Negative electrode material, its manufacturing method, and secondary battery
By controlling the particle size relationships and adding a coating layer to the negative electrode material, the material's stability and capacity are enhanced, addressing the limitations of existing graphite-based electrodes.
Patent Information
- Application Number
- JP2023570326
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-29
- Filing Date
- 2023-06-08
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-06-08
AI Technical Summary
Current negative electrode materials, particularly graphite, have reached their theoretical capacity limit and face significant volumetric expansion issues during cycling, leading to rapid decay due to powdering and crushing, which existing structural designs and methods fail to adequately address.
A negative electrode material with controlled particle size relationships between primary and secondary particles, specifically 10≦D2 50 /D1 max ≦40, D2 min /D2 50 ≧0.08, and D2 50 /D2 max ≧0.24, combined with a coating layer, to enhance adhesion and stability, reducing volumetric expansion.
The controlled particle size distribution and coating improve cycle stability and capacity by minimizing rupture and powdering, concentrating particle sizes, and effectively reducing volumetric expansion.
Smart Images

Figure 2024539793000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims priority to a Chinese patent application filed with the State Intellectual Property Office of the People's Republic of China on September 29, 2022, bearing application number 202211199579X and title "Negative electrode material and its manufacturing method, and secondary battery," the entire contents of which are incorporated herein by reference.
[0002] The present application relates to the technical field of negative electrode materials, and in particular to a negative electrode material and a manufacturing method thereof, and a secondary battery. [Background technology]
[0003] In recent years, with the development of the market, the demand for high energy density anode materials, especially in the field of electric vehicles, is increasing. Currently, the commercialized anode material is graphite, whose capacity is already close to the theoretical upper limit and the scope for further improvement is limited, so the development of a new generation of high energy density anode materials is urgently needed.
[0004] Silicon anodes are next-generation anode materials, and have the advantages of high capacity, abundant sources, and relative safety. However, silicon anode materials have a rapid volume expansion effect during cycling, which leads to material pulverization and crushing, and fast cycle decay of the battery. There are currently many solutions to this problem, including structural design of silicon and adopting methods such as nano-sizing, porosity, and composite coating to improve the performance. However, the conventional structures and processes for suppressing volume expansion are all complicated, and the effect of suppressing volume expansion with increasing capacity is limited.
[0005] Therefore, it is necessary to further reduce the volume expansion effect of the negative electrode material. Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present application is to provide a negative electrode material capable of improving capacity and cycle stability while suppressing volume expansion, a method for producing the same, and a secondary battery. [Means for solving the problem]
[0007] In order to achieve the above object, in a first aspect, the present application provides a negative electrode material, the negative electrode material including secondary particles, the secondary particles including aggregated primary particles, and the primary particles and the secondary particles satisfy the following relationship: 10≦D2 50 / D1 max ≦40(I) D2 min / D2 50 ≧0.08 (II) D2 50 / D2 max ≧0.24 (III) (In formulas (I), (II) and (III), D1 max is the maximum particle size of the primary particles, and D2 50 is the median diameter of the secondary particles, and D2 min is the minimum particle size of secondary particles, and D2 max is the maximum particle size of the secondary particles.)
[0008] In one possible embodiment, the primary particles contain at least one of Li, SiOx, Na, K, Sn, Ge, Si, Fe, Mg, Ti, Zn, Al, P and Cu, of which 0.05% is SiOx, SiOx, Na, K, Sn, Ge, Si, Fe, Mg, Ti, Zn, Al, P and Cu. <x<2である。
[0009] In one possible embodiment, the bulk density of the primary particles is less than 0.7 g / cm 3 The following is the result.
[0010] In one possible embodiment, the median diameter D1 of the primary particles 50 is less than 0.2 μm.
[0011] In one possible embodiment, the median diameter D2 of the secondary particles 50 The range is 0.5 μm to 20 μm.
[0012] In one possible embodiment, the maximum particle size D1 of the primary particles max The range is 0.1 μm to 0.4 μm.
[0013] In one possible embodiment, the minimum particle size D2 of the secondary particles min The range is 0.5 μm to 4 μm.
[0014] In one possible embodiment, the maximum particle size D2 of the secondary particles max The range is 6 μm to 20 μm.
[0015] In one possible embodiment, the specific surface area of the negative electrode material is 10 m 2 / g or less.
[0016] In one possible embodiment, the negative electrode material has a porosity of 10% or less.
[0017] In one possible embodiment, the negative electrode material has a sphericity of 0.7 or more.
[0018] In one possible embodiment, the negative electrode material further comprises a coating layer present on at least a portion of the surface of the primary particles and / or the secondary particles.
[0019] In one possible embodiment, the coating layer comprises at least one of a carbon material, graphene, silicon carbide, a metal oxide and a nitride.
[0020] In one possible embodiment, the coating layer comprises a carbon material, the carbon material comprising at least one of soft carbon, hard carbon, crystalline carbon and amorphous carbon.
[0021] In one possible embodiment, the coating layer comprises a metal oxide, the metal oxide comprising at least one of titanium oxide, aluminum oxide, lithium oxide, cobalt oxide and vanadium oxide.
[0022] In one possible embodiment, the coating layer comprises a nitride, the nitride comprising at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride and carbon nitride.
[0023] In one possible embodiment, the coating layer has a thickness of 1 nm to 500 nm.
[0024] In a second aspect, an embodiment of the present application provides a method for producing a negative electrode material, comprising: A step of granulating a mixed material including the primary particles and the adhesive to obtain a precursor; heat treating the precursor to carbonize the adhesive to obtain a heat treated product; and crushing and classifying the heat-treated product to obtain secondary particles that satisfy the following relationship with the primary particles, thereby obtaining a negative electrode material. 10≦D2 50 / D1 max ≦40(I) D2 min / D2 50 ≧0.08 (II) D2 50 / D2 max ≧0.24 (III) (In formulas (I), (II) and (III), D1 max is the maximum particle size of the primary particles, and D2 50 is the median diameter of the secondary particles, and D2 min is the minimum particle size of secondary particles, and D2 max is the maximum particle size of the secondary particles.)
[0025] In one possible embodiment, the median size of the primary particles is less than or equal to 0.2 μm.
[0026] In one possible embodiment, the primary particles contain at least one of Li, SiOx, Na, K, Sn, Ge, Si, Fe, Mg, Ti, Zn, Al, P and Cu, of which 0.05% is SiOx, Na, K, Sn, Ge, Si, Fe, Mg, Ti, Zn, Al, P and Cu. <x<2である。
[0027] In one possible embodiment, the adhesive comprises at least one of starch, cellulose, tannin, gum arabic, sodium alginate, styrene butadiene rubber, butyl rubber, cellulose ester, ene-based polymers, polyamide, polyacrylate, epoxy resin, phenolic resin, furan resin, unsaturated polyester, acrylic resin, and polyimide.
[0028] In one possible embodiment, the mass ratio of the primary particles to the adhesive is 100:(5 to 55).
[0029] In one possible embodiment, the mixture of primary particles and adhesive further comprises a solvent.
[0030] In one possible embodiment, the solvent comprises at least one of phenol, an alcohol-based solvent, an ether-based solvent, and an alkane-based solvent.
[0031] In one possible embodiment, the mass ratio of the solvent to the primary particles is 100:(5-40).
[0032] In one possible embodiment, the method further includes dispersing the mixed material including the primary particles and the adhesive prior to the step of granulating the mixed material including the primary particles and the adhesive.
[0033] In one possible embodiment, the dispersion treatment includes at least one selected from the group consisting of magnetic stirring, mechanical stirring, abrasive dispersion, and ultrasonic dispersion.
[0034] In one possible embodiment, the temperature of the heat treatment is 500°C to 1000°C.
[0035] In one possible embodiment, the heat-retaining time for the heat treatment is 30 minutes to 900 minutes.
[0036] In one possible embodiment, the heat treatment is performed in a protective atmosphere, the protective atmosphere comprising at least one of nitrogen gas, argon gas, and helium gas.
[0037] In one possible embodiment, the median diameter of the material obtained by pulverization is 0.5 μm to 15 μm.
[0038] In one possible embodiment, the maximum particle size of the material obtained by pulverization is between 5 μm and 45 μm.
[0039] In one possible embodiment, the method further comprises removing particles having a particle size of 0.5 μm or less from the material obtained by the classification process after the classification process.
[0040] In one possible embodiment, the method further comprises pre-grinding and pre-classifying the precursor prior to the step of heat treating the precursor to carbonize the adhesive.
[0041] In one possible embodiment, the pre-grinding further comprises at least one of mechanical grinding, airflow grinding, ultrafine grinding, wet grinding, extrusion grinding and split grinding.
[0042] In one possible embodiment, the median diameter of the material obtained by the pre-grinding is 0.5 μm to 20 μm.
[0043] In one possible embodiment, the maximum particle size of the material obtained by the pre-grinding is between 5 μm and 45 μm.
[0044] In one possible embodiment, the particle size of the material obtained from said pre-classification is greater than 0.5 μm.
[0045] In one possible embodiment, the method further comprises carrying out a fusion treatment of the precursor and the coating material before the step of heat treating the precursor to carbonize the adhesive.
[0046] In one possible embodiment, the coating material comprises at least one of a carbon source, graphene, silicon carbide, a metal oxide, and a nitride.
[0047] In one possible embodiment, the coating material comprises a carbon source, the carbon source comprising at least one of soft carbon, hard carbon, crystalline carbon, and amorphous carbon.
[0048] In one possible embodiment, the coating material comprises a metal oxide, the metal oxide comprising at least one of titanium oxide, aluminum oxide, lithium oxide, cobalt oxide and vanadium oxide.
[0049] In one possible embodiment, the coating material comprises a nitride, the nitride comprising at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride, and carbon nitride.
[0050] In one possible embodiment, the blending process device includes at least one of a mechanical blender, a blender stirrer, and a convection blender.
[0051] In one possible embodiment, the duration of the fusion treatment is 30 minutes to 150 minutes.
[0052] In a third aspect, the present application provides a secondary battery, the secondary battery comprising the anode material according to the first aspect or produced by the method according to the second aspect. Effect of the Invention
[0053] Compared with the prior art, the present application can provide the following beneficial effects:
[0054] The negative electrode material provided in the present application limits the particle size relationship between the primary particles and the secondary particles, thereby making the stacking manner of the primary particles in the secondary particles relatively tight, and the adhesion between the primary particles due to the primary particles being too large can be reduced, and the secondary particles formed by aggregation can be reduced in the bursting and powdering phenomenon during charging and discharging; at the same time, the primary particles can be prevented from being excessively aggregated to form secondary particles with a size that is too large due to the primary particles being too small in size; by controlling the particle size relationship between the primary particles and the secondary particles, the structural stability of the negative electrode material can be improved, and the existence of small and large secondary particles can be effectively reduced, and the particle size distribution of the secondary particles can be relatively concentrated, thereby improving the cycle stability and capacity of the negative electrode material, and reducing the volume expansion effect of the negative electrode material. [Brief description of the drawings]
[0055] In order to more clearly describe the technical solutions of the embodiments of the present application or the prior art, the following briefly introduces drawings necessary for describing the embodiments or the prior art. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative efforts. [Figure 1] 1 is a flowchart showing the production of a negative electrode material according to the present application. [Diagram 2] 1 is a scanning electron microscope (SEM) chart of the negative electrode material produced in Example 1 of the present application. [Diagram 3] 1 is an XRD chart of the negative electrode material prepared in Example 1 of the present application. [Figure 4] FIG. 2 is an initial charge / discharge curve diagram of the negative electrode material prepared in Example 1 of the present application. [Diagram 5] FIG. 2 is a cycle characteristic curve diagram of the negative electrode material prepared in Example 1 of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0056] In order to better understand the technical solution of the present application, the following describes in detail the embodiments of the present application with reference to the accompanying drawings.
[0057] It should be clear that the described embodiments are only some embodiments of the present application, but not all embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative work are included in the protection scope of the present application.
[0058] Moreover, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying the relative importance or the number of the indicated technical features, whereby a feature qualified by "first" or "second" may explicitly or implicitly include one or more of said features.
[0059] In order to facilitate understanding of this application, certain terms are defined herein as appropriate. Unless otherwise defined herein, scientific and technical terms used in this application shall have the meanings commonly understood by those skilled in the art of this application.
[0060] As used herein, the term "primary particle" refers to a particle unit that forms a single non-agglomerated particle or a secondary particle.
[0061] The present application provides a negative electrode material, comprising secondary particles, the secondary particles comprising aggregated primary particles, and the primary particles and the secondary particles satisfy the following relationship: 10≦D2 50 / D1 max ≦40(I) D2 min / D2 50 ≧0.08 (II) D2 50 / D2 max ≧0.24 (III) In formulas (I), (II) and (III), D1 max is the maximum particle size of the primary particles, and D2 50 is the median diameter of the secondary particles, and D2 min is the minimum particle size of secondary particles, and D2max is the maximum particle size of the secondary particles of the negative electrode material.
[0062] Generally, primary particles are easy to spontaneously aggregate to form secondary particles, so the secondary particles have a wide particle size distribution range and a loose structure. The anode material provided in the present application limits the particle size relationship between the primary particles and the secondary particles, so that the stacking manner of the primary particles in the secondary particles is relatively tight, and the adhesion between the primary particles due to the particle size of the primary particles being too large is small, and the secondary particles formed by aggregation can reduce the bursting and powdering phenomenon during charging and discharging; at the same time, the primary particles can be prevented from being excessively aggregated to form secondary particles with a large size due to the particle size of the primary particles being too small; by controlling the particle size relationship between the primary particles and the secondary particles, the structural stability of the anode material is improved, and the existence of small and large secondary particles can be effectively reduced, and the particle size distribution of the secondary particles can be relatively concentrated, so that the cycle stability and capacity of the anode material can be improved, and the volume expansion effect of the anode material can be reduced.
[0063] In this application, 10≦D2 50 / D1 max ≦40, specifically, D2 50 / D1 max may be 10, 15, 20, 25, 30, 35, 40, etc., and may of course be other values within the above range, and are not limited thereto. Within the above range, the particle size of the primary particles and the secondary particles is appropriate, the degree of matching between the primary particles and the secondary particles is high, and the primary particles in the secondary particles are densely stacked, so that the particles in the negative electrode material are not easily powdered, and the stress caused by expansion during the charge and discharge process can be well released, the cycle performance of the material can be improved, and the expansion can be suppressed. The maximum value D1 of the primary particles max If D1 is too large, the adhesion between particles is small, powdering is likely to occur, cycle performance is reduced, and the maximum value D1 of the primary particles maxIf it is too small, the interaction force between particles becomes strong, the adhesion between particles becomes strong, and secondary particles with too large a size are likely to be formed. Secondary particles with too large a size are difficult to release the stress caused by expansion during the charge and discharge process, and the secondary particles may fall off from the current collector or the current collector may be damaged, resulting in a decrease in the performance of the material.
[0064] D2 min / D2 50 ≧0.08, specifically, D2 min / D2 50 may be 0.08, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, etc., or other values within the above range, and are not limited here. Within the above limited range, the number of fine powders in the secondary particles is small, the distribution of the content of the active component in the material is relatively uniform, the particle size distribution of the secondary particles is concentrated, the expansion difference between the secondary particles can be reduced, and the structural stability of the material can be improved.
[0065] D2 50 / D2 max ≧0.24, specifically, D2 50 / D2 max may be 0.24, 0.28, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, etc., and of course other values within the above range are also possible, and are not limited here. Within the above limited range, the particle size distribution of the secondary particles is concentrated and the number of secondary particles with a large particle size is small, so the volume expansion of the material can be effectively reduced and the cycle performance of the material can be improved.
[0066] In some embodiments, the primary particles include at least one of Li, SiOx (0 < x < 2), Na, K, Sn, Ge, Si, Fe, Mg, Ti, Zn, Al, P, and Cu.
[0067] In some embodiments, the primary particles include SiO x (0 < x < 2), specifically, SiO 0.1 , SiO 0.3 , SiO 0.5 , SiO 0.7 , SiO0.8 , SiO1, SiO 1.2 , SiO 1.5 , SiO 1.8 or SiO 1.9 etc., and of course other particles within the above ranges are also possible, and are not limited here.
[0068] In some embodiments, the sphericity of the primary particles is >0.7, and preferably the sphericity of the primary particles is >0.9.
[0069] In some embodiments, the bulk density of the primary particles is 0.7 g / cm 3 The bulk density of the primary particles is specifically 0.7 g / cm or less. 3 , 0.6g / cm 3 , 0.5g / cm 3 , 0.4g / cm 3 , 0.3g / cm 3 , 0.2g / cm 3 , 0.1g / cm 3 The bulk density of the primary particles may be, but is not limited to, 0.4 g / cm or other values within the above range. 3 It is preferable that the concentration is 0.2 g / cm or less. 3 It is even more preferable that:
[0070] In some embodiments, the median diameter of the primary particles is 0.2 μm or less, and specifically may be 1 nm, 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 60 nm, 80 nm, 100 nm, 130 nm, 150 nm, 200 nm, etc., or other values within the above range, and are not limited thereto. The median diameter of the primary particles is preferably 5 nm to 200 nm, and more preferably 10 nm to 200 nm.
[0071] In some embodiments, the maximum particle size D1 of the primary particles max The range is 0.1 μm to 0.4 μm, specifically, D1 maxSpecifically, the maximum particle diameter D1 of the primary particles may be 0.1 μm, 0.20 μm, 0.3 μm, 0.4 μm, etc., and may of course be other values within the above range, and is not limited thereto. max Controlling within the above range indicates that the particle size of the primary particles of the present application is small, the particles are less likely to powder, and the stability of the negative electrode material can be improved.
[0072] In some embodiments, the minimum particle size D2 of the secondary particles min The range is 0.5 μm to 4 μm, specifically, D2 min D2 may be 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, etc., and may of course be other values within the above range, and is not limited here. min Controlling the content of the fine powder in the negative electrode material within the above range indicates that the number of fine powders in the negative electrode material is relatively small, which contributes to the negative electrode material having an advantage of long cycle life.
[0073] In some embodiments, the maximum particle size D2 of the secondary particles max The range is 6 μm to 20 μm, specifically, D2 max D2 may be 6 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, etc., and may of course be other values within the above range, and is not limited here. max By controlling the content within the above range, the expansion of the material can be suppressed relatively well, which contributes to improving the performance of the material.
[0074] In some embodiments, D2 50 The range is 0.5 μm to 20 μm, specifically, D2 50 D2 may be 0.5 μm, 1 μm, 3 μm, 5 μm, 8 μm, 10 μm, 13 μm, 17 μm, 19 μm, 20 μm, etc., and may of course be other values within the above range, and is not limited here. 50 By controlling D2 within the above range, the average particle size of the resulting negative electrode material as a whole becomes smaller, which contributes to reducing the volume expansion of the negative electrode material. 50The thickness is preferably 0.8 μm to 12 μm, and more preferably 1 μm to 8 μm.
[0075] In some embodiments, the specific surface area of the negative electrode material is greater than 10 m 2 / g or less, and the specific surface area of the negative electrode material is specifically 10 m 2 / g, 9m 2 / g, 8m 2 / g, 7m 2 / g, 6m 2 / g, 5m 2 / g, 3m 2 / g, and of course may be other values within the above range, and are not limited thereto.
[0076] In some embodiments, the porosity of the negative electrode material is 10% or less, specifically, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 2.5%, 2% and 1%, etc., and of course, other values within the above range are also possible, and are not limited thereto. Controlling the porosity of the negative electrode material within the above range indicates that the electrolyte is less likely to penetrate into the material, which contributes to improving the stability of the negative electrode material. The porosity of the negative electrode material is preferably 5% or less, and more preferably 2.5% or less.
[0077] In some embodiments, the sphericity of the negative electrode material is 0.7 or more, specifically, the sphericity of the negative electrode material may be 0.7, 0.8, 0.9, etc., and the sphericity within the above range contributes to improving the processing performance of the material.
[0078] In some embodiments, the negative electrode material further comprises a coating layer on at least a portion of the surfaces of the primary particles and / or secondary particles. Preferably, a coating layer is present on the surfaces of the primary particles and a coating layer is also present on the surfaces of the secondary particles, and the materials of the two coating layers may be the same or different.
[0079] In some embodiments, the coating layer comprises at least one of a carbon material, graphene, silicon carbide, a metal oxide, and a nitride.
[0080] In some embodiments, when the material of the coating layer is a carbon material, the secondary particles may be dispersed and embedded in the carbon material, that is, the secondary particles are dispersed in the carbon material to form a silicon carbon composite, and the carbon material establishes a conductive network in the secondary particles, which is beneficial to the capacity of the negative electrode material, and the presence of the carbon material buffers the volume expansion of the particles and improves cycle stability.
[0081] In some embodiments, a carbon coating layer is formed on the surface of the primary particles, and the primary particles having the carbon coating layer aggregate to form secondary particles, which contributes to improving the cycle stability of the negative electrode material.
[0082] In some embodiments, the carbon material comprises at least one of soft carbon, hard carbon, crystalline carbon, and amorphous carbon.
[0083] In one possible embodiment, the metal oxide comprises at least one of titanium oxide, aluminum oxide, lithium oxide, cobalt oxide and vanadium oxide.
[0084] In one possible embodiment, the nitride comprises at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride and carbon nitride.
[0085] In some embodiments, the thickness of the coating layer is 1 nm to 500 nm. Specifically, the thickness of the coating layer may be 1 nm, 5 nm, 10 nm, 30 nm, 50 nm, 80 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, etc., and of course may be other values within the above range and is not limited thereto.
[0086] The present application further provides a method for producing the above-mentioned negative electrode material, as shown in FIG. grinding the mixed material including the primary particles and the adhesive to obtain a precursor; heat treating the precursor to carbonize the adhesive to obtain a heat treated product; The heat treatment product is pulverized and classified to obtain secondary particles that satisfy the following relationship with the primary particles, thereby obtaining a negative electrode material: 10≦D2 50 / D1 max ≦40(I) D2 min / D2 50 ≧0.08 (II) D2 50 / D2 max ≧0.24 (III) In formulas (I), (II) and (III), D1 max is the maximum particle size of the primary particles, and D2 50 is the median diameter of the secondary particles, and D2 min is the minimum particle size of secondary particles, and D2 max is the maximum particle size of the secondary particles.
[0087] In the above technical solution, the present application uses a mixed material of primary particles and adhesive as raw material to produce secondary particles, and through heat treatment, crushing and classification processes, the particle size distribution of the secondary particles is relatively concentrated and the particle size is appropriate, so that the primary particles and secondary particles in the present application have good consistency, thereby reducing the volume expansion of the negative electrode material and improving the structural stability and cycle performance of the negative electrode material.
[0088] The manufacturing method of the present application will be specifically described below.
[0089] In step 100, the mixed material including the primary particles and the adhesive is granulated to obtain a precursor.
[0090] In some embodiments, the median diameter of the primary particles is 0.2 μm or less, specifically, 1 nm, 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 60 nm, 80 nm, 100 nm, 130 nm, 150 nm, and 200 nm, etc., and of course, other values within the above ranges are also possible, and are not limited thereto. The median diameter of the primary particles is preferably 5 nm to 200 nm, and more preferably 10 nm to 200 nm. Currently, most of the negative electrode materials for secondary batteries are made by assembling / constructing primary particles into secondary particles by a specific means or method, and in this process, the morphological parameters and sizes of the primary particles and secondary particles are very important and determine the basic performance of the material. The present application selects primary particles of an appropriate size, and specifically selects raw materials with a median diameter of less than 0.2 μm, so that the particle size dimensions of the raw materials are close, and furthermore, secondary particles are constructed using primary particles with a close particle size dimension, so that the primary particles and secondary particles have good consistency, improving the electrochemical performance of the negative electrode material. If the particle size of the secondary particles produced is too large, the material will be loose, the structure will be unstable, and it will be prone to collapse and expand. If the particle size of the secondary particles produced is too small, the tap density of the material will be reduced, which is disadvantageous to improving the energy density of the material. In addition, if the particle size is too small, the specific surface area of the material will increase, and the initial efficiency of the material will be reduced.
[0091] In some embodiments, the mixed material of the primary particles and the adhesive further comprises a solvent, the solvent comprising at least one of phenol, an alcohol-based solvent, an ether-based solvent, and an alkane-based solvent, the alcohol-based solvent may be, for example, ethanol, ethylene glycol, glycerin, etc., the ether-based solvent may be, for example, ethyl ether, and the alkane-based solvent may be, for example, n-hexane, toluene, xylene, etc.
[0092] In some embodiments, the mass ratio of the solvent to the primary particles is 100:(5 - 40). Specifically, the mass ratio of the solvent to the primary particles can be 100:0.5, 100:10, 100:20, 100:30, 100:40, etc. Of course, other values within the above range are also possible and are not limited here.
[0093] In some embodiments, the primary particles contain at least one of Li, SiOx (0 < x < 2), Na, K, Sn, Ge, Si, Fe, Mg, Ti, Zn, Al, P, and Cu.
[0094] In some embodiments, the primary particles contain SiO x (0 < x < 2), specifically, SiO 0.1 , SiO 0.3 , SiO 0.5 , SiO 0.7 , SiO 0.8 , SiO1, SiO 1.2 , SiO 1.5 , SiO 1.8 or SiO 1.9 and so on, and of course, other particles within the above range are also possible and are not limited here.
[0095] In some embodiments, the sphericity of the primary particles > 0.7, preferably, the sphericity of the primary particles > 0.9. Since the sphericity of the primary particles is higher and the structure is more stable during the cycle process, the problem of crushing of material particles caused by the repeated formation of the SEI film can be avoided.
[0096] In some embodiments, the adhesive contains at least one of starch, cellulose, tannin, gum arabic, sodium alginate, styrene-butadiene rubber, butyl rubber, cellulose ester, ene-based polymer, polyamide, polyacrylate ester, epoxy resin, phenolic resin, furan resin, unsaturated polyester, acrylic resin, and polyimide.
[0097] In some embodiments, the mass ratio of the primary particles to the adhesive is 100:(5-55), specifically, the mass ratio of the primary particles to the adhesive is specifically 100:5, 100:10, 100:20, 100:30, 100:40, 100:55, etc., and of course may be other values within the above range and is not limited here.
[0098] In some embodiments, the method further includes dispersing the mixed material including the primary particles and the adhesive before granulating the mixed material including the primary particles and the adhesive. By dispersing the primary particles and the adhesive, the active material in the material can be dispersed, the active material can be prevented from agglomerating, and the active material can be dispersed into relatively small nanoparticles.
[0099] In some embodiments, the dispersion process includes at least one of magnetic stirring, mechanical stirring, abrasive dispersion, and ultrasonic dispersion.
[0100] Step S200: The precursor is heat-treated to carbonize the adhesive to obtain a heat-treated product.
[0101] In some embodiments, the method further comprises pre-grinding and pre-classifying the precursor prior to heat treating the precursor to carbonize the adhesive.
[0102] In some embodiments, prior to pre-grinding, the mixed material including the primary particles and the adhesive needs to be dried to facilitate the subsequent grinding process.
[0103] In some embodiments, the pre-grinding comprises at least one of mechanical grinding, airflow grinding, ultrafine grinding, wet grinding, extrusion grinding, and fracturing grinding.
[0104] In some embodiments, the median diameter of the material obtained after pre-pulverization is 0.5 μm to 20 μm, specifically, 0.5 μm, 1 μm, 2 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 20 μm, etc., and of course, other values within the above range are also possible, and are not limited here. The median diameter of the material obtained after pre-pulverization is preferably 1 μm to 15 μm, and more preferably 2 μm to 8 μm.
[0105] In some embodiments, the maximum particle size of the material obtained after pre-grinding is 5 μm to 45 μm, specifically, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, etc., and of course, other values within the above range are also possible, and are not limited here. The maximum particle size of the material obtained after pre-grinding is preferably 5 μm to 35 μm, and more preferably 6 μm to 30 μm.
[0106] In the present application, the median size and maximum particle size of the particles after pre-milling are limited, thereby making the particle size of the particles after milling relatively uniform.
[0107] In some embodiments, the particle size of the material obtained by pre-classification is greater than 0.5 μm, i.e., the classification process removes particles with a particle size of 0.5 μm or less to improve the uniformity of the particle size distribution of the active material in the material.
[0108] In some embodiments, the method further includes a step of fusing the precursor and the coating material prior to the step of heat treating the precursor to carbonize the adhesive, the fusing being understood to be performed after the pre-grinding and pre-classification steps.
[0109] In some embodiments, the coating material includes at least one of a carbon source, graphene, silicon carbide, a metal oxide, and a nitride.
[0110] In some embodiments, the carbon source comprises at least one of sucrose, glucose, polyethylene, polyvinyl alcohol, polyethylene glycol, polyaniline, epoxy resin, phenolic resin, furfural resin, acrylic resin, polyethylene oxide, polyvinylidene fluoride, polyacrylonitrile, polyvinyl chloride, and asphalt.
[0111] In one possible embodiment, the coating layer comprises a metal oxide, the metal oxide comprising at least one of titanium oxide, aluminum oxide, lithium oxide, cobalt oxide and vanadium oxide.
[0112] In one possible embodiment, the coating layer comprises a nitride, the nitride comprising at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride and carbon nitride.
[0113] In some embodiments, the equipment for the blending process includes at least one of a mechanical blender, a blender agitator, and a convection blender.
[0114] In some embodiments, the fusion treatment time is 30 min to 150 min. Specifically, the fusion treatment time may be 30 min, 50 min, 70 min, 90 min, 100 min, 110 min, 130 min, 150 min, etc., but of course may be other values within the above range and is not limited thereto.
[0115] In some embodiments, the cutter gap of the fusion process is 0.1 cm to 0.5 cm, specifically, the cutter gap of the fusion process may be 0.1 cm, 0.2 cm, 0.3 cm, 0.4 cm, 0.5 cm, etc., and of course, may be other values within the above range and is not limited thereto.
[0116] In some embodiments, the heat treatment temperature is 500°C to 1000°C. Specifically, the heat treatment temperature may be 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, etc., and of course, may be other values within the above range and is not limited thereto.
[0117] In some embodiments, the heat treatment is performed for a period of time ranging from 30 minutes to 900 minutes. Specifically, the heat treatment may be performed for a period of time ranging from 30 minutes, 60 minutes, 120 minutes, 360 minutes, 480 minutes, 720 minutes, 800 minutes, 900 minutes, etc., but may of course be any other value within the above range and is not limited thereto.
[0118] In some embodiments, the heat treatment is performed in a protective atmosphere, the protective atmosphere comprising any of nitrogen gas, argon gas, and helium gas.
[0119] Step S300: The heat treatment product is pulverized and classified to obtain secondary particles that satisfy the following relationship with the primary particles, thereby obtaining a negative electrode material. 10≦D2 50 / D1 max ≦40(I) D2 min / D2 50 ≧0.08 (II) D2 50 / D2 max ≧0.24 (III)
[0120] In some embodiments, the milling comprises at least one of mechanical milling, airflow milling, ultrafine milling, wet milling, extrusion milling, and cracking milling.
[0121] In some embodiments, the median diameter of the material obtained by pulverization is 0.5 μm to 15 μm, specifically, 0.5 μm, 1 μm, 2 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, etc., and of course, other values within the above range are also possible, and are not limited here. The median diameter of the material obtained by pulverization is preferably 1 μm to 13 μm, and more preferably 2 μm to 10 μm.
[0122] In some embodiments, the maximum particle size of the material obtained by pulverization is 5 μm to 45 μm, specifically, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, etc., and of course, other values within the above range are also possible, and are not limited here. The maximum particle size of the material obtained by pulverization is preferably 5 μm to 40 μm, and more preferably 6 μm to 30 μm.
[0123] In some embodiments, the method further includes removing particles having a particle size of 0.5 μm or less from the material obtained by the classification process after the classification process, where the material having a particle size of 0.5 μm or less is fine particles, and it is understood that removing the fine particles reduces the expansion difference between different particles in the material and improves the stability of the composite material for application in secondary batteries.
[0124] In some embodiments, 10≦D2 50 / D1 max ≦40, specifically, D2 50 / D1 max may be 10, 15, 20, 25, 30, 35, 40, etc., and may of course be other values within the above range, and are not limited thereto. Within the above range, the particle size of the primary particles and the secondary particles is appropriate, the degree of matching between the primary particles and the secondary particles is high, and the primary particles in the secondary particles are densely stacked, so that the particles in the negative electrode material are not easily powdered, and the stress caused by expansion during the charge and discharge process can be well released, the cycle performance of the material can be improved, and the expansion can be suppressed. The maximum value D1 of the primary particles maxIf D1 is too large, the adhesion between particles is small, powdering is likely to occur, cycle performance is reduced, and the maximum value D1 of the primary particles max If is too small, the interparticle interaction force will be strong, the interparticle adhesion will be strong, and secondary particles with too large a size will be easily formed. Secondary particles with too large a size will have difficulty in releasing the stress caused by expansion during the charge and discharge process, and the secondary particles will fall off the current collector or the current collector will be destroyed, resulting in a decrease in the performance of the negative electrode material.
[0125] In some embodiments, D2 min / D2 50 ≧0.08, specifically, D2 min / D2 50 may be 0.08, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, etc., and may of course be other values within the above range, and are not limited here. Within the above limited range, the number of fine powders in the secondary particles is small, the distribution of the content of the active ingredient in the material is relatively uniform, the expansion difference between the secondary particles can be reduced, and the structural stability of the material can be improved.
[0126] In some embodiments, D2 50 / D2 max ≧0.24, specifically, D2 50 / D2 max may be 0.24, 0.28, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, etc., and may of course be other values within the above range, and are not limited here. In the above limited range, the particle size distribution of the secondary particles is concentrated and there are few large secondary particles, so that the volume expansion of the material can be effectively reduced and the cycle performance of the material can be improved.
[0127] The examples of the present application further disclose secondary batteries comprising the negative electrode materials described herein or prepared by the methods described herein. EXAMPLES
[0128] The embodiments of the present application are further described below by dividing them into several embodiments. However, the present application is not limited to the following specific embodiments. They may be modified as appropriate without changing the scope of the main claims.
[0129] Example 1
[0130] (1) Nanosilicon particles are measured by a bulk density tester and sieved by a MALVERN particle size measuring device to determine the median diameter D1 50 is 50 nm, D1 max = 155 nm, volume density 0.29 g / cm 3 of nanosilicon is obtained.
[0131] (2) The nanosilicon obtained in step (1) and polyvinyl alcohol are added to phenol in a mass ratio of 100:28, then ball milled in a planetary ball mill for 2 hours, and rotary evaporated to dryness at 120°C to obtain a first precursor.
[0132] (3) The second precursor is obtained by pre-pulverizing and pre-classifying the first precursor, and has a median diameter of 7.1 μm and a maximum particle size of 23.8 μm.
[0133] (4) The second precursor and the phenolic resin are mixed in a mass ratio of 50:35, and then fusion processing is performed. The fusion time is 40 minutes, and the cutter gap is 0.1 cm. Then, the fused material is placed in a high-temperature box furnace, nitrogen gas is introduced, and the material is heat-treated at 820°C and kept warm for 4 hours.
[0134] (5) The material obtained in step (4) is pulverized and classified to obtain the negative electrode material.
[0135] The negative electrode material produced in this embodiment includes a carbon material and secondary particles dispersed in the carbon material, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nanosilicon particles, and the median diameter D2 of the negative electrode material is 50 is 3.6μm, and the minimum particle size D2 min is 0.6 μm, and the maximum particle size D2max is 10.8 μm, and the sphericity of the negative electrode material is 0.89.
[0136] As shown in FIG. 2, which is the SEM chart of the negative electrode material prepared in Example 1 of the present application, it can be clearly seen that the size distribution of the secondary particles is relatively uniform.
[0137] As shown in FIG. 3, which is the XRD chart of the negative electrode material prepared in Example 1 of the present application, it is clearly shown that the product contains a silicon peak position.
[0138] As shown in FIG. 4, which is the initial charge-discharge curve of the negative electrode material prepared in Example 1 of the present application, it is clear that the initial charge-discharge capacity of the negative electrode material is high and the initial efficiency is also high.
[0139] As shown in FIG. 5, which is the cycle performance curve of the negative electrode material prepared in Example 1 of the present application, it is clearly shown that the negative electrode material has excellent cycle performance, and the capacity retention rate after 100 cycles is 93.1%.
[0140] Example 2
[0141] (1) Nanosilicon particles were measured by a BET tester and sieved by a MALVERN particle size analyzer to determine the median diameter D1 50 is 20nm, D1 max = 103 nm, volume density 0.39 g / cm 3 Thus, nanosilicon having a molecular weight of 10 ... is obtained.
[0142] (2) The nanosilicon obtained in step (1) and fructose are added to ethylene glycol in a mass ratio of 100:48, then ball milled in a planetary ball mill for 62 hours, and rotary evaporated to dryness at 150°C to obtain a first precursor.
[0143] (3) The second precursor is obtained by pre-pulverizing and pre-classifying the first precursor, and has a median diameter of 3.5 μm and a maximum particle size of 10.8 μm.
[0144] (4) The second precursor and glucose are mixed in a mass ratio of 50:35, and then fusion is performed, the fusion time is 30 min, and the cutter gap is 0.15 cm. The mixed material is then placed in a high-temperature box furnace, nitrogen gas is introduced, and the material is heat-treated at 820°C and kept warm for 4 hours.
[0145] (4) The obtained sample is crushed and classified to obtain the negative electrode material.
[0146] The negative electrode material produced in this embodiment includes a carbon material and secondary particles dispersed in the carbon material, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nanosilicon particles, and the median diameter D2 of the negative electrode material is 50 is 1.8μm, and the minimum particle size D2 min is 0.32μm, and the maximum particle size D2 max is 5.8 μm, and the sphericity of the negative electrode material is 0.83.
[0147] Example 3
[0148] (1) Nanosilicon particles were measured by a BET tester and sieved by a MALVERN particle size analyzer to determine the median diameter D1 50 is 20nm, D1 max = 111 nm, volume density 0.14 g / cm 3 Thus, nanosilicon having a formula:
[0149] (2) The nanosilicon obtained in step (1) and fructose are put into ethylene glycol in a mass ratio of 100:58, then ball milled in a planetary ball mill for 9 hours, and the first precursor is rotary evaporated to dryness at 150°C.
[0150] (3) The second precursor is obtained by pre-pulverizing and pre-classifying the first precursor, and has a median diameter of 8.3 μm and a maximum particle size of 16.8 μm.
[0151] (4) The second precursor and asphalt are mixed in a mass ratio of 45:35, and then fusion treatment is performed, the fusion time is 60 minutes, and the cutter gap is 0.15 cm. The mixed material is then placed in a high-temperature box furnace, nitrogen gas is introduced, and the material is heat-treated at 920°C and kept warm for 4 hours.
[0152] (5) The material obtained in step (4) is crushed and classified to obtain the negative electrode material.
[0153] The negative electrode material produced in this embodiment includes a carbon material and secondary particles dispersed in the carbon material, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nanosilicon particles, and the median diameter D2 of the negative electrode material is 50 is 4.3μm, and the minimum particle size D2 min is 0.78μm, and the maximum particle size D2 max is 14.5 μm, and the sphericity of the negative electrode material is 0.92.
[0154] Example 4
[0155] (1) Nanosilicon particles were measured by a BET tester and sieved by a MALVERN particle size analyzer to determine the median diameter D1 50 is 100 nm, D1 max = 249 nm, volume density 0.59 g / cm 3 Thus, nanosilicon having a formula:
[0156] (2) The nanosilicon obtained in step (1) and asphalt are put into butanol in a mass ratio of 90:48, then ball milled in a planetary ball mill for 4 hours, and rotary evaporated to dryness at 150°C to obtain a first precursor.
[0157] (3) The second precursor is obtained by pre-pulverizing and pre-classifying the first precursor, and has a median diameter of 11.3 μm and a maximum particle size of 20.7 μm.
[0158] (4) The second precursor and graphene are mixed in a mass ratio of 40:25, and then fusion is performed. The fusion time is 20 min, and the cutter gap is 0.25 cm. The mixed material is then placed in a high-temperature box furnace, nitrogen gas is introduced, and the material is heat-treated at 950 °C and kept warm for 6 hours.
[0159] (5) The material obtained in step (4) is crushed and classified to obtain the negative electrode material.
[0160] The negative electrode material produced in this embodiment includes secondary particles and graphene layers located on the surfaces of the secondary particles, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nanosilicon particles, and the median diameter D2 of the negative electrode material is 50 is 8.2μm, and the minimum particle size D2 min is 1.08μm, and the maximum particle size D2 max is 16.5 μm, and the sphericity of the negative electrode material is 0.95.
[0161] Example 5
[0162] (1) Nanosilicon particles were measured by a BET tester and sieved by a MALVERN particle size analyzer to determine the median diameter D1 50 30nm, D1 max = 115 nm, volume density 0.25 g / cm 3 Thus, nanosilicon having a formula:
[0163] (2) The nanosilicon obtained in step (1) and asphalt are put into isopropanol in a mass ratio of 90:48, then ball milled in a planetary ball mill for 4 hours, and freeze-dried at -40°C to obtain a first precursor.
[0164] (3) The second precursor is obtained by pre-pulverizing and pre-classifying the first precursor, and has a median diameter of 5.9 μm and a maximum particle size of 15 μm.
[0165] (4) The second precursor and polyethylene glycol are mixed in a mass ratio of 40:25, and then fusion is performed, the fusion time is 50 minutes, and the cutter gap is 0.15 cm. The mixed material is then placed in a high-temperature box furnace, nitrogen gas is introduced, and the material is heat-treated at 950°C and kept at that temperature for 4 hours.
[0166] (5) The material obtained in step (4) is crushed and classified to obtain the negative electrode material.
[0167] The negative electrode material produced in this embodiment includes a carbon material and secondary particles dispersed in the carbon material, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nanosilicon particles, and the median diameter D2 of the negative electrode material is 50 is 4.2μm, and the minimum particle size D2 min is 0.68μm, and the maximum particle size D2 max is 10.5 μm, and the sphericity of the negative electrode material is 0.86.
[0168] Example 6
[0169] (1) Nanosilicon particles were measured by a BET tester and sieved by a MALVERN particle size analyzer to determine the median diameter D1 50 is 150 nm, D1 max = 314 nm, volume density 0.68 g / cm 3 Thus, nanosilicon having a formula:
[0170] (2) The nanosilicon obtained in step (1) and glucose are put into propanol in a mass ratio of 80:68, then ball milled in a planetary ball mill for 4 hours, and rotary evaporated to dryness at 150°C to obtain a first precursor.
[0171] (3) The second precursor is obtained by pre-pulverizing and pre-classifying the first precursor, and has a median diameter of 5.8 μm and a maximum particle size of 9.8 μm.
[0172] (4) The second precursor and titanium nitride are mixed in a mass ratio of 60:55, and then fusion is performed, the fusion time is 40 minutes, and the cutter gap is 0.1 cm. The mixed material is then placed in a high-temperature box furnace, nitrogen gas is introduced, and the material is heat-treated at 750°C and kept at that temperature for 4 hours.
[0173] (5) The material obtained in step (4) is crushed and classified to obtain the negative electrode material.
[0174] The negative electrode material produced in this embodiment includes secondary particles and a titanium nitride layer located on the surface of the secondary particles, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nanosilicon particles, and the median diameter D2 of the negative electrode material is 1. 50 is 3.2μm, and the minimum particle size D2 min is 0.57μm, and the maximum particle size D2 max is 8.9 μm, and the sphericity of the negative electrode material is 0.78.
[0175] Example 7
[0176] (1) Nanosilicon particles were measured by a BET tester and sieved by a MALVERN particle size analyzer to determine the median diameter D1 50 180nm, D1 max = 478 nm, volume density 0.70 g / cm 3 Thus, nanosilicon having a formula:
[0177] (2) The nanosilicon obtained in step (1) and glucose are put into propanol in a mass ratio of 60:48, then ball milled in a planetary ball mill for 4 hours, and rotary evaporated to dryness at 150°C to obtain a first precursor.
[0178] (3) The second precursor is obtained by pre-pulverizing and pre-classifying the first precursor, and has a median diameter of 12.1 μm and a maximum particle size of 20.8 μm.
[0179] (4) The second precursor and silicon carbide are mixed in a mass ratio of 65:35, and then fusion is performed, the fusion time is 80 min, and the cutter gap is 0.15 cm. The mixed material is then placed in a high-temperature box furnace, nitrogen gas is introduced, and the material is heat-treated at 850°C and kept at that temperature for 4 hours.
[0180] (5) The material obtained in step (4) is crushed and classified to obtain the negative electrode material.
[0181] The negative electrode material produced in this embodiment includes secondary particles and a silicon carbide layer located on the surface of the secondary particles, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nanosilicon particles, and the median diameter D2 of the negative electrode material is 50 is 9.0μm, and the minimum particle size D2 min is 1.57μm, and the maximum particle size D2 max is 17.8 μm, and the sphericity of the negative electrode material is 0.76.
[0182] Example 8
[0183] The difference from Example 1 is step (4): the second precursor and the phenolic resin are mixed in a mass ratio of 50:35, and then the resulting material is placed in a high-temperature box furnace, nitrogen gas is introduced, and the material is heat-treated at 820°C and kept at that temperature for 4 hours.
[0184] The negative electrode material produced in this embodiment includes a carbon material and secondary particles dispersed in the carbon material, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nanosilicon particles, and the median diameter D2 of the negative electrode material is 50 is 4.9μm, and the minimum particle size D2 min is 0.39 μm, and the maximum particle size D2 max is 18.4 μm, and the sphericity of the negative electrode material is 0.94.
[0185] Example 9
[0186] The difference from Example 1 is that the nanosilicon particles are replaced with nanogermanium particles, of which the D1 50 30nm, D1 max = 220 nm, bulk density 0.26 g / cm 3 It is.
[0187] The negative electrode material produced in this embodiment includes a carbon material and secondary particles dispersed in the carbon material, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nano-germanium particles, and the median diameter D2 of the negative electrode material is 100 nm. 50 is 3.5μm, and the minimum particle size D2 min is 0.3 μm, and the maximum particle size D2 max is 12.5 μm, and the sphericity of the negative electrode material is 0.88.
[0188] Example 10
[0189] The difference from Example 1 is that the nanosilicon particles are replaced with nanotin particles, of which the D1 50 28nm, D1 max = 185 nm, bulk density 0.25 g / cm 3 It is.
[0190] The negative electrode material produced in this embodiment includes a carbon material and secondary particles dispersed in the carbon material, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nano-tin particles, and the median diameter D2 of the negative electrode material is 100 nm. 50 is 3.6μm, and the minimum particle size D2 min is 0.4μm, and the maximum particle size D2 max is 10.9 μm, and the sphericity of the negative electrode material is 0.89.
[0191] Example 11
[0192] The difference from Example 1 is that the phenolic resin in step (4) is replaced with silicon nitride.
[0193] The negative electrode material produced in this embodiment includes secondary particles, and the surfaces of the secondary particles include a silicon nitride coating layer. The secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer. The primary particles include nanosilicon particles, and the median diameter D2 of the negative electrode material is 1. 50 is 3.4μm, and the minimum particle size D2 min is 0.5 μm, and the maximum particle size D2 max is 11.7 μm, and the sphericity of the negative electrode material is 0.91.
[0194] Example 12
[0195] The difference from Example 1 is step (2), in which the nanosilicon obtained in step (1) and polyvinyl alcohol are added to phenol in a mass ratio of 100:28, and the mixture is rotary evaporated and dried at 120°C to obtain a first precursor.
[0196] The negative electrode material produced in this embodiment includes a carbon material and secondary particles dispersed in the carbon material, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nanosilicon particles, and the median diameter D2 of the negative electrode material is 50 is 6.0μm, and the minimum particle size D2 min is 0.82μm, and the maximum particle size D2 max is 22.2 μm, and the sphericity of the negative electrode material is 0.52.
[0197] Example 13
[0198] The difference from Example 1 is that the nanosilicon particles are replaced with nano-SiO particles, and the D1 of the nano-SiO particles is 50 is 80nm, D1 max = 320 nm, bulk density 0.36 g / cm 3 It is.
[0199] The negative electrode material produced in this embodiment includes a carbon material and secondary particles dispersed in the carbon material, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nano-SiO particles, and the median diameter D2 of the negative electrode material is 100 nm. 50 is 4.5μm, and the minimum particle size D2 min is 0.4μm, and the maximum particle size D2 max is 13.5 μm, and the sphericity of the negative electrode material is 0.93.
[0200] Comparative Example 1
[0201] (1) By sieving the nanosilicon particles, the median diameter D1 50 obtains 300 nm nanosilicon.
[0202] (2) The nanosilicon and polyvinyl alcohol obtained in step (1) are added to phenol in a mass ratio of 100:28, then ball milled in a planetary ball mill for 2 hours, and rotary evaporated to dryness at 120°C to obtain a first precursor.
[0203] (3) The second precursor is obtained by pre-pulverizing and pre-classifying the first precursor, and has a median diameter of 7.1 μm and a maximum particle size of 23.8 μm.
[0204] (4) The second precursor and the phenolic resin are mixed in a mass ratio of 50:35, and then the fusion process is carried out. The fusion time is 40 minutes, and the cutter gap is 0.1 cm. Then, the fused material is placed in a high-temperature box furnace, nitrogen gas is introduced, and the material is heat-treated at 820°C and kept warm for 4 hours.
[0205] (5) The material obtained in step (4) is crushed and classified to obtain the negative electrode material.
[0206] The negative electrode material produced in this comparative example includes a carbon material and secondary particles dispersed in the carbon material, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nanosilicon particles, and the median diameter D2 50is 7.2μm, and the minimum particle size D2 min is 0.42μm, and the maximum particle size D2 max is 33.8 μm, and the sphericity of the negative electrode material is 0.89.
[0207] Comparative Example 2
[0208] The difference from Example 1 is that the crushing and classification treatments were not carried out.
[0209] The negative electrode material produced in this comparative example includes a carbon material and secondary particles dispersed in the carbon material, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nanosilicon particles, and the median diameter D2 50 is 5.2μm, and the minimum particle size D2 min is 0.31 μm, and the maximum particle size D2 max is 33.8 μm, and the sphericity of the negative electrode material is 0.67.
[0210] Comparative Example 3
[0211] The difference from Example 1 is that the primary particles D1 used max is 0.3 μm.
[0212] The negative electrode material produced in this comparative example includes a carbon material and secondary particles dispersed in the carbon material, the secondary particles include aggregated primary particles, and the surfaces of the primary particles have a carbon material coating layer, the primary particles include nanosilicon particles, and the negative electrode material D2 50 = 2μm, D2 min =0.3μm, D2 max = 15 μm, and the sphericity of the negative electrode material is 0.67.
[0213] Test Method: 1. The median diameter, minimum particle size and maximum particle size of the material are measured using a Malvern particle size analyzer, and the measurement standard is ISO13320:2009. 2. The material bulk density is measured using BET test, and the measurement standard is GB / T11107-2018. 3. Use a specific surface area tester to measure the specific surface area of the material. 4. Measure the porosity of the material using the static volume method or mercury intrusion method. 5. Use a particle sphericity analyzer to measure the sphericity of the material. 6. Measure the electrochemical cycle performance as follows:
[0214] The negative electrode material, conductive agent and adhesive are dissolved and mixed in water with a mass percentage of 94:1:5, the solid content is controlled to 50%, coated on a copper foil current collector, and vacuum dried to produce a negative electrode sheet. Then, the ternary positive electrode sheet (lithium nickel manganese cobalt oxide NCM523) produced by conventional mature process, 1 mol / L lithium hexafluorophosphate LiPF6 / (ethylene carbonate EC + dimethyl carbonate DMC + ethyl methyl carbonate EMC) (v / v=1:1:1) electrolyte, Celgard2400 separator and shell are assembled into 18650 cylindrical battery cells by normal production process. The charge and discharge test of the cylindrical battery was performed using LAND battery test equipment from Wuhan Jinnuo electronics Co., Ltd., at room temperature, with constant current charging and discharging at 0.2C, and the charge and discharge voltage was limited to 2.75 to 4.2V, to obtain the initial reversible specific capacity and initial coulombic efficiency (ICE) of the battery. The charge and discharge test was repeated 100 times on the battery in the charge and discharge range of 0.01V to 5V at a current density of 1C, to obtain the capacity retention rate and thickness expansion rate of the pole piece after 50 cycles of the battery.
[0215] The test results are shown in Tables 1 and 2.
[0216] [Table 1]
[0217] [Table 2]
[0218] As shown in the data in Tables 1 and 2 above, the negative electrode materials, primary particles, and secondary particles produced in Examples 1 to 12 of the present application have a particle size distribution within a range of 10≦D2 50 / D1 max ≦40, D2 min / D2 50 ≧0.08, and D2 50 / D2 max ≧0.24, the primary particles and the secondary particles have good consistency, and finally the fine powder in the negative electrode material is reduced, the particle size of the secondary particles is concentrated, the cycle stability of the negative electrode material is improved, and the volume expansion effect of the negative electrode material is reduced.
[0219] The negative electrode material produced in Comparative Example 1 had nanosilicon particles that were too large, which reduced the adhesion between the primary particles, increased the volume expansion of the negative electrode material, increased the burst rate of secondary particles during charging and discharging, and reduced the cycle capacity retention rate.
[0220] The negative electrode material produced in Comparative Example 2 was not subjected to pulverization or classification treatment, and therefore the particle size distribution of the negative electrode material was wide, a certain amount of fine powder was present, and the volume expansion of the material was large.
[0221] The negative electrode material produced in Comparative Example 3 was D2 50 , D1 max , D2 max and D2 min All of the single parameters are within the preferred range, but 10≦D2 50 / D1 max ≦40, D2 50 / D2 max ≧0.24 is not satisfied, and the volume expansion of the negative electrode material is large.
[0222] The above is only a preferred embodiment of the present application, and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and changes. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present application should be included in the protection scope of the present application.
Claims
1. 1. A negative electrode material comprising: a negative electrode material including secondary particles, the secondary particles including aggregated primary particles, and the primary particles and the secondary particles satisfy the following relationship: 10≦D2 50 / D1 max ≦40 (I) <h2 style=";text-align:left;direction:ltr">12<h2 style=";text-align:left;direction:ltr"> min <h2 style=";text-align:left;direction:ltr"> 12<h2 style=";text-align:left;direction:ltr"> 50 <h2 style=";text-align:left;direction:ltr"> ≧0.08 (II) D2 50 / D2 max ≧0.24 (III) (In formulas (I), (II) and (III), D1 max is the maximum particle size of the primary particles, and D2 50 is the median diameter of the secondary particles, and D2 min is the minimum particle size of secondary particles, and D2 max is the maximum particle size of the secondary particles.)
2. The negative electrode material according to claim 1, characterized in that it satisfies at least one of the following characteristics (1) to (7). (1) The primary particles contain at least one of Li, Na, SiOx (0<x<2), K, Sn, Ge, Si, Fe, Mg, Ti, Zn, Al, P, and Cu; (2) The bulk density of the primary particles is 0.7 g / cm 3 That is: (3) Median diameter D1 of the primary particles 50 is 0.2 μm or less; (4) The median diameter D2 of the secondary particles 50 The range is 0.5 μm to 20 μm; (5) Maximum particle size D1 of the primary particles max The range is 0.1 μm to 0.4 μm; (6) The minimum particle size D2 of the secondary particles min The range is 0.5 μm to 4 μm; (7) The maximum particle size D2 of the secondary particles max The range is 6 μm to 20 μm.
3. The negative electrode material according to claim 1, characterized in that the negative electrode material satisfies at least one of the following characteristics (1) to (3). (1) The specific surface area of the negative electrode material is 10 m 2 / g or less, (2) the porosity of the negative electrode material is 10% or less; (3) The sphericity of the negative electrode material is 0.7 or more.
4. 2. The negative electrode material according to claim 1, further comprising a coating layer present on at least a portion of a surface of the primary particles and / or the secondary particles.
5. The negative electrode material according to claim 4, wherein the coating layer satisfies at least one of the following (1) to (2): (1) The coating layer includes at least one of a carbon material, graphene, silicon carbide, a metal oxide, and a nitride; (2) The coating layer includes a carbon material, and the carbon material includes at least one of soft carbon, hard carbon, crystalline carbon, and amorphous carbon; (3) The coating layer contains a metal oxide, and the metal oxide contains at least one of titanium oxide, aluminum oxide, lithium oxide, cobalt oxide, and vanadium oxide; (4) The coating layer includes a nitride, and the nitride includes at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride, and carbon nitride; (5) The thickness of the coating layer is 1 nm to 500 nm.
6. A step of granulating a mixed material including the primary particles and the adhesive to obtain a precursor; heat treating the precursor to carbonize the adhesive to obtain a heat treated product; and crushing and classifying the heat-treated product to obtain secondary particles that satisfy the following relationship with the primary particles, thereby obtaining a negative electrode material. 10≦D2 50 / D1 max ≦40 (I) <h2 style=";text-align:left;direction:ltr">12<h2 style=";text-align:left;direction:ltr"> min <h2 style=";text-align:left;direction:ltr"> 12<h2 style=";text-align:left;direction:ltr"> 50 <h2 style=";text-align:left;direction:ltr"> ≧0.08 (II) D2 50 / D2 max ≧0.24 (III) (In formulas (I), (II) and (III), D1 max is the maximum particle size of the primary particles, and D2 50 is the median diameter of the secondary particles, and D2 min is the minimum particle size of secondary particles, and D2 max is the maximum particle size of the secondary particles.)
7. The method according to claim 6, characterized in that it comprises at least one of the following features (1) to (15): (1) the median diameter of the primary particles is 0.2 μm or less; (2) The primary particles contain at least one of Li, SiOx (0<x<2), Na, K, Sn, Ge, Si, Fe, Mg, Ti, Zn, Al, P, and Cu; (3) The adhesive contains at least one of starch, cellulose, tannin, gum arabic, sodium alginate, styrene-butadiene rubber, butyl rubber, cellulose ester, ene-based polymer, polyamide, polyacrylic acid ester, epoxy resin, phenolic resin, furan resin, unsaturated polyester, acrylic resin, and polyimide; (4) the mass ratio of the primary particles to the adhesive is 100:(5 to 55); (5) The mixture of the primary particles and the adhesive further contains a solvent; (6) The mixed material of the primary particles and the adhesive further contains a solvent, and the solvent contains at least one of phenol, an alcohol-based solvent, an ether-based solvent, and an alkane-based solvent; (7) The mixed material of the primary particles and the adhesive further contains a solvent, and the mass ratio of the solvent to the primary particles is 100:(5 to 40); (8) The method further includes dispersing the mixed material including the primary particles and the adhesive before the step of granulating the mixed material including the primary particles and the adhesive; (9) The method further includes dispersing the mixed material including the primary particles and the adhesive before the step of granulating the mixed material including the primary particles and the adhesive, and the dispersion treatment includes at least one of magnetic stirring, mechanical stirring, abrasive dispersion, and ultrasonic dispersion; (10) The temperature of the heat treatment is 500° C. to 1000° C.; (11) The heat retention time of the heat treatment is 30 minutes to 900 minutes; (12) The heat treatment is performed in a protective atmosphere, and the protective atmosphere contains at least one of nitrogen gas, argon gas, and helium gas; (13) The median diameter of the material obtained by the pulverization is 0.5 μm to 15 μm; (14) The maximum particle size of the material obtained by pulverization is 5 μm to 45 μm; (15) The method further comprises, after the classification treatment, removing particles having a particle size of 0.5 μm or less from the material obtained by the classification treatment.
8. The method according to claim 6, characterized in that at least one of the following characteristics (1) to (5) is satisfied. (1) The method further includes pre-grinding and pre-classifying the precursor before the step of heat-treating the precursor to carbonize the adhesive; (2) The method further includes pre-grinding and pre-classifying the precursor before the step of heat-treating the precursor to carbonize the adhesive, and the pre-grinding includes at least one of mechanical grinding, airflow grinding, ultrafine powder grinding, wet grinding, extrusion grinding, and split grinding; (3) The method further includes pre-pulverizing and pre-classifying the precursor before the step of heat-treating the precursor to carbonize the adhesive, and the median diameter of the material obtained by the pre-pulverization is 0.5 μm to 20 μm; (4) The method further includes pre-pulverizing and pre-classifying the precursor before the step of heat-treating the precursor to carbonize the adhesive, and the maximum particle size of the material obtained by the pre-pulverization is 5 μm to 45 μm; (5) The method further includes pre-grinding and pre-classifying the precursor before the step of heat-treating the precursor to carbonize the adhesive, and the particle size of the material obtained by the pre-classification exceeds 0.5 μm.
9. The method according to claim 6, characterized in that at least one of the following characteristics (1) to (4) is satisfied. (1) The method further includes fusing the precursor and a coating material before the step of heat-treating the precursor to carbonize the adhesive; (2) before the step of heat-treating the precursor to carbonize the adhesive, the method further includes fusing the precursor with a coating material, the coating material including at least one of a carbon source, graphene, silicon carbide, a metal oxide, and a nitride; (3) The method further includes fusing the precursor with the coating material before the step of heat-treating the precursor to carbonize the adhesive, the coating material including a carbon source, the carbon source including at least one of sucrose, glucose, polyethylene, polyvinyl alcohol, polyethylene glycol, polyaniline, epoxy resin, phenolic resin, furfural resin, acrylic resin, polyethylene oxide, polyvinylidene fluoride, polyacrylonitrile, polyvinyl chloride, and asphalt; (4) The method further includes fusing the precursor with a coating material before the step of heat-treating the precursor to carbonize the adhesive, the coating material including a metal oxide, the metal oxide including at least one of titanium oxide, aluminum oxide, lithium oxide, cobalt oxide, and vanadium oxide; (5) The method further includes fusing the precursor with a coating material before the step of heat treating the precursor to carbonize the adhesive, the coating material including a nitride, the nitride including at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride, and carbon nitride; (6) The method further includes fusing the precursor and the coating material before the step of heat-treating the precursor to carbonize the adhesive, and the fusing device includes at least one of a mechanical fusing machine, a fusing stirrer, and a convection fusing machine; (7) The method further includes fusing the precursor and the coating material before the step of heat-treating the precursor to carbonize the adhesive, and the fusing time is 30 minutes to 150 minutes.
10. A secondary battery comprising the anode material according to any one of claims 1 to 5 or the anode material produced by the method according to any one of claims 6 to 9.
Citation Information
Patent Citations
Silicon-carbon negative electrode material, preparation method and lithium ion battery
CN109713280A
Graphite composite material as well as preparation method and application thereof
CN111682177A
Negative electrode material for non-aqueous electrolyte secondary battery and preparation method thereof
CN114068887A
Non-aqueous electrolyte secondary battery
JP2009259798A
Composite electrolyte, secondary battery, battery pack and vehicle
JP2018160445A