Positive electrode active material, its manufacturing method and lithium secondary battery including the same

A phosphorus-doped aluminum oxide coating on high nickel positive electrode active materials addresses stability and resistance issues, enhancing the lifespan and energy density of lithium secondary batteries.

JP2024540233AActive Publication Date: 2024-10-31LG CHEM LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024525913
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-07
Filing Date
2022-12-07
Publication Date
2024-10-31
Estimated Expiration
2042-12-07

AI Technical Summary

Technical Problem

High nickel positive electrode active materials in lithium secondary batteries face issues such as electrolyte decomposition, structural instability, metal elution, and rapid capacity degradation due to their high oxidation potential, leading to safety concerns and decreased performance.

Method used

A coating layer composed of phosphorus-doped aluminum oxide is applied to the surface of high nickel positive electrode active materials using atomic layer deposition, ensuring a thickness of 0.1 to 2.0 nm, which enhances stability and reduces interfacial resistance.

Benefits of technology

The phosphorus-doped aluminum oxide coating improves the lifespan, energy density, and cycle characteristics of the positive electrode, preventing increases in resistance and maintaining capacity retention, thus stabilizing the battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540233000001_ABST
    Figure 2024540233000001_ABST
Patent Text Reader

Abstract

The present invention relates to a cathode active material, the cathode active material including a particulate cathode active material and a coating layer formed on a surface of the particulate cathode active material, the coating layer including aluminum oxide doped with phosphorus (P), and a thickness of the coating layer being 0.1 nm to 2.0 nm, a manufacturing method thereof, and a cathode and a lithium secondary battery including the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0174108 filed on December 7, 2021, and all contents disclosed in the documents of said Korean patent application are incorporated as part of this specification.

[0002] The present invention relates to a positive electrode active material, a method for producing the same, and a positive electrode and a lithium secondary battery each including the same. [Background technology]

[0003] Recently, with the development of technologies such as electric vehicles, the need for high-capacity secondary batteries is increasing. As a result, active research is being conducted on positive electrodes using high nickel (High Ni) positive electrode active materials with excellent capacity characteristics.

[0004] The high oxidation potential of the positive electrode causes the electrolyte to decompose on the surface, which generates gas and causes the lithium secondary battery to expand. In addition, the structure becomes unstable during the process of lithium ion insertion and extraction, which causes metal to leach from the positive electrode and deteriorate it. In particular, this situation is even more severe in high nickel (High Ni) positive electrode active materials, and occurs suddenly, causing a rapid decrease in the remaining capacity of the lithium secondary battery and a decrease in safety.

[0005] To solve these problems, a method of forming a coating layer on the surface of high-nickel positive active material particles has been proposed. However, the positive active material formed in a structure of secondary particles formed by agglomeration of primary particles has a complex surface morphology, and pores of various sizes are distributed within the secondary particles, so it is not easy to form a thin and uniform coating layer inside the pores.

[0006] As a specific example, when a boron-based coating layer is formed on a positive electrode active material, it is known that a relatively uniform coating layer is formed along the surface, but the glassy properties of boron result in a decrease in rolling density, which reduces energy density, or excessive particle cracking during over-rolling. In addition, when an inorganic or organic coating layer is formed on a positive electrode active material, the stability of the positive electrode active material is improved, but the lithium ion conductivity is reduced, which results in an increase in interface resistance and cell resistance. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Korean Patent Publication No. 10-2016-0026306 Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been devised to solve the problems of the conventional art, and aims to provide a positive electrode active material having a coating layer formed thereon, which can improve the stability of the positive electrode active material, prevent a decrease in rolling density, and prevent an increase in resistance.

[0009] Another object of the present invention is to provide a positive electrode active material having a coating layer formed thereon, which can improve the life and energy density of a positive electrode active material having high energy density and prevent a decrease in output characteristics.

[0010] Another object of the present invention is to provide a method for producing the positive electrode active material, a positive electrode including the positive electrode active material, and a lithium secondary battery including the positive electrode active material. [Means for solving the problem]

[0011] In order to solve the above problems, the present invention provides a positive electrode active material, a method for producing the same, and a positive electrode and a lithium secondary battery each including the same.

[0012] (1) The present invention provides a cathode active material comprising: a particulate cathode active material; and a coating layer formed on a surface of the particulate cathode active material, the coating layer comprising aluminum oxide doped with phosphorus (P), and a thickness of the coating layer ranging from 0.1 nm to 2.0 nm.

[0013] (2) The present invention provides the positive electrode active material according to (1) above, wherein the coating layer has a thickness of 0.2 nm or more and 1.0 nm or less.

[0014] (3) The present invention provides a positive electrode active material, in the above (1) or (2), wherein the phosphorus (P)-doped aluminum oxide is represented by the following Chemical Formula 1: [Chemical formula 1] AlO m P n In the above Chemical Formula 1, m is 1.7 or more and 2.6 or less, and n is 0.01 or more and 0.4 or less.

[0015] (4) The present invention provides the positive electrode active material according to the above (3), in which m is 2.0 or more and 2.5 or less, and n is 0.15 or more and 0.30 or less.

[0016] (5) The present invention provides a positive electrode active material according to any one of (1) to (4), wherein the coating layer has a phosphorus (P) content of 1% by weight or more and 15% by weight or less.

[0017] (6) The present invention provides a positive electrode active material according to any one of (1) to (5), wherein the coating layer has a phosphorus (P) content of 8% by weight or more and 12% by weight or less.

[0018] (7) The present invention provides a positive electrode active material according to any one of the above (1) to (6), wherein the particulate positive electrode active material contains a lithium transition metal composite oxide represented by the following chemical formula 2: [Chemical formula 2] Li a Ni b Coc Mn d M 1 e O2 In the above Chemical Formula 2, M 1 is at least one selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, Sn, Y, Zn, F, P and S, and 0.9≦a≦1.2, 0 <b<1、0<c<1、0<d<1、0≦e<0.2、b+c+d+e=1である。

[0019] (8) The present invention provides a method for producing a positive electrode active material, the method including: a step (S1) of loading a particulate positive electrode active material into a reaction chamber for carrying out atomic layer deposition; and a step (S2) of forming a coating layer on a surface of the positive electrode active material by performing a unit process including the following steps (S10) to (S30) a plurality of times, wherein the thickness of the coating layer formed by the step (S2) is 0.1 nm or more and 2.0 nm or less. (S10) injecting a vapor phase aluminum precursor into a reaction chamber and injecting a purge gas; (S20) injecting a gas phase reaction gas into the reaction chamber and injecting a purge gas; (S30) Injecting a gas-phase phosphorus (P)-containing precursor into the reaction chamber and injecting a purge gas.

[0020] (9) The present invention provides a method for producing a positive electrode active material according to the above (8), wherein the unit process including the steps (S10) to (S30) of the step (S2) is represented by the following formula 1 or 2: [Formula 1] [{(S10)-(S20)} x -{(S30)-(S20)} y ] z [Formula 2] [{(S30)-(S20)} y -{(S10)-(S20)} x ] z In the above formulas 1 and 2, "-" indicates the execution order of the unit process, x is the number of times {(S10)-(S20)} is repeated, and is an integer selected from 1 to 5; y is the number of times that {(S30)-(S20)} is repeated, and is an integer selected from 1 to 5; z is [{(S10)-(S20)} x -{(S30)-(S20)} y ] or [{(S30)-(S20)} y -{(S10)-(S20)} x ] is repeated, and is an integer selected from 1 to 20.

[0021] (10) The present invention provides a method for producing a positive electrode active material according to the above (8) or (9), wherein the aluminum precursor is one or more selected from the group consisting of trimethylaluminum, triethylaluminum, aluminum ethoxide, and tris(diethylamido)aluminum.

[0022] (11) The present invention provides the method for producing a positive electrode active material according to any one of the above (8) to (10), wherein the reactive gas is at least one selected from the group consisting of gas-phase water vapor (HO), ozone (O) and oxygen plasma.

[0023] (12) The present invention provides the method for producing a positive electrode active material according to any one of (8) to (11), wherein the phosphorus (P)-containing precursor is at least one selected from the group consisting of trimethylphosphate and triethylphosphate.

[0024] (13) The present invention provides a positive electrode comprising the positive electrode active material according to any one of (1) to (7) above.

[0025] (14) The present invention provides a lithium secondary battery comprising the positive electrode according to (13) above. Effect of the Invention

[0026] The positive electrode active material of the present invention includes aluminum oxide doped with phosphorus (P) and includes a thin and uniform coating layer, thereby improving the life and stability and preventing an increase in interface resistance and cell resistance.

[0027] Furthermore, the positive electrode active material of the present invention has superior rolling characteristics compared to conventional coating layers containing boron, and therefore the energy density of the positive electrode can be improved.

[0028] Furthermore, according to the method for producing a positive electrode active material of the present invention, it is possible to form a thin and uniform coating layer on the surface of the particulate positive electrode active material.

[0029] Furthermore, a lithium secondary battery including the positive electrode active material of the present invention has improved cycle characteristics, excellent capacity retention, and a low rate of increase in resistance due to degradation, thereby suppressing a decrease in output. [Brief description of the drawings]

[0030] [Figure 1] 1 is a graph showing the rolled density by load of the positive electrode active materials produced in Examples 1 to 3 of the present invention and Comparative Examples 1 and 3. [Diagram 2] 1 is a graph showing the discharge capacity according to the number of cycles of lithium secondary batteries including the positive electrode active materials prepared in Examples 1 to 3 and Comparative Examples 1 and 3 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] The present invention will now be described in further detail in order to facilitate understanding of the present invention.

[0032] The terms and words used in the description of the present invention and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0033] In the present invention, the term "primary particle" refers to the smallest particle unit that can be distinguished as a single mass when a cross section of a positive electrode active material is observed through a scanning electron microscope (SEM), and may be composed of a plurality of crystal grains.

[0034] In the present invention, the term "secondary particle" refers to a secondary structure formed by agglomeration of a plurality of primary particles. The average particle size of the secondary particles can be measured using a particle size analyzer.

[0035] In the present invention, the term "average particle size (D 50 The "average particle size" refers to the particle size at the 50% point of the volume cumulative distribution by particle size. The average particle size is determined by dispersing the powder to be measured in a dispersion medium, introducing it into a commercially available laser diffraction particle size measuring device (e.g., S3500 manufactured by Microtrac), measuring the difference in the diffraction pattern according to the particle size when the particles pass through a laser beam, calculating the particle size distribution, and calculating the particle diameter at the 50% point of the volume cumulative distribution by particle size in the measuring device. 50 can be measured.

[0036] positive electrode active material The present invention provides a positive electrode active material.

[0037] According to an embodiment of the present invention, the positive electrode active material includes a particulate positive electrode active material and a coating layer formed on a surface of the particulate positive electrode active material, the coating layer includes aluminum oxide doped with phosphorus (P), and the coating layer may have a thickness of 0.1 nm to 2.0 nm.

[0038] According to an embodiment of the present invention, the coating layer may be formed by atomic layer deposition according to the method for manufacturing a cathode active material described below, whereby the coating layer may be formed thin and uniformly on the surface of the particulate cathode active material. That is, the coating layer may be formed with a uniform thickness on the entire surface of the particulate cathode active material by being formed by atomic layer deposition. Therefore, the thickness of the coating layer may be an arithmetic average thickness of the thickness of the entire coating layer formed on the surface of the particulate cathode active material. In addition, the coating layer may have the same thickness regardless of the surface of the cathode active material including the coating layer.

[0039] According to one embodiment of the present invention, the thickness of the coating layer may be 0.1 nm or more, 0.2 nm or more, 0.3 nm or more, 0.4 nm or more, or 0.5 nm or more, and may be 2.0 nm or less, 1.9 nm or less, 1.8 nm or less, 1.7 nm or less, 1.6 nm or less, 1.5 nm or less, 1.4 nm or less, 1.3 nm or less, 1.2 nm or less, 1.1 nm or less, 1.0 nm or less, 0.9 nm or less, 0.8 nm or less, or 0.7 nm or less. Within this range, an increase in interface resistance is suppressed and rolling characteristics are excellent, so that the energy density of the positive electrode can be improved.

[0040] According to an embodiment of the present invention, the phosphorus (P)-doped aluminum oxide may be represented by the following Formula 1. Here, Formula 1 may be a composition formula showing an average composition of the phosphorus (P)-doped aluminum oxide.

[0041] [Chemical formula 1] AlO m P n

[0042] In the above Chemical Formula 1, m is 1.7 or more and 2.6 or less, and n is 0.01 or more and 0.4 or less.

[0043] In order to manufacture the aluminum oxide doped with phosphorus (P) contained in the coating layer using atomic layer deposition (ALD) as in the manufacturing method of the positive electrode active material described below, an aluminum precursor in the form of a ligand bonded to aluminum as a central element and a phosphorus (P)-containing precursor in the form of a ligand bonded to phosphorus (P) as a central element are required. Here, phosphorus (P) has many valence electrons, and due to steric hindrance caused by the ligand, the reactivity of the phosphorus (P)-containing precursor with the hydroxyl group present on the surface of the deposition target is lower than the reactivity of the aluminum (Al)-containing precursor with the hydroxyl group. In addition, even after the aluminum precursor reacts with the reactive gas (e.g., water), the ligand bonded to aluminum is not completely removed and remains partially, and the steric hindrance effect becomes even worse, so the surface reactivity of the phosphorus (P)-containing precursor becomes even lower. Therefore, when aluminum oxide doped with phosphorus (P) represented by the above formula 1 is formed by atomic layer deposition, the efficiency (remaining rate of the central element in the deposition layer) of the "(S30)-(S20)" process of forming phosphorus (P) oxide is lower than the "(S10)-(S20)" process of forming aluminum oxide in the manufacturing method of the positive electrode active material described below. Also, even if the number of "(S30)-(S20)" processes (y) is increased relative to the number of "(S10)-(S20)" processes (x) in a unit process, when the value of n in the above composition formula exceeds 0.4, the rate of increase in the value of n due to the increase in the number of "(S30)-(S20)" processes (y) is significantly reduced. Therefore, in terms of the effect of increasing the phosphorus (P) content in aluminum oxide doped with phosphorus (P) and the number of atomic layer depositions and the cost efficiency therefor, it is preferable that n is 0.4 or less.

[0044] According to an embodiment of the present invention, in the formula 1, m may be 1.7 or more, 1.8 or more, 1.9 or more, 2.0 or more, or 2.1 or more, and may be 2.6 or less, 2.5 or less, 2.4 or less, 2.3 or less, 2.25 or less, or 2.21 or less. In addition, in the formula 1, n may be 0.01 or more, 0.05 or more, 0.10 or more, 0.15 or more, 0.16 or more, 0.17 or more, or 0.18 or more, and may be 0.40 or less, 0.35 or less, 0.30 or less, or 0.25 or less. Within this range, the cycle characteristics of a lithium secondary battery including the positive electrode active material are further improved, the capacity retention rate is further excellent, and the rate of increase in resistance due to deterioration is further reduced, thereby suppressing the decrease in output.

[0045] According to an embodiment of the present invention, the content of phosphorus (P) in the coating layer may be 1 wt % or more, 2 wt % or more, 3 wt % or more, 4 wt % or more, 5 wt % or more, 6 wt % or more, 7 wt % or more, or 8 wt % or more, and may be 15 wt % or less, 14 wt % or less, 13 wt % or less, or 12 wt % or less. Within this range, the stability of the positive electrode active material and the life of a lithium secondary battery including the same may be improved.

[0046] According to an embodiment of the present invention, the particulate positive electrode active material may include a lithium transition metal composite oxide represented by the following Formula 2:

[0047] [Chemical formula 2] Li a Ni b Co c Mn d M 1 e O2

[0048] In the above Chemical Formula 2, M 1 is at least one selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, Sn, Y, Zn, F, P and S, and 0.9≦a≦1.2, 0 <b<1、0<c<1、0<d<1、0≦e<0.2、b+c+d+e=1である。

[0049] According to one embodiment of the present invention, in Formula 2, M 1 is a doping element that can be contained in the lithium transition metal composite oxide, and can be appropriately selected as necessary.

[0050] According to one embodiment of the present invention, in Formula 2, a is a molar ratio of lithium to transition metal in the lithium transition metal composite oxide, and may be 0.9 or more, 0.95 or more, or 1.0 or more, and may be 1.2 or less, 1.1 or less, 1.07 or less, 1.05 or less, or 1.03 or less.

[0051] According to an embodiment of the present invention, in Formula 2, b, c, d, and e are nickel (Ni), cobalt (Co), manganese (Mn), and a doping element (M 1 ) may be a molar fraction relative to nickel (Ni) among the transition metals. As a specific example, the b is a molar fraction relative to nickel (Ni) among the transition metals, and may be greater than 0, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, or 0.8 or more, and may be less than 1.0, 0.95 or less, 0.9 or less, or 0.85 or less. The c is a molar fraction relative to cobalt (Co) among the transition metals, and may be greater than 0, 0.05 or more, or 0.1 or more, and may be less than 1, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, or 0.2 or less. The d is a molar fraction of manganese (Mn) among the transition metals, and may be greater than 0, 0.05 or more, or 0.1 or more, and may be less than 1, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, or 0.2 or less. The e is a molar fraction of manganese (Mn) among the transition metals. 1), and can be 0, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, 0.10 or more, 0.11 or more, 0.12 or more, 0.13 or more, 0.14 or more, 0.15 or more, 0.16 or more, 0.17 or more, 0.18 or more, or 0.19 or more. and can be less than 0.20, 0.19 or less, 0.18 or less, 0.17 or less, 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, 0.10 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, 0.05 or less, 0.04 or less, 0.03 or less, 0.02 or less, or 0.01 or less.

[0052] According to an embodiment of the present invention, the lithium transition metal composite oxide may be a high-nickel lithium transition metal composite oxide containing nickel (Ni) in an amount of 60 mol % or more among transition metals. In this case, a high energy density can be ensured due to the high nickel content, and the coating layer can prevent a decrease in stability of the positive electrode active material due to the high nickel content.

[0053] According to an embodiment of the present invention, the particulate positive electrode active material may be a secondary particle formed by agglomeration of primary particles. In a specific example, the positive electrode active material may have an average particle size (D 50 ) may be 0.5 μm or more, 1 μm or more, 1.5 μm or more, or 2 μm or more, and may be 20 μm or less, 18 μm or less, 16 μm or less, 14 μm or less, or 12 μm or less. Within this range, the initial charge / discharge efficiency is excellent and the resistance can be reduced. 50 ) may mean the average particle size of secondary particles formed by aggregation of the primary particles.

[0054] According to an embodiment of the present invention, the positive electrode active material has a rolled density of 2.85 g / cc or more, 2.86 g / cc or more, 2.87 g / cc or more, 2.88 g / cc or more, 2.89 g / cc or more, 2.90 g / cc or more, 2.91 g / cc or more, 2.92 g / cc or more, 2.93 g / cc or more, 2.94 g / cc or more, 2.95 g / cc or more, 2.96 g / cc or more, 2.97 g / cc or more, 2.98 g / cc or more, 2.99 g / cc or more, 3.00 g / cc or more, 3.01 g / cc or more, 3.02 g / cc or more, 3.03 g / cc or more, 3.04 g / cc or more, 3.05 g / cc or more, 3.06 g / cc or more, 3.07 g / cc or more, 3.08 g / cc or more, 3.09 g / cc or more, 3.10 g / cc or more, 3.11 g / cc or more, 3.12 g / cc or more, 3.13 g / cc or more, 3.14 g / cc or more, 3.15 g / cc or more, 3.16 g / cc or more, 3.17 g / cc or more, 3.18 g / cc or more, 3.19 g / cc or more, 3.20 g / cc or more, 3.21 g / cc or more, 3.22 g / cc or more, 3.23 g / cc or more, 3.24 g / cc or more, 3.25 g / cc or more, 3.26 g / cc or more, 3.27 g / cc or more, 3.28 g / cc or more, 3.29 g / 0.03g / cc or more, 3.04g / cc or more, 3.05g / cc or more, 3.06g / cc or more, 3.07g / cc or more, 3.08g / cc or more, 3.09g / cc or more, 3.10g / cc or more, 3.11g / cc or more, 3.12g / cc or more, 3.13g / cc or more, 3.14g / cc or more, 3.15g / cc or more, 3.16g / cc or more, or 3.17g / cc or more, and can be 3.50g / cc or less, 3.40g / cc or less, 3.30g / cc or less, or 3.20g / cc or less. When the rolled density of the positive electrode active material measured under a load of 2,000 kgf is equal to or greater than the lower limit, the positive electrode active material has a high energy density and prevents particle cracks from occurring during rolling, thereby improving the life and stability of a lithium secondary battery containing the positive electrode active material and preventing an increase in interface resistance and cell resistance.

[0055] Method for producing positive electrode active material The present invention provides a method for producing a positive electrode active material.

[0056] According to an embodiment of the present invention, the method for preparing the positive electrode active material may be a method for preparing the positive electrode active material described above, and as a specific example, may be a method for forming a coating layer including aluminum oxide doped with phosphorus (P) on a surface of a particulate positive electrode active material, the coating layer having a thickness of 0.1 nm to 2.0 nm.

[0057] According to an embodiment of the present invention, the method for preparing a positive electrode active material includes a step (S1) of loading a particulate positive electrode active material into a reaction chamber for performing atomic layer deposition (ALD), and a step (S2) of forming a coating layer on a surface of the positive electrode active material by performing a plurality of unit processes including the following steps (S10) to (S30), and a thickness of the coating layer formed by the step (S2) may be 0.1 nm or more and 2.0 nm or less.

[0058] (S10) injecting a vapor phase aluminum precursor into a reaction chamber and injecting a purge gas; (S20) injecting a gas phase reaction gas into the reaction chamber and injecting a purge gas; (S30) Injecting a gas-phase phosphorus (P)-containing precursor into the reaction chamber and injecting a purge gas.

[0059] According to one embodiment of the present invention, the step (S1) is a step of loading a particulate positive electrode active material to be coated into a reaction chamber of an ALD system, and may be performed by positioning the particulate positive electrode active material obtained in a powder state in the reaction chamber. Here, the particulate positive electrode active material may be the same as the particulate positive electrode active material described above in the positive electrode active material.

[0060] According to an embodiment of the present invention, the atomic layer deposition is a self-limiting surface treatment method in which a thin film layer is formed one by one with a thickness of the atomic size. The atomic layer deposition is different from a chemical vapor deposition (CVD) method in which a thin film is deposited by thermal decomposition and gas phase reaction of a reactant gas, in that one reactant reacts with the surface of a substrate to perform chemisorption, and then a second or third reactant is injected and chemisorption is performed on the substrate to form a thin film. That is, it is a method of forming a thin film by chemisorption by periodically supplying each reactant, and the reactant reacts only on the surface of the target substrate, for example, the particulate positive electrode active material, and the reactants do not react with each other, so that deposition on an atomic level is possible. In addition, since a thin film layer is formed on any surface exposed during atomic layer deposition, when coating is performed on a particulate positive electrode active material according to the method for producing a positive electrode active material of the present invention, a uniform coating layer can be formed on the entire surface of the particulate positive electrode active material.

[0061] According to one embodiment of the present invention, the step (S2) may be a step of injecting a precursor and / or a reactant gas into a reaction chamber and performing atomic layer deposition on a surface of a particulate positive electrode active material to form a coating layer.

[0062] According to an embodiment of the present invention, the atomic layer deposition in step (S2) can easily form a coating layer by atomic layer deposition at a lower temperature than chemical vapor deposition, which deposits particles formed by a chemical reaction of gas on the surface of a substrate. As a specific example, the atomic layer deposition can be performed at a temperature of 60°C to 240°C. As a more specific example, the atomic layer deposition can be performed at a temperature of 70°C or more, 80°C or more, 90°C or more, 100°C or more, 110°C or more, 120°C or more, 130°C or more, or 140°C or more, or 230°C or less, 220°C or less, 210°C or less, 200°C or less, 190°C or less, 180°C or less, 170°C or less, or 160°C or less. Within this range, the reaction can be smoothly performed and / or the coating layer can be uniformly formed, the phosphorus (P) content in the coating layer can be secured at an appropriate level, and a high-temperature process of 400°C or more is not required, thereby preventing the deterioration of the physical properties of the positive electrode active material.

[0063] According to one embodiment of the present invention, the unit process including steps (S10) to (S30) of step (S2) can be represented by the following formula 1 or 2.

[0064] [Formula 1] [{(S10)-(S20)} x -{(S30)-(S20)} y ] z

[0065] [Formula 2] [{(S30)-(S20)} y -{(S10)-(S20)} x ] z

[0066] In the above formulas 1 and 2, "-" indicates the execution order of the unit process, In the formulas 1 and 2, "-" indicates the order of the unit steps. That is, an expression such as "(S10)-(S20)" means that step (S10) is followed by step (S20).

[0067] In addition, in the formulas 1 and 2, x means the number of times {(S10)-(S20)} is repeated. The x may be an integer selected from 1 to 5, and specifically may be an integer selected from 1 to 3, and more specifically may be 1 or 2.

[0068] In addition, in the formulas 1 and 2, y means the number of times {(S30)-(S20)} is repeated. The y may be an integer selected from 1 to 5, and as a specific example, an integer selected from 1 to 3. As described above, even if the number of times {(S30)-(S20)} is repeated is increased according to y, the content of phosphorus (P) doped in the coating layer does not increase proportionately, and therefore, within the above range, the process efficiency can be further improved.

[0069] According to an embodiment of the present invention, the ratio of x and y can be adjusted to dope aluminum oxide with phosphorus (P) within a desired content range.

[0070] In addition, in the formulas 1 and 2, z is [{(S10)-(S20)} x -{(S30)-(S20)} y ] or [{(S30)-(S20)} y -{(S10)-(S20)} x The z may be an integer selected from 1 to 20, and specifically may be an integer selected from 1 to 15, 2 to 12, 3 to 10, 4 to 8, or 5 to 7, and within this range, the thickness of the coating layer may be adjusted to an appropriate level.

[0071] According to an embodiment of the present invention, the step (S10) included in the unit process may be a step for atomic layer deposition of aluminum from an aluminum precursor, and the aluminum precursor may be an aluminum compound represented by the following Chemical Formula 3:

[0072] [Chemical formula 3] AlR 1 R 2 R 3

[0073] In the above Chemical Formula 3, R 1 ~R 3 Each of them can be an organic group bonded to Al. Specific examples include R 1 ~R 3 may each independently be a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a halogen group, or an amino group, and the amino group may be a secondary amino group or a tertiary amino group substituted with an alkyl group having 1 to 10 carbon atoms. 1 ~R 3 may each independently be an alkyl group having 1 to 5 carbon atoms; an alkoxy group having 1 to 5 carbon atoms; a halogen group; or a secondary amino group or a tertiary amino group substituted with an alkyl group having 1 to 5 carbon atoms. 1 ~R 3 may each independently be an alkyl group having 1 to 3 carbon atoms; an alkoxy group having 1 to 3 carbon atoms; a halogen group; or a tertiary amino group substituted with an alkyl group having 1 to 3 carbon atoms.

[0074] According to an embodiment of the present invention, the aluminum precursor may be at least one selected from the group consisting of trimethylaluminum, triethylaluminum, tri-n-propylaluminum, tri-n-butylaluminum, aluminum ethoxide, dimethylaluminum chloride, diethylaluminum chloride, di-n-propylaluminum chloride, di-n-butylaluminum chloride, tris(dimethylamino)aluminum, and tris(diethylamino)aluminum. As a specific example, the aluminum precursor may be at least one selected from the group consisting of trimethylaluminum, triethylaluminum, aluminum ethoxide, and tris(diethylamido)aluminum.

[0075] According to an embodiment of the present invention, in the step (S10), the aluminum precursor may be injected into the reaction chamber in a state filled in a steel container maintained at 10° C. to 50° C., 10° C. to 40° C., 10° C. to 30° C., or 15° C. to 25° C. When injected into the reaction chamber, the aluminum precursor may be injected in a vaporized state by reducing pressure without using a separate carrier gas, or may be injected using an inert gas as a carrier gas.

[0076] According to one embodiment of the present invention, the step (S20) may be a step for oxidizing an aluminum precursor and / or a phosphorus (P)-containing precursor from a reaction gas, and the reaction gas may be at least one selected from the group consisting of water vapor (HO), ozone (O) and oxygen plasma as an oxidizing agent.

[0077] According to an embodiment of the present invention, in the step (S20), the reaction gas may be injected into the reaction chamber in a state filled in a steel container maintained at 0° C. to 40° C., 0° C. to 30° C., 10° C. to 20° C., or 12° C. to 18° C. When injected into the reaction chamber, the reaction gas may be injected in a state vaporized by reducing pressure without using a separate carrier gas, or may be injected using an inert gas as a carrier gas.

[0078] According to an embodiment of the present invention, the step (S30) may be a step for doping aluminum oxide with phosphorus by atomic layer deposition from a phosphorus (P)-containing precursor, and the phosphorus (P)-containing precursor may be a phosphate-based compound represented by the following Chemical Formula 4 (Chemical Formula 1).

[0079] [ka]

[0080] In the above Chemical Formula 4, R 4 ~R 6 may each independently be hydrogen or an alkyl group having 1 to 10 carbon atoms. 4 ~R 6 may each independently be an alkyl group having 1 to 8 carbon atoms. 4 ~R 6 may each independently be an alkyl group having 1 to 4 carbon atoms.

[0081] According to an embodiment of the present invention, the phosphorus (P)-containing precursor may be at least one selected from the group consisting of trimethylphosphate and triethylphosphate.

[0082] According to one embodiment of the present invention, in the step (S30), the phosphorus-containing precursor may be injected into the reaction chamber in a state filled in a steel container maintained at 50° C. to 100° C., 60° C. to 100° C., 70° C. to 100° C., or 80° C. to 90° C. When injected into the reaction chamber, the phosphorus-containing precursor may be injected in a vaporized state by reducing pressure without using a separate carrier gas, or may be injected using an inert gas as a carrier gas.

[0083] According to one embodiment of the present invention, the purge gas injected during the purging steps (S10) to (S30) may be at least one selected from inert gases such as Ar, N2, He, Ne and / or Kr, and may preferably be Ar or N2.

[0084] positive electrode The present invention provides a positive electrode comprising the positive electrode active material.

[0085] According to an embodiment of the present invention, the positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, and the positive electrode active material layer may include the positive electrode active material.

[0086] According to an embodiment of the present invention, the positive electrode current collector may include a metal having high conductivity, and may be easily attached to the positive electrode active material layer, and may be non-reactive in the voltage range of the battery. The positive electrode current collector may be, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The positive electrode current collector may have a thickness of typically 3 μm to 500 μm, and may have fine irregularities on the surface of the current collector to enhance the adhesive strength of the positive electrode active material. For example, the positive electrode current collector may be used in various forms, such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0087] According to an embodiment of the present invention, the positive electrode active material layer may selectively include a conductive material and a binder, if necessary, together with the positive electrode active material. Here, the positive electrode active material may be included in an amount of 80 wt% to 99 wt%, more specifically, 85 wt% to 98.5 wt%, based on the total weight of the positive electrode active material layer, and within this range, excellent capacity characteristics may be exhibited.

[0088] According to an embodiment of the present invention, the conductive material is used to give conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive tubes such as carbon nanotubes; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. Among these, one type alone or a mixture of two or more types can be used. The conductive material can be included in an amount of 0.1% by weight to 15% by weight based on the total weight of the positive electrode active material layer.

[0089] According to an embodiment of the present invention, the binder serves to improve adhesion between the positive electrode active material particles and adhesion between the positive electrode active material and the current collector.Specific examples of the binder include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylalcohol, polyacrylonitrile, polymethyl methacrylate, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, polymers in which hydrogen is substituted with Li, Na, or Ca, or various copolymers thereof, and the like, and one or more of these may be used alone or in combination. The binder may be included in an amount of 0.1% by weight to 15% by weight based on the total weight of the positive electrode active material layer.

[0090] According to an embodiment of the present invention, the positive electrode may be manufactured by a conventional method for manufacturing a positive electrode, except for using the positive electrode active material. Specifically, the positive electrode may be manufactured by applying a composition for forming a positive electrode active material layer, which is prepared by dissolving or dispersing the positive electrode active material and, if necessary, a binder, a conductive material, and a dispersant in a solvent, onto a positive electrode current collector, followed by drying and rolling, or by casting the composition for forming a positive electrode active material layer onto another support, followed by peeling the composition from the support, and laminating the resulting film onto a positive electrode current collector.

[0091] According to an embodiment of the present invention, the solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), dimethylformamide (DMF), acetone, or water, and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, binder, and dispersant in consideration of the coating thickness of the slurry and the manufacturing yield, and to have a viscosity that can provide excellent thickness uniformity when applied to manufacture a positive electrode.

[0092] According to an embodiment of the present invention, the positive electrode active material layer may have a porosity of 35% or less, and specific examples thereof include 35% or less, 34% or less, 33% or less, 32% or less, 31% or less, 30% or less, 29% or less, 28% or less, 27% or less, 26% or less, or 25% or less, and may be 1% or more, 5% or more, 10% or more, 15% or more, 20% or more, 21% or more, 22% or more, 23% or more, or 24% or more. The porosity of the positive electrode active material layer may be a porosity after rolling, and may be a value calculated by the following Equation 1.

[0093] [Formula 1] Porosity=(1-filling density / true density)×100

[0094] According to an embodiment of the present invention, the true density in Equation 1 may refer to a theoretical density of a composition for forming a positive electrode active material layer in a state in which there are no voids, other than the solvent, for forming a positive electrode active material layer. As a specific example, the true density may be calculated in consideration of the weight ratio of each material other than the solvent contained in the composition for forming a positive electrode active material layer and / or the true density of each material. As a more specific example, the true density may be a value calculated according to Equation 2 below.

[0095] [Formula 2] True density=1 / (Σ(P i / D i ))

[0096] In the above formula 2, P i may mean the weight ratio of each component contained in the composition for forming a positive electrode active material layer other than the solvent, and D i may mean the true density of each of the components contained in the composition for forming a positive electrode active material layer other than the solvent. As a specific example, the true density may mean the reciprocal of the sum of the value obtained by dividing the weight ratio of the positive electrode active material by the true density of the positive electrode active material, the value obtained by dividing the weight ratio of the binder by the true density of the binder, and / or the value obtained by dividing the weight ratio of the conductive material, etc. by the true density of the conductive material. The true density may be measured, for example, by a known true density measuring device.

[0097] According to an embodiment of the present invention, in Equation 1, the packing density may refer to the density of the positive electrode active material layer after a rolling process. As a specific example, the packing density may be a value calculated by sampling an arbitrary point after rolling the positive electrode active material layer formed on the positive electrode current collector, and dividing the amount of the positive electrode active material layer per unit area (loading amount) by the thickness of the positive electrode active material layer. Therefore, the porosity of the positive electrode active material layer may be controlled by the components of the positive electrode active material layer, the loading amount per area of ​​the positive electrode active material layer, and / or the thickness of the positive electrode active material layer.

[0098] According to one embodiment of the present invention, when the components of the positive electrode active material layer and the loading amount per area of ​​the positive electrode active material layer are the same, the porosity can be reduced by making the thickness of the positive electrode active material layer thinner (i.e., making the pressing gap smaller), and the porosity can be increased by making the thickness of the positive electrode active material layer thicker (i.e., making the pressing gap larger). The pressing gap can be appropriately adjusted in consideration of the desired porosity of the positive electrode active material layer.

[0099] Lithium secondary battery The present invention provides a lithium secondary battery including the positive electrode.

[0100] According to an embodiment of the present invention, the lithium secondary battery may include the positive electrode, the negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte. The lithium secondary battery may further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0101] According to an embodiment of the present invention, the negative electrode may include a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector.

[0102] According to an embodiment of the present invention, the negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of typically 3 μm to 500 μm, and may have fine irregularities formed on the surface of the current collector, as with the positive electrode current collector, to strengthen the binding force of the negative electrode active material. For example, the negative electrode current collector may be used in various forms, such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.

[0103] According to an embodiment of the present invention, the negative electrode active material layer may optionally include a binder and a conductive material in addition to the negative electrode active material.

[0104] According to an embodiment of the present invention, the negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β (0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites and Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low crystalline carbon and high crystalline carbon may be used as the carbon material. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, flake-like, spherical or fibrous natural graphite or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes. The negative electrode active material may be included in an amount of 80 wt% to 99 wt% based on the total weight of the negative electrode active material layer.

[0105] According to an embodiment of the present invention, the binder of the negative electrode active material layer is a component that helps bind between the conductive material, the active material, and the current collector, and is usually added in an amount of 0.1% by weight to 10% by weight based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene butadiene rubber, nitrile butadiene rubber, fluororubber, and various copolymers thereof.

[0106] According to an embodiment of the present invention, the conductive material of the negative electrode active material layer is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0107] According to an embodiment of the present invention, the negative electrode may be manufactured by coating a composition for forming a negative electrode active material layer, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent, on a negative electrode current collector and drying the composition. Alternatively, the negative electrode active material layer may be manufactured by casting the composition for forming a negative electrode active material layer on a separate support, peeling it off from the support, and laminating the resulting film on the negative electrode current collector.

[0108] According to an embodiment of the present invention, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used in lithium secondary batteries may be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability is preferred. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymeric material may be used to ensure heat resistance or mechanical strength, and may be selectively used in a single layer or multilayer structure.

[0109] According to an embodiment of the present invention, the electrolyte may be, but is not limited to, an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, a molten inorganic electrolyte, etc. that can be used in manufacturing a lithium secondary battery. As a specific example, the electrolyte may include an organic solvent and a lithium salt.

[0110] According to an embodiment of the present invention, the organic solvent may be any solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as polycarbonate (PC) and polycarbonate-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of a battery and a low-viscosity straight-chain carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred.

[0111] According to one embodiment of the present invention, the lithium salt can be used without any particular limitation as long as it is a compound that can provide lithium ions used in a lithium secondary battery. Specifically, the anion of the lithium salt can be F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - The lithium salt may be at least one selected from the group consisting of LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The lithium salt is preferably used in a concentration range of 0.1M to 2.0M. When the lithium salt concentration is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0112] According to an embodiment of the present invention, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethyl alcohol amine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethyl alcohol, and aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing the decrease in the capacity of the battery, improving the discharge capacity of the battery, etc. Here, the additives may be contained in an amount of 0.1% by weight to 5% by weight based on the total weight of the electrolyte.

[0113] The lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent capacity characteristics, output characteristics and life characteristics, and is therefore useful in portable devices such as mobile phones, notebook computers and digital cameras, and in the field of electric vehicles such as hybrid electric vehicles (HEVs) and electric vehicles (EVs).

[0114] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.

[0115] The lithium secondary battery according to the present invention can be used as a battery cell used as a power source for a small device, and can also be preferably used as a unit battery in a medium- to large-sized battery module including a large number of battery cells.

[0116] According to an embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.

[0117] According to an embodiment of the present invention, the battery module or battery pack may be used as a power source for one or more medium to large devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and an electric vehicle (PHEV), including a plug-in hybrid electric vehicle; or a power storage system.

[0118] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may be embodied in various different forms and should not be construed as limited to the embodiments set forth herein.

[0119] Examples and Comparative Examples Example 1 Average particle size (D 50 ) is a secondary particle with an average composition of LiNi 0.8 Mn 0.1 Co 0.1 A particulate positive active material (GL80, manufactured by LG Chem) was loaded into an ALD system (Lucida C200-PL, manufactured by NCDTech) in which the substrate temperature was maintained at 150° C. Then, the following steps (S11), (S21), and (S31) were performed as unit processes (ALD first unit process) in the order of the following formula 1-1, and the ALD first unit process was performed a total of six times to produce a positive active material coated with phosphorus (P)-doped aluminum oxide.

[0120] [Formula 1-1] (S11)-(S21)-(S31)-(S21)

[0121] (S11) Trimethylaluminum was injected as an aluminum precursor into the ALD system for 1 second. The aluminum precursor was filled in a steel container maintained at 20°C, and the aluminum precursor vaporized by reduced pressure was injected into the system without the use of a separate carrier gas. Then, purging was performed for 50 seconds using an inert gas, Ar.

[0122] (S21) Water vapor was injected as a reaction gas into the ALD system for 1 second. The reaction gas was filled in a steel container maintained at 14°C, and the reaction gas vaporized by depressurization was injected into the system without the use of a separate carrier gas. Then, purging was performed for 50 seconds using an inert gas, Ar.

[0123] (S31) Trimethyl phosphate was injected into the ALD system as a phosphorus (P)-containing precursor for 1 second. The phosphorus-containing precursor was filled in a steel container maintained at 85°C and was vaporized by reducing pressure and injected into the system without the use of a separate carrier gas. Purging was then performed for 50 seconds using an inert gas, Ar.

[0124] Example 2 A positive electrode active material coated with phosphorus (P)-doped aluminum oxide was prepared in the same manner as in Example 1, except that the unit process (ALD third unit process) of steps (S11), (S21), and (S31) in Example 1 was performed in the order of Scheme 1-3 below, and the ALD third unit process was performed a total of six times.

[0125] [Formula 1-3] (S11)-(S21)-{(S31)-(S21)}3

[0126] Example 3 A positive electrode active material coated with phosphorus (P)-doped aluminum oxide was prepared in the same manner as in Example 1, except that the unit process (ALD fourth unit process) of steps (S11), (S21), and (S31) in Example 1 was performed in the order of Scheme 1-4 below, and the ALD fourth unit process was performed twice in total.

[0127] [Formula 1-4] {(S11)-(S21)}3-(S31)-(S21)

[0128] Comparative Example 1 Average particle size (D 50 ) is a secondary particle with an average composition of LiNi 0.8 Mn 0.1 Co 0.1 A particulate positive electrode active material (GL80, manufactured by LG Chem) was dried at 130° C. for 5 hours in a vacuum oven without a separate coating process to prepare a positive electrode active material.

[0129] Comparative Example 2 A cathode active material coated with aluminum oxide was prepared in the same manner as in Example 1, except that the unit process (ALD 5th unit process) of the (S11) and (S21) processes in the following order of Scheme 3 was performed, and the ALD 5th unit process was performed a total of 6 times.

[0130] [Formula 3] (S11)-(S21)

[0131] Comparative Example 3 A positive electrode active material coated with phosphorus (P)-doped aluminum oxide was prepared in the same manner as in Example 1, except that the unit process (ALD third unit process) of steps (S11), (S21), and (S31) in Example 1 was performed in the order of Scheme 1-3 below, and the ALD third unit process was performed a total of 30 times.

[0132] [Formula 1-3] (S11)-(S21)-{(S31)-(S21)}3

[0133] Experimental Example Experimental Example 1: Confirmation of aluminum oxide coating layer components with and without phosphorus (P) doping The silicon wafer was loaded into an ALD system (NCDTech, Lucida C200-PL) in which the substrate temperature was maintained at 150° C. Then, the following (S11), (S21) and (S31) steps were performed in the order of the following formulas 1-1, 1-2, 1-3, 1-4 and 3, respectively, as unit steps (Formula 1-1: ALD 1st unit step; Formula 1-2: ALD 2nd unit step; Formula 1-3: ALD 3rd unit step; Formula 1-4: ALD 4th unit step, Formula 3: ALD 5th unit step). Here, the ALD 1st unit step to the ALD 5th unit step were performed so that the steps (S11)-(S21) were performed a total of 300 times. That is, the ALD 1st unit process to the ALD 3rd unit process and the ALD 5th unit process were performed a total of 300 times, and the ALD 4th unit process was performed a total of 100 times to form an atomic layer deposition film corresponding to an aluminum oxide coating layer doped or undoped with phosphorus (P).

[0134] [Formula 1-1] (S11)-(S21)-(S31)-(S21)

[0135] [Formula 1-2] (S11)-(S21)-{(S31)-(S21)}2

[0136] [Formula 1-3] (S11)-(S21)-{(S31)-(S21)}3

[0137] [Formula 1-4] {(S11)-(S21)}3-(S31)-(S21)

[0138] [Formula 3] (S11)-(S21)

[0139] (S11) Trimethylaluminum was injected as an aluminum precursor into the ALD system for 1 second. The aluminum precursor was filled in a steel container maintained at 20°C, and the aluminum precursor vaporized by reduced pressure was injected into the system without the use of a separate carrier gas. Then, purging was performed for 50 seconds using an inert gas, Ar.

[0140] (S21) Water vapor was injected as a reaction gas into the ALD system for 1 second. The reaction gas was filled in a steel container maintained at 14°C, and the reaction gas vaporized by reducing pressure was injected into the system without using a separate carrier gas. Then, purging was performed for 50 seconds using an inert gas, Ar.

[0141] (S31) Trimethyl phosphate was injected into the ALD system as a phosphorus (P)-containing precursor for 1 second. The phosphorus-containing precursor was filled in a steel container maintained at 85°C, and the vaporized phosphorus-containing precursor was injected into the system by reducing pressure without using a separate carrier gas. Then, purging was performed for 50 seconds using an inert gas, Ar.

[0142] Next, an ellipsometer (MK-2000, manufactured by J.A. Woolam) was used to measure the thickness of the deposited film by fitting psi and delta measurements from 380 nm to 780 nm using the Cauchy model, and the deposited film was analyzed for components by irradiating it with a monochromatic Al K-α X-ray source using X-ray photoelectron spectroscopy (XPS) (K-Alpha+, Thermo Fisher Scientific Inc.), as shown in Table 1 below. Based on the analysis results, the composition ratios of aluminum oxide doped or not doped with phosphorus (P), represented by the following Chemical Formula 1, for the positive electrode active materials coated with phosphorus (P)-doped or not doped aluminum oxide prepared in Examples 1 to 3 and Comparative Examples 1 to 3, are shown in Table 2 below.

[0143] [Table 1]

[0144] [Table 2]

[0145] As shown in Table 1, when atomic layer deposition is performed according to the ALD 1st unit process, the ALD 2nd unit process, and the ALD 3rd unit process, it is confirmed that a deposition film is formed with a deposition thickness of about 0.1 nm per unit process, and when atomic layer deposition is performed according to the ALD 4th unit process, it is confirmed that a deposition film is formed with a deposition thickness of about 0.3 nm per unit process. In addition, it is confirmed that each deposition film contains phosphorus (P) in a content of 4.2 wt% to 11.1 wt%. Meanwhile, when atomic layer deposition is performed according to the ALD 5th unit process, it is confirmed that a deposition film is formed with a deposition thickness of about 0.1 nm per unit process, and it is confirmed that the deposition film does not contain phosphorus (P).

[0146] As a result, the positive electrode active material prepared in Example 1 is expected to have a coating layer having a thickness of 0.576 nm formed on the surface of the particulate positive electrode active material by performing the ALD first unit process a total of six times, and the phosphorus (P) content in the coating layer is expected to be 8.2 wt %.

[0147] In addition, the positive electrode active material prepared in Example 2 is expected to have a coating layer having a thickness of 0.630 nm formed on the surface of the particulate positive electrode active material by performing the ALD third unit process a total of six times, and the phosphorus (P) content in the coating layer is expected to be 11.1 wt %.

[0148] In addition, the positive electrode active material prepared in Example 3 is expected to have a coating layer having a thickness of 0.612 nm formed on the surface of the particulate positive electrode active material by performing the ALD fourth unit process twice in total, and the phosphorus (P) content in the coating layer is expected to be 4.2 wt %.

[0149] In addition, the positive electrode active material prepared in Comparative Example 2 is expected to have a coating layer having a thickness of 0.714 nm formed on the surface of the particulate positive electrode active material by performing the ALD fifth unit process a total of six times, and to have no phosphorus (P) contained in the coating layer.

[0150] In addition, the positive electrode active material produced in Comparative Example 3 was subjected to the ALD third unit process a total of 30 times, so that a coating layer having a thickness of 3.150 nm was formed on the surface of the particulate positive electrode active material, and the phosphorus (P) content in the coating layer was expected to be 11.1 wt%.

[0151] Experimental Example 2: Measurement of rolling density For the positive electrode active materials produced in Examples 1 to 3 and Comparative Examples 1 to 3, the rolling densities were measured under loads of 400 kgf, 800 kgf, 1,200 kgf, 1,600 kgf, and 2,000 kgf using a powder resistivity measurement device (Powder Resistivity Measurement System, manufactured by Loresta Corp.), respectively, and the results are shown in FIG. 1. The rolling densities under a load of 2,000 kg are shown in Table 2 below.

[0152] [Table 3]

[0153] As shown in Table 3, when the coating layer formed on the surface of the particulate positive electrode active material was included, it was confirmed that the rolling density was improved in all cases compared to Comparative Example 1 which did not include a coating layer.

[0154] Experimental example 3: Charge / discharge evaluation Using each of the positive electrode active materials produced in Examples 1 to 3 and Comparative Examples 1 to 3, carbon black (DenkaBlack, manufactured by Denka Corporation) as a conductive material and PVdF (Kureha, KF1300) as a binder were added in a weight ratio of 97.5:1:1.5 (positive electrode active material:conductive material:binder) to a solvent (N-methylpyrrolidone (NMP) manufactured by Oi Chemical Industries, Ltd.) to produce a composition for forming a positive electrode active material layer.

[0155] Each of the prepared compositions for forming a positive electrode active material layer was coated on one side of an aluminum foil current collector having a thickness of 12 μm and dried at 135° C. for 3 hours to form a positive electrode active material layer. Then, the positive electrode active material layer was rolled using a roll pressing method, and a positive electrode having a porosity of 25% in the positive electrode active material layer after rolling was prepared.

[0156] A polypropylene separator (WL20C, manufactured by W-SCOPE) was interposed between each of the prepared positive electrodes and a 300 μm-thick lithium metal thin film as the negative electrode, and a coin-type half cell was prepared using an organic electrolyte of ethylene carbonate (EC) / dimethyl carbonate (DMC) / LiPF6 (Merck Battery grade, EC / DMC=1 / 1, 1M LiPF6).

[0157] The manufactured coin-type half cell was activated and then charged and discharged. Specifically, 30 cycles of charge / discharge were performed at 45° C. under the conditions of a charge cut-off voltage of 4.4 V, a discharge cut-off voltage of 2.5 V, and 0.3 C / 0.3 C, and the discharge capacity and 60-second reference discharge resistance were measured at the first and 30th cycles. The discharge capacity retention rate and discharge resistance increase rate (60 seconds) at 30 cycles were measured with respect to the initial discharge capacity and discharge resistance, and are shown in Table 4 below.

[0158] [Table 4]

[0159] As shown in Table 4, when the positive electrode active materials prepared in Examples 1 to 3 of the present invention were included, the capacity retention rate was improved and the resistance increase rate was significantly reduced compared to when the positive electrode active material of Comparative Example 1 not including a coating layer was included.

[0160] In particular, from the results of Examples 1 and 2 and Example 3, it was confirmed that when the phosphorus (P) content in the aluminum oxide contained in the coating layer was maintained at a predetermined level, as in Examples 1 and 2, the capacity retention rate was further improved and the resistance increase rate was further reduced.

[0161] On the other hand, in the case of the positive electrode active material prepared in Comparative Example 2 in which a coating layer was formed only with aluminum oxide without doping with phosphorus (P), the capacity retention rate and the resistance increase rate were improved compared to the case of the positive electrode active material prepared in Comparative Example 1 which did not include a coating layer, but the improvement was not as significant as in the case of the positive electrode active materials prepared in Examples 1 to 3.

[0162] In addition, in the case of the positive electrode active material of Comparative Example 3 in which the ALD third unit process was performed 30 times and a coating layer having a thickness of 3.150 nm was formed on the surface of the particulate positive electrode active material, it was confirmed that not only did the initial discharge capacity decrease rapidly due to the increased thickness of the coating layer, but also that the improvement in the resistance increase rate was minimal.

[0163] From these results, it was confirmed that the cathode active material of the present invention includes aluminum oxide doped with phosphorus (P) formed by atomic layer deposition and includes a thin and uniform coating layer, thereby improving the life and stability and preventing an increase in interface resistance and cell resistance. As a result, it was confirmed that the cycle characteristics of the lithium secondary battery are improved, the capacity retention rate is excellent, and the resistance increase rate due to degradation is low, thereby suppressing a decrease in output.

Claims

1. A particulate positive electrode active material and a coating layer formed on a surface of the particulate positive electrode active material, The coating layer includes aluminum oxide doped with phosphorus (P), The coating layer has a thickness of 0.1 nm or more and 2.0 nm or less.

2. The cathode active material according to claim 1 , wherein the coating layer has a thickness of 0.2 nm to 1.0 nm.

3. The phosphorus (P)-doped aluminum oxide is represented by the following Chemical Formula 1: [Chemical formula 1] AlO m P n 2. The positive electrode active material according to claim 1, wherein in Chemical Formula 1, m is 1.7 or more and 2.6 or less, and n is 0.01 or more and 0.4 or less.

4. The positive electrode active material according to claim 3 , wherein in Chemical Formula 1, m is 2.0 or more and 2.5 or less, and n is 0.15 or more and 0.30 or less.

5. The positive electrode active material of claim 1 , wherein the coating layer has a phosphorus (P) content of 1 to 15 wt %.

6. The positive electrode active material of claim 1 , wherein the coating layer has a phosphorus (P) content of 8% by weight to 12% by weight.

7. The particulate positive electrode active material includes a lithium transition metal composite oxide represented by the following chemical formula 2: [Chemical formula 2] Li a Ni b Co c Mn d M 1 e O 2 In the above Chemical Formula 2, M 1 is one or more selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, Sn, Y, Zn, F, P, and S, and 0.9≦a≦1.2, 0<b<1, 0<c<1, 0<d<1, 0≦e<0.2, and b+c+d+e=1.

8. A step (S1) of loading a particulate positive electrode active material into a reaction chamber for performing atomic layer deposition; and (S2) forming a coating layer on a surface of a positive electrode active material by performing a unit process including the following steps (S10) to (S30) multiple times, The thickness of the coating layer formed in step (S2) is 0.1 nm or more and 2.0 nm or less; (S10) injecting a vapor phase aluminum precursor into a reaction chamber and injecting a purge gas; (S20) injecting a gas phase reaction gas into the reaction chamber and injecting a purge gas; (S30) injecting a gas-phase phosphorus (P)-containing precursor into a reaction chamber and injecting a purge gas.

9. The unit process including steps (S10) to (S30) of the step (S2) is represented by the following formula 1 or formula 2: [Formula 1] [{(S10)-(S20)} x -{(S30)-(S20)} y ] z [Formula 2] [{(S30)-(S20)} y -{(S10)-(S20)} x ] z In the above formulas 1 and 2, "-" indicates the execution order of the unit process, x is the number of times {(S10)-(S20)} is repeated, and is an integer selected from 1 to 5; y is the number of times {(S30)-(S20)} is repeated, and is an integer selected from 1 to 5; z is [{(S10)-(S20)} x -{(S30)-(S20)} y ] or [{(S30)-(S20)} y -{(S10)-(S20)} x 9. The method for producing a positive electrode active material according to claim 8, wherein the number of times that the step of repeating the steps of (a) to (c) is repeated is an integer selected from 1 to 20.

10. 9. The method for producing a positive electrode active material according to claim 8, wherein the aluminum precursor is at least one selected from the group consisting of trimethylaluminum, triethylaluminum, aluminum ethoxide, and tris(diethylamido)aluminum.

11. The reaction gas is water vapor in gas phase (H 2 O), ozone (O 3 9. The method for producing a positive electrode active material according to claim 8, wherein the oxygen plasma is at least one selected from the group consisting of oxygen plasma and oxygen plasma.

12. The method for producing a positive electrode active material according to claim 8 , wherein the phosphorus (P)-containing precursor is at least one selected from the group consisting of trimethyl phosphate and triethyl phosphate.

13. A positive electrode comprising the positive electrode active material according to claim 1 .

14. A lithium secondary battery comprising the positive electrode according to claim 13.

Citation Information

Patent Citations

  • Positive active material and preparation method and application thereof

    CN112531147A

  • Positive electrode active material and method for producing the same, positive electrode, battery, battery pack, electronic apparatus, electric vehicle, electricity storage device and power system

    JP2014116111A

  • Protective coatings for conversion material cathodes

    US20140234715A1

  • Nano-engineered coatings for anode active materials, cathode active materials, and solid-state electrolytes and methods of making batteries containing nano-engineered coatings

    US20160351973A1

  • High capacity and stable cathode materials

    US20170338471A1