METHOD FOR PRE-LITHIATING ELECTRODE, PRE-LITHIATING ELECTRODE FOR LITHIUM SECONDARY BATTERY, AND APPARATUS FOR PRE-LITHIATING ELECTRODE

The pre-electrode lithiation method addresses the challenges of uneven lithiation and safety risks in silicon-based electrodes by using a dry-on-dry process to form an intermediate layer and transfer lithium metal sequentially, resulting in a pre-lithiated electrode with improved stability and cycle performance.

JP2024540562AActive Publication Date: 2024-10-31LG ENERGY SOLUTION LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024529672
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-05-06
Filing Date
2023-05-08
Publication Date
2024-10-31
Estimated Expiration
2043-05-08

AI Technical Summary

Technical Problem

Existing pre-lithiation methods for silicon-based electrodes in lithium secondary batteries face challenges such as high production costs, safety risks, uneven lithiation, and irreversible capacity issues, particularly due to direct contact between lithium metal and the electrode active material, leading to mechanical instability and reduced cycle performance.

Method used

A pre-electrode lithiation method involving a dry-on-dry process to form an intermediate layer on both sides of the electrode active material layer, followed by sequential lamination and transfer of a lithium metal layer without direct contact, ensuring uniform lithiation and minimizing side reactions.

Benefits of technology

The method produces a pre-lithiated electrode with improved mechanical stability, reduced irreversible capacity, and enhanced cycle performance by adjusting the lithiation rate and preventing lithium loss, thus enhancing battery efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540562000001_ABST
    Figure 2024540562000001_ABST
Patent Text Reader

Abstract

The present application relates to a method for prelithiation of an electrode, a prelithiated electrode for a lithium secondary battery, and an electrode prelithiation apparatus.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to a method for prelithiation of an electrode, a prelithiated electrode for a lithium secondary battery, and an electrode prelithiation apparatus.

[0002] This application claims the benefit of the filing date of Korean Patent Application No. 10-2022-0055970, filed with the Korean Intellectual Property Office on May 6, 2022, the entire contents of which are incorporated herein by reference. [Background technology]

[0003] The rapid increase in the use of fossil fuels has led to an increased demand for alternative and clean energy, and one of the most actively researched fields in this area is power generation and storage using electrochemical reactions.

[0004] At present, a representative example of an electrochemical element that utilizes such electrochemical energy is a secondary battery, and the range of its use is tending to expand more and more.

[0005] As technological development and demand for mobile devices increases, the demand for secondary batteries as energy sources is rapidly increasing. Among such secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used. In addition, research into a method for manufacturing a high-density electrode with a higher energy density per unit volume as an electrode for such high-capacity lithium secondary batteries is being actively conducted.

[0006] In general, a secondary battery is composed of a positive electrode, an electrode, an electrolyte, and a separator. The electrode includes an electrode active material that inserts and removes lithium ions from the positive electrode, and silicon-based particles having a large discharge capacity can be used as the electrode active material.

[0007] Generally, carbon materials such as graphite are used for the electrodes of lithium secondary batteries, but the theoretical capacity density of carbon is 372 mAh / g (833 mAh / cm3 ). Therefore, in order to improve the energy density of the electrode, silicon (Si), tin (Sn), and their oxides and alloys, which are alloyed with lithium, are being considered as electrode materials. Among them, silicon-based materials have attracted attention due to their low cost and high capacity (4200mAh / g).

[0008] However, silicon has a problem in that its mechanical stability is reduced due to volume change (shrinkage or expansion) during the process of lithium ion insertion / extraction, resulting in impaired cycle characteristics. Therefore, there is a need to develop a material that has structural stability and is therefore stable when used as an active material for electrochemical devices, and can ensure cycle characteristics.

[0009] In addition, when silicon-based electrode active materials are used, the problem of large initial irreversible capacity occurs. In the charge / discharge reaction of a lithium secondary battery, lithium released from the positive electrode is inserted into the electrode during charging, and is removed from the electrode and returned to the positive electrode during discharging. However, in the case of silicon-based electrode active materials, the volume change and surface side reaction are intense, and most of the lithium inserted into the electrode during initial charging does not return to the positive electrode, resulting in a problem of large initial irreversible capacity. When the initial irreversible capacity is large, the problem of a rapid decrease in battery capacity and cycles occurs.

[0010] To solve the above problems, a method of prelithiating a silicon electrode containing a silicon-based electrode active material is known. Known prelithiating methods include a method of manufacturing an electrode after lithiating the electrode by a physical / chemical method such as electrolytic plating, lithium metal transfer, or lithium metal deposition, and a method of electrochemically prelithiating the electrode.

[0011] Conventional physicochemical methods have the risk of fire and explosion due to the environmental factors that must be caused by high temperatures, and conventional electrochemical methods have the problem that the initial irreversible capacity cannot be uniformly controlled, which increases production costs.

[0012] In particular, in the lithium metal transfer process, it is difficult to safely and easily transfer lithium metal, and even if it is transferred, highly reactive lithium metal immediately starts to react through direct contact with the electrode active material, causing problems such as particle cracking on the surface of the electrode active material layer.

[0013] Therefore, there is a need for research into processes and apparatus for prelithiating electrodes that are safer and more efficient and that can uniformly prelithiate lithium within the electrode active material layer. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] JP 2009-080971 A Summary of the Invention [Problem to be solved by the invention]

[0015] The present application relates to a method for prelithiation of an electrode, a prelithiated electrode for a lithium secondary battery, and an electrode prelithiation apparatus. [Means for solving the problem]

[0016] One embodiment of the present specification provides a pre-lithiation method for an electrode, comprising the steps of: preparing an electrode having an electrode active material layer coated on at least one surface of an electrode current collector layer; laminating an intermediate layer laminate having a first base material layer, a first release layer, and an intermediate layer sequentially laminated on the electrode active material layer so that the intermediate layer contacts the electrode active material layer, thereby transferring the intermediate layer; removing the first base material layer and the first release layer after the intermediate layer is transferred; laminating a lithium metal layer laminate having a second base material layer, a second release layer, and a lithium metal layer sequentially laminated on the intermediate layer of the electrode active material layer to which the intermediate layer has been transferred so that the lithium metal layer contacts the intermediate layer, thereby transferring the lithium metal layer; and removing the second base material layer after the transfer of the lithium metal layer laminate.

[0017] In yet another embodiment, there is provided an electrode for a lithium secondary battery that is prelithiated according to the electrode prelithiation method of the present application.

[0018] Finally, in one embodiment of the present application, there is provided an electrode pre-lithiation device including: an electrode extraction unit, from which an electrode having an electrode active material layer coated on both sides of an electrode collector layer is extracted; an intermediate layer transfer unit, which laminates an intermediate layer laminate in which a first base material layer, a first release layer, and an intermediate layer are sequentially laminated on the electrode active material layers provided on both sides of the electrode; a lithium metal layer transfer unit, which laminates a lithium metal layer laminate in which a second base material layer, a second release layer, and a lithium metal layer are sequentially laminated on the intermediate layer of the electrode active material layer to which the intermediate layer has been transferred; and an electrode recovery unit. Effect of the Invention

[0019] According to one embodiment of the present invention, a method for pre-lithiation of an electrode is to prepare a pre-lithiation electrode by performing two transfer processes. Specifically, the method includes a process of transferring an intermediate layer onto an upper portion of an electrode active material layer in order to minimize non-uniform pre-lithiation during preparation of the pre-lithiation electrode and to suppress lithium loss due to side reactions during the pre-lithiation of the electrode, so that the pre-lithiation rate can be controlled since lithium metal does not directly contact the electrode active material layer.

[0020] In addition, the intermediate layer according to the present application is formed by a dry-on-dry process in which an intermediate layer laminate having an intermediate layer formed thereon is transferred onto an electrode active material layer, rather than a wet-on-dry process in which an intermediate layer composition is coated on the electrode active material layer. As a result, the present invention has solved the problem of the wet-on-dry process in which the intermediate layer composition penetrates into the pores of the electrode active material layer, filling or blocking the electrode pores, resulting in an increase in electrode resistance, which is a main feature of the present invention.

[0021] In addition, by forming the intermediate layer by the dry-on-dry process as described above, it can be transferred simultaneously onto the electrode active material layers provided on both sides of the electrode current collector layer. When forming the intermediate layer by the wet-on-dry process, it is difficult to perform coating on both sides simultaneously, which causes the electrode to warp or twist. However, the intermediate layer formation according to the present application has the characteristic of being able to solve the above problems and improve the economic efficiency of the process itself by forming the intermediate layer on both sides simultaneously by the dry-on-dry process.

[0022] That is, the electrode pre-lithiation method according to the present invention is characterized in that an intermediate layer for controlling the pre-lithiation rate is simultaneously formed on both sides of an electrode active material layer through a dry-on-dry process, thereby preventing the electrode from warping or twisting, and also preventing the intermediate layer composition from penetrating into the pores of the electrode active material layer, thereby producing a better pre-lithiation electrode.

[0023] The pre-lithiation device for electrodes according to the present application is characterized by including two R2R steps in order to apply the two transfer steps as described above. Specifically, the device has an electrode extraction section, an intermediate layer transfer section, a lithium metal layer transfer section, and an electrode recovery section, and two R2R steps are carried out in each of the intermediate layer transfer section and the lithium metal transfer section. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 illustrates a method for pre-lithiation of an electrode according to one embodiment of the present application. [Diagram 2] FIG. 1 is a diagram of an electrode pre-lithiation device according to one embodiment of the present application. [Diagram 3] 3A and 3B are diagrams showing the electrode shape according to Example 1. In particular, Fig. 3(a) is a diagram showing an electrode having an intermediate layer A according to Example 1 transferred thereon, and Fig. 3(b) is a diagram showing an electrode having a lithium layer transferred thereon to the electrode according to Fig. 3(a). [Figure 4]4A and 4B are diagrams showing the electrode shape according to Example 2. In particular, Fig. 4(a) is a diagram showing an electrode onto which an intermediate layer B according to Example 2 has been transferred, and Fig. 4(b) is a diagram showing an electrode onto which a lithium layer has been transferred according to Fig. 4(a). [Diagram 5] FIG. 2 shows the cycle capacity of half-cells prepared by the pre-lithiation method according to the present invention. [Figure 6] FIG. 2 is a graph showing the cycle capacity retention of a half-cell prepared by the pre-lithiation method according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Before describing the present invention, some terms will first be defined.

[0026] In this specification, when a part is said to "comprise" a certain component, this means that it may further include other components, rather than excluding other components, unless specifically stated to the contrary.

[0027] In this specification, "p to q" means a range of "not less than p and not more than q".

[0028] In this specification, the "specific surface area" is measured by the BET method, and specifically, is calculated from the amount of nitrogen gas adsorption at liquid nitrogen temperature (77K) using a BELSORP-mini II manufactured by BEL Japan Co., Ltd. That is, in this application, the BET specific surface area may mean the specific surface area measured by the above-mentioned measurement method.

[0029] In this specification, "Dn" means the average particle size, which means the particle size at the n% point of the cumulative particle number distribution by particle size. That is, D50 is the particle size at the 50% point of the cumulative particle number distribution by particle size, D90 is the particle size at the 90% point of the cumulative particle number distribution by particle size, and D10 is the particle size at the 10% point of the cumulative particle number distribution by particle size. Meanwhile, the average particle size can be measured using the laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and the difference in the diffraction pattern due to the particle size when the particles pass through a laser beam is measured to calculate the particle size distribution.

[0030] In this specification, when a polymer contains a certain monomer as a monomer unit, it means that the monomer is involved in a polymerization reaction and is contained as a repeating unit in the polymer. In this specification, when a polymer contains a monomer, this is interpreted as the same as when a polymer contains a monomer as a monomer unit.

[0031] In this specification, the term "polymer" is understood to be used in a broad sense including copolymers, unless otherwise specified as a "homopolymer."

[0032] In this specification, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are polystyrene-equivalent molecular weights measured by gel permeation chromatography (GPC) using monodisperse polystyrene polymers (standard samples) of various polymerization degrees that are commercially available for molecular weight measurement as standard substances. In this specification, the molecular weight means the weight average molecular weight unless otherwise specified.

[0033] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings in order to enable those skilled in the art to easily carry out the present invention. However, the present invention may be embodied in many different forms and is not limited to the following description.

[0034] One embodiment of the present specification provides a method for pre-lithiating an electrode, the method including the steps of: preparing an electrode in which both sides of an electrode current collector layer are coated with electrode active material layers; transferring an intermediate layer by laminating an intermediate layer laminate in which a first base material layer, a first release layer, and an intermediate layer are sequentially laminated on the electrode active material layers provided on both sides of the electrode such that the intermediate layer contacts the electrode active material layer; removing the first base material layer and the first release layer after the intermediate layer transfer; transferring a lithium metal layer by laminating a lithium metal layer laminate in which a second base material layer, a second release layer, and a lithium metal layer are sequentially laminated on the intermediate layer of the active material layer to which the intermediate layer has been transferred such that the lithium metal layer contacts the intermediate layer; and removing the second base material layer after the transfer of the lithium metal layer laminate; and pre-lithiating the electrode active material layer.

[0035] Fig. 1 is a diagram showing an electrode pre-lithiation method according to one embodiment of the present application. Fig. 1 shows that an electrode active material layer 20 is formed on one side of an electrode current collector layer 10, but the electrode active material layer 20 is simply shown formed on both sides of the electrode current collector layer 10. That is, the electrode active material layer 20 is applied to both sides of the electrode current collector layer 10, and the other pre-lithiation methods may be the same.

[0036] According to one embodiment of the present invention, a method for pre-lithiating an electrode comprises the steps of: preparing a pre-lithiated electrode by performing two transfer processes; specifically, the method includes a process of transferring an intermediate layer onto an upper portion of an electrode active material layer in order to minimize non-uniform pre-lithiating behavior during preparation of the pre-lithiated electrode and to suppress lithium loss due to side reactions during the pre-lithiating process of the electrode; and since lithium metal does not directly contact the electrode active material layer, the pre-lithiating rate can be controlled.

[0037] Therefore, in the present invention, when applying prelithiation of an electrode to maximize improvement in battery performance, a main feature of the present invention is that the intermediate layer is formed in a dry-on-dry manner in order to minimize problems during prelithiation, i.e., non-uniform prelithiation and lithium loss during the prelithiation process.

[0038] The specific details of the method for pre-lithiation of an electrode according to the present invention will be described below.

[0039] In one embodiment of the present application, the electrode pre-lithiation method includes the step of providing an electrode having an electrode current collector layer coated on at least one surface thereof with an electrode active material layer.

[0040] Specifically, although not shown in FIG. 1, an electrode can be prepared by coating at least one surface of an electrode current collector layer with an electrode slurry containing an electrode composition described below.

[0041] In one embodiment of the present application, the electrode slurry may include an electrode active material layer composition; and a slurry solvent.

[0042] In one embodiment of the present application, the solid content of the electrode slurry may be 5% or more and 80% or less.

[0043] In yet another embodiment, the solid content of the electrode slurry may be in the range of 5% to 80%, preferably 10% to 75%, and more preferably 20% to 70%.

[0044] The solid content of the electrode slurry may refer to the content of the electrode active material layer composition contained in the electrode slurry, and may refer to the content of the electrode active material composition based on 100 parts by weight of the electrode slurry.

[0045] When the solid content of the electrode slurry satisfies the above range, the viscosity is appropriate during the formation of the electrode active material layer, and the particle aggregation phenomenon of the electrode active material layer composition is minimized, thereby enabling the electrode active material layer to be efficiently formed.

[0046] In one embodiment of the present application, the slurry solvent is not limited as long as it can dissolve the electrode active material layer composition, and specifically, NMP or distilled water can be used.

[0047] An electrode according to one embodiment of the present application can be formed by coating and drying the electrode slurry on an electrode current collector layer.

[0048] The drying step may allow the slurry solvent in the electrode slurry to dry.

[0049] In one embodiment of the present application, the slurry solvent may be dried through the drying step, so that an electrode active material layer may be coated on at least one surface of the electrode current collector layer.

[0050] In one embodiment of the present application, the electrode current collector layer generally has a thickness of 1 μm to 100 μm. Such an electrode current collector layer is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the bonding force of the electrode active material can be strengthened by forming fine irregularities on the surface, and it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0051] In one embodiment of the present application, the electrode current collector layer may have a thickness of 1 μm or more and 100 μm or less, and the electrode active material layer may have a thickness of 20 μm or more and 500 μm or less.

[0052] However, the thickness can be varied depending on the type and application of the electrode used, and is not limited thereto.

[0053] In one embodiment of the present application, the electrode active material layer may include a negative electrode active material; an electrode conductive material; and an electrode binder.

[0054] The statement that the electrode active material layer contains a negative electrode active material, an electrode conductive material, and an electrode binder may mean that it includes an electrode active material layer composition containing a silicon-based active material, an electrode conductive material, and an electrode binder.

[0055] In one embodiment of the present application, the electrode active material layer contains a silicon-based active material, an electrode conductive material, and an electrode binder, and the silicon-based active material is SiO x (x = 0), SiO x (0 < x < 2), Si / C, metal impurities, and at least one selected from the group consisting of Si alloys, and provides a method for pre-lithiation of an electrode.

[0056] In one embodiment of the present application, the silicon-based active material may include one or more selected from the group consisting of Si particles (SiO x (x = 0)), SiO x (0 < x < 2), Si / C, metal impurities, and Si alloys.

[0057] In one embodiment of the present application, the silicon-based active material includes at least one selected from the group consisting of SiO x (x = 0) and SiO x (0 < x < 2), and based on 100 parts by weight of the silicon-based active material, the SiO x (x = 0) may be included in an amount of 20 parts by weight or more.

[0058] In one embodiment of the present application, the silicon-based active material may contain metal impurities, which are impurities that may be generated during the purification process of the silicon-based active material, and the content thereof may be included in an amount of 1 part by weight or less based on 100 parts by weight of the silicon-based active material.

[0059] In one embodiment of the present application, particularly, pure silicon (Si) can be used as the silicon-based active material. Using pure silicon (Si) as the silicon-based active material means that when based on a total of 100 parts by weight of the silicon-based active material as described above, pure Si particles (SiO x(x=0)) may be included in the range.

[0060] On the other hand, the average particle size (D50) of the active material of the present invention may be 100 nm to 20 μm, specifically 500 nm to 15 μm, and more specifically 1 μm to 10 μm. When the average particle size is within the above range, the specific surface area of ​​the particles is within an appropriate range, and the viscosity of the electrode slurry is formed within an appropriate range. This allows smooth dispersion of the particles constituting the electrode slurry. In addition, when the size of the active material is equal to or greater than the lower limit of the above range, the contact area between the active material particles and the conductive material is excellent due to the complex of the conductive material and the binder in the electrode slurry, and the conductive network is more likely to be maintained, thereby increasing the capacity retention rate. On the other hand, when the average particle size satisfies the above range, excessively large active material particles are excluded, and the surface of the electrode is formed smoothly, thereby preventing the non-uniformity of the current density during charging and discharging.

[0061] In one embodiment of the present application, the active material generally has a characteristic BET specific surface area. The BET specific surface area of ​​the active material is preferably less than 0.01 m 2 / g~150.0m 2 / g, more preferably 0.1m 2 / g~100.0m 2 / g, particularly preferably 0.2m 2 / g~80.0m 2 / g, most preferably 0.2m 2 / g~18.0m 2 / g. The BET specific surface area is determined in accordance with DIN 66131 (using nitrogen).

[0062] In one embodiment of the present application, the active material may be 60 parts by weight or more based on 100 parts by weight of the electrode active material layer composition.

[0063] In another embodiment, the active material may be contained in an amount of 60 parts by weight or more, preferably 65 parts by weight or more, and more preferably 70 parts by weight or more, based on 100 parts by weight of the electrode active material layer composition, and may be contained in an amount of 95 parts by weight or less, preferably 90 parts by weight or less, and more preferably 80 parts by weight or less.

[0064] The electrode active material layer composition according to the present application uses a conductive material and a binder capable of suppressing the volume expansion rate during charging and discharging in the above ranges, even if a silicon-based active material having a significantly high capacity is used in the above ranges, and thus has the characteristic of excellent output characteristics during charging and discharging without deteriorating the performance of the electrode.

[0065] In one embodiment of the present application, the active material may have a non-spherical morphology, and the sphericity is, for example, 0.9 or less, for example, 0.7 to 0.9, for example, 0.8 to 0.9, for example, 0.85 to 0.9.

[0066] In this application, the circularity is determined by the following formula 1, where A is the area and P is the perimeter.

[0067] [Formula 1] 4πA / P 2

[0068] In the past, it was common to use only graphite-based compounds as negative electrode active materials, but in recent years, as the demand for high-capacity batteries has increased, attempts to mix silicon-based compounds to increase capacity have been increasing. However, silicon-based compounds have a limitation in that their volume expands rapidly during charging and discharging, damaging the conductive path formed in the electrode active material layer and rather reducing the performance of the battery.

[0069] Thus, in one embodiment of the present application, the electrode conductive material may include at least one selected from the group consisting of a dot-like conductive material, a linear conductive material, and a sheet-like conductive material.

[0070] In one embodiment of the present application, the dot-shaped conductive material can be used to improve the conductivity of the electrode, and is preferably conductive without inducing chemical changes. Specifically, the conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, conductive fiber, fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and may preferably include carbon black in that it realizes high conductivity and has excellent dispersibility.

[0071] In one embodiment of the present application, the dot-shaped conductive material has a BET specific surface area of ​​40 m 2 / g or more 70m 2 / g or less, preferably 45m 2 / g or more 65m 2 / g or less, more preferably 50m 2 / g or more 60m 2 / g or less.

[0072] In one embodiment of the present application, the particle diameter of the dotted conductive material may be 10 nm to 100 nm, preferably 20 nm to 90 nm, and more preferably 20 nm to 60 nm.

[0073] In one embodiment of the present application, the conductive material may include a sheet-shaped conductive material.

[0074] The planar conductive material can improve conductivity by increasing surface contact between silicon particles in the electrode, and at the same time, can suppress the disconnection of the conductive path due to volume expansion, and can be expressed as a plate-shaped conductive material or a bulk-type conductive material.

[0075] In one embodiment of the present application, the sheet conductive material may include at least one selected from the group consisting of platelet graphite, graphene, graphene oxide, and graphite flakes, and may be preferably platelet graphite.

[0076] In one embodiment of the present application, the average particle size (D50) of the sheet conductive material may be 2 μm to 7 μm, specifically 3 μm to 6 μm, and more specifically 4 μm to 5 μm. If the range is satisfied, the sufficient particle size makes it easy to disperse without causing an excessive increase in the viscosity of the electrode slurry. Therefore, when dispersing using the same equipment and time, the dispersion effect is excellent.

[0077] In one embodiment of the present application, the sheet conductive material provides an electrode composition having a D10 of 0.5 μm or more and 1.5 μm or less, a D50 of 2.5 μm or more and 3.5 μm or less, and a D90 of 7.0 μm or more and 15.0 μm or less.

[0078] In one embodiment of the present application, the sheet conductive material may be a sheet conductive material having a high BET specific surface area; or a sheet conductive material having a low specific surface area.

[0079] In one embodiment of the present application, the sheet conductive material may be a high-specific surface area sheet conductive material or a low-specific surface area sheet conductive material without any restrictions. However, the sheet conductive material in the present application may be affected to some extent by dispersion in terms of electrode performance, and it may be particularly preferable to use a low-specific surface area sheet conductive material that does not cause dispersion problems.

[0080] In one embodiment of the present application, the sheet conductive material has a BET specific surface area of ​​1 m 2 / g or more.

[0081] In another embodiment, the sheet conductive material has a BET specific surface area of ​​1 m 2 / g or more 500m 2 / g or less, preferably 5m 2 / g or more 300m 2 / g or less, more preferably 5m 2 / g or more 250m 2 / g or less.

[0082] In another embodiment, the sheet conductive material is a high specific surface area sheet conductive material having a BET specific surface area of ​​50 m 2 / g or more 500m 2 / g or less, preferably 80m 2 / g or more 300m 2 / g or less, more preferably 100m 2 / g or more 300m 2 / g or less.

[0083] In another embodiment, the sheet conductive material is a sheet conductive material having a low specific surface area and a BET specific surface area of ​​1 m 2 / g or more 40m 2 / g or less, preferably 5m 2 / g or more 30m 2 / g or less, more preferably 5m 2 / g or more 25m 2 / g or less.

[0084] Other conductive materials may include linear conductive materials such as carbon nanotubes. The carbon nanotubes may be bundled carbon nanotubes. The bundled carbon nanotubes may include a plurality of carbon nanotube units. Specifically, unless otherwise specified, the term "bundle type" refers to a secondary shape in the form of a bundle or rope in which a plurality of carbon nanotube units are arranged side by side with the longitudinal axes of the carbon nanotube units substantially aligned in the same direction or are entangled. The carbon nanotube units have a graphite sheet having a cylindrical shape with a nano-sized diameter and an sp2 bond structure. In this case, the graphite sheet may exhibit conductive or semiconductive properties depending on the angle and structure at which it is wound. The bundled carbon nanotubes may be uniformly dispersed during electrode manufacture compared to entangled carbon nanotubes, and may smoothly form a conductive network within the electrode, thereby improving the conductivity of the electrode.

[0085] In one embodiment of the present application, the electrode conductive material may be 10 parts by weight or more and 40 parts by weight or less based on 100 parts by weight of the electrode active material layer composition.

[0086] In another embodiment, the electrode conductive material may be contained in an amount of 10 parts by weight or more and 40 parts by weight or less, preferably 10 parts by weight or more and 30 parts by weight or less, and more preferably 10 parts by weight or more and 20 parts by weight or less, based on 100 parts by weight of the electrode active material layer composition.

[0087] In one embodiment of the present application, the electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and substances in which hydrogen is substituted with Li, Na, Ca, or the like, or may include various copolymers thereof.

[0088] The electrode binder according to one embodiment of the present application plays a role in suppressing the active material and conductive material to prevent the electrode structure from twisting and deforming during the volume expansion and relaxation of the silicon-based active material, and as long as it fulfills this role, all common binders can be used, specifically, water-based binders can be used, and more specifically, PAM-based binders can be used. A thickener may be included together with the binder, and specifically, CMC can be used as the thickener.

[0089] In one embodiment of the present application, the pre-lithiation method for an electrode includes the steps of: laminating an intermediate layer of an intermediate layer laminate in which a first base material layer, a first release layer, and an intermediate layer are sequentially laminated on an electrode active material layer provided on at least one surface of the electrode, so that the intermediate layer of the intermediate layer laminate is in contact with the electrode active material layer, thereby transferring the intermediate layer; and removing the first base material layer and the first release layer after the intermediate layer transfer.

[0090] 1, an intermediate layer laminate 200 can be seen in which a first base material layer 40, a first release layer 30, and an intermediate layer 35 are sequentially laminated on an electrode active material layer 20. At this time, it can be seen that a lamination process is carried out so that the intermediate layer 35 and the electrode active material layer 20 are in contact with each other. After the intermediate layer lamination, it can be seen that the first base material layer 40 and the first release layer 30 are removed, and thus the intermediate layer 35 is formed on the upper part of the electrode active material layer 20.

[0091] In one embodiment of the present application, the intermediate layer laminate may include a structure in which a first base material layer, a first release layer, and an intermediate layer are laminated in this order.

[0092] Specifically, in one embodiment of the present application, the first base layer may be at least one selected from the group consisting of polyethylene terephthalate (PET), polyimide (PI), poly(methylmethacrylate) (PMMA), polypropylene, polyethylene, and polycarbonate.

[0093] In one embodiment of the present application, the thickness of the first base layer may be in the range of 1 μm or more and 300 μm or less, 5 μm or more and 200 μm or less, or 10 μm or more and 100 μm or less.

[0094] In one embodiment of the present application, in order to improve the peelability of the intermediate layer and ensure transferability to the upper part of the electrode active material layer, the intermediate layer laminate may further include a first release layer on the surface where the first substrate layer and the intermediate layer are in contact.

[0095] That is, the first base layer may have a first release layer formed on at least one surface thereof, or may have a first release layer formed on both surfaces thereof. The first release layer can prevent a reverse peeling problem in which the intermediate layer is transferred onto the first base layer during a winding process for transferring the deposited intermediate layer onto the electrode active material layer, and can easily separate the first base layer after the intermediate layer is transferred onto the electrode active material layer.

[0096] The first release layer may contain at least one selected from the group consisting of silicon-modified polyester in which a silicon chain is graft-bonded to a polyester main chain, Si, melamine, and fluorine.

[0097] In one embodiment of the present application, the first release layer may be formed by a coating method, for example, the coating method may be a method selected from the group consisting of dip coating, spray coating, spin coating, die coating, gravure coating, micro-gravure coating, comma coating, and roll coating, but is not limited thereto, and various coating methods available in the art for forming a coating layer may be used.

[0098] In one embodiment of the present application, there is provided a method for pre-lithiation of an electrode, wherein the intermediate layer comprises an intermediate layer composition, the intermediate layer composition comprising at least one selected from the group consisting of a polymer; an inorganic material; an active material; and a conductive material.

[0099] In one embodiment of the present application, the polymer may be a non-crystalline thermoplastic polymer, such as poly(methylmethacrylate) (PMMA), polystyrene (PS), polyvinyl chloride (PVC), polycarbonate (PC), ABS (acrylonitrile butadiene styrene) resin, or preferably poly(methyl methacrylate) (PMMA), which is an acrylic polymer.

[0100] When the polymer according to an embodiment of the present application is used as an intermediate layer composition, it can provide adhesion and improve lithium transfer performance. In addition, when the intermediate layer does not contain a conductive material and is composed only of a polymer, the intermediate layer acts as a barrier layer between the lithium and the electrode, suppressing pre-lithiation of the electrode, and is characterized in that the intermediate layer dissolves in the electrolyte after electrolyte injection during battery manufacture, causing the electrode to come into contact with lithium, resulting in pre-lithiation. Therefore, when the intermediate layer is composed only of a polymer, the polymer has a characteristic of dissolving in the electrolyte, and the induction of side reactions during battery operation is also minimized.

[0101] According to one embodiment of the present application, the polymer may be included in an amount of 80 parts by weight to 100 parts by weight based on 100 parts by weight of the total intermediate layer composition.

[0102] When the polymer is contained in an amount of 100 parts by weight based on 100 parts by weight of the total intermediate layer composition, it has the characteristic of acting as a barrier layer against a prelithiation reaction in a dry state. When a conductive material, etc. is contained, prelithiation of an electrode is possible through the intermediate layer in a dry state, and the prelithiation rate increases as the content of the conductive material, etc. increases.

[0103] When inorganic materials are used in the intermediate layer composition according to one embodiment of the present application, the inorganic materials may be silica (SiO2), alumina (Al2O3), tungsten oxide (WO3), vanadium oxide (V2O5), and the like.

[0104] When an active material is used in the intermediate layer composition according to one embodiment of the present application, the active material may be a lithium metal oxide such as LiMO2 (M: containing at least one of Ni, Mn, and Co). Examples of the active material include graphite, soft carbon, and hard carbon.

[0105] In one embodiment of the present application, the description of the electrode active material and the electrode conductive material described above can be applied to the description of the active material and the conductive material.

[0106] When a conductive material is used in the intermediate layer composition according to one embodiment of the present application, the conductive material may be a dot-like conductive material or a linear conductive material, or both dot-like conductive material and linear conductive material may be used.

[0107] In one embodiment of the present application, the conductive material may preferably include at least one selected from the group consisting of carbon black, single-walled carbon nanotubes (SWCNTs) and multi-walled carbon nanotubes (MWCNTs), but is not limited thereto.

[0108] In one embodiment of the present application, the conductive material may preferably include any one selected from the group consisting of carbon black, single-walled carbon nanotubes (SWCNTs) and multi-walled carbon nanotubes (MWCNTs) as a first conductive material, and may include the other one as a second conductive material, but is not limited thereto.

[0109] In one embodiment of the present application, the intermediate layer composition may contain the polymer or the first conductive material:second conductive material in a weight ratio of 100:0 to 60:40, preferably 100:0 to 80:20.

[0110] In one embodiment of the present application, when the conductive material exceeds 40 parts by weight based on 100 parts by weight of the total intermediate layer composition, there is a drawback in that the difficulty and cost of producing the intermediate layer laminate increases.

[0111] The intermediate layer having the above composition is formed on the upper part of the electrode active material layer, and the intermediate layer can act as a buffer layer that can prevent rapid pre-lithiation by preventing lithium metal from directly contacting the upper part of the electrode active material layer. That is, the intermediate layer according to the present application can prevent direct contact between the lithium metal and the electrode active material layer, control the pre-lithiation rate, allow pre-lithiation to proceed uniformly in the electrode active material layer, and suppress side reactions associated with rapid pre-lithiation to reduce lithium loss.

[0112] In one embodiment of the present application, there is provided a method for pre-lithiating an electrode, wherein the thickness of the intermediate layer is 200 μm or less.

[0113] In one embodiment of the present application, the thickness of the intermediate layer can satisfy the range of 100 μm or less, 75 μm or less, preferably 50 μm or less, and may satisfy the range of 100 nm or more, preferably 300 nm or more.

[0114] In yet another embodiment, the thickness of the intermediate layer can satisfy the range of 10 μm or less, 5 μm or less, preferably 1 μm or less, and may satisfy the range of 100 nm or more, preferably 300 nm or more.

[0115] By satisfying the above-mentioned thickness of the intermediate layer, the intermediate layer can be easily formed on the first substrate layer and the first release layer, and the intermediate layer can be easily transferred to the electrode. In addition, the intermediate layer has the above-mentioned thickness, and thus serves as an appropriate resistance for lithium ions during pre-lithiation, appropriately controls the pre-lithiation rate, and minimizes the role of the intermediate layer as an electrode resistance even if it remains on the electrode active material layer after cell assembly.

[0116] The intermediate layer according to the present application is characterized in that an intermediate layer composition is coated on the top of a first release layer, dried, and then transferred onto the top of an electrode active material layer.

[0117] In one embodiment of the present application, there is provided an electrode pre-lithiation method, wherein the step of transferring the intermediate layer comprises a dry-on-dry process.

[0118] That is, the intermediate layer is formed not by a wet on dry process in which an intermediate layer composition is coated on the upper part of the electrode active material layer, but by a dry on dry process in which an intermediate layer laminate having an intermediate layer formed thereon is transferred onto the upper part of the electrode active material layer.

[0119] The wet on dry process may refer to a process of applying a coating layer composition on top of a dried layer to coat it, and the dry on dry process may refer to a process of transferring a dried layer itself on top of a dried layer.

[0120] The intermediate layer according to one embodiment of the present application is characterized in that it solves the problem, which is a problem when the wet-on-dry method is used, in that the intermediate layer composition penetrates into the electrode active material layer pores, filling or blocking the electrode pores and causing an increase in electrode resistance.

[0121] That is, the intermediate layer composition itself is a fluid composition, and when it is applied and coated on the electrode active material layer in which voids are formed, the intermediate layer composition permeates into the voids of the electrode active material layer due to the fluidity and capillary phenomenon of the intermediate layer composition, thereby causing the above-mentioned problems. However, the intermediate layer according to the present application is formed on the electrode active material layer by a transfer method, and can solve the above-mentioned problems.

[0122] In addition, by forming the intermediate layer by the dry-on-dry process as described above, it can be transferred simultaneously onto the electrode active material layers provided on both sides of the electrode current collector layer. When forming the intermediate layer by the wet-on-dry process, it is difficult to perform coating on both sides at the same time, which can cause the electrode to warp or twist. However, the intermediate layer formation according to the present application has the characteristic of being able to solve the above problems and improve the economic efficiency of the process itself by forming the intermediate layer on both sides at the same time by the dry-on-dry process.

[0123] In one embodiment of the present application, there is provided a method for pre-lithiation of an electrode, in which a first adhesive strength of a surface where the intermediate layer and the first release layer contact each other is 10 gf / inch or more and 150 gf / inch or less.

[0124] In another embodiment, the first adhesive strength may be in the range of 10 gf / inch or more and 150 gf / inch or less, specifically 15 gf / inch or more and 100 gf / inch or less, and more specifically 20 gf / inch or more and 100 gf / inch or less.

[0125] In one embodiment of the present application, the first adhesive force can be measured using equipment including a peel tester (AR-2000), a first release layer (Nitto 31B), and a rubber roller (2 kg). Specifically, the first release layer is attached to one side of the intermediate layer, and then the rubber roller is used to roll it back and forth once to form a structure in which the first release layer and the intermediate layer are laminated, and the structure is stored at room temperature for 24 hours. Thereafter, the first release layer is peeled off at a width of 25 mm to measure the force, and in this case, the peeling speed is 300 mm / min and the peeling angle is 180°.

[0126] By having the first adhesive strength satisfy the above range as described above, the intermediate layer is easily transferred to the top of the electrode active material layer, the intermediate layer laminate is easily manufactured, and reverse transfer to the first base material layer can be prevented.

[0127] In one embodiment of the present application, the surface roughness (S a ) is the surface roughness (S a The surface roughness (S a ) refers to the surface roughness of the surface in contact with the lithium metal layer, and is measured using a CLSM (Confocal Laser Scanning Microscope) device, specifically an Olympus OLS5100, at a magnification of 50x and a scan area of ​​260 μm × 260 μm, and the average value after 10 measurements per sample is used.

[0128] In general, the electrode active material layer containing the active material has a surface roughness (S a ) is in the range of about 0.4 μm to 0.7 μm, which is much higher than the surface roughness of the lithium metal layer, which is 0.04 μm to 0.06 μm.

[0129] That is, when lithium metal is directly transferred onto an electrode active material layer having a large surface roughness, the contact points between the lithium metal and the electrode active material layer are not uniform, and a large amount of by-products are formed during pre-lithiation. To solve this problem, an intermediate layer having the above-mentioned surface roughness may be included.

[0130] As a result, the surface roughness of the intermediate layer according to the present application is calculated based on the surface roughness (S a ) to allow lithium metal to be transferred more uniformly to the top of the electrode active material layer. 。

[0131] In one embodiment of the present application, the method may include removing the first base layer and the first release layer after transferring the intermediate layer. That is, the first base layer and the first release layer serve as a transfer laminate for facilitating the transfer of the intermediate layer onto the electrode active material layer, and also correspond to a laminate for carrying out a dry-on-dry process.

[0132] In one embodiment of the present application, there is provided a step of transferring a lithium metal layer by laminating a lithium metal layer laminate, in which a second substrate layer, a second release layer and a lithium metal layer are sequentially laminated, onto the intermediate layer of the active material layer to which the intermediate layer has been transferred, so that the lithium metal layer is in contact with the intermediate layer; and a step of removing the second substrate layer after the transfer of the lithium metal layer laminate.

[0133] In one embodiment of the present application, a step of transferring a lithium metal layer by laminating a lithium metal layer laminate, in which a second base layer, a second release layer and a lithium metal layer are sequentially laminated, on the intermediate layer of the electrode active material layer to which the intermediate layer has been transferred, so that the lithium metal layer is in contact with the intermediate layer; removing the second substrate layer after transfer of the lithium metal layer laminate; or The method may further include prelithiating the electrode active material layer in at least one step between the step of transferring the lithium metal layer and the step of removing the second substrate layer. That is, the step of prelithiating the electrode active material layer may be performed at any step after the lithium metal layer is transferred onto the intermediate layer of the electrode active material layer to which the intermediate layer is transferred.

[0134] 1, it can be seen that a lithium metal layer laminate 300 in which a second base material layer 41, a second release layer 31, and a lithium metal layer 36 are sequentially laminated on top of an electrode in which an intermediate layer 35 is formed on top of an electrode active material layer 20 is laminated. It can be seen that the second base material layer 41 is then removed to form a structure in which an electrode current collector layer 10, an electrode active material layer 20, an intermediate layer 35, a lithium metal layer 36, and a second release layer 31 are sequentially laminated.

[0135] In one embodiment of the present application, the lithium metal layer laminate may include a structure in which a second substrate layer, a second release layer, and a lithium metal layer are laminated in this order.

[0136] Specifically, in one embodiment of the present application, the second base layer may be at least one selected from the group consisting of polyethylene terephthalate (PET), polyimide (PI), poly(methylmethacrylate) (PMMA), polypropylene, polyethylene, and polycarbonate.

[0137] In one embodiment of the present application, the above description of the first base layer may be similarly applied to the second base layer.

[0138] In one embodiment of the present application, the above description of the first release layer may be similarly applied to the second release layer.

[0139] In one embodiment of the present application, a deposition method for depositing the lithium metal layer on the second substrate layer on which the second release layer is formed may be selected from among evaporation deposition, chemical vapor deposition (CVD), and physical vapor deposition, but is not limited thereto, and various deposition methods used in the art may be used.

[0140] In one embodiment of the present application, the electrode on which the lithium metal layer laminate is laminated may be subjected to roll pressing with a load of 10 kgf to 500 kgf to carry out the transfer process. Then, a process of removing the second base layer is included. By including the second release layer according to the present application during the removal, it is possible to prevent direct contact between the lithium metal layer and air, and thus it is possible to protect the lithium metal layer.

[0141] In one embodiment of the present application, the thickness of the lithium metal layer may be 1 μm or more and 10 μm or less, and preferably 3 μm or more and 10 μm or less.

[0142] When the thickness of the lithium metal layer satisfies the above range, the lithium metal layer is efficiently transferred to the electrode active material layer, and reverse transfer can be prevented.

[0143] In one embodiment of the present application, even after the step of laminating and transferring the lithium metal layer onto the intermediate layer, the intermediate layer can prevent direct contact between the lithium metal and the electrode active material layer, thereby slowing down the progress of the pre-lithiation step.

[0144] Furthermore, when the intermediate layer according to the present application is first transferred onto the top of the lithium metal layer and then laminated onto the electrode active material layer, unlike the present application, the intermediate layer and the lithium metal layer are simultaneously laminated onto the electrode active material layer, so that pre-lithiation proceeds simultaneously, and it may be difficult to derive uniform contact conditions on the top of the electrode.

[0145] In one embodiment of the present application, the electrode prelithiation method includes the steps of prelithiating the electrode active material layer.

[0146] The above step may refer to a step in which prelithiation may proceed from a point where a lithium metal layer is transferred onto the upper part of the electrode active material layer on which the intermediate layer is formed, and may refer to a step in which prelithiation is completed from a point where prelithiation occurs to a point where the lithium metal layer is completely removed with the naked eye.

[0147] In one embodiment of the present application, the step of prelithiating the electrode is carried out under a temperature condition of 60° C. to 80° C. and 5 kgf / cm 2 ~20kgf / cm 2 It can be prelithiated under pressure conditions of

[0148] Under the above conditions, the pre-lithiation completion time during pre-lithiation can be within the range of 1 hour to 24 hours.

[0149] In other words, an intermediate layer is formed on the upper part of the electrode active material layer according to the present application, which can prevent rapid pre-lithiation, and has the characteristic of being able to satisfy the pre-lithiation completion time as described above and to proceed with pre-lithiation more uniformly.

[0150] On the other hand, when the intermediate layer is composed of a polymer, prelithiation is suppressed in a dry state, but prelithiation may occur after electrolyte injection during battery assembly.

[0151] In one embodiment of the present application, there is provided an electrode for a lithium secondary battery that has been prelithiated according to the electrode prelithiation method of the present application.

[0152] In one embodiment of the present application, there is provided a lithium secondary battery comprising a prelithiated electrode according to the present application; a separator located between the electrode and a counter electrode; and an electrolyte.

[0153] In another embodiment of the present application, the electrode active material layer may include a positive electrode active material; an electrode conductive material; and an electrode binder.

[0154] The electrode active material layer including a positive electrode active material; an electrode conductive material; and an electrode binder may mean that the electrode active material layer includes a positive electrode active material; an electrode conductive material; and an electrode binder.

[0155] In one embodiment of the present application, when the electrode is a positive electrode, the positive electrode may include a positive electrode active material layer formed on a positive electrode current collector and including the positive electrode active material.

[0156] In the positive electrode, the positive electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can usually have a thickness of 3 μm to 500 μm, and fine irregularities can be formed on the surface of the current collector to increase the adhesive force of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0157] The positive electrode active material layer composition may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; a lithium iron oxide such as LiFe3O4; 1+c1 Mn 2-c1 O4 (0≦c1≦0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-c2 M c2 Lithium nickel oxide with Ni site represented by the chemical formula LiMnO2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B and Ga, and satisfies 0.01≦c2≦0.3); 2-c3 M c3 O2 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≦c3≦0.1), chemical formula LiM 1-c4 M' c4Examples of the lithium manganese composite oxide include, but are not limited to, lithium manganese oxide represented by Li2Mn3MO8 (wherein M is a transition metal, and M' is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≦c4≦0.1) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); and LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion. The positive electrode may be Li metal.

[0158] In one embodiment of the present application, the electrode active material layer may include a positive electrode active material; an electrode conductive material; and an electrode binder. x Co y Mn z O2(x+y+z=1);LiNi a Co b Mn c Al d O2(a+b+c+d=1);LiMn2O4;LiNi 0.5 Mn 1.5 O2; and LiM x Fe y The present invention provides a method for pre-lithiation of an electrode comprising at least one selected from the group consisting of PO4 (M: transition metal, x+y=1).

[0159] The positive electrode active material layer may contain a positive electrode conductive material and a positive electrode binder in addition to the above-mentioned positive electrode active material.

[0160] At this time, the positive electrode conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing chemical changes in the battery that is constructed.Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like, and one or more of these can be used alone or in mixture.

[0161] The positive electrode binder plays a role in improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one or more of these may be used alone or in combination.

[0162] In one embodiment of the present application, the separator separates the electrode and the positive electrode and provides a passage for lithium ions to move. Any separator that is generally used in secondary batteries can be used without any particular limitation, and is particularly preferred if it has low resistance to ion movement of the electrolyte and excellent electrolyte humidification ability. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymeric substance may be used to ensure heat resistance or mechanical strength, and may be selectively used in a single layer or multilayer structure.

[0163] In one embodiment of the present application, the electrolytic solution may be, but is not limited to, an organic liquid electrolytic solution, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, or a molten inorganic electrolyte that can be used in the manufacture of a lithium secondary battery.

[0164] Specifically, the electrolyte may contain a non-aqueous organic solvent and a metal salt.

[0165] Examples of the non-aqueous organic solvent include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0166] In particular, ethylene carbonate and propylene carbonate, which are cyclic carbonates among the carbonate-based organic solvents, are preferably used because they are high-viscosity organic solvents with high dielectric constants and good dissociation of lithium salts. When such cyclic carbonates are mixed with chain carbonates having low viscosity and low dielectric constants, such as dimethyl carbonate and diethyl carbonate, in an appropriate ratio, an electrolyte having high electrical conductivity can be produced, and therefore these can be used more preferably.

[0167] The metal salt may be a lithium salt, which is a substance that is easily dissolved in the non-aqueous electrolyte. For example, the anion of the lithium salt may be F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3- , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more selected from the group consisting of:

[0168] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, and aluminum trichloride for the purpose of improving the life characteristics of the battery, suppressing a decrease in battery capacity, and improving the discharge capacity of the battery.

[0169] One embodiment of the present invention provides a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same. The battery module and the battery pack include the secondary battery having high capacity, high rate-limiting characteristics and high cycle characteristics, and therefore can be used as a power source for medium- to large-sized devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.

[0170] In one embodiment of the present invention, an electrode pre-lithiation device is provided, comprising: an electrode extraction section, from which an electrode having an electrode active material layer coated on both sides of an electrode collector layer is extracted; an intermediate layer transfer section, which laminates an intermediate layer laminate in which a first base material layer, a first release layer, and an intermediate layer are sequentially laminated on the electrode active material layers provided on both sides of the electrode; a lithium metal layer transfer section, which laminates a lithium metal layer laminate in which a second base material layer, a second release layer, and a lithium metal layer are sequentially laminated on the intermediate layer of the electrode active material layer to which the intermediate layer has been transferred; and an electrode recovery section.

[0171] In one embodiment of the present application, there is provided an electrode pre-lithiation device, wherein the intermediate layer transfer unit includes an intermediate layer laminate recovery unit that recovers the first base material layer and the first release layer, and the lithium metal layer transfer unit includes a lithium metal layer laminate recovery unit that recovers the second base material layer.

[0172] The pre-lithiation device for electrodes according to the present application is characterized by including two R2R steps in order to apply the two transfer steps as described above. Specifically, the device has an electrode extraction section, an intermediate layer transfer section, a lithium metal layer transfer section, and an electrode recovery section, and two R2R steps are carried out in each of the intermediate layer transfer section and the lithium metal transfer section.

[0173] FIG. 2 is a diagram of an electrode pre-lithiation device according to an embodiment of the present application. Specifically, the electrode pre-lithiation device has an electrode pull-out section 1a including an electrode roll having an electrode current collector layer coated on both sides with an electrode active material layer, from which the electrode is pulled out. Then, the electrode passes through an intermediate layer transfer section 1b, and an intermediate layer can be transferred to both sides of the electrode active material layer. Specifically, the intermediate layer transfer section 1b may include an intermediate layer laminate lamination section 2a and an intermediate layer laminate removal section 2b. It can be seen that R2R lamination is performed once in the intermediate layer laminate lamination section. Then, the electrode passes through a lithium metal layer transfer section 1c, and a lithium metal layer is transferred to the upper part of the intermediate layer. At this time, the lithium metal layer transfer section 1c includes a lithium metal layer laminate lamination section 2c and a lithium metal layer laminate removal section 2d. It can be seen that R2R lamination is performed in the lithium metal layer laminate lamination section. Then, the electrode recovery section 1d is configured to recover the electrode.

[0174] In other words, the pre-lithiation device of the present application is a device that performs two R2R processes, transferring an intermediate layer in a dry-on-dry process and transferring a lithium metal layer. EXAMPLES

[0175] Below, preferred examples are presented to aid in understanding the present invention. However, these examples are intended to illustrate the present description, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical ideas of the present description. Naturally, such changes and modifications fall within the scope of the appended claims.

[0176] Manufacturing Example Electrode fabrication The positive electrode slurry was prepared by adjusting the solid content ratio of the positive electrode material (NCMA): conductive material (MWCNT): binder (PVDF-HFP) to 96 wt%: 2 wt%: 2 wt% and using NMP as a solvent. The capacity per cross-sectional coating area was 4.2 mAh / cm. 2The electrode slurry was coated on both sides of an aluminum current collector (thickness: 15 μm) so that the electrode active material layer was formed on both sides of the aluminum current collector. The electrode active material layer was then rolled and pressed in a vacuum oven at 130° C. for 12 hours to prepare an electrode having an electrode active material layer on both sides of the aluminum current collector.

[0177] Manufacturing of the Interlayer Laminate The composition and thickness of the intermediate layer laminate are shown in Table 1. The intermediate layer laminate is a PET film substrate coated with an adhesive acrylic polymer, and the thicknesses of the PET film and intermediate layer were changed to produce the intermediate layer laminate.

[0178] [Table 1]

[0179] Manufacturing of lithium vapor deposition film The composition and thickness of the lithium deposition film are shown in Table 2. The lithium deposition film is made by coating a 500nm-thick release layer made of acrylic polymer on a 25μm-thick PET substrate, and then depositing a 6.2μm-thick lithium layer on this release layer using thermal evaporation.

[0180] [Table 2]

[0181] Example 1 The electrode and intermediate layer laminate A produced above were subjected to roll lamination, and then the base film (PET) and release layer were removed to produce an electrode with an intermediate layer transferred thereto. The intermediate layer was peeled off at the interface between the release layer and the intermediate layer, and transferred to the electrode. The electrode with the intermediate layer transferred thereto and the lithium vapor-deposited film (C) were subjected to roll lamination, and then the base layer (PET) of the lithium vapor-deposited film was removed to produce a multi-layer (release layer / lithium layer / intermediate layer / electrode layer) electrode with the lithium layer / release layer transferred thereto (dry on dry method) (see Figure 3).

[0182] Example 2 A multi-layer electrode in which an intermediate layer and a lithium layer (including a release layer) were sequentially transferred was manufactured in the same manner as in Example 1, except that an intermediate layer B was used instead of an intermediate layer A (see FIG. 4).

[0183] Comparative Example 1 In Example 1, the electrode to which the intermediate layer (A or B) and the lithium metal layer were not transferred was named a pristine electrode (Comparative Example 1).

[0184] Comparative Example 2 The same procedure as in Example 1 was repeated, except that the intermediate layer (A or B) was not formed on the upper part of the electrode active material layer, and the lithium metal layer was directly transferred onto the upper part of the electrode active material layer formed on both sides of the electrode current collector layer.

[0185] Coin half-cells were manufactured using the electrodes manufactured by the methods of Example 1, Comparative Example 1, and Comparative Example 2, and the initial charge / discharge capacity and cycle performance were evaluated. The results are shown in Table 3 and FIG. 5 below. The electrolyte used in the manufacture of the coin half-cells was 1M LiPF6 in EC / EMC (30:70 vol%), and a lithium metal foil with a thickness of 150 μm was used as the counter electrode. When measuring the initial charge / discharge capacity, the C-rate was 0.1 C, charging was performed under CCCV conditions with an upper limit voltage of 4.3 V and a cutoff current of 0.005 C, and discharging was performed under CC conditions with a lower limit voltage of 3.0 V. The cycle capacity was measured under the conditions of upper and lower limit voltages of 4.3 V / 3.0 V, C-rate of 0.33 C, charging CCCV, and discharging CC.

[0186] [Table 3]

[0187] 5, it was confirmed that the electrode according to Example 1, in which an electrode including a lithium metal layer was manufactured by a sequential transfer process, had an extremely high initial charge capacity compared to the electrodes manufactured by Comparative Examples 1 and 2. Specifically, it was confirmed that the method according to Example 1 includes a process of transferring an intermediate layer onto the electrode active material layer in order to solve the problem of surface active material cracking in a high-capacity positive electrode active material, and thus has the characteristic of preventing rapid pre-lithiation of the active material since lithium metal does not come into direct contact with the electrode active material layer.

[0188] In the case of Example 1, the intermediate layer is formed by the dry on dry process as described above, which is different from the wet on dry process in that the lithium metal layer can be simultaneously transferred onto the upper part of the electrode active material layer provided on both sides of the electrode current collector layer.

[0189] In the case of Example 2, since the intermediate layer is formed to a thin thickness, the pre-lithiation rate can be appropriately controlled, and even if some of the intermediate layer remains on the upper part of the electrode active material layer after the cell is assembled, the role of the intermediate layer as an electrode resistance is minimized.

[0190] It was found that the pristine electrode not including the lithium metal layer of Comparative Example 1 had inferior cycle performance compared to Example 1 (see FIG. 6).

[0191] In the case of Comparative Example 2, an intermediate layer was not formed, and a process of directly transferring a lithium metal layer onto the upper part of the electrode was included. When the process was carried out as in Comparative Example 2, cracks occurred in the active material particles on the surface side of the electrode due to rapid pre-lithiation of the electrode, and it was confirmed that the cycle performance was reduced compared to Example 1 (see FIG. 6). [Explanation of symbols]

[0192] 10 Electrode current collector layer 20...electrode active material layer 30...1st release layer 35 Middle class 40...1st base layer 31...Second release layer 41...Second base material layer 36 Lithium metal layer 100...electrode 200 ··· Interlayer laminate 300 Lithium metal layer stack 1a Electrode lead-out section 1b: Intermediate layer transfer section 1c Lithium metal layer transfer section 1d Electrode recovery section 2a: Intermediate layer laminate lamination section 2b: Intermediate layer laminate removal section 2c Lithium metal layer laminate lamination section 2d Lithium metal layer stack removal section

Claims

1. preparing an electrode having an electrode active material layer coated on at least one surface of an electrode current collector layer; a step of laminating an intermediate layer of an intermediate layer laminate, in which a first base layer, a first release layer, and an intermediate layer are sequentially laminated on the electrode active material layer, so that the intermediate layer contacts the electrode active material layer, thereby transferring the intermediate layer; removing the first substrate layer and the first release layer after transferring the intermediate layer; a step of laminating a lithium metal layer laminate, in which a second base layer, a second release layer and a lithium metal layer are sequentially laminated, on the intermediate layer of the electrode active material layer to which the intermediate layer has been transferred, so that the lithium metal layer is in contact with the intermediate layer, thereby transferring the lithium metal layer; and removing the second substrate layer after transferring the lithium metal layer laminate; 4. An electrode pre-lithiation method comprising:

2. a step of laminating a lithium metal layer laminate, in which a second base layer, a second release layer, and a lithium metal layer are sequentially laminated, on the intermediate layer of the electrode active material layer to which the intermediate layer has been transferred, so that the lithium metal layer is in contact with the intermediate layer, thereby transferring the lithium metal layer; removing the second substrate layer after transfer of the lithium metal layer laminate; or prelithiating the electrode active material layer at least one step between the step of transferring the lithium metal layer and the step of removing the second substrate layer; 10. The electrode pre-lithiation method of claim 1 further comprising:

3. the intermediate layer comprises an intermediate layer composition; 10. The electrode pre-lithiation method of claim 1, wherein the intermediate layer composition comprises at least one selected from the group consisting of a polymer; an inorganic material; an active material; and a conductive material.

4. 2. The electrode pre-lithiation method of claim 1, wherein the intermediate layer has a thickness of 50 μm or less.

5. 10. The electrode pre-lithiation method of claim 1, wherein the step of transferring the intermediate layer comprises a dry on dry process.

6. 2. The method for pre-electrode lithiation according to claim 1, wherein a first adhesive strength of a surface where the intermediate layer and the first release layer contact each other is 10 gf / inch or more and 150 gf / inch or less.

7. The electrode active material layer includes a negative electrode active material; an electrode conductive material; and an electrode binder, The negative electrode active material is graphite, soft carbon, hard carbon, SiO x (x=0), SiO x 2. The electrode pre-lithiation method of claim 1, comprising at least one selected from the group consisting of (0<x<2), Si / C, metal impurities, and Si alloys.

8. The electrode active material layer includes a positive electrode active material; an electrode conductive material; and an electrode binder. The positive electrode active material is LiNi x Co y Mn z O 2 (x+y+z=1);LiNi a Co b Mn c A d O 2 (a+b+c+d=1);LiMn 2 O 4 ;LiNi 0.5 Mn 1.5 O 2 and LiM x Fe y P.O. 4 2. The method of claim 1, further comprising at least one selected from the group consisting of: (M: transition metal, x+y=1).

9. The surface roughness (S a ) is the surface roughness (S a 2. The method of claim 1, wherein the electrode pre-lithiation temperature is at least 5 times lower than that of the electrode pre-lithiation temperature.

10. 2. The method of claim 1, wherein the first base material layer and the second base material layer are at least one selected from the group consisting of polyethylene terephthalate (PET), polyimide (PI), poly(methylmethacrylate) (PMMA), polypropylene, polyethylene, and polycarbonate.

11. 2. The method of claim 1, wherein the lithium metal layer has a thickness of 1 μm or more and 10 μm or less.

12. An electrode for a lithium secondary battery prelithiated by the method for prelithiation of an electrode according to any one of claims 1 to 11.

13. an electrode lead-out portion from which an electrode having an electrode current collector layer coated on both sides with an electrode active material layer is led out; an intermediate layer transfer unit that laminates an intermediate layer laminate in which a first base material layer, a first release layer, and an intermediate layer are sequentially laminated on the electrode active material layers provided on both sides of the electrode; a lithium metal layer transfer unit that laminates a lithium metal layer laminate in which a second base material layer, a second release layer, and a lithium metal layer are sequentially laminated on the intermediate layer of the electrode active material layer to which the intermediate layer has been transferred; and Electrode recovery section; 1. An electrode pre-lithiation device comprising:

14. the intermediate layer transfer unit includes an intermediate layer laminate recovery unit that recovers the first base material layer and the first release layer, The pre-electrode lithiation device according to claim 13 , wherein the lithium metal layer transfer section includes a lithium metal layer laminate recovery section that recovers the second substrate layer.

Citation Information

Patent Citations

  • Nonaqueous secondary battery

    JP2007242590A

  • Transfer film, electrode plate for electrochemical element formed using the same, and lithium secondary battery

    JP2007273459A

  • Method of manufacturing lithium-doped negative electrode

    JP2018190692A

  • Electrode and lithium secondary battery including the same

    JP2019525437A

  • Negative electrode for lithium secondary battery, lithium secondary battery including the same, and method for manufacturing the same

    JP2021527937A