JVD Surface Treatment

The annealing and vacuum deposition method forms a ferrite layer and multi-layered metal coatings on steel substrates, addressing coating deterioration issues by enhancing durability and anti-corrosion properties.

JP2024540908AActive Publication Date: 2024-11-06ARCELORMITTAL SA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024523439
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-19
Filing Date
2022-09-05
Publication Date
2024-11-06
Estimated Expiration
2042-09-05

AI Technical Summary

Technical Problem

Conventional coating methods, such as hot dipping and electrocoating, fail to provide satisfactory coatings for steel grades containing high levels of oxidizing elements like Si, Mn, Al, P, Cr, or B, leading to coating deterioration during molding processes.

Method used

A method involving an annealing process with controlled heating and dew point conditions to form a ferrite surface layer, followed by a skin pass process and a vacuum deposition of metal coatings at supersonic velocities to create a multi-layered metal coating on the steel substrate, which includes a ferrite layer and anti-corrosive layers like zinc or zinc-magnesium.

Benefits of technology

The method enhances the durability of the coating, reducing coating deterioration during shaping operations by minimizing surface irregularities and improving surface affinity, resulting in a robust and anti-corrosive coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540908000002
    Figure 2024540908000002
  • Figure 2024540908000003
    Figure 2024540908000003
  • Figure 2024540908000004
    Figure 2024540908000004
Patent Text Reader

Abstract

This patent relates to a method for depositing a metal coating onto a substrate, including: - an annealing step of forming, in an annealing furnace, a ferrite surface layer having a thickness of 10 μm to 50 μm on the base material, the surface fraction of which is up to 10% and includes accumulated amounts of martensite and bainite, the remainder being ferrite, and the like; - Skin pass process, - a coating step in a vacuum chamber, in which metal vapor is ejected towards at least one side of the substrate to form at least one surface layer of metal.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for depositing a metallic coating on a substrate.The present invention also relates to a coated steel strip.

[0002] The present invention is particularly, but not exclusively, intended to deposit an anticorrosive metal coating, such as a zinc or zinc-magnesium based coating, onto a running steel strip. Such coated steel strip may then be cut and shaped, for example by stamping, bending, or forming, to form parts, which may then be painted to form a coating over the coating. [Background technology]

[0003] Several coating methods exist, such as hot dip galvanizing and electrocoating. However, these conventional methods do not provide satisfactory coatings for steel grades that contain high levels of oxidizing elements, such as Si, Mn, Al, P, Cr or B. As a result, new methods have been developed, such as vacuum deposition techniques, e.g., JVD (Jet Vapor Deposition).

[0004] In JVD, a metal vapour spray propelled at supersonically speed contacts a substrate within a vacuum chamber, as described in WO 97 / 47782 and WO 2009 / 047333. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 97 / 47782 [Patent Document 2] International Publication No. 2009 / 047333 Summary of the Invention

[0006] Nevertheless, it has been observed that such processes sometimes result in degradation of the coating, especially during the moulding process.The aim of the present invention is to remedy this drawback.

[0007] Other features and advantages will become apparent from the following detailed description of the invention.

[0008] For the purposes of illustrating the present invention, various embodiments will now be described with particular reference to the following figures. [Brief description of the drawings]

[0009] [Figure 1] The steel substrate layer after the annealing step according to the present invention is embodied. [Diagram 2] The steel substrate layer after the coating process according to the present invention is embodied. [Diagram 3] Different steps of the three-stage flanging test are embodied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention relates to a method for depositing a metallic coating on a steel substrate, comprising the steps of: i. An annealing process in an annealing furnace, a. a preheating step of heating the steel substrate to a temperature T1 lower than 600°C; b. The steel substrate is treated with 0.1 to 90 volume % of H 2 a heating step of heating from T1 to a recrystallization temperature T2 of 720°C to 1000°C in an atmosphere having a dew point of -25°C to 10°C, the balance of which is an inert gas and unavoidable impurities; c. The steel substrate is treated with 0.1 to 90 volume % H 2 The remainder is inert gas and unavoidable impurities, and the temperature is maintained in the range of 720℃ to 1000℃ in an atmosphere with a dew point of -25℃ to 10℃. such an annealing process allows the formation of a ferritic surface layer having a thickness of 10 μm to 50 μm on the steel substrate and a microstructure comprising an accumulated amount of martensite, austenite, bainite and carbides up to a surface fraction of 10%, the remainder being composed of ferrite; ii. Skin pass process in a temper mill, where the steel substrate is rolled with a reduction of 0.02% to 2%; iii. A coating step in a vacuum chamber, in which at least one metal vapor is ejected towards at least one side of the substrate to form a metal coating. The present invention relates to a method comprising the steps of:

[0011] Prior to the annealing step, the steel substrate may be rolled, for example, it is preferred to hot roll the substrate and then cold roll it.

[0012] Preferably, the method relates to a method for depositing a metal coating on a steel running substrate. Preferably, in the coating step, said at least metal vapour is ejected towards at least one side of said steel running substrate.

[0013] Preferably, the annealing step is carried out in a continuous annealing furnace.

[0014] During preheating, the steel sheet is heated to a temperature T1, which is usually from room temperature to less than 600° C. Preheating can be carried out by any means. For example, preheating can be carried out in an RTF (radiant tube furnace), by means of induction equipment or in a DFF (direct fired furnace).

[0015] Limiting the preheat temperature to less than 600°C is advantageous as it reduces oxidation of the steel sheet. Preferably, T1 is less than 550°C. Even more preferably, T1 is less than 500°C.

[0016] Preferably, in the heating step, the dew point is from -20°C to -1°C. Preferably, in the soaking step, the dew point is from -20°C to -1°C.

[0017] The atmosphere in the heating and soaking processes uses preheated steam and the dew point temperature of the atmosphere is monitored in different sections. 2 A furnace equipped with a N detector 2 -H 2 This can be achieved by introducing a gas.

[0018] Preferably, in the heating step and / or the soaking step, the atmosphere is 0.1 to 10% by volume of H 2 the remainder being inert gases and unavoidable impurities.

[0019] The ferrite surface layer is formed by the conditions in the annealing furnace that change the microstructure of the steel, i.e. by decarburization and phase transformation. Indeed, the oxygen present in the annealing atmosphere reacts with the carbon from the steel to form CO 2 The formation of gases such as CO and CO results in a depletion of carbon atoms under the steel surface, favoring the formation of ferrite. For example, martensitic steels can be converted to ferrite under conditions well known to those skilled in the art. Any means known to those skilled in the art can be used to form a ferrite surface layer on the substrate. Preferably, water injection is performed during annealing to form the desired ferrite surface layer.

[0020] As shown in Figure 1, the steel substrate exiting the annealing furnace comprises at least two layers: a steel bulk layer 10 and a ferritic surface layer 11 on top of the steel bulk 10. An iron oxide layer of 5-15 nm may be present on top of the ferritic layer.

[0021] In the coating step, the coating layer can be applied by any possible means in a vacuum chamber, for example any PVD process. Preferably, the metal coating layer is applied by sputtering. Preferably, the coating step includes at least one coating process, in which at least one metal vapor is ejected at ultrasonic speed towards at least one side of the substrate to form a metal coating.

[0022] The coating process can include one or several coating processes. For example, the coating process can include PVD of a first metal alloy followed by JVD of a second metal alloy, in which at least one metal vapor is ejected at supersonic speed towards at least one side of the substrate to form a metal coating. As a result, the metal coating can include several layers of different metals or metal alloys.

[0023] The coating process may include a pretreatment which may involve an alkaline degreasing step followed by a rinsing step.

[0024] For example, this process makes it possible to produce a coating strip as shown in figure 2. This coating strip comprises a steel bulk 10, a ferrite layer 11, a first metal layer 12 and a second metal layer 13.

[0025] A 5-15 nm iron oxide layer may be present on the ferrite surface layer between the ferrite layer 11 and the first metal layer 12 .

[0026] After studying the causes of coating degradation during forming operations, the inventors discovered that most of the failure occurs within the top coating layer, for example within the metal coating.

[0027] After confirming that most of the damage occurs in the top coating layer, it was found that the surface morphology of the steel substrate has a significant impact on the occurrence of coating degradation, due, among other things, to the fact that an uneven surface containing deep holes and crevices affects the surface affinity with the rinse water in the pre-treatment section of the vacuum deposition process.

[0028] According to the claimed method, the annealing conditions allow the formation of a ferrite layer by decarburization of the steel bulk. The ductile ferrite allows at least partially filling said pores and gaps during the skin pass. As a result, the presence of pores and gaps at the surface, or at least their severity, is reduced and there is a lower amount of residual water on the steel substrate surface before coating. Finally, the coated steel strip according to this method is less susceptible to degradation, especially during its forming operation.

[0029] Preferably, the steel substrate is a strip or band or plate.

[0030] Preferably, the steel substrate has a thickness of 0.5 mm to 5 mm, and even more preferably, the substrate has a thickness of 1 to 3 mm.

[0031] Preferably, the steel substrate contains, by weight percentage, 0.15 < Si < 0.4, 0.5 < Mn < 2.5, 0.1 < C < 0.4, P ≤ 0.03, S ≤ 0.02, 0.01 < Al ≤ 0.1, Cu ≤ 0.2, Ti + Nb ≤ 0.20, Cr + Mo ≤ 1, and the balance consists of Fe and inevitable impurities. Preferably, the steel substrate contains, by surface fraction, a cumulative amount of ferrite, austenite, bainite, and carbide of up to 10%, and the balance has a bulk microstructure composed of martensite. Even more preferably, the steel substrate contains, by surface fraction, a cumulative amount of ferrite, austenite, bainite, and carbide of up to 5%, and the balance has a bulk microstructure composed of martensite. Such a steel substrate is advantageous for automotive applications.

[0032] These steels are known as martensitic steels.

[0033] Preferably, the steel substrate contains, by weight percentage, 0.15 < Si < 0.6, 0.17 < Mn < 2.3, 0.1 < C < 0.4, P ≤ 0.05, S ≤ 0.01, 0.015 < Al ≤ 1.0, Cu ≤ 0.2, B ≤ 0.005, Ti + Nb ≤ 0.15, Cr + Mo ≤ 1.4, and the balance consists of Fe and inevitable impurities. Preferably, the steel substrate contains, by surface fraction, austenite, ferrite, and carbide of up to 10%, and the balance has a microstructure composed of bainite and martensite. Even more preferably, the steel substrate contains, by surface fraction, a cumulative amount of ferrite, austenite, and carbide of up to 5%, and the balance has a microstructure composed of bainite and martensite. Such a steel substrate is advantageous for automotive applications.

[0034] These steels are known as duplex steels.

[0035] Preferably, in the annealing step, the substrate is maintained in a temperature range of 820°C to 930°C.

[0036] Preferably, the ferrite layer has a microstructure composed of ferrite with a cumulative amount of martensite, austenite, bainite, and carbide up to 5% in surface fraction, and the remainder being ferrite.

[0037] Preferably, the ferrite layer has a thickness of 20 μm to 40 μm.

[0038] Preferably, the steel substrate is rolled with a rolling reduction rate of 0.02% to 0.5%.

[0039] Preferably, in the coating step iii., the metal film - contains at least 8% nickel and at least 10% chromium by weight, with the remainder being iron and impurities resulting from the manufacturing process, and is a first metal layer formed on at least one side of the substrate by physical vapor deposition, - includes a second metal layer of at least one metal formed on the first metal layer by jet vapor deposition.

[0040] Preferably, the second metal layer is a corrosion-resistant metal film.

[0041] Preferably, in the coating step iii., the metal film - contains Fe, Ni, Cr, and Ti, with the amount of Ti being ≧ 5% by weight, satisfying the following formula, i.e., 8% < Cr + Ti < 40% by weight, and the remainder being Fe and Ni, and is a first metal layer formed on at least one side of the substrate by physical vapor deposition, - includes a second metal layer of at least one metal formed on the first metal layer by jet vapor deposition.

[0042] Preferably, the second metal layer is a corrosion-resistant metal film.

[0043] Preferably, the first metal layer is formed by sputtering.

[0044] For example, the first metal layer can contain, by weight percentage, 0.02 < C < 0.2, 15 < Cr < 25, 5 < Ni < 22, Mo < 3, 0.5 < Si < 1.5, 1.5 < Mn < 2.5, P < 0.1, S < 0.05, with the balance being Fe and unavoidable impurities.

[0045] For example, the first metal layer can contain, by weight percentage, 0.02 < C < 0.5, 15 < Cr < 20, 9 < Ni < 15, 1.5 < Mo < 3, 0.5 < Si < 1.5, 1.5 < Mn < 2.5, P < 0.1, S < 0.05, with the balance being Fe and unavoidable impurities.

[0046] Preferably, the second metal layer contains aluminum and magnesium or zinc or magnesium and zinc.

[0047] Preferably, the second metal layer results from a coating process in which at least metal vapor is ejected towards the substrate at supersonic speed to form a metal film. Even more preferably, the second metal layer results from a jet vapor deposition process.

[0048] Preferably, the second metal layer contains, by weight percentage, 0 ≦ Mg < 20 and 80 < Zn ≦ 100, with the balance being unavoidable impurities. Even more preferably, the second metal layer contains, by weight percentage, 0 ≦ Mg < 10 and 90 < Zn ≦ 100, with the balance being unavoidable impurities.

[0049] Preferably, the second metal layer is a corrosion protection layer. Preferably, the second metal layer contains 100% Zn by weight percentage. Preferably, the second metal layer contains, by weight percentage, 0 < Mg < 10 and 90 < Zn < 100, with the balance being unavoidable impurities.

[0050] Preferably, the second metal layer contains, by weight percentage, 0 < Mg < 4 and 96 < Zn < 100, with the balance being unavoidable impurities.

[0051] As shown in Figure 2, the present invention is a coated steel strip, - Steel bulk 10 - A ferrite layer 11 having a thickness of 10 μm to 50 μm and containing up to 10% of the cumulative amount of martensite, austenite, bainite, and carbide in surface fraction on the steel bulk, with the remainder being composed of ferrite - An iron oxide layer 12 having a thickness of 5 to 15 nm on the ferrite layer, - A first metal layer 12 on the steel oxide layer, - Related to a coated steel strip including a second metal layer 13 having a thickness of 5 to 10 μm on the first metal layer.

[0052] Preferably, the coated steel strip is manufactured according to the aforementioned method in which the first and second metal layers are coated.

[0053] Preferably, the coated steel strip has a thickness of 0.5 mm to 5 mm. Even more preferably, the coated steel strip has a thickness of 1 to 3 mm.

[0054] One possibility is that the steel bulk 10 contains, in weight percent, 0.15 < Si < 0.4, 0.5 < Mn < 2.5, 0.1 < C < 0.4, P ≤ 0.03, S ≤ 0.02, 0.01 < Al ≤ 0.1, Cu ≤ 0.2, T1 + Nb ≤ 0.20, Cr + Mo ≤ 1, with the remainder being Fe and inevitable impurities. Preferably, the steel substrate has a microstructure containing up to 10% of ferrite, austenite, bainite, and carbide in surface fraction, with the remainder being composed of martensite. Even more preferably, the steel substrate has a microstructure containing up to 5% of ferrite, austenite, bainite, and carbide in surface fraction, with the remainder being composed of martensite. Such steel substrates are advantageous for automotive applications. These steels are known as martensitic steels.

[0055] Another possibility is that the steel bulk 10 contains, by weight percent, 0.15 < Si < 0.6, 0.17 < Mn < 2.3, 0.1 < C < 0.4, P ≤ 0.05, S ≤ 0.01, 0.015 < Al ≤ 1.0, Cu ≤ 0.2, B ≤ 0.005, T1 + Nb ≤ 0.15, Cr + Mo ≤ 1.4, with the balance being composed of Fe and inevitable impurities, and has a microstructure containing, by surface fraction, up to 10% austenite, ferrite and carbide, with the balance being composed of bainite and martensite.

[0056] Preferably, the steel bulk has a strength of 450 MPa or more.

[0057] An iron oxide layer of 5 - 10 nm may be present on the ferrite surface layer.

[0058] Preferably, the ferrite layer has a microstructure containing, by surface fraction, up to 5% cumulative amount of martensite, austenite, bainite and carbide, with the balance being composed of ferrite.

[0059] Preferably, the ferrite layer has a thickness of 20 μm - 40 μm.

[0060] Preferably, the first metal layer has a thickness of 2 - 15 nm.

[0061] Preferably, the first metal layer contains, by weight, at least 8% nickel and at least 10% chromium, with the balance being iron and impurities.

[0062] For example, the first metal layer contains, by weight percent, 0.02 < C < 0.2, 15 < Cr < 25, 5 < Ni < 22, Mo < 3, 0.5 < Si < 1.5, 1.5 < Mn < 2.5, P < 0.1, S < 0.05, with the balance being Fe and inevitable impurities.

[0063] For example, the first metal layer contains, by weight percent, 0.02 < C < 0.5, 15 < Cr < 20, 9 < Ni < 15, 1.5 < Mo < 3, 0.5 < Si < 1.5, 1.5 < Mn < 2.5, P < 0.1, S < 0.05, and the balance consists of Fe and unavoidable impurities.

[0064] Preferably, the second metal vapor is an anticorrosion layer. Preferably, the second metal vapor contains, by weight percent, 100% Zn. Preferably, the second metal vapor contains, by weight percent, 0 < Mg < 3, 97 < Zn < 100, and the balance consists of unavoidable impurities.

Example

[0065] [Experiment] The purpose of the experiment is to evaluate the effect of the claimed method on the film damage of the coated steel strip.

[0066] A first series of five samples of MS1500 steel sheets having a thickness of 1.5 to 2.0 mm of the type sold under the brand of MartINsite(R) 1500 by ArcelorMittal were prepared. The exact composition of the steel used for the samples is C 0.22%, Mn 1.8%, Si 0.26%, Cr 0.17%, Al 0.03%. The percentages are by weight, and the balance is iron and potential impurities resulting from the manufacturing.

[0067] All samples were subjected to the following steps.

[0068] The annealing process includes a heating process and a soaking process.

[0069] The heating process has a temperature T2 of 860°C to 870°C in an atmosphere containing 5% by volume of H 2 and the balance is N 2 and unavoidable impurities. The dew point of the heating process was either -40°C to -30°C (dry annealing) or -20°C to -1°C (wet annealing).

[0070] The soaking process contains 5% by volume of H 2 and the balance is N 2and unavoidable impurities in the atmosphere, the temperature being 860°C to 870°C. The dew point of the soaking step was either -40°C to -30°C (dry annealing) or -20°C to -1°C (wet annealing).

[0071] Then, some samples (n° 1, 3, 4, 5) were subjected to a skin pass with a reduction of 0.1% and one sample (n° 2) was not subjected to a skin pass.

[0072] The skin was followed by PVD of a 15 nm first layer of metal vapor containing 0.02% C, 16-18% Cr, 10.5-13% Ni, 2-2.5% Mo, 1% Si, 2% Mn, 0.04% P, 0.03% S, with the remainder being Fe and potential impurities from manufacturing, and JVD of a second layer of 7.5 μm Zn.

[0073] All samples were then tested using a three-stage flanging test as shown in FIG.

[0074] In the first step, a sample having a thickness “t” is bent through a first bending zone B. 1 The specimens are bent to form an angle of 130° on a given punch radius R at t = 2.5. In the first series, all specimens had a ratio between punch radius and specimen thickness of 2.5, i.e. R / t = 2.5.

[0075] Next, in the second step, the second bending zone B 2 The sample is moved so as to position the bending mold perpendicular to the specimen.

[0076] In the third step, the second bending zone B 2 while bending the strip to form an angle of 90° in the first bending zone B 1 Bend it so that it is flat again.

[0077] This test allows the coated steel strip to be deformed in a first step and in a third step the coated steel strip is compressed in the first bend zone by unbending the first bend.

[0078] Finally, the adhesive is pressed into the first bending zone and depending on the amount of material adhering to the adhesive, the quality is classified into two categories: "OK" or "NOK".

[0079] The properties of each test specimen are shown in the table below.

[0080] [Table 1]

[0081] Samples 1 and 2 are not according to the present invention. Samples 3 to 5 are according to the present invention.

[0082] It is clear that a good quality of the coating can be achieved when the steel sheet is subjected to the process according to the invention. It is also clear that a good coating quality cannot be reliably ensured if at least one of the two steps preceding the coating step, such as the annealing step or the skin pass step, is not carried out according to the invention.

[0083] Only the method according to the invention therefore makes it possible to reliably obtain a coating which is not prone to degradation, in particular during its forming operations.

Claims

1. 1. A method for depositing a metallic coating on a steel substrate, comprising: i. An annealing step in an annealing furnace, a. A preheating step of heating the steel substrate to a temperature T1 lower than 600° C.; b. The substrate is mixed with 0.1 to 90% by volume of H 2 a heating step of heating from T1 to a recrystallization temperature T2 of 720°C to 1000°C in an atmosphere having a dew point of -25°C to 10°C, with the balance being inert gas and unavoidable impurities; and then c. The substrate is mixed with 0.1 to 90% by volume of H 2 The balance is an inert gas and unavoidable impurities, and the temperature is maintained in the range of 720°C to 1000°C in an atmosphere with a dew point of -25°C to 10°C. an annealing step which allows the formation of a ferritic surface layer having a thickness of 10 μm to 50 μm on said substrate and a microstructure comprising an accumulated amount of martensite, austenite, bainite and carbides up to a surface fraction of 10%, the remainder being composed of ferrite; ii. A skin pass process in a temper mill, where the substrate is rolled with a reduction of 0.02% to 2%; iii. A coating step in a vacuum chamber, in which at least one metal vapor is ejected towards at least one side of the substrate to form a metal coating. The method includes:

2. The method of claim 1 , wherein the steel substrate has a thickness of from 0.5 mm to 5 mm.

3. 3. The method of claim 1 or 2, wherein the steel substrate has a composition comprising, in weight percent, 0.15<Si<0.4, 0.5<Mn<2.5, 0.1<C<0.4, P≦0.03, S≦0.02, 0.01<Al≦0.1, Cu≦0.2, T1+Nb≦0.20, Cr+Mo≦1, with the balance being Fe and unavoidable impurities.

4. 4. The method of claim 3, wherein the steel substrate has a bulk microstructure comprising a maximum of 10% surface fraction of accumulated amounts of ferrite, austenite, bainite and carbides, with the remainder being composed of martensite.

5. 3. The method of claim 1 or 2, wherein the steel substrate has a composition, in weight percent, of 0.15<Si<0.6, 0.17<Mn<2.3, 0.1<C<0.4, P≦0.05, S≦0.01, 0.015<Al≦1.0, Cu≦0.2, B≦0.005, T1+Nb≦0.15, Cr+Mo≦1.4, with the balance being Fe and unavoidable impurities.

6. 6. The method of claim 5, wherein the steel substrate has a bulk microstructure containing a surface fraction of up to 5% ferrite with the remainder composed of martensite and bainite.

7. The method according to any one of claims 1 to 6, wherein in the annealing step, the substrate is maintained at a temperature in the range of 820°C to 930°C.

8. 8. The method according to claim 1, wherein the ferritic layer has a microstructure comprising up to 5% surface fraction of accumulated martensite, austenite, bainite and carbides, the remainder being composed of ferrite.

9. The method according to any one of the preceding claims, wherein the ferrite layer has a thickness of 20 μm to 40 μm.

10. In the coating step, a first metal layer, comprising by weight at least 8% nickel and at least 10% chromium, the remainder being iron and impurities resulting from the manufacturing process, formed on at least one side of said substrate by physical vapour deposition; A method according to any one of the preceding claims, in which a second metal vapour is ejected towards at least said side of said substrate to form at least one layer of metal on said first metal layer.

11. The method according to any one of claims 1 to 10, wherein the second metal vapor is a corrosion protection layer.

12. The method according to any one of claims 1 to 11, wherein in the coating step, the surface layer is formed by JVD.

13. A coated steel strip comprising: - Steel Bulk 10 a ferritic layer 11 on top of the steel bulk, with a thickness between 10 μm and 50 μm and a surface fraction up to 10% and having a microstructure comprising accumulated amounts of martensite, austenite, bainite and carbides, the remainder being composed of ferrite; - an iron oxide layer 12 having a thickness of 5 to 15 nm on said ferrite layer, a first metal layer 13 on said oxidized steel layer, a second metal layer 14 having a thickness of 5 to 10 μm on said first metal layer; Coated steel strip including:

14. Coated steel strip according to claim 13, produced according to any one of claims 10 to 12.

Citation Information

Patent Citations

  • A method for manufacturing easily formable flat steel products, a flat steel product, and a method for manufacturing parts from the flat steel product.

    JP2013513725A

  • Cold-rolled steel sheet, manufacturing method, and vehicle

    JP2016529392A

  • Multilayer substrate and manufacturing method

    JP2017512909A

  • Zinc hot-dipped steel sheet

    WO2019026116A1

  • Method and device for continuous coating of a moving substrate by means of a metallic vapour