Depolymerization of plastics using silica-based catalysts

Supported heteropolyacids effectively depolymerize complex plastic waste into high-quality liquid products for cracker feedstocks, addressing the inefficiencies of existing catalysts by enhancing pyrolysis efficiency and reducing solid residues.

JP2024540149AInactive Publication Date: 2024-10-31BASELL POLIOLEFINE ITALIA SRL

Patent Information

Application Number
JP2024525548
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-22
Filing Date
2022-11-15
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing catalysts for plastic depolymerization are ineffective when dealing with complex plastic waste feedstocks, leading to unpredictable performance and reduced catalytic activity due to catalyst poisoning effects.

Method used

The use of supported heteropolyacids, particularly those containing transition metals like W, Mo, and V, and non-metals like Si and P, as catalysts for depolymerizing plastic waste, including polyethylene and polypropylene, under controlled atmospheric conditions to enhance pyrolysis efficiency.

Benefits of technology

The process achieves high yields of liquid depolymerization products suitable for use as cracker feedstocks, with improved quality and reduced solid residue, even with complex plastic waste, by utilizing supported heteropolyacids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540149000001
    Figure 2024540149000001
  • Figure 2024540149000002
    Figure 2024540149000002
  • Figure 2024540149000003
    Figure 2024540149000003
Patent Text Reader

Abstract

Described herein is a method for depolymerizing plastic waste using supported heteropolyacid catalysts, which provides high quality liquid depolymerization products that can be used as cracker feedstock with high efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to catalytic methods for depolymerizing plastic feedstocks and to specific catalysts for depolymerization, more particularly to methods for depolymerizing plastic feedstocks in the presence of a supported heteropolyacid catalyst. [Background technology]

[0002] The production of plastics has increased dramatically over the past few decades because plastics are cheap, durable materials that can be used to manufacture a variety of products that find use in a wide range of applications. Due to the durability of the polymers used to produce plastics, more and more plastics are filling landfills around the world, taking over natural habitats, and causing environmental problems. Even degradable and biodegradable plastics can persist for decades, depending on local environmental factors such as UV exposure levels, temperature, and the presence of suitable microorganisms.

[0003] Currently, plastic recycling mainly includes mechanical recycling and chemical recycling. Globally, mechanical recycling is the most widely used method for new uses of plastics, in which plastics are mechanically transformed without changing their chemical structure, making them available for the production of new materials. The general mechanical recycling process includes collecting plastic waste, sorting the plastic waste into different types and colors of plastics, baling the plastics by pressing or crushing the plastics, washing and drying the plastics, reprocessing the plastics into pellets by agglomerating, extruding, and cooling, and finally obtaining recycled raw materials. It is the most widely used technique for polyolefins such as polyethylene (PE) and polypropylene (PP).

[0004] Chemical recycling, on the other hand, involves reprocessing plastics, modifying their structure, so that they can be used as raw materials in various industries or as basic materials or feedstocks to manufacture new plastic products. Chemical recycling typically involves collecting plastics and then heating them to a temperature where the polymers break down into smaller fragments. This process, also known as depolymerization, is the basic process of converting plastic waste material into liquid fuels by pyrolysis (cracking) in the absence of oxygen. Plastic waste is first melted in a stainless steel chamber, usually under an inert purge gas such as nitrogen. The chamber then heats the molten material to a gaseous state, which is then aspirated and condensed in one or more condensers to produce a hydrocarbon fraction that includes linear and branched chain aliphatic, cycloaliphatic, and aromatic hydrocarbons. The resulting mixture can be used as fuel or as a feedstock for further thermocatalytic processes to obtain refined chemicals such as monomers that can be reintroduced into the plastics manufacturing cycle.

[0005] The process of converting the molten plastic mass into a gas stream can in principle only take place by the action of heat (thermal depolymerization), but it has been shown that the presence of catalysts at this stage allows the depolymerization to take place more efficiently at lower temperatures. For this purpose, various catalysts have often been proposed, based on depolymerization tests carried out on virgin polymers or on precisely pre-sorted recycled plastics consisting essentially of a single polymer. Under these "unrealistic" conditions, the catalysts may show a somewhat high depolymerization activity only for thermal depolymerization. However, these tests do not provide any information on how the catalysts can function under real conditions, and in particular on whether and to what extent they are affected by catalyst poisoning effects arising from the components of real plastic waste.

[0006] For example, zeolite-based catalysts show good depolymerization activity for virgin or sorted recycled plastics, but when used with more complex plastic waste feedstocks, the catalytic activity drops significantly. Indeed, the performance of catalysts in the depolymerization of complex plastic waste feedstocks is unpredictable. Summary of the Invention [Problem to be solved by the invention]

[0007] Surprisingly, the present inventors have discovered that certain supported heteropolyacids can produce improved and efficient pyrolysis products for use as cracker feedstocks.

[0008] Accordingly, one aspect of the present disclosure is a process for depolymerizing plastics, the process comprising: a) providing a molten plastic waste feedstock comprising at least recycled polypropylene and polyethylene; b) exposing the molten product obtained in (a) to a temperature in the range of 280°C to 600°C to obtain a depolymerized product; The process is characterized by contacting either or both of the molten product and the depolymerized product with a catalyst comprising a supported heteropolyacid, the transition metal portion of which comprises a transition metal selected from the group consisting of W, Mo, and V, and the non-metal portion of which comprises a non-metal element selected from Si, P, and As.

[0009] Preferably, the amount of catalyst used is in the range of 0.1 to 20% by weight, more preferably 0.1 to 10% by weight, especially 0.1 to 5% by weight, based on the total weight of the plastic waste material and the catalyst. Preferably, the plastic waste feedstock comprises a mixture of polyethylene and polypropylene in a weight ratio of 85:15 to 15:85, more preferably 80:20 to 20:80. The polyethylene may be one or more of high density polyethylene (HDPE), low-density polyethylene (LDPE), linear low density polyethylene (LLDPE). The polypropylene (PP) may be either a propylene homopolymer or a propylene copolymer with low amounts of ethylene and / or butene. Additionally, the feedstock may include other polyolefins such as polybutene. In certain embodiments, the feedstock may also include polymer mixtures incorporating other materials such as polystyrene (PS), ethyl-vinyl acetate copolymer (EVA), ethyl-vinyl alcohol copolymer (EVOH), polyvinyl chloride (PVC), or mixtures thereof. In a preferred embodiment, the feedstock is comprised of a mixture of greater than 80% by weight polyethylene and polypropylene, where the polypropylene comprises greater than 50% by weight of the polypropylene / polyethylene mixture.

[0010] When carrying out the depolymerization process, care must be taken to avoid introducing an oxygen-containing atmosphere into the depolymerization system. A barrier to potentially oxygen-containing atmospheres can be obtained by a range of means, such as a nitrogen blanket and a vacuum system connected to the extruder barrel.

[0011] More specifically, the plastic feed mixture can be fed into the feeding system of the depolymerization reactor by a hopper, or two or more hoppers in parallel, and oxygen present in the atmosphere of the plastic waste material is substantially removed in the hopper(s). In small scale tests, the plastic feedstock can be fed directly to the depolymerization reactor, whereas in larger scale tests, it is preferred to feed the depolymerization reactor via an extruder through which the plastic feedstock is fed. Preferably, the plastic scrap is heated to a temperature where substantially all of the lumps melt, and then injected into the depolymerization reactor. The extruder receives the finely chopped plastic scrap in a feed hopper and conveys the scrap stream to a melting section where the polymer is heated by the combined action of the mixing energy and heat provided by the barrel heaters. Typically, the melting point is in the range of 250°C to 350°C.

[0012] Additives can be incorporated into the melt as needed to reduce the corrosiveness of the plastic scrap or to improve the efficiency of the depolymerization.

[0013] During extrusion, one or more degassing steps may be envisaged to remove any residual moisture present in the product.

[0014] The melt stream may be filtered to remove solid impurities present in the plastic waste before being fed to the reactor.

[0015] Any extrusion system can be used, such as a single screw extruder, a twin screw extruder, a twin screw extruder with a gear pump, or a combination thereof.

[0016] Mixing of the plastic waste feedstock with the catalyst can be performed directly in the depolymerization reactor or beforehand outside the reactor. If mixing is performed in the depolymerization reactor, the catalyst can be fed according to several options. The simplest method, preferably used in small-scale systems, is to pour the solid catalyst directly into the reactor under nitrogen atmosphere. According to another option, the powder catalyst can be fed to the reactor in the form of a liquid hydrocarbon slurry or a semi-solid paste using a dedicated device.

[0017] Alternatively, the mixing may take place outside the depolymerization reactor. In this case, several options are possible. According to one of the options, the catalyst is mixed with the plastic scrap in a homogenizer device and then the mixture is pelletized. The pellets thus obtained, which may also contain other additives, are then fed into an extruder hopper, which is used to feed the polymerization reactor. It is also possible to feed the plastic scrap and the catalyst separately into the hopper. In this case, the mixing can take place in the extruder when the plastic scrap is molten, which is then fed into the depolymerization reactor.

[0018] The depolymerization reactor is preferably a stirred vessel with inlets for the plastic feedstock and catalyst and an outlet for the gaseous depolymerization product, and operating in the temperature range of 300°C to 550°C, more preferably 350°C to 500°C, especially 350°C to 450°C.

[0019] Indeed, as a result of the depolymerization process, a gas stream is generated which is sent to a condensation unit where it is fully or partially liquefied.

[0020] The condensation section receives the exhaust gas from the depolymerization reactor and partially condenses the exhaust gas into an oily depolymerization product substantially composed of hydrocarbons. A portion of the non-condensable gas can be recovered and stored separately. The condensation section can consist of one or more stages operating at different temperatures, with or without pressure, to recover the maximum amount of product depending on the volatility of the resulting compounds formed. The temperature range can, of course, vary depending on the operating pressure.

[0021] Preferably the condensation section has at least two condensation stages, preferably operating at descending temperatures, for example in a small scale installation the first condensation stage operates in the temperature range 100-120°C and the second condensation stage operates in the temperature range 2°C to -20°C.

[0022] It is also possible to subject the depolymerization product obtained from the condensation stage to a second depolymerization stage, which is carried out in the presence of the supported heteropolyacid already described. The second depolymerization stage can be carried out under conditions similar to those described for the previous depolymerization stage. When this set-up is provided, it is also preferred to recycle the catalyst and part of the liquid or semi-liquid mass to the first depolymerization reactor from which the solid residue is discharged. As in the first depolymerization step, the gaseous discharge can be condensed in a subsequent condensation stage.

[0023] At the end of the process, preferably at least 80% by weight, preferably 90% by weight, of the plastic raw material has been converted into liquid or gaseous depolymerization products.

[0024] As mentioned above, a primary use of the depolymerized product according to the present disclosure may be as a cracker feedstock. In this regard, it may be preferred to produce a high yield of liquid depolymerized product from the depolymerization process. In a preferred embodiment, the amount of liquid depolymerized product is greater than 60% by weight of the plastic waste feedstock, more preferably 65-85% by weight.

[0025] It is further believed to be preferred that the liquid depolymerization product has a composition as suitable as possible for use as a cracker feedstock, including very low or no C28 or higher fractions. Preferably, the amount of higher than C28 fractions in the liquid depolymerization product is 4% or less, preferably less than 3%, more preferably less than 2% based on the total amount of liquid depolymerization product.

[0026] Also, the quality of the cracker feedstock is higher if the depolymerized oil obtained from real plastic waste has low values ​​of C6-C8 aromatics and internal olefin index (IOI), the latter defined as the molar ratio between internal double bonds to double bonds at the chain end positions (α-olefins), determined as described in the characterization section. Preferably, the IOI in the liquid depolymerized product is less than 1 wt.%, more preferably less than 0.5 wt.%.

[0027] As used herein, "C6-C8 aromatic compound" refers to a hydrocarbon having sigma bonds and delocalized pi electrons forming rings between carbon atoms, with a total of 6 to 8 carbon atoms.

[0028] As previously mentioned, the catalyst comprises a heteropolyacid deposited on a support.

[0029] Heteropolyacids may be considered to belong to a class of complex oxygen-containing acid compounds that are formally derived from two or more different inorganic acids by the removal of water from two or more molecules of the acid. In other words, one of the acids may be considered to be formed by the combination of several molecules of an anhydride of a transition metal (e.g., molybdenum trioxide or tungsten trioxide), while the other acid is considered to be derived from an anhydride of a nonmetal (e.g., phosphorus or silicon).

[0030] Preferably, in the catalyst according to the present disclosure, the support is selected from inorganic oxides, more preferably Al 2 O 3 , SiO 2 and TiO 2 Preferably, the support is selected from Al 2 O 3 or SiO 2 Heteropolyacids are represented by the formula H n [XM 12 O 40 wherein X is a heteroatom selected from Si, P, and As, M is a transition metal selected from W, Mo, and V, and n is a number that balances the remaining negative valences of the oxygen atoms.

[0031] Preferably, the transition metal compound is W or Mo, in particular W. In a preferred embodiment, ATMC is present in an amount such that the molar ratio of W or Mo to additional transition metal compound (ATMC) is in the range of 0.5 to 100, more preferably 5 to 100, in particular 20 to 100. In a particularly preferred embodiment, no additional transition metal compound (ATMC) is present. Preferably, the heteropolyacid is selected from those in which the non-metallic element is Si or P, in particular Si. In particular, supported tungstosilicic acid (TSA) is particularly preferred. Silica-supported TSA is particularly preferred.

[0032] The amount of heteropolyacid on the support, expressed as the amount of transition metal, ranges from 0.5 to 20% by weight, preferably from 1 to 15% by weight, and more preferably from 1.5 to 10% by weight, based on the total weight of the supported catalyst. Taking into account the weight of the heteropolyacid complex, its amount based on the total weight of the supported catalyst can range from 1 to 26% by weight, preferably from 1.5 to 20% by weight, and more preferably from 2 to 15% by weight.

[0033] Particularly preferred are catalysts which provide high performance and at the same time have a transition metal content of 1 to 15% by weight, preferably 2 to 12% by weight, in particular 2 to 7% by weight, based on the total weight of the catalyst.

[0034] According to a preferred embodiment, a catalyst poison inhibitor can be used with the catalyst. Preferably, the catalyst poison inhibitor is Ca(OH) 2 , Mg(OH) 2 , Ba(OH) 2 , Sr(OH )2 , CaO, phyllosilicates, aluminosilicates, and Zr(HPO 4 ) 2 Among these, Zr(HPO 4 ) 2 , Ca(OH) 2 Among the phyllosilicates, the use of bentonite is preferred.

[0035] The data reported in this disclosure shows that the virgin resin and even complex plastic waste can be converted into liquid depolymerization products with high yields and compositions suitable for use as cracker feedstocks by the process according to this disclosure.

[0036] Characteristic evaluation The characteristics are determined according to the following method.

[0037] Analysis method Characteristic evaluation of the liquid product: The liquid products from the two traps were characterized by gas chromatography (GC) and proton NMR (1H NMR).

[0038] The GC analysis of the liquid products of each experiment was performed using an Agilent 7890 GC (Agilent Technologies, Santa Clara, California) equipped with a standard non-polar column and a flame ionization detector. For the GC data, the weight percentages of x < nC7 (boiling point < 98 °C, referred to as LF1), nC7 < x < nC11 (boiling point 98 °C < BP < 203 °C, referred to as LF2), nC12 < x < nC28 (boiling point 203 °C < BP < 434 °C, referred to as LF3), and x > C28 (boiling point > 434 °C, referred to as LF4) were used to evaluate the characteristics of the liquid products.

[0039] NMR data were used to characterize the proportions of aromatic, paraffinic, and olefinic protons in the liquid product. Examples were analyzed with CDCl3 (0.6 g of depolymerized polymer / metal oxide mixture plus 0.4 g of CDCl3). Data were collected on a Bruker AV500MHz NMR spectrometer (Bruker Corporation, Billerica, MA) at 25 °C using a 5 mm Prodigy probe. One-dimensional 1H NMR data were processed using TOPSPIN® software (Bruker) with an exponential line broadening window function. Quantitative measurements were performed with a 15 s relaxation delay, a 30° flip angle pulse, and 32 scans to facilitate accurate integration. Spectral integrals of aromatic olefinic and paraffinic protons were obtained and used to quantify the relative ratios of these protons.

[0040] Silicon dioxide SiO 2 (White sand), Aluminum(III) oxide Al 2 O 3 , and titanium dioxide TiO 2 A commercial sample of is available from Sigma Aldrich, and CBV400 HY zeolite is available from Zeolyst International.

[0041] The heteropolyacids used in the various examples are commercially available from common suppliers such as Merck, Alfa Aesar, and ABCR.

[0042] Determination of Al and Ti The determination of Al, Ti content in the solid catalyst components was carried out by inductively coupled plasma optical emission spectroscopy using an "ICP spectrometer ARL Accuris". Samples were prepared by analytically weighing 0.1-0.3 grams of catalyst and 2 grams of a 1 / 1 mixture of lithium metaborate / lithium tetraborate in a "Fluxy" platinum crucible. After adding a few drops of KI solution, the crucible was inserted into a special device "Claisse Fluxy" for complete combustion. The residue was then cooled to room temperature with 5% v / v HNO3 The elements are collected in solution and analyzed by ICP at the following wavelengths: aluminum, 394.40 nm; titanium, 368.52 nm.

[0043] Determination of Si and W The determination of the Si, W content in the solid catalyst components was carried out by inductively coupled plasma optical emission spectroscopy on an "ICP spectrometer Icap7000". The samples were prepared by analytically weighing 0.01-0.10 grams of catalyst into a plastic 100 mL volumetric flask. 20 mL of hydrofluoric acid (48%) was diluted to 10 percent with demineralized water and added to the flask. Subsequently, a cold solution of 1.5 g of boric acid (purity >99.5%) dissolved in 50 mL of demineralized water was also added. Finally, the contents of the flask were filled up to the mark with demineralized water and mixed. Subsequently, the resulting solution was directly analyzed by ICP at the following wavelengths: tungsten, 224.875 nm, silicon, 212.412 nm. EXAMPLES

[0044] General depolymerization procedure General procedure for depolymerization tests in a 500 mL round-bottom glass reactor 30 g of polymer plastics were placed in a 500 mL three-neck round-bottom glass reactor equipped with a thermocouple and a nitrogen inlet. The polymer plastics could be both virgin resins obtained directly from polyolefin production plants (Examples 1-7 and Comparative Examples 1-3) and samples of real plastic waste (rpw) from pre-sorted municipal collections (Examples 8 and Comparative Examples).

[0045] Analysis of the actual plastic waste used in the examples showed that it consisted of approximately 97% by weight polyolefins (PP / PE ratio approximately 30 / 70), with the residue containing traces of other common polymers (PET, PS, PA, PU) and inorganic contaminants.

[0046] The solid catalyst (2.5% by weight relative to the plastic) is then introduced in an appropriate amount into the glass reactor. A blank test without catalyst may also be performed. Two glass condensers are connected in series and kept at 110°C and -8°C respectively using an oil bath (Cryostat Julabo). The reactor is placed in an electric heating system (mantle bath) and the desired power is set, the temperature is increased up to 450°C. The pyrolysis process occurs and the following experimental parameters are recorded:

[0047] L%, the sum of the yield of liquid condensable at 110°C and the yield of liquid condensable at -8°C (relative to the polymer input) S%, yield of solid / waxy residue in reactor, excluding catalyst (relative to polymer input) Yield of non-condensable gaseous products in both condensers G% (relative to the polymer input) The results are reported in Tables 1 and 2.

[0048] Comparative Example 1 Using virgin polypropylene as the depolymerization feedstock and without using a depolymerization catalyst, the depolymerization experiments were carried out according to the general depolymerization procedure disclosed above. The results are reported in Table 1.

[0049] Comparative Example 2 Virgin polypropylene is used as the depolymerization raw material, and SiO is used as the depolymerization catalyst. 2 The depolymerization experiments were carried out according to the general depolymerization procedure disclosed above, and the results are reported in Table 1.

[0050] Comparative Example 3 Depolymerization experiments were carried out according to the general depolymerization procedure disclosed above using virgin polypropylene as the depolymerization feedstock and CBV400 HY zeolite as the depolymerization catalyst. The results are reported in Table 1.

[0051] Example 1 Preparation of silica (32 wt%) modified with phosphomolybdic acid (SiPMo-A) In a 250 mL round-bottom flask equipped with a magnetic stirrer, add 4.6 g of phosphomolybdic acid hydrate H at room temperature. 3 [P(Mo 3 O 10 ) 4 ]xH 2 200 g of SiO2 [MW = 1825.25 g / mol (anhydrous basis)] was added and dissolved in a minimum amount of demineralized water (20 mL). After stirring at room temperature for 15 minutes, 10.0 g of silicon dioxide SiO2 was added. 2 was added. Additional water was slowly added (total amount 150 mL) to obtain a moist homogeneous slurry and stirring was continued for 30 min at room temperature. The latter was stirred for 1 h at room temperature using a rotary evaporator. Subsequently, the solid was first dried using a rotary evaporator with stirring, by increasing the temperature to 100 °C and applying a vacuum (about 50 mmHg). Finally, the solid was dried in an oven under vacuum at 105 °C for 2 h. 13.8 g of a free-flowing powder was obtained. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using virgin polypropylene as the depolymerization feedstock. The results are reported in Table 1.

[0052] Example 2 Preparation of alumina modified with tungstosilicic acid (50 wt%) (AlWSi-A) In a 100 mL round-bottom flask equipped with a magnetic stirrer, add 4.5 g of tungstosilicic acid hydrate H at room temperature. 4 [Si(W 3 O 10 ) 4 ]xH 2 2.5 g of aluminum(III) oxide (AlO) (MW = 2878.17 g / mol (anhydrous basis)) was added and dissolved in a minimum amount of demineralized water (20 mL). After stirring at room temperature for 15 minutes, 4.5 g of aluminum(III) oxide (AlO) (MW = 2878.17 g / mol (anhydrous basis)) was added and dissolved in a minimum amount of demineralized water (20 mL). 2 O 3was added. Additional water was slowly added (total amount 60 mL) to obtain a moist homogeneous slurry and stirring was continued for 30 min at room temperature. The latter was then stirred at room temperature for 1 h and filtered through a G5 frit. The solid was then dried at 105 °C under vacuum for 8 h. 6.2 g of a free-flowing powder was obtained: Al = 39.6 wt.%. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using virgin polypropylene as the depolymerization feedstock. The results are reported in Table 1.

[0053] Example 3 Preparation of alumina modified with tungstosilicic acid (50 wt%) (AlWSi-A) In a 100 mL round-bottom flask equipped with a magnetic stirrer, add 4.6 g of phosphotungstic acid hydrate H at room temperature. 3 [P(Mo 3 O 10 ) 4 ]xH 2 The mixture was stirred at room temperature for 15 minutes, and then 4.5 g of aluminum(III) oxide Al was added. 2 O 3 was added. Additional water was slowly added (total amount 60 mL) to obtain a moist homogeneous slurry and stirring was continued for 30 min at room temperature. The latter was then stirred at room temperature for 1 h and filtered through a G5 frit. The solid was then dried at 105 °C under vacuum for 8 h. 6.2 g of a free-flowing powder was obtained: Al = 39.6 wt.%. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using virgin polypropylene as the depolymerization feedstock. The results are reported in Table 1.

[0054] Example 4 Preparation of zeolite beta (50 wt%) modified with tungstosilicic acid (BetaWSi-A) In a 250 mL round-bottom flask equipped with a magnetic stirrer, add 4.5 g of tungstosilicic acid hydrate H at room temperature. 4 [Si(W 3 O 10 ) 4 ]xH2 O [MW=2878.17 g / mol (anhydrous basis)] was added and dissolved in a minimum amount of demineralized water (20 mL). After stirring for 15 min at room temperature, 4.5 g of ZEOLITE H-BETA POWDER were added. Additional water was slowly added (total amount 150 mL) to obtain a moist homogeneous slurry and stirring was continued for 30 min at room temperature. The latter was stirred for 1 h at room temperature using a rotary evaporator. Subsequently, the solid was first dried while stirring using a rotary evaporator, the temperature was increased to 100 °C and a vacuum (about 50 mmHg) was applied. Finally, the solid was dried in an oven under vacuum at 105 °C for 2 h. 7.9 g of a free-flowing powder was obtained. Si=19.4 wt.%, Al=0.6 wt.%. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using virgin polypropylene as the depolymerization feedstock. The results are reported in Table 1.

[0055] Example 5 Preparation of silica (50 wt%) modified with tungstosilicic acid (SiWSi-A) 9.0 g of tungstosilicic acid hydrate H 4 [Si(W 3 O 10 ) 4 ]xH 2 O [MW = 2878.17 g / mol (anhydrous basis)] was dissolved in a few mL of demineralized water at room temperature. This solution was added dropwise at room temperature to a slurry of Silica ES70Y (9.0 g) marketed by PQ Corporation in 40 mL of demineralized water previously prepared in a 250 mL round-bottom flask equipped with a mechanical stirrer. The reaction mixture was stirred at room temperature for 1 h to obtain a moist homogeneous slurry. Subsequently, the water was removed by increasing the temperature to 100 °C and gradually applying a vacuum (up to about 5 mmHg) while stirring using a rotary evaporator. Finally, the solid was dried in an oven under vacuum at 105 °C for 2 h. 12.0 g of a free-flowing powder was obtained. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using virgin polypropylene as the depolymerization feedstock. The results are reported in Table 1.

[0056] Example 6 Preparation of silica (33 wt%) modified with phosphotungstic acid (SiPW-A) 4.91 g of phosphotungstic acid hydrate H 3 [P(W 3 O 10 ) 4 ]xH 2 O [MW = 2880.05 g / mol (anhydrous basis)] was dissolved in 10 mL of demineralized water at room temperature. This solution was added dropwise at room temperature to a slurry of Silica ES70Y (10.05 g) marketed by PQ Company in 120 mL of demineralized water previously prepared in a 250 mL round-bottom flask equipped with a mechanical stirrer. The reaction mixture was stirred at room temperature for 1 h to obtain a moist homogeneous slurry. Subsequently, the water was removed by increasing the temperature to 100 °C and gradually applying a vacuum (up to about 5 mmHg) while stirring using a rotary evaporator. Finally, the solid was dried in an oven under vacuum at 105 °C for 2 h. 14.7 g of a free-flowing powder was obtained: Si = 31.2 wt.%, W = 20.8 wt.%. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using virgin polypropylene as the depolymerization feedstock. The results are reported in Table 1.

[0057] Example 7 Preparation of silica (18 wt%) modified with tungstosilicic acid (SiWSi-A) In a 1 L round bottom flask equipped with a mechanical stirrer, add 11.25 g of tungstosilicic acid hydrate H 4 [Si(W 3 O 10 ) 4 ]xH 2O [MW=2878.17 g / mol (anhydrous basis)] was taken and dissolved in 20 mL of demineralized water. The solution was stirred for 15 min at room temperature and then 50.0 g of silica ES70Y (commercially available from PQ Corporation) was added. In order to obtain a moist homogeneous slurry, demineralized water (120 mL) was added and the resulting reaction mixture was stirred for 2 h at room temperature. Subsequently, the water was removed by increasing the temperature to 75 ° C and gradually applying a vacuum (about 5 mmHg) while stirring using a rotary evaporator. Finally, the solid was dried in an oven under vacuum at 105 ° C for 2 h. 50.5 g of a free-flowing powder was obtained: Si=36.7 wt.%, W=12.5 wt.%. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using virgin polypropylene as the depolymerization feedstock. The results are reported in Table 1.

[0058] Comparative Example 4 The depolymerization experiments were carried out according to the general depolymerization procedure disclosed above, but using real plastic waste as the depolymerization feedstock and without the use of a depolymerization catalyst. The results are reported in Table 2.

[0059] Example 8 Preparation of titanium dioxide with tungstosilicic acid (TiWSi-A) Titanium(IV) isopropoxide (Sigma Aldrich, 28.0 mL, d=0.955 g / mL) was placed in a 500 mL round-bottom flask equipped with a mechanical stirrer at room temperature under nitrogen and mixed with ethanol (Silcompa, 240 mL, d=0.789 g / mL) for 10 min to obtain a homogenous solution. 0.28 M aqueous HCl (0.33 mL) was then added slowly to obtain a white slurry. A second 250 mL round-bottom flask equipped with a mechanical stirrer was charged with urea (Merck, 17.2 g), ethanol (Silcompa 109 mL) and deionized water (17.2 mL) at room temperature to obtain a colorless solution. This urea-alcohol solution (total volume approx. 144 mL) was added to the initial hydrolysis solution of titanium (total volume approx. 268 mL) and the resulting mixture was stirred at room temperature under nitrogen for several hours. An aliquot (205 mL) of this mixture was taken and diluted with 2.25 g of tungstosilicic acid hydrate H in 22.5 mL of ethanol. 4 [Si(W 3 O 10 ) 4 ]xH 2 A solution of 0 was added (30 wt% of tungstosilicic acid in the final material). The final sample was stored in a beaker until dry and then extracted with distilled water in a continuous stirring system for 2 days to remove urea. The solid was then dried in an oven at 100 °C under vacuum for 20 h. 6.0 g of a free-flowing powder was obtained: Ti = 41.5 wt%. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using real plastic waste as the depolymerization feedstock. The results are reported in Table 2.

[0060] Example 9 Preparation of silica (20 wt%) modified with tungstosilicic acid (SiWSi-A) Tungstosilicic Acid Hydrate H 4 [Si(W 3 O 10 ) 4 ]xH 2O [62.5 g, 0.0217 mol, MW=2878.17 g / mol (anhydrous basis)] was dissolved in 120 mL of deionized water at room temperature, giving a colorless solution. The latter was stirred at room temperature for 30 min. Silica ES70Y (250.8 g) marketed by PQ Company was suspended in 1 L of deionized water at room temperature in a 2 L round-bottom flask equipped with a mechanical stirrer. The tungstosilicic acid solution in water was slowly added to the slurry of silica in water and the resulting mixture was stirred at room temperature for 12 h. The final slurry was filtered through a G4 frit and the white solid was washed with deionized water and then dried under vacuum at 105 °C / 24 h. The final compound is a free-flowing white powder (275.6 g): Si=35.9 wt%, W=5.2 wt%. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using real plastic waste as the depolymerization feedstock. The results are reported in Table 2.

[0061] Example 10 Preparation of silica (20 wt%) modified with phosphotungstic acid (SiPW-A) 7.85 g of phosphotungstic acid hydrate H 3 [P(W 3 O 10 ) 4 ]xH 2O [MW = 2880.05 g / mol (anhydrous basis)] was dissolved in 20 mL of demineralized water at room temperature. This solution was added dropwise at room temperature to a slurry of Silica ES70Y (39.25 g) marketed by PQ company in 100 mL of demineralized water previously prepared in a 250 mL round-bottom flask equipped with a mechanical stirrer. The reaction mixture was stirred at room temperature for 2 h to obtain a moist homogeneous slurry. Subsequently, the water was removed by increasing the temperature to 75 °C and gradually applying a vacuum (about 5 mmHg) while stirring using a rotary evaporator. Finally, the solid was dried in an oven under vacuum at 105 °C for 2 h. 43.4 g of a free-flowing powder was obtained: Si = 39.5 wt.%, W = 9.5 wt.%. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using real plastic waste as the depolymerization feedstock. The results are reported in Table 2.

[0062] Example 11 Preparation of silica (18 wt%) modified with tungstosilicic acid (SiWSi-A) 2.25 g of tungstosilicic acid hydrate H 4 [Si(W 3 O 10 ) 4 ]xH 2O [MW = 2878.17 g / mol (anhydrous basis)] was dissolved in a few mL of demineralized water at room temperature. This solution was added dropwise at room temperature to a slurry of Silica ES70Y (10.0 g) marketed by PQ company in 40 mL of demineralized water previously prepared in a 250 mL round-bottom flask equipped with a mechanical stirrer. The reaction mixture was stirred at room temperature for 1 h to obtain a moist homogeneous slurry. Subsequently, the water was removed by increasing the temperature to 100 °C and gradually applying a vacuum (up to about 5 mmHg) while stirring using a rotary evaporator. Finally, the solid was dried in an oven under vacuum at 105 °C for 2 h. 16.5 g of a free-flowing powder was obtained: Si = 46.0 wt.%, W = 11.2 wt.%. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using real plastic waste as the depolymerization feedstock. The results are reported in Table 2.

[0063] Example 12 Preparation of silica (20 wt%) modified with tungstosilicic acid (SiWSi-A) and copper dichloride (10 wt%) A 250 mL round-bottom flask equipped with a mechanical stirrer was charged at room temperature with 12.00 g of tungstosilicic acid hydrate modified silica (20 wt%) prepared as described in Example 6. At the end of the addition, the temperature was raised to 80 °C in order to obtain a homogeneous slurry, and the resulting reaction mixture was stirred at this temperature for 1 h. The latter was filtered through a G4 frit, the solid was washed with deionized water, and then dried in an oven under vacuum at 120 °C / 1 h. Finally, a calcination step was carried out in air at 550 °C / 3.5 h. The final compound is a free-flowing white powder (7.65 g): Si = 42.4 wt%, W < 0.1 wt%, Cu = 0.5 wt%, Cl = 85 ppm. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using real plastic waste as the depolymerization feedstock. The results are reported in Table 2.

[0064] Example 13 Preparation of silica (20 wt%) modified with tungstosilicic acid (SiWSi-A) and zinc dichloride (10 wt%) A 250 mL round-bottom flask equipped with a mechanical stirrer was charged at room temperature with 12.00 g of tungstosilicic acid hydrate modified silica (20 wt%), prepared as described in Example 6. Subsequently, another 30 mL of demineralized water was added to obtain a moist homogeneous slurry, the temperature was raised to 80 °C, and the resulting reaction mixture was stirred at this temperature for 1 h. Then, the water was removed by gradually applying a vacuum while stirring, and the solid was dried in an oven under vacuum at 120 °C / 1 h. Finally, a calcination step was carried out in air at 550 °C / 3.5 h. The final compound is a free-flowing white powder (10.20 g): Si = 39.0 wt%, W = 4.5 wt%, Zn = 5.05 wt%, Cl = 1300 ppm. The catalyst thus obtained was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, using real plastic waste as the depolymerization feedstock. The results are reported in Table 2.

[0065] Example 14 The depolymerization is carried out in a larger depolymerization unit, including a depolymerization reactor consisting of a mechanically stirred (jacketed for heating) reactor with an inlet for the plastic waste from the extruder, an inlet for the depolymerization catalyst, and an outlet for the evolved gas. The gas withdrawn from the reactor was sent to a condensation unit, from which non-condensable gases and pyrolysis oil were obtained. Thermocouples were located in the reactor to monitor and record the temperature.

[0066] The plastic waste feedstock was pre-analyzed for polyolefin content (97 wt%) with residuals including other common polymers (PET, PS, PA, PU) and traces of inorganic contaminants.

[0067] The raw materials were homogenized and granulated before being charged into the hopper, which feeds into an extruder operating at a temperature of 290°C and discharging continuously at 4 kg / h into the depolymerization reactor. The depolymerization reactor was operated at a pressure of 4 barg and a temperature of approximately 410°C. The catalyst prepared according to the procedure of Example 9 was continuously injected into the reactor in the form of a suspension in white oil using a syringe system. The mass ratio between the solid catalyst and the reaction phase was 3.5% by weight. The total depolymerization time was about 3 hours. Finally, the reactor was cooled and opened for cleaning.

[0068] The gas phase of the reactor was sent to a condensation unit formed by a cooling / scrubber column operating at 25 °C, from which a liquid and gas stream were obtained. The resulting gas stream was sent to the vent and the condensed liquid stream was analyzed by GC-FID. Since the number of compounds was very large, the analytical results were reported by taking the specific hydrocarbons as internal retention time standards and grouping the resulting compounds according to their retention times. The results are shown in Table 3.

[0069] The residual content was calculated after excluding the amounts of catalysts and inorganic components originally contained in the actual plastic waste used.

[0070] Comparative Example 5 Thermal depolymerization experiments Depolymerization experiments were carried out using the process settings and conditions described in Example 14, the only difference being that no catalyst was fed. The results of utility in the product (relative to the feedstock) are reported in Table 3 along with the GC-FID analysis reports generated on samples of the produced oil.

[0071] Comparative Example 6 Depolymerization experiments were carried out using the process settings and conditions described in Example 14, except that CBV400 HY zeolite was used as the depolymerization catalyst. The results of utility in the product (relative to the feedstock) are reported in Table 3 along with the GC-FID analysis reports generated on samples of the produced oil.

[0072] [Table 1] The results shown in Table 1 show that the examples carried out with heteropolyacid catalysts, especially with supported tungstosilicic acid (abbreviated as TSA), yield a higher amount of liquid fraction compared to the non-catalyzed depolymerization experiments.

[0073] [Table 2] When used in the depolymerization of real plastic waste, the heteropolyacid catalysts produce better depolymerized products than those obtained by thermal depolymerization alone.

[0074] [Table 3] When used for the depolymerization of real plastic waste, the heteropolyacid catalysts show a combination of better depolymerization activity (lower solid residues) and product quality than the zeolite HY catalyst.

[0075] Example 15 The catalyst prepared according to Example 9 was used in depolymerization experiments carried out according to the general depolymerization procedure disclosed above, where as depolymerization feedstock a real plastic waste (RPW) sample was used, which consisted of about 94 wt. % polyolefins with a PP / PE ratio of about 30 / 70, and the residue contained traces of other common polymers (PET, PS, PA, PU) and inorganic contaminants. In addition, as a catalyst poison suppressing phyllosilicate, Fulcat 435 (commercially available from BYK Chemie GmbH) was used at 2.5 wt. % based on the amount of RPW. The results are reported in Table 4.

[0076] Example 16 The depolymerization was carried out according to the same catalyst and conditions as in Example 15, but with ZrH(PO) instead of Fulcat 435 as the catalyst poison inhibitor. 4 (commercially available from Merck-Sigma Aldrich) was used. The results are reported in Table 4.

[0077] Example 17 The depolymerization was carried out according to the same conditions as in Example 15, and the catalyst used was prepared as described in Example 2, but with acid-treated Al as the catalyst support. 2 O 3 The difference was that . The results are reported in Table 4.

[0078] Comparative Example 7 The depolymerization was carried out according to the same conditions as in Example 15, except that no catalyst and no catalyst poison inhibitor were used. The results are reported in Table 4.

[0079] [Table 4] PSA = catalyst poison inhibitor

Claims

1. 1. A process for depolymerizing plastics, comprising: a) providing a molten plastic waste feedstock comprising at least recycled polypropylene and polyethylene; b) subjecting the molten product obtained in (a) to a temperature in the range of 280°C to 600°C to obtain a depolymerized product; The process is characterized in that either or both of the molten product and the depolymerized product are contacted with a catalyst comprising a supported heteropolyacid, the transition metal portion of which comprises a transition metal selected from the group consisting of W, Mo and V, and the non-metal portion of which comprises a non-metal element selected from Si, P and As.

2. 2. The process according to claim 1, wherein the amount of catalyst is in the range of 0.1 to 20 wt.%, preferably 0.1 to 10 wt.%, in particular 0.1 to 5 wt.%, based on the total weight of the plastic waste feedstock and the catalyst.

3. 3. The process according to any one or more of claims 1 to 2, wherein the plastic waste feedstock comprises a mixture of polyethylene and polypropylene in a weight ratio of from 85:15 to 15:85, more preferably from 80:20 to 20:

80.

4. The support is selected from inorganic oxides, more preferably Al 2 O 3 , SiO 2 and TiO 2 The process according to any one or more of claims 1 to 3, selected from:

5. The process according to any one or more of claims 1 to 4, wherein the heteropolyacid is preferably selected from those in which the transition metal compound is W or Mo, in particular W.

6. 7. The process of claim 6, wherein the additional transition metal compound (ATMC) is present in an amount such that the molar ratio of W or Mo to ATMC ranges from 0.5 to 100.

7. The process according to any one or more of claims 1 to 6, wherein the heteropolyacid is selected from those in which the non-metallic element is Si or P.

8. 8. The process of claim 7, wherein the heteropolyacid is selected from those in which the non-metallic element is Si.

9. The process according to any one or more of the preceding claims, wherein the amount of transition metal is in the range of 1 to 20% by weight based on the total amount of supported catalyst.

10. 10. The process of any one or more of claims 1 to 9, wherein the catalyst comprises supported tungstosilicate (TSA).

11. 9. The process of claim 8, wherein the catalyst comprises silica supported tungstosilicate (TSA).

12. The process according to any one or more of claims 9 to 10, wherein the amount of W is in the range of 1 to 15 wt% based on the total amount of supported catalyst.

13. 2. The process of claim 1, wherein the amount of liquid depolymerization product is greater than 60% by weight of the initially fed plastic waste feedstock.

14. 14. The process according to any one or more of claims 1 to 13, wherein the amount of fraction higher than C28 in the liquid depolymerization product is less than or equal to 4% relative to the total amount of liquid depolymerization product.

15. 15. The process of any one or more of claims 1 to 14, wherein the liquid depolymerized product has an Internal Olefin Index (IOI) of less than or equal to 1 wt%.

Citation Information

Patent Citations

  • Method for converting heavy hydrocarbon oil into light fractions

    JP1982123290A

  • Converting heavy hydrocarbon oil to light hydrocarbon oil

    JP1982205484A

  • Method of pyrolyzing plastic and plastic pyrolysis catalyst for use therein

    JP1996253773A

  • Thermal-decomposition apparatus for plastic

    JP1997059647A

  • Method for producing wax and grease base oil raw materials by catalytic depolymerization of waste plastics

    JP2013539476A

Cited By

  • Catalyst composition for decomposing homopolymers and method for decomposing homopolymers using the same

    JP7839580B1

  • Catalyst composition for decomposing homopolymer and method for decomposing homopolymer using same

    WO2026204477A1