Method for producing iridium chloride hydrate and method for producing iridium chloride

A method for producing iridium chloride hydrate through mixing, calcination, and hydrochloric acid dissolution under pressure addresses low yield and environmental issues in existing methods, achieving high purity and sustainability.

JP2024541733AActive Publication Date: 2024-11-11HEESUNG CATALYSTS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024530517
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-02
Filing Date
2022-12-02
Publication Date
2024-11-11
Estimated Expiration
2042-12-02

AI Technical Summary

Technical Problem

Existing methods for producing iridium chloride from iridium metal powder face low yield, incomplete dissolution, and environmental pollution due to the release of nitrogen oxides during high-temperature aqua regia processing.

Method used

A method involving mixing iridium metal powder with an alkali metal compound, calcination to form alkali-containing iridium oxide, followed by hydrochloric acid washing and dissolution under pressure to produce iridium chloride hydrate, which avoids nitrogen oxide generation and achieves high purity.

Benefits of technology

The method achieves high conversion of iridium metal to chloride hydrate with low alkali metal content and no nitrogen oxides, ensuring high product purity and environmental sustainability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541733000001_ABST
    Figure 2024541733000001_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing iridium chloride hydrate, the method including: a mixing step of preparing a mixture of iridium metal powder and an alkali metal compound; a calcination step of calcining the mixture to produce alkali-containing iridium oxide; a hydrochloric acid aqueous solution washing step of washing the alkali-containing iridium oxide with an aqueous hydrochloric acid solution to obtain iridium oxide; and a hydrochloric acid dissolution reaction step of dissolving the iridium oxide in hydrochloric acid under pressure and then reacting the iridium oxide.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing iridium chloride hydrate and iridium chloride from iridium metal powder. [Background technology]

[0002] The most common commercially available form of iridium is as a metallic powder. However, unlike platinum or palladium, iridium metal powder does not dissolve in acid solutions, alkaline solutions, or aqua regia (a mixture of concentrated hydrochloric acid and concentrated nitric acid).

[0003] In order to produce an iridium aqueous solution by dissolving iridium metal powder, it is mixed with an alkali metal (such as Na or K) and then heat-treated to convert it into an oxide, which is then dissolved in aqua regia.

[0004] However, even with this method, it is difficult to completely dissolve iridium metal, and the product yield is not high. Therefore, the undissolved iridium metal must be recovered and the same process must be repeated starting from the heat treatment step.

[0005] In addition, the process of dissolving iridium oxide in aqua regia is carried out at high temperatures, and the nitric acid contained in the aqua regia is released as steam, which can cause environmental pollution. Summary of the Invention [Problem to be solved by the invention]

[0006] According to one embodiment of the present invention, there is provided a method for producing iridium chloride hydrate, which has a high conversion rate of iridium metal, no unreacted iridium due to the high solubility of iridium metal, a low content of alkali metal, and a high purity product, and is environmentally friendly because no nitrogen oxides are generated.

[0007] Another embodiment of the present invention provides a method for producing iridium chloride utilizing the produced iridium chloride hydrate. [Means for solving the problem]

[0008] According to one embodiment of the present invention, there is provided a method for producing iridium chloride hydrate, the method including: a mixing step of preparing a mixture of iridium metal powder and an alkali metal compound; a calcination step of calcining the mixture to produce an alkali-containing iridium oxide; a hydrochloric acid aqueous solution washing step of washing the alkali-containing iridium oxide with an aqueous hydrochloric acid solution to obtain iridium oxide; and a hydrochloric acid dissolution reaction step of dissolving the iridium oxide in hydrochloric acid under pressure and then reacting the iridium oxide.

[0009] The alkali metal compound can include an alkali metal hydroxide, an alkali metal peroxide, or a mixture thereof.

[0010] The alkali metal hydroxide may include sodium hydroxide, potassium hydroxide, lithium hydroxide, or mixtures thereof.

[0011] The alkali metal peroxide may include sodium peroxide, potassium peroxide, lithium peroxide, or mixtures thereof.

[0012] The alkali metal hydroxide may include a mixture of sodium hydroxide and sodium peroxide.

[0013] The mixture may contain 0.5 to 1 part by weight of the alkali metal compound per part by weight of the iridium metal powder.

[0014] The mixture may contain 1 to 3 parts by weight of alkali metal peroxide per part by weight of iridium metal powder.

[0015] The alkali-containing iridium oxide may include a compound represented by the following Chemical Formula 1:

[0016] [Chemical formula 1]

[0017] Nax Ir y O z

[0018] In Chemical Formula 1, x is an integer from 2 to 4, y is an integer from 1 to 3, and z is an integer from 3 to 8.

[0019] The alkali-containing iridium oxide may include Na2IrO3, Na4IrO4, Na4Ir3O8, or mixtures thereof.

[0020] In the firing step, firing is carried out at high temperatures of 750° C. or higher.

[0021] Between the calcination step and the hydrochloric acid aqueous solution washing step, a water washing step of washing the alkali-containing iridium oxide with water at 60° C. to 70° C. for 2 hours to 4 hours may be further included.

[0022] In the hydrochloric acid aqueous solution washing step, the concentration of the hydrochloric acid aqueous solution is 5% to 10%.

[0023] The method may further include a step of drying the iridium oxide that has been washed with the aqueous hydrochloric acid solution to obtain a cake.

[0024] The iridium oxide cake has an alkali metal content of 10 ppm or less.

[0025] In the hydrochloric acid dissolution reaction step, the content of hydrochloric acid per 1 part by weight of iridium oxide is 5 parts by weight to 15 parts by weight.

[0026] The hydrochloric acid dissolution reaction step can be carried out under pressure of 5 to 10 pressures.

[0027] The hydrochloric acid dissolution reaction step can be carried out under pressure at 130°C to 170°C for 2 to 6 hours.

[0028] The method may further include a step of filtering the iridium chloride hydrate produced in the hydrochloric acid dissolution reaction step.

[0029] The iridium chloride hydrate produced has an alkali metal content of 10 ppm or less.

[0030] According to another embodiment of the present invention, there is provided a method for producing iridium chloride, comprising concentrating the obtained iridium chloride hydrate to produce iridium chloride. Effect of the Invention

[0031] The method for producing iridium chloride hydrate according to one embodiment of the present invention has a high conversion rate of iridium metal, high solubility of iridium metal means that there is no unreacted iridium, low alkali metal content means that the product is highly pure, and no nitrogen oxides are generated, which is environmentally advantageous. [Brief description of the drawings]

[0032] [Figure 1] 1 is a process flow diagram illustrating steps for producing iridium chloride hydrate and iridium chloride according to one embodiment.

[0033] [Diagram 2] 1 is a graph showing the results of XRD analysis of alkali-containing iridium oxide produced at different firing temperatures in Experimental Example 1.

[0034] [Diagram 3] 1 is a graph showing the results of XRD analysis of iridium oxide produced under different cleaning conditions in Experimental Example 2.

[0035] [Figure 4] 1 is a graph showing the results of XRD analysis of iridium chloride hydrate measured in Experimental Example 3.

[0036] [Diagram 5] 1 is a photograph showing the iridium chloride hydrate and iridium chloride produced in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0037] The advantages and features of the techniques described below, and the manner in which they are achieved, will become apparent from the following detailed description of the embodiments taken in conjunction with the accompanying drawings. However, the embodied forms are not limited to the embodiments disclosed below. Unless otherwise defined, all terms (including technical and scientific terms) used herein are used with the meaning commonly understood by one of ordinary skill in the art. Additionally, terms defined in commonly used dictionaries are not to be interpreted ideally or excessively unless specifically and explicitly defined. Throughout the specification, when a part is said to "comprise" a certain element, this means that it can further include other elements, but not to the exclusion of other elements, unless specifically stated to the contrary.

[0038] Also, the singular includes the plural unless the phrase specifically states otherwise.

[0039] FIG. 1 is a process flow diagram illustrating steps for producing iridium chloride hydrate and iridium chloride according to one embodiment of the present invention.

[0040] With reference to FIG. 1, the method for producing iridium chloride hydrate and iridium chloride will be described in detail.

[0041] The method for producing iridium chloride hydrate includes a mixing step (S1-1), a calcination step (S1-2), a hydrochloric acid aqueous solution washing step (S1-4), and a hydrochloric acid dissolution reaction step (S1-5).

[0042] In the mixing step (S1-1), a mixture of iridium metal powder and an alkali metal compound is prepared.

[0043] The alkali metal compound can include an alkali metal hydroxide, an alkali metal peroxide, or a mixture thereof, for example, a solid mixture of an alkali metal hydroxide and an alkali metal peroxide.

[0044] The alkali metal hydroxide can include sodium hydroxide, potassium hydroxide, lithium hydroxide, or mixtures thereof, for example, the alkali metal hydroxide is sodium hydroxide (NaOH).

[0045] The alkali metal peroxide can include sodium peroxide, potassium peroxide, lithium peroxide, or mixtures thereof, for example, the alkali metal peroxide can be sodium peroxide (Na2O2).

[0046] As an example, the alkali metal hydroxide may include a mixture of sodium hydroxide and sodium peroxide.

[0047] The mixture may contain 0.5 parts by weight to 1 part by weight, for example 0.6 parts by weight to 0.7 parts by weight, of the alkali metal compound per part by weight of the iridium metal powder. If the content of the alkali metal compound is less than 0.5 parts by weight per part by weight of iridium metal powder, the amount of alkali component adsorbed on the surface of the iridium metal may be insufficient, and oxidation may not occur uniformly during the firing process. If the content exceeds 1 part by weight, the excess alkali metal compound may cover the surface of the iridium metal, preventing the oxidizing agent from coming into contact with the iridium metal.

[0048] Alternatively, the mixture may contain from 1 part by weight to 3 parts by weight, for example 1.75 parts by weight to 2.25 parts by weight, of an alkali metal peroxide in an alkali metal compound per part by weight of the iridium metal powder. If the content of alkali metal peroxide is less than 1 part by weight per part by weight of iridium metal powder, iridium metal may still remain after calcination due to a lack of oxidizing agent, and if it exceeds 3 parts by weight, iridium metal may be peroxidized to form iridium nanoparticles, which may make it difficult to pass through the filter paper in the subsequent filtration process to obtain the product.

[0049] In this case, when the alkali metal compound contains a mixture of an alkali metal hydroxide and an alkali metal peroxide, the weight ratio of the alkali metal hydroxide to the alkali metal peroxide is 1:2 to 1:4, for example, 1:2.5 to 1:3.5. If the weight ratio of the alkali metal peroxide is less than 2, iridium metal may remain even after calcination due to a lack of oxidizing agent, and if it exceeds 4, iridium metal may be overoxidized to form iridium nanoparticles, which may make it difficult to pass through the filter paper in the subsequent filtration process to obtain the product.

[0050] In the calcination step (S1-2), the mixture is calcined to produce an alkali-containing iridium oxide.

[0051] The firing is carried out at 750°C or higher. If the calcination temperature is less than 750° C., unreacted iridium metal may remain, whereas if the calcination temperature is 750° C. or higher, the iridium metal may be completely converted to alkali-containing iridium oxide. For example, the firing is carried out by increasing the temperature to 750° C. or higher over a period of 5 to 10 hours and maintaining the temperature at 750° C. or higher for 2 to 4 hours.

[0052] The alkali-containing iridium oxide produced by calcination may include a compound represented by the following Chemical Formula 1.

[0053] [Chemical formula 1]

[0054] Na x Ir y O z

[0055] In Chemical Formula 1, x is an integer from 2 to 4, y is an integer from 1 to 3, and z is an integer from 3 to 8.

[0056] For example, the alkali-containing iridium oxide represented by Chemical Formula 1 can include Na2IrO3, Na4IrO4, Na4Ir3O8, or a mixture thereof.

[0057] Optionally, the alkali-containing iridium oxide obtained in the calcination step may be washed with water prior to the hydrochloric acid aqueous solution washing step (S1-3).

[0058] The water may be deionized water, distilled water, or ultrapure water, for example, deionized water may be utilized.

[0059] As an example, the water washing step may be performed by washing iridium oxide with water containing alkali at 60° C. to 70° C. for 2 to 4 hours. If the temperature of the water washing step is less than 60°C, the washing will not be complete and there may be residual alkaline ions after washing. If it exceeds 70°C, the washing water may evaporate and become concentrated. If the water washing step time is less than 2 hours, the washing may not be complete, and if it exceeds 4 hours, the working time may be unnecessarily long.

[0060] Optionally, after the water washing step, a further filtration step can be included. For example, filtration may be performed hot using a paper filter on the water-washed solution.

[0061] Optionally, after the filtration step, a water washing step may be further carried out. For example, after filtration, the mixture may be washed with pre-prepared high-temperature water at 60°C to 70°C.

[0062] Through the water washing step, the alkali metal ions in the alkali-containing iridium oxide can be partially removed, and thus, a portion of the iridium oxide can be obtained. However, even after the water washing step, about 400 ppm or more of alkali metal components may remain.

[0063] In the hydrochloric acid washing step (S1-4), the iridium oxide containing alkali is washed with a hydrochloric acid solution to reduce the content of the remaining alkali metal components to 10 ppm or less, thereby producing iridium oxide.

[0064] The concentration of the aqueous hydrochloric acid solution may be 5% to 10%. If the concentration of the hydrochloric acid solution is less than 5%, the cleaning effect will not be good and alkali metals may still remain; if it exceeds 10%, in addition to alkali metals, some iridium metals may also be dissolved.

[0065] Optionally, a further filtration step can be included after the aqueous hydrochloric acid washing step. For example, filtration is performed at high temperature using a paper filter after washing with an aqueous hydrochloric acid solution.

[0066] Optionally, the iridium oxide that has been washed with the aqueous hydrochloric acid solution can be dried to produce a cake.

[0067] Drying is carried out at 100° C. or higher for 12 to 24 hours. If the drying temperature is less than 100°C, not only will the drying time be longer, but moisture may remain even after drying.

[0068] The content of remaining alkali metal components can be reduced through the step of washing with an aqueous hydrochloric acid solution. Thereby, the iridium oxide cake can have an alkali metal content of 10 ppm or less, for example, 0 ppm to 5 ppm.

[0069] If the content of alkali metal exceeds 10 ppm, the purity of the final product iridium chloride decreases, which may have a negative effect on the catalytic reaction when producing a catalyst using the same.

[0070] In the hydrochloric acid dissolution reaction step (S1-5), iridium oxide is dissolved in hydrochloric acid under pressure and then reacted to produce iridium chloride hydrate.

[0071] The content of hydrochloric acid relative to 1 part by weight of iridium oxide can be 5 parts by weight to 15 parts by weight, for example, 8 parts by weight to 10 parts by weight. If the content of hydrochloric acid per 1 part by weight of iridium oxide is less than 5 parts by weight, the content of chloride ions required for the reaction is insufficient, and therefore 100% conversion of iridium oxide to iridium chloride may not be achieved. If the content of hydrochloric acid exceeds 15 parts by weight, excessive energy costs may be required for evaporation of the hydrochloric acid aqueous solution in the subsequent concentration process.

[0072] The hydrochloric acid dissolution reaction step is carried out under pressure, and by way of example, in a pressurized vessel. The pressure during pressurization is 5 to 10 pressures, for example, 6 to 8 pressures. Since the pressure increases in proportion to the reaction temperature, if the reaction is carried out within the following temperature range, there is no need to separately adjust the pressure.

[0073] The hydrochloric acid dissolution reaction step is carried out under pressure at 130° C. to 170° C. for 2 to 6 hours, for example, at 150° C. to 170° C. for 2 to 4 hours. If the temperature in the hydrochloric acid dissolution reaction step is less than 130°C, it may be difficult to convert 100% of iridium oxide to iridium chloride. If it exceeds 170°C, the conversion to iridium chloride is easy, but the pressure vessel may corrode or deform, making commercial application difficult. If the time is less than 2 hours, the conversion reaction rate of iridium chloride may decrease, and if it exceeds 6 hours, excessive energy costs may be incurred.

[0074] Optionally, a filtration step may be further included after the hydrochloric acid dissolution reaction step.

[0075] Through the filtration step, the iridium chloride hydrate produced in the hydrochloric acid dissolution reaction step can be obtained. For example, filtration is performed by using a paper filter to filter the solution that has undergone the hydrochloric acid dissolution reaction at a high temperature. At this time, a minimum amount of rinsing solution, such as deionized water, is used to recover the remaining solution.

[0076] The iridium chloride hydrate produced may be, for example, a compound represented by H2IrCl6·xH2O. The iridium chloride hydrate obtained in the hydrochloric acid dissolution reaction step is substantially completely dissolved, for example, 99.9% or more dissolved, and has an alkali metal content of 10 ppm or less.

[0077] In one embodiment of the method for producing iridium chloride hydrate, the calcination step (S2-1) induces complete oxidation of iridium metal to increase the production yield, the hydrochloric acid aqueous solution washing step (S1-4) uses a single solvent of hydrochloric acid aqueous solution to prevent the generation of nitrogen oxides, and the alkali metal content in the obtained iridium chloride is 10 ppm or less by removing alkali metal components used as an oxidant using hydrochloric acid before the pressure reaction, and the hydrochloric acid dissolution reaction step (S1-5) has a solubility of 99.9% or more through the pressure reaction, and since there is no unreacted iridium, the purity of the product is very high.

[0078] In another embodiment of the method for producing iridium chloride, the produced iridium chloride hydrate is concentrated to produce iridium chloride (S2-1).

[0079] As an example, the concentration can be performed by vacuum distillation.

[0080] The iridium chloride produced may be, for example, a compound represented by IrCl4·xH2O. [Example]

[0081] Specific examples of the invention are presented below. However, the following examples are merely intended to specifically illustrate and explain the invention, and should not be construed as limiting the scope of the invention.

[0082] [Production Example: Production of Iridium Chloride Hydrate]

[0083] Example 1

[0084] 13.3 g of NaOH powder and 40.2 g of Na2O2 powder are added to 20 g of Ir metal powder and physically mixed.

[0085] The mixed powder is placed in a crucible and fired at 750°C, then allowed to cool gradually. The firing is carried out in stages, with the temperature increased to 750°C for 6 hours and maintained at that temperature for 2.5 hours. During firing, the lid of the crucible is left open.

[0086] The calcined powder is placed in 500 ml of deionized water and the solution is heated to 65° C. with ultrasonic mixing. Once the temperature reaches 65° C., the mixture is stirred using a magnetic spin bar for 2 hours.

[0087] The stirred solution is filtered hot through a paper filter. After filtration, wash with 2 L of previously prepared hot water at 65°C.

[0088] In addition, 200 g of 10% HCl solution (180 g deionized water + 20 g HCl) is prepared and then washed additionally.

[0089] After the cleaning was completed, the cleaning solution was subjected to ICP analysis, and the results confirmed that no Ir component was present in the cleaning solution.

[0090] After washing, the powder was dried at 120°C for more than 12 hours to remove Na. x IrO y Collect the cake.

[0091] The dried cake is placed in a pressure vessel and mixed with 242 g of HCl.

[0092] The prepared pressure vessel is placed in a heat treatment furnace, and the high-temperature pressurized reaction is carried out at 150°C for 4 hours, after which it is cooled.

[0093] The dissolved solution is filtered using a paper filter. A minimum amount of rinse solution (deionized water) is used to recover residual solution.

[0094] (Examples 2 to 11 and Comparative Examples 1 to 2)

[0095] Iridium chloride hydrate was produced in the same manner as in Example 1, except that the reaction conditions in Example 1 were changed as shown in Table 1 below.

[0096] For reference, in Comparative Examples 1 and 2, aqua regia (hydrochloric acid:nitric acid=3:1 volume ratio) is used instead of hydrochloric acid in the dissolution reaction stage.

[0097] [Table 1]

[0098] [Experimental Example 1: XRD analysis results of products at different firing temperatures]

[0099] The state of the iridium oxide containing alkali produced by changing the firing temperature to 750°C, 650°C, 700°C, and 800°C in Example 1 and Examples 4 to 6 was analyzed by XRD, and the results are shown in Figure 2.

[0100] Referring to FIG. 2, it can be seen that at firing temperatures below 750°C, iridium metal that did not react with the oxidizing agent Na2O2 remained, and IrO2, which is a simple oxide without being combined with Na ions, was also produced.

[0101] On the other hand, under firing conditions of 750℃ or higher, the iridium metal completely combines with the sodium ions and the oxidizing agent, and becomes completely sodium. x IrO yIt can be confirmed that it is converted into

[0102] [Experimental Example 2: XRD analysis results of products according to washing conditions]

[0103] The state of iridium oxide produced by changing the washing conditions in Examples 1, 7, and 8 was analyzed by XRD, and the results are shown in FIG.

[0104] Example 1 is the result of first washing with deionized water and second washing with 10% hydrochloric acid aqueous solution, Example 8 is the result of first washing with deionized water and second washing with 5% hydrochloric acid aqueous solution, and Example 7 is the result of first washing with deionized water and not second washing with hydrochloric acid aqueous solution.

[0105] Referring to FIG. 3, most of the Na ions contained in the iridium oxide are removed by washing with deionized water, but some remain in the iridium oxide.

[0106] It can be seen that if a secondary cleaning is performed using an aqueous hydrochloric acid solution with a concentration of 5% to 10% after cleaning with deionized water, most of the Na ions in the iridium oxide are eventually removed.

[0107] Specifically, the results of XRD analysis show that when only deionized water washing is performed, Na x IrO y The peak of Na is still present, but after an additional wash with aqueous hydrochloric acid, x IrO y It can be seen that the peak disappears.

[0108] In addition, elemental analysis (ICP analysis) was performed on the oxide from which the sodium ions had been removed. As a result, after additional washing with a hydrochloric acid solution, the sodium ions in the iridium oxide were measured to be at the 10 ppm level when washed with a 5% hydrochloric acid solution, and at the 4 ppm level when washed with a 10% hydrochloric acid solution.

[0109] [Experimental Example 3: Confirmation of the produced iridium chloride hydrate]

[0110] The iridium content of the product produced in Example 1 is measured by ICP analysis.

[0111] As a result, a yield of 99.9% or more was confirmed based on the initial Ir powder, and the residual Na content in the product was 4.1 ppm, confirming that it had been almost completely removed.

[0112] In addition, the product was dried at 80° C. to remove moisture and then subjected to XRD analysis. The results are shown in FIG. In FIG. 4, Reference Example 1 shows the results for reagent grade H2IrCl6·xH2O (manufactured by Aldrich). Referring to FIG. 4, it was confirmed that the crystal shape was the same as that of reagent grade H2IrCl6·xH2O (manufactured by Aldrich).

[0113] The product produced is dried at 100°C for 4 hours and the dried product is recovered. The dried product was analyzed by ion chromatography and found to have a Cl / Ir molar ratio of 4.2.

[0114] The results of the thermogravimetric analysis are shown in Table 2.

[0115] [Table 2]

[0116] Referring to Table 2, Example 1 and Reference Example 1 had almost the same residual amount after thermal analysis at 900°C. This confirmed that the dried product was produced using IrCl4.

[0117] In addition, the produced product was diluted 1000 times and the color was compared with that of the commercially available Reference Example 1. The results are shown in FIG. In FIG. 5, (A) is a photograph of iridium metal powder, (B) is a photograph of the product H2IrCl6 solution, (B') is a photograph of the product H2IrCl6 solution after 1000-fold dilution and dissolution, and (Ref. B') is a photograph of Reference Example 1. (C) is a photograph of IrCl4, which is the dried product, (C') is a photograph of IrCl4, which is the dried product, after it was diluted 1000 times and dissolved, and (Ref. C') is a photograph of Reference Example 1. In FIG. 5, Reference Example 1 is reagent grade (manufactured by Aldrich) H2IrCl 6· Results for xH2O.

[0118] Referring to FIG. 5, the product was confirmed to be H2IrCl6·xH2O, and the dried product was confirmed to be IrCl4·xH2O.

[0119] [Experimental Example 4: Measurement of yield and Na content of produced iridium chloride hydrate]

[0120] The yield and Na content of the iridium chloride hydrates produced in Examples 1 to 11 and Comparative Examples 1 and 2 were measured, and the results are shown in Table 3.

[0121] [Table 3]

[0122] Referring to Table 3, Examples 1 to 3 are the cases where the catalysts were prepared by adjusting the ratio of the alkali metal compound and the iridium metal during calcination. In the case of Example 2, the iridium metal was not completely oxidized, and therefore, complete dissolution was not achieved in the final oxide dissolution reaction step. In the case of Example 3, an excessive amount of alkali metal compound was added, and thus, there was a problem that the iridium oxide was dissolved and eluted in deionized water during the cleaning process.

[0123] In Example 1 and Examples 4 to 6, the catalysts were produced at different calcination temperatures during calcination. When the firing temperature is below 750°C, unoxidized iridium exists, and the dissolution rate is low during the dissolution reaction stage. Only when firing is performed at a temperature above 750°C does the single Na x IrO y It can be seen that a complex oxide form is formed.

[0124] Examples 1, 7, and 8 are results of comparing the amount of Na ions in the product depending on the degree of washing with the hydrochloric acid aqueous solution in the washing step. In Example 7, the secondary washing using an aqueous hydrochloric acid solution was not carried out, and as a result, it was confirmed that a large amount of Na ions remained in the final product. Example 8 shows the results of washing with an aqueous hydrochloric acid solution prepared with a concentration of 5%, and it was confirmed that even a small amount of hydrochloric acid had an excellent washing effect.

[0125] Example 1 and Examples 9 to 11 are cases in which production was carried out at different dissolution reaction temperatures in the dissolution reaction stage. It was confirmed that when pressure dissolution was performed at temperatures below 150°C, a low dissolution rate was observed, but complete dissolution occurred at temperatures above 150°C.

[0126] Example 1, Comparative Example 1, and Comparative Example 2 are produced by using different dissolving methods in the dissolving reaction stage. In the case of the aqua regia dissolution method, the temperature could not be raised above 100°C when performed at normal pressure, and low solubility was observed. In particular, Comparative Example 1 showed low solubility and a high residual rate of Na ions in the product because washing with a hydrochloric acid aqueous solution was not performed in the washing step.

[0127] Therefore, as in Example 1, iridium oxide is produced by additionally removing Na ions using a 5% to 10% hydrochloric acid aqueous solution at a weight ratio of iridium metal and alkali metal compound of 2.6 and a calcination temperature of 750°C or higher, and an iridium chloride solution with a dissolution rate of 99% or higher can be produced by subjecting the iridium oxide produced in this manner to a pressurized reaction at 150°C or higher.

[0128] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the claims also fall within the scope of the present invention. [Industrial Applicability]

[0129] In one embodiment, a method for producing iridium chloride hydrate is provided that has a high conversion rate of iridium metal, does not contain unreacted iridium due to the high solubility of iridium metal, has a low content of alkali metals, and has a high product purity. In addition, no nitrogen oxides are generated, which is environmentally friendly.

[0130] Another embodiment provides a method for producing iridium chloride utilizing the produced iridium chloride hydrate.

Claims

1. a mixing step of preparing a mixture of iridium metal powder and an alkali metal compound; a calcination step of calcining the mixture to produce an alkali-containing iridium oxide; a step of washing the alkali-containing iridium oxide with an aqueous hydrochloric acid solution to obtain iridium oxide; a hydrochloric acid dissolution reaction step of dissolving the iridium oxide in hydrochloric acid under pressure and then reacting the iridium oxide; A method for producing iridium chloride hydrate, comprising:

2. 2. The method for producing iridium chloride hydrate according to claim 1, wherein the alkali metal compound comprises an alkali metal hydroxide, an alkali metal peroxide, or a mixture thereof.

3. the alkali metal hydroxide comprises sodium hydroxide, potassium hydroxide, lithium hydroxide, or a mixture thereof; 3. The method for producing iridium chloride hydrate according to claim 2, wherein the alkali metal peroxide comprises sodium peroxide, potassium peroxide, lithium peroxide, or a mixture thereof.

4. 4. The method for producing iridium chloride hydrate according to claim 3, wherein the alkali metal hydroxide comprises a mixture of the sodium hydroxide and the sodium peroxide.

5. 2. The method for producing iridium chloride hydrate according to claim 1, wherein the mixture contains 0.5 to 1 part by weight of the alkali metal compound per 1 part by weight of the iridium metal powder.

6. 3. The method for producing iridium chloride hydrate according to claim 2, wherein the mixture contains 1 to 3 parts by weight of the alkali metal peroxide per 1 part by weight of the iridium metal powder.

7. 2. The method for producing iridium chloride hydrate according to claim 1, wherein the alkali-containing iridium oxide comprises a compound represented by the following Chemical Formula 1: [Chemical formula 1] Na x Ir y O z (In the above Chemical Formula 1, x is an integer of 2 to 4, y is an integer of 1 to 3, and z is an integer of 3 to 8.)

8. The alkali-containing iridium oxide is Na 2 IrO 3 , Na 4 IrO 4 , Na 4 Ir 3 O 8 or a mixture thereof.

9. 2. The method of claim 1, wherein the calcination is performed at a high temperature of 750° C. or more.

10. Between the calcination step and the hydrochloric acid aqueous solution washing step, 2. The method for producing iridium chloride hydrate according to claim 1, further comprising a water washing step of washing the iridium oxide containing the alkali with water at 60° C. to 70° C. for 2 to 4 hours.

11. 2. The method for producing iridium chloride hydrate according to claim 1, wherein the concentration of the aqueous hydrochloric acid solution in the washing step is 5% to 10%.

12. 2. The method of claim 1, further comprising the step of drying the iridium oxide that has been washed with the aqueous hydrochloric acid solution to obtain a cake.

13. 13. The method for producing iridium chloride hydrate according to claim 12, wherein the iridium oxide cake has an alkali metal content of 10 ppm or less.

14. 2. The method of claim 1, wherein the amount of hydrochloric acid per 1 part by weight of the iridium oxide in the hydrochloric acid dissolution reaction is 5 to 15 parts by weight.

15. 2. The method for producing iridium chloride hydrate according to claim 1, wherein the hydrochloric acid dissolving reaction step is carried out under pressure of 5 to 10 pressures.

16. 2. The method for producing iridium chloride hydrate according to claim 1, wherein the hydrochloric acid dissolving reaction step is carried out under pressure at 130° C. to 170° C. for 2 hours to 6 hours.

17. 2. The method of claim 1, further comprising the step of filtering the iridium chloride hydrate produced in the hydrochloric acid dissolution reaction step.

18. 2. The method for producing iridium chloride hydrate according to claim 1, wherein the produced iridium chloride hydrate has an alkali metal content of 10 ppm or less.

19. A method for producing iridium chloride, comprising concentrating the iridium chloride hydrate obtained by the method for producing iridium chloride hydrate according to claim 1 to produce iridium chloride.

Citation Information

Patent Citations

  • Rapid preparation method of chloroiridic acid

    CN108455688A

  • Method for directly preparing chloroiridic acid from iridium-containing waste

    CN112357979A

  • Method for producing highly pure iridium(III) chloride hydrate

    JP2020515487A

  • Process for the production of high purity iridium(III)chloride hydrate

    US20190337819A1