Method for in-situ synthesis of graphene Y2O3 / ZrO2 / MgO composite ceramic membrane on surface of magnesium alloy building template

Through microarc oxidation technology, graphene Y2O3/ZrO2/MgO composite ceramic film is prepared on the surface of magnesium alloy building formwork, which solves the problems of low hardness, poor wear resistance and insufficient corrosion resistance of magnesium alloy building formwork, and achieves efficient hardness improvement and The corrosion resistance is enhanced, and the process is simple and the cost is low.

CN119040989APending Publication Date: 2024-11-29CHANGAN UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411031864.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

During the use of magnesium alloy building formwork, there are problems such as low hardness, poor wear resistance and insufficient corrosion resistance, which leads to scratching, corrosion and staining on the surface. The existing coating process has high cost and slow film formation speed. Complex process and other problems.

Method used

The graphene Y2O3/ZrO2/MgO composite ceramic membrane is prepared on the surface of magnesium alloy building formwork by microarc oxidation technology. By preparing appropriate electrolyte and setting appropriate electrical parameters, the in-situ growth of the ceramic membrane is achieved, and the hardness and corrosion resistance are improved. , and the micropores of the ceramic membrane are sealed through graphene to enhance the anti-fouling performance.

Benefits of technology

It significantly improves the hardness, wear resistance and corrosion resistance of magnesium alloy building formwork, reduces surface roughness and cost, extends service life, and improves pollution resistance, solving the surface easy scratch, corrosion and pollution easily The problem.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040989A_ABST
    Figure CN119040989A_ABST
Patent Text Reader

Abstract

The invention discloses a method for in-situ synthesis of a graphene Y2O3 / ZrO2 / MgO composite ceramic membrane on the surface of a magnesium alloy building template, and the method comprises the following steps: S1, cleaning the surface of the magnesium alloy building template by using an alkaline oil removal liquid, and drying to obtain the magnesium alloy building template with a smooth surface; s2, mixing the graphene dispersion liquid and a zirconium salt system electrolyte containing nano Y2O3 particles according to the volume ratio of 1: 2 to obtain a micro-arc oxidation electrolyte; s3, the magnesium alloy building formwork with the smooth surface and the stainless steel plate with the smooth surface are placed in a micro-arc oxidation electrolyte, and micro-arc oxidation treatment is conducted for 20-30 min; s4, hole sealing treatment is carried out on the ceramic film formed on the surface of the magnesium alloy building template after micro-arc oxidation treatment; and the magnesium alloy building template subjected to ceramic membrane hole sealing treatment is cleaned and dried, and the in-situ synthesized graphene modified Y2O3 / ZrO2 / MgO composite ceramic membrane on the surface of the magnesium alloy building template is obtained. The magnesium alloy building template produced by the method has corrosion resistance, wear resistance and pollution resistance, and the prepared ceramic membrane is compact and uniform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface processing and preparation of coatings for magnesium alloy building templates, and specifically relates to a method for in-situ synthesis of a graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of a magnesium alloy building template. Background Art

[0002] Magnesium alloys have low density, high specific strength, good thermal conductivity, strong electromagnetic shielding and radiation resistance, excellent damping and vibration reduction, and cutting performance. They have important application value in transportation, electronics, aerospace, and defense industries. However, due to the low standard electrode potential of magnesium at room temperature, poor corrosion resistance, and low hardness and poor wear resistance of magnesium alloys, their application range is limited.

[0003] In recent years, the construction industry has required a shift towards greening and environmental protection. Lightweight and recyclable building formwork materials have become a future development trend. Wood formwork has relatively weak strength and bearing capacity, is easily affected by moisture, deformed and damaged, has low reuse rate, and damages the environment. Steel formwork is heavy and requires large machinery for installation and disassembly, which is inconvenient to operate and is prone to rust and deformation in high temperature and humid environments. Plastic formwork is sensitive to temperature, prone to deformation, has low hardness, is easy to wear, and has relatively weak strength and bearing capacity. Magnesium alloy building formwork has low cost and light weight, improves workers' work efficiency, reduces the construction process's dependence on large machinery, effectively reduces construction period, and reduces construction costs, and is deeply favored by the construction industry.

[0004] However, although magnesium alloy building formwork has so many excellent properties, there are still some problems in the use process: 1. Magnesium alloy materials are relatively soft, and it is inevitable to scratch the surface during daily construction, causing serious wear; 2. Magnesium alloy materials have poor corrosion resistance, and are prone to serious corrosion in outdoor construction environments, thus affecting the load-bearing capacity and stability of the building formwork, causing safety hazards. There are many ways to improve the surface hardness, wear resistance and corrosion resistance of magnesium alloys, including surface alloying and surface coating treatment. The surface hardness of magnesium alloy can be improved by preparing hard wear-resistant layer by laser cladding, spraying and other methods, but the obtained surface is very rough and has low smoothness, and there is an interface between the coating and the magnesium alloy substrate, which is easy to cause defects such as peeling and cracking; by using PVD and CVD methods to deposit coatings of TiC, TiN, TiN / AlN and other components on the surface of magnesium alloy, high hardness, high wear resistance and other properties can be obtained, but the CVD process is mostly above 800°C, and the high temperature process affects the mechanical properties and dimensional accuracy of magnesium alloy parts. The hard wear-resistant layer prepared on the surface of magnesium alloy by PVD method is relatively mature, but there are problems such as slow film formation speed, high cost, and difficulty in handling deep holes and fine cracks in parts.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] In order to solve the problems in the prior art, the present invention adopts micro-arc oxidation technology, prepares appropriate electrolytes, and sets appropriate electrical parameters to prepare hard ceramic films on the surface of magnesium alloy building templates. The prepared ceramic film layer grows in situ on the surface of the original metal substrate, and the film-base combination is firm, and has the properties of wear resistance, corrosion resistance, insulation, etc. At the same time, the micro-arc oxidation technology has the advantages of green and environmentally friendly electrolytes, low cost, and simple operation. The micro-arc oxidation ceramic film with high hardness, scratch resistance, wear resistance, corrosion resistance, and anti-fouling prepared on the surface of magnesium alloy building templates has a good application and promotion prospect.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] The present invention provides a method for in-situ synthesis of a graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of a magnesium alloy building template, comprising the following steps:

[0009] S1. Pre-treating the surface of the magnesium alloy building formwork: cleaning the surface of the magnesium alloy building formwork with an alkaline degreasing solution and drying the surface to obtain a magnesium alloy building formwork with a smooth surface;

[0010] S2. Prepare a zirconium salt system micro-arc oxidation electrolyte containing nano Y2O3 particles and graphene: mix the graphene dispersion and the zirconium salt system electrolyte containing nano Y2O3 particles in a volume ratio of 1:2 to obtain a micro-arc oxidation electrolyte, and place the mixture in a PVC micro-arc oxidation tank for standby use;

[0011] S3, micro-arc oxidation treatment: placing the obtained micro-arc oxidation electrolyte in a PVC micro-arc oxidation tank, and placing the magnesium alloy building formwork and stainless steel plate with a smooth surface in the micro-arc oxidation electrolyte, and performing micro-arc oxidation treatment for 20 to 30 minutes;

[0012] S4, ceramic membrane sealing treatment: sealing treatment is performed on the ceramic membrane formed on the surface of the magnesium alloy building formwork after micro-arc oxidation treatment;

[0013] S5. Ceramic membrane polishing treatment: The magnesium alloy building formwork after the ceramic membrane sealing treatment is cleaned and dried to obtain an in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic membrane on the surface of the magnesium alloy building formwork.

[0014] Furthermore, in step S1, the surface of the magnesium alloy building formwork is washed with an alkaline degreasing liquid for 15 to 20 minutes and then washed with deionized water. 10 to 20 g of Na2CO3, 1 to 3 g of OP emulsifier, 10 to 20 g of Na3PO4 and 10 to 20 g of Na2SiO3 are added to every 1 L of deionized water to prepare an alkaline degreasing liquid.

[0015] Further, the zirconium salt system electrolyte containing nano Y2O3 particles in step S2 is prepared by adding 30-45g of (NaPO3)6, 20-25g of Na3PO4, 35-50g of C6H5O7Na3·2H2O, 35-40g of K2ZrF6, 4-6g of PEG-1000, 10-15g of EDTA-Na and 0.5-1g of nano Y2O3 particles with an average particle size of 50nm to 1L of deionized water.

[0016] The graphene dispersion is prepared by adding 20-30 g of sodium dodecyl sulfate and 1 g of graphene to every 1 L of deionized water.

[0017] Furthermore, when preparing the graphene dispersion, 20 to 30 g of sodium dodecyl sulfate and 1 g of graphene are added to 1 L of deionized water, and the mixture is placed in an ultrasonic disperser and dispersed for 3 to 4 hours to fully disperse the graphene.

[0018] Sodium dodecyl sulfate is an anionic surfactant that is adsorbed on both sides of the graphene sheet. Relying on electrostatic repulsion or van der Waals force, the graphene is evenly dispersed in the aqueous solution and presents a negative charge.

[0019] Furthermore, the graphene added to the micro-arc oxidation electrolyte can in-situ seal the micropores on the surface of the micro-arc oxidation ceramic membrane by applying a secondary voltage during the ceramic membrane sealing treatment, thereby preventing the corrosive medium from diffusing and penetrating through the micropores of the micro-arc oxidation ceramic membrane.

[0020] Furthermore, in step S3, the magnesium alloy building template and the stainless steel plate with smooth surface need to be completely immersed in the micro-arc oxidation electrolyte, the stainless steel plate is connected to the negative electrode of the micro-arc oxidation power supply as a cathode, and the magnesium alloy building template is connected to the positive electrode of the micro-arc oxidation power supply as an anode.

[0021] Furthermore, during the micro-arc oxidation treatment in step S3, the micro-arc oxidation power supply adopts a DC pulse power supply, the power supply pulse frequency is 1000-1200 Hz, the duty cycle is 5-15%, the micro-arc oxidation termination voltage is 350-450V, and the temperature of the micro-arc oxidation electrolyte is 15-25°C.

[0022] Furthermore, the specific steps of step S4 of the ceramic membrane sealing treatment are: after the micro-arc oxidation treatment is completed, the power supply voltage of the micro-arc oxidation power supply is directly reduced to 150-200V without turning off the power supply, and the ceramic membrane sealing treatment is performed for 5-8 minutes.

[0023] Furthermore, in step S5, the specific method for cleaning the magnesium alloy building formwork is: after ultrasonic cleaning the magnesium alloy building formwork in deionized water at room temperature for 1 to 2 minutes, place it in deionized water heated to 100° C. and boil it for 10 minutes, take it out and dry it.

[0024] Furthermore, the inlet and outlet pipelines of the micro-arc oxidation electrolyte are connected to a cooling device to form a cooling cycle for the micro-arc oxidation electrolyte and maintain the temperature of the micro-arc oxidation electrolyte at 15-25°C. An agitator is also installed inside the micro-arc oxidation electrolyte to mix the micro-arc oxidation electrolyte evenly by stirring.

[0025] Compared with the prior art, the present invention has the following advantages:

[0026] (1) The present invention uses lightweight magnesium alloy as the building formwork material. Compared with aluminum alloy, the same volume of magnesium alloy can reduce the weight of the building formwork by about 33%, thereby improving work efficiency, reducing the dependence of the construction process on large machinery, shortening the construction period, and reducing construction costs;

[0027] (2) The present invention performs micro-arc oxidation surface treatment on the magnesium alloy building formwork in a zirconium salt system electrolyte to quickly obtain a Y2O3 / ZrO2 / MgO composite ceramic film with thick thickness and high hardness, which significantly improves the wear resistance of the magnesium alloy building formwork, reduces material wear during use, increases the number of recycling times of the formwork, and reduces construction costs;

[0028] (3) The present invention obtains a ceramic film containing ZrO2 on the surface of the magnesium alloy building formwork. Since ZrO2 has phase transformation toughening, residual stress toughening and microcrack toughening effects, the cracking tendency caused by the high hardness and brittleness of the magnesium alloy micro-arc oxidation ceramic film is reduced, and the surface quality of the magnesium alloy micro-arc oxidation ceramic film is improved;

[0029] (4) The present invention obtains a ceramic film containing Y2O3 by adding nano Y2O3 particles to the magnesium alloy micro-arc oxidation electrolyte to participate in the film-forming reaction. The addition of nano Y2O3 particles reduces the number and diameter of micropores on the surface of the ceramic film, improves the density of the ceramic film, and reduces the surface roughness. At the same time, Y2O3 makes the ZrO2 component in the ceramic film have excellent chemical stability and high corrosion resistance, improves the corrosion resistance of the magnesium alloy building formwork, and prolongs the service life of the magnesium alloy building formwork;

[0030] (5) In addition to the high-hardness, high-corrosion-resistant ZrO2 component, the micro-arc oxidation ceramic membrane prepared by the method of the present invention also adds graphene to the micro-arc oxidation electrolyte. By applying a secondary voltage, the micropores on the surface of the micro-arc oxidation ceramic membrane are in-situ sealed, which prevents the corrosive medium from diffusing and penetrating through the micropores of the micro-arc oxidation ceramic membrane, further improving the corrosion resistance of the magnesium alloy building formwork. At the same time, graphene significantly reduces the friction coefficient of the ceramic membrane and improves the wear resistance of the magnesium alloy building formwork. In addition, the graphene present on the surface and in the micropores of the ceramic membrane makes the ceramic membrane have good hydrophobicity, and the magnesium alloy building formwork has excellent anti-fouling properties;

[0031] (6) In the process of the present invention, the micro-arc oxidation treatment and the ceramic membrane sealing treatment for ceramic membrane preparation are carried out in the same tooling and electrolyte. When switching from the micro-arc oxidation treatment to the sealing treatment, the workpiece does not need to be removed from the electrolyte, and only the power supply voltage needs to be adjusted, thereby making the process and operation steps relatively simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic diagram of the structure of the tooling used in the micro-arc oxidation reaction of the present invention;

[0033] Figure 2 The surface morphology photos and cross-sectional morphology diagrams of the ceramic membranes of samples 1 to 3 in the embodiments of the present invention are shown;

[0034] Among them, a is the surface morphology of sample 1, b is the cross-sectional morphology of sample 1, c is the surface morphology of sample 2, d is the cross-sectional morphology of sample 2, e is the surface morphology of sample 3, and f is the cross-sectional morphology of sample 3;

[0035] Figure 3 The XRD diffraction pattern of the ceramic film of sample 1 in the embodiment of the present invention;

[0036] Figure 4 The friction coefficient variation and average friction coefficient diagram of samples 1 to 3 in the embodiment of the present invention;

[0037] Among them, a is the friction coefficient variation diagram of samples 1 to 3, and b is the average friction coefficient diagram of samples 1 to 3;

[0038] Figure 5 The wear morphology of samples 1 to 3 in the embodiment of the present invention;

[0039] Among them, a and b are the wear morphology images of sample 1, b is the local image of a magnified 20 times,

[0040] c and d are the wear morphology images of sample 2, d is a partial image of c magnified 20 times,

[0041] e and f are the wear morphology images of sample 3, and f is a partial image of e magnified 20 times;

[0042] Figure 6 Graphs showing polarization curves of samples 1 and 4 in the embodiments of the present invention;

[0043] Figure 7 The contact angle diagram of deionized water droplets on the surfaces of samples 1 to 4 in the present invention is shown in FIG.

[0044] Among them, a is the surface contact angle diagram of sample 1, b is the surface contact angle diagram of sample 2, c is the surface contact angle diagram of sample 3, and d is the surface contact angle diagram of sample 4;

[0045] Among them, 1-micro-arc oxidation power supply, 2-negative electrode of power supply, 3-positive electrode of power supply, 4-cooling device, 5-electrolyte, 6-PVC micro-arc oxidation tank, 7-stainless steel plate, 8-agitator, 9-magnesium alloy building template. DETAILED DESCRIPTION

[0046] The present invention is further explained below in conjunction with the drawings and specific embodiments of the specification. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0047] According to an embodiment of the present invention, Figure 1 As shown, the method for in-situ synthesis of graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of magnesium alloy building template provided by the present invention is operated by the tooling used in micro-arc oxidation reaction. Specifically, the micro-arc oxidation power supply 1 provides pulse current, the obtained micro-arc oxidation electrolyte 5 is placed in the PVC micro-arc oxidation tank 6, and the magnesium alloy building template 9 and the stainless steel plate with a smooth surface are completely immersed in the micro-arc oxidation electrolyte 5, the stainless steel plate 7 is connected to the negative power supply 2 of the micro-arc oxidation power supply 1 as a cathode, and the magnesium alloy building template 9 is connected to the positive power supply 3 of the micro-arc oxidation power supply 1 as an anode. The inlet and outlet pipelines of the micro-arc oxidation electrolyte 5 are connected to the cooling device 4, so that the micro-arc oxidation electrolyte 5 forms a cooling cycle, and the temperature of the micro-arc oxidation electrolyte 5 is maintained at 15-25°C. A stirrer 8 is also installed inside the micro-arc oxidation electrolyte 5 to mix the micro-arc oxidation electrolyte 5 evenly by stirring.

[0048] The graphene Y2O3 / ZrO2 / MgO composite ceramic film prepared by the method of in-situ synthesis of a graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of a magnesium alloy building template provided by the present invention improves the corrosion resistance, wear resistance and anti-fouling properties of the magnesium alloy building template.

[0049] According to the embodiments of the present invention, the method of the present invention is described in detail through the following specific embodiments.

[0050] Example 1

[0051] Step 1: Pre-treat the surface of magnesium alloy building formwork:

[0052] Add 10g Na2CO3, 1g OP emulsifier, 20g Na3PO4 and 20g Na2SiO3 to every 1L of deionized water to prepare an alkaline degreasing solution. Use the alkaline degreasing solution to wash the surface of the magnesium alloy building formwork for 15 minutes, then wash with deionized water and dry, and the surface of the magnesium alloy building formwork will be smooth.

[0053] Step 2: Prepare a zirconium salt system micro-arc oxidation electrolyte containing nano Y2O3 particles and graphene:

[0054] A zirconium salt system electrolyte containing nano Y2O3 particles was prepared by adding 35 g of (NaPO3)6, 20 g of Na3PO4, 35 g of C6H5O7Na3·2H2O, 35 g of K2ZrF6, 4 g of PEG-1000, 10 g of EDTA-Na and 0.5 g of nano Y2O3 particles with an average particle size of 50 nm to 1 L of deionized water;

[0055] A graphene dispersion was obtained by adding 20 g of sodium dodecyl sulfate and 1 g of graphene to 1 L of deionized water, and dispersing the mixture in an ultrasonic disperser for 3 h to fully disperse the graphene.

[0056] The zirconium salt system electrolyte containing nano Y2O3 particles and the graphene dispersion were mixed in a volume ratio of 2:1 to prepare a micro-arc oxidation electrolyte, which was placed in a reaction tank for standby use.

[0057] Step 3: Micro-arc oxidation treatment:

[0058] The obtained micro-arc oxidation electrolyte is placed in a PVC micro-arc oxidation tank, and the magnesium alloy building template and stainless steel plate with a smooth surface are completely immersed in the micro-arc oxidation electrolyte. The stainless steel plate is connected to the negative electrode of the micro-arc oxidation power supply as a cathode, and the magnesium alloy building template is connected to the positive electrode of the micro-arc oxidation power supply as an anode. When performing micro-arc oxidation treatment, the micro-arc oxidation power supply adopts a DC pulse power supply with a power pulse frequency of 1000 Hz, a duty cycle of 5%, a micro-arc oxidation termination voltage of 350 V, an electrolyte temperature of 25°C, and a micro-arc oxidation treatment of 20 minutes.

[0059] Step 4: Ceramic membrane sealing treatment:

[0060] After the micro-arc oxidation treatment is completed, the power supply voltage is directly reduced to 150V without turning off the power supply, and the treatment is carried out for 6 minutes. Since sodium dodecyl sulfate is an anionic surfactant, it is adsorbed on both sides of the graphene sheet. Relying on the electrostatic repulsion or van der Waals force, the graphene is evenly dispersed in the aqueous solution and presents a negative charge. The graphene added to the micro-arc oxidation electrolyte is in-situ sealed on the micropores on the surface of the micro-arc oxidation ceramic membrane by applying a secondary voltage during the ceramic membrane sealing treatment, which hinders the corrosion medium from diffusing and penetrating through the micropores of the micro-arc oxidation ceramic membrane, so that the graphene in the electrolyte seals the micro-arc oxidation ceramic membrane.

[0061] Step 5: Polishing of ceramic film:

[0062] The magnesium alloy building template after ceramic membrane sealing treatment is cleaned and dried to obtain an in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic membrane on the surface of the magnesium alloy building template;

[0063] The magnesium alloy building formwork was ultrasonically cleaned in deionized water for 1 minute at room temperature, then boiled in deionized water heated to 100°C for 10 minutes, and then taken out and dried.

[0064] The in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic film on the surface of the magnesium alloy building formwork prepared in Example 1 is used as sample 1.

[0065] Example 2

[0066] Step 1: Pre-treat the surface of magnesium alloy building formwork:

[0067] Add 15g Na2CO3, 2g OP emulsifier, 10g Na3PO4 and 10g Na2SiO3 to every 1L of deionized water to prepare an alkaline degreasing solution. Use the alkaline degreasing solution to wash the surface of the magnesium alloy building formwork for 18 minutes, then wash with deionized water and dry, and the surface of the magnesium alloy building formwork will be smooth.

[0068] Step 2: Prepare a zirconium salt system micro-arc oxidation electrolyte containing nano Y2O3 particles and graphene:

[0069] A zirconium salt system electrolyte containing nano Y2O3 particles was prepared by adding 45 g of (NaPO3)6, 25 g of Na3PO4, 50 g of C6H5O7Na3·2H2O, 40 g of K2ZrF6, 6 g of PEG-1000, 15 g of EDTA-Na and 1 g of nano Y2O3 particles with an average particle size of 50 nm to every 1 L of deionized water;

[0070] A graphene dispersion was obtained by adding 30 g of sodium dodecyl sulfate and 1 g of graphene to 1 L of deionized water, and dispersing the mixture in an ultrasonic disperser for 4 hours to fully disperse the graphene.

[0071] The zirconium salt system electrolyte containing nano Y2O3 particles and the graphene dispersion were mixed in a volume ratio of 2:1 to prepare a micro-arc oxidation electrolyte, which was placed in a reaction tank for standby use.

[0072] Step 3: Micro-arc oxidation treatment:

[0073] The obtained micro-arc oxidation electrolyte is placed in a PVC micro-arc oxidation tank, and the magnesium alloy building template and stainless steel plate with a smooth surface are completely immersed in the micro-arc oxidation electrolyte. The stainless steel plate is connected to the negative electrode of the micro-arc oxidation power supply as a cathode, and the magnesium alloy building template is connected to the positive electrode of the micro-arc oxidation power supply as an anode. When performing micro-arc oxidation treatment, the micro-arc oxidation power supply adopts a DC pulse power supply with a power pulse frequency of 1200Hz, a duty cycle of 10%, a micro-arc oxidation termination voltage of 450V, an electrolyte temperature of 25°C, and a micro-arc oxidation treatment for 30min.

[0074] Step 4: Ceramic membrane sealing treatment:

[0075] After the micro-arc oxidation treatment is completed, the power supply voltage is directly reduced to 200V without turning off the power supply, and the treatment is carried out for 8 minutes. Since sodium dodecyl sulfate is an anionic surfactant, it is adsorbed on both sides of the graphene sheet. Relying on the electrostatic repulsion or van der Waals force, the graphene is evenly dispersed in the aqueous solution and presents a negative charge. The graphene added to the micro-arc oxidation electrolyte is in-situ sealed on the micropores on the surface of the micro-arc oxidation ceramic membrane by applying a secondary voltage during the ceramic membrane sealing treatment, thereby preventing the corrosive medium from diffusing and penetrating through the micropores of the micro-arc oxidation ceramic membrane, so that the graphene in the electrolyte seals the micro-arc oxidation ceramic membrane.

[0076] Step 5: Polishing of ceramic film:

[0077] The magnesium alloy building template after ceramic membrane sealing treatment is cleaned and dried to obtain an in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic membrane on the surface of the magnesium alloy building template;

[0078] The magnesium alloy building formwork was ultrasonically cleaned in deionized water for 2 minutes at room temperature, then placed in deionized water heated to 100° C. and boiled for 10 minutes, and then taken out and dried.

[0079] The in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic film on the surface of the magnesium alloy building formwork prepared in Example 2 is used as Sample 2.

[0080] Example 3

[0081] Step 1: Pre-treat the surface of magnesium alloy building formwork:

[0082] Add 20g Na2CO3, 3g OP emulsifier, 15g Na3PO4 and 15g Na2SiO3 to every 1L of deionized water to prepare an alkaline degreasing solution. Use the alkaline degreasing solution to wash the surface of the magnesium alloy building formwork for 20 minutes, then wash with deionized water and dry, and the surface of the magnesium alloy building formwork will be smooth.

[0083] Step 2: Prepare a zirconium salt system micro-arc oxidation electrolyte containing nano Y2O3 particles and graphene:

[0084] A zirconium salt system electrolyte containing nano Y2O3 particles was prepared by adding (NaPO3)6 40g, Na3PO4 23g, C6H5O7Na3·2H2O 45g, K2ZrF6 40g, PEG-1000 5g, EDTA-Na12g and nano Y2O3 particles with an average particle size of 50nm to every 1L of deionized water;

[0085] A graphene dispersion was obtained by adding 25 g of sodium dodecyl sulfate and 1 g of graphene to 1 L of deionized water, and dispersing the mixture in an ultrasonic disperser for 4 h to fully disperse the graphene.

[0086] The zirconium salt system electrolyte containing nano Y2O3 particles and the graphene dispersion were mixed in a volume ratio of 2:1 to prepare a micro-arc oxidation electrolyte, which was placed in a reaction tank for standby use.

[0087] Step 3: Micro-arc oxidation treatment:

[0088] The obtained micro-arc oxidation electrolyte is placed in a PVC micro-arc oxidation tank, and the magnesium alloy building template and stainless steel plate with a smooth surface are completely immersed in the micro-arc oxidation electrolyte. The stainless steel plate is connected to the negative electrode of the micro-arc oxidation power supply as a cathode, and the magnesium alloy building template is connected to the positive electrode of the micro-arc oxidation power supply as an anode. When performing micro-arc oxidation treatment, the micro-arc oxidation power supply adopts a DC pulse power supply with a power pulse frequency of 1100 Hz, a duty cycle of 8%, a micro-arc oxidation termination voltage of 400 V, an electrolyte temperature of 25°C, and a micro-arc oxidation treatment of 25 minutes.

[0089] Step 4: Ceramic membrane sealing treatment:

[0090] After the micro-arc oxidation treatment is completed, the power supply voltage is directly reduced to 180V without turning off the power supply, and the treatment is carried out for 7 minutes. Since sodium dodecyl sulfate is an anionic surfactant, it is adsorbed on both sides of the graphene sheet. Relying on the action of electrostatic repulsion or van der Waals force, the graphene is evenly dispersed in the aqueous solution and presents a negative charge. The graphene added to the micro-arc oxidation electrolyte is in-situ sealed on the micropores on the surface of the micro-arc oxidation ceramic membrane by applying a secondary voltage during the ceramic membrane sealing treatment, thereby preventing the corrosive medium from diffusing and penetrating through the micropores of the micro-arc oxidation ceramic membrane, so that the graphene in the electrolyte seals the micro-arc oxidation ceramic membrane.

[0091] Step 5: Polishing of ceramic film:

[0092] The magnesium alloy building template after ceramic membrane sealing treatment is cleaned and dried to obtain an in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic membrane on the surface of the magnesium alloy building template;

[0093] The magnesium alloy building formwork was ultrasonically cleaned in deionized water for 1 minute at room temperature, then boiled in deionized water heated to 100°C for 10 minutes, and then taken out and dried.

[0094] The in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic film on the surface of the magnesium alloy building formwork prepared in Example 3 is used as Sample 3.

[0095] Comparative Example 1

[0096] The AZ91D magnesium alloy template substrate without in-situ synthesis of graphene-modified Y2O3 / ZrO2 / MgO composite ceramic film was used as sample 4.

[0097] The following will compare and analyze the performance of samples 1 to 4 through performance testing experiments on scanning electron microscope surface morphology and cross-sectional morphology, phase composition, thickness, surface roughness, hardness, wear resistance, bonding strength, corrosion resistance, and wetting angle.

[0098] 1. Analysis of surface morphology and cross-sectional morphology of samples 1 to 3 by scanning electron microscopy

[0099] The surface morphology and cross-sectional morphology of samples 1 to 3 were observed using a field emission scanning electron microscope (SEM). Figure 2As shown in the figure, the surface morphology photos of the ceramic membrane show that there are many discharge micropores distributed on the surface of samples 1 to 3, and there is an obvious "crater" shape around the micropores caused by the rapid solidification of molten material. The pores on the surface of the ceramic membranes of samples 1 to 3 are evenly distributed, with small pore sizes and fewer surface defects. Since the surface of the nano Y2O3 particles added to the electrolyte carries a negative charge, they can quickly move to the surface of the ceramic membrane under the action of the electric field to promote the film-forming reaction and reduce surface defects of the membrane layer. The addition of nano Y2O3 particles helps to improve the morphology of the ceramic membrane and improve the surface quality of the ceramic membrane.

[0100] like Figure 2 As shown in the cross-sectional morphology photograph of the ceramic membrane, it can be seen that there are some unevenly distributed micropores inside the cross-section of the ceramic membrane, but the micropores do not extend to the interface between the ceramic membrane and the substrate, and the ceramic membrane and the substrate are tightly bonded.

[0101] Therefore, it can be concluded that the in-situ synthesized graphene modified Y2O3 / ZrO2 / MgO composite ceramic membrane prepared by the method of the present invention has good bonding with the magnesium alloy matrix, is not easy to fall off, has fewer surface defects, and has higher quality.

[0102] 2. Analysis of phase composition of samples 1 to 3

[0103] The phase composition of the ceramic membrane of sample 1 was tested by X-ray diffractometer. Figure 3 It can be seen that graphene has no obvious effect on the phase composition of the ceramic membrane. The ceramic membrane is mainly composed of ZrO2, MgO, MgF 2、 It is composed of ZrF4 and Y2O3 phases, and contains high-hardness MgO and ZrO2 phases, which can significantly improve the microhardness of the ceramic film; it contains corrosion-resistant MgF2 and ZrO2 phases, which can significantly improve the corrosion resistance of the ceramic film.

[0104] 3. Thickness analysis of samples 1 to 3

[0105] The thickness of the ceramic film was tested using a coating thickness gauge. Five points were taken on the surface of each sample to be tested, and the average value was taken as the thickness of the ceramic film of the sample to be tested. The test results are shown in Table 1.

[0106] Table 1 Ceramic film thickness test results (unit: μm)

[0107] Experimental samples Data 1 Data 2 Data 3 Data 4 Data 5 average value Sample 1 28.1 29.3 27.7 27.6 26.9 27.9 Sample 2 32.1 31.6 33.2 32.8 31.5 32.2 Sample 3 29.8 31.2 30.2 29.7 28.9 30.0

[0108] As can be seen from Table 1, samples 1 to 3 prepared by the method of the present invention have an average ceramic film thickness of 27 to 32 μm as tested by a coating thickness gauge. The in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic film prepared by the method of the present invention has a thick thickness and can provide excellent protection for the magnesium alloy building template substrate.

[0109] 4. Comparative analysis of surface roughness of samples 1 to 4

[0110] The roughness of the ceramic film was tested using an SJ-210 surface roughness measuring instrument. To ensure the credibility of the measurement data, 5 points were taken on the surface of each sample to be tested, and the average value of the 5 times was taken as the surface roughness R of the sample to be tested. a The test results are shown in Table 2.

[0111] Table 2 Ceramic membrane surface roughness R a Test results (unit: μm)

[0112] Experimental samples Data 1 Data 2 Data 3 Data 4 Data 5 average value Sample 1 1.61 1.49 1.36 1.39 1.46 1.46 Sample 2 1.39 1.42 1.55 1.59 1.49 1.49 Sample 3 1.58 1.52 1.49 1.52 1.42 1.51 Sample 4 1.25 1.28 1.31 1.25 1.21 1.26

[0113] As can be seen from Table 2, the roughness of the ceramic membranes of samples 1 to 3 is not much different from that of the ceramic membrane of sample 4. The addition of graphene and nano Y2O3 particles improves the roughness of the surface of the ceramic membrane generated by micro-arc oxidation on the surface of the magnesium alloy building template. It can be seen that the surface flatness of the in-situ synthesized graphene modified Y2O3 / ZrO2 / MgO composite ceramic membrane prepared by the method of the present invention is relatively high.

[0114] 5. Comparative analysis of hardness of samples 1 to 4

[0115] The hardness of the ceramic films of samples 1 to 4 was measured using a HV-1000A microhardness tester. During the measurement, the indenter load of the hardness tester was set to 100 g, the dwell time was 15 s, and 5 points were taken on the surface of each sample to be tested for testing. The average value of 5 times was taken as the microhardness of the sample to be tested. The test results are shown in Table 3.

[0116] Table 3 Ceramic film microhardness test results (unit: HV)

[0117] Experimental samples Data 1 Data 2 Data 3 Data 4 Data 5 average value Sample 1 855.7 866.5 861.3 861.3 859.8 861.0 Sample 2 999.3 1001.9 1011.5 1010 1015.6 1007.7 Sample 3 908.6 910.7 910.3 915.4 908.7 910.7 Sample 4 96.1 93.9 94.3 96.8 94.0 95.0

[0118] As can be seen from Table 3, samples 1 to 3 prepared by the method of the present invention, after microhardness test, found that the average microhardness of sample 1 was 861.0HV, which was the lowest value among the prepared samples, while the average microhardness of the untreated magnesium alloy sample 4 was only 95.0HV. Because the Zr element added to the solution enters the ceramic film through the complex reaction of micro-arc oxidation to form high-hardness MgO phase and ZrO2 phase. It can be seen that the in-situ synthesized graphene modified Y2O3 / ZrO2 / MgO composite ceramic film prepared by the method of the present invention significantly improves the hardness of the magnesium alloy building template.

[0119] 6. Analysis of wear resistance of samples 1 to 3

[0120] The friction and wear test of samples 1 to 3 was carried out using an MMQ-02G ball-disc wear tester, and the friction coefficient of the ceramic film was measured in the rotation mode. The grinding material was a GCr15 friction ball with a diameter of 6 mm, the applied load was 8N, the rotation speed was 100 rpm, and the wear radius was 4 mm. All tests were carried out at room temperature. The test results are shown in Figure 4 shown.

[0121] Depend on Figure 4 It can be seen that the friction coefficients of the ceramic films of samples 1 to 3 are relatively low, and the fluctuations of the friction coefficients are relatively small.

[0122] The wear scar microstructures of samples 1 to 3 after the friction and wear test were observed using a scanning electron microscope (SEM). Figure 5 As shown. Figure 5 It can be seen that the wear marks on the ceramic membranes of samples 1 to 3 are not obvious, the surface morphology has not changed significantly compared with before wear, and the wear of the ceramic membrane is relatively slight. The high-hardness ZrO2 and MgO phases contained in the ceramic membrane make the hardness of the ceramic membrane significantly higher than that of the magnesium alloy matrix, reducing the cutting effect of the grinding pair or abrasive particles on the surface of the ceramic membrane. In addition, the addition of graphene and Y2O3 reduces the surface roughness of the ceramic membrane, and the lamellar structure of graphene plays a role in reducing wear and lubrication, reducing the friction coefficient of the ceramic membrane and improving the wear resistance of the ceramic membrane. It can be seen that the in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic membrane prepared by the method described in the present invention significantly increases the wear resistance of the magnesium alloy building formwork.

[0123] VII. Analysis of the binding force of samples 1 to 3

[0124] The RevetestXpress scratch tester was used to test the bonding strength between the micro-arc oxidation ceramic film and the magnesium alloy sample. The working principle of the Revetest Xpress scratch tester is: under the premise of the set maximum load, scratch length, loading speed and sliding speed, as the diamond indenter moves forward at a uniform speed and presses down, the force exerted by the indenter on the ceramic film becomes larger and larger. When it increases to a certain extent, the ceramic film is separated from the base metal material, and a sound wave signal is generated and received by the acoustic emission sensor. The load applied at this time is the bonding strength between the ceramic film and the magnesium alloy building template matrix. During the test, each sample surface was repeated 5 times, each time with an interval width of 5mm, and the average value of 5 times was taken as the bonding strength between the ceramic film to be tested and the magnesium alloy matrix. The test results are shown in Table 4.

[0125] Table 4 Bonding strength between ceramic membrane and magnesium alloy building formwork substrate (unit: MPa)

[0126] Experimental samples Data 1 Data 2 Data 3 Data 4 Data 5 average value Sample 1 15.86 16.21 15.37 16.34 16.16 15.99 Sample 2 17.24 16.91 16.77 17.02 16.10 16.81 Sample 3 13.55 14.36 14.39 13.24 14.15 13.94

[0127] As can be seen from Table 4, the lowest average bonding strength between the ceramic membranes of samples 1 to 3 prepared by the technical solution and the magnesium alloy substrate is 13.94 MPa, which is much higher than the national standard GB / T5210-2006 "Adhesion Test of Paint and Varnish Pull-off Method" that the adhesion between the coating and the metal material should not be less than 5 MPa. It can be seen that the in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic membrane prepared by the method of the present invention has a strong bonding strength with the magnesium alloy building template substrate, good film quality, and is not easy to fall off.

[0128] 8. Comparative analysis of corrosion resistance of samples 1 to 4

[0129] The polarization curves of samples 1 to 4 were measured using an electrochemical workstation. A three-electrode system was used for detection, in which the sample was the working electrode and the test area was 1 cm 2 , saturated calomel electrode as reference electrode, platinum sheet as auxiliary electrode. The corrosive medium is 3.5% (mass fraction) NaCl aqueous solution, and its temperature is 25℃. The sample is immersed in the corrosive medium for 0.5h to stabilize the open circuit potential, the scanning speed is 10mV / s, and the scanning range is -2.2V~-1.0V.

[0130] Figure 6 The polarization curves of samples 1 to 4 show that the corrosion potentials of samples 1 to 3 are -1.286 V, -1.427 V, and -1.116 V, respectively, which are more positive than the corrosion potential of sample 4, -1.490 V. The corrosion current densities of samples 1 to 3 are 3.52×10 -7 A / cm 2 , 1.98×10 -7 A / cm 2 ,8.67×10 -8 A / cm 2 Compared with the corrosion current density of sample 4, which is 1.1×10 -6 A / cm 2 It is reduced by 1 to 2 orders of magnitude, indicating that the micro-arc oxidation ceramic film on its surface greatly improves its corrosion resistance. Since the ceramic film contains a highly corrosion-resistant ZrO2 phase, and the addition of nano Y2O3 particles reduces the diameter of the micropores on the surface of the ceramic film, graphene seals the micropores on the surface of the micro-arc oxidation ceramic film in situ under the action of the secondary voltage, further preventing the corrosive medium from corroding the magnesium alloy building template matrix. It can be seen that the in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic film prepared by the method of the present invention helps to improve the corrosion resistance of the magnesium alloy building template and reduce its corrosion tendency, thereby extending its service life.

[0131] IX. Comparative Analysis of Wetting Angles of Samples 1 to 4

[0132] The surface contact angles of samples 1 to 4 were measured using the angle measurement method. During the measurement, deionized water was dropped on the sample surface, and a microscope lens and a camera were used to obtain an image of the shape of the drop on the sample surface. Figure 7 As shown, a tangent line is drawn at the intersection of the solid, liquid and gas phases in the picture, and the angle is measured with a protractor. The test results are shown in Table 5.

[0133] Table 5 Ceramic membrane contact angle test results

[0134] Experimental samples Sample 1 Sample 2 Sample 3 Sample 4 Contact angle (°) 94.0 101.5 96.0 41.5

[0135] It can be seen from Table 5 that the contact angles of the ceramic membrane surfaces of samples 1 to 3 prepared by the method of the present invention are all greater than 90 degrees, indicating that they have good hydrophobicity, that is, the surface of the sample prepared by the present invention has better hydrophobicity than sample 4. Since the micropores on the surface of the ceramic membrane are closed by graphene, the adsorption of water by the micropores is reduced. At the same time, graphene itself is hydrophobic, blocking the penetration of water molecules in the ceramic membrane. It can be seen that the in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic membrane prepared by the method of the present invention makes the magnesium alloy building template have excellent anti-fouling properties.

[0136] From the above embodiments and comparative experimental analysis, it is obvious that the surface in-situ synthesized graphene modified Y2O3 / ZrO2 / MgO composite ceramic film disclosed by the present invention improves the corrosion resistance, wear resistance and anti-fouling properties of the magnesium alloy building formwork, and the prepared ceramic film is dense and uniform, which solves the problem that the surface of the magnesium alloy building formwork is easily scratched, corroded and contaminated during the use; at the same time, the process is simple, the energy consumption is low, and the formed ceramic film has high hardness and wear resistance; the electrode potential is high and corrosion resistance; the surface wetting angle is large and stain resistance, thereby providing a magnesium alloy building formwork that is safer and more practical.

[0137] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for in-situ synthesis of graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of magnesium alloy building template, characterized in that: The steps include: S1. Pre-treating the surface of the magnesium alloy building formwork: cleaning the surface of the magnesium alloy building formwork with an alkaline degreasing solution and drying the surface to obtain a magnesium alloy building formwork with a smooth surface; S2. Prepare a zirconium salt system micro-arc oxidation electrolyte containing nano Y2O3 particles and graphene: mix the graphene dispersion and the zirconium salt system electrolyte containing nano Y2O3 particles in a volume ratio of 1:2 to obtain a micro-arc oxidation electrolyte, and place the mixture in a PVC micro-arc oxidation tank for standby use; S3, micro-arc oxidation treatment: placing the obtained micro-arc oxidation electrolyte in a PVC micro-arc oxidation tank, and placing the magnesium alloy building formwork and stainless steel plate with a smooth surface in the micro-arc oxidation electrolyte, and performing micro-arc oxidation treatment for 20 to 30 minutes; S4, ceramic membrane sealing treatment: sealing treatment is performed on the ceramic membrane formed on the surface of the magnesium alloy building formwork after micro-arc oxidation treatment; S5. Ceramic membrane polishing treatment: The magnesium alloy building formwork after the ceramic membrane sealing treatment is cleaned and dried to obtain an in-situ synthesized graphene-modified Y2O3 / ZrO2 / MgO composite ceramic membrane on the surface of the magnesium alloy building formwork.

2. The method for in-situ synthesis of graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of magnesium alloy building formwork according to claim 1, characterized in that: In step S1, the surface of the magnesium alloy building formwork is washed with an alkaline degreasing liquid for 15 to 20 minutes, and then washed with deionized water. 10 to 20 g of Na2CO3, 1 to 3 g of OP emulsifier, 10 to 20 g of Na3PO4 and 10 to 20 g of Na2SiO3 are added to each 1 L of deionized water to prepare an alkaline degreasing liquid.

3. The method for in-situ synthesis of graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of magnesium alloy building formwork according to claim 1, characterized in that: The zirconium salt system electrolyte containing nano Y2O3 particles in step S2 is prepared by adding 30-45 g of (NaPO3)6, 20-25 g of Na3PO4, 35-50 g of C6H5O7Na3·2H2O, 35-40 g of K2ZrF6, 4-6 g of PEG-1000, 10-15 g of EDTA-Na and 0.5-1 g of nano Y2O3 particles with an average particle size of 50 nm to 1 L of deionized water. The graphene dispersion is prepared by adding 20-30 g of sodium dodecyl sulfate and 1 g of graphene to every 1 L of deionized water.

4. The method for in-situ synthesis of graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of magnesium alloy building formwork according to claim 3, characterized in that: When preparing the graphene dispersion, 20-30 g of sodium dodecyl sulfate and 1 g of graphene are added to 1 L of deionized water, and the mixture is placed in an ultrasonic disperser for 3-4 hours to fully disperse the graphene. Sodium dodecyl sulfate is an anionic surfactant that is adsorbed on both sides of the graphene sheet. Relying on electrostatic repulsion or van der Waals force, the graphene is evenly dispersed in the aqueous solution and presents a negative charge.

5. The method for in-situ synthesis of graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of magnesium alloy building formwork according to any one of claims 1 to 4, characterized in that: The graphene added to the micro-arc oxidation electrolyte can in-situ seal the micropores on the surface of the micro-arc oxidation ceramic membrane by applying a secondary voltage during the ceramic membrane sealing treatment, thereby preventing the corrosive medium from diffusing and penetrating through the micropores of the micro-arc oxidation ceramic membrane.

6. The method for in-situ synthesis of graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of magnesium alloy building formwork according to claim 1, characterized in that: In step S3, the magnesium alloy building template and the stainless steel plate with smooth surface need to be completely immersed in the micro-arc oxidation electrolyte, the stainless steel plate is connected to the negative electrode of the micro-arc oxidation power supply as a cathode, and the magnesium alloy building template is connected to the positive electrode of the micro-arc oxidation power supply as an anode.

7. The method for in-situ synthesis of graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of magnesium alloy building formwork according to claim 1, characterized in that: During the micro-arc oxidation treatment in step S3, the micro-arc oxidation power supply adopts a DC pulse power supply, the power pulse frequency is 1000-1200 Hz, the duty cycle is 5-15%, the micro-arc oxidation termination voltage is 350-450V, and the temperature of the micro-arc oxidation electrolyte is 15-25°C.

8. The method for in-situ synthesis of graphene Y2O3ZrO2MgO composite ceramic film on the surface of magnesium alloy building formwork according to claim 1, characterized in that: The specific steps of step S4 ceramic membrane sealing treatment are: after the micro-arc oxidation treatment is completed, the power supply voltage of the micro-arc oxidation power supply is directly reduced to 150-200V without turning off the power supply, and the ceramic membrane sealing treatment is carried out for 5-8 minutes.

9. The method for in-situ synthesis of graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of magnesium alloy building formwork according to claim 1, characterized in that: The specific method for cleaning the magnesium alloy building formwork in step S5 is: Cleaning treatment: After ultrasonic cleaning of the magnesium alloy building formwork in deionized water for 1 to 2 minutes at room temperature, place it in deionized water heated to 100°C and boil it for 10 minutes, then take it out and dry it.

10. The method for in-situ synthesis of graphene Y2O3 / ZrO2 / MgO composite ceramic film on the surface of magnesium alloy building formwork according to claim 1, characterized in that: The inlet and outlet pipelines of the micro-arc oxidation electrolyte are connected to the cooling device, so that the micro-arc oxidation electrolyte forms a cooling cycle and maintains the temperature of the micro-arc oxidation electrolyte at 15-25°C. An agitator is also installed inside the micro-arc oxidation electrolyte to mix the micro-arc oxidation electrolyte evenly through stirring.

Citation Information

Cited By

  • Preparation method of composite coating and composite coating

    CN119243287A

  • Composite coating preparation method and composite coating

    CN119243287B