Cathode material, cathode and lithium secondary battery including same
A lithium nickel oxide-based positive electrode material with a controlled specific surface area and boron content, combined with a coating layer, addresses particle cracking issues, enhancing life characteristics and resistance in lithium secondary batteries.
Patent Information
- Application Number
- JP2024524731
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-03
- Filing Date
- 2022-11-02
- Publication Date
- 2024-10-31
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Lithium nickel cobalt manganese oxide-based positive electrode materials suffer from particle cracking during manufacturing, leading to increased contact with electrolyte, gas generation, and reduced life characteristics due to high specific surface area and side reactions.
A lithium nickel oxide-based positive electrode material with a specific surface area of 0.2 to 0.4 m^2/g, containing boron in the range of 500 to 1000 ppm, and a coating layer to minimize particle cracking and improve life characteristics.
The proposed material reduces particle cracking and maintains excellent life characteristics while minimizing resistance increase, achieving a balance between BET specific surface area and boron content.
Smart Images

Figure 2024539981000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0150057, filed on November 3, 2021, and all contents disclosed in the documents of said Korean patent application are incorporated herein by reference.
[0002] The present invention relates to a positive electrode material, a positive electrode including the same, and a lithium secondary battery, and more particularly to a positive electrode material having a small increase in initial resistance, excellent life characteristics, and small generation of fine powder during electrode production, and a positive electrode and a lithium secondary battery including the same. [Background technology]
[0003] A lithium secondary battery generally comprises a positive electrode, a negative electrode, a separator and an electrolyte, and the positive electrode and the negative electrode contain active materials capable of intercalating and deintercalating lithium ions.
[0004] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMnO4, etc.), lithium iron phosphate compound (LiFePO4), etc. have been used as positive electrode active materials for lithium secondary batteries. Among these, lithium cobalt oxide has the advantages of high operating voltage and excellent capacity characteristics, but the raw material cobalt is expensive and its supply is unstable, making it difficult to commercially apply it to large-capacity batteries. Lithium nickel oxide has poor structural stability and is difficult to achieve sufficient life characteristics. On the other hand, lithium manganese oxide has excellent stability but poor capacity characteristics. Therefore, in order to compensate for the problems of lithium transition metal oxides containing Ni, Co, or Mn alone, lithium composite transition metal oxides containing two or more transition metals have been developed, and lithium nickel cobalt manganese oxide containing Ni, Co, and Mn is widely used.
[0005] Lithium nickel cobalt manganese oxide generally has the form of spherical secondary particles formed by agglomeration of tens to hundreds of primary particles, but there is a problem that particle cracking occurs during the rolling process during the manufacture of the positive electrode, in which the primary particles of lithium nickel cobalt manganese oxide are separated. When particle cracking occurs in the positive electrode active material, the contact area with the electrolyte increases, gas generation due to side reactions with the electrolyte and deterioration of the active material increase, resulting in a problem of reduced life characteristics.
[0006] In order to improve the life characteristics of lithium nickel cobalt manganese oxide, a technique has been proposed in which a coating layer is formed on the surface of the lithium nickel cobalt manganese oxide to prevent contact with the electrolyte. However, this method has problems in that the effect of improving the life characteristics is insufficient and the initial resistance characteristics decrease as the thickness of the coating layer increases.
[0007] Therefore, there is a need for the development of a cathode material that generates less fine powder during rolling and can achieve excellent life characteristics. Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made to solve the above problems, and aims to provide a cathode material having a lower BET than conventional cathode materials, containing a specific content of boron (B), and exhibiting less particle cracking during electrode manufacturing and excellent life characteristics. [Means for solving the problem]
[0009] According to one embodiment, the present invention provides a cathode material including a cathode active material including a lithium nickel-based oxide having a molar fraction of nickel of 50 to 90 mol % among metal elements other than lithium, and a coating layer formed on the surface of the lithium nickel-based oxide and containing boron (B), the BET specific surface area of the cathode material being 0.2 to 0.4 m 2 / g, and the boron (B) is contained in an amount of 500 ppm to 1000 ppm relative to the total weight of the positive electrode material.
[0010] Here, the lithium nickel-based oxide may have a composition represented by the following [Chemical Formula 1]. [Chemical formula 1] Li x [Ni a Co b Mn c M 1 d ]O2 In the above [Chemical Formula 1], M 1 may be one or more selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta and Nb, and is preferably Zr; and 0.8≦x≦1.2, 0.5≦a≦0.9, 0 <b<0.5、0<c<0.5、0≦d≦0.2である。
[0011] Meanwhile, the Zr may be contained in an amount of 4000 ppm to 5000 ppm based on the total weight of the positive electrode material.
[0012] The coating layer may further include tungsten (W), and the tungsten (W) is preferably included in an amount of 4000 pm or less based on the total weight of the positive electrode material.
[0013] The positive electrode active material may have a crystalline grain size of 90 nm to 110 nm.
[0014] The positive electrode active material may be in the form of secondary particles formed by agglomeration of a large number of primary particles, and the primary particles may have an average particle size of 500 nm to 1 μm.
[0015] The cathode material may have a bimodal particle size distribution, specifically, an average particle size D 50 The large particle size of the positive electrode active material is 8 μm or more, and the average particle size D 50 The large particle size positive electrode active material and the small particle size positive electrode active material may be contained in a weight ratio of 9:1 to 6:4.
[0016] According to another embodiment, the present invention provides a positive electrode comprising the positive electrode material and a lithium secondary battery comprising the positive electrode. Effect of the Invention
[0017] The cathode material of the present invention has a BET specific surface area of 0.2 to 0.4 m 2 / g, which is lower than conventional materials, and contains boron (B) in an amount of 500 ppm to 1000 ppm. When the BET specific surface area and boron content of the positive electrode material simultaneously satisfy the ranges of the present invention, particle cracking during rolling of the positive electrode is reduced, and excellent life characteristics are exhibited. [Brief description of the drawings]
[0018] [Figure 1] 1 is a scanning electron microscope (SEM) image showing the surface shape of large particle diameter positive electrode active material particles prepared in Example 8. [Diagram 2] 1 is a scanning electron microscope (SEM) image showing a cross-sectional shape of a large particle size positive electrode active material particle prepared in Example 8. [Diagram 3] 1 is a scanning electron microscope (SEM) image showing the surface shape of large particle diameter positive electrode active material particles prepared in Comparative Example 11. [Figure 4] 1 is a scanning electron microscope (SEM) image showing a cross-sectional shape of a large particle size positive electrode active material particle prepared in Comparative Example 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will now be described in more detail.
[0020] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0021] In the present invention, the term "primary particle" refers to a particle unit that does not have grain boundaries when observed at a magnification of 5,000 to 20,000 using a scanning electron microscope. The term "average particle size of primary particles" refers to the arithmetic average value calculated after measuring the particle sizes of primary particles observed in a scanning electron microscope image.
[0022] In the present invention, the term "secondary particles" refers to particles formed by agglomeration of a plurality of primary particles.
[0023] In the present invention, the "average particle size D 50 " means the particle size at 50% of the volume cumulative particle size distribution of the positive electrode active material powder. 50 can be measured using a laser diffraction method. For example, the positive electrode active material powder is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), and ultrasonic waves of about 28 kHz are irradiated at an output of 60 W, and a volume cumulative particle size distribution graph is obtained, and the particle diameter corresponding to 50% of the volume cumulative amount is obtained.
[0024] In the present invention, the "grain size" can be quantitatively analyzed using X-ray diffraction analysis (XRD) using Cu Kα X-rays. Specifically, the average crystal size of the grains can be quantitatively analyzed by placing the particles to be measured in a holder, irradiating the particles with X-rays, and analyzing the diffraction grating output. Sampling was performed by placing a powder sample of the particles to be measured in a groove recessed in the center of a general powder holder, making the surface uniform using a slide glass, and preparing the sample at the same height as the edge of the holder. Then, X-ray diffraction analysis was performed using a Bruker D8 Endeavor (light source: CU Kα, λ=1.54Å) equipped with a LynxEye XE-T position sensitive detector under the conditions of FDS 0.5°, step size 0.02° for 2θ=15°~90° range, and total scan time of about 20 minutes. The measured data were subjected to Rietveld refinement, taking into account the charge at each site (metal ions at transition metal sites are +3, Ni ions at Li sites are +2) and cation mixing. When analyzing the grain size, instrumental brodding was taken into account using the Fundamental Parameter Approach (FPA) implemented in the Bruker TOPAS program, and the entire peak in the measurement range was used for fitting. The peak shape was fitted using only the Lorenzian contribution as FP (First Principle) among the peak types available in TOPAS, and strain was not considered here.
[0025] In the present invention, the "specific surface area" is measured by the BET method, and specifically, it can be calculated from the amount of nitrogen gas adsorption at liquid nitrogen temperature (77K) using BELSORP-mino II manufactured by BEL Japan.
[0026] In the present invention, the content of each component of the positive electrode active material can be measured by inductively coupled plasma mass spectrometry (ICP). Specifically, a sample to be measured is pretreated with an acid, and then measured using an ICP-OES (PerkinElmer, Optima7300DV) device.
[0027] Cathode material The cathode material according to the present invention will now be described.
[0028] The cathode material according to the present invention is a cathode material comprising a cathode active material including a lithium nickel-based oxide in which the molar fraction of nickel among metal elements other than lithium is 50 to 90 mol %, and a coating layer containing boron (B) formed on the surface of the lithium nickel-based oxide, and the BET specific surface area of the cathode material is 0.2 to 0.4 m 2 / g, and the boron (B) is contained in an amount of 500 ppm to 1000 ppm with respect to the total weight of the positive electrode material.
[0029] Conventionally, lithium nickel oxide has been used as a positive electrode active material, and generally has a 0.5m 2 / g~1.5m 2 The positive electrode active material has a specific surface area of about 0.2 to 0.4 m2 / g. Such a conventional positive electrode active material has high internal porosity and excellent resistance characteristics, but has problems in that particles are easily broken during electrode production, resulting in a large amount of fine powder, and side reactions with the electrolyte are frequent, resulting in poor life characteristics. Reducing the specific surface area of the positive electrode active material reduces particle cracking and improves life characteristics, but increases initial resistance, resulting in reduced output characteristics and initial capacity characteristics. The present inventors have conducted extensive research to solve these problems and have found that a specific surface area of the positive electrode material powder can be reduced to 0.2 to 0.4 m2. 2 The inventors have found that when a cathode material containing a specific amount of boron is used while reducing the amount of boron in the cathode to a level of 0.1 g, the increase in resistance can be minimized and particle cracking during rolling of the cathode and life characteristics can be improved, leading to the completion of the present invention.
[0030] Specifically, the positive electrode material according to the present invention includes a positive electrode active material including a lithium nickel-based oxide and a coating layer containing boron (B) formed on the surface of the lithium nickel-based oxide.
[0031] The lithium nickel-based oxide may be a lithium nickel cobalt manganese-based oxide in which the molar fraction of nickel among metal elements other than lithium is 50 to 90 mol %, preferably 60 to 90 mol %, and more preferably 65 to 85 mol %.
[0032] More specifically, the lithium nickel-based oxide may have a composition represented by the following [Chemical Formula 1].
[0033] [Chemical formula 1] Li x [Ni a Co b Mn c M 1 d ]O2
[0034] In the above [Chemical Formula 1], M 1 is one or more selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta and Nb, preferably one or more selected from the group consisting of Zr, Y, Mg and Ti, and more preferably Zr. 1 Although the element is not necessarily included, when included in an appropriate amount, it can play a role in promoting grain growth during firing or improving the stability of the crystal structure.
[0035] The x represents the molar ratio of lithium in the lithium nickel-based oxide and may be 0.8≦x≦1.2, 0.9≦x≦1.1, or 1≦x≦1.1.
[0036] The a represents a molar ratio of nickel among metals other than lithium in the lithium nickel-based oxide, and may be 0.5≦a≦0.9, 0.6≦a≦0.9, 0.65≦a≦0.85, or 0.65≦a≦0.80.
[0037] The b represents the molar ratio of cobalt among the metals other than lithium in the lithium nickel-based oxide, and is 0 <b<0.5、0.01≦b≦0.4、0.01≦b≦0.3、または0.05≦b≦0.2であることができる。
[0038] The c represents the molar ratio of manganese among metals other than lithium in the lithium nickel-based oxide, and is 0 <c<0.5、0.01≦c≦0.4、0.05≦c≦0.4、または0.1≦b≦0.4であることができる。
[0039] The d is M among the metals other than lithium in the lithium nickel-based oxide. 1 It denotes the molar ratio of the elements and can be 0≦d≦0.2 or 0≦d≦0.1.
[0040] Preferably, the lithium nickel-based oxide may be a lithium nickel cobalt manganese oxide doped with Zr. When Zr is doped, the effect of suppressing particle cracking during electrode rolling is more excellent. Here, the Zr may be included in an amount of 3000 ppm to 6000 ppm, preferably 3500 ppm to 5500 ppm, more preferably 4000 ppm to 5000 ppm based on the total weight of the positive electrode material. When the Zr content satisfies the above range, the capacity reduction can be minimized and particle cracking can be effectively suppressed.
[0041] Next, the coating layer is formed on the surface of the lithium nickel-based oxide and contains boron (B). When a coating layer containing boron (B) is formed on the surface of the lithium nickel-based oxide, the coating layer minimizes contact between the electrolyte and the lithium nickel-based oxide, suppressing the occurrence of side reactions between the electrolyte and the lithium nickel-based oxide and the elution of transition metals, thereby improving the life characteristics and reducing particle cracking during rolling.
[0042] Here, the boron (B) is contained in an amount of 500 ppm to 1000 ppm based on the total weight of the positive electrode material. If the boron (B) content is out of this range, the life characteristics, reduction of particle cracking, and suppression of resistance increase are not very effective.
[0043] Meanwhile, the coating layer may further include tungsten (W) in addition to boron. When the coating layer further includes tungsten, the coating layer is more effective in reducing lithium by-products remaining on the surface of the lithium nickel-based oxide and suppressing an increase in initial resistance than when the coating layer includes only boron.
[0044] Here, the tungsten (W) is preferably contained in an amount of 4000 pm or less, preferably 3500 to 4000 ppm based on the total weight of the positive electrode material. When the tungsten content satisfies the above range, it is possible to obtain a more excellent effect in terms of reducing residual lithium and suppressing an increase in initial resistance.
[0045] On the other hand, the positive electrode active material may have a crystalline grain size of 80 nm to 150 nm, preferably 80 nm to 120 nm, and more preferably 90 nm to 110 nm. When the crystalline grain size of the positive electrode active material satisfies the above range, the effect of improving cycle characteristics can be obtained.
[0046] Meanwhile, the positive electrode active material may be in the form of secondary particles formed by agglomeration of a number of primary particles, and the average particle size of the primary particles may be 1 μm or less, preferably 500 nm to 1 μm. When the average particle size of the primary particles satisfies the above range, an effect of improving cycle characteristics can be obtained.
[0047] On the other hand, the cathode material according to the present invention may have a bimodal particle size distribution, specifically, an average particle size D 50 a large particle diameter positive electrode active material having an average particle diameter D of 8 μm or more, preferably 8 μm to 20 μm, and more preferably 8 μm to 15 μm; 50 and a small particle size positive electrode active material having a particle size of 6 μm or less, preferably 2 μm to 6 μm, and more preferably 3 μm to 5 μm. When the positive electrode material has a bimodal particle size distribution, the small particle size positive electrode active material particles are filled into the gaps between the large particle size positive electrode active material particles during the production of the positive electrode, thereby increasing the electrode density, and the contact area between the positive electrode active material particles is increased, thereby obtaining the effect of improving the energy density.
[0048] The large particle size positive electrode active material and the small particle size positive electrode active material may have the same composition and only differ in average particle size, or may have different compositions and average particle sizes.
[0049] Meanwhile, at least one of the large particle size positive electrode active material and the small particle size positive electrode active material may be the above-mentioned positive electrode active material of the present invention, i.e., the above-mentioned positive electrode active material including a coating layer containing lithium nickel-based oxide and boron, and preferably, both the large particle size positive electrode active material and the small particle size positive electrode active material may be the above-mentioned positive electrode active material of the present invention.
[0050] Meanwhile, the cathode material according to the present invention may contain the large particle diameter cathode active material and the small particle diameter cathode active material in a weight ratio of 9:1 to 6:4, preferably 8:2 to 6:4. When the mixing ratio of the large particle diameter cathode active material and the small particle diameter cathode active material satisfies the above range, the effect of suppressing particle cracking during rolling is more excellent. This is because if there is an excessive amount of the large particle diameter cathode active material, contact between the large particles increases and particle cracking may increase during rolling, and if there is an excessive amount of the small particle diameter cathode active material, the density of the entire cathode material decreases and particle cracking may increase.
[0051] The cathode material of the present invention has a BET specific surface area of 0.2 to 0.4 m 2 / g, preferably 0.25 to 0.35 m 2 / g, and contains boron (B) in an amount of 500 ppm to 1000 ppm, preferably 600 ppm to 900 ppm, based on the total weight of the positive electrode material. Here, the BET specific surface area and B content are values measured for the positive electrode material powder, and are distinguished from the BET specific surface area and B content of individual positive electrode active material particles. For example, when a large particle size positive electrode active material and a small particle size positive electrode active material having different compositions are included, the BET specific surface area and B content of each of the large particle size positive electrode active material and the small particle size positive electrode active material may differ from the BET specific surface area and B content of the entire positive electrode material powder.
[0052] Meanwhile, the BET specific surface area of the positive electrode material is determined by the combined effect of the density of the positive electrode active material precursor, the calcination temperature, and the content of the coating element. Therefore, a positive electrode material having a desired BET can be manufactured by appropriately adjusting the density of the precursor, the calcination temperature, and the content of the coating element.
[0053] According to the research of the present inventors, when the BET specific surface area and boron content of the positive electrode material simultaneously satisfy the above ranges, the life characteristics, initial resistance characteristics, and particle cracking suppression effect are all excellent, and in particular, the life characteristics and particle cracking suppression effect are remarkably improved. Specifically, when the BET specific surface area of the positive electrode material is 0.2 m 2 / g~0.4m 2 / g but the boron content is outside the above range, or the boron content of the positive electrode material is 500 to 1000 ppm but the BET specific surface area is outside the above range, the life characteristics and the effect of suppressing particle cracking are not very good.
[0054] Manufacturing method of cathode material Next, a method for producing the cathode material of the present invention will be described.
[0055] The cathode material according to the present invention may be prepared by a method of mixing a precursor for a cathode active material and a lithium raw material, calcining the mixture to prepare a lithium nickel-based oxide, mixing the lithium nickel-based oxide with a boron-containing coating raw material, and heat-treating the mixture to form a coating layer.
[0056] In order to produce a cathode material having a low BET specific surface area, it is preferable to use a cathode active material precursor having a high density, and the density of the cathode active material precursor can be adjusted by adjusting the pH during the coprecipitation reaction. Specifically, in the present invention, the cathode active material precursor has a BET specific surface area of 5 to 50 m 2 / g, preferably 10 to 30m 2 / g, more preferably 10 to 15m 2 / g.
[0057] Specifically, the positive electrode active material precursor may be prepared by a method in which an aqueous transition metal solution, an ammonium cation complex forming agent, and a basic compound are supplied to a reactor and reacted to form positive electrode active material precursor particles.
[0058] Here, the transition metal aqueous solution may contain nickel, cobalt and manganese elements, and may be prepared by mixing a nickel source material, a cobalt source material and a manganese source material in water.
[0059] The nickel source material may be Ni(OH)2, NiO, NiOOH, NiCO3·2NI(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, a fatty acid nickel salt, or a nickel halide, and any one or a mixture of two or more of these may be used.
[0060] The cobalt source material may be Co(OH)2, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, or Co(SO4)2·7H2O, and any one or a mixture of two or more of these may be used.
[0061] The manganese source material may be manganese oxides such as Mn2O3, MnO2, and Mn3O4; manganese salts such as MnCO3, Mn(NO3)2, MnSO4, manganese acetate, manganese dicarboxylate, manganese citrate, and manganese fatty acid salt; oxyhydroxide, or manganese chloride, and any one or a mixture of two or more of these may be used.
[0062] Optionally, the aqueous transition metal solution may contain doping elements (M 1 ), wherein the M 1 may include at least one selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta, and Nb. When the positive electrode active material further includes a doping element, it may have an effect of improving the life characteristics, discharge characteristics, and / or stability.
[0063] The aqueous solution of the transition metal is 1 When the aqueous transition metal solution is prepared, the doping element M 1 Optionally, further raw materials may be added.
[0064] The doping element M 1The raw material contains doping element M 1 At least one selected from the group consisting of acetates, sulfates, sulfides, hydroxides, oxides, and oxyhydroxides, including the above, may be used.
[0065] Meanwhile, the ammonium cation complexing agent may be at least one selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and NH4CO3, and may be added to the reactor in the form of a solution in which the compound is dissolved in a solvent. The solvent may be water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water.
[0066] The basic compound may be at least one selected from the group consisting of NaOH, KOH, and Ca(OH)2, and may be added to the reactor in the form of a solution in which the basic compound is dissolved in a solvent, where the solvent may be water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water.
[0067] In the precursor particle formation step, the pH of the reaction solution may be 8 to 11, preferably 9 to 10, and the temperature of the reaction solution may be 40°C to 60°C, preferably 45°C to 55°C. The pH of the reaction solution may be controlled by adjusting the amount of a basic compound added using a pH sensor or the like. When the pH and temperature of the reaction solution satisfy the above ranges, the precursor particles can be smoothly grown, and a precursor with high density can be produced.
[0068] When the precursor particles have grown sufficiently through the above process, the precursor particles are separated from the reaction solution, washed, and then dried to obtain precursor particles for a positive electrode active material.
[0069] Next, the precursor for the positive electrode active material is mixed with a lithium raw material and then calcined to prepare a positive electrode active material.
[0070] The lithium source material can be any compound containing a lithium source, and is preferably at least one selected from the group consisting of lithium carbonate (Li2CO3), lithium hydroxide (LiOH·H2O), LiNO3, CH3COOLi, and Li2(COO)2.
[0071] The precursor and the lithium source material may be mixed so that the molar ratio of transition metal (Me):lithium (Li) contained in the precursor is 1:1 to 1:1.2, preferably 1:1 to 1:1.1. If the lithium source material is mixed below this range, the capacity of the produced positive electrode active material may be reduced, and if the lithium source material is mixed above this range, the particles may be sintered during the firing process, making it difficult to produce the positive electrode active material, and the capacity may be reduced and separation of the positive electrode active material particles may occur after firing.
[0072] In addition, if necessary, during the firing, M 1 The doping element M may be mixed with other materials. 1 may be, for example, at least one selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta and Nb, and the doping element M 1 The raw material contains the doping element M 1 The metal oxide may be at least one selected from the group consisting of acetates, sulfates, sulfides, hydroxides, oxides, and oxyhydroxides, including
[0073] The firing may be performed at 800° C. to 1000° C. for 10 to 35 hours, preferably at 850° C. to 950° C. for 15 to 30 hours, but is not limited thereto.
[0074] Next, the lithium nickel-based oxide and a boron-containing coating raw material are mixed and then heat-treated to form a coating layer.
[0075] The boron-containing coating source material is, for example, H2BO3, HBO2, H3BO3, H2B4O7, B2O3, C6H5B(OH)2, (C6H5O)3B, (CH3(CH2) 30 )3B, C3H9B3O6, (C3H7O3)B, etc. The coating raw material is mixed in an amount such that the content of boron (B) is 500 ppm to 1000 ppm based on the total weight of the cathode material.
[0076] If necessary, a tungsten-containing coating source material can be mixed together during the formation of the coating layer. The tungsten-containing coating source material can be, for example, WO3, Li3WO4, (NH4) 10 W 12 O 41 .5H2O, etc. The tungsten-containing coating raw material is preferably mixed in an amount such that the tungsten content is 4000 ppm or less based on the total weight of the cathode material.
[0077] Meanwhile, the mixing of the lithium nickel-based oxide and the coating raw material may be performed as a solid-phase mixing, and the heat treatment may be performed at a temperature of 200°C to 700°C or 300°C to 600°C, but is not limited thereto.
[0078] Meanwhile, when the cathode material according to the present invention is a bimodal cathode material including a large particle size cathode active material and a small particle size cathode active material, the cathode material of the present invention can be manufactured by preparing a large particle size lithium nickel-based oxide and a small particle size lithium nickel-based oxide, respectively, mixing the large particle size lithium nickel-based oxide and the small particle size lithium nickel-based oxide to form a mixture, mixing the mixture with a boron-containing coating raw material, and then heat-treating the mixture to form a coating layer on the surfaces of the large particle size lithium nickel-based oxide and the small particle size lithium nickel-based oxide.
[0079] positive electrode Next, the positive electrode according to the present invention will be described.
[0080] The positive electrode according to the present invention includes the above-mentioned positive electrode material according to the present invention. Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and including the above-mentioned positive electrode material of the present invention.
[0081] In the positive electrode, the positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can usually have a thickness of 3 to 500 μm, and fine irregularities can be formed on the surface of the positive electrode current collector to increase the adhesive force of the positive electrode active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0082] The positive electrode active material layer may contain a conductive material and a binder in addition to the above-mentioned positive electrode material.
[0083] The conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives. One or a mixture of two or more of these can be used. The conductive material can be usually contained in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight based on the total weight of the positive electrode active material layer.
[0084] The binder serves to improve the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, more preferably 1 to 10% by weight, based on the total weight of the positive electrode active material layer.
[0085] The positive electrode may be manufactured by a conventional method for manufacturing a positive electrode. For example, the positive electrode may be manufactured by mixing a positive electrode active material, a binder, and / or a conductive material in a solvent to prepare a positive electrode slurry, applying the positive electrode slurry onto a positive electrode current collector, and then drying and rolling the positive electrode slurry. Here, the types and contents of the positive electrode active material, binder, and conductive material are as described above.
[0086] The solvent may be a solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to have a viscosity that can dissolve or disperse the positive electrode active material, conductive material, and binder and provide excellent thickness uniformity during subsequent coating for the production of a positive electrode, taking into consideration the coating thickness of the slurry and the manufacturing yield.
[0087] Alternatively, the positive electrode can be produced by casting the positive electrode slurry on a separate support, peeling the resulting film from the support, and laminating the film on a positive electrode current collector.
[0088] Lithium secondary battery Next, the lithium secondary battery according to the present invention will be described.
[0089] The lithium secondary battery of the present invention includes the positive electrode according to the present invention. Specifically, the lithium secondary battery includes a positive electrode, a negative electrode facing the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, the positive electrode being as described above. The lithium secondary battery may also optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.
[0090] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.
[0091] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of usually 3 to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0092] The negative electrode active material layer includes a negative electrode active material, and optionally a binder and a conductive material.
[0093] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β (0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the above-mentioned metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used.
[0094] Also, a metallic lithium thin film may be used as the negative electrode active material. Also, the carbon material may be either low crystalline carbon or high crystalline carbon. Typical low crystalline carbons are soft carbon and hard carbon, and typical high crystalline carbons are amorphous, plate-like, flaky, spherical or fibrous natural graphite or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, carbon microbeads, mesophase pitches, and high temperature fired carbon such as petroleum or coal tar pitch derived cokes.
[0095] The conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery to be constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and one or more of these can be used alone or in combination. The conductive material can usually be contained in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, based on the total weight of the negative electrode active material layer.
[0096] The binder serves to improve the adhesion between the negative electrode active material particles and the adhesive strength between the negative electrode active material and the negative electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, more preferably 1 to 10% by weight, based on the total weight of the negative electrode active material layer.
[0097] For example, the negative electrode active material layer may be manufactured by applying a negative electrode slurry containing a negative electrode active material, and optionally a binder and a conductive material, onto a negative electrode current collector and drying the applied negative electrode slurry, or by casting the negative electrode slurry onto a separate support, peeling the negative electrode slurry from the support, and laminating the resulting film onto the negative electrode current collector.
[0098] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent humidification ability of the electrolyte solution is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, etc., can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used as a single layer or a multilayer structure.
[0099] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.
[0100] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0101] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethyl alcohol and isopropyl alcohol, nitriles such as R-CN (R is a C2-C20 straight-chain, branched or cyclic hydrocarbon group that can contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of a battery and a low-viscosity straight-chain carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferred.
[0102] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used as the lithium salt. The concentration of the lithium salt is preferably within a range of 0.1 to 5.0M, preferably 0.1 to 3.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0103] In addition to the electrolyte components, the electrolyte may further contain additives for the purpose of improving the life characteristics of the battery, suppressing the decrease in the battery capacity, and improving the discharge capacity of the battery. For example, the additives may be haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethyl alcohol amine, cyclic ethers, ethylene diamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethyl alcohol, or aluminum trichloride, which may be used alone or in combination, but are not limited thereto. The additives may be contained in an amount of 0.1 to 10% by weight, preferably 0.1 to 5% by weight, based on the total weight of the electrolyte.
[0104] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention rate, and is therefore useful in portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0105] According to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.
[0106] The battery module or the battery pack may be used as a power source for one or more medium- to large-sized devices including a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0107] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may be embodied in various different forms and should not be construed as limited to the embodiments set forth herein.
[0108] Example 1 1. Manufacturing of large particle size positive electrode active material <Preparation of precursor> After 4L of distilled water was put into a coprecipitation reactor (volume 20L), 100mL of 28wt% ammonia solution was added while maintaining the temperature at 50℃ in a nitrogen atmosphere, and then NiSO4, CoSO4, and MnSO4 were mixed so that the molar ratio of nickel:cobalt:manganese was 0.7:0.1:0.23.2mol / L transition metal solution was added at 30mL / hr and 28wt% ammonia solution was added at 42mL / hr. The mixture was stirred at an impeller speed of 400rpm, and a 40wt% sodium hydroxide solution was added to maintain the pH of the reaction solution at 9.0, allowing the coprecipitation reaction to occur for 24 hours to form precursor particles.
[0109] The precursor particles were separated, washed, and then dried in an oven at 130° C. to produce a precursor.
[0110] <Production of lithium nickel oxide> The positive electrode active material precursor prepared as above, LiOH and ZrO2 were mixed in a molar ratio of (Ni+Co+Mn):Li:Zr of 1:1.05:0.0043, and then calcined at 850°C for 10 hours to prepare lithium nickel oxide. The average particle size (D 50 ) was 9 μm.
[0111] 2. Manufacturing of small particle size positive electrode active material The positive electrode active material precursor, lithium nickel-based oxide, and positive electrode active material were prepared in the same manner as above, except that the coprecipitation reaction time during the formation of the precursor particles was 12 hours to prepare the positive electrode active material precursor. The average particle size (D 50 ) was 4 μm.
[0112] 3. Manufacturing of cathode materials The large particle diameter positive active material and the small particle diameter positive active material prepared as above were mixed in a weight ratio of 70:30.
[0113] Then, the positive electrode active material mixture and boric acid were mixed in a weight ratio of 1:0.00286, and heat-treated at 400° C. for 5 hours to prepare a positive electrode material.
[0114] Example 2 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 840° C. when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00429 when producing the positive electrode material.
[0115] Example 3 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 840° C. when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00572 when producing the positive electrode material.
[0116] Comparative Example 1 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 860° C. when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00229 when producing the positive electrode material.
[0117] Comparative Example 2 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 840° C. when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00629 when producing the positive electrode material.
[0118] Example 4 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 840° C. when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00286 when producing the positive electrode material.
[0119] Example 5 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 830°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00429 when producing the positive electrode material.
[0120] Example 6 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 830°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00527 when producing the positive electrode material.
[0121] Comparative Example 3 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 850° C. when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00229 when producing the positive electrode material.
[0122] Comparative Example 4 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 830°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00629 when producing the positive electrode material.
[0123] Comparative Example 5 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 860°C when producing the large particle size and the small particle size lithium nickel-based oxide, and Al2O3 was mixed in place of boric acid in the production of the positive electrode material so that the weight ratio of the positive electrode active material mixture:Al2O3 was 1:0.00283.
[0124] Example 7 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 830°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00286 when producing the positive electrode material.
[0125] Example 8 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 820°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00429 when producing the positive electrode material.
[0126] Example 9 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 820°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00572 when producing the positive electrode material.
[0127] Comparative Example 6 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 840° C. when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00229 when producing the positive electrode material.
[0128] Comparative Example 7 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 820°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00629 when producing the positive electrode material.
[0129] Comparative Example 8 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 830°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00229 when producing the positive electrode material.
[0130] Comparative Example 9 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 820°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00286 when producing the positive electrode material.
[0131] Comparative Example 10 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 810°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00429 when producing the positive electrode material.
[0132] Comparative Example 11 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 810°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00572 when producing the positive electrode material.
[0133] Comparative Example 12 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 800° C. when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00629 when producing the positive electrode material.
[0134] Comparative Example 13 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 810°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00229 when producing the positive electrode material.
[0135] Comparative Example 14 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 800° C. when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00286 when producing the positive electrode material.
[0136] Comparative Example 15 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was set to 790° C. when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00429 when producing the positive electrode material.
[0137] Comparative Example 16 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was set to 780° C. when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00572 when producing the positive electrode material.
[0138] Comparative Example 17 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was set to 770°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture and boric acid were mixed in a weight ratio of 1:0.00629 when producing the positive electrode material.
[0139] Example 10 The large particle size positive electrode active material, the small particle size positive electrode active material, and the positive electrode material were produced in the same manner as in Example 1, except that the firing temperature was 840°C when producing the large particle size and the small particle size lithium nickel-based oxide, and the positive electrode material mixture, boric acid, and WO3 were mixed in a weight ratio of 1:0.00572:0.00504 when producing the positive electrode material.
[0140] Experimental Example 1 The BET specific surface area and coating element (B, Al, W) contents of the cathode material powders produced in Examples 1 to 10 and Comparative Examples 1 to 17 were measured.
[0141] The specific surface area was measured by the BET method using a BELSORP-mini after taking 3 g of the positive electrode material powder, and the boron content was measured by the ICP method using an ICP-OES (PerkinElmer, Optima7300DV) device after taking 1 g of the positive electrode material powder.
[0142] The measurement results are shown in Table 1 below.
[0143] [Table 1A]
[0144] [Table 1B]
[0145] Experimental example 2: Evaluation of particle cracking 3 g of the cathode material powder produced in Examples 1 to 10 and Comparative Examples 1 to 17 was placed in a cylindrical metal mold with a diameter of 2 cm and pressed at a pressure of 9 tons, and then the volume cumulative particle size distribution (PSD) was measured to measure the fine powder generation rate of less than 1 μm. The particle size distribution was measured using a Microtrac S-3500, and the fine powder generation rate of 1 μm or less was converted into volume % based on the total weight of the cathode material. The measurement results are shown in Table 2 below.
[0146] Experimental Example 3: The surfaces and cross sections of the large particle diameter positive electrode active material particles of the positive electrode materials produced in Example 8 and Comparative Example 11 were observed by SEM.
[0147] FIG. 1 is an SEM image of the surface of the large particle size positive electrode active material of Example 8, and FIG. 2 is an SEM image of the cross section of the large particle size positive electrode active material of Example 8.
[0148] FIG. 3 is an SEM image of the surface of the large particle size positive electrode active material of Comparative Example 11, and FIG.
[0149] 1 to 4, it can be seen that the positive electrode active material of Example 8 has a higher surface density and fewer internal pores than the positive electrode active material of Comparative Example 11.
[0150] Experimental example 4: Evaluation of life characteristics The cathode materials prepared in Examples 1 to 10 and Comparative Examples 1 to 17, carbon black, and PVDF binder were mixed in N-methylpyrrolidone at a weight ratio of 96:2:2 to prepare cathode slurries. The cathode slurries were applied to one side of an aluminum current collector, dried at 100°C, and rolled to prepare cathodes.
[0151] The negative electrode used was a lithium metal electrode.
[0152] An electrode assembly was prepared by interposing a porous polyethylene separator between the positive and negative electrodes, and the electrode assembly was placed inside a battery case, and an electrolyte was injected into the case to prepare a half-cell. The electrolyte was prepared by dissolving LiPF6 at a concentration of 1.0 M in a mixed organic solvent in which ethylene carbonate / ethyl methyl carbonate / diethyl carbonate were mixed in a volume ratio of 3:4:3.
[0153] Each half-cell battery prepared above was charged at 45° C. in CC-CV mode at 0.7 C to 4.4 V, and discharged at a constant current of 0.5 C to 3.0 V as one cycle. 50 charge-discharge cycles were performed to measure the capacity retention and evaluate the life characteristics. The measurement results are shown in Table 2 below.
[0154] [Table 2A]
[0155] [Table 2B]
[0156] Referring to Table 2, it can be seen that the cathode materials of Examples 1 to 10, in which the BET and B contents are within the ranges of the present invention, generate significantly less fine powder when pressed at 9 ton compared to the cathode materials prepared according to the comparative examples, and have excellent life characteristics when applied to secondary batteries.
[0157] Experimental Example 5: Evaluation of initial resistance characteristics The cathode materials prepared in Examples 7, 8, 9 and Comparative Examples 2, 4, 9, 10, and 11, carbon black, and PVDF binder were mixed in N-methylpyrrolidone at a weight ratio of 96:2:2 to prepare cathode slurries. The cathode slurries were applied to one side of an aluminum current collector, dried at 100°C, and rolled to prepare cathodes.
[0158] The negative electrode used was a lithium metal electrode.
[0159] An electrode assembly was prepared by interposing a porous polyethylene separator between the positive and negative electrodes, and the electrode assembly was placed inside a battery case, and an electrolyte was injected into the case to prepare a half-cell. The electrolyte was prepared by dissolving LiPF6 at a concentration of 1.0 M in a mixed organic solvent in which ethylene carbonate / ethyl methyl carbonate / diethyl carbonate were mixed in a volume ratio of 3:4:3.
[0160] Each half-cell battery prepared above was charged to 4.4 V at 0.7 C, and then discharged to 3.0 V at a constant current of 0.5 C. The initial resistance was calculated by dividing the voltage change in the first 30 seconds after the start of discharge by the current value, and the resistance of the remaining cells was expressed as a relative value with the resistance of the cell prepared using the cathode material of Example 9 as the reference (100%). The measurement results are shown in Table 3 below.
[0161] [Table 3]
[0162] As shown in Table 3, in the case of the cells using the cathode materials of Examples 7 and 8, the initial resistance does not increase significantly and remains at a similar level, despite the fact that the cells have a lower specific surface area than the cells using the cathode materials of Comparative Examples 9 to 11, which have the same coating element content. On the other hand, in the case of the cells using the cathode materials of Comparative Examples 2 and 4, which have coating element contents outside the range of the present invention, the initial resistance increases significantly.
Claims
1. A positive electrode material including a positive electrode active material including a lithium nickel-based oxide in which the mole fraction of nickel among metal elements other than lithium is 50 mol% to 90 mol%, and a coating layer formed on the surface of the lithium nickel-based oxide and containing boron (B), The BET specific surface area of the positive electrode material is 0.2 m 2 / g to 0.4m 2 / g, and the boron (B) is contained in an amount of 500 ppm to 1000 ppm based on the total weight of the positive electrode material.
2. The cathode material according to claim 1 , wherein the lithium nickel-based oxide has a composition represented by the following [Chemical Formula 1]: [Chemical formula 1] Li x [Ni a Co b Mn c M 1 d ]O 2 In the above [Chemical Formula 1], M 1 is one or more elements selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta, and Nb, and 0.8≦x≦1.2, 0.5≦a≦0.9, 0<b<0.5, 0<c<0.5, and 0≦d≦0.
2.
3. Said M 1 The cathode material according to claim 2 , wherein is Zr.
4. 3. The cathode material according to claim 2, wherein the Zr is contained in an amount of 4000 ppm to 5000 ppm based on the total weight of the cathode material.
5. 10. The cathode material of claim 1, wherein the coating layer further comprises tungsten (W).
6. 6. The cathode material according to claim 5, wherein the tungsten (W) is contained in an amount of 4000 ppm or less based on the total weight of the cathode material.
7. The cathode material according to claim 1, wherein the cathode active material has a crystalline grain size of 90 nm to 110 nm.
8. the positive electrode active material is a secondary particle formed by agglomeration of a plurality of primary particles, 2. The cathode material according to claim 1, wherein the average particle size of the primary particles is 500 nm to 1 μm.
9. 10. The cathode material of claim 1, wherein the cathode material has a bimodal particle size distribution.
10. The cathode material has an average particle size D 50 a large particle diameter positive electrode active material having an average particle diameter D 50 10. The cathode material according to claim 9, further comprising a small particle size cathode active material having a particle size of 6 μm or less.
11. The cathode material according to claim 10, wherein the large particle size cathode active material and the small particle size cathode active material are contained in a weight ratio of 9:1 to 6:
4.
12. A positive electrode comprising the positive electrode material of any one of claims 1 to 11.
13. A lithium secondary battery comprising the positive electrode according to claim 12.
Citation Information
Patent Citations
Method for manufacturing a positive electrode active material, and a positive electrode active material for lithium secondary batteries manufactured thereby.
JP2015536558A
Positive electrode active material for secondary battery, method for producing the same, and secondary battery including the same
JP2018531500A
Positive electrode active material for secondary battery, method for producing the same, and lithium secondary battery including the same
JP2020537314A
Positive electrode active material and method of producing the same
JP2021015790A
Lithium complex oxide
JP2021070626A