Novel conductive additives in lithium and sodium batteries.
The use of a porous carbon network with carbon nanofibers as conductive additives addresses the limitations of lithium and sodium batteries by enhancing conductivity and stability, leading to faster charging and discharging rates and improved safety.
Patent Information
- Application Number
- JP2024525832
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-26
- Filing Date
- 2022-10-25
- Publication Date
- 2024-10-31
AI Technical Summary
Lithium batteries face challenges such as scarcity of resources, rising prices, and low reuse rates, while sodium batteries suffer from low coulombic efficiency and poor rate capacity, necessitating improved conductive additives to enhance charging and discharging rates, reduce internal resistance, and increase battery lifetime.
Incorporating a porous, chemically interconnected carbon network comprising carbon nanofibers as conductive additives in the anodes and/or cathodes of lithium and sodium batteries, which enhances electronic conductivity and mitigates the 'shuttle effect' in lithium-sulfur batteries.
The carbon nanofiber networks improve charge/discharge rates, reduce charging time, and enhance the stability and safety of lithium and sodium batteries, allowing for rapid charging and discharging without compromising safety.
Smart Images

Figure 2024540213000006 
Figure 2024540213000007 
Figure 2024540213000008
Abstract
Description
[Technical field]
[0001] The present invention is in the field of lithium and sodium batteries. In particular, the present invention relates to conductive additives in the anode and / or cathode of rechargeable lithium and sodium batteries. The present invention preferably relates to sodium-ion and lithium-ion batteries, most preferably lithium-ion batteries (including lithium-sulfur batteries). [Background technology]
[0002] There are various types of batteries available, but today lithium is the first choice for the negative electrode material. The reason is the specific capacity of lithium, which is much higher than that of zinc and lead, for example. Lithium is the lightest and most electropositive metal with high energy and power density. The demand for lithium batteries or "lithium secondary batteries" continues to increase, especially as a power source for portable electronic devices, such as smartphones or laptops (including their liquid crystal displays (LCD) or organic light emitting diodes (OLED)), energy storage for power generation equipment (i.e., from surplus wind and solar renewable energy), uninterruptible power supplies (UPS), and a power source for driving the motors of electric and hybrid vehicles.
[0003] Lithium batteries are the most widely used power batteries, but the production of lithium batteries faces great challenges, such as increasing scarcity of lithium resources, rising prices of upstream materials, and low recycling rates. To overcome these challenges of lithium batteries, sodium batteries, which utilize the intercalation process of sodium ions between the positive and negative electrodes, have become a solid alternative choice. The advantages of sodium batteries are that the reserves of sodium resources are much more abundant than those of lithium, their distribution is more widespread, and the cost of sodium is much lower than that of lithium, and for these reasons, sodium batteries have the potential to replace lithium batteries as long as challenges such as low coulombic efficiency and poor rate capacity are overcome or reduced to a satisfactory equilibrium point.
[0004] Lithium and sodium batteries are typically composed of four main components: a cathode, an anode, a separator, and an electrolyte. The electrolyte serves as a conductive medium through which lithium ions can be transported to and from the electrodes. The electrolyte may be either solid-state or liquid. In the context of this invention, "lithium battery" or "sodium battery" includes both solid-state (with solid electrolyte) and liquid-state (with liquid electrolyte) batteries. In the context of this invention, the terms "lithium ion battery" and "sodium ion battery" are reserved for battery technologies with liquid electrolytes.
[0005] The cathode of a lithium battery generally comprises a lithium-metal-oxide (e.g., lithium cobalt oxide (LiCoO2)). The cathode of a lithium battery may also comprise sulfur or a sulfur composite. Lithium-sulfur (Li-S) batteries have the advantage of having high theoretical capacity and specific energy, and thus have attracted increasing interest in the art. However, sulfur has low electrical conductivity. In addition, Li-S batteries are known to degrade easily due to a process commonly known as the polysulfide "shuttle effect". The materials commonly used as active materials in the anode of a lithium battery are intercalation compounds, alloys, and conversion compounds (transition metal oxides). Of the intercalation compounds used in the anode of a lithium battery, the most common is graphite. Another common compound used in the anode of a lithium battery is silicon or a silicon-based compound. Generally, silicon materials have a high specific capacity compared to graphite. Overall, graphite has remained the predominant intercalation anode material in commercial lithium batteries because it is safe and offers a low working potential, low cost, and good cycle life with sufficient energy density for many portable power applications. However, batteries using graphite anodes typically suffer from the relatively slow diffusion rate of lithium ions into carbon materials (10 -12 cm2 / s to 10 -6 cm 2 / s), this characteristic, combined with the suboptimal electronic conductivity, makes the charge / discharge rates of graphite alone suboptimal, thus resulting in long charge and discharge times for the battery.
[0006] To improve the charge / discharge rate of the battery, conductive additives are traditionally added to graphite to improve the electronic conductivity of the anode (Roselin et al., "Recent Advances and Perspectives of Carbon-Based Nanostructures as Anode Materials for Li-ion Batteries", Materials 2019, 12, 1229). These additives build a conductive interpenetrating network to increase and maintain the electrical conductivity of the electrode, allowing for faster charging and discharging. In addition, the conductive additives absorb and hold the electrolyte, allowing for intimate contact between the lithium ions and the active material. Conductive additives for lithium batteries are generally carbon nanomaterials selected from carbon black, Super P, acetylene black, carbon nanofibers and carbon nanotubes, all of which exhibit low weight, high chemical inertia and high specific surface area (Zhang Q et al., "Carbon nanomaterials used as conductive additives in lithium ion batteries", Recent Pat Nanotechnol., 2010 Jun;4(2):100-10).
[0007] Carbon black is a frequently used conductive additive to either electrochemically active graphite in the anode or metal oxides in the cathode, added to improve electronic conductivity and thereby improve the charge and discharge rates of lithium batteries. In practice, lithium battery composite electrodes generally incorporate 1-10 wt% carbon black additive in the formulation. Nevertheless, thermal carbon black exhibits low crystallinity resulting in low electrical conductivity, high brittleness, and a wide particle size distribution of spherical particles resulting in non-uniform properties between batches. Moreover, carbon black can be highly reactive to organic electrolytes, especially at voltages higher than 4.2 V (US Pat. No. 9,368,798), inevitably posing a safety risk. In addition, Liu et al. (Liu Z et al., "Effects of conducting carbon on the electrochemical performance of LiCO2and LiMn2O4cathodes", J. Power Sources 2001;97-8:361-5) investigated the effect of carbon black on the electrochemical performance of LiCoO2 and LiMn2O4 cathodes and found that the poor performance of LiCoO2 or LiMn2O4 mainly resulted from incomplete charging caused by poor particle contact between the oxide and carbon black.
[0008] US Patent No. 7,550,232 discloses the use of carbon nanotubes (CNTs) and graphite in the anode of a lithium battery, however, US Patent No. 7,550,232 does not demonstrate any improvement in charge and discharge rate and does not provide a conductive additive for the cathode of a lithium battery.
[0009] Sodium batteries pose their own challenges. For example, sodium ions (1.02 Å) are 55% larger than lithium ions (0.69 Å), making it more difficult to reversibly accommodate sodium ions in the anode. In fact, graphite materials used commercially as anodes in lithium batteries have not been able to achieve acceptable performance in sodium batteries, as the graphite anodes used to date in sodium batteries absorb too little sodium, making the sodium battery less powerful. To overcome the limitations of graphite as an anode material, alternative anode materials, such as red phosphorus (P), have been used. However, (1) native red P has a very low electrical conductivity (approximately 10 -14 Scm -1 );(2) The large volume expansion during sodiation / desodiumation can result in significant capacity fade (Wang et al., "Influence of Conductive additives on the stability of red phosphorus-carbon anodes for sodium-ion batteries", Scientific Reports 2019.9:946). The introduction of conductive additives into the synthesis of these anode materials could effectively overcome these shortcomings.
[0010] For both sodium and lithium batteries, there remains a need in the art to find conductive additive materials with high electrical conductivity that can help improve the charge and discharge rates of lithium or sodium batteries, increase their life span, reduce the internal resistance of the battery cell, and retain electrolyte. More specifically, the properties of conductive additive materials in the anode and cathode need to be further developed to obtain lithium or sodium batteries with fast charge and discharge rates while having physical properties that allow for safe manufacture and use. Summary of the Invention
[0011] The inventors have discovered that carbon networks comprising carbon nanofibers can be beneficially used to replace existing conductive additives, such as carbon black currently used in lithium or sodium batteries, to the extent that they achieve all of the above goals in the art, particularly longevity (stability over extended cycling) and fast charge and discharge rates, while possessing physical properties that allow for safe manufacture and use.
[0012] Advantageously, the inventors have found that anodes and / or cathodes comprising carbon networks with carbon nanofibers as conductive additives according to the present invention can contribute to the life (stability over extended cycling) of lithium and sodium batteries by improving electronic conductivity; see Fig. 3, Fig. 5 and Table 4 herein. Because of the high electronic conductivity of carbon networks with carbon nanofibers according to the present invention, the reversibility of the charge / discharge process is also enhanced; see Fig. 3 and Table 4 herein. Importantly, the inventors have also found that the charge and discharge rates can be improved by adding carbon networks with carbon nanofibers according to the present invention as additives to the anodes and / or cathodes of lithium and sodium batteries; see Fig. 4 and Fig. 6 herein.
[0013] Without wishing to be bound by any theory, the inventors believe that these advantageous properties can be attributed to the inherent electronic conductivity and open pore structure of the network due to the crystallinity, accessible porosity, filament length to diameter ratio, and d-spacing, which may aid in the rate of lithium or sodium ion intercalation. In addition, the inventors have found that the use of carbon networks comprising carbon nanofibers according to the present invention as an additive to the anode and / or cathode of lithium or sodium batteries allows for high charge / discharge rates, thus providing the battery with reduced charging times. In particular, it allows for the production of batteries that charge in minutes instead of hours.
[0014] In a preferred embodiment, these porous carbon networks form intragranular porous networks, where the carbon nanofibers are interconnected by chemical bonds through connectors with other carbon nanofibers in the network, where the pores in the network have intragranular pore diameter sizes of 5-150 nm using mercury intrusion porosimetry according to ASTM D4404-10, and where the carbon nanofibers have an average aspect ratio of fiber length to thickness of at least 2. The porous networks are preferably characterized by d-spacings of 0.340-0.5 nm, more preferably 0.35-0.45 nm, and even more preferably 0.355-0.375 nm. The d-spacings are measured by XRD. Importantly, this d-spacing is larger than that of graphite (0.335 nm), facilitating the intercalation of lithium and sodium ions. This large d-spacing is particularly beneficial for the intercalation of sodium ions in sodium batteries due to the large volume of sodium ions.
[0015] The present invention therefore resides in the use of carbon networks comprising carbon nanofibers as an additive in the anodes and / or cathodes of lithium or sodium batteries, anodes and / or cathodes comprising carbon networks comprising these carbon nanofibers as additives, and lithium or sodium batteries comprising these anodes and / or cathodes. The present invention also relates in the broadest sense to solid-state lithium and sodium batteries, the present invention preferably relates to sodium-ion or lithium-ion batteries, more preferably to lithium-ion batteries.
[0016] Furthermore, the inventors have found that carbon networks comprising carbon nanofibers according to the invention can provide a conductive scaffold and act as a sulfur host material in the cathode of a lithium-sulfur (Li-S) battery. Advantageously, the networks of the invention can mitigate the "shuttle effect", which occurs when Li2S is charged in the cathode of a Li-S battery. xis formed, diffuses to the anode, where it is reduced to polysulfides, and diffuses back to the cathode. This continuous process results in the continuous leakage of active material from the cathode. The "shuttle effect" is the main reason for the cell degradation and large sulfur volume expansion during discharge of Li-S batteries. The porous and chemically interconnected carbon network comprising carbon nanofibers has a functionalized surface; see Table 2, where the pH of the network is shown to be slightly acidic to neutral (5.0-7.0). In other words, the surface comprises groups that change the hydrophobic nature of the surface (typical of carbon) to a more hydrophilic nature. The surface of the carbon network comprises carboxyl groups, hydroxyl groups, and phenolic substances. These groups add some polarity to the surface and may change the properties of the compound material in which the functionalized carbon network is embedded. Without wishing to be bound by theory, it is believed that the network of the present invention can mitigate the "shuttle effect" by functionalizing the surface groups. The hydrophilic functionalization results in the polysulfides being more strongly bound to the carbon and prevents them from migrating to the anode.Thus, in a further aspect, the present invention resides in the use of a carbon network comprising carbon nanofibers as an additive to the cathode of a Li-S battery. [Brief description of the drawings]
[0017] [Figure 1A] Schematic diagram of a continuous furnace carbon black production process according to the present invention, containing along the axis of a reactor 3 a combustion zone 3 a, a reaction zone 3 b and a termination zone 3 c, by burning a fuel a in an oxygen-containing gas b and generating a flow of hot waste gas a1 in the combustion zone by passing the waste gas a1 from the combustion zone 3 a to the reaction zone 3 b, spraying (atomizing) a single-phase emulsion c in the reaction zone 3 b containing the hot waste gas, carbonizing said emulsion at high temperature and quenching or stopping the reaction in the termination zone 3 c by spraying water d, in order to obtain a crystalline carbon network e according to the present invention. [Figure 1B]Schematic diagram of a semi-batch carbon black production process in which a single-phase emulsion c is sprayed through nozzle 4 at the top of reactor 3 into hot reaction zone 3b, the hot emulsion is carbonized in reaction zone 3b, and the crystalline carbon network e is collected at the bottom of the reactor. In addition, there are two gas inlets entering the reactor from the top for adding an inert gas f, preferably nitrogen, for oxygen level control and / or exhaustion, and for introducing a carbon-containing gas g, preferably acetylene or ethylene, into the reactor. [Diagram 2] Schematic side view of a lithium or sodium battery according to the invention, exemplified here as a lithium-ion or sodium-ion battery, including an anode 5 and / or cathode 6 comprising a carbon network comprising carbon nanofibers according to an embodiment of the invention. The lithium-ion or sodium-ion battery also includes a separator 7 between the anode and cathode, and an electrolyte 8. Release of electrons from the anode to the cathode (oxidation) and release of lithium or sodium ions occurs during a discharge cycle. [Diagram 3] 2 is a graph showing the specific capacity of a lithium ion battery anode comprising a carbon network comprising carbon nanofibers as a conductive additive in accordance with the present invention. [Figure 4] 1 is a graph showing the cycling capability at various C-rates of a lithium ion battery anode comprising a carbon network with carbon nanofibers as a conductive additive according to the present invention, capacity versus cycles, and a series of cycles at different C-rates. [Diagram 5] 2 is a graph showing the specific capacity of a lithium ion battery anode comprising a carbon network comprising carbon nanofibers as a conductive additive in accordance with the present invention. [Figure 6] 1 is a graph showing the cycling capability at various C-rates of a lithium ion battery anode comprising a carbon network with carbon nanofibers as a conductive additive according to the present invention, capacity versus cycles, and a series of cycles at different C-rates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] 1. Use of a porous, chemically interconnected carbon network comprising carbon nanofibers as a conductive additive material in the anode and / or cathode of a rechargeable lithium or sodium battery.
[0019] 2. Use according to embodiment 1, wherein the carbon network comprising carbon nanofibers represents from 0.1 to 20% by weight, preferably more than 0.1% by weight and less than 20% by weight, of the total mass of the cathode and / or the carbon network comprising carbon nanofibers represents from 0.1 to 10% by weight, preferably more than 0.1% by weight and less than 10% by weight, of the total mass of the anode.
[0020] 3. The use according to aspect 1 or 2, wherein the carbon network comprises crystalline carbon nanofibers.
[0021] 4. The use according to any one of the preceding aspects, wherein the carbon nanofibers have an average fiber length of 30 to 10,000 nm.
[0022] 5. The use of any one of the preceding embodiments, wherein the carbon network forms an intraparticle porous network, wherein the carbon nanofibers are interconnected by chemical bonds with other carbon nanofibers in the network via connectors, and wherein the pores in the network have an intraparticle pore diameter size of 5-150 nm using mercury intrusion porosimetry according to ASTM D4404-10, and wherein the carbon nanofibers have an average aspect ratio of fiber length to thickness of at least 2, and preferably have a d-spacing in the range of 0.340-0.5 nm.
[0023] 6. The use of any one of the preceding aspects, wherein the lithium or sodium battery is suitable for smart phones, laptops, digital cameras and camcorders, as uninterruptible power supplies (UPS), as energy storage in power generation equipment, in medical and communication systems, and in electric and / or hybrid vehicles.
[0024] 7. A lithium or sodium battery anode and / or cathode comprising a porous, chemically interconnected carbon network comprising carbon nanofibers as a conductive additive material, preferably a lithium-ion or sodium-ion battery anode and / or cathode.
[0025] 8. Anode and / or cathode of a lithium or sodium battery comprising a porous, chemically interconnected carbon network comprising carbon nanofibers, in which the carbon network comprising carbon nanofibers represents 0.1-20% by weight, preferably more than 0.1% by weight and less than 20% by weight, of the total mass of the cathode and / or the carbon network comprising carbon nanofibers represents 0.1-10% by weight, preferably more than 0.1% by weight and less than 10% by weight, of the total mass of the anode.
[0026] 9. The lithium or sodium battery anode and / or cathode of embodiment 7 or 8, wherein the carbon network forms an intraparticle porous network, wherein the carbon nanofibers are interconnected by chemical bonds with other carbon nanofibers in the network via connectors, and wherein the pores in the network have an intraparticle pore diameter size of 5 to 150 nm using mercury intrusion porosimetry according to ASTM D4404-10, and the carbon nanofibers have an average aspect ratio of fiber length to thickness of at least 2, and preferably have a d-spacing in the range of 0.340 to 0.5 nm.
[0027] 10. The anode and / or cathode of a lithium or sodium battery according to any of aspects 7 to 9, wherein the anode and / or cathode also comprises 0.1 to 10 wt. % of a binder.
[0028] 11. The anode and / or cathode of a lithium or sodium battery according to any of aspects 7 to 10, wherein the cathode and / or anode also comprises 0.1 to 10 wt. %, preferably 0.5 to 5 wt. %, and most preferably 1 to 3 wt. % of one or more further conductive additives selected from conductive carbon black, Super P, acetylene black, carbon nanofibers, and carbon nanotubes.
[0029] 12. A rechargeable lithium or sodium battery comprising an anode and / or a cathode according to any one of aspects 7 to 11, wherein the lithium or sodium battery is preferably a lithium-ion or sodium-ion battery.
[0030] 13. The lithium or sodium battery of embodiment 12, wherein the battery is suitable for inclusion in smartphones, laptops, digital cameras and camcorders, as uninterruptible power supplies (UPS), as energy storage in power generation equipment, in medical and communication systems, and in electric and / or hybrid vehicles.
[0031] 14. Use according to any one of aspects 1 to 6, a lithium or sodium battery anode and / or cathode according to any one of aspects 7 to 11, or a lithium or sodium battery according to aspect 12 or 13, wherein the carbon network is obtained by a process for producing a crystalline carbon network by injecting a water-in-oil or bicontinuous microemulsion c comprising metal catalyst nanoparticles into a reactor 3 containing a reaction zone 3b and a termination zone 3c at a temperature above 600° C., preferably above 700° C., more preferably above 900° C., even more preferably above 1000° C., more preferably above 1100° C., preferably at most 3000° C., more preferably at most 2500° C., most preferably at most 2000° C., to produce a crystalline carbon network e, transporting these networks e to a termination zone 3c, and quenching or stopping the formation of the crystalline carbon network in the termination zone by spraying into water d.
[0032] 15. A battery-powered device comprising an anode and / or cathode of a lithium or sodium battery according to any one of aspects 7 to 11, or a lithium or sodium battery according to aspect 12 or 13, wherein the lithium or sodium battery is preferably a lithium-ion or sodium-ion battery.
[0033] 16. The device of aspect 15, which is a smartphone, a laptop, a digital camera, a camcorder, a medical and communication system, an uninterruptible power supply (UPS), an energy storage device for a power generation unit, or an electric and / or hybrid vehicle.
[0034] 17. The use according to any one of aspects 1 to 6, wherein the lithium battery is a lithium-sulfur (Li-S) battery.
[0035] 18. The lithium battery cathode of any one of aspects 7-11, wherein the cathode comprises a sulfur composite comprising a porous, chemically interconnected carbon network comprising carbon nanofibers as a conductive additive material.
[0036] 19. The battery anode of any one of aspects 8-11, wherein the battery is a lithium battery, and wherein the anode comprises 90-99.9 wt. % of an additional active material, and wherein the additional active material is graphite, silicon, a silicon-based compound (SiO2), or a combination thereof.
[0037] 20. The battery anode of embodiment 19, wherein the additional active material is silicon, a silicon-based compound (SiO2), or a combination thereof, and wherein the silicon, a silicon-based compound (SiO2), or a combination thereof is mixed with a carbon network comprising carbon nanofibers in the anode, or the carbon network comprising carbon nanofibers is coated with the silicon, a silicon-based compound (SiO2), or a combination thereof.
[0038] The following is copied from Roselin (Roselin et al., "Recent Advances and Perspectives of Carbon-Based Nanostructures as Anode Materials for Li-ion Batteries", Materials 2019, 12, 1229), the contents of which are incorporated herein by reference, describing the operating principles of batteries as exemplified by lithium-ion (Li-ion) batteries.
[0039] A battery is a device that changes chemical energy into electrical energy through electrochemical oxidation-reduction reactions (redox reactions). The essential electrochemical unit that accomplishes such energy change is known as a "cell." A battery contains a group of interconnected cells. The number of cells utilized depends on the capacity and voltage desired for a particular application. A small number of electrochemical cells are linked in parallel in an array to obtain a lithium-ion battery of the indicated voltage and capacity. Each cell contains the following parts: a negative terminal (anode) where electrochemical oxidation occurs during discharge; a positive terminal (cathode) where electrochemical reduction occurs; an electrolyte that facilitates the transport of ions from one electrode to another; a separator that provides electronic isolation between the electrodes; and a casing that contains the other cell parts. Lithium-ion cells use a solid reductant as the anode and a solid oxidant as the cathode.
[0040] The cathode materials used in the majority of commercial Li-ion batteries are LiCoO2 or LiNiO2, and the anode materials are carbonaceous. During charging of the cell, the cathode material releases Li ions into the electrolyte, and electrons are extracted from the cathode by applying an external field and then transferred to the anode. Charge-compensating Li ions are attracted by the negative electrode and then inserted into the negative electrode. During discharging of the cell, the reverse reaction occurs: the anode provides the intercalated Li ions to the electrolyte and provides electrons to the external circuit. At the cathode, Li ions intercalate from the electrolyte and provide charge from the external circuit. Common carbon anode materials are graphite or coke types, or a combination of both, and common cathode materials include LiMn2O4, LiCoO2, and LiNiO2. The electrolyte can be either solid or liquid. Liquid electrolytes are usually non-aqueous solutions of Li salts and various solvents, including ethers, esters, and carbonates. The cell reactions occurring at the cathode and anode during charging and discharging of the cell are represented as follows (Equations (1)-(4)): Charging At the cathode: LiMO2 → Li 1-x MO2+xLi + +xe - (1) At the anode: xLi + +xe - +C→Li x C (2) Discharging At the cathode: Li 1-x MO2+xLi + +xe - →LiMO2(3) At the anode: Li x C → xLi + +xe - +C (4) When the electrodes are connected to an external load, electrons flow through the external circuit and ions move through the electrolyte. The flow of charge results from electrochemical (i.e. redox) reactions at the electrodes, involving chemical species and electrons, that occur at various voltages. The output voltage of the battery is given by the voltage difference between the two redox reactions. In primary batteries, the redox reactions cannot be reversed and the battery is meant to be discharged once, whereas in secondary (i.e. rechargeable) batteries, the redox reactions are reversible, resulting in multiple charge and discharge cycles. The above example of the electrochemical reactions of a lithium battery may be extended, mutatis mutandis, to a sodium battery.
[0041] The present invention relates to secondary or rechargeable batteries, and in particular to providing a conductive additive to the cathode and / or anode in the above redox reactions (1) and / or (2). In the context of the present invention, "lithium battery" or "sodium battery" includes both solid-state (with solid electrolyte) and liquid-state (with liquid electrolyte) batteries. In the context of the present invention, the terms "lithium ion battery" and "sodium ion battery" are reserved for battery technologies with liquid electrolytes.
[0042] In a first aspect, the present invention can be described as the use of a porous, chemically interconnected carbon network comprising carbon nanofibers (i.e. a porous carbon network comprising chemically interconnected carbon nanofibers) as a conductive additive in an electrode of a lithium or sodium battery. The conductive additive can be applied to the cathode and / or anode, preferably to both the cathode and the anode. In this context, a "conductive additive" should be understood as a material that is added to the main active material (the material that spontaneously participates in the electrochemical charge and / or discharge reaction) in the cathode and / or anode in order to enhance the intrinsic properties of the active material, e.g. electronic conductivity.
[0043] In this regard, the present invention pertains to a cathode and / or anode for a lithium or sodium battery comprising a porous, chemically interconnected carbon network comprising carbon nanofibers (i.e., a porous carbon network comprising chemically interconnected carbon nanofibers) as a conductive additive to enhance the intrinsic properties of the active material. In particular, the present invention pertains to a cathode and / or anode for a lithium or sodium battery comprising a porous, chemically interconnected carbon network comprising carbon nanofibers.
[0044] In a preferred embodiment, the cathode for a lithium or sodium battery comprises a porous, chemically interconnected carbon network comprising carbon nanofibers in an amount of 0.1-20% by weight of the cathode, preferably greater than 0.1% by weight and less than 20% by weight, more preferably 0.5-15% by weight, even more preferably 1-10% by weight, and most preferably 1.5-5% by weight, the remainder being preferably an active cathode material capable of intercalating and releasing lithium or sodium ions. Preferably, the active material, relative to the amount of carbon network in the preceding sentence, is present in an amount of 80-99.9% by weight of the cathode, more preferably 85-99.5% by weight, even more preferably 90-99% by weight, and most preferably 95.0-98.5% by weight, respectively. It is preferred that the above numbers relating to the amount of carbon network and active material together account for 100% of the cathode.
[0045] In a preferred embodiment, the anode for a lithium or sodium battery comprises a porous, chemically interconnected carbon network comprising carbon nanofibers in an amount of 0.1-10% by weight of the anode, preferably greater than 0.1% by weight and less than 10% by weight, more preferably 0.5-8% by weight, even more preferably 1-6% by weight, and most preferably 1.5-5% by weight, with the remainder being preferably an active anode material capable of intercalating and releasing lithium or sodium ions. Preferably, the active material, relative to the amount of carbon network in the preceding sentence, is present in an amount of 90-99.9% by weight of the anode, more preferably 92-99.5% by weight, even more preferably 94-99% by weight, and most preferably 95.0-98.5% by weight, respectively. It is preferred that the above numbers relating to the amount of carbon network and active material together account for 100% of the anode.
[0046] In the case of a lithium battery, preferably, the active material in the anode is an intercalation compound, such as graphite, an alloy, such as tin, a silicon-based alloy, and / or a conversion compound, such as a transition metal oxide (MO, where M is Sn, Mo, Ga, Zn, Si, Ge, Co, Ni, Cu, or Fe). In a preferred embodiment, the active material in the anode is graphite. In the case of a lithium battery, preferably, the additional active material in the anode is an intercalation compound, such as graphite, an alloy, such as tin, a silicon-based alloy, a silicon or silicon-based compound, such as SiO2, and / or a conversion compound, such as a transition metal oxide (MO, where M is Sn, Mo, Ga, Zn, Si, Ge, Co, Ni, Cu, or Fe). In a preferred embodiment, the additional active material in the anode of a lithium battery is graphite, silicon, a silicon-based compound (SiO2), or a combination thereof. In another preferred embodiment, the additional active material in the anode of the lithium battery is silicon, a silicon-based compound (SiO2), or a combination thereof. Most preferably, the additional active material is silicon or graphite. When the additional active material in the anode is silicon, a silicon-based compound (SiO2), or a combination thereof, the silicon, the silicon-based compound (SiO2), or a combination thereof is mixed with the carbon network comprising the carbon nanofibers of the present invention in the anode, or the carbon network comprising the carbon nanofibers of the present invention is coated with the silicon, the silicon-based compound (SiO2), or a combination thereof. In the case of a lithium battery, preferably, the active material in the cathode is lithium or sodium metal, an alkali metal, and / or a lithium or sodium metal oxide. In a preferred embodiment, the active material in the cathode is LiCoO2 or LiMn2O4 in the case of a lithium cathode. In another preferred embodiment, the active material in the cathode is lithium iron phosphate (LiFePO4). In a further preferred embodiment, the active material in the cathode is sulfur, a sulfur compound, or a sulfur complex.
[0047] For sodium batteries, the active material in the anode is preferably an oxide such as TiO2 for an intercalation type anode, an oxide such as Fe2O3 for a conversion type anode, or an oxide such as Sn x O2 and Sb2O3, or "hard carbon", a disordered carbon material consisting of a non-graphitizable, non-crystalline and amorphous carbon structure. For sodium batteries, preferably the active material in the cathode is an O3 type layered metal oxide, such as NaFeO2, a P2 type layered metal oxide, such as Na 0.6 MnO2, biphasic layered metal oxides, e.g. Na 0.78 Ni 0.2 Fe 0.38 Mn 0.42 O2, or an oxide with anionic redox capability. Preferably, the active material in the cathode of a sodium battery is sodium oxide (NaMO2, M=V, Fe, Mn, Cu, Co, and Ni), sodium phosphate (Na7V3(P2O7)4, NaFePO4, transition metal oxides (VO5), or Prussian Blue (PB, Na2M[Fe(CN)6]).
[0048] The anode and / or cathode of both lithium and sodium batteries may also comprise 0.1-10% by weight, preferably 2-8% by weight, most preferably 4-6% by weight of a binder. Preferably, the binder is selected from styrene-butadiene rubber (SBR) based and polyvinylidene fluoride (PVDF) based binders. Preferably, the binder is PVDF (polyvinylidene difluoride).
[0049] The advantageous effect of the use of the carbon network according to the invention as a conductive additive in the electrodes of lithium or sodium batteries is a higher electrical conductivity. In addition, the carbon network passes high levels of Fe and / or other metals without problems, which increases the industrial application and safety of the electrode. The carbon network according to the invention has a greater distance between the interlayers compared to carbon black; this allows the viscosity to remain reduced when compared to carbon black, even when adding a higher amount of additive material. While the use of conventional conductive additives is associated with an increase in viscosity, which hinders both processing and maximum loading, the carbon network according to the invention can be added in increased numbers without adversely affecting the viscosity.
[0050] The present invention also relates to a secondary or rechargeable lithium or sodium battery comprising the above-mentioned cathode and / or anode. Preferably, the secondary or rechargeable battery is a secondary or rechargeable lithium-ion or sodium-ion battery, most preferably a lithium-ion battery. In a further preferred embodiment, the secondary or rechargeable battery is a Li-S battery.
[0051] In addition to the aforementioned anode and cathode, secondary or rechargeable lithium or sodium batteries also comprise an electrolyte, which may be in liquid or solid state. The liquid electrolyte may comprise an organic solvent and a salt of an alkali metal, preferably a lithium or sodium salt in the case of lithium-ion and sodium-ion batteries, respectively. The electrolyte of a lithium or sodium battery may also be in solid state and may comprise an inorganic ceramic / glass ceramic, an organic polymer and / or a ceramic-polymer composite electrolyte. Secondary or rechargeable lithium or sodium batteries may also comprise a separator between the anode and the cathode. The separator may comprise a polymer, such as polypropylene.
[0052] The cathode and / or anode for lithium or sodium batteries or lithium or sodium batteries of the present invention are particularly suitable for use in the manufacture of battery-powered electric devices. Thus, the present invention extends to a battery-powered electric device comprising at least one cathode and / or anode for lithium or sodium batteries or at least one lithium or sodium battery comprising a porous and chemically interconnected carbon network comprising carbon nanofibers according to the present invention. Here, the battery-powered electric device may be a smartphone, a laptop, a digital camera and a camcorder, as an uninterrupted power supply (UPS), as an energy storage for power generation equipment (i.e. from surplus wind and solar renewable energy), medical and communication systems, and electric and / or hybrid vehicles. Preferably, the anode for lithium or sodium batteries or lithium or sodium batteries according to the present invention are used in uninterrupted power supply (UPS) systems, portable consumer electronics, and electric and / or hybrid vehicles.
[0053] Although it is particularly advantageous to use the network according to the invention as the sole conductive additive, the cathode and / or anode for lithium or sodium battery according to the invention may further comprise conventional additives (non-active materials) together with the additive comprising the porous, chemically interconnected carbon network comprising carbon nanofibers in order to further improve the electrochemical performance of the lithium or sodium battery according to the invention. It is considered to be within the competence of the person skilled in the art to select suitable conductive additives available in the art. In a preferred embodiment, the cathode and / or anode for lithium or sodium battery according to the invention or the lithium or sodium battery may contain 0.1-10% by weight, preferably 0.5-5% by weight, most preferably 1-3% by weight of one or more further conductive additives selected from conductive carbon black, Super P, acetylene black, carbon nanofibers and carbon nanotubes. In a preferred embodiment, the further conductive additive is carbon black. [Carbon network with carbon nanofibers] The porous chemically interconnected carbon network comprising carbon nanofibers or the porous carbon network comprising chemically interconnected carbon nanofibers is preferably characterized as follows.
[0054] Those skilled in the art will understand that a porous network refers to a three-dimensional structure that allows fluids or gases to pass through. A porous network can also be described as a porous medium or a porous material. The porous crystalline carbon network according to the present invention (or the porous carbon network particles according to the present invention) can also be viewed as a large molecule in which carbon atoms are originally interconnected by covalent bonds. Here, referring to a porous network made by a plurality of molecules or particles, it is understood that the porous carbon network particles are particles with chemically interconnected (i.e., covalently bonded) fibers with intraparticle porosity, as opposed to interparticle porosity, in which the pores are formed by the spaces between physically aggregated particles or molecules. In the context of the present invention, the carbon network particles according to the present invention can also be viewed as large molecules in which the pores are embedded, and therefore the intraparticle porosity can also be described as intramolecular porosity. Thus, intraparticle porosity and intramolecular porosity have the same meaning in the present document and can be used interchangeably.
[0055] The network of the present invention can be seen as one large molecule, so there is no need to fuse the particles or parts of the network together. Therefore, the carbon network with porous, chemically interconnected carbon nanofibers is preferred to be a carbon network with non-fused, intraparticle-porous, chemically interconnected, crystalline carbon nanofibers with intraparticle porosity. Without being bound by theory, it is believed that the advantage of having a crystalline network with intraparticle porosity over an (amorphous) network with interparticle porosity is that it is firstly more robust and more resilient to crushing or breaking when a force is applied. For comparison purposes, carbon black consists of aggregates or agglomerates of spherical particles that can form a three-dimensional structure, with the spheres fused together with amorphous connections that have weaker porosity. The pores between the particles are weaker and more prone to collapse due to particle-particle interfaces. The pores within the particles are stronger due to the covalently bonded structure with crystalline arrangements that surround them, and can withstand large forces and pressures without collapsing. This is in sharp contrast to conventional carbon black, which consists of aggregates or agglomerates of spherical particles that may form a three-dimensional structure, where the spheres are fused together (not chemically "interconnected") with amorphous connections between the individual particles. In summary, intraparticle porosity (the trademark for the network of the present invention) refers to the situation where the carbon atoms surrounding the pores are covalently connected in crystalline form, whereas interparticle porosity refers to the pores being between particles that are physically aggregated or agglomerated, or between particles that have amorphous connections. The intraparticle pore volume can be characterized in terms of mercury intrusion porosimetry (ASTM D4404-10) or nitrogen absorption method (ISO 9277:10). The pore volume of the porous carbon network of the present invention is measured using mercury intrusion porosimetry (ASTM D4404-10) and is in the range of 0.05 to 5 cm. 3 / g, preferably 0.1 to 4 cm 3 / g, more preferably 0.3 to 3.5 cm 3 / g, most preferably 0.5 to 3 cm 3 / g. Additionally, or alternatively, the carbon network comprising carbon nanofibers may be characterized as having an intraparticle pore diameter size of 5-200 nm, preferably 10-150 nm, and most preferably 20-130 nm, as measured using mercury intrusion porosimetry (ASTM D4404-10). Following the same ASTM test method, the network may have an interparticle pore diameter of 10-500 μm, more preferably 80-400 μm.
[0056] The porous network is preferably characterized by a d-spacing in the range of 0.340 to 0.50 nm, more preferably in the range of 0.35 to 0.45 nm, and even more preferably in the range of 0.355 to 0.375 nm. The d-spacing is measured by XRD.
[0057] Those skilled in the art will readily understand that the term chemically interconnected in the context of a carbon network comprising porous, chemically interconnected carbon nanofibers implies that the carbon nanofibers are interconnected to other carbon nanofibers by chemical bonds. It is also understood that chemical bonds are synonymous with molecular or covalent bonds. Typically, the locations where carbon nanofibers are connected are referred to as connections or fiber connections and may therefore be conveniently designated as "covalent connections". These terms are used interchangeably in this document. In the carbon network according to the invention, the connections are formed by carbon atoms that are covalently connected. It further follows that the length of the fiber is defined as the distance between connections connected by the fibrous carbon material.
[0058] In a preferred embodiment, at least a portion of the fibers in the carbon network comprising the carbon nanofibers of the present invention are crystalline carbon nanofibers. Preferably, at least 20% by weight of the carbon in the carbon network of the present invention is crystalline, more preferably at least 40% by weight, even more preferably at least 60% by weight, even more preferably at least 80% by weight, and most preferably at least 90% by weight. Alternatively, the amount of crystalline carbon is 20-90% by weight, more preferably 30-70% by weight, more preferably 40-50% by weight, compared to the total carbon in the carbon network of the present invention. Here, "crystallinity" has its usual meaning and refers to the degree of structural order in a material. In other words, the carbon atoms in the nanofibers are arranged in a more or less regular and periodic manner. The area or volume that is crystalline can be expressed as crystallites. Carbon crystallites are therefore individual carbon crystals.
[0059] A measure of the size of the carbon crystallites is the stacking height of the graphitic layers. Standard ASTM grade carbon black has stacking heights of graphitic layers in the range of 11-13 Å (angstroms) within these crystallites. In a preferred embodiment, the carbon network comprising the carbon nanofibers of the invention preferably has a stacking height of at least 15 Å (angstroms), preferably at least 16 Å, more preferably at least 17 Å, even more preferably at least 18 Å, even more preferably at least 19 Å, and even more preferably at least 20 Å. If necessary, carbon networks containing crystallites as large as 100 Å (angstroms) can be produced. Thus, the carbon networks of the invention have stacking heights of 15-100 Å (angstroms), more preferably up to 80 Å, even more preferably up to 60 Å, even more preferably up to 40 Å, and even more preferably up to 30 Å. It is therefore understood that the stacking height of the graphitic layers within the crystallites in the carbon network of the present invention is 15 to 90 Å (angstroms), more preferably 16 to 70 Å, even more preferably 17 to 50 Å, still more preferably 18 to 30 Å, and most preferably up to 25 Å.
[0060] A carbon network comprising porous, chemically interconnected carbon nanofibers may be defined as having chemically interconnected carbon nanofibers, where the carbon nanofibers are interconnected through parts of the connections, and where a plurality (typically 3 or more, preferably at least 10 or more) of nanofibers are covalently bonded. The carbon nanofibers are part between the connections of the network. The fibers are typically solid (i.e., non-hollow) and elongated, preferably having an average diameter or thickness of 1-500 nm, preferably 5-350 nm, more preferably up to 100 nm, in one embodiment 10-100 nm, compared to an average particle size of 10-400 nm for carbon black particles. In one embodiment, the average fiber length (i.e., the average distance between two connections) is preferably in the range of 30-10,000 nm, more preferably 50-5,000 nm, more preferably 100-5,000 nm, more preferably at least 200-5,000 nm, and may be determined, for example, using SEM.
[0061] The nanofibers or structures may be described in terms of an average aspect ratio of fiber length to thickness of at least 2, preferably at least 3, more preferably at least 4, most preferably at least 5, and preferably at most less than 50; in sharp contrast to the amorphous (physically associated) aggregates formed from spherical particles obtained through conventional carbon black manufacturing. The average aspect ratio of fiber length to thickness may be determined, for example, using SEM.
[0062] A carbon nanofiber structure can be defined as a carbon network formed by chemically interconnected (covalently bonded) carbon nanofibers. The carbon network has a three-dimensional organization with gaps between the carbon nanofibers (intracene porosity, see above) accessible to a continuous phase, which may be a liquid (e.g., a solvent or aqueous phase), a gas, or any other phase. The carbon network is at least 0.5 μm in diameter, preferably at least 1 μm in diameter, preferably at least 5 μm in diameter, more preferably at least 10 μm in diameter, even more preferably at least 20 μm in diameter, and most preferably at least 25 μm in diameter in all dimensions. Alternatively, the carbon network is at least 1 μm in diameter in two dimensions and at least 5 μm in diameter, preferably at least 10 μm in diameter, more preferably at least 20 μm in diameter, and most preferably at least 25 μm in diameter in the other dimensions. Here, and also throughout this document, the term dimension is used in the usual way to refer to a spatial dimension. There are three spatial dimensions that are mutually orthogonal and define a space in the usual physical sense. Further, the carbon network may be at least 10 μm in diameter in two dimensions and at least 15 μm in diameter in the other dimension, preferably at least 20 μm in diameter, more preferably at least 25 μm in diameter, more preferably at least 30 μm in diameter, and most preferably at least 50 μm in diameter. These measurements are based on laser diffraction.
[0063] The carbon network comprising carbon nanofibers may have a volume-based aggregate size of 0.1 to 100 μm, preferably 1 to 50 μm, more preferably 1 to 40 μm, more preferably 5 to 35 μm, more preferably 5 to 25 μm, and most preferably 5 to 20 μm, as measured using laser diffraction (ISO 13320-1) or dynamic light scattering analysis. In a most preferred embodiment, the network has a volume-based aggregate size of 5 to 10 μm, as measured using laser diffraction (ISO 13320-1) or dynamic light scattering analysis. The network preferably has an advantageously narrow particle size distribution, especially compared to traditional carbon black. The particle size distribution may be characterized as between 10 nm and 200 nm, preferably 10 to 100 nm, as determined using transmission electron microscopy and measuring the diameter of the fibers. The network may be characterized by a set strength between 0.5 and 1, more preferably between 0.6 and 1, as determined by the c-OAN / OAN ratio measured according to ASTM D3493-16 / ASTM D2414-16, respectively. The c-OAN is preferably 20-200 cc / 100 g. This is a high strength that advantageously prevents the collapse of the internal porosity even in high pressure applications.
[0064] The porous, chemically interconnected carbon network comprising carbon nanofibers may also comprise carbon black particles incorporated as part of the network. These particles are found deep in the connections between the carbon nanofibers, but there may also be carbon black particles present in other parts of the network. The carbon black particles preferably have a diameter at least 0.5 times that of the carbon nanofibers, more preferably at least the same diameter as the carbon nanofibers, even more preferably at least twice the diameter of the carbon nanofibers, even more preferably at least three times the diameter of the carbon nanofibers, even more preferably at least four times the diameter of the carbon nanofibers, and most preferably at least five times the diameter of the carbon nanofibers. It is preferred that the diameter of the carbon black particles is no more than 10 times the diameter of the carbon nanofibers. Such a mixed network is designated a hybrid network.
[0065] The porous and chemically interconnected carbon network with carbon nanofibers has a functionalized surface. In other words, the surface is provided with groups that change the hydrophobic nature of the surface (typical of carbon) to a more hydrophilic nature. The surface of the carbon network is provided with carboxyl, hydroxyl and phenolic groups. These groups add some polarity to the surface and may change the properties of the compound material in which the functionalized carbon network is embedded. The surface area of the carbon network with carbon nanofibers, measured according to the Brunauer-Emmett-Teller (BET) method (ISO 9277:10), is preferably between 15 and 300 m. 2 / g, more preferably 20 to 270m 2 / g, and more preferably 30 to 250 m 2 / g, most preferably 30 to 210 m 2 / g.
[0066] The porous and chemically interconnected carbon network with carbon nanofibers contains only a small amount of metal catalyst nanoparticles, typically at least 10 ppm based on the weight of the carbon network with carbon nanofibers. These are the fingerprints of the preparation method. There is a preferred amount of metal nanoparticles of 5000 ppm or less, more preferably 3000 ppm or less, especially 2000 ppm or less, based on the weight of the network measured by ICP-OES (Inductively Coupled Plasma Optical Emission Spectroscopy). These metal particles are also embedded in the network. These particles can have an average particle size between 1 nm and 100 nm. Preferably, the particles are monodisperse particles with a deviation from the average particle size within 10%, more preferably within 5%. Non-limiting examples of nanoparticles contained in the carbon network with carbon nanofibers are noble metals (Pt, Pd, Au, Ag), iron group elements (Fe, Co and Ni), Ru and Cu. Suitable metal complexes include (i) platinum precursors, such as HPtCl; HPtCl·xH0; KPtCl; KPtCl·xH0; Pt(NH)(NO); Pt(CHO), (ii) ruthenium precursors, such as Ru(NO)(NO); Ru(dip)Cl [dip=4,7-diphenyl-1,10-phenanthroline]; RuCl, or (iii) palladium precursors, such as Pd(NO). or (iv) a nickel precursor, for example NiCl2 or NiCl2·xH2O; Ni(NO3)2; Ni(NO3)2·xH2O; Ni(CH3COO)2; Ni(CH3COO)2·xH2O; Ni(AOT)2 [AOT = bis(2-ethylhexyl)sulfosuccinate], where x may be any integer selected from 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10, typically 6, 7 or 8.
[0067] Porous, chemically interconnected carbon networks comprising carbon nanofibers are preferably obtained by a process for the production of crystalline carbon networks in a reactor 3 containing a reaction zone 3b and a termination zone 3c, by injecting a thermodynamically stable water-in-oil, oil-in-water or bicontinuous microemulsion c, preferably a water-in-oil or bicontinuous microemulsion c, bicontinuous microemulsion c, comprising metal catalyst nanoparticles, into the reaction zone 3b at a temperature above 600° C., preferably above 700° C., more preferably above 900° C., even more preferably above 1000° C., more preferably above 1100° C., preferably at most 3000° C., more preferably at most 2500° C., most preferably at most 2000° C., in order to produce crystalline carbon networks e, transporting these networks e to the termination zone 3c, and quenching or stopping the formation of the crystalline carbon networks in the termination zone by spraying into water d.
[0068] In a more preferred embodiment, the network is a furnace-type carbon black reactor 3, which contains, along the axis of the reactor 3, a combustion zone 3a, a reaction zone 3b and a termination zone 3c, and which comprises burning a fuel a in an oxygen-containing gas b and passing waste gas a1 from the combustion zone 3a to the reaction zone 3b to generate a flow of hot waste gas a1 in the combustion zone, and in the reaction zone 3b containing the hot waste gas, a water-in-oil, oil-in-water or bicontinuous microemulsion c, preferably a water-in-oil or bicontinuous microemulsion b, to obtain a crystalline carbon network e. and carbonizing the emulsion at a temperature above 600° C., preferably above 700° C., more preferably above 900° C., even more preferably above 1000° C., more preferably above 1100° C., preferably at most 3000° C., more preferably at most 2500° C., most preferably at most 2000° C., and quenching or stopping the reaction in a termination zone 3 c by spraying into water d.
[0069] In the above, "chemically interconnected" is understood to mean that the nanofibers are covalently bonded to one another and are distinct from physical aggregates.
[0070] The network is preferably obtained by the above process, where further processing details are provided in the section headed "Process for obtaining a carbon network comprising carbon nanofibers" herein below, and in FIG. 1A. [Process for obtaining a carbon network with carbon nanofibers] The process for obtaining the porous, chemically interconnected carbon network comprising carbon nanofibers can best be described as a modified carbon black production process, where "modified" is understood to mean that a suitable oil, preferably an oil comprising at least 14C atoms (greater than C14), such as a carbon black feedstock oil (CBFS), is provided to the reaction zone of a carbon black reactor as part of a single-phase emulsion, which is a thermodynamically stable water-in-oil, oil-in-water or bicontinuous microemulsion, preferably a water-in-oil or bicontinuous microemulsion, most preferably a bicontinuous microemulsion, comprising metal catalyst nanoparticles. The emulsion is preferably provided to the reaction zone by spraying, thus atomizing, the emulsion into droplets. The process can be carried out in batch or semi-batch mode, but the modified carbon black production process is advantageously carried out as a continuous process. The single-phase emulsion is a microemulsion comprising metal catalyst nanoparticles. The preferred single-phase emulsion comprises CBFS oil, which may also be referred to in the context of the present invention as an "emulsified CBFS".
[0071] The process for the production of carbon networks can be carried out in a reactor 3 containing a reaction zone 3b and a termination zone 3c by injecting a single-phase emulsion c, which is a water-in-oil, oil-in-water or bicontinuous microemulsion c, preferably a water-in-oil or bicontinuous microemulsion c, most preferably a bicontinuous microemulsion c, into the reaction zone 3b at a temperature above 600° C., preferably above 700° C., more preferably above 900° C., even more preferably above 1000° C., more preferably above 1100° C., preferably up to 3000° C., more preferably up to 2500° C., most preferably up to 2000° C., in order to produce a carbon network with porous and chemically interconnected carbon nanofibers, in which the single-phase emulsion e is sprayed into the reaction zone 3b, and quenching or stopping the formation of the carbon network with porous and chemically interconnected carbon nanofibers by spraying into water d. The single-phase emulsion is preferably sprayed into the reaction zone. Please refer to Figure 1A.
[0072] Alternatively, a process for the production of a porous, chemically interconnected carbon network comprising carbon nanofibers comprises burning a fuel a in an oxygen-containing gas b in a furnace-type carbon black reactor 3, which contains a combustion zone 3a, a reaction zone 3b and a termination zone 3c along the axis of the reactor 3, and generating a flow of hot waste gas a1 in the combustion zone by passing the waste gas a1 from the combustion zone 3a to the reaction zone 3b, and producing a single-phase emulsion c according to the invention, preferably water-in-oil, oil-in-water or bicontinuous microemulsion c, preferably water-in-oil or This is carried out by spraying (atomizing) a bicontinuous microemulsion c, most preferably a bicontinuous microemulsion c, carbonizing the emulsion at high temperatures (temperatures above 600°C, preferably above 700°C, more preferably above 900°C, even more preferably above 1000°C, more preferably above 1100°C, preferably up to 3000°C, more preferably up to 2500°C, most preferably up to 2000°C), and quenching or stopping the reaction in a termination zone 3c (i.e. the formation of a porous, chemically interconnected carbon network with carbon nanofibers) by spraying into water d. The reaction zone 3b is equipped with at least one inlet (preferably a nozzle) for introducing the emulsion, preferably by atomization. Reference is made to FIG. 1A.
[0073] The residence time for the emulsion in the reaction zone of the furnace carbon black reactor may be relatively short, preferably in the range of 1-1000 ms, more preferably 10-100 ms. Longer residence times may have an effect on the properties of the carbon network. An example may be the size of the crystallites, which are larger when longer residence times are used.
[0074] In accordance with conventional carbon black manufacturing processes, the oil phase may be aromatic and / or aliphatic, preferably comprising at least 50% by weight C14 or higher, more preferably at least 70% by weight C14 or higher (based on the total weight of oil). A list of typical oils that may be used, but is not limited to obtaining a stable emulsion, is carbon black feedstock oil (CBFS), phenolic oil, anthracene oil, (short-medium-long chain) fatty acids, fatty acid esters and paraffins. The oil is preferably C14 or higher. In one aspect, the oil preferably has high aromaticity. Within this field, aromaticity is preferably characterized in terms of the Bureau of Mines Correlation Index (BMCI). The oil preferably has a BMCI greater than 50. In one aspect, the oil has low aromaticity, preferably a BMCI less than 15.
[0075] CBFS is an economically attractive oil source in the context of the present invention, preferably a heavy hydrocarbon mix comprising mainly C14-C50, the sum of C14-C50 preferably amounting to at least 50% by weight of the feedstock, more preferably at least 70% by weight. Some of the most important feedstocks used to produce carbon black include clarified slurry oil (CSO) obtained from fluid catalytic cracking of light oils, ethylene cracker residue from naphtha steam cracking, and coal tar oil. The presence of paraffins (smaller than C15) substantially reduces compatibility, and higher aromaticity is preferred. The concentration of aromatics determines the rate at which carbon nuclei are formed. Carbon black feedstocks preferably have a high BMCI and can provide high yields with minimal heat input, thus reducing the cost of production. In a preferred embodiment, and based on current CBFS specifications, the oil, including the mixture of oils, has a BMCI value of greater than 120. It is not difficult for a person skilled in the art to understand which are suitable CBFS, but it is noted, merely as a guideline, that the BMCI value for the CBFS (from the point of view of yield) is preferably greater than 120, even more preferably greater than 132. The amount of asphaltenes in the oil is preferably less than 10% by weight, preferably less than 5.0% by weight of the CBFS. The CBFS preferably has a low sulfur content, since sulfur adversely affects the quality of the product, leading to lower yields and corroding equipment.
[0076] It is preferred that the sulfur content of the oil according to ASTM D1619 be less than 8.0 wt.%, preferably less than 4.0 wt.%, more preferably less than 2.0 wt.%.
[0077] The emulsion, preferably the emulsion with CBFS, is a "single-phase emulsion", which is understood to mean that the oil and water phases appear optically as one miscible mixture, showing no physical separation of oil, water or surfactant to the naked eye. The single-phase emulsion is a water-in-oil, oil-in-water or bicontinuous microemulsion, preferably a water-in-oil or bicontinuous microemulsion, most preferably a bicontinuous microemulsion. The process of complete emulsion breakage (coalescence), i.e., the system separates into bulk oil and water phases, is generally believed to be controlled by four different droplet disappearance mechanisms: Brownian flocculation, creaming, sedimentation flocculation, and disproportionation.
[0078] The amount of water and oil is not considered critical, provided that the above microemulsion is obtained, but it is noted that a reduced amount of water (and an increased amount of oil) improves the yield. The water content is typically between 5% and 50% by weight of the emulsion, preferably 10-40% by weight, even more preferably up to 30% by weight, more preferably 10-20% by weight of the emulsion. Higher amounts of water may be considered, but at the expense of yield. Without wishing to be bound by any theory, the inventors believe that the shape and morphology of the network thus obtained is attributable to the aqueous phase.
[0079] The choice of surfactant is not considered to be a limiting factor, as long as the combination of oil, water and surfactant results in a stable microemulsion as defined herein above. As a further guide to the skilled artisan, it is noted that surfactants can be selected based on the hydrophobicity or hydrophilicity of the system, i.e., hydrophilic-lipophilic balance (HLB). The HLB of a surfactant is a measure of the degree to which the surfactant is hydrophilic or lipophilic, and is determined by calculating values for different regions of the molecule by the Griffin or Davies method. The appropriate HLB value depends on the type of oil and the amount of oil and water in the emulsion, and can be easily determined by the skilled artisan based on the requirement of maintaining a thermodynamically stable single-phase emulsion as defined herein above. It has been found that emulsions with more than 50% by weight of oil and preferably less than 30% by weight of water phase are best stabilized by surfactants with HLB values of more than 7, preferably more than 8, more preferably more than 9, and most preferably more than 10. On the other hand, emulsions with 50% or less by weight of oil are best stabilized by surfactants with HLB values less than 12, preferably less than 11, more preferably less than 10, most preferably less than 9, especially less than 8. The surfactant is preferably selected to be compatible with the oil phase. When the oil is an emulsion with a CBFS, surfactants with high aromaticity are preferred by the CBFS, and oils with low BMCI, such as those characterized by a BMCI less than 15, are best stabilized using aliphatic surfactants. The surfactant can be cationic, anionic or nonionic, or a mixture thereof. To increase the yield, one or more nonionic surfactants are preferred, since no residual ions are left in the final product. To obtain a clean tail gas stream, the surfactant structure is preferably low in sulfur and nitrogen, preferably sulfur and nitrogen-free. Non-limiting examples of typical non-ionic surfactants that can be used to obtain a stable emulsion are the commercially available series Tween, Span, Hypermer, Pluronic, Emulan, Neodol, Triton X and Tergitol.
[0080] In the context of the present invention, a microemulsion is a dispersion made of water, oil (preferably CBFS) and surfactant, which is an optically homogeneous and thermodynamically stable liquid, with the diameter of the dispersed domains varying from approximately 1 to 500 nm, preferably 1 to 100 nm, usually 10 to 50 nm. In a microemulsion, the domains of the dispersed phase are either particulate (i.e. droplets) or interconnected (giving a bicontinuous microemulsion). In a preferred embodiment, the surfactant tail forms a continuous network in the oil phase of the water-in-oil, oil-in-water or bicontinuous microemulsion, preferably the water-in-oil or bicontinuous microemulsion, most preferably the bicontinuous microemulsion. The water domains should contain a metal catalyst, preferably with an average particle size between 1 nm and 100 nm.
[0081] The single-phase emulsion, i.e. water-in-oil, oil-in-water or bicontinuous microemulsion, preferably water-in-oil or bicontinuous microemulsion, most preferably bicontinuous microemulsion, further comprises metal catalyst nanoparticles, preferably having an average particle size between 1 nm and 100 nm. Those skilled in the art find ample guidance in the field of carbon nanotubes (CNTs) to produce and use these types of nanoparticles. These metal nanoparticles have been found to improve network formation, both in terms of speed and yield, and reproducibility. Methods for producing suitable metal nanoparticles can be found in Vinciguerra et al., "Growth mechanisms in chemical vapour deposited carbon nanotubes," Nanotechnology (2003) 14, 655; Perez-Cabero et al., "Growing mechanism of CNTs: a kinetic approach," J. Catal. (2004) 224, 197-205; Gavillet et al., "Microscopic mechanisms for the catalyst assisted growth of single-wall carbon nanotubes," Carbon. (2002) 40, 1649-1663, and Amelinckx et al., "A formation mechanism for catalytically grown helix-shaped graphite nanotubes," Science (1994) 265, 635-639, the contents of which with respect to producing metal nanoparticles are incorporated herein by reference.
[0082] Metal catalyst nanoparticles are used in water-in-oil, oil-in-water or bicontinuous microemulsions, preferably water-in-oil or bicontinuous microemulsions, most preferably bicontinuous microemulsions. Advantageously, the uniformity of the metal particles is controlled by mixing a first (bicontinuous) microemulsion, in which the aqueous phase contains a metal complex salt that can ultimately be reduced to metal particles, with a second (bicontinuous) microemulsion, in which the aqueous phase contains a reducing agent capable of reducing the metal complex salt, and upon mixing, the metal complex is reduced, thus forming the metal particles. The controlled (bicontinuous) emulsion environment stabilizes the particles against sintering or Ostwald ripening. The size, concentration and durability of the catalyst particles are easily controlled. It is considered routine experimentation to adjust the average metal particle size within the above ranges, for example by modifying the molar ratio of metal precursor to reducing agent. Smaller particles are obtained by increasing the relative amount of reducing agent. The metal particles thus obtained are monodisperse, with deviations from the average particle size preferably within 10%, more preferably within 5%. Furthermore, the present technology does not restrict the actual metal precursors, as long as they can be reduced. Non-limiting examples of nanoparticles included in the carbon network comprising carbon nanofibers are noble metals (Pt, Pd, Au, Ag), iron group elements (Fe, Co and Ni), Ru and Cu.Suitable metal complexes include (i) platinum precursors, such as HPtCl; HPtCl·xH0; KPtCl; KPtCl·xH0; Pt(NH)(NO); Pt(CHO), (ii) ruthenium precursors, such as Ru(NO)(NO); Ru(dip)Cl [dip=4,7-diphenyl-1,10-phenanthroline]; RuCl, or (iii) palladium precursors, such as Pd(NO). 2, or (iv) nickel precursors, such as NiCl2 or NiCl2·xH2O; Ni(NO3)2; Ni(NO3)2·xH2O; Ni(CH3COO)2; Ni(CH3COO)2·xH2O; Ni(AOT)2 [AOT=bis(2-ethylhexyl)sulfosuccinate], where x can be any integer selected from 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10, typically 6, 7 or 8. Non-limiting suitable reducing agents are hydrogen gas, sodium boron hydride, sodium bisulfate, hydrazine or hydrazine hydrate, ethylene glycol, methanol and ethanol. Citric acid and dodecylamine are also suitable. The type of metal precursor is not essential to the invention. The metal of the particles of the (bicontinuous) microemulsion is preferably selected from the group consisting of Pt, Pd, Au, Ag, Fe, Co, Ni, Ru and Cu, and mixtures thereof, in order to control the morphology of the carbon structure network finally formed. The metal nanoparticles are finally embedded inside these structures, and the metal particles are physically attached to the structures. Although there is no minimum concentration of metal particles at which these networks are formed (indeed, the networks are formed using the modified carbon black manufacturing process according to the invention), it has been found that the yield increases with the metal particle concentration. In a preferred embodiment, the active metal concentration is at least 1 mM, preferably at least 5 mM, preferably at least 10 mM, more preferably at least 15 mM, more preferably at least 20 mM, in particular at least 25 mM, most preferably up to 3500 mM, preferably up to 3000 mM. In one embodiment, the metal nanoparticles comprise up to 250 μM. There is a catalyst concentration relative to the amount of aqueous phase of the (bicontinuous) microemulsion.
[0083] Atomization of the single phase emulsion, preferably an emulsion comprising a CBFS, is preferably achieved by spraying using a nozzle system 4, whereby the emulsion droplets come into contact with the hot waste gas a1 in the reaction zone 3b, resulting in traditional carbonization, network formation and subsequent aggregation to produce the carbon network according to the invention. The injection step preferably involves high temperatures above 600°C, preferably between 700°C and 3000°C, more preferably between 900°C and 2500°C, more preferably between 1100°C and 2000°C. [Example] EXAMPLES
[0084] Characterization of the cathode and / or anode of a lithium-ion battery comprising a carbon network comprising carbon nanofibers as a conductive additive according to the present invention The performance of lithium ion batteries comprising a cathode and / or anode comprising a carbon network comprising carbon nanofibers as a conductive additive according to the present invention ("carbon network") was compared with the performance of a lithium ion battery in which the anode comprises only artificial graphite (AG) and no additive, and with a lithium ion battery comprising AG in combination with conductive carbon black (Super C65) as a conductive additive. Two grades of carbon networks were used, designated hereafter as A and B. Both grades A and B were produced in a furnace-type black reactor by using the same feedstock. The residence times for grades A and B were in the range of 400-800 ms and 10-100 ms, respectively (based on theoretical models).
[0085] Grades D and C were also produced in a furnace carbon black reactor by using the same feedstock and residence time as A and B, respectively. Grade D was produced by using a 30% higher feed rate compared to A, while Grade C was produced by using a 30% lower feed rate compared to B.
[0086] Although the experiments reported here were performed with anodes, the work and results are not expected to be any different for cathodes for lithium-ion batteries. (Anode (& conductive additive) paste preparation) PVDF (300 mg) was dissolved in NMP (7.000 g) using mechanical stirring for 45 min. Conductive additive (300 mg) was added and 4 mm diameter glass beads (1.0 g) were added to increase the shear during mixing. The paste was mixed in a Speedmixer (Hauschildt) at 2500 rpm for 2 min, then further mixed at 2500 rpm for 10 min to obtain a dispersion. Artificial graphite (6.00 g) was added in a Speedmixer (Hauschildt) and mixed at 2500 rpm for 2 min, then further mixed at 2500 rpm for 10 min to obtain an anode paste.
[0087] [Table 1]
[0088] The viscosity increase of the anode paste when using Super C65 as the conductive additive was considerably higher when compared to using the same amounts of A and B instead. Indeed, when the proportion of Super C65 in the anode paste composition was increased beyond 400 mg, the anode paste could not be cast. However, when the A content was increased to 600 mg (while keeping the mass of the other components constant), a castable paste was still obtained. This therefore demonstrated that there was a clear advantage in terms of achieving a higher loading of conductive additive when using the network of the present invention, and processing could be improved. Castable pastes were obtained with C and D. (Anode preparation) The glass plate was thoroughly cleaned and dried using acetone. A few drops of NMP were added to the glass plate by capillary force to hold the copper foil (>99.9% Cu, 10 micron thickness, Nanografi) in place. The copper foil was cleaned using NMP and subsequently dried using a lint-free cloth. The anode paste was cast using a doctor blade set at various heights as specified in the table. The glass plate was transferred to an oven and kept at 110° C. overnight. The anodes were punched out (14 mm diameter). (Half-cell preparation) The spring, spacer, lithium disk (15.6 mm), a few drops of electrolyte (EC / EMC 1:1 1M LiPF6), electrolyte (EC / EMC 1:1 1M LiPF6) soaked separator (20 mm), a few drops of electrolyte (EC / EMC 1:1 1M LiPF6), and anode facing down were crimped together in a CR2032 coin cell in a glove box. After removing the half cell from the glove box, it was used immediately for electrochemical testing. The anode material is characterized in Table 2.
[0089] [Table 2]
[0090] a.Capacity A fresh half-cell was discharged at a constant discharge current of 0.2C until the potential dropped to 0.01V (approximately 5 hours of discharge). The half-cell was then held at 0.01V for 1 hour or until the discharge current was less than 1% of the initial discharge current. The half-cell was then left to equilibrate for 1 hour before being charged at 0.2C to 2.0V (approximately 5 hours of charge). The half-cell was then held at 2.0V for 1 hour or until the charge current was less than 1% of the initial charge current. The capacity was calculated by multiplying the charge current by the time it took to reach 2.0V, including the current required to hold the potential at 2.0V for 1 hour.
[0091] [Table 3]
[0092] b. Cycle ability (cycle life) The new half-cell was discharged at a constant discharge current of 0.2C until the potential dropped to 0.01V (approximately 5 hours of discharge). The half-cell was then held at 0.01V for 1 hour or until the discharge current was less than 1% of the initial discharge current. The half-cell was then left to equilibrate for 1 hour before being charged at 0.2C to 2.0V (approximately 5 hours of charge). The half-cell was then held at 2.0V for 1 hour or until the charge current was less than 1% of the initial charge current. This was a single cycle. The cycle was repeated (in terms of number of times) as many times as possible and the capacity loss was monitored as a function of cycles.
[0093] FIG. 3 shows that the specific capacity when using the AG anode (square) decreases dramatically and steadily with the number of cycles, while the specific capacity when using the AG / A anode (crossed) decreases more slowly from the beginning and practically balances after 100 cycles. FIG. 5 shows that the specific capacity for the AG / C (crossed) and AG / D (triangle) anodes does not decrease as steeply. From 20 to 100 cycles, the capacity is maintained at around 95%. This behavior is an improvement compared to the AG anode (FIG. 3), which showed a capacity loss of 50% around 50 cycles. This demonstrates that a longer cycle life is achieved when using the anode according to the invention. These results are also summarized in Table 4.
[0094] [Table 4]
[0095] c. Charge / discharge rate: Cycle ability at various C rates A lithium ion battery anode was prepared according to Table 5.
[0096] [Table 5]
[0097] The new half-cell was discharged at a constant discharge current of 0.5C until the potential dropped to 0.01V (about 2 hours discharge). The half-cell was then held at 0.01V for 1 hour or until the discharge current was less than 1% of the initial discharge current. The half-cell was then left to equilibrate for 1 hour and then charged at 0.5C to 2.0V (about 2 hours charge). The half-cell was then held at 2.0V for 1 hour or until the charge current was less than 1% of the initial charge current. This cycle was repeated 10 times. The discharge and charge currents were then changed to 1.0C (about 1 hour (discharge) charge) and this was repeated 10 times. The discharge and charge currents were then changed to 5.0C (12 minutes (discharge) charge) and this was repeated 10 times. The discharge and charge currents were then changed to 10.0C (6 minutes (discharge) charge) and this was repeated 10 times. Then, to observe the decrease in capacity after these 55 cycles, the discharge and charge currents were changed back to 0.5C (about 2 hours charge / discharge), and this was repeated 10 times. For grades C, D, and AG, after 10 cycles at 10.0C, the discharge and charge currents were changed back to 20.0C (3 minutes charge / discharge), and this was repeated 10 times. Then, to observe the decrease in capacity after these 66 cycles, the discharge and charge currents were changed back to 0.5C (about 2 hours charge / discharge), and this was repeated 10 times.
[0098] The results of these experiments are shown in Figures 4 and 6. Figure 4 shows that the specific capacity of the AG / grade B anode (squares) is generally superior to that of the AG anode (triangles), while the specific capacity of the AG / grade A (dashes) is significantly higher than that of the AG anode (triangles). Figure 6 shows that for AG / grade C (triangles) and grade D (circles), the specific capacity did not decrease as much as for AG (squares) at 10C. Even up to 20C, the capacity of AG / grade C and AG / grade D was superior to AG. When the C rate was reduced from 20C to 0.5C, 95-100% of the initial capacity could still be recovered for AG / grade C and AG / grade D. In contrast, the initial capacity of AG could not be recovered.
Claims
1. Use of a porous, chemically interconnected carbon network comprising carbon nanofibers as a conductive additive material in the anode and / or cathode of a rechargeable lithium or sodium battery.
2. 2. Use according to claim 1, wherein the carbon network comprising carbon nanofibers represents from 0.1 to 20% by weight, preferably more than 0.1% and less than 20% by weight, of the total mass of the cathode and / or the carbon network comprising carbon nanofibers represents from 0.1 to 10% by weight, preferably more than 0.1% and less than 10% by weight, of the total mass of the anode.
3. The use according to claim 1 or 2, wherein the carbon network comprises crystalline carbon nanofibers.
4. The use according to any one of claims 1 to 3, wherein the carbon nanofibers have an average fibre length of 30 to 10,000 nm.
5. 5. The use according to any one of claims 1 to 4, wherein the carbon network forms an intraparticle porous network, the carbon nanofibers are interconnected with other carbon nanofibers in the carbon network by chemical bonds via connections, the pores in the carbon network have an intraparticle pore diameter size of 5 to 150 nm using mercury intrusion porosimetry according to ASTM D4404-10, and the carbon nanofibers have an average aspect ratio of fiber length to thickness of at least 2, preferably with a d-spacing in the range of 0.340 to 0.5 nm.
6. 6. The use according to any one of claims 1 to 5, wherein the rechargeable lithium or sodium battery is suitable for smartphones, laptops, digital cameras and camcorders, as an uninterruptible power supply (UPS), as energy storage for power generation equipment, for medical and communication systems, and for electric and / or hybrid vehicles.
7. The use according to any one of claims 1 to 6, wherein the rechargeable lithium battery is a lithium-sulfur (Li-S) battery.
8. An anode and / or cathode of a lithium or sodium battery comprising a porous, chemically interconnected carbon network comprising carbon nanofibers as a conductive additive material, preferably a lithium-ion or sodium-ion battery anode and / or cathode.
9. 1. An anode and / or cathode of a lithium or sodium battery comprising a porous, chemically interconnected carbon network comprising carbon nanofibers, wherein said carbon network comprising carbon nanofibers represents 0.1-20% by weight, preferably greater than 0.1% and less than 20% by weight, of the total mass of the cathode, and / or wherein said carbon network comprising carbon nanofibers represents 0.1-10% by weight, preferably greater than 0.1% and less than 10% by weight, of the total mass of the anode.
10. 10. The lithium or sodium battery anode and / or cathode of claim 8 or 9, wherein the carbon network forms an intraparticle porous network, the carbon nanofibers are interconnected with other carbon nanofibers in the carbon network by chemical bonds through connections, the pores in the carbon network have intraparticle pore diameter sizes of 5 to 150 nm using mercury intrusion porosimetry according to ASTM D4404-10, and the carbon nanofibers have an average aspect ratio of fiber length to thickness of at least 2, preferably with a d-spacing in the range of 0.340 to 0.5 nm.
11. 11. The anode and / or cathode of a lithium or sodium battery according to claim 8, wherein the anode and / or cathode also comprises 0.1 to 10% by weight of a binder.
12. 12. The anode and / or cathode of a lithium or sodium battery according to any one of claims 8 to 11, wherein the cathode and / or anode also comprises 0.1 to 10 wt.%, preferably 0.5 to 5 wt.%, most preferably 1 to 3 wt.% of one or more further conductive additives selected from conductive carbon black, Super P, acetylene black, carbon nanofibers and carbon nanotubes.
13. 13. The lithium battery cathode of claim 8, wherein the cathode comprises, as a conductive additive material, a sulfur composite comprising a porous, chemically interconnected carbon network comprising carbon nanofibers.
14. The battery is a lithium battery, the anode comprises 90 to 99.9 wt. % of an additional active material, the additional active material being selected from the group consisting of graphite, silicon, silicon-based compounds (SiO 2 13. The battery anode of claim 9, wherein said anode is selected from the group consisting of tungsten, tin, tantalum, tantalum hydroxide, tin ...
15. The additional active material is silicon, a silicon-based compound (SiO 2 ) or a combination thereof, 2 ) or a combination thereof is mixed with the carbon network comprising the carbon nanofibers in the anode, or the carbon network comprising the carbon nanofibers is preferably made of silicon, the silicon-based compound (SiO 2 15. The battery anode of claim 14, wherein the battery anode is coated with a metal oxide, a fluorine atom ...
16. 16. A rechargeable lithium or sodium battery comprising an anode and / or a cathode according to any one of claims 8 to 15, said rechargeable lithium or sodium battery being preferably a lithium-ion or sodium-ion battery.
17. 17. The rechargeable lithium or sodium battery of claim 16, wherein the rechargeable battery is suitable for inclusion in smartphones, laptops, digital cameras and camcorders, as uninterruptible power supplies (UPS), as energy storage for power generation equipment, in medical and communication systems, and in electric and / or hybrid vehicles.
18. Use of a carbon network according to any one of claims 1 to 7, obtained by a process for producing a crystalline carbon network by injecting a water-in-oil or bicontinuous microemulsion c comprising metal catalyst nanoparticles into a reactor 3 containing a reaction zone 3b and a termination zone 3c at a temperature above 600°C, preferably above 700°C, more preferably above 900°C, even more preferably above 1000°C, more preferably above 1100°C, preferably at most 3000°C, more preferably at most 2500°C, most preferably at most 2000°C, in order to produce a crystalline carbon network e, transporting these networks e to the termination zone 3c, and quenching or stopping the formation of the crystalline carbon network in the termination zone by spraying into water d, anode and / or cathode of a lithium or sodium battery according to any one of claims 8 to 15, or a rechargeable lithium or sodium battery according to claim 16 or 17.
19. A battery-powered device comprising an anode and / or cathode of a lithium or sodium battery according to any one of claims 8 to 15 or a rechargeable lithium or sodium battery according to claim 16 or 17, wherein the rechargeable lithium or sodium battery is preferably a lithium-ion or sodium-ion battery.
20. 20. The device of claim 19, wherein the device is a smartphone, a laptop, a digital camera, a camcorder, a medical and communication system, an uninterruptible power supply (UPS), an energy storage device for a power generation unit, or an electric and / or hybrid vehicle.
Citation Information
Patent Citations
Negative electrode material, negative electrode using the same, and lithium ion battery and lithium polymer battery using negative electrode
JP2004220910A
Negative electrode material, negative electrode using the same, and lithium ion secondary battery using the negative electrode
JP2004303613A
Electrode for secondary battery, its manufacturing method, and secondary battery
JP2008277128A
Material for forming electrode and its use
JP2013077426A
Porous carbon nanotube microspheres and manufacturing method and use thereof, metallic lithium-framework carbon composite material and manufacturing method thereof, negative electrode, and battery