Super-hydrophobic phosphate chemical conversion film, chemical conversion film treating agent and preparation method

Through the cross-linking effect of phytic acid and chitosan and low surface energy modification, a phosphate chemical conversion film with superhydrophobic properties was prepared, which solved the problem of poor protection effect of traditional film layers in humid environments and improved the magnesium alloy Corrosion resistance and durability, and achieve green and environmentally friendly industrial applications.

CN118996402APending Publication Date: 2024-11-22SHANGHAI SPACE PRECISION MACHINERY RES INST
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411032599.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional phosphate chemical conversion films have poor protection effects in humid or halogen ions, and due to defects and cracks during film formation, their corrosion resistance and durability are insufficient, making it difficult to effectively apply on magnesium alloys.

Method used

The cross-linking effect of phytic acid and chitosan and combined with bionic superhydrophobic technology, a superhydrophobic phosphate conversion film is prepared on the surface of magnesium alloy, and the physical barrier performance of the film layer is improved through low-surface energy modifiers to avoid membranes caused by hydrogen evolution. Layer defects.

Benefits of technology

It significantly improves the density, corrosion resistance and durability of the film layer, provides better physical barrier performance, and uses raw materials that are safe, environmentally friendly and low-cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996402A_ABST
    Figure CN118996402A_ABST
Patent Text Reader

Abstract

The invention provides a super-hydrophobic phosphate chemical conversion coating, a chemical conversion coating treating agent and a preparation method, and the preparation method comprises pretreatment, chemical conversion treatment and low surface energy modification. The super-hydrophobic phosphate conversion film with good corrosion resistance is prepared on the surface of the magnesium alloy by utilizing the cross-linking effect of phytic acid (PA) and chitosan (CS) and combining a bionic super-hydrophobic technology. Compared with a traditional phosphate chemical conversion film, the conversion film provided by the invention is more compact, and meanwhile, due to the super-hydrophobic performance, the corrosion resistance and durability are greatly improved; in addition, the used raw materials are safe, easy to obtain, green and environmentally friendly, and have potential application value in industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface coatings, and in particular relates to a super-hydrophobic phosphate chemical conversion film, a chemical conversion film treating agent and a preparation method. Background Art

[0002] Magnesium alloy has low density and high specific strength. It is an ideal material for the lightweight development of equipment manufacturing industry. It has broad application prospects in aviation, aerospace, high-speed rail and automobile industries. However, the poor corrosion resistance of magnesium and magnesium alloys seriously restricts its application in major equipment. If the corrosion problem is not solved, the lightweight advantage of magnesium alloy cannot be brought into play. Therefore, strengthening the corrosion protection of magnesium alloy and adopting reliable surface protection technology are the key to breaking through the bottleneck of magnesium alloy application. The chemical conversion process is simple, efficient and low-cost, and is favored by industrial production. In the chemical conversion process, chromate chemical conversion technology is mature, but Cr (VI) in the conversion liquid is toxic and pollutes the environment. Therefore, the chemical conversion of magnesium alloy is currently developing towards chromium-free. In recent years, phosphate chemical conversion film (PCC) has received more and more attention due to its green and environmentally friendly advantages, and has been widely used in the surface protection of magnesium alloys. The PCC film layer can transform the metal surface from an activated state to a passivated state, inhibit the formation of corrosion micro-batteries, and thus play a certain protective role. However, when the PCC film is in a humid environment or an environment containing halogen ions, its protective effect is often unsatisfactory. In addition, due to the combined influence of material properties and process characteristics, PCC films often have a large number of defects and cracks, which greatly reduces their corrosion protection and durability. Therefore, it is urgent to improve the corrosion protection performance of PCC films.

[0003] At present, the research ideas for improving the protective performance of PCC film are mainly to prepare a relatively dense and uniform film layer by optimizing the conversion liquid composition and conversion process. Although the quality of PCC film and its corrosion resistance can be improved to a certain extent by optimizing the PCC preparation process, the improvement effect is very limited. This is because the formation of defects in the film formation process of PCC is inevitable: (1) Hydrogen evolution is difficult to avoid during the film formation process. The formation of chemical conversion film must rely on the magnesium alloy matrix reaction to lose electrons to produce hydrogen, which increases the pH of the interface and induces deposition. Hydrogen evolution is difficult to avoid during the film formation process, and hydrogen evolution will inevitably cause the formation of film defects. (2) The electrochemical properties of the magnesium alloy surface are uneven. The chemical elements and microstructures in the magnesium alloy are unevenly distributed, which makes the electrochemical activity of the matrix surface uneven. The precipitated phase in the magnesium alloy can form a micro-galvanic pair with the a phase, and the formation of the conversion film mainly depends on the electrochemical dissolution of the magnesium alloy. During the film formation process, the cathode phase is the preferred nucleation site, and a film layer full of cracks will be deposited. This type of film has poor corrosion resistance. Different phases have different film formation rates, so the film layer will crack at the phase interface due to the large growth stress. The cracks provide a path for the penetration of corrosive media and become weak sites prone to corrosion. Water is an important factor that causes corrosion of magnesium alloys, so hydrophobic treatment is an effective measure to enhance its corrosion resistance. In recent years, super-hydrophobic surfaces inspired by lotus leaves have shown great competitiveness and application potential in the field of metal corrosion protection due to their excellent hydrophobic properties. However, the preparation of super-hydrophobic surfaces often requires fluorosilanes for low surface energy modification, but fluorosilanes are costly and environmentally unfriendly, so fluorine-free and low-surface energy coatings with good universality are still in urgent need of development. Summary of the invention

[0004] In order to overcome the deficiencies in the prior art, the inventors have conducted intensive research and provided a super-hydrophobic phosphate chemical conversion film and a preparation method thereof, and prepared a super-hydrophobic phosphate conversion film with good corrosion resistance on the surface of a magnesium alloy by cross-linking phytic acid (PA) and chitosan (CS) and combining bionic super-hydrophobic technology. Compared with the traditional phosphate chemical conversion film, the conversion film provided by the present invention is more compact, and at the same time, due to its super-hydrophobic properties, the corrosion resistance and durability are greatly improved; in addition, the raw materials used are safe and easy to obtain, green and environmentally friendly, and have potential application value in industrial production.

[0005] The technical solution provided by the present invention is as follows:

[0006] In a first aspect, a super-hydrophobic phosphate chemical conversion film comprises a pretreatment agent, a chemical conversion agent and a low surface energy modifier;

[0007] The pretreatment agent includes: 20-50g / L NH4H2PO4, 20-40g / L MnSO4·H2O, 0.5-2g / L NaNO3;

[0008] The chemical conversion agent comprises an A solution and a B solution, wherein the A solution comprises 3-30 g / L phytic acid, 2-20 g / L tetrasodium EDTA and 10-30 g / L Na3PO4·12H2O, and the solvent is water; the B solution is a 0.3 wt% to 0.8 wt% chitosan solution, the pH value is 4 to 6, and the solvent is water;

[0009] The low surface energy modifier is an ethanol / water solution of HDTMS with a volume concentration of 0.5% to 5%.

[0010] In a second aspect, a method for preparing a super-hydrophobic phosphate chemical conversion film comprises:

[0011] The prepared magnesium alloy part is immersed in a pretreatment agent for pretreatment, and after the pretreatment is completed, it is taken out and blown dry; the pretreatment agent comprises: 20-50g / L NH4H2PO4, 20-40g / L MnSO4·H2O, 0.5-2g / L NaNO3;

[0012] The pretreated magnesium alloy parts are first immersed in solution A, and then rinsed with deionized water; then the cleaned magnesium alloy parts are immersed in solution B, and then rinsed with deionized water to prepare a chemical conversion film; wherein solution A includes 3-30g / L phytic acid, 2-20g / L tetrasodium EDTA and 10-30g / L Na3PO4·12H2O, and the solvent is water; solution B is a 0.3wt% to 0.8wt% chitosan solution, and the solvent is water;

[0013] The magnesium alloy part after chemical conversion treatment is immersed in a low surface energy modifier for surface hydrophobicity treatment. After the treatment is completed, it is taken out and dried to obtain a magnesium alloy part with a super-hydrophobic phosphate chemical conversion film.

[0014] In combination with the second aspect, in the step of immersing the prepared magnesium alloy part in a pretreatment agent for pretreatment, the treatment temperature is 50 to 80° C. and the treatment time is 5 to 10 minutes.

[0015] In combination with the second aspect, in the step of preparing the chemical conversion film, the magnesium alloy part is immersed in solution A for 0.5-5 minutes, and in solution B for 2-8 minutes.

[0016] In combination with the second aspect, in the step of preparing the chemical conversion film, the immersion process of the magnesium alloy part in solution A and solution B in sequence is regarded as one cycle, and the entire preparation process includes 1-5 cycles.

[0017] In combination with the second aspect, in the step of immersing the magnesium alloy part after chemical conversion treatment in a low surface energy modifier for surface hydrophobic treatment, the low surface energy modifier is an ethanol / water solution of HDTMS with a volume concentration of 0.5%-5%; the treatment time is 2-10h.

[0018] In combination with the second aspect, in the step of taking out and drying, the drying temperature is 50-80°C.

[0019] In a third aspect, a super-hydrophobic phosphate chemical conversion membrane is prepared by the preparation method of the super-hydrophobic phosphate chemical conversion membrane described in the second aspect, and the thickness of the membrane layer is 5-20 μm.

[0020] A super-hydrophobic phosphate chemical conversion film, a chemical conversion film treating agent and a preparation method provided by the present invention have the following beneficial effects:

[0021] (1) The present invention provides a super-hydrophobic phosphate chemical conversion film and a preparation method thereof. Compared with the traditional phosphate chemical conversion system, the cross-linking effect of phytic acid and chitosan is used to effectively improve the compactness of the conversion film. The formation of the traditional phosphate chemical conversion film depends on the reaction between the magnesium alloy substrate and the conversion liquid to lose electrons and produce hydrogen to increase the interface pH and induce deposition. Hydrogen evolution is difficult to avoid during the film formation process, and hydrogen evolution will inevitably cause the formation of film defects. In contrast, the conversion film prepared by the present invention does not rely on the increase of the interface pH to induce deposition, but prepares the conversion film on the surface of the magnesium alloy through the cross-linking effect between the six negatively charged phosphate groups in the phytic acid molecules and the chitosan molecules, thereby avoiding film defects caused by hydrogen evolution and improving the quality of the film.

[0022] (2) The present invention provides a super-hydrophobic phosphate chemical conversion film and a preparation method thereof, which greatly improves the physical barrier performance of the film layer to corrosive media by modifying the chemical conversion film with low surface energy, and successfully solves the disadvantage of low corrosion resistance of traditional phosphate conversion films;

[0023] (3) The present invention provides a super-hydrophobic phosphate chemical conversion film and a preparation method thereof, wherein the phytic acid and chitosan used are both environmentally friendly natural compounds, green and non-toxic, and the raw materials are easily available, safe and environmentally friendly; in addition, HDTMS is used in the low surface energy modification process instead of traditional fluorosilane, which is environmentally friendly and has lower cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Process flow chart of the super-hydrophobic phosphate chemical conversion membrane of the present invention.

[0025] Figure 2 a is a SEM microscopic morphology of the phosphate chemical conversion film layer prepared in Comparative Example 1, Figure 2b is the SEM microscopic morphology of the phosphate chemical conversion film layer prepared in Example 1.

[0026] Figure 3 This is the electrochemical impedance spectrum of the super-hydrophobic phosphate chemical conversion film layer prepared in Example 1.

[0027] Figure 4 This is the electrochemical impedance spectrum of the phosphate chemical conversion film layer prepared in Comparative Example 2.

[0028] Figure 5 This is a contact angle image of the super-hydrophobic phosphate chemical conversion film layer prepared in Example 1. DETAILED DESCRIPTION

[0029] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.

[0030] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.

[0031] The present invention provides a method for preparing a super-hydrophobic phosphate chemical conversion film, such as Figure 1 As shown, the following steps are included:

[0032] (1) Pretreatment: Immerse the prepared magnesium alloy sample in a pretreatment agent at a treatment temperature of 50-80°C, such as 50°C, for a treatment time of 5-10 min, such as 5 min, and take it out and blow dry after the pretreatment. The components of the pretreatment solution include: 20-50g / L NH4H2PO4, 20-40g / L MnSO4·H2O, and 0.5-2g / L NaNO3.

[0033] Before the magnesium alloy sample undergoes chemical conversion, pretreatment of the surface of the magnesium alloy sample can effectively reduce the defects of the subsequent conversion film and improve the quality of the film layer. This is because: on the one hand, the oxide film produced on the surface of the magnesium alloy sample in the pretreatment process can protect the substrate to a certain extent from unwanted corrosion caused by the subsequent coating process; on the other hand, the film generated by the pretreatment can slow down hydrogen evolution as a substrate layer, weaken the adverse effect of hydrogen escape on the coating quality, and avoid the direct influence of the micro-galvanic couples in the magnesium alloy substrate on the subsequent film formation, thereby making the subsequent coating have fewer defects.

[0034] (2) Chemical conversion treatment: The pretreated magnesium alloy sample is first immersed in solution A for 0.5-5 min, and then rinsed with deionized water; then the cleaned sample is immersed in solution B for 2-8 min, and then rinsed with deionized water. The entire immersion process of solution A and solution B is one cycle. The entire preparation process includes 1-5 cycles, and is carried out at room temperature.

[0035] Wherein, solution A includes 3-30 g / L phytic acid (PA), 2-20 g / L tetrasodium EDTA and 10-30 g / L Na3PO4·12H2O, and the solvent is water; solution B is 0.3% to 0.8% such as 0.5% (mass ratio) chitosan (CS) solution, acetic acid is used to adjust the pH to 4 to 6, and the solvent is water.

[0036] Compared with the traditional phosphate chemical conversion system, the cross-linking effect of phytic acid and chitosan can effectively improve the compactness of the conversion film. The formation of the traditional phosphate chemical conversion film depends on the reaction between the magnesium alloy substrate and the conversion liquid to lose electrons and produce hydrogen to increase the interface pH and induce deposition. Hydrogen evolution is difficult to avoid during the film formation process, and hydrogen evolution will inevitably cause the formation of film defects. In contrast, the conversion film prepared by the present invention does not rely on the increase of the interface pH to induce deposition, but prepares the conversion film on the surface of the magnesium alloy through the cross-linking effect between the six negatively charged phosphate groups in the phytic acid molecules and the chitosan molecules, thereby avoiding film defects caused by hydrogen evolution and improving the quality of the film.

[0037] The film layer formed on the surface of magnesium alloy by the cross-linking of phytic acid and chitosan serves as the main structure of the conversion film, avoiding film defects caused by violent hydrogen evolution and improving the density of the film layer. It can not only separate the substrate from the corrosive medium and delay the penetration of the corrosive medium, but also has an uneven microstructure, which provides a certain roughness for the construction of super-hydrophobicity, thus creating favorable conditions for achieving super-hydrophobicity. After the subsequent low surface energy modification, the contact angle of the film layer increased significantly, showing super-hydrophobicity, further improving the physical barrier performance of the film layer.

[0038] (3) Low surface energy modification: The sample after chemical conversion treatment is immersed in an ethanol / water solution of hexadecyltrimethoxysilane (HDTMS) for modification for 2-10 hours, and then taken out and dried at 50-80° C., such as 60° C. Wherein, the concentration of HDTMS in the ethanol / water solution of HDTMS is 0.5%-5% (volume concentration), and the ratio of ethanol to water is (10:1) to (5:1), such as 5:1 (volume ratio).

[0039] Test the performance of super hydrophobic phosphate chemical conversion film:

[0040] (1) Coating thickness

[0041] Test method: Use a film thickness gauge to measure the thickness of the coating.

[0042] Test results: The thickness of the film layer is 5-20μm.

[0043] (2) Surface morphology

[0044] Test method: Use scanning electron microscope to observe the microscopic morphology of the coating surface.

[0045] Test results: The results show that compared with the phosphate chemical conversion film prepared by traditional methods, this film has fewer micropores and microcracks on the surface and better density.

[0046] (3) Corrosion resistance

[0047] Test method: Electrochemical impedance spectroscopy (EIS) and salt spray test were performed using an electrochemical workstation and a salt spray test chamber, respectively. The corrosion resistance of the coating was examined by electrochemical impedance spectroscopy (EIS) and salt spray test.

[0048] Test results: The electrochemical impedance spectroscopy results show that the low-frequency impedance modulus of the coating is higher than 10 4 Ω·cm 2 , showing excellent corrosion resistance. The salt spray test results show that the coating can resist neutral salt spray for more than 96 hours.

[0049] (4) Wetting performance

[0050] Test method: Use a contact angle meter to test the contact angle of the film layer.

[0051] Test results: The contact angle test results show that the contact angle of the film layer is greater than 150°, showing super hydrophobicity.

[0052] Example

[0053] Example 1

[0054] This embodiment relates to a super-hydrophobic phosphate chemical conversion film layer, and its preparation method and performance are as follows:

[0055] (1) Pretreatment

[0056] Raw material components: NH4H2PO4, MnSO4·H2O and NaNO3.

[0057] Preparation process: immerse the prepared magnesium alloy sample in the pretreatment solution, the treatment temperature is 50℃, the treatment time is 5min; take it out and blow dry after the treatment. The composition of the pretreatment agent is: 35g / L NH4H2PO4, 30g / L MnSO4·H2O, 1.5g / L NaNO3.

[0058] (2) Chemical conversion treatment

[0059] Raw material components: phytic acid (PA), tetrasodium EDTA, Na3PO4·12H2O and chitosan.

[0060] Preparation process: The pretreated magnesium alloy sample is first immersed in solution A for 0.5 min, and then rinsed with deionized water; then the cleaned sample is immersed in solution B for 3 min, and then rinsed with deionized water. After 3 cycles of the above steps, blow dry with cold air for standby use. The whole process is carried out at room temperature. Among them, solution A includes 10g / L phytic acid (PA), 5g / tetrasodium LEDTA and 20g / L Na3PO4·12H2O, and the solvent is water; solution B is 0.5% (mass ratio) chitosan solution, and the solvent is water.

[0061] (3) Low surface energy modification

[0062] Raw material components: hexadecyltrimethoxysilane (HDTMS).

[0063] Preparation process: The sample after chemical conversion treatment is immersed in an ethanol / water solution of hexadecyltrimethoxysilane (HDTMS) for modification for 6 hours, and then taken out and dried at 60°C. The concentration of HDTMS in the ethanol / water solution of HDTMS is 2% (volume concentration), and the ratio of ethanol to water is 5:1 (volume ratio).

[0064] (4) Coating performance test

[0065] The coating thickness is 10±3μm, and the conversion film has an uneven convex structure. Figure 2 b; Compared with the traditional phosphate chemical conversion film, the film has fewer defects; the electrochemical test results show that the low-frequency impedance modulus of the coating is as high as 5.17×10 4 Ω·cm 2 ,See Figure 3 , which is an order of magnitude higher than the traditional phosphate chemical conversion film; the neutral salt spray test results show that the film layer is resistant to neutral salt spray for more than 96 hours; the contact angle test results show that the contact angle of the film layer is 156.5°, such as Figure 5 , showing super hydrophobicity.

[0066] Example 2

[0067] This embodiment relates to a super-hydrophobic phosphate chemical conversion film layer, and its preparation method and performance are as follows:

[0068] (1) Pretreatment

[0069] Raw material components: NH4H2PO4, MnSO4·H2O and NaNO3.

[0070] Preparation process: immerse the prepared magnesium alloy sample in the pretreatment agent, the treatment temperature is 50℃, the treatment time is 5min; take it out and blow dry after the treatment. The composition of the pretreatment solution is: 40g / L NH4H2PO4, 20g / L MnSO4·H2O, 0.5g / L NaNO3.

[0071] (2) Chemical conversion treatment

[0072] Raw material components: phytic acid (PA), tetrasodium EDTA, Na3PO4·12H2O and chitosan.

[0073] Preparation process: The pretreated magnesium alloy sample is first immersed in solution A for 0.5 min, and then rinsed with deionized water; then the cleaned sample is immersed in solution B for 3 min, and then rinsed with deionized water. After 5 cycles of the above steps, blow dry with cold air for standby use. The whole process is carried out at room temperature. Among them, solution A includes 3g / L phytic acid (PA), 2g / tetrasodium LEDTA and 10g / L Na3PO4·12H2O, and the solvent is water; solution B is 0.5% (mass ratio) chitosan solution, and the solvent is water.

[0074] (3) Low surface energy modification

[0075] Raw material components: hexadecyltrimethoxysilane (HDTMS).

[0076] Preparation process: The sample after chemical conversion treatment is immersed in an ethanol / water solution of hexadecyltrimethoxysilane (HDTMS) for modification for 10 hours, and then taken out and dried at 60°C. The concentration of HDTMS in the ethanol / water solution of HDTMS is 5% (volume concentration), and the ratio of ethanol to water is 5:1 (volume ratio).

[0077] (4) Coating performance test

[0078] The coating thickness is 15±5μm, and the conversion film has an uneven convex structure. Compared with the traditional phosphate chemical conversion film, the film has fewer defects. The electrochemical test results show that the low-frequency impedance modulus of the coating is as high as 6.48×10 4 Ω·cm 2 , which is one order of magnitude higher than the traditional phosphate chemical conversion film; the neutral salt spray test results show that the film layer is resistant to neutral salt spray for more than 100 hours; the contact angle test results show that the contact angle of the film layer is 153.4°, which is super hydrophobic.

[0079] Example 3

[0080] This embodiment relates to a super-hydrophobic phosphate chemical conversion film layer, and its preparation method and performance are as follows:

[0081] (1) Pretreatment

[0082] Raw material components: NH4H2PO4, MnSO4·H2O and NaNO3.

[0083] Preparation process: immerse the prepared magnesium alloy sample in the pretreatment agent, the treatment temperature is 50℃, the treatment time is 5min; take it out and blow dry after the treatment. The composition of the pretreatment solution is: 40g / L NH4H2PO4, 20g / L MnSO4·H2O, 0.5g / L NaNO3.

[0084] (2) Chemical conversion treatment

[0085] Raw material components: phytic acid (PA), tetrasodium EDTA, Na3PO4·12H2O and chitosan.

[0086] Preparation process: The pretreated magnesium alloy sample is first immersed in solution A for 0.5 min, and then rinsed with deionized water; then the cleaned sample is immersed in solution B for 3 min, and then rinsed with deionized water. After 2 cycles of the above steps, blow dry with cold air for standby use. The whole process is carried out at room temperature. Among them, solution A includes 20g / L phytic acid (PA), 10g / LEDTA tetrasodium and 20g / L Na3PO4·12H2O, and the solvent is water; solution B is 0.5% (mass ratio) chitosan solution, and the solvent is water.

[0087] (3) Low surface energy modification

[0088] Raw material components: hexadecyltrimethoxysilane (HDTMS).

[0089] Preparation process: The sample after chemical conversion treatment is immersed in an ethanol / water solution of hexadecyltrimethoxysilane (HDTMS) for modification for 3 hours, and then taken out and dried at 60°C. The concentration of HDTMS in the ethanol / water solution of HDTMS is 2% (volume concentration), and the ratio of ethanol to water is 5:1 (volume ratio).

[0090] (4) Coating performance test

[0091] The coating thickness is 8±3μm, and the conversion film has an uneven convex structure. Compared with the traditional phosphate chemical conversion film, the film has fewer defects. The electrochemical test results show that the low-frequency impedance modulus of the coating is as high as 2.08×10 4 Ω·cm 2, which is one order of magnitude higher than the traditional phosphate chemical conversion film; the neutral salt spray test results show that the film layer is resistant to neutral salt spray for more than 96 hours; the contact angle test results show that the contact angle of the film layer is 155°, which is super hydrophobic.

[0092] Comparative Example

[0093] Comparative Example 1

[0094] This comparative example relates to a phosphate chemical conversion film layer, and its preparation method is the same as that of Example 1, except that no pretreatment is performed. The thickness of the chemical conversion film prepared in this comparative example is 10±3μm; there are many defects and cracks on the surface, as shown in FIG. Figure 2 a; The low-frequency impedance modulus of the coating is 1.14×10 4 Ω·cm 2 , resistant to neutral salt spray for 72h; contact angle 150.4°, super hydrophobic.

[0095] Comparative Example 2

[0096] This comparative example relates to a phosphate chemical conversion film layer, and its preparation method is the same as that of Example 1, except that no low surface energy modification treatment is performed. The thickness of the chemical conversion film prepared in this comparative example is 10±3μm; the low frequency impedance modulus of the coating is 7.48×10 3 Ω·cm 2 ,See Figure 4 , resistant to neutral salt spray for 24 hours; contact angle is less than 10°, and is hydrophilic.

[0097] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0098] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.

Claims

1. A super-hydrophobic phosphate chemical conversion film treating agent, characterized in that: Includes pretreatment agents, chemical conversion agents and low surface energy modifiers; The pretreatment agent includes: 20-50g / L NH4H2PO4, 20-40g / L MnSO4·H2O, 0.5-2g / L NaNO3; The chemical conversion agent comprises an A solution and a B solution, wherein the A solution comprises 3-30 g / L phytic acid, 2-20 g / L tetrasodium EDTA and 10-30 g / L Na3PO4·12H2O, and the solvent is water; the B solution is a 0.3 wt% to 0.8 wt% chitosan solution, the pH value is 4 to 6, and the solvent is water; The low surface energy modifier is an ethanol / water solution of hexadecyltrimethoxysilane HDTMS with a volume concentration of 0.5% to 5%.

2. A method for preparing a super-hydrophobic phosphate chemical conversion film, characterized in that: include: Immerse the prepared magnesium alloy part in a pretreatment agent for pretreatment, and take it out and blow dry it after the pretreatment is completed; The pretreatment agent includes: 20-50g / L NH4H2PO4, 20-40g / L MnSO4·H2O, 0.5-2g / L NaNO3; The pretreated magnesium alloy parts are first immersed in solution A, and then rinsed with deionized water; then the cleaned magnesium alloy parts are immersed in solution B, and then rinsed with deionized water to prepare a chemical conversion film; wherein solution A includes 3-30g / L phytic acid, 2-20g / L tetrasodium EDTA and 10-30g / L Na3PO4·12H2O, and the solvent is water; solution B is a 0.3wt% to 0.8wt% chitosan solution, and the solvent is water; The magnesium alloy part after chemical conversion treatment is immersed in a low surface energy modifier for surface hydrophobicity treatment. After the treatment is completed, it is taken out and dried to obtain a magnesium alloy part with a super-hydrophobic phosphate chemical conversion film.

3. The method for preparing a super-hydrophobic phosphate chemical conversion film according to claim 2, characterized in that: In the step of immersing the prepared magnesium alloy part into a pretreatment agent for pretreatment, the treatment temperature is 50 to 80° C. and the treatment time is 5 to 10 minutes.

4. The method for preparing a super-hydrophobic phosphate chemical conversion film according to claim 2, characterized in that: In the step of preparing the chemical conversion film, the magnesium alloy part is immersed in solution A for 0.5-5 minutes, and in solution B for 2-8 minutes.

5. The method for preparing a super-hydrophobic phosphate chemical conversion film according to claim 2, characterized in that: In the step of preparing the chemical conversion film, the immersion process of the magnesium alloy part in solution A and solution B in sequence is regarded as one cycle, and the whole preparation process includes 1-5 cycles.

6. The method for preparing a super-hydrophobic phosphate chemical conversion film according to claim 2, characterized in that: In the step of immersing the magnesium alloy piece after chemical conversion treatment in a low surface energy modifier for surface hydrophobicity treatment, the low surface energy modifier is an ethanol / water solution of HDTMS with a volume concentration of 0.5%-5%.

7. The method for preparing a super-hydrophobic phosphate chemical conversion film according to claim 2, characterized in that: In the step of immersing the magnesium alloy part after chemical conversion treatment in a low surface energy modifier for surface hydrophobicity treatment, the treatment time is 2-10 hours.

8. The method for preparing a super-hydrophobic phosphate chemical conversion film according to claim 2, characterized in that: In the step of taking out and drying, the drying temperature is 50-80°C.

9. A super-hydrophobic phosphate chemical conversion film, characterized in that: The super-hydrophobic phosphate chemical conversion film is prepared by the preparation method of any one of claims 2 to 9.

10. The super-hydrophobic phosphate chemical conversion film according to claim 9, characterized in that: The thickness of the film layer is 5-20 μm.

Citation Information

Cited By

  • High-performance nickel alloy composite nano coating for rail transit cable bridge

    CN121759860A