Method for manufacturing positive electrode active material for lithium secondary battery and positive electrode active material manufactured by the same

A niobium-based compound coating on the positive electrode active material, combined with compression filtration, addresses the non-uniformity issues in all-solid-state batteries, enhancing performance by reducing resistance and improving charge/discharge efficiency and life.

JP2024541725AInactive Publication Date: 2024-11-11LG ENERGY SOLUTION LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024529875
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-30
Filing Date
2023-08-23
Publication Date
2024-11-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

All-solid-state batteries face issues with uneven deposition and non-uniform distribution of the positive electrode, leading to increased electrical resistance, reduced energy density, and accelerated deterioration due to insufficient formation of triple points and interfaces between the active material, solid electrolyte, and conductive material.

Method used

A method involving the use of a niobium-based compound coating on the positive electrode active material surface, facilitated by a hydrophilic functional group introduced via an aqueous solvent, followed by compression filtration to remove residual solvent, ensuring uniform coating and reduced reactivity with sulfide-based solid electrolytes.

Benefits of technology

The method enhances the uniformity of the electrode layer, reduces electrical resistance, and improves the charge/discharge efficiency and life characteristics of all-solid-state batteries by minimizing side reactions and ensuring optimal ion conduction paths.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541725000001_ABST
    Figure 2024541725000001_ABST
Patent Text Reader

Abstract

The present invention relates to a method for producing a positive electrode active material for a lithium secondary battery, the method including: (a) mixing a positive electrode active material capable of reversibly absorbing and releasing lithium ions with a solvent to produce a positive electrode active material dispersion; (b) adding and mixing raw materials for a coating material containing lithium (Li) and niobium (Nb) to produce a coating liquid containing a niobium-based compound; (c) adding the coating liquid of step (b) to the positive electrode active material dispersion of step (a) to form a coating layer on the surface of the positive electrode active material; and (d) squeezing and filtering the product of step (c) to remove the solvent; and to a positive electrode active material for a lithium secondary battery produced thereby.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0125099 filed on September 30, 2022, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a method for producing a positive electrode active material for a lithium secondary battery and a positive electrode active material produced thereby. [Background technology]

[0003] Lithium-ion secondary batteries, which have high energy density, low self-discharge rate, and long lifespan, are suitable for meeting the demand for high-capacity batteries. However, because lithium-ion secondary batteries have a structure in which the negative and positive electrodes are separated by a separator, if the separator is damaged due to deformation or external impact, a short circuit may occur, which causes stability problems against overheating, and research to improve this problem is steadily progressing.

[0004] All-solid-state batteries have been proposed as a solution to overcome the safety issues of lithium-ion secondary batteries. Unlike conventional batteries that use liquid electrolytes, all-solid-state batteries have an electrolyte layer containing a solid electrolyte. The solid electrolyte of the all-solid-state battery may have a positive electrode layer and a negative electrode layer containing a solid electrolyte on both sides. Each electrode of the all-solid-state battery may be bonded to a current collector.

[0005] Since solid-state batteries use solid electrolytes instead of liquid electrolytes, there is very little risk of liquid evaporation due to temperature changes or electrolyte leakage due to external impacts. Therefore, they have the advantage of being safe from explosions and fires. Solid-state batteries also reduce weight and volume because they do not require parts to prevent leakage or explosion.

[0006] All-solid-state batteries are classified into oxide-based, polymer-based, and sulfide-based batteries according to the raw materials of the solid electrolyte. Of these, sulfide-based all-solid-state batteries have a high lithium ion conductivity (10 -2S / cm) compared to other batteries and has excellent temperature stability, so it is attracting a lot of attention.

[0007] The method for manufacturing the positive and negative electrodes of solid-state batteries is similar to that for manufacturing the positive and negative electrodes of conventional lithium-ion batteries. Active material, conductive material, and binder solid particles are mixed with a solvent in a certain ratio to produce a mixture slurry with low fluidity, which is then coated onto a metal current collector as a thin film, and then dried and pressed. In solid-state batteries, a solid electrolyte is mixed in during the slurry production step.

[0008] Compared to liquid electrolytes, it is not easy for solid electrolytes to form an interface with active materials. The binder prevents the formation of an interface between the active material and solid electrolyte, resulting in a large increase in electrical resistance. This causes the problem of a drop in output. Even if a material with high ionic conductivity is used as the solid electrolyte, the crystallized solid electrolyte must be pulverized into fine particles in order to mix it with the electrode slurry. In addition, because it is mixed with a solvent, the problem of reduced conductivity occurs due to material constraints rather than the inherent properties of the material. The ionic conductivity (10 -5 S / cm~10 -2 S / cm) is the ionic conductivity of a battery that uses a liquid electrolyte (10 -2 It is known that the ion exchange rate is lower than that of the conventional ion exchange rate (S / cm).

[0009] It is presumed that the low ionic conductivity of all-solid-state batteries is due to the inability to form triple junctions in the electrodes. Since the triple junctions are the points where electrochemical reactions occur in the electrodes, it is desirable to form many triple junctions in the electrodes to allow many electrochemical reactions to occur.

[0010] When electrode active material, solid electrolyte, conductive material, and binder are mixed together to prepare a slurry, the active material may be isolated by the conductive material (dead active material) in the electrode structure, or the solid electrolyte may be isolated by the active material (dead solid electrolyte). When an isolated solid electrolyte occurs, the active material and solid electrolyte are wasted. In addition, the migration path of lithium ions is blocked, which causes an additional problem of reduced energy density.

[0011] Among the methods for manufacturing solid-state batteries, a method is known in which the powders constituting the battery are sequentially placed in a cylindrical mold, pressurized, and current collectors are bonded onto the positive and negative electrodes. This method does not allow the positive electrode (layer) to be uniformly deposited on the electrolyte layer. This method does not allow the formation of a uniform current distribution in the positive electrode, which may cause deviations in current density and lead to deterioration of battery performance.

[0012] In addition to uneven deposition of the positive electrode, uneven distribution of the composition within the positive electrode can also be problematic. Uneven distribution of the positive electrode composition can lead to localized overcharging of the electrode, degradation of the active material, and dendrite growth of lithium metal, which accelerates the degradation of the charge-discharge life of the battery.

[0013] In the end, when manufacturing an all-solid-state battery, it is necessary to increase the number of contact interfaces between the active material, solid electrolyte, and conductive material to ensure optimal ion conduction paths. It is also important to ensure that the electrode mixture is uniformly distributed on the current collector and that the materials in the electrode mixture are uniformly distributed. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] JP 2012-234648 A [Patent Document 2] Korean Patent Publication No. 2022-0045460 Summary of the Invention [Problem to be solved by the invention]

[0015] An object of the present invention is to provide a method for producing a positive electrode active material for a lithium secondary battery, which can uniformly and effectively introduce a coating layer containing a niobium-based compound onto the surface of the positive electrode active material.

[0016] Another object of the present invention is to provide a positive electrode active material for a lithium secondary battery produced by the above-mentioned production method. [Means for solving the problem]

[0017] One embodiment of the present invention provides a method for producing a positive electrode active material for a lithium secondary battery, the method including: (a) mixing a positive electrode active material capable of reversibly absorbing and releasing lithium ions with a solvent to produce a positive electrode active material dispersion; (b) introducing and mixing raw materials of a coating material containing lithium (Li) and niobium (Nb) to produce a coating liquid containing a niobium-based compound; (c) introducing the coating liquid of step (b) into the positive electrode active material dispersion of step (a) to form a coating layer on a surface of the positive electrode active material; and (d) squeezing and filtering the product of step (c) to remove the solvent.

[0018] The step (a) may include first mixing a positive electrode active material capable of reversibly absorbing and releasing lithium ions with an organic solvent, and then further adding an aqueous solvent to the mixture.

[0019] In the step (a), the aqueous solvent may be further added to introduce a hydrophilic functional group onto the surface of the positive electrode active material.

[0020] The positive electrode active material dispersion may contain 10 to 50% by weight of solids based on the total weight of the dispersion.

[0021] The surface coating layer of the positive electrode active material may contain 1.0 to 1.2 wt % of a niobium-based compound based on the total weight of the solid content in the positive electrode active material dispersion.

[0022] The aqueous solvent may be added in an amount of 1.2 to 1.4% by weight based on the total weight of the solid content in the positive electrode active material dispersion liquid.

[0023] The squeeze filtration may be carried out under a pressure of 0.3 to 0.5 MPa.

[0024] The coating layer may have a thickness of 10 to 30 nm.

[0025] The method may further include a step of drying the product from which the solvent has been removed at 80 to 120° C. after step (d).

[0026] Another embodiment of the present invention provides a positive electrode active material for a lithium secondary battery prepared by the above method. Effect of the Invention

[0027] An object of the present invention is to provide a method for producing a positive electrode active material for a lithium secondary battery, which can uniformly and effectively coat the surface of a positive electrode active material with a niobium-based compound by introducing a hydrophilic functional group via an aqueous solvent onto the surface of the positive electrode active material when forming a coating layer containing a niobium-based compound in order to reduce the reactivity between a sulfide-based solid electrolyte and a positive electrode active material in a lithium secondary battery, particularly an all-solid-state battery.

[0028] In addition, instead of removing the residual solvent using a conventional high temperature, the present invention removes the residual solvent by squeezing and filtering the cathode active material dispersion having the coating layer containing the niobium-based compound formed thereon, thereby solving the problem that the niobium-based compound is not introduced onto the surface of the cathode active material but is instead released, which is caused by removing the residual solvent using a conventional high temperature. [Brief description of the drawings]

[0029] [Figure 1] FIG. 2 is a view showing an SEM image of the positive electrode active material for a lithium secondary battery according to Example 1 of the present invention. [Diagram 2]FIG. 2 is a SEM image of a positive electrode active material for a lithium secondary battery according to Comparative Example 1 of the present invention. [Diagram 3] FIG. 4 is a SEM image of a positive electrode active material for a lithium secondary battery according to Comparative Example 3 of the present invention. [Figure 4] FIG. 13 is a SEM image of a positive electrode active material for a lithium secondary battery according to Comparative Example 7 of the present invention. [Diagram 5] FIG. 2 is a diagram showing an energy dispersive X-ray (EDX) image of the positive electrode active material of Example 1 of the present invention. [Figure 6] FIG. 2 is a diagram showing an energy dispersive X-ray (EDX) image of the positive electrode active material of Comparative Example 1 of the present invention. [Figure 7] FIG. 2 is a view showing a field emission transmission electron microscope (FE-TEM) image of the positive electrode active material of Example 1 of the present invention. [Figure 8] FIG. 2 is a view showing a field emission transmission electron microscope (FE-TEM) image of the positive electrode active material of Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Hereinafter, the embodiments of the present invention will be described in detail. Prior to this, the terms and words used in the present specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as being consistent with the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term to best describe his / her invention. Therefore, since the configurations described in the embodiments described in this specification are merely the most preferred embodiments of the present invention, and do not entirely represent the technical idea of ​​the present invention, it should be understood that there are various equivalents and modifications that can replace them at the time of this application.

[0031] Throughout the specification of this application, when a part is said to "comprise" a certain element, this means that it can further include other elements, rather than excluding other elements, unless specifically stated to the contrary.

[0032] The term "nano" as used herein means nanoscale, including sizes below 1 μm.

[0033] Hereinafter, a method for manufacturing a positive electrode active material for a lithium secondary battery according to an embodiment will be described.

[0034] The present invention relates to a method for producing a positive electrode active material for a lithium secondary battery, which is capable of uniformly and effectively coating the surface of the positive electrode active material with a niobium-based compound.

[0035] All-solid-state batteries, which have been developed to improve the stability problem of lithium-ion secondary batteries, include a positive electrode, a negative electrode, and a solid electrolyte, and a sulfide-based solid electrolyte, which has high lithium ion conductivity and excellent stability, is mainly used for the positive electrode.

[0036] The sulfide-based solid electrolyte and the positive electrode active material react with each other at the interface between them to generate a resistive material that hinders smooth operation of the all-solid-state battery, and the generated resistive material reduces the initial capacity and operation efficiency of the all-solid-state battery.

[0037] To solve these problems, research has been conducted to improve the performance of solid-state batteries by coating the positive electrode active material of solid-state batteries with lithium niobate (LiNbO3) and other materials to reduce their reactivity with sulfide-based solid electrolytes.

[0038] However, in the process of coating the positive electrode active material with lithium niobate or the like, a heat treatment is performed in a high temperature environment to evaporate the organic solvent contained in the coating solution. At this time, the lithium niobate or the like is not completely coated on the surface of the positive electrode active material, and instead, the surface is formed of free material, resulting in a problem of an uneven coating layer.

[0039] Therefore, the present inventors have found a method for producing a positive electrode active material for a lithium secondary battery, in which a coating layer containing a niobium-based compound is formed on the surface of the positive electrode active material in order to prevent a side reaction between the solid electrolyte of an all-solid-state battery, particularly a sulfide-based solid electrolyte, and the positive electrode active material, and by introducing an aqueous solvent to first introduce a hydrophilic functional group onto the surface of the positive electrode active material, the method can be used to uniformly and effectively coat the surface of the positive electrode active material with the niobium-based compound, thereby completing the present invention.

[0040] In addition, the present inventors have found that, instead of removing the residual solvent using high heat as in the conventional method, the residual solvent is removed by squeezing and filtering the cathode active material dispersion having the coating layer containing the niobium-based compound formed thereon, thereby solving the problem that the niobium-based compound is not introduced onto the surface of the cathode active material but is released when the residual solvent is removed using high heat as in the conventional method, and thus the present invention has been completed.

[0041] A method for manufacturing a positive electrode active material for a lithium secondary battery according to an embodiment of the present invention includes: (a) mixing a positive electrode active material capable of reversibly absorbing and releasing lithium ions with a solvent to prepare a positive electrode active material dispersion; (b) adding and mixing raw materials of a coating material containing lithium (Li) and niobium (Nb) to prepare a coating liquid containing a niobium-based compound; (c) adding the coating liquid of step (b) to the positive electrode active material dispersion of step (a) to form a coating layer on a surface of the positive electrode active material; and (d) squeezing and filtering the product of step (c) to remove the solvent.

[0042] First, a positive electrode active material capable of reversibly absorbing and releasing lithium ions and a solvent are mixed to prepare a positive electrode active material dispersion (step (a)).

[0043] The positive electrode active material capable of reversibly absorbing and releasing lithium ions may be used without limitation as long as it can be used as a positive electrode active material for lithium ion secondary batteries. For example, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2) or a compound substituted with one or more transition metals; 1+x Mn 2-x Lithium manganese oxides such as LiMnO4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, and Cu2V2O7; and the chemical formula LiNi 1-x M x Lithium nickel oxide represented by the formula (I) is represented by the formula (I) in which M is Co, Mn, Al, Cu, Fe, Mg, B or Ga, and at least one of the above elements is contained, and x is 0.01 to 0.3. 0.8 Co 0.1 M 0.1 O2; chemical formula LiMn 2-x M x Lithium manganese composite oxide represented by Li2Mn3MO8 (wherein M=Co, Ni, Fe, Cr, Zn or Ta, and x=0.01 to 0.1) or Li2Mn3MO8 (wherein M=Fe, Co, Ni, Cu or Zn); LiNi x Mn 2-x The positive electrode active material may include, but is not limited to, lithium manganese composite oxides having a spinel structure represented by the formula LiMn2O4, in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion, disulfide compounds, Fe2(MoO4)3, and the like. The positive electrode active material may be included in an amount of 70 to 95% by weight, 75 to 95% by weight, or 80 to 95% by weight with respect to 100% by weight of the electrode layer.

[0044] In one embodiment of the present invention, the step (a) may include first mixing a positive electrode active material capable of reversibly absorbing and desorbing lithium ions with an organic solvent, and then further adding an aqueous solvent to the mixture.

[0045] The organic solvent may be used without any particular limitation as long as it can effectively disperse the positive electrode active material. Specifically, it is preferable to use an alcohol-based solvent such as ethanol or isopropyl alcohol.

[0046] By further adding an aqueous solvent to the mixture of the positive electrode active material and the organic solvent, it becomes possible to introduce hydrophilic functional groups onto the surface of the positive electrode active material.

[0047] In the case of a niobium-based compound contained in a solution for forming a positive electrode active material coating layer, which will be described later, a “hydrolysis-condensation” reaction is induced with the hydrophilic functional group introduced by the aqueous solvent, and the niobium-based compound plays a role in being effectively coated on the surface, compared to a positive electrode active material in which a hydrophilic functional group is not introduced.

[0048] This is understood to be because in the case of organic solvents, the function of dispersing the positive electrode active material takes precedence, and the ability to introduce hydrophilic functional groups onto the surface of the positive electrode active material is reduced compared to aqueous solvents.

[0049] The type of the aqueous solvent is not particularly limited as long as it does not affect the physical properties of the positive electrode active material. Specifically, deionized water, ultrapure water, distilled water, or the like may be used.

[0050] The hydrophilic functional group introduced onto the surface of the positive electrode active material by the aqueous solvent may be, for example, a hydroxy group (-OH).

[0051] If, in the process of preparing the positive electrode active material dispersion, an aqueous solvent instead of an organic solvent is first mixed with the positive electrode active material, the positive electrode active material may not be uniformly dispersed in the aqueous solvent, and may harden or aggregate, and hydrophilic functional groups may not be effectively introduced onto the surface of the positive electrode active material. Therefore, it is preferable to prepare the positive electrode active material dispersion by first mixing the positive electrode active material with the organic solvent, and then further adding the aqueous solvent.

[0052] In one embodiment of the present invention, the positive electrode active material dispersion liquid may contain 10 to 50 wt % of solid content based on the total weight of the positive electrode active material dispersion liquid. For example, the content of the solid content may be 20 to 50 wt %, 30 to 50 wt %, preferably 40 to 50 wt % based on the total weight of the positive electrode active material dispersion liquid.

[0053] If the solid content in the positive electrode active material dispersion is less than 10 wt %, the loading capacity of the positive electrode active material in the electrode is reduced, which may lead to a reduction in the capacity of the lithium secondary battery. If the solid content exceeds 50 wt %, there is a problem that aggregation of the solid content may occur due to non-uniform stirring during the preparation of the positive electrode active material dispersion.

[0054] In one embodiment of the present invention, the aqueous solvent may be added in an amount of 1.2 to 1.4 wt % based on the total weight of the solid content in the positive electrode active material dispersion liquid. For example, the content of the aqueous solvent may be 1.25 to 1.4 wt %, 1.3 to 1.4 wt %, preferably 1.34 to 1.4 wt % based on the total weight of the solid content in the positive electrode active material dispersion liquid.

[0055] If the amount of the aqueous solvent is less than 1.2 wt%, it is difficult to effectively introduce hydrophilic functional groups onto the surface of the positive electrode active material, and therefore the coating layer of the niobium-based compound may not be properly formed. If the amount of the aqueous solvent is more than 1.4 wt%, gelation may occur, causing aggregation of the positive electrode active material, and therefore a non-uniform coating layer may be formed. Therefore, the amount of the aqueous solvent is appropriately adjusted within the above range.

[0056] Next, raw materials for the coating material containing lithium (Li) and niobium (Nb) are added and mixed to produce a coating liquid containing a niobium-based compound (step (b)).

[0057] The solvent for preparing the coating solution may be an aqueous solvent such as deionized water, ultrapure water, or distilled water, or an organic solvent such as ethanol or isopropyl alcohol.

[0058] The raw materials for the coating material may be raw materials containing lithium and niobium that can be completely dissolved in an aqueous or organic solvent, and it is more preferable to use lithium ethoxylate and niobic acid. The amount of raw materials to be added is preferably 0.05M to 0.3M for each of the lithium element and the niobium element based on the molar concentration (M) meaning the molar ratio of the element per liter, and more preferably, the coating material may be produced with a solution concentration of 0.1M to 0.2M.

[0059] Even if the raw material of the coating material is dissolved in the solvent during the process of manufacturing the coating solution, if the hydrogen ion concentration and reaction temperature are not precisely adjusted, a localized reprecipitation reaction may occur and niobium oxide (Nb2O5) precipitates may be generated. Therefore, the hydrogen ion concentration, reaction temperature, and reaction time are adjusted within the preferred ranges.

[0060] Next, the coating liquid from step (b) is added to the positive electrode active material dispersion liquid from step (a) to form a coating layer on the surface of the positive electrode active material (step (c)).

[0061] The coating liquid of step (b) can be added dropwise little by little until the formation of a coating layer on the surface of the positive electrode active material is completed. For example, the coating liquid may be added dropwise at a rate of 1 mL / min to 20 mL / min.

[0062] During the preparation of the positive electrode active material dispersion, hydrophilic functional groups are introduced onto the surface of the positive electrode active material by the aqueous solvent, and as a result, the niobium-based compound in the coating solution can bind to the hydrophilic functional groups on the surface of the positive electrode active material to effectively form a uniform coating layer.

[0063] In one embodiment of the present invention, the surface coating layer of the positive electrode active material may contain 1.0 to 1.2% by weight of a niobium-based compound based on the total weight of the solid content in the positive electrode active material dispersion.

[0064] If the content of the niobium-based compound is less than 1.0 wt%, it may be difficult to form a coating layer and it may be difficult to reduce a side reaction between the sulfide-based solid electrolyte and the positive electrode active material. If the content of the niobium-based compound is more than 1.2 wt%, the niobium-based compound may aggregate or a non-uniform coating layer may be formed on the surface of the positive electrode active material. Therefore, the content of the niobium-based compound is appropriately adjusted to within the above range.

[0065] Next, the coating liquid is added to the positive electrode active material dispersion liquid, and the product in which a coating layer is formed on the surface of the positive electrode active material is squeezed and filtered to remove the solvent (step (d)).

[0066] When the product of the positive active material having the coating layer of the niobium-based compound is subjected to squeeze filtration, heat is not generated and detachment of the niobium-based compound in the coating layer can be prevented compared to the conventional case where the residual solvent is removed through a separate heat treatment process, so that the formation of an uneven coating layer can be prevented. Through the squeeze filtration process, the excess organic solvent added to prepare the positive active material dispersion and the excess aqueous solvent added to introduce hydrophilic functional groups on the surface of the positive active material can be almost completely removed.

[0067] The compression filtration may be performed using a known technique. As an apparatus for compression filtration, a pressure filter, a filter press, a screw press, a V-shaped disk press, or the like may be used.

[0068] The squeeze filtration may be performed by applying a predetermined pressure using the known mechanism, for example, a pressure of 0.3 to 0.5 MPa. If the squeeze filtration pressure is less than 0.3 MPa, the organic solvent may remain inside the product in which a coating layer is formed on the surface of the positive electrode active material, and lithium niobate, etc. may not be completely coated on the surface of the positive electrode active material, and may be formed of free substances, resulting in the formation of an uneven coating layer.

[0069] In one embodiment of the present invention, the method may further comprise a step of drying the product from which the solvent has been removed after the press-filtration step (step (d)).

[0070] The cathode active material product having the coating layer formed through step (d) is in a state in which most of the solvent has been removed by compression filtration, so that even if an additional drying step is performed, the niobium-based compound formed on the surface of the cathode active material is not liberated.

[0071] The drying process is a process for removing residual solvent and moisture contained in the positive electrode active material on which the coating layer is formed, and may be performed in a vacuum oven at 80 to 120° C. for 8 to 16 hours. Examples of the drying method include drying with warm air, hot air, or low humidity air, vacuum drying, and drying by irradiation with (far) infrared rays or electron beams. After the drying process, a cooling process may be further included, and the cooling process may be slow cooling to room temperature so that a coating layer is appropriately formed on the surface of the positive electrode active material.

[0072] The positive electrode active material produced through the above steps has a coating layer containing a niobium compound formed on the surface thereof, which reduces reactivity with the sulfide-based solid electrolyte and improves the performance of the all-solid-state battery.

[0073] The thickness of the coating layer containing the niobium compound may be, for example, 10 to 30 nm, for example, 15 to 25 nm, and preferably 20 to 25 nm. If the thickness of the coating layer is less than 10 nm, the effect of reducing the reactivity with the solid electrolyte due to the niobium compound may be reduced, and if the thickness of the coating layer is more than 30 nm, it may affect the absorption and release of lithium ions or the coating layer may act as a resistor to act as a resistor of the all-solid-state battery, so it is appropriately adjusted within the above range.

[0074] Another embodiment of the present invention provides a positive electrode active material for a lithium secondary battery, which is prepared by the method for preparing a positive electrode active material.

[0075] Another embodiment of the present invention provides a lithium secondary battery including the positive electrode active material prepared by the method.

[0076] The lithium secondary battery may include a positive electrode, a negative electrode, and an electrolyte interposed between the positive electrode and the negative electrode, and in one embodiment, the lithium secondary battery may be an all-solid-state battery including a solid electrolyte membrane.

[0077] The positive electrode may include a current collector and a positive electrode active material layer formed on at least one side of the current collector, and the positive electrode active material layer may include a positive electrode active material, a solid electrolyte, and a conductive material. In a specific embodiment of the present invention, the positive electrode active material layer may further include a binder material. The addition of the binder material can increase the bonding strength between the positive electrode active material layer and the current collector and / or the solid electrolyte layer, and can also help improve the bonding strength between components contained in the positive electrode active material, independently or in combination with the binder material.

[0078] The positive electrode active material may be any material usable as a positive electrode active material for a lithium ion secondary battery without any limitations, and as described above, a detailed description thereof will be omitted here.

[0079] The solid electrolyte contained in the positive electrode is, for example, Li2S-P2S5, Li2S-LiI-P2S5, Li2S-P2S5-LiCl, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2 and Li2S-GeS2-ZnS, Li6PS5Cl, Li6PS5Br and Li6PS5Cl. x Br (1-x)(wherein x is 10≦x≦90) and combinations thereof, and preferably includes Li6PS5Cl, Li6PS5Br, and Li6PS5Cl, which have an Argyrodite structure. x Br (1-x) (wherein x is 0.1≦x≦0.9) and combinations thereof. The solid electrolyte may be typically included in the range of 1 to 30% by weight, 1 to 20% by weight, or 1 to 15% by weight relative to 100% by weight of the electrode layer.

[0080] The conductive material is not particularly limited as long as it has conductivity without causing a chemical change in the battery, and may include, for example, one or a mixture of two or more selected from the following conductive materials: graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers such as VGCF (vapor grown carbon fiber); metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives. The conductive material may be included in an amount of 1 to 10% by weight, or 1 to 5% by weight, based on 100% by weight of the electrode layer.

[0081] The binder is not particularly limited as long as it is a component that assists in binding the active material to the conductive material and the like and in binding to the current collector, and examples thereof include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber, fluororubber, various copolymers, etc. The binder may usually be contained in a range of 1 to 20% by weight, or 1 to 10% by weight, relative to 100% by weight of the electrode layer.

[0082] The negative electrode may be a negative electrode current collector, or may include a negative electrode active material layer formed on a surface of the current collector.

[0083] The negative electrode current collector is not particularly limited as long as it has conductivity without causing a chemical change in the all-solid-state battery, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, aluminum-cadmium alloy, etc. Also, the negative electrode current collector may be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric body, etc., on whose surface fine irregularities are formed, similar to the positive electrode current collector.

[0084] The negative electrode active material layer may contain one or more elements belonging to alkali metals, alkaline earth metals, group 3B, and transition metals. In a specific embodiment of the present invention, non-limiting examples of the alkali metal include at least one metal selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), and francium (Fr), and preferably includes lithium. Alternatively, the negative electrode may be a lithium metal or a lithium alloy as a negative electrode active material. The lithium alloy may be an alloy of lithium and at least one metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba, Ra, Al, and Sn. In a specific embodiment of the present invention, the negative electrode may be a laminate in which a negative electrode current collector and a lithium metal thin film having a predetermined thickness are bonded by compression.

[0085] In one embodiment of the present invention, the negative electrode and / or the positive electrode may further include various additives for the purpose of complementing or improving physicochemical properties. The additives are not particularly limited, and may include one or more additives such as an oxidation stabilizing additive, a reduction stabilizing additive, a flame retardant, a heat stabilizer, an antifogging agent, etc.

[0086] For the negative electrode and the positive electrode, the organic solvent used in the production of the electrode slurry may be cyclopentane, cyclohexane, or a mixture thereof, i.e., aliphatic cyclic hydrocarbons, toluene, xylene, or a mixture thereof, i.e., aromatic hydrocarbons, or the aliphatic and aromatic hydrocarbon solvents may be used alone or in combination of two or more. The organic solvent may be appropriately selected depending on the drying speed and environmental conditions.

[0087] The solid electrolyte membrane may be provided between the negative electrode and the positive electrode.

[0088] The solid electrolyte membrane may include a solid electrolyte and a binder.

[0089] Examples of the solid electrolyte contained in the solid electrolyte film include Li2S-P2S5, Li2S-LiI-P2S5, Li2S-P2S5-LiCl, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2, Li2S-GeS2-ZnS, Li6PS5Cl, Li6PS5Br, and Li6PS5Cl. x Br (1-x) (wherein x is 0.1≦x≦0.9) and combinations thereof. The solid electrolyte may be typically contained in an amount of 80 to 100% by weight, 90 to 100% by weight, or 95 to 100% by weight relative to 100% by weight of the solid electrolyte membrane.

[0090] The binder contained in the solid electrolyte membrane is not particularly limited as long as it is a component that helps bind the solid electrolyte, and examples thereof include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber, fluororubber, various copolymers, etc. The binder may usually be contained in a range of 1 to 20% by weight, or 1 to 10% by weight, relative to 100% by weight of the solid electrolyte membrane.

[0091] The ionic conductivity of the solid electrolyte membrane is, for example, 5×10 -3 S / cm super~1×10 -1 The ionic conductivity of the solid electrolyte membrane may be 5×10 S / cm or less. -3 If the ionic conductivity is less than 1×10 S / cm, lithium ion conduction between the positive and negative electrodes in the all-solid-state battery structure cannot be provided as a main pathway, making it difficult to achieve basic cell performance. The higher the ionic conductivity of the solid electrolyte membrane, the more advantageous it is. However, when the characteristics of the solid electrolyte, the limits of performance realization, and atmospheric stability are taken into consideration, it is difficult to achieve a ionic conductivity of less than 1×10 -1 It is preferable to limit the range to S / cm or less.

[0092] Specific examples of the present invention are described below. However, the examples described below are merely for the purpose of specifically illustrating or explaining the present invention, and the present invention is not limited thereby. Furthermore, since the contents not described here can be sufficiently technically inferred by a person skilled in the art, the description thereof will be omitted.

[0093] Working Example Example 1 (1) Place Li(Ni) as the positive electrode active material in a vessel with a diameter of 30 cm. x Co y Mn zAfter 26 kg of O and 4.0 L of ethanol were added and dispersed, 80.4 g of distilled water was further added and stirred at 200 rpm for 20 minutes to prepare a positive electrode active material dispersion.

[0094] (2) Next, lithium precursor lithium ethoxide (CH3CH2OLi) was dissolved in ethanol for 1 hour, and then niobium precursor pentaethoxide (Nb(OCH2CH3)5) was added to the solution to prepare a coating solution. At this time, the coating solution was mixed so that the niobium compound was 1.0 wt % based on the total weight of the solid content in the positive electrode active material dispersion.

[0095] (3) Next, the coating liquid was poured into the positive electrode active material dispersion liquid to form a coating layer on the surface of the positive electrode active material. The coating liquid was dropped into a container containing the positive electrode active material dispersion liquid at a rate of 2 to 10 mL / min.

[0096] (4) The positive electrode active material having the coating layer formed thereon was passed through a pressure filter and squeezed at a pressure of 0.5 MPa to remove the residual solvent.

[0097] (5) The positive electrode active material from which the solvent had been removed was collected, placed in a vacuum oven, and dried at 80°C for 12 hours to produce a positive electrode active material for lithium secondary batteries with a surface coating layer of lithium niobate (LiNbO3).

[0098] The prepared positive electrode active material was observed with a field emission transmission electron microscope (FE-TEM) as shown in Figure 7, which shows that a coating layer containing a niobium-based compound was formed on the surface of the positive electrode active material to a thickness of about 20 nm. Also, as shown in Figure 8, it can be seen that the coating layer on the surface of the positive electrode active material contains a niobium-based compound.

[0099] Example 2 A positive electrode active material for a lithium secondary battery having a surface coating layer of lithium niobate (LiNbO3) was prepared in the same manner as in Example 1, except that the coating solution was prepared so that the niobium compound was 1.2 wt % based on the total weight of the solid content in the positive electrode active material dispersion.

[0100] Comparative Examples 1 to 7 A positive electrode active material for a lithium secondary battery was prepared in the same manner as in Example 1, except that the solid content in the positive electrode active material dispersion, the niobium-based compound content in the coating solution, and the amount of the aqueous solvent were adjusted as shown in Table 1 below.

[0101] [Table 1]

[0102] Experimental Example 1: Confirmation of surface characteristics of positive electrode active material (1) Evaluation of SEM images Particle samples of the positive electrode active materials for lithium secondary batteries prepared according to Example 1, Comparative Example 1, Comparative Example 3, and Comparative Example 7 were collected, and surface characteristics of the positive electrode active materials were confirmed through scanning electron microscope (SEM) analysis. The results are shown in FIGS. 1 to 4.

[0103] Referring to FIG. 1, in the case of the cathode active material according to Example 1, it can be seen that the surface of the cathode active material is uniformly coated with the niobium-based compound by further adding an aqueous solvent before adding the coating solution of the niobium-based compound to the cathode active material dispersion.

[0104] In contrast, referring to FIG. 2, in the case of the positive electrode active material according to Comparative Example 1, a separate aqueous solvent was not added in the step of preparing the positive electrode active material, so that a hydrophilic functional group was not introduced onto the surface of the positive electrode active material. As a result, the niobium-based compounds contained in the coating solution aggregated with each other by themselves, failing to form a uniform coating layer.

[0105] Referring to FIG. 3, in the case of the positive electrode active material according to Comparative Example 3, the amount of aqueous solvent added in the preparation step of the positive electrode active material was small, and thus hydrophilic functional groups were not sufficiently introduced onto the surface of the positive electrode active material, and therefore the niobium-based compound was not sufficiently introduced into the coating layer.

[0106] Referring to FIG. 4, in the case of the positive active material according to Comparative Example 7, since the solid content in the positive active material dispersion was excessive, the excess positive active material that could not form a coating layer aggregated with each other and appeared in the coating layer.

[0107] (2) Evaluation of energy dispersive X-ray (EDX) images The surface characteristics of the positive electrode active materials for lithium secondary batteries prepared according to Example 1 and Comparative Example 1 were confirmed through energy dispersive X-ray (EDX) analysis, and the results are shown in FIGS. 5 and 6.

[0108] Referring to FIG. 5, in the case of the positive electrode active material for a lithium secondary battery prepared according to Example 1, an aqueous solvent was further added to the positive electrode active material dispersion in a step before forming a coating layer of a niobium-based compound, so that a hydrophilic functional group was introduced onto the surface of the positive electrode active material, and the niobium-based compound shown in red was uniformly coated on the surface of the positive electrode active material.

[0109] Referring to FIG. 6, in the case of the positive electrode active material for a lithium secondary battery prepared according to Comparative Example 1, since no separate aqueous solvent is added to the positive electrode active material dispersion, a hydrophilic functional group is not introduced onto the surface of the positive electrode active material, and the niobium-based compound shown in red is not uniformly coated on the surface of the positive electrode active material.

[0110] Experimental Example 2 All-solid-state batteries were produced using the positive electrode active materials produced in Example 1, Example 2, and Comparative Examples 1 to 7, and the charge / discharge efficiency and life characteristics of each of these batteries were evaluated.

[0111] (Production of positive electrodes) First, a mixture was prepared so that the weight ratio of the positive electrode active material prepared in Example 1, Example 2, and Comparative Examples 1 to 7, the sulfide-based LPSCl (Li6PS5Cl, JeongKwan Co.Ltd) solid electrolyte, the binder, and the conductive material was 65:25:5:5. That is, based on 100 parts by weight of the positive electrode active material prepared according to Example 1, Example 2, and Comparative Examples 1 to 7, 38.46 parts by weight of the LPSCl solid electrolyte, 7.69 parts by weight of the NBR binder, and 7.69 parts by weight of the conductive material Super-P were mixed to prepare a mixture. At this time, the NBR binder was a solution containing nitrile butadiene rubber (NBR) and xylene, and the amount of NBR was 5 wt%. The NBR binder did not contain lithium salt.

[0112] Specifically, the positive electrode active material, LPSCl solid electrolyte, and Super-p prepared according to Example 1, Example 2, and Comparative Examples 1 to 7 were first weighed out in the above weight ratio, and then mixed for 30 minutes using a mortar to prepare a mixed powder. The mixed powder was transferred to a Thinky mixer dedicated container, and then mixed with NBR binder in the above weight ratio, and then placed in the mixer and mixed three times for 5 minutes at 1,800 rpm to prepare a mixture. Next, xylene was mixed into the mixture to adjust the viscosity to an appropriate level, and zircon balls were added and mixed for 5 minutes at 1,800 rpm to prepare a slurry. The slurry was cast on aluminum foil and dried in a vacuum oven at 60° C. for 24 hours, and the loading amount was 3 mg / cm. 2 A positive electrode of 1000g was produced.

[0113] (Manufacturing of solid electrolyte layer) A mixture was prepared so that the weight ratio of Li6PS5Cl as a sulfide-based solid electrolyte to the binder was 70:30. That is, 42.9 parts by weight of polyethylene oxide (PEO) binder was mixed with 100 parts by weight of Li6PS5Cl as a solid electrolyte to prepare the mixture. At this time, the PEO binder was prepared so that the mixing ratio (molar ratio) of polyethylene oxide (PEO, molecular weight 200,000) to Li6PS5Cl was [EO]:[Li]=15:1.

[0114] Specifically, first, the solid electrolyte Li6PS5Cl and the PEO binder were weighed in the above weight ratio, and then the mixture was stirred at 2,000 rpm for 5 minutes using a Thinky mixer to prepare a mixture.

[0115] The mixture was mixed with acetonitrile (ACN) and stirred in a Thinky mixer to adjust the viscosity to an appropriate level. Then, 2 mm zircon balls were added and the mixture was stirred in a Thinky mixer at 2,000 rpm for 5 minutes to prepare a slurry. The slurry was cast on a PET (polyethylene terephthalate) film and dried at room temperature to prepare a solid electrolyte layer with a thickness of 150 μm.

[0116] (Manufacturing of all-solid-state batteries) The produced positive electrode and solid electrolyte layer were punched to a diameter of 14 cm and 16 cm, respectively, and then laminated. Next, a laminate was produced by heating to about 60° C. and pressing at 0.3 MPa for 0.5 minutes. A negative electrode containing lithium metal was placed on the laminate, and an all-solid-state battery containing the positive electrode active material of Example 1, Example 2, and Comparative Examples 1 to 7 was produced in a 2032 standard coin cell.

[0117] Each of the all-solid-state batteries of Example 1, Example 2, and Comparative Examples 1 to 7 was charged at 25° C. with a constant current of 0.2 C up to 4.25 V, and then discharged with a constant current of 0.2 C up to 3.0 V. This was counted as one cycle, and the charge capacity and discharge capacity in the first cycle were measured. The discharge capacity in the first cycle was divided by the charge capacity, and the value multiplied by 100 was taken as the charge / discharge efficiency (%), which is shown in Table 2 below.

[0118] In addition, for each of the all-solid-state batteries of Example 1, Example 2, and Comparative Examples 1 to 7, 50 cycles of charge and discharge were performed at 45° C. and 1C / 1C, and then the 50 cycle discharge capacity retention rate (%) was calculated according to the following formula 1, and is shown in Table 2 below.

[0119] [Formula 1] 50-cycle discharge capacity retention rate (%) = discharge capacity of the all-solid-state battery at the 50th cycle / discharge capacity of the all-solid-state battery at the 1st cycle × 100

[0120] [Table 2]

[0121] Referring to Table 2, in the case of the all-solid-state batteries incorporating the cathode active materials according to Examples 1 and 2, compared to the all-solid-state batteries according to Comparative Examples 1 to 7, it can be seen that a coating layer including a niobium-based compound is uniformly formed as a result of introducing a hydrophilic functional group onto the surface of the cathode active material by introducing an aqueous solvent during the preparation of the cathode active material, and the coating layer suppresses reactivity with the sulfide-based solid electrolyte, thereby improving the charge / discharge capacity and life characteristics of the all-solid-state battery.

[0122] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention.

Claims

1. (a) mixing a positive electrode active material capable of reversibly absorbing and releasing lithium ions and a solvent to prepare a positive electrode active material dispersion; (b) adding and mixing raw materials of a coating material containing lithium (Li) and niobium (Nb) to produce a coating solution containing a niobium-based compound; (c) adding the coating liquid of the step (b) to the positive electrode active material dispersion liquid of the step (a) to form a coating layer on the surface of the positive electrode active material; (d) filtering the product of step (c) by pressing to remove the solvent; The present invention relates to a method for producing a positive electrode active material for a lithium secondary battery.

2. In the step (a), a positive electrode active material capable of reversibly absorbing and releasing lithium ions and an organic solvent are mixed together, and then, The method for producing a positive electrode active material for a lithium secondary battery according to claim 1 , further comprising adding an aqueous solvent to the mixture.

3. 3. The method for producing a positive electrode active material for a lithium secondary battery according to claim 2, wherein the aqueous solvent is further added to introduce a hydrophilic functional group onto a surface of the positive electrode active material.

4. 2. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the positive electrode active material dispersion liquid contains 10 to 50% by weight of solids based on the total weight of the positive electrode active material dispersion liquid.

5. 2. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the surface coating layer of the positive electrode active material contains 1.0 to 1.2 wt % of a niobium-based compound based on the total weight of the solid content in the positive electrode active material dispersion.

6. 3. The method for producing a positive electrode active material for a lithium secondary battery according to claim 2, wherein the aqueous solvent is added in an amount of 1.2 to 1.4 wt % based on the total weight of the solid content in the positive electrode active material dispersion.

7. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the squeeze filtration is carried out under a pressure of 0.3 to 0.5 MPa.

8. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the coating layer has a thickness of 10 to 30 nm.

9. 2. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1, further comprising the step of drying the product from which the solvent has been removed at 80 to 120° C. after the step (d).

10. A positive electrode active material for lithium secondary batteries, produced by the method for producing a positive electrode active material for lithium secondary batteries according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for manufacturing positive electrode active material for nonaqueous electrolyte secondary batteries, positive electrode active material for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery arranged by use thereof

    JP2015122299A

  • Braces for upper body massage

    KR1020220136039A

  • Method of manufacturing positive electrode active material for lithium ion secondary battery, positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery

    US20220102696A1

  • Method for manufacturing coated active material

    JP2012234648A

  • KR2022-0045460