was changed in the range of 21 to 29 layers, and the layer thickness was changed in the range of 3305.7 nm to 4147.69 nm. In these Examples, the number of layers of the alternating layers in which the low refractive index material 42 and the high refractive index material 40 are alternately stacked in the second multilayer film 38 was changed in the range of 13 to 19 layers, and the layer thickness was changed in the range of 1049.9 nm to 2572.77 nm. Therefore, in the above Examples, the thickness of the first multilayer film 36 was 1.5 times or more that of the second multilayer film 38. This is considered to be because the refractive index of the silicon layer of the second multilayer film 38 is relatively high. In the second multilayer film 38 of each Example, the total thickness of the silicon layer was in the range of 414.6 nm to 708 nm. Also, Example 4, which has the highest number of layers in the first multilayer film 36, appeared to provide superior anti-reflection performance at high angles of incidence regardless of polarization. It should be noted that the above examples are designed for a specific wavelength range near 1550 nm, and alternative windows with different numbers, quantities, and materials of layers are contemplated. It should be understood that such alternative windows are within the scope of the present disclosure, although they may not fall within the scope described in this section. The above examples are not intended to be limiting.
[0153] Example 7 - The window 24 of Example 7 had a first multilayer 36 on a first side 32 of a substrate 30 of aluminosilicate glass (Corning Code 2320). The window 24 of Example 7 also had a second multilayer 38 on a second side 34 of the substrate 30. The first multilayer 36 was a multilayer of SiO2 as the low index material 42 and SiN as the high index material 40. x The structure was such that 27 layers were alternately stacked. The 18th layer was a scratch-resistant layer made of a high refractive index material 40 having a thickness of 2000 nm. The 1st to 17th layers were light control layers that spaced the scratch-resistant layer from the end face 44. The total thickness of the 1st to 17th layers was 1825.13 nm. The 19th to 27th layers were refractive index matching layers that spaced the scratch-resistant layer from the first surface 32. The total thickness of the 19th to 27th layers was 314.7 nm. In this example, the scratch-resistant layer accounted for 48.31% of the thickness of the first multilayer film 36.
[0154] The second multilayer film 38 of Example 7 was configured by alternately stacking 25 layers of low refractive index material 42 and high refractive index material 40. In this example, the low refractive index material 42 was SiO2, and the high refractive index material 40 was SiN x As shown in the table, the 30th layer, the 32nd layer, and the 34th layer (the three layers of the high refractive index material 40 closest to the substrate 30 (in this embodiment, the 28th layer)) were made of SiN. x and the other layers of high refractive index material 40 were Si. Layer 36 (the Si layer closest to substrate 30) was the thinnest Si layer with a thickness of 12.03 nm. The total thickness of the silicon layers was 1199.18 nm, accounting for 43.89% of the total thickness of second multilayer 38.
[0155] The first multilayer film 36 of Example 7 has a scratch-resistant layer made of SiN x The difference between the first multilayer film 36 of Example 6 and the second multilayer film 36 of Example 7 is that the first multilayer film 36 of Example 7 is made of a material having a refractive index of 2.04658, whereas the refractive index of the second multilayer film 36 of Example 6 is 1.96. x Since the material is harder, it is considered that the scratch resistance is improved compared to Example 6. Also, the second multilayer film 38 of Example 7 is different from the second multilayer film 38 of Example 6 in that silicon, which has a lower extinction coefficient, is used for the second multilayer film 38. Unlike the material shown in FIG. 39, the extinction coefficient of the Si material of this example at 1550 nm is less than 0.05 (for example, less than 0.01, less than 0.005). It is considered that the use of such a material with a low extinction coefficient widens the high transmittance bandwidth near 1550 nm, making it less susceptible to the effects of wavelength shift.
[0156] In Example 7, the thicknesses of each layer in the first multilayer film 36 and the second multilayer film 38 were set as shown in Table 7 below, and were used to calculate the transmittance, reflectance, and CIELAB color space values shown in Figures 43 to 49.
[0157] [Table 7]
[0158] 43 is a graph showing the modeled transmittance of window 24 of Example 7 across the spectral range of 400 nm to 1600 nm for light incident on window 24. The graph shows the predicted performance for light incident on window 24 at a 15° angle of incidence (average performance for both polarizations) and for light incident on window 24 at a 60° angle of incidence (performance for S-polarized and P-polarized light). As shown, the quantities, thicknesses, number of layers, and materials of first multilayer film 36 and second multilayer film 38 of window 24 of Example 7 are configured such that the average transmittance of window 24 for light in the wavelength range of 1500 nm to 1575 nm incident on window 24 at a 15° angle of incidence is greater than 99.5%. In addition, the quantity, thickness, number of layers, and material of the first multilayer film 36 and the second multilayer film 38 of the window 24 in Example 7 are configured so that the average P-polarized light transmittance and average S-polarized light transmittance of the window 24 obtained in the target wavelength range of 1500 nm to 1575 nm exceeds 91% for light incident on the first and second surfaces at an angle of 60° or less relative to the normal to the first and second surfaces.
[0159] FIG. 44 is a plot showing the reflectance at the end face 44 and end face 48 of the window 24 according to Example 7 (e.g., the reflectance at the inner and outer surfaces of the window 24) obtained by modeling. As is clear from FIG. 44, the quantity, thickness, number of layers, and material of the first multilayer film 36 and the second multilayer film 38 of the window 24 in Example 7 are configured such that the reflectance at the end face 44 of the first multilayer film 36 of the window 24 and the reflectance at the end face 48 of the second multilayer film 38 for light incident on the substrate 30 at an incident angle of 15° (these curves overlap in FIG. 44) are less than 0.5% in the wavelength range of approximately 1500 nm to 1575 nm. The reason why the reflectance at the end face 44 is approximately the same as the reflectance at the end face 48 is because the first multilayer film 36 and the second multilayer film 38 are made of a material having a relatively low absorbance in the above-mentioned wavelength range.
[0160] Fig. 45 is a graph showing the transmittance of the window 24 according to Example 7 in the wavelength range of 350 nm to 1600 nm obtained by modeling. As shown in Fig. 45, the quantity, thickness, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 7 are configured such that the average transmittance of the window 24 for light incident on the first multilayer film 36 at an angle of incidence of 15° (average of both polarizations) is less than 5% across the visible spectrum. Fig. 46 is a graph showing the reflectance of the window 24 according to Example 7 in the wavelength range of 350 nm to 1600 nm obtained by modeling. As shown in FIG. 46, the quantities, thicknesses, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 7 are configured so that the average reflectance (average of both polarizations) of the window 24 for light incident on the first multilayer film 36 at an angle of incidence of 15° (light from outside the window 24) is less than 5% across the entire visible spectrum. FIG. 47 is a graph of the two-sided transmittance of the window 24 according to Example 7 obtained by modeling. As shown, the quantities, thicknesses, number of layers, and materials of the first multilayer film 36 and the second multilayer film 38 of the window 24 of Example 7 are configured so that the average transmittance of the window 24 for light incident on the window 24 at an angle of incidence of 15° is less than 0.1% in the wavelength range of 400 nm to 650 nm. In fact, in the wavelength range of 400 nm to 700 nm, the transmittance exhibited by window 24 is below 1% throughout the entire range (and further, in the wavelength range of 400 nm to 650 nm, the transmittance is below 0.1% throughout the entire range).
[0161] As is evident from FIG. 48, the quantity, thickness, number of layers, and materials of the first multilayer 36 and the second multilayer 38 of the window 24 of Example 7 are configured to provide a desaturated appearance of the window 24 when viewed from the end face 44 of the first multilayer. FIG. 48 shows CIELAB single-sided reflected color data for light reflected from the end face 44 of Example 7, obtained by simulation under D65 illuminant and 1964 standard observer conditions (all CIELAB color measurements described herein are expressed under these conditions). Characterization of the color of the single-sided reflected light can be performed using CIELAB color coordinates. As shown, the b* values range from about -1.0 to about 0.6, and the a* values range from about -1.5 to 3.6. FIG. 49 shows the L* values for light reflected from the end face 44 of Example 7, obtained by simulation under D65 illuminant and 1964 standard observer conditions. The L* value shown in Example 7 was 35 or less over the entire incidence angle range of 0° to 60° (25 or less over the entire incidence angle range of 0° to 50°).
[0162] Aspect (1) of the present disclosure relates to a window for a detection system. The window includes a substrate, a first multilayer film, and a second multilayer film. The substrate has a first surface and a second surface, and the first surface and the second surface are the main surfaces of the substrate. The first multilayer film is disposed on the first surface of the substrate. The first multilayer film includes alternating layers of one or more high refractive index materials and one or more low refractive index materials, and the refractive index of the one or more high refractive index materials of the first multilayer film is higher than the refractive index of the one or more low refractive index materials of the first multilayer film. The second multilayer film is disposed on the second surface of the substrate. The second multilayer film includes alternating layers of one or more high refractive index materials and one or more low refractive index materials, and the refractive index of the one or more high refractive index materials of the second multilayer film is higher than the refractive index of the one or more low refractive index materials of the second multilayer film. In addition, the maximum hardness of the window measured by performing a Berkovich indentation hardness test on the first multilayer film is at least 8 GPa. The quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured so that the average transmittance of the window measured in a target wavelength range of 50 nm width within a range of 1400 nm to 1600 nm exceeds 90% for light incident on the first and second surfaces at an angle of incidence of 15° or less, the average reflectance of the window measured in a target wavelength range of 50 nm width within a range of 1400 nm to 1600 nm is less than 1% for light incident on the first and second surfaces at an angle of incidence of 15° or less, and the average transmittance of the window measured in a range of 400 nm to 700 nm is less than 5% for light incident on the first and second surfaces at an angle of incidence of 15° or less.
[0163] Aspect (2) of the present disclosure relates to a window as recited in aspect (1), in which the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that, for light incident on the first and second surfaces at an angle of incidence of 60° or less, the average P-polarized light transmittance and average S-polarized light transmittance of the window measured in a target wavelength range of 50 nm width within the range of 1400 nm to 1600 nm is greater than 85%.
[0164] Aspect (3) of the present disclosure relates to a window as recited in aspect (2), in which the window has an average P-polarized light transmittance and an average S-polarized light transmittance greater than 92% for light incident on the first and second surfaces at an angle of incidence of 60° or less in a 50 nm wide target wavelength range within the range of 1400 nm to 1600 nm.
[0165] An aspect (4) of the present disclosure relates to a window according to any one of aspects (1) to (3), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the CIELAB L* value of the window for an incident angle of 60° or less relative to the first multilayer film is 45 or less.
[0166] An aspect (5) of the present disclosure relates to the window of aspect (4), wherein the first multilayer film has a CIELAB L* value of 30 or less for an incident angle of 60° or less.
[0167] An aspect (6) of the present disclosure relates to a window according to any one of aspects (1) to (5), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the CIELAB a* and b* values of the window when viewed from the first multilayer film side are between −6.0 and 6.0.
[0168] An aspect (7) of the present disclosure relates to a window as defined in any one of aspects (1) to (5), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the average reflectance of the window across the entire visible spectrum for light perpendicularly incident on the first multilayer film is 10% or less.
[0169] An aspect (8) of the present disclosure relates to a window as recited in any one of aspects (1) to (7), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the average transmittance of the window, determined in a 50 nm wide target wavelength range within the range of 1400 nm to 1600 nm, exceeds 95% for light perpendicularly incident on the first and second surfaces.
[0170] An aspect (9) of the present disclosure relates to the window according to any one of aspects (1) to (5), wherein the substrate is a glass substrate.
[0171] An aspect (10) of the present disclosure relates to the window according to aspect (9), wherein the region continuous with the first surface of the substrate is a region subjected to compressive stress, and the absolute value of the maximum compressive stress is at least 600 MPa.
[0172] An embodiment (11) of the present disclosure relates to the window according to any one of embodiments (1) to (10), wherein the thickness of the substrate is from about 100 μm to about 5 mm.
[0173] An embodiment (12) of the present disclosure relates to the window according to any one of embodiments (1) to (11), wherein the substrate has a refractive index of about 1.45 to about 1.55 for electromagnetic waves having a wavelength of 1550 nm.
[0174] An aspect (13) of the present disclosure relates to a window according to any one of aspects (1) to (12), wherein the one or more high refractive index materials have a refractive index of about 1.7 to about 4.0, and the one or more low refractive index materials have a refractive index of about 1.3 to about 1.6.
[0175] An aspect (14) of the present disclosure relates to a window according to any one of aspects (1) to (13), wherein the difference in refractive index between any one or more high refractive index materials and any one or more low refractive index materials is about 0.5 or more.
[0176] An aspect (15) of the present disclosure relates to a window according to any one of aspects (1) to (14), wherein one of the alternating layers in the first multilayer film that is furthest from the substrate constitutes the material of the window end, and the material of the window end includes a low refractive index material.
[0177] An aspect (16) of the present disclosure relates to the window of aspect (15), wherein the first multilayer film includes a scratch-resistant layer, the scratch-resistant layer being formed from one of one or more high refractive index materials and having a thickness of 500 nm or greater.
[0178] An aspect (17) of the present disclosure relates to the window according to aspect (16), wherein the scratch-resistant layer has a thickness of 1500 nm or more and 5000 nm or less.
[0179] An embodiment (18) of the present disclosure relates to the window of embodiment (17), wherein the scratch resistant layer is spaced from the edge by multiple of the alternating layers of one or more low refractive index materials and one or more high refractive index materials in the first multilayer.
[0180] An embodiment (19) of the present disclosure relates to the window according to embodiment (18), wherein the scratch resistant layer is spaced at least 1000 nm from the edge.
[0181] An embodiment (20) of the present disclosure relates to the window of any of embodiments (1) to (19), wherein the one or more high refractive index materials in the second multilayer film comprises silicon.
[0182] An embodiment (21) of the present disclosure relates to the window of embodiment (20), wherein the second multilayer film comprises two or more silicon layers.
[0183] An embodiment (22) of the present disclosure relates to the window of embodiment (21), wherein the silicon layer of the second multilayer closest to the substrate has the smallest thickness of the two or more silicon layers.
[0184] An embodiment (23) of the present disclosure relates to the window according to embodiment (21), wherein the total thickness of the silicon layers included in the second multilayer film is 250 nm or more.
[0185] An embodiment (24) of the present disclosure relates to the window of embodiment (22), wherein the window has a total thickness of 500 nm or more.
[0186] An embodiment (25) of the present disclosure relates to the window of any of embodiments (21) to (24), wherein one or more of the layers of high refractive index material in the second multilayer film is not silicon.
[0187] An aspect (26) of the present disclosure relates to the window of any one of aspects (1) to (25), wherein the first multilayer film has a maximum hardness of at least 10 GPa as measured by subjecting the first multilayer film to a Berkovich indentation hardness test.
[0188] An aspect (27) of the present disclosure relates to the window of any one of aspects (1) to (26), wherein the first multilayer film has a hardness, measured by Berkovich indentation hardness testing, of at least 8 GPa over a depth range of 300 nm to 2000 nm.
[0189] An aspect (28) of the present disclosure relates to the window of any one of aspects (1) to (27), wherein the first multilayer film has a hardness of at least 9 GPa over a depth range of 750 nm to 2000 nm, as measured by Berkovich hardness testing.
[0190] Aspect (29) of the present disclosure relates to a window for a detection system. The window includes a substrate, a first multilayer film, and a second multilayer film. The substrate has a first surface and a second surface, and the first surface and the second surface are the main surfaces of the substrate. The first multilayer film is disposed on the first surface of the substrate. The first multilayer film includes alternating layers of one or more high refractive index materials and one or more low refractive index materials, and the refractive index of the one or more high refractive index materials of the first multilayer film is higher than the refractive index of the one or more low refractive index materials of the first multilayer film. The second multilayer film is disposed on the second surface of the substrate. The second multilayer film includes alternating layers of one or more high refractive index materials and one or more low refractive index materials, and the refractive index of the one or more high refractive index materials of the second multilayer film is higher than the refractive index of the one or more low refractive index materials of the second multilayer film. The first multilayer film has a maximum hardness of at least 8 GPa as measured by performing a Berkovich indentation hardness test. The quantity, thickness, number of layers, and materials of the alternating layers in the first and second multilayer films are configured so that, for light incident on the first and second surfaces at an angle of 15° or less, the average reflectance of the window determined in a 50 nm wide target wavelength range within the range of 1400 nm to 1600 nm is below 0.5%, the CIELAB L* value of the window for an incident angle of 60° or less to the first multilayer film is 45 or less, and the CIELAB a* and b* values of the window when viewed from the first multilayer film side are -6.0 or greater and 6.0 or less.
[0191] An embodiment (30) of the present disclosure relates to the window of embodiment (29), wherein the first multilayer has a CIELAB L* value of 30 or less for an incident angle of 60° or less.
[0192] An aspect (31) of the present disclosure relates to a window as recited in any one of aspects (29) to (30), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the average transmittance of the window, determined in a target wavelength range of 50 nm within the range of 1400 nm to 1600 nm, exceeds 95% for light incident on the first and second surfaces at an angle of incidence of 15° or less.
[0193] An aspect (32) of the present disclosure relates to a window as recited in any one of aspects (29) to (31), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the average transmittance of the window measured in the range of 400 nm to 700 nm is below 5% for light incident on the first and second faces at an angle of incidence of 15° or less.
[0194] An aspect (33) of the present disclosure relates to a window as recited in any one of aspects (29) to (32), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that, for light incident on the first and second surfaces at an angle of incidence of 60° or less, the average P-polarized light transmittance and average S-polarized light transmittance of the window measured in a target wavelength range of 50 nm width within the range of 1400 nm to 1600 nm is greater than 85%.
[0195] An aspect (34) of the present disclosure relates to a window as recited in aspect (33), wherein the window has an average P-polarized light transmittance and an average S-polarized light transmittance of greater than 92% for light incident on the first and second surfaces at an angle of incidence of 60° or less over a 50 nm wide wavelength range of interest within the range of 1400 nm to 1600 nm.
[0196] An aspect (35) of the present disclosure relates to a window according to any one of aspects (29) to (34), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured so that the average reflectance of the window across the entire visible spectrum for light perpendicularly incident on the first multilayer film is 10% or less.
[0197] An aspect (36) of the present disclosure relates to a window as recited in any one of aspects (29) to (35), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the average transmittance of the window, determined in a 50 nm wide target wavelength range within the range of 1400 nm to 1600 nm, exceeds 95% for light perpendicularly incident on the first and second surfaces.
[0198] An aspect (37) of the present disclosure relates to a window according to any one of aspects (29) to (36), wherein the first multilayer film has a maximum hardness of at least 10 GPa as measured by subjecting the first multilayer film to a Berkovich indentation hardness test.
[0199] An aspect (38) of the present disclosure relates to the window of any of aspects (29) to (37), wherein the first multilayer film has a hardness, measured by Berkovich indentation hardness testing, of at least 8 GPa over a depth range of 300 nm to 2000 nm.
[0200] An aspect (39) of the present disclosure relates to a window according to any one of aspects (29) to (38), wherein one of the alternating layers in the first multilayer film that is furthest from the substrate constitutes the material of the edge of the window, the material of the edge of the window comprising a low refractive index material, and the first multilayer film comprises a scratch-resistant layer formed from one or more high refractive index materials and having a thickness of 1500 nm or more and 5000 nm or less.
[0201] An embodiment (40) of the present disclosure relates to the window of embodiment (39), wherein the scratch-resistant layer is spaced from the edge by multiple ones of the alternating layers of one or more low refractive index materials and one or more high refractive index materials in the first multilayer, and the scratch-resistant layer is spaced from the edge by at least 1000 nm.
[0202] An embodiment (41) of the present disclosure relates to the window according to any one of embodiments (29) to (40), wherein the one or more high refractive index materials in the second multilayer film comprises silicon.
[0203] An embodiment (42) of the present disclosure relates to the window of embodiment (41), wherein the second multilayer film comprises two or more silicon layers.
[0204] An embodiment (43) of the present disclosure relates to the window of embodiment (42), wherein the silicon layer of the second multilayer closest to the substrate has the smallest thickness of the two or more silicon layers.
[0205] An embodiment (44) of the present disclosure relates to the window according to embodiment (43), wherein the total thickness of the silicon layers included in the second multilayer film is 250 nm or more.
[0206] An embodiment (45) of the present disclosure relates to the window of embodiment (44), wherein the window has a total thickness of 500 nm or more.
[0207] An embodiment (46) of the present disclosure relates to the window of any of embodiments (42) to (45), wherein one or more of the layers of high refractive index material in the second multilayer film is not silicon.
[0208] An aspect (47) of the present disclosure relates to a window for a detection system. The window comprises a substrate, a first multilayer film, and a second multilayer film. The substrate has a first surface and a second surface, the first surface and the second surface being the main surface of the substrate. The first multilayer film is disposed on the first surface of the substrate. The first multilayer film includes alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the first multilayer film being higher than the refractive index of the one or more low refractive index materials of the first multilayer film. The second multilayer film is disposed on the second surface of the substrate. The second multilayer film includes alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the second multilayer film being higher than the refractive index of the one or more low refractive index materials of the second multilayer film, and the one or more high refractive index materials of the second multilayer film include silicon. Additionally, the maximum hardness of the window, as measured by performing a Berkovich hardness test on the first multilayer, is at least 8 GPa. The number, thickness, number of layers, and materials of the alternating layers in the first and second multilayers are configured such that the average reflectance of the window measured in a 50 nm wide target wavelength range within a range of 1400 nm to 1600 nm for light incident on the first and second faces at an angle of 15° or less is less than 1%, and the average transmittance of the window measured in a 50 nm wide target wavelength range within a range of 1400 nm to 1600 nm for light incident on the first and second faces at an angle of 15° or less is greater than 90%.
[0209] An aspect (48) of the present disclosure relates to a window as recited in aspect (47), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the average transmittance of the window measured in the range of 400 nm to 700 nm is below 5% for light incident on the first and second faces at an angle of incidence of 15° or less.
[0210] An aspect (49) of the present disclosure relates to a window as recited in any one of aspects (47) to (48), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that, for light incident on the first and second surfaces at an angle of incidence of 60° or less, the average P-polarized light transmittance and average S-polarized light transmittance of the window are greater than 85% in a target wavelength range of 50 nm within the range of 1400 nm to 1600 nm.
[0211] An aspect (50) of the present disclosure relates to a window as recited in aspect (49), wherein the window has an average P-polarized light transmittance and an average S-polarized light transmittance of greater than 92% for light incident on the first and second surfaces at an angle of incidence of 60° or less over a 50 nm wide wavelength range of interest within the range of 1400 nm to 1600 nm.
[0212] An aspect (51) of the present disclosure relates to a window according to any one of aspects (47) to (50), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the CIELAB L* value of the window for an incident angle of 60° or less relative to the first multilayer film is 45 or less.
[0213] An embodiment (52) of the present disclosure relates to the window of embodiment (51), wherein the first multilayer has a CIELAB L* value of 30 or less for an incident angle of 60° or less.
[0214] An aspect (53) of the present disclosure relates to a window according to any one of aspects (47) to (52), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the CIELAB a* and b* values of the window when viewed from the first multilayer film side are between −6 and 6.
[0215] An aspect (54) of the present disclosure relates to a window according to any one of aspects (47) to (53), wherein the quantities, thicknesses, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the average reflectance of the window across the entire visible spectrum for light perpendicularly incident on the first multilayer film is 10% or less.
[0216] An aspect (55) of the present disclosure is a method for manufacturing a multilayer structure comprising the steps of: forming a first multilayer film with a first layer having a first refractive index and a second layer having a second refractive index; The window according to any one of aspects (47) to (54), wherein the first multilayer film includes a scratch-resistant layer, the scratch-resistant layer being formed from one of one or more high refractive index materials and having a thickness of 1500 nm or more and 5000 nm or less.
[0217] In an embodiment (56) of the present disclosure, the scratch-resistant layer is spaced from the end surface by a plurality of layers among the alternating layers in which one or more low refractive index materials and one or more high refractive index materials are alternately stacked in the first multilayer film; The window of embodiment (55), wherein the scratch resistant layer is spaced at least 1000 nm from the edge.
[0218] An embodiment (57) of the present disclosure relates to the window of any of embodiments (47) to (56), wherein the second multilayer film comprises two or more silicon layers.
[0219] An embodiment (58) of the present disclosure relates to the window of embodiment (57), wherein the silicon layer of the second multilayer closest to the substrate has the smallest thickness of the two or more silicon layers.
[0220] An embodiment (59) of the present disclosure relates to the window according to embodiment (57), wherein the total thickness of the silicon layers included in the second multilayer film is 250 nm or more.
[0221] An embodiment (60) of the present disclosure relates to the window of embodiment (59), wherein the window has a total thickness of 500 nm or more.
[0222] An embodiment (61) of the present disclosure relates to a window according to any one of embodiments (57) to (60), wherein one or more of the layers of high refractive index material in the second multilayer film is not silicon.
[0223] An embodiment (62) of the present disclosure relates to a window according to embodiment (61), wherein the layer of the one or more layers of high refractive index material in the second multilayer film that is not silicon is the layer of the one or more layers of high refractive index material closest to the substrate.
[0224] It will be apparent to those skilled in the art that various modifications and variations can be made without departing from the spirit and scope of the appended claims.
[0225] Preferred embodiments of the present invention will be described below in detail.
[0226] EMBODIMENT 1 a substrate having a first surface and a second surface, the first surface and the second surface being major surfaces of the substrate; a first multilayer disposed on the first surface of the substrate, the first multilayer including alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the first multilayer being higher than the refractive index of the one or more low refractive index materials of the first multilayer; a second multilayer disposed on the second surface of the substrate, the second multilayer including alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the second multilayer being higher than the refractive index of the one or more low refractive index materials of the second multilayer; 1. A window for a detection system comprising: the maximum hardness of the window is at least 8 GPa as measured by performing a Berkovich hardness test on the first multilayer; The number, thickness, number of layers, and material of the alternating layers in the first multilayer film and the second multilayer film are the average transmittance of the window is greater than 90% for light incident on the first surface and the second surface at an angle of incidence of 15° or less in a target wavelength range of 50 nm in a range of 1400 nm to 1600 nm; the average reflectance of the window is less than 1% in the target wavelength range of 1400 nm to 1600 nm with respect to light incident on the first surface and the second surface at an angle of 15° or less; A window configured such that the average transmittance of the window measured in a range of 400 nm to 700 nm for light incident on the first surface and the second surface at an angle of incidence of 15° or less is less than 5%.
[0227] EMBODIMENT 2 The window of embodiment 1, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured such that the average P-polarized light transmittance and average S-polarized light transmittance of the window, determined in the target wavelength range of 50 nm width within the range of 1400 nm to 1600 nm, exceeds 85% for light incident on the first surface and the second surface at an incident angle of 60° or less.
[0228] EMBODIMENT 3 The window of embodiment 2, wherein the average P-polarized light transmittance and the average S-polarized light transmittance of the window are greater than 92% in the target wavelength range of 1400 nm to 1600 nm, the average P-polarized light transmittance being determined for light incident on the first surface and the second surface at an angle of incidence of 60° or less.
[0229] EMBODIMENT 4 4. The window of any one of claims 1 to 3, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured such that the CIELAB L* value of the window is 45 or less for an angle of incidence of 60° or less with respect to the first multilayer film.
[0230] EMBODIMENT 5 5. The window of embodiment 4, wherein the CIELAB L* value for an incidence angle of 60° or less on the first multilayer is 30 or less.
[0231] EMBODIMENT 6 A window as described in any one of embodiments 1 to 5, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured such that the CIELAB a* and b* values of the window when viewed from the first multilayer film side are greater than or equal to -6.0 and less than or equal to 6.0.
[0232] EMBODIMENT 7 6. The window of any one of embodiments 1 to 5, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured such that the average reflectance of the window across the entire visible spectrum for light perpendicularly incident on the first multilayer film is 10% or less.
[0233] EMBODIMENT 8 The window of any one of embodiments 1 to 7, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured such that the average transmittance of the window, determined in the target wavelength range of 50 nm width within the range of 1400 nm to 1600 nm, exceeds 95% for light perpendicularly incident on the first surface and the second surface.
[0234] EMBODIMENT 9 9. The window of any one of embodiments 1 to 8, wherein the substrate is a glass substrate.
[0235] EMBODIMENT 10 10. The window of embodiment 9, wherein an area of the substrate contiguous with the first surface is subjected to compressive stress, the maximum absolute value of the compressive stress being at least 600 MPa.
[0236] EMBODIMENT 11 11. The window of any one of embodiments 1 to 10, wherein the substrate has a thickness of about 100 μm to about 5 mm.
[0237] EMBODIMENT 12 12. The window according to any one of the preceding embodiments, wherein the substrate has a refractive index of about 1.45 to about 1.55 for electromagnetic waves having a wavelength of 1550 nm.
[0238] EMBODIMENT 13 13. The window of any of the preceding embodiments, wherein the one or more high refractive index materials have a refractive index of about 1.7 to about 4.0, and the one or more low refractive index materials have a refractive index of about 1.3 to about 1.6.
[0239] EMBODIMENT 14 14. The window of any one of the preceding embodiments, wherein the difference in refractive index between any of the one or more high refractive index materials and any of the one or more low refractive index materials is about 0.5 or more.
[0240] EMBODIMENT 15 A window as described in any one of embodiments 1 to 14, wherein one of the alternating layers in the first multilayer film that is located farthest from the substrate constitutes the material of the edge of the window, and the material of the edge of the window includes the low refractive index material.
[0241] EMBODIMENT 16 16. The window of embodiment 15, wherein the first multilayer comprises a scratch-resistant layer formed from one of the one or more high refractive index materials and having a thickness of 500 nm or more.
[0242] EMBODIMENT 17 17. The window of embodiment 16, wherein the thickness of the scratch resistant layer is equal to or greater than 1500 nm and equal to or less than 5000 nm.
[0243] EMBODIMENT 18 18. The window of embodiment 17, wherein the scratch resistant layer is spaced from the edge by multiple ones of the alternating layers of the one or more low refractive index materials and the one or more high refractive index materials in the first multilayer.
[0244] EMBODIMENT 19 19. The window of embodiment 18, wherein the scratch resistant layer is spaced at least 1000 nm from the edge.
[0245] EMBODIMENT 20 20. The window of any one of the preceding embodiments, wherein the one or more high refractive index materials in the second multilayer comprises silicon.
[0246] EMBODIMENT 21 21. The window of embodiment 20, wherein the second multilayer comprises two or more silicon layers.
[0247] EMBODIMENT 22 22. The window of embodiment 21, wherein the silicon layer of the second multilayer closest to the substrate has the smallest thickness of the two or more silicon layers.
[0248] EMBODIMENT 23 22. The window of embodiment 21, wherein the silicon layers in the second multilayer have a total thickness of 250 nm or greater.
[0249] EMBODIMENT 24 23. The window of embodiment 22, wherein the total thickness is 500 nm or greater.
[0250] EMBODIMENT 25 25. The window of any one of embodiments 21 to 24, wherein the one or more layers of high refractive index material in the second multilayer include a non-silicon layer.
[0251] EMBODIMENT 26 26. The window of any one of the preceding embodiments, wherein the maximum hardness, as measured by subjecting the first multilayer to Berkovich hardness testing, is at least 10 GPa.
[0252] EMBODIMENT 27 27. The window of any one of the preceding embodiments, wherein the first multilayer film has a hardness of at least 8 GPa over a depth range of 300 nm to 2000 nm as measured by Berkovich hardness testing.
[0253] EMBODIMENT 28 28. The window of any of the preceding embodiments, wherein the first multilayer has a hardness of at least 9 GPa over a depth range of 750 nm to 2000 nm as measured by Berkovich hardness testing.
[0254] EMBODIMENT 29 a substrate having a first surface and a second surface, the first surface and the second surface being major surfaces of the substrate; a first multilayer disposed on the first surface of the substrate, the first multilayer including alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the first multilayer being higher than the refractive index of the one or more low refractive index materials of the first multilayer; a second multilayer disposed on the second surface of the substrate, the second multilayer including alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the second multilayer being higher than the refractive index of the one or more low refractive index materials of the second multilayer; 1. A window for a detection system comprising: the first multilayer film has a maximum hardness of at least 8 GPa as measured by a Berkovich indentation hardness test; The number, thickness, number of layers, and material of the alternating layers in the first multilayer film and the second multilayer film are the average reflectance of the window is less than 0.5% for light incident on the first surface and the second surface at an angle of 15° or less in a target wavelength range of 50 nm within a range of 1400 nm to 1600 nm; the window has a CIELAB L* value of 45 or less for an angle of incidence of 60° or less with respect to the first multilayer; a window configured such that the CIELAB a* and b* values of the window when viewed from the first multilayer film side are greater than or equal to -6.0 and less than or equal to 6.0.
[0255] EMBODIMENT 30 30. The window of embodiment 29, wherein the CIELAB L* value for an incidence angle of 60° or less on the first multilayer is 30 or less.
[0256] EMBODIMENT 31 A window as described in any of embodiments 29 to 30, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured so that the average transmittance of the window, determined in the target wavelength range of 50 nm width within the range of 1400 nm to 1600 nm, exceeds 95% for light incident on the first surface and the second surface at an incident angle of 15° or less.
[0257] EMBODIMENT 32 A window as described in any of embodiments 29 to 31, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured such that the average transmittance of the window measured in the range of 400 nm to 700 nm for light incident on the first surface and the second surface at an incident angle of 15° or less is less than 5%.
[0258] EMBODIMENT 33 A window as described in any of embodiments 29 to 32, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured so that the average P-polarized light transmittance and average S-polarized light transmittance of the window, determined in the target wavelength range of 50 nm width within the range of 1400 nm to 1600 nm, exceeds 85% for light incident on the first surface and the second surface at an incident angle of 60° or less.
[0259] EMBODIMENT 34 34. The window of embodiment 33, wherein the average P-polarized light transmittance and the average S-polarized light transmittance of the window are greater than 92% in the target wavelength range of 1400 nm to 1600 nm, the average P-polarized light transmittance being determined for light incident on the first surface and the second surface at an angle of incidence of 60° or less.
[0260] EMBODIMENT 35 A window as described in any one of embodiments 29 to 34, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured so that the average reflectance of the window over the entire visible spectrum for light perpendicularly incident on the first multilayer film is 10% or less.
[0261] EMBODIMENT 36 A window as described in any of embodiments 29 to 35, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured so that the average transmittance of the window, determined in the target wavelength range of 50 nm width within the range of 1400 nm to 1600 nm, for light perpendicularly incident on the first surface and the second surface, exceeds 95%.
[0262] EMBODIMENT 37 37. The window of any one of embodiments 29 to 36, wherein the maximum hardness measured by subjecting the first multilayer to Berkovich indentation hardness testing is at least 10 GPa.
[0263] EMBODIMENT 38 38. The window of any one of embodiments 29 to 37, wherein the first multilayer has a hardness of at least 8 GPa over a depth range of 300 nm to 2000 nm as measured by Berkovich hardness testing.
[0264] EMBODIMENT 39 one of the alternating layers in the first multilayer film that is furthest from the substrate constitutes a material for an edge of the window, the material for the edge of the window including the low refractive index material; 39. The window of any one of claims 29 to 38, wherein the first multilayer film includes a scratch-resistant layer, the scratch-resistant layer being formed from one of the one or more high refractive index materials and having a thickness of 1500 nm or more and 5000 nm or less.
[0265] EMBODIMENT 40 the scratch-resistant layer is spaced from the end surface by a plurality of layers among the alternating layers in which the one or more low refractive index materials and the one or more high refractive index materials are alternately stacked in the first multilayer film; 40. The window of embodiment 39, wherein the scratch resistant layer is spaced at least 1000 nm from the edge.
[0266] EMBODIMENT 41 41. The window of any one of embodiments 29 to 40, wherein the one or more high refractive index materials in the second multilayer comprises silicon.
[0267] EMBODIMENT 42 42. The window of embodiment 41, wherein the second multilayer comprises two or more silicon layers.
[0268] EMBODIMENT 43 43. The window of embodiment 42, wherein the silicon layer of the second multilayer closest to the substrate has the smallest thickness of the two or more silicon layers.
[0269] EMBODIMENT 44 44. The window of embodiment 43, wherein the silicon layers in the second multilayer have a total thickness of 250 nm or more.
[0270] EMBODIMENT 45 45. The window of embodiment 44, wherein the total thickness is 500 nm or greater.
[0271] EMBODIMENT 46 46. The window of any one of embodiments 42 to 45, wherein the one or more layers of high refractive index material in the second multilayer include a non-silicon layer.
[0272] EMBODIMENT 47 a substrate having a first surface and a second surface, the first surface and the second surface being major surfaces of the substrate; a first multilayer disposed on the first surface of the substrate, the first multilayer including alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the first multilayer being higher than the refractive index of the one or more low refractive index materials of the first multilayer; a second multilayer disposed on the second surface of the substrate, the second multilayer including alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the second multilayer being higher than the refractive index of the one or more low refractive index materials of the second multilayer, and the one or more high refractive index materials of the second multilayer including silicon; 1. A window for a detection system comprising: the maximum hardness of the window is at least 8 GPa as measured by performing a Berkovich hardness test on the first multilayer; The number, thickness, number of layers, and material of the alternating layers in the first multilayer film and the second multilayer film are the average reflectance of the window measured in a target wavelength range of 1400 nm to 1600 nm with a width of 50 nm for light incident on the first surface and the second surface at an angle of 15° or less is less than 1%, A window configured so that the average transmittance of the window, determined in the target wavelength range of 1400 nm to 1600 nm and having a width of 50 nm, exceeds 90% for light incident on the first surface and the second surface at an angle of incidence of 15° or less.
[0273] EMBODIMENT 48 48. The window of embodiment 47, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured such that the average transmittance of the window measured in the range of 400 nm to 700 nm is less than 5% for light incident on the first surface and the second surface at an angle of incidence of 15° or less.
[0274] EMBODIMENT 49 A window as described in any of embodiments 47 to 48, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured so that the average P-polarized light transmittance and average S-polarized light transmittance of the window, determined in the target wavelength range of 50 nm width within the range of 1400 nm to 1600 nm, exceeds 85% for light incident on the first surface and the second surface at an incident angle of 60° or less.
[0275] EMBODIMENT 50 50. The window of embodiment 49, wherein the average P-polarized light transmittance and the average S-polarized light transmittance of the window are greater than 92% in the target wavelength range of 1400 nm to 1600 nm, the average P-polarized light transmittance being determined for light incident on the first surface and the second surface at an angle of incidence of 60° or less.
[0276] EMBODIMENT 51 51. A window as described in any one of embodiments 47 to 50, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured such that the CIELAB L* value of the window for an incident angle of 60° or less to the first multilayer film is 45 or less.
[0277] EMBODIMENT 52 52. The window of embodiment 51, wherein the CIELAB L* value for an incidence angle of 60° or less on the first multilayer is 30 or less.
[0278] EMBODIMENT 53 A window as described in any of embodiments 47 to 52, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured such that the CIELAB a* and b* values of the window when viewed from the first multilayer film side are greater than or equal to -6 and less than or equal to 6.
[0279] EMBODIMENT 54 54. A window as described in any one of embodiments 47 to 53, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first multilayer film and the second multilayer film are configured such that the average reflectance of the window over the entire visible spectrum for light perpendicularly incident on the first multilayer film is 10% or less.
[0280] EMBODIMENT 55 one of the alternating layers in the first multilayer film that is furthest from the substrate constitutes a material for an edge of the window, the material for the edge of the window including the low refractive index material; 55. The window of any one of embodiments 47 to 54, wherein the first multilayer film includes a scratch-resistant layer, the scratch-resistant layer being formed from one of the one or more high refractive index materials and having a thickness of 1500 nm or more and 5000 nm or less.
[0281] EMBODIMENT 56 the scratch-resistant layer is spaced from the end surface by a plurality of layers among the alternating layers in which the one or more low refractive index materials and the one or more high refractive index materials are alternately stacked in the first multilayer film; 56. The window of embodiment 55, wherein the scratch resistant layer is spaced at least 1000 nm from the edge.
[0282] EMBODIMENT 57 57. The window of any one of embodiments 47 to 56, wherein the second multilayer comprises two or more silicon layers.
[0283] EMBODIMENT 58 58. The window of embodiment 57, wherein the silicon layer of the second multilayer closest to the substrate has the smallest thickness of the two or more silicon layers.
[0284] EMBODIMENT 59 58. The window of embodiment 57, wherein the silicon layers in the second multilayer have a total thickness of 250 nm or more.
[0285] EMBODIMENT 60 60. The window of embodiment 59, wherein the total thickness is 500 nm or greater.
[0286] EMBODIMENT 61 61. The window of any one of embodiments 57 to 60, wherein the one or more layers of high refractive index material in the second multilayer include a non-silicon layer.
[0287] EMBODIMENT 62 62. The window of embodiment 61, wherein the layer of the one or more layers of high refractive index materials in the second multilayer film that is not silicon is the layer of the one or more layers of high refractive index materials closest to the substrate. [Explanation of symbols]
[0288] 10 Vehicles 12 LIDAR system 14 Vehicle roof 16 Front of vehicle 18 Electromagnetic radiation detector 20. Cabinet 22 Outgoing electromagnetic wave 24 Windows 26 Outside world 28 Reflected electromagnetic waves 30 Substrate 32 First side of the board 34 Second side of the board 35 Board thickness 36 First multilayer film 38 Second multilayer film 40 High refractive index materials 42 Low refractive index materials 44 End face of first multilayer film 46 Thickness of the first multilayer 48 End face of second multilayer film 50 Thickness of the second multilayer
Claims
1. a substrate having a first surface and a second surface, the first surface and the second surface being major surfaces of the substrate; a first multilayer disposed on the first surface of the substrate, the first multilayer including alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the first multilayer being higher than the refractive index of the one or more low refractive index materials of the first multilayer; a second multilayer disposed on the second surface of the substrate, the second multilayer including alternating layers of one or more high refractive index materials and one or more low refractive index materials, the refractive index of the one or more high refractive index materials of the second multilayer being higher than the refractive index of the one or more low refractive index materials of the second multilayer; 1. A window for a detection system comprising: the maximum hardness of the window as measured by performing a Berkovich hardness test on the first multilayer is at least 8 GPa; The number, thickness, number of layers, and material of the alternating layers in the first multilayer film and the second multilayer film are: the average transmittance of the window is greater than 90% for light incident on the first surface and the second surface at an angle of incidence of 15° or less in a target wavelength range of 50 nm in a range of 1400 nm to 1600 nm; the average reflectance of the window is less than 1% for light incident on the first surface and the second surface at an angle of 15° or less in the target wavelength range of 1400 nm to 1600 nm with a width of 50 nm; A window configured such that for light incident on the first surface and the second surface at an angle of incidence of 15° or less, the window has an average transmittance of less than 5% measured over a range of 400 nm to 700 nm.
2. 2. The window of claim 1 , wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the average P-polarized light transmittance and average S-polarized light transmittance of the window is greater than 85% over the 50 nm wide wavelength range of interest within the range of 1400 nm to 1600 nm for light incident on the first and second faces at an angle of incidence of 60° or less.
3. the number, thickness, number of layers, and materials of the alternating layers in the first and second multilayers are configured such that the window has a CIELAB L* value of 45 or less for an angle of incidence of 60° or less relative to the first multilayer; 3. The window of claim 1 or 2, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the CIELAB a* and b* values of the window when viewed from the first multilayer film are greater than or equal to -6.0 and less than or equal to 6.
0.
4. 3. The window of claim 1 or 2, wherein the quantity, thickness, number of layers, and materials of the alternating layers in the first and second multilayer films are configured such that the average reflectance of the window across the visible spectrum for light perpendicularly incident on the first multilayer film is 10% or less.
5. the refractive index of said one or more high refractive index materials is from about 1.7 to about 4.0, and the refractive index of said one or more low refractive index materials is from about 1.3 to about 1.6; 3. The window of claim 1 or 2, wherein the difference in refractive index between any of the one or more high refractive index materials and any of the one or more low refractive index materials is about 0.5 or more.
6. 3. The window of claim 1, wherein one of the alternating layers in the first multilayer film that is furthest from the substrate constitutes the material of an edge of the window, the material of the edge of the window comprising the low refractive index material.
7. the first multilayer film includes a scratch-resistant layer, the scratch-resistant layer being formed from one of the one or more high refractive index materials and having a thickness of 1500 nm or more and 5000 nm or less; 7. The window of claim 6, wherein the scratch resistant layer is spaced from the edge by multiple ones of the alternating layers of the one or more low refractive index materials and the one or more high refractive index materials in the first multilayer.
8. The window of claim 7 , wherein the scratch resistant layer is spaced at least 1000 nm from the edge.
9. the one or more high refractive index materials in the second multilayer include silicon; 3. The window of claim 1 or 2, wherein the second multilayer comprises two or more silicon layers.
10. The total thickness of the silicon layers included in the second multilayer film is 250 nm or more; 10. The window of claim 9, wherein the one or more layers of high refractive index material in the second multilayer have a non-silicon layer.
Citation Information
Patent Citations
Hardcoated glass-ceramic articles
US20180275318A1
Optical member
WO2020204194A1
Hardened optical windows with Anti-reflective, reflective, and absorbing layers for infrared sensing systems
WO2020247292A1
Cited By
Optical filter and near-infrared light sensor module
WO2026191910A1