Multilayer composite material for lithium-ion secondary batteries and its preparation method and application
A multilayer composite material with a carbon matrix, nanosilicon composite, and carbon shell, stabilized by Si-C and Si-N bonds, addresses the capacity and volume change issues of silicon electrodes, enhancing lithium-ion battery performance.
Patent Information
- Application Number
- JP2024531617
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-10
- Filing Date
- 2022-06-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-06-23
AI Technical Summary
Conventional graphite negative electrodes in lithium-ion batteries have limited theoretical capacity, and silicon-based electrodes face significant volume change issues, hindering their practical application in high-capacity anodes.
A multilayer composite material for lithium-ion batteries comprising a carbon matrix, nanosilicon-based composite material, and carbon shell, prepared via vapor phase growth methods, with Si-C, Si-N bonds, and boron or phosphorus doping to stabilize the structure and enhance electrochemical performance.
The composite material exhibits reduced body expansion, improved cycle characteristics, and enhanced rate capabilities due to the stable three-layer structure and amorphous bond formation, making it suitable for high-performance lithium-ion batteries.
Smart Images

Figure 2024541567000001_ABST
Abstract
Description
[Technical field]
[0001] [Cross reference] This application claims priority to a Chinese patent application filed with the China Patent Office on December 10, 2021, bearing application number 202111510520.3 and titled "Multilayer composite material for lithium-ion secondary batteries and its preparation method and application."
[0002] [Technical field] The present invention relates to the technical field of materials, in particular to a multi-layer composite material for lithium-ion secondary batteries and its preparation method and application. [Background technology]
[0003] In the past few decades, commercialized lithium-ion batteries have achieved great success due to their advantages of long cycle life, high energy density, and environmental friendliness. Conventional secondary lithium-ion batteries mainly consist of a negative electrode (usually a carbonaceous material such as graphite), a positive electrode (e.g. LiCoO2, LiMn2O2, and LiFePO4), and a separator impregnated with an electrolyte, in which lithium ions shuttle between the two electrodes through the liquid electrolyte, and the charge is transferred via an external circuit.
[0004] However, the theoretical capacity of conventional graphite anode materials is limited to 372mAh / g, which cannot meet the ever-increasing requirements for high-performance storage capacity.With the increasing demand for portable electronic devices, electric vehicles, and renewable energy applications, the development of high-capacity anode materials with excellent electrochemical performance has proven to be an important solution for realizing lithium-ion storage and improving the overall energy density.
[0005] Silicon is a promising alternative to graphite anodes in lithium-ion batteries due to its natural abundance, environmentally friendly properties, low discharge potential, and high theoretical capacity (4200mAh / g). However, the large volume change of silicon (300%-400%) has hindered the practical application of silicon-based anodes.
[0006] Research has found that the combination of silicon and carbon materials can effectively improve the shortcomings of silicon anodes. In Patent Document 1, nanosilicon and nanographite sheets are uniformly dispersed in water, then an organic carbon solution is added and spray-dried, and the resulting powder is calcined to obtain a silicon-carbon composite material. This material improves to some extent the problems of poor electrical conductivity and cycle stability of silicon, but the preparation method is compounded with carbon materials through physical mixing, and it is difficult to uniformly disperse silicon and carbon materials, which affects its electrochemical performance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Chinese Patent No. 108598389 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention provides a multi-layer composite material for lithium ion secondary batteries and its preparation method and application. The multi-layer composite material for lithium ion secondary batteries of the present invention has a stable structure, and compared with conventional silicon-based materials, the interaction between the multi-layer structure and the composite material allows the material to have smaller volume expansion, and better cycle characteristics and rate characteristics. [Means for solving the problem]
[0009] In a first aspect, an embodiment of the present invention provides a multi-layer composite material for a lithium ion secondary battery, the multi-layer composite material comprising a carbon matrix, a nano silicon based composite material, and a carbon shell; the carbon matrix is a matrix material for depositing a nano silicon based composite material; The nanosilicon-based composite material is prepared by vapor deposition of silane and one or more gaseous compounds containing any one of C, N, B, and P elements, the particle size of the nanosilicon-based composite material is 0.1 to 200 nm, the carbon atoms in the nanosilicon-based composite material are uniformly embedded on an atomic scale, the carbon atoms and silicon atoms are bonded to form amorphous Si-C bonds, the nitrogen atoms and silicon atoms are bonded to form amorphous Si-N bonds, and defects are generated in the silicon crystals in the nanosilicon-based composite material by boron doping and / or phosphorus doping, The carbon shell is coated with an outer layer of a carbon matrix onto which a nano silicon based composite material is deposited.
[0010] Preferably, the carbon shell is prepared by vapor, liquid or solid phase coating.
[0011] Preferably, when the multilayer composite material contains C element, the solid-state nuclear magnetic resonance NMR spectrum of the multilayer composite material shows that, when the silicon peak is at -70 ppm to -130 ppm, the Si-C resonance peak is present between 20 ppm to -20 ppm, and the area ratio of the Si-C resonance peak to the silicon peak is 0.1 to 5.0.
[0012] Preferably, in the multilayer composite material, the mass of the nanosilicon-based composite material accounts for 20% to 80% of the total mass, and the mass of any of the C, N, B, and P elements composited with silicon accounts for 0.1% to 50% of the mass of the nanosilicon-based composite material; The mass of the carbon matrix accounts for 20% to 70% of the total mass, The mass of the carbon shell accounts for 0 to 10% of the total mass.
[0013] In a second aspect, an embodiment of the present invention provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery according to the first aspect, the method comprising: introducing a protective gas, which is nitrogen gas, argon gas, hydrogen gas or any mixture thereof, into a reaction vessel filled with a carbon matrix at a flow rate of 1 to 2 L / min; introducing silane and one or more gaseous compounds containing any one of C, N, B, and P elements into a reaction vessel and performing vapor deposition on the carbon matrix; providing a carbon coating on the deposited product by at least one of vapor coating, liquid coating, and solid coating to obtain the multilayer composite material for lithium ion secondary batteries; Including, Here, the gas flow rate of silane is 0.5-10 L / min, the gas flow rate of the gaseous compound is 0.5-10 L / min, the deposition temperature is 500-1500° C., and the deposition time is 1-20 hours.
[0014] Preferably, the reaction vessel comprises a batch reactor or a continuous type reactor, specifically comprising either a rotary furnace, a tubular furnace, a bell furnace or a fluidized bed.
[0015] Preferably, the silane comprises one or more of monosilane, disilane, tetrafluorosilane, chlorosilane, hexamethyldisilane, dimethylsiloxane.
[0016] Preferably, the gaseous compound containing a C element comprises one or more of acetylene, methane, propylene, ethylene, propane and gaseous ethanol; The gaseous compound containing an N element includes at least one of nitrogen, ammonia, urea, melamine, and hydrazine, The gaseous compound containing the B element includes one or more of diborane, trimethyl borate, tripropyl borate, and boron tribromide; The gaseous compound containing the element P includes phosphine and / or phosphorus oxychloride.
[0017] In a third aspect, an embodiment of the present invention provides an anode material for a lithium-ion secondary battery comprising the multilayer composite material according to the first aspect above.
[0018] In a fourth aspect, an embodiment of the present invention provides a lithium battery comprising the multilayer composite material for a lithium ion secondary battery according to the first aspect above. Effect of the Invention
[0019] The multilayer composite material for lithium ion secondary batteries according to the embodiment of the present invention has the characteristics of small volume expansion and excellent cycle characteristics and rate characteristics due to the interaction between the three-layer structure of the carbon matrix, the nanosilicon-based composite material, and the carbon shell and the composite material. In particular, the nanosilicon-based composite material prepared by vapor deposition of silane and one or more gaseous compounds containing any of the elements C, N, B, and P has carbon atoms embedded uniformly on an atomic scale, and carbon atoms and silicon atoms bond to form amorphous Si-C bonds, which makes the structure of the material more stable during the lithium insertion and desorption process, reduces volume expansion, and has better cycle characteristics when used in the negative electrode of a lithium battery. Nitrogen atoms and silicon atoms bond to form amorphous Si-N bonds, which are favorable for the insertion and desorption of lithium ions, and improve the rate characteristics of the lithium ion battery. Boron doping and / or phosphorus doping form defects in the silicon crystals in the nanosilicon-based composite material, which reduces volume expansion during charging and improves the cycle characteristics of the battery. [Brief description of the drawings]
[0020] Hereinafter, the technical solutions in the embodiments of the present invention will be described in more detail with reference to the drawings and examples.
[0021] [Figure 1] FIG. 1 is a schematic diagram of a multilayer composite material for a lithium ion secondary battery according to an embodiment of the present invention. [Diagram 2] 1 is a flow chart of a method for preparing a multi-layer composite material for a lithium-ion secondary battery according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a diagram showing a solid-state nuclear magnetic resonance (NMR) spectrum of the multilayer composite material according to Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The present invention will be further described below with reference to the drawings and specific examples. However, it should be understood that these examples are merely for the purpose of explaining the present invention in more detail and are not intended to limit the present invention in any manner, i.e., they are not intended to limit the scope of protection of the present invention.
[0023] The present invention proposes a multi-layer composite material for lithium ion secondary batteries, and Fig. 1 is a schematic diagram of a multi-layer composite material according to an embodiment of the present invention. As shown in Fig. 1, the multi-layer composite material includes a carbon matrix, a nano silicon-based composite material, and a carbon shell, The carbon matrix is a matrix material for depositing the nano silicon-based composite material, and may specifically include one or more of porous activated carbon, carbon nanotubes, carbon fibers, and mesocarbon microbeads; The nanosilicon-based composite material is prepared by vapor deposition of silane and one or more gaseous compounds containing any of the elements C, N, B, and P. The particle size of the nanosilicon-based composite material is 0.1 to 200 nm. The carbon atoms in the nanosilicon-based composite material are uniformly embedded on an atomic scale, the carbon atoms and the silicon atoms are bonded to form amorphous Si-C bonds, the nitrogen atoms and the silicon atoms are bonded to form amorphous Si-N bonds, and defects are generated in the silicon crystals in the nanosilicon-based composite material by boron doping and / or phosphorus doping. The carbon shell is coated on the outer layer of the carbon matrix on which the nanosilicon based composite is deposited. The carbon shell is specifically prepared by vapor, liquid or solid phase coating.
[0024] When the multi-layer composite material contains C element, the NMR spectrum of the solid-state nuclear magnetic resonance of the multi-layer composite material shows that, when the silicon peak is at -70 ppm to -130 ppm, there is a Si-C resonance peak between 20 ppm to -20 ppm, and the area ratio of the Si-C resonance peak to the silicon peak is 0.1 to 5.0.
[0025] In the multilayer composite material, the mass of the nanosilicon-based composite material accounts for 20% to 80% of the total mass, the mass of any of the C, N, B, and P elements composited with silicon accounts for 0.1% to 50% of the mass of the nanosilicon-based composite material, the mass of the carbon matrix accounts for 20% to 70% of the total mass, and the mass of the carbon shell accounts for 0 to 10% of the total mass.
[0026] The material of the present invention is prepared according to the preparation method flow chart shown in Figure 2. As shown in Figure 2, it mainly includes the following steps: In step 110, a protective gas is introduced into the reaction vessel filled with the carbon matrix at a flow rate of 1 to 2 L / min; Specifically, the reaction vessel includes a batch reactor or a continuous reactor, specifically including a rotary furnace, a tubular furnace, a bell-type furnace, or a fluidized bed. The protective gas introduced is nitrogen gas, argon gas, hydrogen gas, or a mixture of any two or three of these gases.
[0027] In step 120, silane and one or more gaseous compounds containing any of the elements C, N, B, and P are introduced into the reaction vessel and vapor-deposited onto the carbon matrix; Here, the silane includes one or more of monosilane, disilane, tetrafluorosilane, chlorosilane, hexamethyldisilane, and dimethylsiloxane.
[0028] The gaseous compound containing a C element includes one or more of acetylene, methane, propylene, ethylene, propane, and gaseous ethanol; The gaseous compound containing an N element includes at least one of nitrogen, ammonia, urea, melamine, and hydrazine, The gaseous compound containing the B element includes one or more of diborane, trimethyl borate, tripropyl borate, and boron tribromide; The gaseous compound containing the element P includes phosphine and / or phosphorus oxychloride.
[0029] In the case where the compounds containing the above elements N, B, and P are themselves liquid or solid at room temperature and pressure, the gaseous compounds are formed by transporting a solution of the above elemental compounds using a carrier gas, and are then transported into a reaction vessel.
[0030] The gas flow rate of silane is 0.5-10 L / min, the gas flow rate of the gaseous compound is 0.5-10 L / min, the deposition temperature is 500-1500° C., and the deposition time is 1-20 hours.
[0031] In step 130, the deposited product is carbon-coated by at least one of vapor, liquid, and solid phase coating to obtain a multi-layer composite material for lithium-ion secondary batteries.
[0032] Gas phase coating, liquid phase coating, and solid phase coating are all commonly used coating methods in the industry, and those skilled in the art already know how to use the above methods to achieve carbon coating, so detailed descriptions thereof are omitted here.
[0033] The multilayer composite material for lithium ion secondary batteries proposed in the present invention is used as a negative electrode material for lithium ion batteries and is applied to lithium ion batteries.
[0034] The multilayer composite material for lithium ion secondary batteries according to the embodiment of the present invention has the characteristics of small volume expansion and excellent cycle characteristics and rate characteristics due to the interaction between the three-layer structure of the carbon matrix, the nanosilicon-based composite material, and the carbon shell and the composite material. In particular, the nanosilicon-based composite material prepared by vapor deposition of silane and one or more gaseous compounds containing any of the elements C, N, B, and P has carbon atoms embedded uniformly on an atomic scale, and carbon atoms and silicon atoms bond to form amorphous Si-C bonds, which makes the structure of the material more stable during the lithium insertion and desorption process, reduces volume expansion, and has better cycle characteristics when used in the negative electrode of a lithium battery. Nitrogen atoms and silicon atoms bond to form amorphous Si-N bonds, which are favorable for the insertion and desorption of lithium ions, and improve the rate characteristics of the lithium ion battery. Boron doping and / or phosphorus doping form defects in the silicon crystals in the nanosilicon-based composite material, which reduces volume expansion during charging and improves the cycle characteristics of the battery.
[0035] In order to better understand the technical solution of the present invention, several specific examples are given below to describe the specific process of preparing a multi-layer composite material using the method according to the above embodiment of the present invention, and the application method and battery characteristics thereof in a lithium ion secondary battery.
[0036] [Example 1] This embodiment provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery, which includes the following steps: (1) Nitrogen gas is introduced at a flow rate of 1 L / min as a protective gas for silane deposition into a rotary furnace, which is a reaction vessel filled with a carbon matrix. (2) Monosilane and methane, a compound containing C element, are introduced in gas form into a reaction vessel and vapor-phase deposition is performed on a carbon matrix. The gas flow rate of monosilane is 0.5 L / min, the gas flow rate of methane is 0.5 L / min, the deposition temperature is 500 °C, and the deposition time is 20 hours. (3) A carbon coating is applied to the deposited product by vapor phase coating to obtain a multilayer composite material for lithium-ion secondary batteries.
[0037] [Example 2] This embodiment provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery, which includes the following steps: (1) Argon gas is introduced at a flow rate of 1.5 L / min as a protective gas for silane deposition into a tubular furnace, which is a reaction vessel filled with a carbon matrix. (2) Disilane and ammonia, a compound containing N element, are introduced in gas form into a reaction vessel and vapor-phase deposition is performed on a carbon matrix. The gas flow rate of disilane is 0.8 L / min, the gas flow rate of ammonia is 0.8 L / min, the deposition temperature is 600 °C, and the deposition time is 12.5 hours. (3) A carbon coating is applied to the deposited product by liquid phase coating to obtain a multilayer composite material for lithium-ion secondary batteries.
[0038] [Example 3] This embodiment provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery, which includes the following steps: (1) Nitrogen gas is introduced at a flow rate of 2 L / min into a bell-type furnace, which is a reaction vessel filled with a carbon matrix, as a protective gas for silane deposition. (2) Tetrafluorosilane and tripropyl borate, a compound containing B element, are introduced into the reaction vessel in gas form and vapor-phase deposition is performed on the carbon matrix. The gas flow rates of tetrafluorosilane and tripropyl borate are 1 L / min, the deposition temperature is 700 °C, and the deposition time is 10 h. (3) A carbon coating is applied to the deposited product by solid-phase coating to obtain a multilayer composite material for lithium-ion secondary batteries.
[0039] [Example 4] This embodiment provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery, which includes the following steps: (1) Argon gas is introduced at a flow rate of 2 L / min as a protective gas for silane deposition into a fluidized bed, which is a reaction vessel filled with a carbon matrix. (2) Chlorosilanes and phosphorus oxychloride, a compound containing P element, are introduced into the reaction vessel in gas form and vapor-phase deposition is carried out on the carbon matrix. The gas flow rate of chlorosilane is 1.25 L / min, the gas flow rate of phosphorus oxychloride gaseous compound is 1.25 L / min, the deposition temperature is 800 °C, and the deposition time is 8 hours. (3) A carbon coating is applied to the deposited product by vapor phase coating to obtain a multilayer composite material for lithium-ion secondary batteries.
[0040] [Example 5] This embodiment provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery, which includes the following steps: (1) Argon gas is introduced at a flow rate of 1.5 L / min as a protective gas for silane deposition into a tubular furnace, which is a reaction vessel filled with a carbon matrix. (2) Disilane and gaseous compounds containing C, N, B and P elements, methane, ammonia, trimethyl borate and phosphorus oxychloride, are introduced in gas form into a reaction vessel and vapor-phase deposition is performed on a carbon matrix. The gas flow rate of disilane is 0.8 L / min, the gas flow rates of methane, ammonia, trimethyl borate and phosphorus oxychloride gaseous compounds are all 0.2 L / min, the deposition temperature is 600°C and the deposition time is 12.5 hours. (3) A carbon coating is applied to the deposited product by liquid phase coating to obtain a multilayer composite material for lithium-ion secondary batteries.
[0041] [Example 6] This embodiment provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery, which includes the following steps: (1) Nitrogen gas is introduced at a flow rate of 2 L / min into a bell-type furnace, which is a reaction vessel filled with a carbon matrix, as a protective gas for silane deposition. (2) Tetrafluorosilane and gaseous compounds containing C, N, B and P elements, propylene, urea, tripropyl borate and phosphine, are introduced in gas form into a reaction vessel and vapor-phase deposition is performed on a carbon matrix. The gas flow rate of tetrafluorosilane is 1 L / min, the gas flow rates of propylene, urea, tripropyl borate and phosphine gaseous compounds are all 0.25 L / min, the deposition temperature is 700°C and the deposition time is 10 hours. (3) A carbon coating is applied to the deposited product by solid-phase coating to obtain a multilayer composite material for lithium-ion secondary batteries.
[0042] [Example 7] This embodiment provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery, which includes the following steps: (1) Nitrogen gas is introduced at a flow rate of 2 L / min as a protective gas for silane deposition into a rotary furnace, which is a reaction vessel filled with a carbon matrix. (2) Hexamethyldisilane and compounds containing C, N, B and P elements, propane, hydrazine, diborane and phosphine, are introduced in gas form into a reaction vessel and vapor-phase deposition is performed on a carbon matrix. The gas flow rate of hexamethyldisilane is 2 L / min, the gas flow rates of propane, hydrazine, diborane and phosphine are all 0.5 L / min, the deposition temperature is 900°C and the deposition time is 5 hours. (3) A carbon coating is applied to the deposited product by liquid phase coating to obtain a multilayer composite material for lithium-ion secondary batteries.
[0043] [Example 8] This embodiment provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery, which includes the following steps: (1) Argon gas is introduced at a flow rate of 2 L / min as a protective gas for silane deposition into a tubular furnace, which is a reaction vessel filled with a carbon matrix. (2) Monosilane, disilane, ethanol, which is a compound containing C, N, B and P elements, nitrogen gas, trimethyl borate and phosphorus oxychloride are introduced in gas form into a reaction vessel and vapor-phase deposition is performed on a carbon matrix. The gas flow rates of monosilane and disilane are both 1.2 L / min, the gas flow rates of ethanol, nitrogen gas, trimethyl borate and phosphorus oxychloride gaseous compounds are 0.6 L / min, the deposition temperature is 1000°C, and the deposition time is 4 hours. (3) A carbon coating is applied to the deposited product by solid-phase coating to obtain a multilayer composite material for lithium-ion secondary batteries.
[0044] [Example 9] This embodiment provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery, which includes the following steps: (1) Nitrogen gas is introduced at a flow rate of 2 L / min into a bell-type furnace, which is a reaction vessel filled with a carbon matrix, as a protective gas for silane deposition. (2) Monosilane, disilane, tetrafluorosilane, acetylene, methane, nitrogen gas, ammonia, diborane, trimethyl borate, phosphine, and phosphorus oxychloride, which are compounds containing the elements C, N, B, and P, are introduced into a reaction vessel in the form of gas, and vapor-phase deposition is performed on a carbon matrix. The gas flow rates of monosilane, disilane, and tetrafluorosilane are 1.3 L / min, and the gas flow rates of acetylene, methane, nitrogen gas, ammonia, diborane, trimethyl borate, phosphine, and phosphorus oxychloride gaseous compounds are all 0.5 L / min, the deposition temperature is 1100°C, and the deposition time is 2.5 hours. (3) A carbon coating is applied to the deposited product by vapor phase coating to obtain a multilayer composite material for lithium-ion secondary batteries.
[0045] [Example 10] This embodiment provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery, which includes the following steps: (1) Argon gas is introduced at a flow rate of 2 L / min as a protective gas for silane deposition into a fluidized bed, which is a reaction vessel filled with a carbon matrix. (2) Monosilane, disilane, hexamethyldisilane, methane, propylene, ammonia, urea, trimethyl borate, boric acid, phosphine and phosphorus oxychloride, which are compounds containing the elements C, N, B and P, are introduced into a reaction vessel in the form of gas and vapor-phase deposited on a carbon matrix. The gas flow rates of monosilane, disilane and tetrafluorosilane are 1.7 L / min, and the gas flow rates of methane, propylene, ammonia, urea, trimethyl borate, boric acid, phosphine and phosphorus oxychloride gaseous compounds are all 0.6 L / min, the deposition temperature is 1200°C and the deposition time is 2 hours. (3) A carbon coating is applied to the deposited product by liquid phase coating to obtain a multilayer composite material for lithium-ion secondary batteries.
[0046] [Example 11] This embodiment provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery, which includes the following steps: (1) Nitrogen gas is introduced at a flow rate of 2 L / min as a protective gas for silane deposition into a rotary furnace, which is a reaction vessel filled with a carbon matrix. (2) Monosilane, disilane, dimethylsiloxane, ethylene, propane, urea, melamine, tripropyl borate, boron tribromide, phosphine, and phosphorus oxychloride, which are compounds containing the elements C, N, B, and P, are introduced into a reaction vessel in the form of gas and vapor-phase deposited on a carbon matrix. The gas flow rates of monosilane, disilane, and dimethylsiloxane are all 2.7 L / min, and the gas flow rates of ethylene, propane, urea, melamine, tripropyl borate, boron tribromide, phosphine, and phosphorus oxychloride gaseous compounds are all 1 L / min, the deposition temperature is 1400°C, and the deposition time is 1.25 hours. (3) A carbon coating is applied to the deposited product by solid-phase coating to obtain a multilayer composite material for lithium-ion secondary batteries.
[0047] [Example 12] This embodiment provides a method for preparing a multi-layer composite material for a lithium-ion secondary battery, which includes the following steps: (1) Argon gas is introduced at a flow rate of 2 L / min as a protective gas for silane deposition into a tubular furnace, which is a reaction vessel filled with a carbon matrix. (2) Monosilane, disilane, tetrafluorosilane, hexamethyldisilane, acetylene, propane, ammonia, hydrazine, tripropyl borate, boron tribromide, phosphine and phosphorus oxychloride, which are compounds containing the elements C, N, B and P, are introduced into a reaction vessel in the form of gas and vapor-phase deposited on a carbon matrix. The gas flow rates of monosilane, disilane, tetrafluorosilane and hexamethyldisilane are all 2.5L / min, the gas flow rates of acetylene, propane, ammonia, hydrazine, tripropyl borate, boron tribromide, phosphine and phosphorus oxychloride gaseous compounds are all 1L / min, the deposition temperature is 1500°C and the deposition time is 1 hour. (3) A carbon coating is applied to the deposited product by vapor phase coating to obtain a multilayer composite material for lithium-ion secondary batteries.
[0048] [Comparative Example 1] This comparative example provides a method for preparing a silicon-carbon composite material based on the prior art, which includes the following steps: (1) Silicon particles, polyvinylpyrrolidone as a precursor of the carbon source, graphite, and citric acid as an antioxidant are added to an ethanol system, and ground in a mass ratio of 1:1:1:0.1 to obtain a dispersion. (2) The dispersion is spray-dried to obtain silicon-carbon powder. (3) The powder is then vapor-coated to finally obtain a silicon-carbon composite material.
[0049] The composite materials obtained in the above examples and comparative examples were combined with commercially available graphite in proportion to produce a composite material of 450 mAh / g, which was then assembled with lithium cobalt oxide into a button-type all-solid-state battery, which was then cycled at a 1C rate to evaluate its cycle characteristics. The data are shown in Table 1.
[0050] [Table 1]
[0051] As can be seen from the results in Table 1, in the comparative example, the silicon-carbon composite material prepared by mechanical mixing has high coulombic efficiency in the first cycle but poor cycle performance, while the multilayer composite material of the present invention has better cycle performance.
[0052] The present invention can further improve the first cycle coulombic efficiency and cycle performance of the material by adjusting the deposition time, temperature and gas flow rate. If the gas flow rate and temperature are too high, the decomposition of silane is too fast, and it is deposited directly on the surface of the carbon matrix, and the deposited silicon is not uniformly combined with the elements C, N, B and P, which affects the performance of the battery. If the temperature is too low, the decomposition of silane is incomplete, and it cannot be combined well with the elements C, N, B and P, which affects the cycle performance.
[0053] The multilayer composite material for lithium ion secondary batteries according to the embodiment of the present invention has the characteristics of small volume expansion and excellent cycle characteristics and rate characteristics due to the interaction between the three-layer structure of the carbon matrix, the nanosilicon-based composite material, and the carbon shell and the composite material. In particular, the nanosilicon-based composite material prepared by vapor deposition of silane and one or more gaseous compounds containing any of the elements C, N, B, and P has carbon atoms embedded uniformly on an atomic scale, and carbon atoms and silicon atoms bond to form amorphous Si-C bonds, which makes the structure of the material more stable during the lithium insertion and desorption process, reduces volume expansion, and has better cycle characteristics when used in the negative electrode of a lithium battery. Nitrogen atoms and silicon atoms bond to form amorphous Si-N bonds, which are favorable for the insertion and desorption of lithium ions, and improve the rate characteristics of the lithium ion battery. Boron doping and / or phosphorus doping form defects in the silicon crystals in the nanosilicon-based composite material, which reduces volume expansion during charging and improves the cycle characteristics of the battery.
[0054] The above specific embodiments further describe the objectives, technical solutions and beneficial effects of the present invention. The above are only specific embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
[0055] (Additional Note) (Appendix 1) A multilayer composite material for a lithium ion secondary battery, comprising: The multi-layer composite material includes a carbon matrix, a nano silicon based composite material, and a carbon shell; the carbon matrix is a matrix material for depositing a nano silicon based composite material; The nanosilicon-based composite material is prepared by vapor deposition of silane and one or more gaseous compounds containing any one of C, N, B, and P elements, the particle size of the nanosilicon-based composite material is 0.1 to 200 nm, the carbon atoms in the nanosilicon-based composite material are uniformly embedded on an atomic scale, the carbon atoms and silicon atoms are bonded to form amorphous Si-C bonds, the nitrogen atoms and silicon atoms are bonded to form amorphous Si-N bonds, and defects are generated in the silicon crystals in the nanosilicon-based composite material by boron doping and / or phosphorus doping, The carbon shell is coated with an outer layer of a carbon matrix on which a nano silicon based composite material is deposited. A multilayer composite material for a lithium ion secondary battery, comprising:
[0056] (Appendix 2) The carbon shell is prepared by vapor phase coating, liquid phase coating or solid phase coating. 2. The multilayer composite material for a lithium ion secondary battery according to claim 1,
[0057] (Appendix 3) When the multilayer composite material contains C element, the NMR spectrum of the solid-state nuclear magnetic resonance of the multilayer composite material shows that when the silicon peak is at -70 ppm to -130 ppm, the Si-C resonance peak is present between 20 ppm to -20 ppm, and the area ratio of the Si-C resonance peak to the silicon peak is 0.1 to 5.0; 2. The multilayer composite material for a lithium ion secondary battery according to claim 1,
[0058] (Appendix 4) In the multilayer composite material, the mass of the nanosilicon-based composite material accounts for 20% to 80% of the total mass, and the mass of any of the C, N, B, and P elements composited with silicon accounts for 0.1% to 50% of the mass of the nanosilicon-based composite material; The mass of the carbon matrix accounts for 20% to 70% of the total mass, The mass of the carbon shell accounts for 0 to 10% of the total mass. 2. The multilayer composite material for a lithium ion secondary battery according to claim 1,
[0059] (Appendix 5) A method for preparing a multilayer composite material for a lithium ion secondary battery according to any one of claims 1 to 4, comprising the steps of: introducing a protective gas, which is nitrogen gas, argon gas, hydrogen gas or any mixture thereof, into a reaction vessel filled with a carbon matrix at a flow rate of 1 to 2 L / min; introducing silane and one or more gaseous compounds containing any one of C, N, B, and P elements into a reaction vessel and performing vapor deposition on the carbon matrix; providing a carbon coating on the deposited product by at least one of vapor coating, liquid coating, and solid coating to obtain the multilayer composite material for lithium ion secondary batteries; Including, Wherein, the gas flow rate of silane is 0.5-10 L / min, the gas flow rate of the gaseous compound is 0.5-10 L / min, the deposition temperature is 500-1500° C., and the deposition time is 1-20 hours; A preparation method comprising the steps of:
[0060] (Appendix 6) The reaction vessel may be a batch reactor or a continuous reactor, specifically a rotary furnace, a tubular furnace, a bell furnace or a fluidized bed. The preparation method according to claim 5,
[0061] (Appendix 7) The silane includes one or more of monosilane, disilane, tetrafluorosilane, chlorosilane, hexamethyldisilane, and dimethylsiloxane; The preparation method according to claim 5,
[0062] (Appendix 8) The gaseous compound containing a C element includes one or more of acetylene, methane, propylene, ethylene, propane, and gaseous ethanol; The gaseous compound containing an N element includes at least one of nitrogen, ammonia, urea, melamine, and hydrazine, The gaseous compound containing the B element includes one or more of diborane, trimethyl borate, tripropyl borate, and boron tribromide; The gaseous compound containing the P element includes phosphine and / or phosphorus oxychloride. The preparation method according to claim 5,
[0063] (Appendix 9) The multilayer composite material for a lithium ion secondary battery according to any one of claims 1 to 5 is included. A negative electrode material characterized by:
[0064] (Appendix 10) The multilayer composite material for a lithium ion secondary battery according to any one of claims 1 to 5 is included. A lithium-ion battery characterized by:
Claims
1. A multilayer composite material for a lithium ion secondary battery, comprising: The multi-layer composite material includes a carbon matrix, a nano silicon based composite material, and a carbon shell; the carbon matrix is a matrix material for depositing a nano silicon based composite material; The nanosilicon-based composite material is prepared by vapor deposition of silane and one or more gaseous compounds containing any one of C, N, B, and P elements, the particle size of the nanosilicon-based composite material is 0.1 to 200 nm, the carbon atoms in the nanosilicon-based composite material are uniformly embedded on an atomic scale, the carbon atoms and silicon atoms are bonded to form amorphous Si-C bonds, the nitrogen atoms and silicon atoms are bonded to form amorphous Si-N bonds, and defects are generated in the silicon crystals in the nanosilicon-based composite material by boron doping and / or phosphorus doping, The carbon shell is coated with an outer layer of a carbon matrix on which a nano silicon based composite material is deposited. A multilayer composite material for a lithium ion secondary battery, comprising:
2. The carbon shell is prepared by vapor phase coating, liquid phase coating or solid phase coating. The multilayer composite material for a lithium ion secondary battery according to claim 1 .
3. When the multilayer composite material contains C element, the solid-state nuclear magnetic resonance NMR spectrum of the multilayer composite material shows that when the silicon peak is at -70 ppm to -130 ppm, the Si-C resonance peak is present between 20 ppm and -20 ppm, and the area ratio of the Si-C resonance peak to the silicon peak is 0.1 to 5.0; The multilayer composite material for a lithium ion secondary battery according to claim 1 .
4. In the multilayer composite material, the mass of the nano silicon-based composite material accounts for 20% to 80% of the total mass, and the mass of any of the C, N, B, and P elements composited with silicon accounts for 0.1% to 50% of the mass of the nano silicon-based composite material; The mass of the carbon matrix accounts for 20% to 70% of the total mass; The mass of the carbon shell accounts for 0 to 10% of the total mass. The multilayer composite material for a lithium ion secondary battery according to claim 1 .
5. A method for preparing the multilayer composite material for a lithium ion secondary battery according to any one of claims 1 to 4, comprising the steps of: introducing a protective gas, which may be nitrogen gas, argon gas, hydrogen gas, or any mixture thereof, into a reaction vessel filled with a carbon matrix at a flow rate of 1 to 2 L / min; introducing silane and one or more gaseous compounds containing any one of C, N, B, and P elements into a reaction vessel and performing vapor deposition on the carbon matrix; providing a carbon coating on the deposited product by at least one of vapor, liquid and solid coating to obtain the multilayer composite material for lithium ion secondary batteries; Including, Wherein, the gas flow rate of silane is 0.5-10 L / min, the gas flow rate of the gaseous compound is 0.5-10 L / min, the temperature of the deposition is 500-1500° C., and the deposition time is 1-20 hours; A preparation method comprising the steps of:
6. The reaction vessel may be a batch reactor or a continuous reactor, specifically a rotary furnace, a tubular furnace, a bell furnace or a fluidized bed.
6. The method according to claim 5 .
7. The silane includes one or more of monosilane, disilane, tetrafluorosilane, chlorosilane, hexamethyldisilane, and dimethylsiloxane; 6. The method according to claim 5 .
8. The gaseous compound containing a C element includes one or more of acetylene, methane, propylene, ethylene, propane, and gaseous ethanol; The gaseous compound containing an N element includes at least one of nitrogen, ammonia, urea, melamine, and hydrazine; The gaseous compound containing the B element includes one or more of diborane, trimethyl borate, tripropyl borate, and boron tribromide; The gaseous compound containing the P element includes phosphine and / or phosphorus oxychloride.
6. The method according to claim 5 .
9. The multilayer composite material for a lithium ion secondary battery according to any one of claims 1 to 5 is included. A negative electrode material characterized by:
10. The multilayer composite material for a lithium ion secondary battery according to any one of claims 1 to 5 is included. A lithium-ion battery characterized by:
Citation Information
Patent Citations
Negative electrode active material, method for producing same, and lithium secondary battery having negative electrode including same
WO2020036397A1
Lithium ion battery silicon carbon cathode material, preparation method and application thereof