Protected electrode structure for solid-state cells

The enclosed electrode structure in solid state batteries addresses interface issues by encapsulating the electrode with a solid electrolyte composite, enhancing performance through densification and preventing electrode extrusion, thus improving cycle life and reducing resistance.

JP2024540188APending Publication Date: 2024-10-31SOLID POWER OPERATING INC

Patent Information

Application Number
JP2024525697
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-01
Filing Date
2022-10-31
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Solid state battery cells face issues such as cell shorting, increased resistance, and reduced specific capacity due to poor quality solid interfaces between layers, which inhibit lithium ion or electron transfer.

Method used

An enclosed electrode structure is developed, where the electrode is encapsulated by a solid electrolyte composite, enhancing the interface quality through densification and encapsulation, using techniques like calendering to form a protected electrode stack.

Benefits of technology

The solution improves the solid state interfaces, leading to better cycle life, specific cell capacity, and lower cell resistance, while preventing electrode extrusion and promoting uniform material contact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540188000001_ABST
    Figure 2024540188000001_ABST
Patent Text Reader

Abstract

To provide an enclosed electrode for an improved electrochemical cell. An enclosed electrode for an electrochemical cell includes an electrode layer and a solid electrolyte composite, the solid electrolyte composite contacting and enclosing the electrode layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is related to and claims priority under 35 U.S.C. § 119 to U.S. Provisional Patent Application No. 63 / 263,370 (filed November 1, 2021, entitled "Protected Electrode Structure for Solid-State Cells"), the entire disclosure of which is hereby incorporated by reference in its entirety for all purposes.

[0002] Technical Field Various aspects described in this disclosure relate to solid-state primary and secondary electrochemical cells, electrodes and electrode materials, electrolyte compositions, and corresponding methods of making and using these electrochemical cells. [Background technology]

[0003] Background and Introduction With the ever-increasing adoption of mobile devices, electric vehicles, and the development of Internet of Things (IoT) devices, there is an ever-increasing need for battery technology with improved reliability, capacity (Ah), thermal properties, life span, and rechargeability. Solid-state battery cells utilize a non-flammable, solid electrolyte, as opposed to the flammable, liquid electrolyte used in conventional batteries. Thus, solid-state battery cells are relatively safer than conventional batteries. However, in some solid-state battery cells, the transfer of lithium ions or electrons is hindered because the solid interface has increased resistance compared to conventional batteries that use liquid electrolytes.

[0004] As an example of the increased resistance of the solid interface, International Patent Publication WO2021 / 077197(A1) describes a solid-state battery cell in which various stacked layers including a positive electrode collector-a positive electrode active material layer-a solid electrolyte layer-a negative electrode active material layer-a negative electrode current collector are bonded by applying pressure thereto to form a stack, or in another embodiment, a stack is formed by pressing a positive electrode collector-a positive electrode active material layer-a solid electrolyte layer-a negative electrode active material layer-a negative electrode current collector. When using this stacking method, serious problems occur in the solid-state battery cell, such as shorting of the cell, increased cell resistance, and reduced specific cell capacity. These problems in the solid-state battery cell may be due to poor quality of the solid interfaces between the layers. Summary of the Invention [Problem to be solved by the invention]

[0005] Thus, further improvements are needed in solid-state battery cells, their chemistries, and their manufacture. Aspects of the present disclosure were conceived in light of, among other things, these observations. [Means for solving the problem]

[0006] The present disclosure describes an enclosed electrode for an electrochemical cell that includes an electrode layer and a solid electrolyte composite, the solid electrolyte composite contacting and encapsulating the electrode layer. [Brief description of the drawings]

[0007] [Figure 1A] FIG. 1A shows a proposed layout of one embodiment of an enclosed electrode structure 105 prior to assembly. [Figure 1B] FIG. 1B shows a proposed arrangement of one embodiment of the enclosed electrode structure 105 after the three layers are assembled, with the outer boundary 170 of the first SSE and the outer boundary 180 of the second SSE both being longer than the electrode 130 and not attached to the electrode. [Figure 1C]FIG. 1C shows a proposed configuration of one embodiment of the enclosed electrode structure 105 after assembling the three layers and applying pressure to the structure. [Figure 1D] FIG. 1D shows the encapsulated electrode structure 105 after continued application of pressure has been applied to the structure, causing SSE 110 and SSE 120 to contact and form an integrated SSE 125, which encapsulates or seals electrode 135. [Diagram 2] FIG. 2 is a flow chart for a method of forming an enclosed electrode structure. [Figure 3A] FIG. 3A shows a proposed process for one embodiment of an enclosed electrode structure 310 and shear device 320 in place. [Figure 3B] FIG. 3B illustrates the proposed treatment of one embodiment of the enclosed electrode structure 310 immediately after shearing has been initiated by the shearing device 320. [Figure 3C] FIG. 3C illustrates a proposed processing of one embodiment of an enclosed electrode structure 310 after a shearing device 320 shears the solid electrolyte composite along the edge of the enclosed electrode 310 to form an enclosed electrode structure 330 and removes remaining SSE 331. [Figure 4] FIG. 4 is a flow chart for a method of compartmentalizing an enclosed electrode structure. [Figure 5A] FIG. 5A shows the three-dimensional structure of one embodiment of an electrode 500. [Figure 5B] FIG. 5B shows the three-dimensional structure of one embodiment of solid electrolyte composite layer 540. [Figure 5C] FIG. 5C shows the three-dimensional structure of one embodiment of an enclosed electrode structure 580 prior to assembling the three layers. [Figure 5D] FIG. 5D shows a three-dimensional representation of the enclosed electrode structure 590 after a continuous application of pressure has been applied to the layered construct. [Figure 6A] FIG. 6A is a side view of a calendaring apparatus and a method for forming a protected electrode. [Figure 6B]FIG. 6B is a top view of the SSE / electrode / SSE stack of FIG. 6A. [Figure 6C] FIG. 6C is a cross-sectional view of the SSE / electrode / SSE of FIG. 6A taken along line CC. [Figure 6D] FIG. 6D is a cross-sectional side view of the SSE / electrode / SSE stack of FIG. 6A at 618. [Figure 6E] FIG. 6E is a side view of the SSE / electrode / SSE stack undergoing densification by calender rollers. [Figure 7A] FIG. 7A is a first set of SEM images of a first example of a protected electrode. [Figure 7B] FIG. 7B is a second set of SEM images of a second example of a protected electrode. [Figure 7C] FIG. 7C is a third set of SEM images of a third example of a protected electrode. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In one embodiment, an enclosed electrode for an electrochemical cell contains one or more electrode active materials. In another embodiment of an enclosed electrode for an electrochemical cell, two or more sides of the electrode layer are encapsulated by a solid electrolyte composite.

[0009] In another embodiment, an enclosed electrode for an electrochemical cell comprises one or more anode active materials or one or more cathode active materials. In another embodiment, an enclosed electrode for an electrochemical cell comprises one or more alkali metals, alkaline earth metals, transition metals, or alloys thereof. In another embodiment, an enclosed electrode for an electrochemical cell comprises lithium metal or a lithium metal alloy.

[0010] In another embodiment of the surrounded electrode for an electrochemical cell, the electrode layer comprises one or more electrode layers. In another embodiment of the surrounded electrode for a solid-state electrochemical cell, the solid-electrolyte composite comprises one or more solid electrolyte materials.

[0011] In another embodiment of the surrounded electrode for a solid electrochemical cell, the solid electrolyte composite comprises one or more polymers in an amount of 0.5% to 80% by weight of the solid electrolyte composite. In another embodiment of the surrounded electrode for a solid electrochemical cell, the solid electrolyte composite comprises one or more polymers comprising at least one thermoplastic elastomer. In one embodiment, the one or more polymers comprise fluorine.

[0012] In another embodiment of the enclosed electrode for a solid-state electrochemical cell, the electrode layer comprises one or more solid sulfide electrolytes.

[0013] In another embodiment, an enclosed electrode for an electrochemical cell includes an engineered surface coating that includes one or more of the elements lithium, carbon, and oxygen. In one embodiment, the engineered surface coating has a thickness of 1 nm to 100 μm.

[0014] In another embodiment, the surrounded electrode for the electrochemical cell comprises an surrounded anode or an surrounded cathode.

[0015] The present disclosure also describes a method of making an enclosed electrode for a solid-state electrochemical cell, the method including providing an enclosed electrode, disposing the enclosed electrode between two layers of a solid electrolyte composite, and compressing the two layers of the solid electrolyte composite to contact and enclose the electrode.

[0016] In another embodiment of the method, the compressing includes applying a pressure in the range of 100 to 400,000 PSI, thereby densifying and deforming the solid electrolyte composite to coat one or more surfaces of the encapsulated electrodes.

[0017] The present disclosure also describes an enclosed electrode for an electrochemical cell having an electrode layer having a first side, a second side, and a surrounding surface, a first layer of solid electrolyte composite abutting and extending beyond a boundary of the first side of the electrode layer, a second layer of solid electrolyte composite abutting and extending beyond a boundary of the second layer of the electrode layer, portions of the first and second layers of solid electrolyte composite extending beyond the boundary of the first and second sides of the electrode layer abutting and completely encapsulating the electrode, and the portion of the solid electrolyte composite extending beyond the boundary of the first and second sides of the electrode layer has a lower density than the portion of the solid electrolyte composite within the boundary of the first and second sides.

[0018] In one embodiment of the surrounded electrode, the electrode layer comprises one or more active electrode materials including lithium metal or a lithium alloy. In another embodiment of the surrounded electrode, the electrode layer comprises an anode capable of conducting alkali metal ions.

[0019] In one embodiment of the surrounded electrode, the electrode layer comprises a current collector comprising stainless steel or copper foil.

[0020] In one embodiment of the surrounded electrode, the anode includes an engineered coating.

[0021] The present disclosure provides solid-state battery cells having improved solid-state interfaces between the positive electrode layer and the solid electrolyte layer, and between the negative electrode layer and the solid electrolyte layer. Additionally, the present application discloses novel cell structures that promote cycle life, specific cell capacity, and relatively low cell resistance.

[0022] BRIEF DESCRIPTION OF THE DRAWINGS The present disclosure can be understood by reference to the following detailed description taken in conjunction with the drawings, which are briefly described below. It should be noted that, for simplicity of illustration, certain elements in the drawings have not been drawn to scale. FIG. 1A shows a proposed layout of one embodiment of an enclosed electrode structure 105 prior to assembly. FIG. 1B shows a proposed arrangement of one embodiment of the enclosed electrode structure 105 after the three layers are assembled, with the outer boundary 170 of the first SSE and the outer boundary 180 of the second SSE both being longer than the electrode 130 and not attached to the electrode. FIG. 1C shows a proposed configuration of one embodiment of the enclosed electrode structure 105 after assembling the three layers and applying pressure to the structure. FIG. 1D shows the encapsulated electrode structure 105 after continued application of pressure has been applied to the structure, causing SSE 110 and SSE 120 to contact and form an integrated SSE 125, which encapsulates or seals electrode 135. FIG. 2 is a flow chart for a method of forming an enclosed electrode structure. FIG. 3A shows a proposed process for one embodiment of an enclosed electrode structure 310 and shear device 320 in place. FIG. 3B illustrates the proposed treatment of one embodiment of the enclosed electrode structure 310 immediately after shearing has been initiated by the shearing device 320. FIG. 3C illustrates a proposed processing of one embodiment of an enclosed electrode structure 310 after a shearing device 320 shears the solid electrolyte composite along the edge of the enclosed electrode 310 to form an enclosed electrode structure 330 and removes remaining SSE 331. FIG. 4 is a flow chart for a method of partitioning an enclosed electrode structure. FIG. 5A shows the three-dimensional structure of one embodiment of an electrode 500. FIG. 5B shows the three-dimensional structure of one embodiment of solid electrolyte composite layer 540. FIG. 5C shows the three-dimensional structure of one embodiment of an enclosed electrode structure 580 prior to assembling the three layers. FIG. 5D shows a three-dimensional representation of the enclosed electrode structure 590 after a continuous application of pressure has been applied to the layered construct. FIG. 6A is a side view of a calendaring apparatus and a method for forming a protected electrode. FIG. 6B is a top view of the SSE / electrode / SSE stack of FIG. 6A. FIG. 6C is a cross-sectional view of the SSE / electrode / SSE of FIG. 6A taken along line CC. FIG. 6D is a cross-sectional view of the SSE / electrode / SSE stack of FIG. 6A at 618. FIG. 6E is a side view of the SSE / electrode / SSE stack undergoing densification by calender rollers. FIG. 7A is a first set of SEM images of a first example of a protected electrode. FIG. 7B is a second set of SEM images of a second example of a protected electrode. FIG. 7C is a third set of SEM images of a third example of a protected electrode.

[0023] Aspects of the present disclosure are encapsulated electrode structures and methods for their manufacture. Aspects of the present disclosure can provide techniques that can facilitate and be more uniform in the densification of electrode structures, resulting in useful improvements in the performance of electrodes and batteries that include the electrodes. Aspects of the present disclosure can provide the ability to handle soft electrode materials, such as electrodes that include lithium layers, relatively well. For example, by encapsulating a relatively soft electrode in a relatively hard electrolyte material prior to densification, the relatively soft electrode material is captured by the surrounding electrolyte, preventing extrusion of the electrode material under densification pressures, which can be high. These and other advantages of various aspects of the present disclosure are described in more detail below.

[0024] In the following description, specific details are provided to provide a thorough understanding of various aspects of the technology. Moreover, in various embodiments described in the present disclosure, some known methods, processes, devices, and systems are not described in detail to avoid obscuring the technology.

[0025] The term "battery" can be used in various ways in the art and in this description, and can refer to an individual cell having an anode and a cathode separated by an electrolyte, which may be a solid electrolyte, and can also refer to an assembly of multiple such cells connected in various configurations. A solid electrolyte cell can have more than one anode and cathode separated by a solid electrolyte layer, and can ultimately be stored in a flexible "pouch" that accommodates the expansion and contraction of the anode and cathode as the cell is charged and recharged. Although many examples are described in this description as being applicable to batteries or individual cells, it should be understood that the systems and methods described can be applied to many different types of batteries, battery chemistries, and can include batteries that include individual cells to different possible cell interconnections, such as parallel, series, and parallel and series connected cells. The various embodiments described in this disclosure may also be applied to various structural battery devices, such as pouch cells and other cell structures that can accommodate size variations in the electrodes, whether the anode or cathode, or both.

[0026] 1A-1D are a set of schematic illustrations of process steps for forming an enclosed electrode structure 105, and relate to process 200 of FIG. 2. The illustrations shown in FIGS. 1A-1D are schematic cross-sectional views. FIG. 1A shows a proposed configuration of one embodiment of an enclosed electrode structure 105, prior to assembly of three layers that will form the enclosed electrode. One layer of the enclosed electrode structure 105 is a first solid electrolyte composite (SSE) 110, which has an upper surface 140, a lower surface 145, and a peripheral surface 142. The SSE layer may also be referred to as a separator layer. The peripheral surface is the surface that defines the edge between the upper and lower surfaces. References to upper and lower herein are in terms of the structures shown in the drawings and are made so for the convenience of the reader. Manufacturing techniques may provide layers in other arrangements, whereby the upper may be considered lower, the lower may be considered upper, and so on. Another layer of the enclosed electrode structure is the electrode 130, which has an upper (first) surface 160, a lower (second) surface 165, and a surrounding surface 162. Yet another layer of the enclosed electrode structure 105 is the second SSE 120, which has an upper surface 155, a lower surface 150, and a surrounding surface 152. The first SSE 110 is disposed to operatively couple to the electrode 130, with the lower surface of the first SSE 145 operatively coupling to the upper surface of the electrode 160. The lower surface of the electrode 165 operatively coupling to the upper surface of the second SSE 155.

[0027] In some embodiments, the length of each of the SSEs 110 and 120 may be the same or different and may range from 5 millimeters to 1 meter. In another embodiment, the length ranges from 1 cm to 500 cm. In yet another embodiment, the length ranges from 2 cm to 100 cm. In a further embodiment, the length ranges from 2 cm to 50 cm. In another embodiment, the length ranges from 3 cm to 30 cm. In some embodiments, the length of each of the SSEs 110 and 120 may be the same as the length of the electrode 130 or may be longer than the length of the electrode 130. In another embodiment, one of the SSEs 110 or 120 may be slightly shorter than the length of the electrode 130 and the other SSE 110 or 120 may be longer than the length of the electrode 130.

[0028] In some aspects, the width of each of the SSEs 110 and 120 can be between 5 millimeters and 1 meter. In other aspects, the width of each of the SSEs 110 and 120 can be between 1 cm and 500 cm. In yet other embodiments, the width of each of the SSEs 110 and 120 can be between 2 cm and 100 cm. In further aspects, the width of each of the SSEs 110 and 120 can be between 2 cm and 50 cm. In other aspects, the width of each of the SSEs 110 and 120 can be between 3 cm and 30 cm. In some aspects, the width of each of the SSEs 110 and 120 can be the same as the width of the electrode 130 or can be greater than the width of the electrode 130.

[0029] In some embodiments, the height of each of the SSEs 110 and 120 may be between 1 micron and 1 mm. In other embodiments, the height of each of the SSEs 110 and 120 may be between 5 microns and 500 microns. In yet other embodiments, the height of each of the SSEs 110 and 120 may be between 10 microns and 250 microns. In yet other embodiments, the height of each of the SSEs 110 and 120 may be between 15 microns and 200 microns. In other embodiments, the height of each of the SSEs 10 and 120 may be between 20 microns and 100 microns. In some embodiments, the height of each of the SSEs 110 and 120 may be the same as the height of the electrode 130 or may be greater than the height of the electrode 130.

[0030] 1B shows a proposed arrangement of one embodiment of an enclosed electrode structure 105 after the three layers (SSE 110, electrode 130, and SSE 120) are assembled, with the outer boundary 170 of the first SSE and the outer boundary 180 of the second SSE extending beyond the length of the electrode 130 and not contacting the electrode at any point. In an alternative embodiment, at least one of the first SSE 170 and the second SSE 180 is the same length as the electrode, and the other of the first SSE 170 and the second SSE 180 is substantially longer than the electrode 130.

[0031] While various techniques for lamination and densification are possible, in one example, the protected electrode layers are passed through a calender press. In one example, producing an enclosed electrode includes a stack of a center electrode layer, a solid electrolyte (SSE) layer, and a carrier film layer (e.g., an aluminum foil layer), with the carrier film layer being removed prior to use in a cell. The aluminum carrier layer is not shown in FIGS. 1A-1D. In one embodiment, the center electrode layer may be a lithium foil, and the layers may be initially arranged in an aluminum-SSE-lithium-SSE-aluminum stack. The SSE layer includes a sulfide-based solid electrolyte material and a binder and is cast onto the aluminum foil. The stack may be fed into a calender press apparatus including a first roller and a second roller to laminate or otherwise operatively bond the lithium foil layer to the SSE layer. These rollers exert a compressive force on the stack to laminate the layers together while reducing the porosity of the material in the stack (densification), promoting material contact within and between the layers, adhering or otherwise laminating some layers, and / or partially or completely separating some layers (e.g., the outer aluminum foil layers). The pressure applied to the stack by the calender press may be related to the spacing between the first and second rollers.

[0032] FIG. 6A is a diagram illustrating the fabrication of a solid protected electrode stack 602 using a calender press apparatus 604 according to one embodiment of the disclosure. In one embodiment, the protected solid electrode stack 602 may have two separator layers of a composite blend of a solid electrolyte (SSE) and a binder. The SSE 606 may be coated as a thin layer onto a carrier film 608. In one example, the carrier film 608 may be an aluminum foil, however, other materials may be used. A thin foil 610 of lithium metal may be placed between two facing SSE layers 606. To fabricate a protected electrode (e.g., anode) stack, two different sheets of SSE 606 on the foil 608 may be oriented such that the SSE layers face each other with the lithium metal layer 610 between the two SSE sheets. Other combinations of layers and other compositions of layers may be used for other types of stacks, such as for example, for a cathode stack. In this embodiment, the layers forming the electrode stack 602 are applied between the calendar rollers 614, 616 in a stack of aluminum-SSE-lithium-SSE-aluminum. When assembled into a cell, the protected anode is constructed from the SSE-lithium-SSE stack and the aluminum foil is removed. The composite SSE layer 606 in this configuration may conduct ions but not electrons during use in a battery cell, such that the SSE layer may provide electrical isolation with respect to the central lithium anode material layer 610. The respective rollers of the calendar press 604 are spaced apart a distance less than the thickness of the stack before calendaring, such that pressure on the stack applied between the calendar rollers 614, 616 may reduce the porosity of the material within the stack, bond or bond some layers, and / or cause the SSE layer 606 to be partially or completely separated from the aluminum foil 608 while being laminated to the lithium foil 610 layer. It should be understood that in some instances the calender press does not peel off the outer foil layer and a subsequent peeling operation may be used, while in other instances the calendering process weakens the SSE adhesion to the outer foil making subsequent removal more efficient.The pressure exerted on the stack by the calender rollers 614, 616 may be adjusted via a calender controller 612 configured to adjust the space (gap) between the calender rollers. Upon removal of the aluminum foil 608 from the stack, a SSE-Li-SSE stack is produced, which may be used as an anode in an electrochemical cell. Other stacks may have the same or different layer types or layer compositions for use in electrochemical cells.

[0033] FIG. 6B is a top view of the various sheets forming the protected electrode stack, and note that the electrodes, e.g., lithium layers, are recessed (e.g., have a relatively small width) from the outer edges of the SSE sheets. The first 626A and second 626B regions of the upper and lower SSE layers are stacked and densified between the calender rollers to form a protective boundary between the 626A / 626B regions in a portion of the electrode layer 610A. FIG. 6C is a cross-section at CC of the stack before calendering, and FIG. 6D is a side cross-section of the protected electrode stack at point 618 after calendering, highlighting the recession of the inner electrode layers from their respective ends of the SSE layers. From the perspective of FIG. 6B, it can be seen that the lateral ends of the electrode layers are recessed from their respective lateral ends of the SSE layers.

[0034] FIG. 6E is a close-up of the calender rollers 614 and 666, showing how the stack SSE 606 / electrode 610 / SSE 606 is laminated / densified using the rollers. The view in FIG. 6E does not show the aluminum foil 608 layer. FIG. 6E further illustrates how a progressive protective boundary is created in the electrode 610. As the sheet is fed through the calender press, the previously densified portion of the electrode layer 620 (or the portion undergoing densification) is directly adjacent to the portion of the electrode layer 622 that is between the rollers and undergoing densification. The previously densified stack thus forms a protective boundary at the leading edge of the portion of the electrode undergoing densification, in addition to those at the sides of the sheet where the width of the upper and lower SSE layers exceeds the width of the electrode layer, thus providing a third boundary 620 to facilitate densification as the stack progresses between the rollers. It should be noted that the electrode layers in some instances are not densified due to material properties. For example, in the case of a lithium electrode layer, the SSE layer is densified, but the metallic lithium layer is not densified. However, the lithium layer may extrude or flow under densification pressure as shown in this disclosure. Conversely, for example, a non-metallic anode electrode layer, such as a silicon composite, graphite composite, etc., or a cathode layer, such as an NMC composite, pyrite composite, sulfur composite, etc., is densified.

[0035] FIG. 1C shows a proposed arrangement of one embodiment of an enclosed electrode structure 105 after the three layers (SSE 110, electrode 130, and SSE 120) have been stacked and pressure has been applied to the configuration. As pressure is applied, SSE 110 and SSE 120 begin to compress and densify to form SSE 112 and SSE 122, which form around electrode 132, which may also begin to compress and densify. As noted elsewhere, some electrode materials, such as lithium, do not densify, while other electrode materials, such as non-metals, do. In a calendering operation using cylindrical rollers, the initial compression and densification shown in FIG. 1C occurs as the stack is first fed between the rollers, and the final compression and densification shown in FIG. 1D occurs in the region of highest densification pressure where the separation between the upper and lower rollers is minimal.

[0036] Figure 1D shows the enclosed electrode structure 105 after continued application of pressure has been applied to the construct, causing SSEs 110 and 120 to contact one another to form a unified SSE 125, which encases the electrode 135. Referring again to Figure 6D, after the stack goes through a roller densification step in an example using a calendar press, an unified SSE 624 is formed along and around the side 632 of the electrode 610.

[0037] An enclosed electrode structure may refer to an electrode or electrode layer 130 that is enclosed by a solid electrolyte material SSE or one or more solid electrolyte layers SSE such that a first (e.g., upper) and second (e.g., lower) surface of the electrode are in contact with the solid electrolyte material of upper and lower layers that are laminated to respective adjacent SSE layers and that are pressed together to enclose the electrode ends that are recessed from the respective areas where the upper and lower SSE layers contact each other during densification. The electrode may be exposed at at least one end side of the assembled stack, as described in more detail below.

[0038] In some embodiments, an enclosed electrode structure may refer to an electrode or electrode layer that, when referring to a rectangular shaped electrode, is enclosed along at least two ends or sides in a solid electrolyte material. When enclosed, the electrode layer is between solid electrolyte layers such that all faces and at least one side of the electrode or electrode layer are in contact with the solid electrolyte material or one or more solid electrolyte layers. In another embodiment, an enclosed electrode structure may refer to an electrode or electrode layer that is enclosed in a solid electrolyte material or one or more solid electrolyte layers such that all faces and at least two sides of the electrode or electrode layer are in contact with the solid electrolyte material or one or more solid electrolyte layers. In yet another embodiment, an enclosed electrode structure may refer to an electrode or electrode layer that is enclosed in a solid electrolyte material or one or more solid electrolyte layers such that all faces and at least three sides of the electrode or electrode layer are in contact with the solid electrolyte material or one or more solid electrolyte layers. In still further embodiments, an enclosed electrode structure may refer to an electrode or electrode layer that is enclosed in a solid electrolyte layer or layers such that all faces and all but two sides of the electrode or electrode layer are in contact with the solid electrolyte material or layers. The side or sides of the electrode that are not enclosed by the solid electrolyte can provide electrical contact to the electrode to form it into a battery.

[0039] Referring again to FIG. 1B, after densification and defoiling, a protected electrode, e.g., an anode, may be formed by trimming the sheet of SSE-Li-SSE stack into individual sections. The dotted lines shown in FIG. 1B are where such a trimming process may take place. As can be seen, the upper and lower ends (faces) of the electrode are surrounded by the SSE layer, while the front and rear ends (faces) of the electrode are exposed after trimming. As can be seen in FIG. 1D, the upper and lower surfaces of the electrode are also surrounded by the upper and lower SSE layers, respectively.

[0040] In forming an enclosed anode, the electrode 130 may be free-standing and may have a thickness ranging from 1 μm to 1 mm. A free-standing anode is one that does not have an "attached" or separate current collector. In the examples described in this disclosure, when the anode is formed of lithium or an alloy of lithium, the lithium is the active material that provides power to the cell and the current collectors.

[0041] An example of a non-self-supporting type is one in which the active material is disposed on a current collector, for example, lithium deposited on a copper foil. In some embodiments, the anode has a thickness in the range of 2 μm to 750 μm. In another embodiment, the anode has a thickness in the range of 3 μm to 500 μm. In another embodiment, the anode has a thickness of 4 μm to 250 μm. In another embodiment, the anode has a thickness of 5 μm to 150 μm. In another embodiment, the anode has a thickness of 5 μm to 100 μm. In another embodiment, the anode has a thickness of 5 μm to 75 μm. In another embodiment, the anode has a thickness of 5 μm to 50 μm. In another embodiment, the anode has a thickness of 5 μm to 45 μm. In yet another embodiment, the anode has a thickness of 5 μm to 35 μm. In another embodiment, the anode has a thickness of 1 μm to 15 μm.

[0042] In some embodiments of the enclosed anode, electrode 130, may have one or more layers of material. In some embodiments, 2-10 layers may be used. In other embodiments, 2-5 layers may be used.

[0043] In further embodiments, the surrounded anode may be or may include a current collector, such as, but not limited to, stainless steel and copper foil. In one embodiment, the surrounded electrode has 3-10 current collectors. The surrounded anode may have one or more anode active materials in contact with one or more sides of the current collector, examples of active materials include silicon-containing materials (Si, SiO2, Si-lithium alloys, Si-Na alloys), carbon-containing materials (graphite, graphene, carbon black, etc.), aluminum, magnesium, tin, germanium, and titanium-containing, such as LTO (Li4Ti5O 12 ).

[0044] In some applications, it may be necessary for one or more materials contained in the enclosed anode to have an engineered coating on one or more of its surfaces. In some embodiments, one or more of the anode active materials have an engineered coating. In another embodiment, one or more of the current collectors have an engineered coating. In yet another embodiment, the engineered coating is one or more carbon-based materials, such as, but not limited to, graphite, graphene, carbon nanotubes, and carbon black. In a further embodiment, the carbon-based coating may be a composite containing one or more materials that can be alloyed with an alkali metal, such as, but not limited to, Au, Ag, Zn, Zr, In, Ge, Si, Sn, or Al. In another embodiment, the engineered coating may be one or more oxygen-containing species, such as, but not limited to, Li2CO3, Li2O, Li2SO4, Na2CO3, Al2O3, ZrO2, or SiO2. In yet another aspect, the engineered coating can be one or more sulfide-containing species, such as, but not limited to, elemental sulfur, CuS, CuSO4, NiS, NiSO4, or FeS2. In a further aspect, the engineered coating can be one or more nitrogen-containing species, such as, but not limited to, LiNO3, Li3N, Li2NH, LiNH2, LiCN, NaNO3, AgNO3, or Cu(NO3)2. In a further aspect, the engineered coating can be one or more halogen-containing species, such as, but not limited to, LiF, LiCl, LiBr, NaF, KF, Li 0.5 Na 0.5 F, Li 0.5 Na 0.5 Cl, Na 0.5 K 0.5 F, Na 0.5 K 0.5 In yet another embodiment, the engineered coating is one or more phosphorus-containing species, such as, but not limited to, Li3PO4, P2S5, or P2O5. In another embodiment, the engineered coating can be one or more polymers, such as, but not limited to, styrene, butadiene, one or more halogen, sulfur, or nitrogen-containing polymers.

[0045] For surrounded anode engineered coatings, the electrode 130 may have a thickness ranging from 1 nm to 100 μm. In some embodiments, the thickness ranges from 50 μm to 75 μm. In other embodiments, the thickness ranges from 1 μm to 50 μm.

[0046] Similar to forming an enclosed anode, in forming an enclosed cathode, suitable electrodes and suitable solid electrolyte composites 110 and 120 may be prepared. Just as single or multiple layers may be used as electrode 130 in forming an enclosed anode, a multiple layer structure may be used in forming an enclosed cathode. For example, a multiple layer structure, such as one or more cathode active materials in contact with one or more sides of a current collector, may be used as electrode 130. To surround this multiple layer electrode structure, solid electrolyte composites 110 and 120 may be applied as may be done for an anode electrode. In this multiple layer structure, the cathode active material may be an NMC material (a material containing nickel, magnesium, and cobalt), such as, but not limited to, NMC111 (LiNi 0.33 Mn 0.33 Co 0.33 O2), NMC433(LiNi 0.4 Mn 0.3 Co 0.3 O2), NMC532(LiNi 0.5 Mn 0.3 Co 0.2 O2), NMC622(LiNi 0.6 Mn 0.2 Co 0.2 O2), or NMC811(LiNi 0.8 Mn 0.1 Co 0.1In another embodiment, the cathode active material can be a Li-Mn spinel substituted with various elements, such as, but not limited to, Li-Mn-Ni-O, Li-Mn-Al-O, Li-Mn-Mg-O, Li-Mn-Co-O, Li-Mn-Fe-O, or Li-Mn-Zn-O. In another embodiment, the cathode active material can be a lithium metal phosphate, such as, but not limited to, LiFePO4, LiMnPO4, LiCoPO4, LiCoPO4, or LiNiPO4. In another embodiment, the cathode active material can be one or more of LiCoO2 or NCA (nickel, cobalt, aluminum containing materials) (e.g., LiNi 0.8 Co 0.15 Al 0.05 In another embodiment, the cathode active material can be one or more conversion cathodes, such as S, Li2S, TiS2, MoS2, VS2, CrS2, FeS2, FeF2, FeF3, CuF2, or MnO. Additionally, in this multi-layered structure, the current collector can be aluminum, stainless steel, copper, or nickel.

[0047] When forming an enclosed cathode, the cathode may have a thickness of 1 μm to 1000 μm. In some embodiments, the cathode may have a thickness of 3 μm to 900 μm. In other embodiments, the cathode may have a thickness of 5 μm to 800 μm. In other embodiments, the cathode may have a thickness of 10 μm to 700 μm. In other embodiments, the cathode may have a thickness of 12.5 μm to 600 μm. In other embodiments, the cathode may have a thickness of 15 μm to 500 μm. In other embodiments, the cathode may have a thickness of 17.5 μm to 400 μm. In other embodiments, the cathode may have a thickness of 20 μm to 300 μm. In other embodiments, the cathode may have a thickness of 22.5 μm to 200 μm. In still other embodiments, the cathode may have a thickness of 25 μm to 100 μm. In another embodiment, the cathode has a thickness of 25 μm to 75 μm.

[0048] The solid electrolyte composites 110 and 120 may contain a sulfide solid electrolyte and one or more binders, which may be in the form of a polymer, in which case the solid electrolyte composites 110 and 120 may be 0% to 80% by weight of the composite being polymer. In another embodiment, the polymer may be 1% to 70% by weight of the composite. In another embodiment, the polymer may be 3% to 60% by weight of the composite. In another embodiment, the polymer may be 4% to 50% by weight. In another embodiment, the polymer may be 5% to 40% by weight of the composite. In another embodiment, the polymer may be 10% to 30% by weight of the composite.

[0049] The polymer in the solid electrolyte composites 110 and 120 may be one or more fluorine-containing polymers, such as, but not limited to, polytetrafluoroethylene (PTFE), polyvinylene difluoride (PVdF), poly(vinylene difluoride-hexafluoropropylene) copolymer (PVdF-HFP), etc. In another embodiment, a thermoplastic elastomer may be used, such as, but not limited to, styrene-butadiene rubber (SBR), styrene butadiene styrene copolymer (SBS), styrene isoprene copolymer (SIS), polyacrylonitrile (PAN), nitrile butylene rubber (NBR), polybutadiene, polyisoprene, poly(methacrylate) nitrile-butadiene rubber (PMMA-NBR), etc. In another embodiment, acrylic resins may be used, such as, but not limited to, polymethyl(meth)acrylate, polyethyl(meth)acrylate, polyisopropyl(meth)acrylate, polyisobutyl(meth)acrylate, polybutyl(meth)acrylate, etc. In another embodiment, polycondensation polymers may be used, such as, but not limited to, polyurea, polyamide paper, polyimide, polyester, etc., or combinations thereof.

[0050] Solid electrolyte composites 110 and 120 may have one or more sulfide solid electrolytes containing one or more of a lithium-containing element, a phosphorus-containing element, or a sulfur-containing element. In another aspect, solid electrolyte composites 110 and 120 may have one or more oxysulfide solid electrolytes containing one or more of a lithium-containing element, a sulfur-containing element, or an oxygen-containing element. In another aspect, the solid electrolyte composite may contain one or more halogens, for example, one or more of F, Cl, Br, or I. In another aspect, the solid electrolyte composite may contain one or more pseudohalogens, for example, but not limited to, CN, OH, SH, SCH, NH, NH2, NO3, BF4, or BH4.

[0051] Examples of sulfide solid electrolytes include, but are not limited to, one or more of the following: Li2S-P2S5, Li2S-P2S5-LiX, Li2S-SiS2, Li2S-SiS2-LiX, Li2S-SiS2-P2S5, Li2S-SiS2-P2S5-LiX, Li2S-SiS2-B2S3-LiX, Li3N-P2S5, Li3N-Li2S-P2S5-LiX, and Li2S-B2S3; where each component is mixed in a glass or glass-ceramic forming ratio. Examples of oxysulfide solid electrolytes can include one or more of the following: Li2S-P2O5, Li2S-P2O5-LiX, Li3PO4-P2O5-LiX, Li2S-P2S5-Li2O, and Li2S-P2S5-Li2O-LiX; where each component is mixed in a glass or glass-ceramic forming ratio. In some aspects, Li2S-P2S5 may represent one or more of Li3PS4, Li4P2S6, Li7PS6, and Li7P3S 11 and the like. In some aspects, Li2S-P2S5-LiX may represent one or more of Li 7-y PS 6-y X y where 0 < y ≦ 2, and X may be one or more of a halogen or a pseudohalogen. In another aspect, Li2S-P2S5-LiX may represent Li7P2S8X, and X may be one or more of a halogen or a pseudohalogen. In another aspect, Li2S-P2S5-LiX may represent Li8P3S11 X, which may be one or more of a halogen or pseudohalogen.

[0052] Additionally, the solid electrolyte material may vary in its structural makeup. In some embodiments, the solid electrolyte material may have a glass or glass-like structure. In other embodiments, the solid electrolyte material may have a crystalline structure. In other embodiments, the solid electrolyte material may have a ceramic structure. In other embodiments, the solid electrolyte material may have a glass-like ceramic structure.

[0053] One type of solid electrolyte may be used alone, or two or more types of solid electrolyte may be used. When two or more types of solid electrolyte are used, the two or more types of solid electrolyte may be mixed together, or each of the two or more types of solid electrolyte may be formed into two or more layers, so that a multi-layer structure is formed.

[0054] The solid electrolyte composites 110 and 120 may contain one or more materials other than the sulfide electrolyte or polymer. In some embodiments, the material other than the sulfide electrolyte or polymer may be one or more lithium salts, such as, but not limited to, LiPF6, LiBF4, LiClO4, LiN(CF3SO2)2, LiN(FSO2)2, or LiN(CF3CF2SO2). In other embodiments, the material other than the sulfide electrolyte or polymer is one or more oxides, such as, but not limited to, ZrO2 or Al2O3.

[0055] In some embodiments, the solid electrolyte composite layers 110 and 120 may be one or more electrically insulating materials or electrically conductive layers. In other embodiments, the solid electrolyte composites 110 and 120 may be referred to as ionically conductive materials or layers.

[0056] The composition of the solid electrolyte composites 110 and 120 should be formulated so that the solid electrolyte composites 110 and 120 deform and densify appropriately when pressure is applied thereto. The deformation and densification properties may be specified according to given values ​​for Poisson's ratio, viscosity, density, etc. Furthermore, the viscous response of the solid electrolyte composites 110 and 120 may be specified by a given response, such as shear thinning, shear thickening, thixotropy, power law response, etc. Additionally, one or more relationships between the properties of the solid electrolyte composites 110 and 120 and the properties of the electrode 130 may be specified and used for control. Additionally, the solid electrolyte composites 110 and 120 should provide sufficient adhesion to the electrode 130 and should provide sufficient self-adhesion to support the formation of the enclosed electrode 105. The properties of the solid electrolyte composites 110 and 120 and the electrode 130, such as tackiness, surface energy, and wetting properties, may be defined and used for process control. The solid electrolyte composites 110 and 120 may have various volumetric and surface defects (e.g., as indicated by open voids on the surface and inside the solid electrolyte composite 110). These defects, if not removed, may result in reduced life or other performance issues in electrochemical cells constructed therefrom. Additionally, the solid electrolyte composites 110 and 120 may differ in various properties and / or composition. In addition to the thickness and material descriptions above, the surface finish, ductility, malleability, mechanical stiffness (elastic modulus), yield strength, elongation at break, toughness, adhesion, and compressibility may be given values ​​and used for process control. As described throughout the progression of Figures 1A-1D, the various voids and surface defects are reduced in size or effectively eliminated after densification.

[0057] The dimensions of the solid electrolyte composite layers 110 and 120 should be such that when the solid electrolyte composite layers 110 and 120 are in contact with the electrode 130, the boundary between the first surface 145 and the second surface 140 of the solid electrolyte composite layers 110 and 120 extends beyond the boundary between the first surface 160 and the second surface 160 of the electrode 130.

[0058] In some embodiments, the dimensions of the solid electrolyte composite layers 110 and 120 should be such that when the solid electrolyte composite layers 110 and 120 are in contact with the electrode 130, the peripheral surface 142 of the solid electrolyte composite layer 110 and the peripheral surface 152 of the solid electrolyte composite layer 120 extend beyond the peripheral surface 162 of the electrode 130.

[0059] The peripheral surface can be used to refer to at least two surfaces of the electrode layer or solid electrolyte composite layer that are substantially perpendicular to the first and second surfaces of the electrode layer or solid electrolyte composite layer. In some embodiments, the peripheral surface can be used to refer to each individual surface of the electrode layer or solid electrolyte composite layer that is substantially perpendicular to the first and second surfaces of the electrode layer or solid electrolyte composite layer.

[0060] The portion of the solid electrolyte composite layer 110 that extends beyond the boundary of the first surface 160 of the electrode layer 130 when in contact with the electrode 130 may be referred to as the solid electrolyte composite layer outer edge 170 ( FIG. 1B ). In some embodiments, the solid electrolyte composite layer outer edge 170 may be expressed by the difference between the width of the first surface 145 of the solid electrolyte composite layer 110 and the width of the first surface 160 of the electrode 130 when the solid electrolyte composite layer 110 and the electrode 130 are in contact or electrical contact. In other embodiments, the solid electrolyte composite layer outer edge 170 may be expressed by the difference between the length of the first surface 145 of the solid electrolyte composite layer 110 and the length of the first surface 160 of the electrode 130 when the solid electrolyte composite layer 110 and the electrode 130 are in contact or electrical contact. The portion of the solid electrolyte composite layer 120 that extends beyond the boundary of the first surface 165 of the electrode 130 when in contact with the electrode 130 may be referred to as the solid electrolyte composite layer outer edge 180. In some embodiments, the solid electrolyte composite layer outer edge 180 may be represented by the difference between the width of the first surface 155 of the solid electrolyte composite layer 120 and the width of the first surface 165 of the electrode 130 when the solid electrolyte composite layer 120 and the electrode 130 are in contact or electrical contact. In other embodiments, the solid electrolyte composite layer outer edge 180 may be represented by the difference between the length of the first surface 155 of the solid electrolyte composite layer 120 and the length of the first surface 165 of the electrode 130 when the solid electrolyte composite layer 120 and the electrode 130 are in contact or electrical contact.

[0061] In some embodiments, the solid electrolyte composite layer outer end 170 and the solid electrolyte composite layer outer end 180 may have different overall areas, and the width of the solid electrolyte composite layer outer end 170 may be smaller than the width of the solid electrolyte composite layer outer end 180. In another embodiment, the width of the solid electrolyte composite layer outer end 170 may be larger than the width of the solid electrolyte composite layer outer end 180. In a further embodiment, the solid electrolyte composite layer 110 may have a width larger than the width of the solid electrolyte composite layer 120. In an even further embodiment, the solid electrolyte composite layer 110 may have a width larger than the width of the solid electrolyte composite layer 120. In an even further embodiment, the solid electrolyte composite layer 110 may have a width smaller than the width of the solid electrolyte composite layer 120. In another embodiment, the length of the solid electrolyte composite layer 110 may be larger than the length of the solid electrolyte composite layer 120. In yet another embodiment, the length of the solid electrolyte composite layer 110 may be smaller than the length of the solid electrolyte composite layer 120.

[0062] In some embodiments, the dimensions of the solid electrolyte composite layers 110 and 120 should be such that when the solid electrolyte composite layers 110 and 120 are in contact with the electrode 130, the peripheral surface 142 of the solid electrolyte composite layer 110 and the peripheral surface 152 of the solid electrolyte composite layer 120 extend beyond only one side, S1, of the peripheral surface 162 of the electrode 130. In other embodiments, the dimensions of the solid electrolyte composite layers 110 and 120 should be such that when the solid electrolyte composite layers 110 and 120 are in contact with the electrode 130, the peripheral surface 142 of the solid electrolyte composite layer 110 and the peripheral surface 152 of the solid electrolyte composite layer 120 extend beyond two sides of the peripheral surface 162 of the electrode 130, and the two surfaces S1 and S3 are parallel to each other. In yet another embodiment, the dimensions of the solid electrolyte composite layers 110 and 120 should be such that when the solid electrolyte composite layers 110 and 120 are in contact with the electrode 130, the peripheral surface 142 of the solid electrolyte composite layer 110 and the peripheral surface 152 of the solid electrolyte composite layer 120 extend beyond three sides of the peripheral surface 162 of the electrode 130, and two sides S1 and S3 may be parallel to each other while being perpendicular to the other side, S2. In yet a further embodiment, the dimensions of the solid electrolyte composite layers 110 and 120 should be such that when the solid electrolyte composite layers 110 and 120 are in contact with the electrode 130, the peripheral surface 142 of the solid electrolyte composite layer 110 and the peripheral surface 152 of the solid electrolyte composite layer 120 extend beyond four sides of the peripheral surface 162 of the electrode 130, where two sides, S1 and S3, may be parallel to each other, and two sides, S2 and S4, may be parallel, however, S1 and S3 may be perpendicular to S2 and S4.

[0063] Referring to FIG. 2, process 200 begins at step 210, where various materials to be used in the enclosed electrode structure may be prepared. For example, to form an enclosed electrode structure including an enclosed anode structure, an anode active material may be selected for the electrode, such as a metal foil made of one or more alkali metals, such as, but not limited to, Li, Na, or K. In another embodiment, the enclosed anode active material may be one or more alkali metal alloys, such as, but not limited to, Li-Al, Li-Zn, Li-Mg, Li-Na, Li-K, Li-Na-K, Li-In, Li-Au, Li-Ag, Na-Al, or Na-Zn. In yet another embodiment, the enclosed anode active material may be one or more alkaline earth metals, such as, but not limited to, Mg, Ca, or Ba. In a further embodiment, the surrounded anode active material may be one or more alkaline earth metal alloys, for example, but not limited to, Mg-Al, Mg-Zn, Mg-Ca, Mg-Na, Ca-Al, or Ca-Zn. In yet a further embodiment, the surrounded anode may be one or more materials with which lithium is deposited, the materials alloying with lithium being, for example, but not limited to, silicon metal, silicon-carbon composite, Ag, Au, Sn, Pb, In, Ni, Al, or Sb. To form the surrounded anode, a solid electrode composite may be prepared as appropriate for use with the selected electrode material. In step 220, the SSE and electrodes are layered. In step 230, the SSE and electrodes are contacted to form a stack. In step 240, pressure is applied to the stack. In step 250, the stack is formed, in particular the SSE layer is formed around the electrodes so that the edges are covered, and pressure is applied and the electrodes are surrounded by the SSE.

[0064] In step 220, the prepared electrode 130 and solid electrolyte composites 110 and 120 may be layered in preparation for contacting in step 230 (FIG. 1B). In some examples, a dendrite-inhibiting layer may be included between the electrode 130 and the solid electrolyte composite layers 110 and 120. Additionally, various surface treatments may be applied to the electrode 130 or the solid electrolyte composites 110 and 120 to improve wettability, deformation, and / or defect conditions. After contacting, during step 240, pressure is applied substantially perpendicular to the outer surfaces of the contacted and layered electrode 130 and the solid electrolyte composites 110 and 120. The pressure may be applied uniformly or may be spatially varying across the surface of the solid electrolyte composite external to the layered material. The pressure may be applied non-uniformly via fixed rigidity mechanical means or in a conformal manner via air or hydraulic means. As described above, in one possible example, calender rollers may be used.

[0065] As pressure is applied to the solid electrolyte composites 110 and 120, the portions of the solid electrolyte composites 110 and 120 within the boundaries of the first and second faces 160 and 165 of the electrode 130 begin to compress and densify while the SSE layers at the outer edges contact and surround the electrodes. Initially, the density of the portions of the solid electrolyte composites 110 and 120 beyond the boundaries of the first and second faces 160 and 165 of the electrode 130, indicated at 170 and 180, remains substantially unchanged (FIG. 1B), but then also begins to densify. If a calender roller with some separation distance is applied uniformly to the stack, including both where the electrodes are and where the two SSE layers abut, the relative thickness difference between where the two abutting SSE layers are and the relatively thick regions where the upper and lower SSE layers have an electrode layer between them results in a gradual and relatively low densification pressure where only the two SSE layers abut. However, due to the encirclement, the relatively large pressures are concentrated in the densification and lateral extrusion does not occur, or any lateral extrusion is quickly suppressed as the encirclement forms.

[0066] In some instances, the densification process is established such that the outer edge regions of the SSE layers abut and encase the electrode prior to application of significant pressure that may result in lateral extrusion of the electrode material. In this way, the electrode is encased prior to application of pressure that would otherwise result in lateral extrusion of the electrode material. In such cases, for example, a first "light" lamination pressure may be applied, thereby allowing the SSE to form around the electrode. A second "heavy" lamination may then be applied, thereby sufficiently densifying the layers to form a protected electrode. The light and heavy pressures will depend on the materials present, the electrode extrusion characteristics, etc. Such techniques may be particularly useful when relatively thick electrodes are used that require the SSE layers to deform more around the edges of the electrode before the SSE layers can contact and fuse. However, in many cases, a constant lamination pressure may be applied (not two or more pressures) and only one lamination / densification step is required to allow the SSE layers to fuse before lithium is extruded beyond the SSE layers. In the case of lithium, for example, some lithium flow or extrusion may occur, but fusion of the SSE layers occurs so quickly that very small lateral flows of lithium do not result in significant effects.

[0067] Continued application of pressure to the solid electrolyte composites, now 112 and 122, may further compress and densify the portions of the solid electrolyte composites 112 and 122 that are within the boundaries of the first and second sides 160 and 165 of the electrode 130. During this compression and densification, the portions of the solid electrolyte composites 112 and 122 that are beyond the outer boundaries of the first and second sides 160 and 165 of the electrode 132 may come into contact to form the enclosed electrode 105. Continued application of pressure may cause the portions of the solid electrolyte composites 112 and 122 that are within the boundaries of the first and second sides 160 and 165 of the electrode 132 to reach a desired density. Additionally, the density of the portions of solid electrolyte composites 170 and 180 that are now in contact increases, but remains less dense than the density of the portions of solid electrolyte composites 112 and 122 that are within the boundaries of first surface 160 and second surface 165 of electrode 132.

[0068] In some embodiments, portions of the solid electrolyte composite beyond the boundary of the first surface 160 and the second surface 165 of the electrode 132 may contact and fuse during the densification process.

[0069] During application of pressure, the electrode 130 may deform through various stages, an initial deformation to electrode 132, and a final deformation to the relatively thin electrode 135. This deformation of the electrode is limited due to its encapsulation by the solid electrolyte composite 125, which provides mechanical encapsulation of the electrode. This physical structure allows for application of pressure well beyond the pressure point where the electrode active material, such as lithium metal or lithium metal alloy, would otherwise deform and flow in an undesirable manner. Fully encapsulating the lithium metal or other electrode active material with the solid electrolyte composite prior to full densification of the layer prevents the lithium or other electrode active material from extruding beyond the peripheral surfaces 142 or 152 of the solid electrolyte composites 110 and 120 and otherwise deforming in an undesirable manner.

[0070] As the density of the solid electrolyte composites 110 and 120 increases, their ionic conductivity increases. Due to the difference in density, the portions of the solid electrolyte composites 110 and 120 that are within the boundaries of the first and second faces 160 and 165 of the electrode 130 may have a relatively higher ionic conductivity than the portions of the solid electrolyte composites 110 and 120 that are outside the boundaries of the first and second faces 160 and 165 of the electrode 130. Since ions preferentially follow the path of least resistance (highest ionic conductivity), ionic conduction occurs primarily within the boundaries of the first and second faces 160 and 165 of the electrode 130 or within the peripheral surface 162 of the electrode 130.

[0071] As the application of pressure and the resulting densification process continues, possible defects in the solid electrolyte composites 110 and 120 may be reduced. Densification may utilize times ranging from 0.01 seconds to 5 minutes and pressures ranging from 100 psi to 400,000 psi. In another embodiment, the pressure may range from 500 psi to 50,000 psi. In a further embodiment, the pressure may range from 1000 psi to 20,000 psi. The applied pressure may vary with time under pressure, for example, with an incremental ramp of 100 to 1000 psi / s, within a range of 0.01 s to 300 s. Densification and / or calendering may be performed at a temperature range of about -10°C to 200°C. In another embodiment, the temperature range may be 0°C to 150°C. In another embodiment, the temperature range may be 10°C to 125°C. In another embodiment, the temperature range may be 25°C to 120°C. In another embodiment, the temperature range may be from 45° C. to 115° C. In another embodiment, the temperature range may be from 70° C. to 110° C. The external pressure and / or temperature may be constant or variable over the duration of the process used.

[0072] Pressure must be applied appropriately so that the solid electrolyte composites 110 and 120 come into contact and complete the enclosure in step 250. In some embodiments, the solid electrolyte composites 110 and 120 may adhere under the applied pressure.

[0073] If insufficient pressure is used, the solid electrolyte composites 110 and 120 or 112 and 122 may not be in contact with each other. If adhesion of the solid electrolyte composites 110 and 120 is desired, if insufficient pressure is used, the adhesion of the contacting portions may be insufficient to ensure sealing of the enclosure. Alternatively, if too much pressure is used, the solid electrolyte composites 110 and 120 may deform in a non-uniform manner, may wrinkle and / or distort, and result in a defective enclosure.

[0074] When densified solid electrolyte composites 110 and 120 are used, the portions extending beyond the boundary of the first and second sides of the electrode 130, referred to as 170 and 180, may not be sufficiently adhered and may not fully complete the enclosure. To aid in the formation of the portions extending outside the boundary of the first and second sides of the electrode 130, referred to as 170 and 180, the solid electrolyte composites 110 and 120 may vary with respect to their extension beyond the first and second boundaries of the electrode 130, referred to as 170 and 180. This difference may be due to the width (W SEC ) of the width (W E ) may be expressed by comparing the ratio to

[0075] If the yield strength of one or more materials of the electrodes is less than the pressure required to densify the solid electrolyte composites 110 and 120, the width of the solid electrolyte composite layer before densification may be greater than the width of the electrode 130, or W SEC ≧W E It may be. W SEC ≧W EHaving this configuration allows the solid electrolyte composite to fully surround the electrode 130 and prevents one or more materials of the electrode from extending beyond the peripheral surfaces 142 and 152 of the solid electrolyte composites 110 and 120 when a pressure greater than the yield strength of one or more of the electrode components is applied. If the electrode is not fully surrounded and a pressure greater than the yield strength of one or more of the electrode components is applied, one or more of those components may be extruded beyond the peripheral surfaces 142 and 152 of the solid electrolyte composites 110 and 120. This may cause a short circuit in the electrochemical cell.

[0076] The electrode 130 may comprise one or more materials having a room temperature compressive yield strength of between 50 psi and 400,000 psi. In some embodiments, when the electrode comprises a material such as lithium metal, the electrode may have a room temperature yield strength of 105 psi. In another embodiment, when the electrode comprises a material such as copper, the electrode may have a room temperature yield strength of 9000 psi. In another embodiment, when the electrode comprises a material such as magnesium, the electrode may have a room temperature yield strength of 30,000 psi. In a further embodiment, when the electrode comprises a material such as steel, the electrode may have a room temperature yield strength of 380,000 psi.

[0077] 3A-3C are illustrations of a set of process steps for sectioning an enclosed electrode. In FIG. 3A, the enclosed electrode 310 and the shearing device 320 may be appropriately positioned. In FIG. 3B, the shearing device 320 may be brought into contact with the enclosed electrode 310 and shearing may be initiated. In FIG. 3C, the shearing device 320 may be designed with cutting ends and bodies that facilitate shearing of the solid electrolyte composite along the edge of the enclosed electrode 310 and transport of the solid electrolyte composite surrounding the electrode itself, such that the enclosed electrodes 330 and 331 to be sectioned are formed to be trimmed by the shearing action.

[0078] In some aspects, the shearing device may have one or more cutting features, such as polymeric, metallic, or ceramic blades or tips. In other embodiments, the shearing device may be a device capable of generating an electromagnetic radiation source, such as a microwave, infrared, visible, or ultraviolet, or electromagnetic radiation source, and may be in the form of a laser. In further aspects, the shearing device may be capable of generating plasma at various temperature ranges ranging from room temperature to 1500°C.

[0079] Process 400 begins at step 410, where the surrounded electrode may be prepared for segmentation. Preparation may include, for example, bringing the surrounded electrode to an appropriate temperature for segmentation. At process step 420, the surrounded electrode and shear device may be properly positioned. At step 430, the shear device may be brought into contact with the surrounded electrode and shearing may commence. At step 440, the shear device may be removed and at step 450, the segmented material may be separated. Process 400 ends at step 460, where subsequent applications of process 200 after FIG. 2 may be followed to ensure re-envelopment or removal of any additional defects.

[0080] 5A is a three-dimensional view of an electrode 500 (also shown in FIGS. 1A and 1B). The electrode 500 may have multiple surfaces, including a circumferential surface 510, a first surface 520, and a second surface 530. In some embodiments, the circumferential surface 510 may be substantially perpendicular to the first surface 520 and the second surface 530.

[0081] 5B shows a three-dimensional view of solid electrolyte composite 540 (also shown as SSE 110 and / or 120 in FIGS. 1A and 1B). SSE 540 may have multiple faces and may have a peripheral face 550, a first face 560, and a second face 570. In some embodiments, peripheral face 550 may be substantially perpendicular to first face 560 and second face 560.

[0082] 5A-5D, it should be understood that the representations of the electrodes and SSEs are not necessarily to scale. In many instances, the thickness of the peripheral portions of these components will be relatively small compared to the depicted lengths and thicknesses. Thus, the peripheral surface of the electrodes will be closer to the edge or boundary.

[0083] The solid electrolyte composite layer 540 may be configured such that the solid electrolyte composite is applied to the carrier in the form of a slurry, dry powder, melt, solution, or deposit. This is completed in such a manner that a layer is formed when the solid electrolyte composite is applied to the carrier. This may be accomplished, for example, by coating, casting, dry powder, or deposition. The carrier may comprise one or more metal foils or plastic films. In some embodiments, the carrier may be removed from the solid electrolyte composite layer 540 before or after compression or densification.

[0084] 5C is an illustration of an enclosed electrode structure 590 before the layers are assembled, which is a three-dimensional view of the enclosed electrode structure before the layers are assembled. One layer of the enclosed electrode structure 590 is a first solid electrolyte composite (SSE) 541, which has a top surface 561, a bottom surface 571, and a peripheral surface 554. Another layer of the enclosed electrode structure 590 is an electrode 505, which has a top surface 521, a bottom surface 531, and a peripheral surface 556. Yet another layer of the enclosed electrode structure 590 is a second SSE 542, which has a top surface 572, a bottom surface 562, and a peripheral surface 555. The first SSE 541 is disposed to adhere to the electrode 505, with the bottom surface 571 of the first SSE adhered to the top surface 521 of the electrode. The bottom surface 531 of the electrode is attached to a top surface 572 of the second SSE.

[0085] FIG. 5D shows the enclosed electrode structure 590 after continued application of pressure has been applied to the structure, with SSE 541 and SSE 542 contacting to form an integrated SSE 525, which encases electrode 535.

[0086] 7A-7C show scanning electron microscope (SEM) images of three different protected electrode stacks, eg, SSE-electrode-SSE, processed according to the techniques described herein.

[0087] In all examples, the electrolyte material is a Li3PS4 sulfide electrolyte. Prior to formation of the protected electrodes, the electrodes were 35 μm thick, approximately 1 in 2 The lithium metal squares were then kept in an argon environment prior to formation.

[0088] To form the solid electrolyte layer (separator layer), 92% w / w Li3PS4 sulfide electrolyte and 8% w / w styrene butadiene rubber (SBR) were mixed with xylene using a Flacktek mixer. The mixture was then cast onto an aluminum 25 μm thick carrier foil using a 200 μm blade. The coated layer was then dried under inert conditions. The solid electrolyte layer was then deposited on a 1.9 in. 2 or approximately 1.375 in length and width.

[0089] The SSE layers had a width approximately 0.375 inches greater and a length 0.375 inches greater than the electrode layers. Thus, if a square electrode were centered between the square SSE layers, there would be approximately 0.1875 inches of outer edges of the upper and lower SSE layers facing each other with no electrode material between them. During formation and densification, the approximately 0.1875 inch border areas of the SSE material meet, forming the electrode protection boundary described herein. This protrusion surrounds the electrode on all four sides, so that this protection forms a square perimeter around the electrode.

[0090] To demonstrate the effectiveness of the protected electrode technology described herein and some of its features, three different experiments were performed on the sample materials described above.

[0091] In a first example, a protected electrode was formed as follows: A square piece of lithium metal foil, as described above, was centered over a first 45 μm thick SSE layer such that the lithium metal was in contact with the solid electrolyte. In this configuration, the length and width of the solid electrolyte layer extended approximately 0.1875 inches beyond the length and width of the lithium metal foil. A second 45 μm thick SSE layer was centered over the lithium metal foil such that the solid electrolyte was in contact with the lithium metal foil. In this configuration, the length and width of the second solid electrolyte layer extended approximately 0.1875 inches beyond the length and width of the lithium metal foil. The resulting stack was constructed such that the layers were in the following order: a layer of aluminum foil, followed by a separator layer containing solid electrolyte, followed by a layer of lithium metal, followed by a separator layer containing solid electrolyte, followed by a layer of aluminum foil. As noted above, the SSE layers abut directly against one another at a square perimeter around the electrode, with the abutment dimension being 0.1875 inches.

[0092] The stack was then placed in a press and laminated at room temperature by applying a pressure of about 4200 psi (or 8200 psi) for a period of 4 seconds, after which the pressure was removed. FIG. 7A is an SEM image through a slice of the protected electrode structure 700 showing the electrode 702, the upper (first) SSE layer 704, the lower (second) SSE layer 706, and the boundary region 708, where the upper and lower SSE layers are laminated together to form a homogenous, unified, "fused" material with no visually discernible boundary between them. In some instances, for example with a larger SSE grain size than in the illustrated example, the SSE layers may not fuse, but instead form an interlocking network that may prevent extrusion of the electrode. The stacking of the upper and lower SSE layers also forms an enveloping (protective) region at the periphery of the electrode, thereby inhibiting the electrode from extruding and facilitating the densification process between the SSE layers and the electrode.

[0093] In the example of Figure 7A, little or no extrusion of the electrode occurred before the SSE layers fused to form boundary region 708. Thus, as shown, the electrode at the boundary region defines a blunt end, reflecting little or no extrusion. This is in contrast to the relatively sharper electrode that results from some extrusion and is described in more detail below with respect to Figures 7B and 7C.

[0094] The protected electrode structure of the second example was prepared in the same manner as the first example, except that the stack was laminated by applying a pressure of about 8400 psi for a period of 4 seconds, and removing the pressure after 4 seconds. Thus, the lamination pressure was about twice that applied in the first example. FIG. 7B is an SEM image through a slice of the protected electrode structure 710, showing the electrode 712, the upper (first) SSE layer 714, the lower (second) SSE layer 716, and the boundary region 718, where the upper and lower SSE layers were laminated together to form a homogenous material with no visibly discernible boundary between them. The stacking of the upper and lower SSE layers also formed an enclosing (protective) region at the periphery of the electrode, which inhibited the electrode from extruding and facilitated the densification process between the SSE layers and the electrode.

[0095] In FIG. 7B (and FIG. 7C), the electrode defines a pointed region 730 (pointed region 732) where SSE layer 714 and SSE layer 716 have fused and an interface region 718. The pointed region indicates that the electrode has been pushed very slightly toward the interface region as lamination pressure is applied to the stack to fuse the SSE layers and protect the electrode. The SEM images are along a cross section of the densified stack. Extending outward to the pointed region 730, the electrode defines two faces that converge at a tip. Similarly, the SSE layers define two surfaces that converge toward the interface region where they are fused. In both FIG. 7B and 7C, SEM images at the respective tips 730 and 732 are shown along with angle and thickness measurements. Referring first to Figure 7B, the tip is at about 38 degrees, with the upper and lower SSE layers at an angle of 19 degrees relative to the plane of the unextruded electrode (or 71 degrees, as shown in the figure, relative to a perpendicular line between the upper and lower planes of the unextruded electrode). Referring to Figure 7C, the tip is at about 49 degrees, with the upper and lower SSE layers at 24 and 25 degrees (or 66 and 65 degrees, as shown in the figure). Overall, the angles of the pointed regions can range from 10 degrees to 60 degrees.

[0096] To further illustrate the formation of the protective boundary of the fused upper and lower layers, as well as the slight extrusion that terminates as the boundary forms, Figures 7B and 7C also include SEM images with electrode thickness measurements at the points where the respective tips form.

[0097] In the final example of FIG. 7C, a protected electrode structure was prepared in the same manner and with the same pressure as in the second example, except that the first and second SSE layers used had a thickness of 75 μm. The electrode layer thickness was the same in all three examples. FIG. 7C is an SEM image through a slice of a protected electrode structure 720, showing an electrode 722, an upper (first) SSE layer 724, a lower (second) SSE layer 726, and a boundary region 728, where the upper and lower SSE layers were laminated together to form a homogenous material with no visually discernible boundary between them. The stacking of the upper and lower SSE layers also formed an enveloping (protective) region at the perimeter of the electrode, which inhibited extrusion of the electrode and promoted the densification process between the SSE layers and the electrode.

[0098] Table 1 shows the gap difference between the three examples. As can be seen, the gap size is generally smaller in the SSE layers above and below the electrode compared to the gap thickness of the SSE layers outside the boundary of the electrode. At higher lamination pressures, as can be seen, the difference in gap size between the three layers and the boundary region where there are only two layers of abutting SSE is substantially higher compared to lower lamination pressures. [Table 1]

[0099] As seen from the experimental data and SEM images, by surrounding the electrode during densification, the void size can be reduced more substantially where the electrode and SSE layer are located compared to the outer edge region where the SSE layer abuts and surrounds the electrode. It is further understood that by surrounding the electrode, a higher relative densification (smaller void size) can occur compared to the densification of a similar structure under the same pressure with only the difference between a surrounded and unsurrounded electrode. In the case of an unsurrounded electrode, some material would be pushed laterally under the densification pressure, especially when considering the relatively soft lithium anode material, whereas by capturing the electrode through the surrounding by the SSE layer, the lateral extrusion is prevented by the relatively hard SSE material, thereby increasing the relative efficiency of the densification process for the relatively reduced void size and providing a relatively large material contact between the electrode layer and the SSE layer.

[0100] The features described above and in the claims may be combined in various ways without departing from the scope thereof. It should therefore be noted that the matters contained in the above description or shown in the accompanying drawings should be interpreted as explanatory and not in a limiting sense. The above-described aspects should be considered as examples and should not be considered as limiting the scope of the present disclosure. In addition to the above aspects, a review of the detailed description and the accompanying drawings will show that there are other aspects. Thus, many combinations, permutations, variations, and modifications of the above aspects not expressly shown in this disclosure will still be within the scope of the present disclosure. The claims are intended to include the general and specific features described in this disclosure, and are intended to include all descriptions of the scope of the present method and system, which may be included for convenience of language.

Claims

1. An electrode layer, and solid electrolyte complex Including, the solid electrolyte composite is in contact with and surrounds the electrode layer; An enclosed electrode for an electrochemical cell.

2. 10. The enclosed electrode for an electrochemical cell of claim 1 comprising one or more electrode active materials.

3. 10. The surrounded electrode for an electrochemical cell of claim 1, wherein at least an upper surface, a lower surface, and at least two sides are surrounded by the solid electrolyte composite.

4. 10. The enclosed electrode for an electrochemical cell of claim 1 comprising one or more anode active materials or one or more cathode active materials.

5. 10. The enclosed electrode for an electrochemical cell of claim 1 comprising one or more of an alkali metal, an alkaline earth metal, a transition metal, or an alloy thereof.

6. 10. The enclosed electrode for an electrochemical cell of claim 1, wherein the enclosed electrode comprises lithium metal or a lithium metal alloy.

7. The enclosed electrode for an electrochemical cell of claim 1 , wherein the electrode layer comprises one or more electrode layers.

8. 10. The enclosed electrode for a solid-state electrochemical cell of claim 1, wherein the solid electrolyte composite comprises one or more solid electrolyte materials.

9. 10. The enclosed electrode for a solid electrochemical cell of claim 1, wherein the solid electrolyte composite comprises one or more polymers in an amount of 0.5% to 80% by weight of the solid electrolyte composite.

10. 10. The enclosed electrode for a solid-state electrochemical cell of claim 9, wherein the one or more polymers comprise at least one thermoplastic elastomer.

11. 10. The enclosed electrode for a solid-state electrochemical cell of claim 9, wherein the one or more polymers comprise fluorine.

12. 10. The enclosed electrode for a solid-state electrochemical cell of claim 1 , wherein the electrode layer comprises one or more solid sulfide electrolytes.

13. 10. The enclosed electrode for a solid-state electrochemical cell of claim 1 comprising an engineered surface coating comprising one or more of the elements lithium, carbon, or oxygen.

14. 2. The enclosed electrode for a solid-state electrochemical cell of claim 1, wherein the engineered surface coating has a thickness of from 1 nm to 100 μm.

15. 13. The enclosed electrode for a solid-state electrochemical cell of claim 1 comprising an enclosed anode or an enclosed cathode.

16. 1. A method for making an enclosed electrode for a solid-state electrochemical cell, comprising: Providing an enclosed electrode; disposing the surrounded electrode between two layers of a solid electrolyte composite, wherein the electrode and the two layers of the solid electrolyte composite define a stack, a portion of the stack including at least three layers including the electrode and the two solid electrolyte composites, and another portion of the stack including at least the two layers of the solid electrolyte composite and not including the electrode; and compressing the stack to contact and surround the electrode, where the other portion of the stack is densified and surrounds a side of the electrode adjacent the other portion; A method comprising:

17. 17. The method of claim 16, wherein the compressing comprises applying a pressure in the range of 100 to 400,000 PSI, thereby densifying and deforming the solid electrolyte composite so that two or more surfaces of the enclosed electrode are covered.

18. 1. An enclosed electrode for an electrochemical cell, comprising: an electrode layer having a first surface, a second surface, and a surrounding surface; a first layer of solid electrolyte composite in contact with and extending beyond the boundary of the first surface of the electrode layer; a second layer of solid electrolyte composite in contact with and extending beyond the boundary of the second surface of the electrode layer; Including, A portion of the first layer and the second layer of the solid electrolyte composite that extends beyond the boundary between the first surface and the second surface of the electrode layer contacts and surrounds the electrode, and a portion of the solid electrolyte composite extending beyond the boundary between the first surface and the second surface of the electrode layer has a density lower than a density of a portion of the solid electrolyte composite within the boundary between the first surface and the second surface. An enclosed electrode for an electrochemical cell.

19. 20. The enclosed electrode of claim 18, wherein the electrode layer comprises one or more active electrode materials including lithium metal or a lithium alloy.

20. 20. The enclosed electrode of claim 18, wherein the electrode layer comprises an anode capable of conducting alkali metal ions.

21. 20. The enclosed electrode of claim 18, wherein the electrode layer comprises a current collector comprising stainless steel or copper foil.

22. 21. The enclosed electrode of claim 20, wherein the anode comprises an engineered coating.

23. 20. The surrounded electrode of claim 18, wherein the first surface portion and the second surface portion converge to a pointed region where the electrode is surrounded by portions of the first and second layers of solid electrolyte composite that extend beyond the boundaries of the first and second surfaces of the electrode layer.

24. 24. The enclosed electrode of claim 23, wherein the pointed region forms an angle in the range of 10 degrees to 60 degrees.

25. 20. The surrounded electrode of claim 18, wherein the electrode is extruded during densification such that the first surface portion and the second surface portion converge into a pointed region, and the extrusion occurs until the electrode is surrounded.

Citation Information

Patent Citations

  • Stacked battery and manufacturing method therefor

    JP2007273349A

  • Thin film electrochemical cell for lithium polymer battery and method for manufacturing the same

    JP2008517433A

  • Method for manufacturing all-solid battery

    JP2015153663A

  • electrodes of solid-state batteries

    JP2015534242A

  • METHOD FOR MANUFACTURING LAMINATED STRUCTURE ALL-SOLID BATTERY

    JP2016507865A

Cited By

  • Method for manufacturing electrode

    WO2026110746A1