Coated steel sheet with excellent corrosion resistance and weldability and its manufacturing method
A Zn-Mg-Al based plating layer with controlled composition and manufacturing process enhances corrosion resistance, weldability, and chemical conversion treatment properties in plated steel sheets, overcoming the limitations of conventional zinc-based plated steel sheets.
Patent Information
- Application Number
- JP2024519260
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-30
- Filing Date
- 2022-09-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-09-28
AI Technical Summary
Existing zinc-based plated steel sheets face issues with corrosion resistance, weldability, and chemical conversion treatment properties due to the adverse effects of high aluminum content, leading to poor paint adhesion and weld joint integrity.
A Zn-Mg-Al based plating layer with controlled composition and manufacturing process, including shot blasting and precise control of component distribution, ensures optimal corrosion resistance, weldability, and chemical conversion treatment properties by managing the content of Zn, Al, and Mg within specific relational expressions.
The solution provides a plated steel sheet with enhanced corrosion resistance, improved weldability, and superior chemical conversion treatment properties, addressing the limitations of conventional zinc-based plated steel sheets.
Smart Images

Figure 2024539568000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a highly corrosion-resistant plated steel sheet having excellent corrosion resistance and weldability, and a method for producing the same. [Background technology]
[0002] When exposed to a corrosive environment, zinc-based plated steel sheets have the property of sacrificial corrosion protection, in which zinc, which has a lower redox potential than iron, corrodes first, suppressing the corrosion of the steel. In addition, as the zinc in the plated layer oxidizes, it forms dense corrosion products on the surface of the steel, isolating the steel from the oxidizing atmosphere and improving the corrosion resistance of the steel. Due to these advantageous properties, the range of applications of zinc-based plated steel sheets has recently expanded to include building materials, home appliances, and automotive steel sheets.
[0003] However, the corrosive environment is gradually worsening due to increased air pollution accompanying industrial advancement, and strict regulations on resources and energy conservation are creating a growing need for the development of steel materials with superior corrosion resistance to conventional galvanized steel materials.
[0004] In order to solve these problems, various researches are being conducted on the manufacturing technology of zinc alloy-coated steel sheets that improve the corrosion resistance of steel materials by adding elements such as aluminum (Al) and magnesium (Mg) to the zinc plating bath. A representative example is Zn-Mg-Al zinc alloy-coated steel sheets, which further add Mg to the Zn-Al plating composition.
[0005] On the other hand, Zn-Mg-Al zinc alloy plated steel sheets are often used after painting or welding, but when a large amount of Al is distributed on the surface of the plated layer, the Al oxides deteriorate the chemical conversion treatment required for pre-painting treatment, resulting in poor paint adhesion. Furthermore, there is also the problem that pores remain in the weld metal due to the influence of Al vapor during arc welding, reducing the strength of the welded joint.
[0006] In addition, although processed zinc-based plated steel sheets are often attached to the outside of products, they do not meet the required surface quality due to surface damage factors such as partial peeling caused by deterioration of paint adhesion and poor shape of welded joints caused by weld pores, and therefore there was a need to improve the appearance quality.
[0007] Therefore, no technology has been developed to date that can satisfy the high demand for excellent properties such as corrosion resistance, weldability, and chemical conversion treatability. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Korean Patent Publication No. 2010-0073819 Summary of the Invention [Problem to be solved by the invention]
[0009] According to one aspect of the present invention, there is provided a plated steel sheet having excellent corrosion resistance and weldability, and a method for producing the same.
[0010] According to another aspect of the present invention, there are provided a plated steel sheet which is excellent in all of corrosion resistance, weldability and chemical conversion treatability, and a method for producing the same.
[0011] The object of the present invention is not limited to the above. Anyone having ordinary skill in the art to which the present invention pertains will have no difficulty in understanding additional objects of the invention from the entire contents of the specification of the present invention. [Means for solving the problem]
[0012] One aspect of the present invention is Base steel sheet; and a Zn-Mg-Al-based coating layer provided on at least one surface of the base steel sheet; The above-mentioned plating layer provides a plated steel sheet that satisfies the following Relational Expressions 1 and 2. [Equation 1] -10.0≦[Zn] 1 / 10t -[Zn] s <=-5.0 (In the above Relational Formula 1, the above [Zn] 1 / 10t represents the weight percent content of Zn at a position 1 / 10t from the surface of the plating layer in the thickness direction (t is the total thickness of the plating layer), and the above [Zn] s represents the weight percent content of Zn on the surface of the plating layer.) [Equation 2] +3.0≦[Al] 1 / 10t -[Al] s ≦+13.0 (In the above Relational Formula 2, the above [Al] 1 / 10t represents the weight percent content of Al at the 1 / 10t position (t is the total thickness of the plating layer) from the surface of the plating layer in the thickness direction, and the above [Al] s represents the weight percent content of Al on the surface of the plating layer.)
[0013] Another aspect of the present invention is a step of performing a first shot blasting process by projecting metal balls having a grain size of 0.6 to 1.0 mm at 400 to 1200 kg / min onto the surface of the base steel sheet, the metal balls being moved in a shot blasting cabin in which the metal balls are circulated at a rotation speed of 1200 to 2000 mpm; a step of performing a secondary shot blasting process by projecting metal balls having a grain size of 0.2 to 0.5 mm at 400 to 1200 kg / min onto the surface of the base steel sheet, the metal balls being moved in the shot blasting cabin in which the metal balls are circulated at a rotation speed of 1200 to 2000 mpm; a step of immersing the shot blasted base steel sheet in a galvanizing bath containing, by weight, 4.0-7.0% Mg, 8.2-19.5% Al, the balance Zn and other unavoidable impurities, and maintained at a temperature of Ts+20°C to Ts+80°C relative to the solidification start temperature (Ts) on the equilibrium diagram, to perform hot-dip galvanizing; cooling the hot-dip galvanized steel sheet from a solidification start temperature to a solidification finish temperature at an average cooling rate of 2 to 8°C / s using an inert gas. Effect of the Invention
[0014] Advantageous Effects of Invention According to one aspect of the present invention, there is provided a plated steel sheet having excellent corrosion resistance and weldability, and a method for manufacturing the same.
[0015] According to another aspect of the present invention, it is possible to provide a plated steel sheet which is excellent in all of corrosion resistance, weldability and chemical conversion treatability, and a method for producing the same.
[0016] The various yet significant advantages and effects of the present invention are not limited to the above, but can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]
[0017] [Figure 1] 1 is a diagram showing a component analysis profile using GDS for the plated steel sheet obtained in Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The terms used in the present specification are intended to describe the embodiments and are not intended to limit the present invention. In addition, the singular forms used in the present specification also include the plural forms unless the related definition clearly indicates otherwise.
[0019] The meaning of "comprise" as used in the specification is to specify a feature and does not exclude the presence or addition of other features.
[0020] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which this invention belongs. Dictionary-defined terms are to be interpreted as having a meaning consistent with the relevant technical literature and the presently disclosed content.
[0021] Hereinafter, a "plated steel sheet" according to one aspect of the present invention will be described in detail. In the present invention, the content of each element is expressed in percent by weight unless otherwise specified.
[0022] In conventional Zn-Mg-Al zinc alloy plated steel sheets, magnesium is added to improve corrosion resistance. However, if too much magnesium is added, there is a problem that more dross is generated floating in the plating bath, and the dross must be removed frequently. Therefore, the upper limit of magnesium addition is limited to 3%.
[0023] Therefore, research was conducted to further improve corrosion resistance by increasing the amount of Mg added beyond 3%, but the more Mg added, the more floating dross generated in the plating bath became significantly more difficult to manage, and the appearance of the product became darker and surface damage was introduced, making it difficult to ensure the appearance quality.
[0024] Therefore, in order to solve the above-mentioned problems, technical attempts have been made to increase the amount of Al added as the amount of Mg added increases, so that Al oxide is preferentially formed on the surface of the coating bath over Mg oxide, thereby suppressing floating dross on the Mg oxide base and preventing the phenomenon that the appearance of the product is easily blackened.
[0025] However, even if a component system with a high content of Al is set and plating workability and appearance quality are ensured, the Al oxides inevitably formed on the surface of the plating layer cause surface damage such as partial peeling due to deterioration of paint adhesion and poor shape of welded joints due to weld porosity, making it difficult to ensure appearance quality after painting and welding.
[0026] Therefore, in the conventional technology, it has been technically difficult to provide a Zn-Mg-Al zinc alloy plated steel sheet that ensures excellent corrosion resistance and at the same time excellent weldability and / or chemical conversion treatability.
[0027] Therefore, the present inventors conducted extensive research in order to solve the above-mentioned problems and at the same time provide a plated steel sheet that is excellent not only in corrosion resistance but also in weldability and / or chemical conversion treatability. As a result, the present inventors discovered that an important factor is the change in the content of each component (e.g., Zn and Al, and also including Mg) in a surface layer region from the surface of the plated layer to a 1 / 10t position in the thickness direction (t is the total thickness of the plated layer) after the effects of oxidation have been removed from the plated layer, and thus completed the present invention.
[0028] Therefore, the following will specifically describe the configuration of a plated steel sheet that has excellent corrosion resistance and, at the same time, excellent weldability and / or chemical conversion treatability.
[0029] First, the plated steel sheet according to the present invention includes a base steel sheet; and a Zn-Mg-Al-based plating layer provided on at least one surface of the base steel sheet.
[0030] In the present invention, the type of base steel sheet is not particularly limited. For example, the base steel sheet may be an Fe-based base steel sheet used as a base steel sheet for ordinary zinc-based plated steel sheets, i.e., a hot-rolled steel sheet or a cold-rolled steel sheet, but is not limited thereto. Alternatively, the base steel sheet may be, for example, a carbon steel, an extra-low carbon steel, or a high manganese steel used as a material for construction, home appliances, or automobiles.
[0031] However, as an example, the above-mentioned base steel sheet has, by weight%, C: more than 0% (more preferably, 0.001% or more) and 0.18% or less, Si: more than 0% (more preferably, 0.001% or more) and 1.5% or less, Mn: 0.01 to 2.7%, P: more than 0% (more preferably, 0.001% or more) and 0.07% or less, S: more than 0% (more preferably, 0.001% or more) and 0.015% or less, Al: more than 0% (more preferably, It may have a composition including: Nb: more than 0% (more preferably, 0.001% or more) and 0.06% or less, Cr: more than 0% (more preferably, 0.001% or more) and 1.1% or less, Ti: more than 0% (more preferably, 0.001% or more) and 0.06% or less, B: more than 0% (more preferably, 0.001% or more) and 0.03% or less, and the balance being Fe and other unavoidable impurities.
[0032] Although not particularly limited, according to one embodiment of the present invention, at least one surface of the base steel sheet may be provided with a Zn-Mg-Al-based plating layer made of a Zn-Mg-Al-based alloy. The plating layer may be formed on only one surface of the base steel sheet, or may be formed on both surfaces of the base steel sheet. In this case, the Zn-Mg-Al-based plating layer refers to a plating layer that contains Mg and Al and mainly contains Zn (i.e., contains 50% or more Zn).
[0033] Although not particularly limited, according to one embodiment of the present invention, the thickness of the Zn-Mg-Al-based coating layer may be 9 to 100 μm, and more preferably 20 to 90 μm. If the thickness of the coating layer is less than 9 μm, the coating layer may be locally too thin due to an error caused by the thickness deviation of the coating layer, and the corrosion resistance may be poor. If the thickness of the coating layer exceeds 100 μm, the cooling of the hot-dip coating layer may be delayed, and there may be room for solidification defects such as sagging to occur on the surface of the coating layer, and the productivity of the steel sheet may decrease in order to solidify the coating layer.
[0034] Meanwhile, although not particularly limited, according to an embodiment of the present invention, an Fe-Al-based inhibition layer may be further included between the base steel sheet and the Zn-Mg-Al-based coating layer. The Fe-Al-based inhibition layer is a layer mainly containing (for example, 60% or more) an intermetallic compound of Fe and Al, and examples of the intermetallic compound of Fe and Al include FeAl, FeAl3, Fe2Al5, etc. In addition, a component derived from the coating layer such as Zn, Mg, etc. may be further included, for example, 40% or less. The inhibition layer is a layer formed by alloying Fe diffused from the initial coating base steel sheet and coating bath components. The inhibition layer can play a role in improving the adhesion between the base steel sheet and the coating layer, and at the same time, can play a role in preventing Fe diffusion from the base steel sheet to the coating layer. The inhibition layer can be formed continuously or discontinuously between the base steel sheet and the Zn-Mg-Al-based coating layer. In this case, with respect to the inhibition layer, contents commonly known in the art can be similarly applied, except for the above description.
[0035] Although not particularly limited, according to one embodiment of the present invention, the thickness of the inhibition layer may be 0.01 to 2.50 μm. The inhibition layer plays a role in preventing alloying and ensuring corrosion resistance, but since it is brittle, it may affect workability, so the thickness may be 2.50 μm or less. However, in order to play the role of an inhibition layer, the thickness may be 0.01 μm or more. From the viewpoint of further improving the above-mentioned effects, the upper limit of the thickness of the inhibition layer may be preferably 1.80 μm. In addition, the lower limit of the thickness of the inhibition layer may be 0.02 μm. In this case, the thickness of the inhibition layer may mean the minimum thickness in a direction perpendicular to the interface of the base steel sheet.
[0036] On the other hand, although not particularly limited, according to one embodiment of the present invention, the Zn-Mg-Al-based plating layer may contain, by weight %, 4.0-7.0% Mg, 8.2-19.5% Al, the balance being Zn and other inevitable impurities. Each component will be specifically described below.
[0037] Mg: 4.0% or more and 7.0% or less Mg is an element that plays a role in improving the corrosion resistance of plated steel materials, and in the present invention, the Mg content in the plated layer is controlled to 4.0% or more to ensure the desired excellent corrosion resistance. On the other hand, if Mg is added excessively, dross may be generated, so the Mg content is controlled to 7.0% or less. On the other hand, from the viewpoint of further maximizing the above-mentioned effects, more preferably, the lower limit of the Mg content may be 4.7%, or the upper limit of the Mg content may be 6.0%.
[0038] Al: 8.2% or more and 19.5% or less Generally, when Mg is added at 1% or more, the effect of improving corrosion resistance is exhibited, but when Mg is added at 2% or more, the generation of floating dross in the coating bath due to oxidation of Mg in the coating bath increases, and the dross needs to be removed frequently. Due to this problem, in the conventional technology, Mg is added at 1.0% or more in Zn-Mg-Al zinc alloy coating to ensure corrosion resistance, but the upper limit of Mg content was set at 3.0% and put into common use. However, as mentioned above, in order to further improve corrosion resistance, the Mg content needs to be increased to 4% or more, but if the coating layer contains Mg at 4% or more, there is a problem of dross generation due to oxidation of Mg in the coating bath, so Al needs to be added at 8.2% or more. However, if Al is added excessively to suppress dross, the melting point of the coating bath increases, and the operating temperature becomes too high, which can cause problems due to high-temperature work such as erosion of the coating bath structure and denaturation of the steel material. Furthermore, if the Al content in the coating bath is excessive, Al will react with Fe in the base steel and will not contribute to the formation of the Fe-Al inhibiting layer, and the reaction between Al and Zn will occur rapidly, resulting in the excessive formation of a lumpy outburst phase, which may actually worsen the corrosion resistance. Therefore, it is preferable to control the upper limit of the Al content in the coating layer to 19.5%. On the other hand, from the viewpoint of maximizing the above-mentioned effects, it is more preferable that the lower limit of the Al content be 11.0%, or the upper limit of the Al content be 18.0%.
[0039] The balance is Zn and other unavoidable impurities. In addition to the above-mentioned composition of the coating layer, the balance may be Zn and other inevitable impurities. The inevitable impurities may include all impurities that are unintentionally mixed in the normal manufacturing process of hot-dip galvanized steel sheets, and the meaning thereof can be easily understood by a person skilled in the art.
[0040] According to the present invention, the plating layer satisfies the following relations 1 and 2. [Equation 1] -10.0≦[Zn] 1 / 10t -[Zn] s <=-5.0 (In the above Relational Formula 1, the above [Zn] 1 / 10t represents the weight percent content of Zn at a position 1 / 10t from the surface of the plating layer in the thickness direction (t is the total thickness of the plating layer), and the above [Zn] s represents the weight percent content of Zn on the surface of the plating layer.) [Equation 2] +3.0≦[Al] 1 / 10t -[Al] s ≦+13.0 (In the above Relational Formula 2, the above [Al] 1 / 10t represents the weight percent content of Al at the 1 / 10t position (t is the total thickness of the plating layer) from the surface of the plating layer in the thickness direction, and the above [Al] s represents the weight percent content of Al on the surface of the plating layer.)
[0041] The inventors conducted extensive research to ensure improved corrosion resistance compared to conventional techniques while at the same time ensuring weldability and / or chemical conversion treatability, and as a result, found that, excluding the effects of oxidation in the plating layer, an important factor is the change in the content of each component (e.g., Zn and Al, and also Mg) in the surface layer region from the surface of the plating layer to the 1 / 10t position in the thickness direction (t is the total thickness of the plating layer).
[0042] In the present invention, the Zn-Mg-Al-based coating layer can contain a Zn single phase and a Zn-MgZn2-Al ternary eutectic phase, which are phases commonly appearing in highly corrosion-resistant coated steel sheets. Usually, the lower the Al and Mg contents in the coating layer, the greater the amount of the Zn single phase and the Zn-MgZn2-Al ternary eutectic phase generated in the entire coating layer, and the greater the Al and Mg contents in the coating layer, the greater the amount of the MgZn2 phase and the Al single phase generated. In this case, in a coating composition system such as that of the present invention, in which the Mg content is 4% or more, the Al content must also increase at the same time as the Mg content increases in order to suppress dross, so that the Al single phase also coexists accordingly. Therefore, through extensive research, the inventors have found that suppressing the nucleation and growth of the above-mentioned MgZn2 phase and single Al phase on the surface of the coating layer and promoting it inside the coating layer makes it possible to increase the distribution of the single Zn phase, Al-Zn binary eutectic phase and Zn-MgZn2-Al ternary eutectic phase on the surface of the coating layer, and contributes to producing a coating layer surface that has a high Zn content and at the same time a low Al content.
[0043] That is, the inventors have confirmed that the region that ensures the above-mentioned corrosion resistance and at the same time directly affects the weldability and chemical conversion treatability is the surface layer region from the surface of the coating layer to the 1 / 10t position in the thickness direction. Therefore, it has been found that by controlling the change in the Zn content and the change in the Al content in the surface layer region of the coating layer so as to satisfy the above-mentioned Relational Expressions 1 and 2, a coated steel sheet that is excellent not only in corrosion resistance but also in weldability and / or chemical conversion treatability can be effectively obtained.
[0044] On the other hand, although not particularly limited, according to one embodiment of the present invention, from the viewpoint of further maximizing the above-mentioned effects, it is more preferable to use [Zn] defined by the above-mentioned Relational Formula 1. 1 / 10t -[Zn] s The lower limit of the value can be -9.9, or the above [Zn] 1 / 10t -[Zn] s The upper limit of the value can be -5.3 (most preferably -7.0). Also, [Al] as defined in the above Relation 2 can be 1 / 10t -[Al]s The lower limit of the value can be +6.4, or the above [Al] 1 / 10t -[Al] s The upper limit of the value can be +11.1.
[0045] Furthermore, although not particularly limited, according to one embodiment of the present invention, the inventors have conducted extensive research to further improve corrosion resistance and have further discovered that selectively controlling the profile of the Mg content in the thickness direction so as to further satisfy the following Relational Formula 3 allows corrosion to progress uniformly in the thickness direction, thereby achieving an effect of improving corrosion resistance to an even higher level. [Equation 3] -1.0≦[Mg] 1 / 10t -[Mg] s ≦+1.0 (In the above Relational Formula 3, the above [Mg] 1 / 10t represents the weight percent content of Mg at a position 1 / 10t from the surface of the coating layer in the thickness direction (t is the total thickness of the coating layer), and the above [Mg] s represents the weight percent content of Mg on the surface of the plating layer.)
[0046] According to one embodiment of the present invention, the sacrificial corrosion protection cell acting as the corrosion resistance mechanism of the Zn-Mg-Al-based plating layer has a large potential difference, with the potential of MgZn2 being -1.2V on the hydrogen reduction potential and the potential of Al being -0.7V on the hydrogen reduction potential, and acts as an anode and a cathode, respectively, to form a galvanic cell between the adjacent MgZn2 phase and the microstructure of the Al single phase. That is, when the anode (MgZn2) of the sacrificial corrosion protection cell, from which dissolution occurs as corrosion progresses, is irregularly formed in the depth direction of the plating layer, the potential difference between the anode and cathode of the galvanic cell having the above-mentioned excellent corrosion resistance and sacrificial corrosion protection is formed to be different depending on the position of the flat plate, and corrosion occurs first at a specific portion, so that corrosion can progress unevenly depending on the position. Therefore, by controlling the change in Mg content of the surface layer of the plating layer to be small so as to satisfy the above-mentioned relational expression 3, uniform corrosion in the thickness direction can be promoted, and the overall corrosion resistance can be further improved.
[0047] On the other hand, although not particularly limited, according to one embodiment of the present invention, from the viewpoint of further maximizing the above-mentioned effects, it is more preferable to use [Mg] defined in the above Relation 3. 1 / 10t -[Mg] s The lower limit of the value can be -0.8, or the above [Mg] 1 / 10t -[Mg] s The upper limit of the value can be +0.8.
[0048] The method for measuring the content of each component at the 1 / 10t position defined by the above-mentioned Relational Formulas 1 to 3 and the content of each component on the surface of the plating layer is not particularly limited, but can be measured, for example, by the following method.
[0049] That is, after cutting the plated steel material vertically, the content distribution of each component such as Zn, Al, Mg, and Fe in the cross section of the plated layer is measured using a glow discharge spectrometry (GDS). Next, in order to eliminate the influence of oxidation of the plated layer, the region from the outermost surface of the plated layer to 0.1 μm in the thickness direction is excluded in the present invention. Therefore, in this specification, the above-mentioned "surface of the plated layer" means a point 0.1 μm from the outermost surface of the plated layer in the thickness direction, excluding the region affected by the oxidation. Therefore, the content of each component in the surface of the plated layer defined by the above-mentioned Relational Formulas 1 to 3 can be defined as the content of each component (Zn, Al, and Mg) at a position 0.1 μm from the outermost surface of the plated layer.
[0050] Meanwhile, in order to define the content of each component at the 1 / 10t position in the thickness direction from the surface of the above-mentioned coating layer, the thickness (t) of the entire coating layer is defined as the distance t from the surface of the coating layer to the position where the contents of Zn and Fe are equal to each other, based on the profile of each component measured using the above-mentioned GDS. This makes it possible to define the 1 / 10t position of the total thickness t of the above-mentioned coating layer, and therefore the content of each component (Zn, Al, and Mg) measured by GDS at the point of 1 / 10t can be measured.
[0051] For example, in the case of Example 7 defined in Figure 1, the value of t up to the position where the contents of Zn and Fe are equal to each other is about 34 μm. Therefore, since the 1 / 10t position means a point about 3.4 μm from the surface of the plating layer, by measuring the weight percent content of each component at a point about 3.4 μm from the surface of the plating layer, [Zn] 1 / 10t , [Al] 1 / 10t , [Mg] 1 / 10t The value of can be measured.
[0052] In addition, although not particularly limited, according to one embodiment of the present invention, the Mg content by weight at a 2 / 3t position from the surface of the plating layer in the thickness direction may be within a range of ±0.5 wt% of the average Mg content by weight in the plating layer. By satisfying this range, corrosion progresses uniformly in the thickness direction, and an effect of improving corrosion resistance to a higher level can be achieved.
[0053] On the other hand, although not particularly limited, from the viewpoint of maximizing the above-mentioned effects, it is more preferable that the Mg content by weight at the 2 / 3t position in the thickness direction from the surface of the plating layer satisfies the range of ±0.3 wt% of the average Mg content by weight in the plating layer.
[0054] In this case, the method for measuring the average content by weight of Mg in the coating layer is not particularly limited, but as an example, it can be defined as an average value calculated by measuring the Mg content at each point every 0.5 μm up to the shortest distance t, excluding the region from the outermost surface of the coating layer to 0.1 μm, based on the change in Mg content in the thickness direction measured using the above-mentioned GDS.
[0055] Similarly, the Mg content by weight at the 2 / 3t position in the thickness direction from the surface of the above-mentioned plating layer can mean the Mg content at the 2 / 3t position, based on t as defined above, excluding the region from the outermost surface of the plating layer to 0.1 μm.
[0056] On the other hand, although not particularly limited, according to one embodiment of the present invention, the area ratio of the Al single phase having a Zn solid solution ratio of 27 atomic % or more on the surface of the coating layer may be selectively 2.0 to 10.1%. If the area ratio of the Al single phase having a Zn solid solution ratio of 27 atomic % or more is less than 2.0% or exceeds 10.0%, there is a possibility that one or more of the properties of weldability and chemical conversion treatability may be deteriorated. From the viewpoint of further improving the above-mentioned effect, preferably, the lower limit of the area ratio of the Al single phase having a Zn solid solution ratio of 27 atomic % or more may be 2.2%, or the upper limit of the area ratio of the Al single phase having a Zn solid solution ratio of 27 atomic % or more may be 4.0%.
[0057] In this specification, the term "Al single phase" refers to a phase mainly composed of Al, regardless of the Zn solid solution rate, and refers to a phase in which the remainder is Al, excluding the dissolved Zn and impurities such as Mg that are inevitably contained. Specifically, in the conventional technology, it was generally known that only an Al single phase with a low Zn solid solution rate of less than 27% exists as an Al single phase. However, as a result of intensive research by the present inventors, it was found that the Al single phase present on the surface of the coating layer is not only an Al single phase with a low Zn solid solution rate of less than 27%, but also an Al single phase with a high Zn solid solution rate of 27% or more. Furthermore, in order to additionally improve the above-mentioned corrosion resistance, weldability, chemical conversion treatability, etc., it was found that the area ratio of the Al single phase with a Zn solid solution rate of 27% or more is controlled to be low, but that the inclusion of 2.0 area % or more is an effective element in terms of reducing Al oxides generated on the surface of the coating layer that adversely affect weldability and chemical conversion treatability.
[0058] In addition, the method for measuring the area ratio of the Al single phase in which the Zn solid solution rate on the surface of the coating layer is 27 atomic % or more is not particularly limited. However, as an example, an image derived under the measurement conditions of a scanning electron microscope (SEM) is used using an automatic image generation software based on the Super-pixel algorithm of RISA (microstructural phase fraction analysis software) of the Pohang Research Institute of Industrial Science and Technology (RIST). The Super-pixel algorithm divides the entire image into several thousand to several tens of thousands of regions (super-pixels), compares super-pixels with similar patterns and characteristics to measure the similarity, calculates a histogram of pixel brightness values, and automatically selects super-pixels when the similarity is equal to or greater than a predefined threshold. As an example of specifying a predefined threshold, the boundaries of the Al single phase in the image derived by SEM are defined in advance for each phase based on the Zn solid solution rate of 27 atomic % solid solution in the Al single phase structure using EDS, which makes it possible to create a histogram of brightness values and distinguish structures on the software. The technical concept of the above-mentioned RISA (microstructural phase fraction analysis software) can be found in Korean Patent Publication No. 2019-0078331.
[0059] Next, a "method for producing a plated steel sheet" according to another aspect of the present invention will be described in detail. However, this does not necessarily mean that the plated steel sheet of the present invention must be produced by the following production method.
[0060] According to an embodiment of the present invention, the method may further include a step of preparing a base steel sheet, and the type of the base steel sheet is not particularly limited. It may be an Fe-based base steel sheet used as a base steel sheet for a typical hot-dip galvanized steel sheet, i.e., a hot-rolled steel sheet or a cold-rolled steel sheet, but is not limited thereto. In addition, the base steel sheet may be, for example, a carbon steel, an extra-low carbon steel, or a high manganese steel used as a material for construction, home appliances, and automobiles, but is not limited thereto. In this case, the above description may be similarly applied to the base steel sheet.
[0061] According to the present invention, a primary shot blasting treatment is performed on a steel sheet moving through a shot blasting cabin where metal material circulates at a rotation speed of 1200-2000mpm, by projecting metal balls having a grain size of 0.6-1.0mm onto the surface of the base steel sheet at 400-1200kg / min. By satisfying the conditions for the primary shot blasting treatment, it is possible to primarily remove surface oxides on the base steel sheet before plating, thereby ensuring the effect of minimizing the effects of oxides.
[0062] Following the primary shot blasting treatment, a secondary shot blasting treatment is performed by projecting metal balls with a grain size of 0.2 to 0.5 mm onto the surface of the base steel sheet at 400 to 1200 kg / min while the steel sheet is moving through a shot blasting cabin where metal material circulates at a rotation speed of 1200 to 2000 mpm. By satisfying the conditions for the secondary shot blasting treatment, it is possible to secure the effect of imparting fine plastic deformation to the steel sheet surface, increasing the dislocation density in the base steel structure, and activating the plating reaction.
[0063] Next, the base steel sheet that has been subjected to the above primary and secondary shot blasting treatments is immersed in a plating bath containing, by weight, 4.0 to 7.0% Mg, 8.2 to 19.5% Al, the balance Zn and other unavoidable impurities, and maintained at a temperature of Ts+20°C to Ts+80°C, where Ts is the start of solidification on the equilibrium diagram, to perform hot-dip galvanization.
[0064] In this regard, according to an embodiment of the present invention, the reasons for adding components and limiting the contents in the above-mentioned coating bath may be the same as those described above for the components of the coating layer, except for the small amount of Fe content that may flow in from the base steel sheet.
[0065] Meanwhile, in order to prepare the coating bath having the above composition, a composite ingot containing the desired Zn, Al, and Mg or a Zn-Mg or Zn-Al ingot containing individual components can be used. In order to replenish the coating bath consumed in hot dip coating, the ingot is melted and supplied. In this case, a method of directly immersing the ingot in the coating bath and melting it can be selected, or a method of melting the ingot in a separate port and then replenishing the molten metal to the coating bath can be selected.
[0066] Also, the temperature of the plating bath may be maintained at a temperature 20 to 80°C higher than the solidification start temperature (Ts) on the equilibrium diagram (i.e., Ts+20°C to Ts+80°C). In this case, the solidification start temperature on the equilibrium diagram may be in the range of 390 to 460°C, or the temperature of the plating bath may be maintained in the range of 440 to 520°C, without being particularly limited thereto. The higher the temperature of the plating bath, the more fluidity and uniform composition can be secured in the plating bath, and the less the amount of floating dross can be generated. If the temperature of the plating bath is less than Ts+20°C, the ingot dissolves very slowly, and the viscosity of the plating bath is high, making it difficult to secure excellent surface quality of the plating layer. On the other hand, if the temperature of the plating bath exceeds Ts+80°C, there may be a problem that ash defects due to Zn evaporation are induced on the plating surface.
[0067] Meanwhile, the hot-dip galvanized steel sheet is cooled using an inert gas at an average cooling rate of 2 to 8°C / s from the solidification start temperature to the solidification end temperature based on the surface temperature. According to the present invention, such slow cooling contributes to promoting nucleation and growth inside the coating layer rather than on the surface of the coating layer. Therefore, if the average cooling rate is less than 2°C / s, the MgZn2 structure develops very coarsely on the surface, and the entire coating layer becomes brittle, which causes frequent cracking, which may be disadvantageous in ensuring uniform corrosion resistance and workability. On the other hand, if the average cooling rate exceeds 8°C / s, the change from the liquid phase to the solid phase during the hot-dip coating process occurs too rapidly, and a locally non-uniform phase is formed on the surface of the coating layer, which may result in color deviation in the width direction of the coated steel sheet and a decrease in corrosion resistance.
[0068] In addition, although not particularly limited, according to an embodiment of the present invention, optionally, the method may further include a step of performing pre-temper rolling of the shot blasted base steel sheet, in which a roll reduction of 100 to 400 tons is applied to the steel sheet surface using a dull roll having a surface roughness Ra of 1.8 to 2.8 μm, prior to the hot-dip galvanizing.
[0069] The present inventors have conducted extensive research to further improve the weldability and / or chemical conversion treatability, and as a result have found that by performing a pre-pass milling (SPM) process using a dull roll that satisfies the above-mentioned conditions, it is possible to irregularly control the surface shape of the base steel sheet, thereby maximizing the number of sites for generating solidification nuclei inside the coating layer in the subsequent coating process.
[0070] Specifically, if the surface roughness Ra of the dull roll is less than 1.8 μm, a problem may occur in that nucleation in the surface layer of the coating layer is promoted rather than nucleation inside the coating layer, whereas if the surface roughness Ra of the dull roll is more than 2.8 μm, a problem may occur in that excessive dents are formed on the base steel sheet, resulting in non-uniform thickness of the hot-dip coating layer formed in the subsequent coating process in the width direction.
[0071] Furthermore, if the roll reduction of the dull roll is less than 100 tons, the shape control effect of the base steel sheet is low, making it difficult to expect the above-mentioned effect of promoting solidification nucleation inside the coating layer. If the roll reduction of the dull roll exceeds 400 tons, there is a risk of inducing C-warp or the like in the base steel sheet, making it difficult to expect the effect of contributing to uniform formation in the coating layer thickness direction.
[0072] As described above, by precisely controlling the coating composition and manufacturing conditions, it is possible to effectively provide a plated steel sheet that is excellent not only in corrosion resistance but also in weldability and / or chemical conversion treatability. EXAMPLES
[0073] The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are for illustrative purposes only and are not intended to limit the scope of the present invention. The scope of the present invention is determined by the matters described in the claims and matters reasonably inferred therefrom.
[0074] (Example) A primary and secondary shot blasting treatment was performed on a base steel sheet having a composition of C: 0.018%, Si: 0.01%, Mn: 0.2%, P: 0.009%, S: 0.005%, Al: 0.1%, Nb: 0.02%, Cr: 0.2%, Ti: 0.02%, B: 0.015%, the balance being Fe and impurities, under the conditions shown in Table 1 below. Then, a pre-temper rolling (SPM) treatment was performed so as to satisfy the conditions shown in Table 1 below. After this, hot-dip galvanizing was performed so as to satisfy the plating bath composition (the balance being Zn and impurities) and plating bath temperature shown in Table 2 below, and then cooling was performed using inert gas N2 so as to satisfy the conditions shown in Table 2 below.
[0075] [Table 1] Bright*: Uses a bright roll with a surface roughness Ra of 0.2 to 0.6 μm. Dull*: A dull roll with a surface roughness Ra of 1.8 to 2.8 μm is used.
[0076] [Table 2] Ts*: Solidification start temperature on the equilibrium phase diagram [℃] Te*: End of solidification temperature [℃]
[0077] Test pieces of the above-mentioned plated steel sheets were prepared, and the plating layers were dissolved in a hydrochloric acid solution. The dissolved liquid was then analyzed by inductively coupled plasma (ICP) method to determine the compositions of the plating layers, which are shown in Table 3 below (the remainder corresponds to Zn and impurities).
[0078] In addition, cross-sectional test pieces were prepared by cutting the steel sheet in the thickness direction (i.e., the direction perpendicular to the rolling direction) so that the interface between the coating layer and the base steel could be observed, and photographs were taken with a scanning electron microscope (SEM). It was confirmed that a 0.02 μm-thick Fe-Al-based inhibitor layer was formed between the base steel sheet and the Zn-Mg-Al-based coating layer.
[0079] In addition, a GDS measuring device was used to perform a component analysis from the surface of the plating layer in the thickness direction, and the content of each component of Zn, Al, and Mg at the 1 / 10t position and the content at the surface at 0.1 μm from the surface were measured, excluding the region up to a point 0.1 μm from the surface, in order to eliminate the effects of oxidation, and the results are shown in Table 3 below.
[0080] [Table 3] [Zn] 1 / 10t : Zn weight percentage content at 1 / 10t position from the surface of the plating layer in the thickness direction (t is the total thickness of the plating layer) [Zn] s : Zn content by weight on the surface of the plating layer [Al] 1 / 10t: The weight percent content of Al at 1 / 10t position (t is the total thickness of the plating layer) from the surface of the plating layer in the thickness direction [Al] s : Weight percent of Al on the surface of the plating layer [Mg] 1 / 10t : Magnesium content by weight at 1 / 10t position from the surface of the plating layer in the thickness direction (t is the total thickness of the plating layer) [Mg] s : weight percent of Mg on the surface of the plating layer
[0081] Furthermore, the Mg content by weight at the 2 / 3t position from the surface of the plating layer in the thickness direction was measured in the same manner as described above in the specification. Similarly, the average Mg content by weight in the plating layer was also measured in the same manner as described above in the specification.
[0082] In addition, the surface of the plating layer was photographed by SEM, and then the area ratio of the Al single phase with a Zn solid solution rate of 27 atomic % or more was measured. The values are shown in Table 4 below.
[0083] [Table 4] S Al *: Area ratio [%] of the aluminum single phase with Zn solid solution rate of 27 atomic % or more on the surface of the coating layer
[0084] The characteristics of each of the examples and comparative examples were evaluated according to the following criteria, and the evaluation results of the characteristics are shown in Table 5 below.
[0085] <Corrosion resistance> In order to evaluate the corrosion resistance, a salt spray tester was used in accordance with a test method in accordance with ISO14993, and the evaluation was performed according to the following criteria. ◎: The time it takes for red rust to appear is 40 times longer than that for Zn plating of the same thickness. ○: The time it takes for red rust to appear is 30 to 40 times longer than that of Zn plating of the same thickness. △: The time it takes for red rust to appear is 20 to 30 times longer than that of Zn plating of the same thickness. ×: The time it takes for red rust to appear is less than 20 times longer than that for Zn plating of the same thickness.
[0086] <Chemical conversion treatment> To evaluate the chemical conversion treatability, the steel sheets were subjected to the steps of degreasing, water washing, surface preparation, and phosphating in the order of magnitude, and the free acidity in the phosphate solution was 0.7-0.9, the total acidity was 19-21, and the accelerator was 4-4.5. In addition, using a scanning electron microscope (SEM), three random points on the steel sheet surface were observed at a magnification of 1,000 times, and 20 phosphate particles were selected in order of the largest size in the longitudinal direction within one observation field, and the average was calculated, and the average value of the three points was calculated again, and the result was used to evaluate the results as follows: ○: Length of phosphate particle in the long direction < 5 μm △: Length of phosphate particles in the long direction: 5 to 8 μm ×: Length of phosphate particle in the long direction >8 μm
[0087] <Weldability> To evaluate weldability, the amount of spatter generation, which affects welding workability, and the porosity, which affects the tensile strength of the weld, were evaluated. The above weldability evaluation was performed by gas metal arc (GMA) welding under the following conditions: gas CO2, welding material KC-28 solid wire, current 150A, voltage 20V, and welding speed 0.6m / min. The amount of spatter generation was measured by taking photographs five times every 5 seconds immediately after the start of welding and comparing the relative amounts generated, and the weld porosity was measured by measuring the distribution rate (%) of pore defects in the weld line after radioactive non-destructive testing of the weld. ○: Less than 5 times the amount of sputtering compared to the same thickness of Zn plating, porosity less than 15% △: Spatter amount is 5 times or more but less than 15 times that of Zn plating of the same thickness, and porosity is 15% or more but less than 30%. ×: The amount of sputtering is 15 times or more compared to the same thickness of Zn plating, and the porosity is 30% or more.
[0088] In addition, the steel sheets obtained from each of the Examples and Comparative Examples were evaluated for corrosion resistance, chemical conversion treatability, and weldability, and the evaluation results are shown in Table 5 below.
[0089] [Table 5]
[0090] As can be seen from Table 5 above, in the case of Examples 1 to 9, which satisfy all of the plating compositions and manufacturing conditions of the present invention, it was confirmed that, by satisfying Relational Expressions 1 and 2 defined in the present invention, one or more of the properties of corrosion resistance, chemical conversion treatability, and weldability of the plated steel sheet are all superior to those of the comparative examples.
[0091] In particular, in the case of Examples 7 to 9 above, the Mg content by weight from the surface of the plating layer to the 2 / 3t position in the thickness direction was within ±0.5 wt% of the average Mg content by weight in the plating layer, thereby providing even better corrosion resistance than Examples 1 to 6.
[0092] On the other hand, in the case of Comparative Examples 1 to 4 which do not satisfy the plating composition of the present invention, it was confirmed that one or more of the above-mentioned properties of corrosion resistance, chemical conversion treatability and weldability deteriorated.
[0093] Specifically, in Comparative Examples 1 and 3, since the Mg content of the plating layer was not achieved, not only was the corrosion resistance most degraded, but also the [Al] defined by Relation 2 was not achieved. 1 / 10t -[Al] s It was confirmed that the values of 1.0 and 1.2 were not satisfied, and the chemical conversion treatability and weldability were deteriorated.
[0094] In addition, in Comparative Examples 2 and 4, although the Mg content of the plating layer was sufficient and corrosion resistance was ensured, the Relational Formulas 1 and 2 were not satisfied and the Al content in the surface of the plating layer was excessive, so that the chemical conversion treatability and weldability were significantly deteriorated.
[0095] In addition, in the case of Comparative Examples 5 to 8, which satisfy the plating composition specified in the present invention but do not satisfy the manufacturing conditions, although corrosion resistance can be ensured by satisfying the plating composition, chemical conversion treatability and weldability were deteriorated because Relational Formulas 1 and 2 were not satisfied.
Claims
1. Base steel sheet; and a Zn-Mg-Al-based plating layer provided on at least one surface of the base steel sheet; The plated steel sheet, wherein the plating layer satisfies the following Relational Expressions 1 and 2. [Relationship 1] -10.0≦[Zn] 1/10t -[Zn] s ≦-5.0 (In the above-mentioned relational formula 1, the [Zn] 1/10t represents the weight percent content of Zn at a 1 / 10t position (t is the total thickness of the plating layer) from the surface of the plating layer in the thickness direction, and the [Zn] s represents the weight percent Zn content on the surface of the plating layer.) [Relationship 2] <h2 style=";text-align:left;direction:ltr">+3.0≦[Al]<h2 style=";text-align:left;direction:ltr"> 1/10t <h2 style=";text-align:left;direction:ltr"> -[Al]<h2 style=";text-align:left;direction:ltr"> s <h2 style=";text-align:left;direction:ltr"> ≦+13.0 (In the above-mentioned Relational Formula 2, the above-mentioned [Al] 1/10t represents the weight percent content of Al at a 1 / 10t position (t is the total thickness of the plating layer) from the surface of the plating layer in the thickness direction, and the [Al] s represents the weight percent content of Al on the surface of the plating layer.)
2. The plated steel sheet according to claim 1, further comprising: an Fe-Al-based inhibiting layer provided between the base steel sheet and the Zn-Mg-Al-based plating layer.
3. The plated steel sheet according to claim 1, wherein the plating layer contains, by weight percent, 4.0 to 7.0% Mg, 8.2 to 19.5% Al, and the balance being Zn and other inevitable impurities.
4. The plated steel sheet according to claim 1 , further satisfying the following relational expression 3: [Relationship 3] -1.0≦[Mg] 1/10t -[Mg] s ≦+1.0 (In the above-mentioned Relational Formula 3, the above-mentioned [Mg] 1/10t represents the weight percent content of Mg at a position 1 / 10t from the surface of the plating layer in the thickness direction (t is the total thickness of the plating layer), and the [Mg] s represents the weight percent Mg content on the surface of the plating layer.)
5. 2. The plated steel sheet according to claim 1, wherein the Mg content by weight at a 2 / 3t position from the surface of the plating layer in the thickness direction satisfies ±0.5 wt% of the average Mg content by weight in the plating layer.
6. 2. The plated steel sheet according to claim 1, wherein an area ratio of an Al phase having a Zn solid solution rate of 27 atomic % or more on a surface of the plated layer is 2.0 to 10.1%.
7. performing a first shot blasting process by projecting metal balls having a grain size of 0.6 to 1.0 mm at 400 to 1200 kg / min onto the surface of the base steel sheet in a shot blasting cabin where metal material circulates at a rotation speed of 1200 to 2000 mpm; performing a secondary shot blasting process by projecting metal balls having a grain size of 0.2 to 0.5 mm at 400 to 1200 kg / min onto the surface of the base steel sheet in the shot blasting cabin where the metal material circulates at a rotation speed of 1200 to 2000 mpm; dipping the shot blasted steel sheet in a galvanizing bath containing, by weight, 4.0-7.0% Mg, 8.2-19.5% Al, the balance Zn and other inevitable impurities, and maintained at a temperature of Ts+20°C to Ts+80°C relative to the solidification start temperature (Ts) on the equilibrium diagram, to perform hot-dip galvanizing; and cooling the hot-dip galvanized steel sheet from a solidification start temperature to a solidification finish temperature at an average cooling rate of 2 to 8°C / s using an inert gas.
8. 8. The method for producing a plated steel sheet according to claim 7, further comprising the step of performing pre-temper rolling of the shot blasted base steel sheet by applying a roll reduction of 100 to 400 tons to a steel sheet surface using a dull roll having a surface roughness Ra of 1.8 to 2.8 μm, prior to the hot-dip galvanization.
Citation Information
Patent Citations
Production of cr-containing steel sheet excellent in adhesion of electroplating
JP1992362193A
Manufacture of cold rolled steel sheet with high glossness and excellent image clarity
JP1993154505A
Feed screw and its manufacture
JP1999201257A
Plated steel material with excellent abrasion resistance and white rust resistance and its manufacturing method
JP2019501296A
Hot dip zn-al-mg alloy plated steel sheet having excellent corrosion resistance and method for manufacturing the same
KR1020150073315A