Electroactive Materials for Metal-Ion Batteries

A composite particulate material with a porous framework and modifier domains addresses the volume change issues in silicon anodes, enhancing cycle efficiency and stability by limiting domain size and reducing SEI formation in rechargeable metal ion batteries.

JP2024541865AActive Publication Date: 2024-11-13NEXEON LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2024523387
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-21
Filing Date
2022-10-21
Publication Date
2024-11-13
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

Existing rechargeable metal ion batteries face challenges with the mechanical stress and capacity loss due to volume changes in silicon-based anodes, leading to fracture and delamination, and excessive solid electrolyte interface (SEI) formation, which reduces electrochemical capacity over multiple charge-discharge cycles.

Method used

A composite particulate material is developed, comprising a porous particle framework with electroactive material domains, such as silicon, and modifier material domains within its pore network, which limits the size of electroactive material domains, reduces surface area, and prevents excessive SEI formation, enhancing cycle efficiency and stability.

Benefits of technology

The composite particles exhibit improved reversible capacity retention and reduced mechanical stress, maintaining high electrochemical performance over multiple cycles by controlling the deposition and expansion of silicon within the porous framework.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541865000001
    Figure 2024541865000001
  • Figure 2024541865000002
    Figure 2024541865000002
  • Figure 2024541865000003
    Figure 2024541865000003
Patent Text Reader

Abstract

The present invention relates to a particulate material and a method for preparing the same. The particulate material comprises a plurality of composite particles. The composite particles comprise a porous particle framework comprising micropores and / or mesopores. The total pore volume of the micropores and mesopores measured by gas adsorption is less than 0.4 cm. 3 / g~2.2cm 3 / g. The composite particle includes a plurality of electroactive material domains and a plurality of modifier material domains disposed within the interior pore volume of the porous particle framework, at least a portion of the modifier material domains being located between adjacent electroactive material domains.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates generally to electroactive materials suitable for use in electrodes for rechargeable metal-ion batteries, and more particularly to particulate materials having high electrochemical capacity suitable for use as anode active materials in rechargeable metal-ion batteries. [Background technology]

[0002] Rechargeable metal-ion batteries are widely used in portable electronic devices such as mobile phones and laptops, and are increasingly being applied in electric or hybrid vehicles. Rechargeable metal-ion batteries generally include an anode in the form of a metal current collector with a layer of electroactive material, defined herein as a material capable of inserting and releasing metal ions during charging and discharging of the battery. The terms "cathode" and "anode" are used herein in the sense that the battery is loaded such that the anode is the negative electrode. When the metal-ion battery is charged, metal ions are transported from the metal-ion-containing cathode layer through the electrolyte to the anode and are inserted into the anode material. The term "battery" is used herein to refer to both devices containing a single anode and a single cathode, as well as devices containing multiple anodes and / or multiple cathodes.

[0003] There is interest in improving the gravimetric and / or volumetric capacity of rechargeable metal-ion batteries. To date, commercially available lithium-ion batteries have been primarily limited to the use of graphite as the anode active material. Upon charging a graphite anode, lithium is inserted between the graphite layers, with the empirical formula Li xC6, where x is greater than 0 and less than or equal to 1. As a result, graphite has a maximum theoretical capacity of 372 mAh / g in lithium-ion batteries, with practical capacities somewhat lower (approximately 340 mAh / g to 360 mAh / g). Other materials, such as silicon, tin, and germanium, can intercalate lithium at significantly higher capacities than graphite, but are not yet in widespread commercial use due to the difficulty of maintaining sufficient capacity over many charge-discharge cycles.

[0004] In particular, silicon has been recognized as a promising alternative to graphite in the manufacture of rechargeable metal-ion batteries with high gravimetric and volumetric capacities due to its extremely high capacity relative to lithium (see, for example, Non-Patent Document 1). Silicon has a theoretical maximum specific capacity of about 3600 mAh / g (Li ion battery) at room temperature. 15 The anode is a type of anode that is based on the silicon-based lithium-ion battery (Si4). However, when lithium is intercalated into bulk silicon, the volume of the silicon material increases significantly, up to 400% of its original volume when silicon is lithiated to its maximum capacity. Repeated charge-discharge cycles generate significant mechanical stresses in the silicon material, leading to fracture and delamination of the silicon anode material. The volumetric shrinkage of silicon particles upon delithiation can result in loss of electrical contact between the anode material and the current collector. To make matters even more difficult, the solid electrolyte interface (SEI) layer that forms on the silicon surface is not mechanically durable enough to accommodate the expansion and contraction of silicon. As a result, the newly exposed silicon surface leads to further decomposition of the electrolyte, an increase in the thickness of the SEI layer, and irreversible consumption of lithium. Collectively, these failure mechanisms result in unacceptable electrochemical capacity loss over successive charge-discharge cycles.

[0005] Numerous approaches have been proposed to overcome the problems associated with the volume changes observed during charging of silicon-containing anodes. Fine silicon structures with cross sections less than about 150 nm, such as silicon films and silicon nanoparticles, have been reported to be more resistant to volume changes during charging and discharging compared to silicon particles in the micron size range. However, none of these are suitable for commercial-scale application without morphology modification. Nanoscale particles are difficult to manufacture and handle, and silicon films do not provide sufficient bulk capacitance.

[0006] US Patent Publication 2007 / 0133963 discloses that capacity retention can be improved by using silicon particles with a high aspect ratio, i.e., the ratio of the maximum dimension to the minimum dimension of the particle. The small cross-section of such particles reduces the structural stress on the material due to volume changes during charging and discharging. However, such particles can be difficult and expensive to manufacture, and can be fragile. Also, the large surface area can lead to the formation of excessive SEI, leading to excessive capacity loss during the first charge-discharge cycle.

[0007] It is also commonly known that electroactive materials such as silicon can be deposited within the pores of porous support materials such as activated carbon materials. These composites offer some of the beneficial charge-discharge properties of nanoscale silicon particles while avoiding the difficulties of handling nanoparticles. Guo et al. (Non-Patent Document 2) disclose a silicon-carbon composite in which a porous carbon substrate provides a conductive scaffold with silicon nanoparticles deposited uniformly distributed within the substrate's pore structure. The composite has been shown to improve capacity retention over multiple charging cycles, but the initial capacity of the composite in mAh / g is significantly lower than that for silicon nanoparticles.

[0008] The present inventors have previously reported the development of a class of electroactive materials having a composite structure in which nanoscale electroactive materials, such as silicon, are deposited within the pore network of highly porous conductive particulate materials, such as porous carbon materials. For example, US Pat. No. 5,399,433 and US Pat. No. 5,499,433 report that the improved electrochemical performance of these materials can be attributed to the manner in which the electroactive materials are located in the porous materials in the form of small domains with dimensions on the order of a few nanometers or less. These fine electroactive structures are believed to have lower resistance to elastic deformation and higher fracture resistance than larger electroactive structures, and therefore can be lithiated and delithiated without excessive structural stress. As a result, the electroactive materials exhibit excellent reversible capacity retention over many charge-discharge cycles. Second, by controlling the loading of silicon within the porous carbon skeleton such that only a portion of the pore volume is occupied by uncharged silicon, the unoccupied pore volume of the porous carbon skeleton can accommodate a significant amount of silicon expansion within. Moreover, as mentioned above, by locating the nanoscale electroactive material domains within small mesopores and / or micropores, only a small area at the electroactive material surface is accessible to the electrolyte, thus limiting SEI formation. Further exposure during subsequent charge-discharge cycles is substantially prevented, so that the role of SEI formation as a failure mechanism leading to capacity loss is significantly reduced. This is in clear contrast to the excessive SEI formation that characterizes the materials disclosed by, for example, Guo (see above).

[0009] The materials described in US Pat. No. 5,399,413 and US Pat. No. 5,499,426 have been synthesized by chemical vapor infiltration (CVI) in different reactor systems (static, rotating and FBR). The porous conductive particles are contacted with a flow of silicon-containing precursor (CVI), typically silane gas, at atmospheric pressure and temperatures between 400° C. and 700° C., until the required amount of silicon is deposited in the micropores and small mesopores. The deposition of silicon is performed in a single step (single-step deposition). Although it is convenient to perform the deposition of silicon in a single step, it allows little control over the length scale of the deposited silicon. The deposition of coarser silicon domains is believed to result in a reversible capacity retention decrease due to excessive structural stress and uncontrolled SEI formation upon subsequent charge-discharge cycles.

[0010] Thus, there is a need in the art for electroactive material-containing composite particles that overcome the shortcomings of composite particles obtained from conventional single-step and multi-step deposition processes. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] International Publication No. 2007 / 083155 [Patent Document 2] International Publication No. 2020 / 095067 [Patent Document 3] International Publication No. 2020 / 128495 [Non-patent literature]

[0012] [Non-Patent Document 1] Insertion Electrode Materials for Rechargeable Lithium Batteries, Winter, M. et al. in Adv. Mater. 1998, 10, No. 10 [Non-Patent Document 2] Journal of Materials Chemistry A, 2013, pp. 14075-14079 Summary of the Invention

[0013] In a first aspect, the present invention provides a particulate material comprising a plurality of composite particles, the composite particles comprising: (a) a porous particle framework containing micropores and / or mesopores, the total pore volume of the micropores and mesopores being less than or equal to 0.4 cm as measured by gas adsorption; 3 / g~2.2cm 3 / g; and (b) a plurality of electroactive material domains and a plurality of modifier material domains disposed within an interior pore volume of the porous particulate scaffold, at least a portion of the modifier material domains being located between adjacent electroactive material domains; The present invention provides a particulate material comprising:

[0014] The present invention therefore generally relates to a composite particulate material comprising a plurality of electroactive material (e.g. silicon) domains within the pore network of a porous particle. The porous particle thus forms a framework for the electroactive material domains. The term "electroactive material domains" as used herein refers to bodies of electroactive material, e.g. elemental silicon, having a maximum dimension determined by the dimensions of the micropores and / or mesopores of the porous particle in which they are located. The electroactive domains may therefore also be described as nanoscale electroactive domains, where the term "nanoscale" is generally understood to refer to dimensions less than 100 nm. However, due to the dimensions of the micropores and mesopores, the electroactive material domains have a maximum dimension in any direction that is typically less than, and usually significantly less than, 50 nm. The domains may take the form of, for example, regular or irregular particles or bounded layers or coated regions. The electroactive material domains are present in combination with modifier material domains, with at least a portion of the modifier material domains being located between adjacent electroactive material domains. The multiple electroactive material domains may be distinct electroactive material domains. The electroactive material domains may comprise (or consist of) amorphous electroactive material or crystalline electroactive material.

[0015] Several different factors contribute to the improved performance of these materials when compared to materials that include a similar porous particle framework but without the modifier material. The modifier material can act as a barrier that effectively prevents the size of the individual domains of electroactive material from increasing as more electroactive material is deposited within the porous particle, for example in further deposition steps. The modifier material thus limits the length scale of the deposited electroactive material, allowing the electroactive material to further deposit and form distinct electroactive material domains. Thus, composite particles are obtained that have both the desired electroactive material loading and the desired length scale of the electroactive material domains. Furthermore, the modifier material can reduce the exposed surface area of ​​the electroactive material domains, thus minimizing SEI formation and oxidation of the electroactive material surface. Furthermore, the modifier material effectively prevents exposure of the electroactive material to the electrolyte, thus reducing SEI formation. During extended cycling of the composite material, the structure of the composite particle can also be destroyed, opening voids and channels to expose electroactive surfaces that were previously located within the closed pore space. This problem is exacerbated when the composite is cycled at higher temperatures, increasing the reaction energy from repeated volume changes and chemical interactions with the electrolyte solvent and other cell components. The addition of modifier materials protects the electroactive material domain surfaces, thus reducing the amount of degradation that can occur in such scenarios. The modifier material can also act as a conductive component, for example, a conductive carbon layer (e.g., a hydrocarbon passivation layer or a nitride passivation layer) can be used as a modifier material, acting as a conductivity enhancer located throughout the interior volume of the composite particle. This is believed to further improve the cycle efficiency and improve the rate performance of the composite.

[0016] The porous particle framework comprises a three-dimensionally interconnected open pore network including micropores and / or mesopores, and optionally a small amount of macropores. In accordance with conventional IUPAC terminology, the term "micropores" is used herein to refer to pores with a diameter of less than 2 nm, the term "mesopores" is used herein to refer to pores with a diameter of 2 nm to 50 nm, and the term "macropores" is used herein to refer to pores with a diameter of more than 50 nm.

[0017] References herein to the volume of micropores, mesopores and macropores in the porous particulate scaffold, and to the distribution of pore volume within the porous particulate scaffold, shall all be understood to relate to the internal pore volume of the porous particulate scaffold alone (i.e., in the form of the porous particle prior to deposition of electroactive and modifier materials). References herein to the BET surface area of ​​the porous particulate scaffold shall also be understood to relate to the BET surface area of ​​the porous particulate scaffold alone.

[0018] The porous particle skeleton is 0.4 cm 3 / g~2.2cm 3 / g (i.e., total pore volume in the range of 0 nm to 50 nm). Typically, the porous particle scaffold contains both micropores and mesopores. However, it is not excluded that a porous particle scaffold containing micropores and no mesopores, or mesopores and no micropores, may be used.

[0019] More preferably, the total volume of the micropores and mesopores in the porous particle framework is at least 0.45 cm 3 / g, or at least 0.5 cm 3 / g, at least 0.55 cm 3 / g, or at least 0.6 cm 3 / g, or at least 0.65 cm 3 / g, or at least 0.7 cm 3 / g, or at least 0.75 cm 3 / g, or at least 0.8 cm 3 / g, at least 0.85 cm3 / g, or at least 0.9 cm 3 / g, or at least 0.95 cm 3 / g, or at least 1 cm 3 / g. The use of a highly porous scaffold may be advantageous as it allows for greater amounts of silicon to be accommodated within the pore structure.

[0020] The internal pore volume of the porous particulate scaffold is suitably limited such that the increased fragility of the porous particulate scaffold outweighs the benefit of the increased pore volume to accommodate a larger amount of silicon. Preferably, the total volume of the micropores and mesopores in the porous particulate scaffold is less than 2 cm 3 / g or less, or 1.8 cm 3 / g or less, or 1.6 cm 3 / g or less, or 1.5cm 3 / g or less, or 1.45 cm 3 / g or less, or 1.4cm 3 / g or less, or 1.35 cm 3 / g or less, or 1.3 cm 3 / g or less, or 1.25 cm 3 / g or less, or 1.2 cm 3 / g or less, or 1.1cm 3 / g or less, or 1cm 3 / g or less, or 0.95 cm 3 / g or less.

[0021] Preferably, the total volume of the micropores and mesopores in the porous particle framework is less than 0.45 cm 3 / g~2.2cm 3 / g, or 0.5 cm 3 / g~2cm 3 / g, or 0.55 cm 3 / g~2cm 3 / g, or 0.6 cm 3 / g~1.8cm 3 / g, or 0.65 cm 3 / g~1.8cm 3 / g, or 0.7 cm 3 / g~1.6cm 3 / g, or 0.7 cm 3 / g~1.5cm 3 / g, or 0.7 cm 3 / g~1.4cm 3 / g range.

[0022] The total volume of micropores and mesopores in the porous particle framework is also 0.55 cm 3 / g~1.4cm 3 / g, or 0.6 cm 3 / g~1.4cm 3 / g, or 0.6 cm 3 / g~1.3cm 3 / g, or 0.65 cm 3 / g~1.3cm 3 / g, or 0.65 cm 3 / g~1.2cm 3 / g, or 0.7 cm 3 / g~1.2cm 3 / g, or 0.7 cm 3 / g~1.1cm 3 / g, or 0.7 cm 3 / g~1cm 3 / g, or 0.75 cm 3 / g~0.95cm 3 / g.

[0023] The total volume of micropores and mesopores in the porous particle framework is also 0.4 cm 3 / g~0.75cm 3 / g, or 0.4 cm 3 / g~0.7cm 3 / g, or 0.4 cm 3 / g~0.65cm 3 / g, or 0.45 cm 3 / g~0.75cm 3 / g, or 0.45 cm 3 / g~0.7cm 3 / g, or 0.45 cm 3 / g~0.65cm 3 / g, or 0.45 cm 3 / g~0.6cm 3 / g.

[0024] The total volume of micropores and mesopores in the porous particle framework is also 0.6 cm 3 / g~2cm 3 / g, or 0.6 cm 3 / g~1.8cm 3 / g, or 0.7 cm 3 / g~1.8cm 3 / g, or 0.7 cm 3 / g~1.6cm 3 / g, or 0.8 cm 3 / g~1.6cm 3 / g, or 0.8 cm 3 / g~1.5cm 3 / g, or 0.8 cm 3 / g~1.4cm 3 / g, or 0.9 cm 3 / g~1.5cm 3 / g, or 0.9 cm 3 / g~1.4cm 3 / g or 1cm 3 / g~1.4cm 3 / g.

[0025] "P.D. n The collective term "pore size" as used herein refers to the n-th percentile pore size on a volume basis relative to the total volume of micropores and mesopores. For example, "PD 50 The term "pore size" refers to the pore size below which 50% of the total micropore and mesopore volume is found.

[0026] PD of porous particle framework 50 The pore size may be 30 nm or less, preferably 25 nm or less, or 20 nm or less, or 15 nm or less, or 12 nm or less, or 10 nm or less, or 8 nm or less, or 6 nm or less, or 5 nm or less, or 4 nm or less, or 3 nm or less, or 2.5 nm or less, or 2 nm or less, or 1.5 nm or less. 50 The term "pore size" refers to the median pore size on a volume basis relative to the total volume of the micropores and mesopores. Thus, at least 50% of the total volume of the micropores and mesopores is preferably in the form of pores having a diameter of less than 30 nm.

[0027] PD of porous particle framework 30 The pore size may be 25 nm or less, or 20 nm or less, or 15 nm or less, or 12 nm or less, or 10 nm or less, or 8 nm or less, or 6 nm or less, or 5 nm or less, or 4 nm or less, or 3 nm or less, or 2.5 nm or less, or 2 nm or less, or 1 nm or less.

[0028] PD of porous particle framework 90 The pore size may be 35 nm or less, or 30 nm or less, or 25 nm or less, or 20 nm or less, or 15 nm or less, or 12 nm or less, or 10 nm or less, or 8 nm or less, or 6 nm or less, or 5 nm or less, or 4 nm or less, or 3 nm or less, or 2.5 nm or less, or 2 nm or less. 90 The pore size is at least 2.5 nm, or at least 3 nm, or at least 3.5 nm, or at least 4 nm. For example, the PD of the porous particle scaffold 90 The pore diameter is preferably in the range of 2.5 nm to 20 nm, or 3 nm to 15 nm, or 3.5 nm to 10 nm, or 4 nm to 8 nm.

[0029] PD of porous particle framework 10 The pore size may be 10 nm or less, or 9 nm or less, or 8 nm or less, or 7 nm or less, or 6 nm or less, or 5 nm or less, or 4 nm or less, or 3 nm or less, or 2.5 nm or less, or 2 nm or less, or 1.5 nm or less, or 1 nm or less. 10 The pore size is at least 0.3 nm, or at least 0.4 nm, or at least 0.5 nm. For example, the PD of the porous particle scaffold 10 The pore diameter is preferably in the range of 0.3 nm to 10 nm, or 0.3 nm to 5 nm, or 0.3 nm to 1 nm, or 0.4 nm to 1 nm, or 0.5 nm to 1 nm.

[0030] To avoid any misunderstanding, P.D. n For purposes of determining the value, any macropore volume (pore diameters greater than 50 nm) is not taken into account.

[0031] Preferably, the volume of the micropores in the porous particle framework is at least 0.25 cm 3 / g, or at least 0.3 cm 3 / g, at least 0.4 cm 3 / g, or at least 0.5 cm 3 Preferably, the volume of the micropores in the porous particle framework is less than 1.7 cm 3 / g or less, or 1.5cm 3 / g or less, or 1.2 cm 3 / g. The volume of the micropores in the porous particle framework is 0.3 cm 3 / g~1.7cm 3 / g, or 0.3 cm 3 / g~1.5cm 3 / g, or 0.3 cm 3 / g~1.2cm 3 The volume of the micropores in the porous particle framework may be in the range of 0.4 cm 3 / g~1.7cm 3 / g, or 0.5 cm 3 / g~1.7cm 3 The volume of the micropores in the porous particle framework may be in the range of 0.4 cm 3 / g~1.5cm 3 / g, or 0.5 cm 3 / g~1.2cm 3 / g range. While a certain amount of micropore-sized voids in the porous particle scaffold helps achieve deposition of small sized electroactive material domains within the pores, too high a micropore volume may overly restrict infiltration of the porous particle scaffold with the precursors of the electroactive and modifier domains.

[0032] The volume ratio of micropores to mesopores in the porous particle framework can in principle be in the range of 100:0 to 0:100. Preferably, the volume ratio of micropores to mesopores is 90:10 to 30:70, or 85:15 to 40:60, or 80:20 to 50:50, or 70:30 to 55:45.

[0033] The total volume of micropores and mesopores, as well as the pore size distribution of micropores and mesopores, were determined using quenched solid-state density functional theory (QSDFT) at 77 K for 10°C according to standard methodologies specified in ISO 15901-2 and ISO 15901-3. -6 The pore volume and pore size distribution are determined using nitrogen gas adsorption up to a relative pressure of p / p0. Nitrogen gas adsorption is a technique for characterizing the porosity and pore size distribution of a material by condensing a gas in the pores of a solid. As the pressure is increased, the gas condenses initially in the pores with the smallest diameter, until a saturation point is reached where all pores are filled with liquid. The nitrogen gas pressure is then reduced in stages to allow the liquid to evaporate from the system. The pore volume and pore size distribution can be determined by analysis of the adsorption and desorption isotherms and the hysteresis between them. Suitable instruments for measuring the pore volume and pore size distribution by nitrogen gas adsorption include the TriStar II and TriStar II Plus porosity analyzers available from Micromeritics Instrument Corporation, USA, and the Autosorb IQ porosity analyzer available from Quantachrome Instruments.

[0034] Nitrogen gas adsorption is effective for measuring the pore volume and pore size distribution of pores with diameters up to 50 nm, but is less reliable for pores with much larger diameters. Therefore, for the purposes of the present invention, nitrogen adsorption is used to determine the pore volume and pore size distribution of only pores with diameters up to 50 nm (i.e., only micropores and mesopores). Similarly, PD 50 The value of is determined for the total volume of micropores and mesopores only.

[0035] Given the limitations of available analytical techniques, it is not possible to measure the pore volume and pore size distribution over the full range of micropores, mesopores, and macropores using a single technique. When a porous particle or porous particle framework contains macropores, the volume of pores with diameters greater than 50 nm and ranging up to 100 nm can be measured by mercury intrusion porosimetry, preferably at a depth of 0.3 cm.3 / g or less, or 0.2 cm 3 / g or less, or 0.1cm 3 / g or less, or 0.05 cm 3 / g or less. Although a small proportion of macropores can be useful to facilitate electrolyte access into the pore network, the advantages of the present invention are substantially obtained by containing the silicon in the micropores and smaller mesopores.

[0036] Any pore volume measured by mercury porosimetry at pore diameters of 50 nm or less is disregarded (as described above, nitrogen adsorption is used to characterize mesopores and micropores). Pore volume measured by mercury porosimetry above 100 nm is assumed to be interparticle porosity for purposes of this invention, and this pore volume is also disregarded.

[0037] Mercury porosimetry is a technique for characterizing the porosity and pore size distribution of a material by applying various levels of pressure to a sample of the material immersed in mercury. The pressure required to force mercury into the pores of the sample is inversely proportional to the pore size. Mercury porosimetry values ​​reported herein were obtained according to ASTM UOP578-11, with a surface tension of mercury at room temperature, γ, of 480 mN / m and a contact angle, φ, of 140°. The density of mercury at room temperature is 13.5462 g / cm 3 There are many high-precision mercury intrusion instruments available commercially, such as the AutoPore IV series of automated mercury intrusion meters available from Micromeritics Instrument Corporation, USA. For a complete review of mercury intrusion methods, refer to "Analytical Methods in Fine Particle Technology, 1997, Micromeritics Instrument Corporation" by PA Webb and C. Orr (ISBN 0-9656783-0).

[0038] It will be understood that intrusion techniques such as gas adsorption and mercury porosimetry are only effective for determining the pore volume of pores accessible to nitrogen or mercury from the exterior of the porous particle. The porosity values ​​defined herein should be understood to refer to the open pores, i.e., the volume of pores accessible to fluids from the exterior of the porous particle. Completely enclosed pores that cannot be identified by nitrogen adsorption or mercury porosimetry shall not be considered in determining the porosity values ​​herein. Similarly, any pore volume located within pores that are small enough to be below the detection limit by nitrogen adsorption shall not be considered.

[0039] The pore size distribution of the porous particulate scaffold may be unimodal, bimodal or multimodal. As used herein, the term "pore size distribution" refers to the distribution of pore sizes relative to the cumulative total internal pore volume of the porous particulate scaffold. A bimodal or multimodal pore size distribution may be preferred, as the proximity of the micropores to the larger diameter pores provides the advantage of efficient transport of ions through the porous network to the silicon.

[0040] The porous particle scaffold is preferably at least 100 mm 2 / g, or at least 500m 2 / g, or at least 750m 2 / g, or at least 1000m 2 / g, or at least 1250m 2 / g, or at least 1500m 2 The term "BET surface area" as used herein should be taken to refer to the surface area per unit mass calculated from measurements of the physical adsorption of gas molecules on a solid surface using the Brunauer-Emmett-Teller theory and in accordance with ISO 9277. Preferably, the BET surface area of ​​the porous particle scaffold is greater than 4000 m 2 / g or less, or 3500m 2 / g or less, or 3250m 2 / g or less, or 3000m 2 / g or less, or 2500m 2 / g or less, or 2000m2 For example, the porous particle skeleton is 100 m 2 / g~4000m 2 / g, or 500m 2 / g~4000m 2 / g, or 750m 2 / g~3500m 2 / g, or 1000m 2 / g~3250m 2 / g, 1000m 2 / g~3000m 2 / g, or 1000m 2 / g~2500m 2 / g, or 1000m 2 / g~2000m 2 / g.

[0041] The porous particle skeleton is preferably electrically conductive. The electrically conductive porous particle skeleton comprises or consists of an electrically conductive carbon material. The electrically conductive porous carbon particle skeleton preferably comprises at least 80% by weight of carbon, more preferably at least 90% by weight of carbon, more preferably at least 95% by weight of carbon, optionally at least 98% by weight or at least 99% by weight of carbon. The carbon may be crystalline carbon or amorphous carbon, or a mixture of amorphous carbon and crystalline carbon. The carbon may be either carbon or soft carbon.

[0042] As used herein, the term "hard carbon" refers to carbon atoms that are primarily distributed in nanoscale polyaromatic domains. 2 It refers to a disordered carbon matrix that adopts a hybridized (three-way bond) state. The polyaromatic domains are cross-linked by chemical bonds, e.g., COC bonds. Because the polyaromatic domains are chemically cross-linked, the hard carbon cannot be converted to graphite at high temperatures. The high G band (approx. 1600 cm) in the Raman spectrum -1 ), hard carbon has graphite-like properties. However, the high D band in the Raman spectrum (approximately 1350 cm -1 ), carbon is not entirely graphite-like.

[0043] The term "soft carbon" as used herein also refers to carbon atoms that are primarily dispersed in polyaromatic domains having dimensions in the range of 5 nm to 200 nm. 2 It refers to a disordered carbon matrix that adopts a hybridized (three-way bond) state. In contrast to hard carbon, the polyaromatic domains in soft carbon are not cross-linked by chemical bonds but are held together by intermolecular forces; that is, at high temperatures, soft carbon can be graphitized. The porous carbon skeleton preferably has at least 50% sp 2 For example, the porous carbon skeleton preferably contains 50% to 98% sp 2 Hybrid carbon, 55%-95% sp 2 Hybrid carbon, 60%-90% sp 2 Hybrid carbon, or 70% to 85% sp 2 It may contain hybridized carbon.

[0044] A variety of different materials can be used to prepare porous particles suitable for forming porous particle scaffolds through pyrolysis. Examples of organic materials that can be used include plant biomass, including lignocellulosic materials (coconut shells, rice husks, wood, etc.), and fossil carbon sources such as coal. Examples of resins and polymeric materials that form porous carbon particles upon pyrolysis include phenolic resins, novolac resins, pitch, melamine, polyacrylates, polystyrene, polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), and various copolymers containing monomer units of acrylates, styrene, α-olefins, vinylpyrrolidone, and other ethylenically unsaturated monomers. Depending on the starting materials and the conditions of the pyrolysis process, a variety of different carbon materials are available in the art. A variety of different specifications of porous carbon particles are available from suppliers.

[0045] To increase the mesopore and micropore volume, the porous carbon particles can be subjected to a chemical or gas activation process. Suitable activation processes include contacting the pyrolyzed carbon with one or more of oxygen, steam, CO, CO2, and KOH at temperatures ranging from 600°C to 1000°C.

[0046] Mesopores can also be obtained by known templating processes using extractable pore formers such as MgO and other colloidal or polymeric templates, which can be removed by thermal or chemical means after pyrolysis or activation.

[0047] Alternatives to carbon-based particle skeletons include titanium nitride (TiN), titanium carbide (TiC), silicon carbide (SiC), and nickel oxide (NiO x ), titanium silicon nitride (TiSiN), nickel nitride (NiN), molybdenum nitride (MoN), titanium oxynitride (TiO x N 1-x ), silicon oxycarbide (SiOC), boron nitride (BN), or vanadium nitride (VN). Preferably, the porous particle skeleton comprises titanium nitride (TiN), silicon oxycarbide (SiOC) or boron nitride (BN). Further alternatives to carbon-based particle skeletons include metal oxides, such as those of the formula TiO x In one embodiment, the porous particle framework comprises an oxide of titanium having the formula: where x has a value greater than 1 and less than 2.

[0048] The porous particle scaffold may be irregular or spheroidal in shape.

[0049] The multiple electroactive material domains may each comprise the same electroactive material, or different electroactive material domains may comprise different electroactive materials. Preferably, the electroactive material domains comprise an electroactive material selected from elemental silicon, elemental tin, elemental germanium, elemental aluminum, and mixtures and alloys thereof. For example, some electroactive material domains may comprise (or consist of) elemental silicon, while other electroactive material domains may comprise (or consist of) elemental germanium. A preferred electroactive material is silicon. Preferably, at least some of the electroactive material domains comprise or consist of elemental silicon. More preferably, all of the electroactive material domains comprise or consist of elemental silicon.

[0050] As used herein, a "modifier material domain" refers to a material domain that has a chemical composition distinct from the electroactive material domain. At least a portion of the modifier material domain is located between adjacent electroactive material domains. The requirement that "at least a portion of the modifier material domain is located between adjacent electroactive material domains" should be interpreted to mean that the pore space of the porous particle framework is occupied successively by an electroactive material domain, then a modifier material domain, then a further electroactive material domain. Thus, the electroactive material does not form an extended network throughout the pore space, but is interrupted by the modifier material domain. Thus, within a single pore space, there is a sequence of: [Electroactive material domain(s)] ↓ [Modifier material domain(s)] ↓ [Electroactive material domain(s)] There is an assembly of material domains according to

[0051] This sequence of materials is generally obtained by sequentially depositing an electroactive material and a modifier material within the pores of a porous particulate scaffold, as discussed in more detail below, and the sequence can be extended, if desired, by further electroactive material domains and / or by further modifier material domains.

[0052] Modifier material domains located between adjacent electroactive material domains can act as a barrier separating the electroactive material domains and limit the length scale of consecutive electroactive material domains within the composite particle. Modifier material domains located between adjacent electroactive material domains can act as a barrier separating the electroactive material domains. Modifier material domains located between adjacent electroactive material domains can function to limit the length scale of consecutive electroactive material domains within the composite particle.

[0053] The electroactive material domain and the modifier material domain may be separate domains and there may be a clear boundary between the two, or there may be a compositional gradient between the electroactive domain and the modifier material domain. The modifier material domain may be a coating (e.g., a film) on at least some or all of the surface of the electroactive material domain. The modifier material domain may be chemically bonded (e.g., covalently, ionically, or metallically bonded) to the electroactive material domain. For example, the modifier material domain may comprise a passivation layer at the surface of the electroactive material domain, or may comprise an alloy of the electroactive material at the surface of the electroactive material domain, or may comprise a doped electroactive material at the surface of the electroactive material domain. Alternatively, the modifier material domain may not be chemically bonded to the electroactive material domain. For example, the modifier material may comprise or consist of a solid state electrolyte or an inert filler.

[0054] The modifier material domains may include one or more of carbon, nitrogen and / or oxygen.

[0055] The modifier material domain can be a passivation layer.

[0056] The modifier material domain may be an oxide passivation layer. One type of modifier material is, for example, a native oxide passivation layer formed by exposing the surface of the electroactive material domain to air or another oxygen-containing gas. When the electroactive material domain contains silicon, the modifier material domain may contain silicon oxide of the formula SiO x (where 0 < x ≦ 2). The silicon oxide is preferably amorphous silicon oxide.

[0057] The modifier material domain may be a nitride passivation layer. Another type of modifier material is, for example, a nitride passivation layer formed by exposing the surface of the electroactive material domain to ammonia or another nitrogen-containing molecule. When the electroactive material domain contains silicon, the modifier material domain may contain silicon nitride of the formula SiN x (where 0 < x ≦ 4 / 3). The silicon nitride is preferably amorphous silicon nitride. The nitride modifier material is more preferred than the oxide modifier material. Stoichiometric nitrides (e.g., SiN x (where 0 < x ≦ 4 / 3)) are conductive, so the nitride modifier domain functions as a conductive network that enables faster charging and discharging of the electroactive material. The nitride modifier material domain is also thought to improve the capacity retention rate. Phosphine may also be used as a passivating agent as a phosphorus analogue of ammonia.

[0058] The modifier material domain may be an oxynitride passivation layer. Another type of modifier material is, for example, an oxynitride passivation layer formed by exposing the surface of the electroactive material domain to ammonia (or another nitrogen-containing molecule) and oxygen gas. When the electroactive material domain contains silicon, the modifier material domain may contain silicon oxynitride of the formula SiO x N y (where 0 < x < 2, 0 < y < 4 / 3, and 0 < (2x + 3y) ≦ 4). The silicon nitride is preferably amorphous silicon oxynitride.

[0059] The modifier material domain may be a carbide passivation layer. Another type of modifier material is a carbide passivation layer. When the electroactive material domain contains silicon, the modifier material domain may contain silicon carbide of the formula SiC x (where 0 < x ≦ 1). The silicon carbide is preferably amorphous silicon carbide. The silicon carbide layer may be formed by contacting the electroactive material domain surface with a carbon-containing precursor, such as methane or ethylene, at an elevated temperature.

[0060] Another type of modifier material is a passivation layer that includes an organic moiety covalently bonded to at least a portion of the surface of the electroactive material domain. For example, the modifier material domain may include a carbon-containing organic moiety covalently bonded to the electroactive material domain surface. For example, the modifier material domain may include a hydrocarbyl covalently bonded to the electroactive material domain surface.

[0061] Passivating agents suitable for forming a passivation layer that includes an organic moiety include compounds that contain an alkene, alkyne or carbonyl functional group, more preferably a terminal alkene, terminal alkyne, aldehyde or ketone group.

[0062] The covalently bonded organic modifier material domain can be formed by inserting an organic compound into the M-H groups (where M represents an atom of the electroactive material) on the electroactive material surface to form a covalent passivation surface that is resistant to oxidation by air. When silicon is the electroactive material, the passivation reaction between the silicon surface and the passivating agent can be understood as one form of hydrosilylation as schematically shown below.

Chemical formula

[0063] Because hydride terminations can decompose to produce hydrogen gas, which can be detrimental to the electrode topography, it is advantageous to replace the hydride terminations at the surface of the electroactive material domains with covalently bonded organic modifier material domains, such as carbon-containing organic moieties. Additionally, the Si-C bonds are believed to improve electrical conductivity.

[0064] Suitable organic compounds that can be used to form modifier material domains through passivation of the electroactive material domain surfaces include compounds that contain an alkene, alkyne or carbonyl functional group, more preferably a terminal alkene, terminal alkyne or aldehyde group. For example, the modifier material domains may be formed by passivation of the electroactive material domain surfaces with one or more compounds of the following formula:

[0065] Preferred passivating agents include those having the following formula: (i)R 1 -CH=CH-R 1 , (ii)R 1 -C≡CR 1 , and (iii) O=CR 1 R 1 (In the formula, each R 1 independently represent H, an unsubstituted or substituted aliphatic or aromatic hydrocarbyl group having 1 to 20 carbon atoms, or two R 1 The group includes one or more compounds that form an unsubstituted or substituted ring structure containing 3 to 8 carbon atoms in the ring.

[0066] The modifier material may be a hydrocarbyl covalently bonded to the surface of at least a portion of the electroactive material domain. The modifier material may be a C 2~22 The modifier material may be a saturated or unsaturated C group covalently bonded to the surface of at least a portion of the electroactive material domains. 2~22 The modifier material may be a linear or branched C aryl group covalently bonded to the surface of at least a portion of the electroactive material domains.2~22 The modifier material may be a monocyclic or polycyclic C group covalently bonded to the surface of at least a portion of the electroactive material domains. 2~22 The modifier material may be a hydrocarbyl. The modifier material may be a C that is covalently bonded to the surface of at least a portion of the electroactive material domains. 2~22 Alkyl, C 2~22 Alkenyl, C 2~22 Alkynyl, C 3~22 Cycloalkyl, C 3~22 Cycloalkenyl, C 3~22 Cycloalkynyl or C 6~22 The modifier material may be covalently bonded to the surface of at least a portion of the electroactive material domains. [ka] It will be understood that the bond crossed by the dotted line is to an atom on the surface of the electroactive material domain. For example, if the electroactive material is silicon, the bond crossed by the dotted line is to Si.

[0067] Particularly preferred passivators include those having the formula: (i) CH2=CH-R 1 , and (ii) HC≡CR 1 (In the formula, R 1 is as defined above. 1 is non-substitutive.

[0068] Specific examples of suitable organic compounds that can be used to form modifier material domains through passivation of the electroactive material domain surfaces include ethylene, propylene, 1-butene, butadiene, 1-pentene, 1,4-pentadiene, 1-hexene, 1-octene, styrene, divinylbenzene, acetylene, phenylacetylene, norbornene, norbornadiene, and bicyclo[2.2.2]oct-2-ene. Mixtures of different passivating agents can also be used.

[0069] Further examples of organic compounds that can be used to form modifier material domains through passivation of the electroactive material domain surface include compounds that contain an active hydrogen atom bonded to oxygen, nitrogen, sulfur, or phosphorus. For example, the passivator may be an alcohol, amine, thiol, or phosphine. It is understood that reaction of an -XH group with a hydride group at the electroactive material surface results in the elimination of H2 and the formation of a direct bond between X and the electroactive material surface.

[0070] Suitable passivators in this category include those having the following formula: (iv) HX-R 2 , and (v) HX-C(O)-R 1 (wherein X is O, S, NR 1 Or PR 1 Each R 1 are independently as defined above, and R 2 represents an unsubstituted or substituted aliphatic or aromatic hydrocarbyl group having 1 to 20 carbon atoms, or R 1 and R 2 taken together form an unsubstituted or substituted ring structure containing 3 to 8 carbon atoms in the ring.

[0071] Preferably, X represents O or NH. Particularly preferably, X represents NH.

[0072] Preferably, R 2 represents an optionally substituted aliphatic or aromatic group having from 2 to 10 carbon atoms. Amine groups may also be incorporated into 4- to 10-membered aliphatic or aromatic ring structures, such as in pyrrolidine, pyrrole, imidazole, piperazine, indole, or purine.

[0073] As a further alternative, the modifier material domain may comprise a pyrolytic carbon material, which may be formed by CVI using a suitable carbon-containing precursor, as discussed in more detail below. The use of pyrolytic carbon materials is advantageous in that the surface area of ​​the composite particles is significantly reduced, which is believed to improve cycle life and preserve capacity.

[0074] As a further alternative, the modifier material domains may be conductive metals or metal alloys. Conductive metal or metal alloy domains may be formed by CVI using suitable metal-containing precursors, as discussed in more detail below. Examples of suitable conductive metals include silver, gold, copper, and titanium.

[0075] As a further alternative, the modifier material domain may include an electroactive material comprising a dopant selected from the group consisting of boron, aluminum, gallium, indium, phosphorus, arsenic, antimony and bismuth. The dopant is preferably boron or phosphorus. The electroactive material may be the same electroactive material in the electroactive material domain or may be different. The electroactive material may be selected from the group consisting of elemental silicon, elemental tin, elemental germanium, elemental aluminum, and mixtures and alloys thereof. The preferred electroactive material is silicon.

[0076] As a further alternative, the modifier material domain may comprise or consist of a solid-state electrolyte, which may be an organic solid electrolyte or an inorganic solid electrolyte.

[0077] Examples of organic solid electrolytes include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate ester polymers, polyester sulfides, polyvinyl alcohol, polyvinylidene fluoride, and polymers containing ionically dissociable groups.

[0078] Examples of inorganic solid electrolytes include nitrides, halides and sulfides of lithium salts, such as Li5NI2, Li3N, LiI, LiSiO4, Li2SiS3, Li4SiO4, LiOH and Li3PO4.

[0079] As a further alternative, the modifier material domain may include or consist of an inert filler.

[0080] It is preferred that the modifier material is oxygen-free. The use of oxygen-free modifier materials is believed to contribute to providing composite particles with a low total oxygen content, which is believed to reduce first cycle losses, improve electronic conductivity, improve cycle life, and maintain capacity. Examples of oxygen-free modifier materials include nitride passivation layers, carbide passivation layers, hydrocarbyls covalently bonded to electroactive material domain surfaces, pyrolytic carbon materials, conductive metals or metal alloys, electroactive materials containing dopants, solid state electrolytes, and inert fillers.

[0081] In a preferred embodiment, the modifier material comprises a hydrocarbyl (e.g., C) group covalently bonded to the surface of at least a portion of the electroactive material domains. 2~22 Hydrocarbyl), or nitride passivation layers as described herein. These modifier materials are believed to provide lower total oxygen content, improve electrical conductivity, and reduce chemical reactivity of the electroactive material domains.

[0082] The composite particles may optionally further include outer modifier material domains located between the outermost electroactive material domain and the exterior of the composite particle. These modifier material domains form a barrier between the electroactive material and the exterior of the composite particle, thereby inhibiting contact of the outermost electroactive material domain with the electrolyte that would otherwise tend to result in SEI formation. The outer modifier material domains may be formed from any of the modifier materials described herein. A preferred modifier material for the outer modifier material domains is a pyrolytic carbon material. Another preferred modifier material for the outer modifier material domains is a native oxide of the electroactive material.

[0083] In a preferred embodiment, the particulate material of the present invention comprises a plurality of elemental silicon domains (as electroactive domains) and a plurality of modifier material domains disposed within the interior pore volume of a porous particle framework, the modifier material domains comprising organic moieties located between adjacent elemental silicon domains and a passivation layer covalently bonded to the surface of at least a portion of the elemental silicon domains. The composite particle may further comprise an outer modifier material domain which is a silicon oxide domain.

[0084] In a further preferred embodiment, the particulate material of the present invention comprises a plurality of elemental silicon domains (as electroactive domains) and a plurality of pyrolytic carbon domains disposed within the interior pore volume of the porous particle framework, at least a portion of the pyrolytic carbon domains being located between adjacent elemental silicon domains. The composite particle may further comprise an outer modifier material domain which is a silicon oxide domain.

[0085] In a further preferred embodiment, the particulate material of the present invention comprises a plurality of elemental silicon domains (as electroactive domains) and a plurality of metal or metal alloy domains disposed within the interior pore volume of the porous particle framework, at least some of the metal or metal alloy domains being located between adjacent elemental silicon domains. The composite particle may further comprise an outer modifier material domain which is a silicon oxide domain.

[0086] A range of different electroactive material loadings in the composite particles may be used in the present invention. For example, the amount of electroactive material in the composite particles may range from 5% to 85% by weight, based on the total mass of the composite particle. Preferably, the amount of electroactive material in the composite particles is 10% to 85% by weight, or 15% to 85% by weight, or 20% to 80% by weight, or 25% to 80% by weight, or 30% to 75% by weight, or 35% to 75% by weight, or 40% to 70% by weight, or 45% to 65% by weight, based on the total mass of the composite particle.

[0087] The composite particles can comprise 40% to 70% by weight, or 45% to 70% by weight, or 48% to 70% by weight, or 50% to 70% by weight, or 40% to 65% by weight, or 45% to 65% by weight, or 48% to 65% by weight, or 50% to 65% by weight, or 40% to 60% by weight, or 45% to 60% by weight, or 48% to 60% by weight, or 50% to 60% by weight of the electroactive material, based on the total mass of the composite particle.

[0088] Preferably, the composite particles comprise 10% to 85% by weight, or 15% to 85% by weight, or 20% to 80% by weight, or 25% to 80% by weight, or 30% to 75% by weight, or 35% to 75% by weight, or 40% to 70% by weight, or 45% to 65% by weight of silicon based on the total mass of the composite particles.

[0089] The composite particles may contain 40% to 70% by weight, or 45% to 70% by weight, or 48% to 70% by weight, or 50% to 70% by weight, or 40% to 65% by weight, or 45% to 65% by weight, or 48% to 65% by weight, or 50% to 65% by weight, or 40% to 60% by weight, or 45% to 60% by weight, or 48% to 60% by weight, or 50% to 60% by weight of silicon based on the total mass of the composite particles.

[0090] The amount of electroactive material (e.g., silicon) in the composite particles can be selected such that at least 25% and up to 90% or more of the internal pore volume of the porous particle skeleton is occupied by the electroactive material. For example, the electroactive material (e.g., silicon) may occupy 25%-80%, or 25%-60%, or 25%-55%, or 30%-50%, or 53%-55%, or 40%-60%, or 25%-45%, or 25%-40% of the internal pore volume of the porous particle skeleton. Within these preferred ranges, the pore volume of the porous particle skeleton is effective to accommodate the expansion of the electroactive material (e.g., silicon) during charge and discharge, but excess pore volume that does not contribute to the volumetric capacity of the particulate particles is avoided. However, the amount of electroactive material is also not so high as to prevent effective lithiation due to inadequate metal ion diffusion rates or due to inadequate expansion volume resulting in mechanical resistance to lithiation.

[0091] When the electroactive material is silicon, the amount of silicon in the composite particles is determined by the mass ratio of silicon to porous particle skeleton of [0.5 × P 1 ~1.9×P 1 ]:1, where P 1 is cm 3 The total pore volume of the micropores and mesopores in the porous particle framework is a dimensionless quantity, expressed as a measure of the total pore volume of the micropores and mesopores in the porous particle framework, expressed as g / g (e.g., if the porous particle or porous particle framework has a volume of 1.2 cm 3 / g, then P 1 = 1.2). This relationship takes into account the density of silicon and the pore volume of the porous particle framework, and defines the weight ratio of silicon at which the pore volume is approximately 20% to 82% occupied.

[0092] The amount of electroactive material (e.g. silicon) in the composite particles can be determined by elemental analysis. Elemental analysis can be used to determine the composition of the porous particles that form only the porous particle skeleton, and the composition of the composite particles containing the electroactive material. For example, determining the weight percentage of carbon in the porous carbon particles only takes into account the possibility that the porous carbon particles contain trace amounts of heteroatoms. Both measurements taken together allow the weight percentage of the electroactive material (e.g. silicon) relative to the porous carbon particles to be reliably determined.

[0093] The silicon content is preferably determined by ICP-OES (Inductively Coupled Plasma Optical Emission Spectroscopy). Many ICP-OES instruments are commercially available, such as the iCAP™ 7000 series of ICP-OES analyzers available from ThermoFisher Scientific. The carbon content (and optionally the hydrogen, nitrogen and oxygen content) in the composite particles and in the porous carbon particles alone is preferably determined by IR absorption. A suitable instrument for determining the carbon, hydrogen, nitrogen and oxygen content is the TruSpec™ Micro elemental analyzer available from Leco Corporation.

[0094] At least 85% by weight of the electroactive material mass in the composite particles can be located within the internal pore volume of the porous particle skeleton. Preferably, at least 90% by weight, more preferably at least 95% by weight, and even more preferably at least 98% by weight of the electroactive material (e.g., silicon) mass in the composite particles is located within the internal pore volume of the porous particle skeleton, with no or little electroactive material (e.g., silicon) located on the external surface of the composite particles. The reaction kinetics of the CVI process ensure that preferential deposition of the electroactive material (e.g., silicon) occurs on the internal surface of the porous particles.

[0095] The composite particles preferably have a low total oxygen content. Oxygen may be present in the composite particles, for example, as part of the porous particle skeleton or as an oxide layer on any exposed silicon surface. Preferably, the total oxygen content of the composite particles is less than 15% by weight, more preferably less than 10% by weight, more preferably less than 5% by weight, for example less than 4% by weight, or less than 3% by weight, or less than 2% by weight, or less than 1% by weight, or less than 0.5% by weight, based on the total mass of the composite particles. Preferably, the total oxygen content of the composite particles is less than 5% by weight, or less than 4% by weight, or less than 3% by weight, or less than 2% by weight, or less than 1% by weight, or less than 0.5% by weight, based on the total mass of the composite particles.

[0096] The composite particles may comprise a ratio of total oxygen content to silicon content relative to the total mass of the composite particles of 0.1:1 or less.

[0097] The composite particles preferably have a low total chlorine content. Chlorine may be present in the composite particles, for example, as part of the by-product of electroactive material deposition. Preferably, the total chlorine content of the composite particles is less than 100 ppm, or less than 90 ppm, or less than 80 ppm, or less than 70 ppm, based on the total mass of the composite particles. Without being bound by theory, it is believed that chlorine is an impurity in the composite particles that is detrimental to cell performance.

[0098] The composite particles preferably have a low total content of transition metals and / or alkali metals, for example the total content of transition metals and alkali metals in the composite particles may be less than 0.5 wt.-%, based on the total weight of the composite particles.

[0099] Optionally, the composite particle comprises 0.0001% to 0.5% by weight, such as 0.001% to 0.1% by weight, of zirconium based on the total mass of the composite particle.

[0100] The composite particles preferably have a D in the range of 0.5 μm to 30 μm. 50 The composite particles at the end of the CVI process have a particle diameter of D 50If the particle size is greater than 30 μm, it is preferably milled, for example by milling, to a D of 30 μm or less prior to use in electrode manufacture. 50 Reduce the size of the composite particles to a particle size of 30 μm or less D 50 The composite particles with particle size have excellent dispersibility in slurries, structural robustness, and high capacity retention over repeated charge-discharge cycles, making them suitable for forming dense electrode layers of uniform thickness in the conventional thickness range of 20 μm to 50 μm.

[0101] Optionally, D for composite particles 50 The particle size may be at least 1 μm, or at least 2 μm, or at least 3 μm, or at least 4 μm, or at least 5 μm. 50 The particle size may be 20 μm or less, or 18 μm or less, or 16 μm or less, or 14 μm or less, or 12 μm or less, or 10 μm or less, or 8 μm or less.

[0102] For example, the composite particles may have a D in the range of 1 μm to 25 μm, or 1 μm to 20 μm, or 1 μm to 18 μm, or 1 μm to 16 μm, or 2 μm to 16 μm, or 2 μm to 14 μm, or 2 μm to 12 μm, or 2 μm to 10 μm, or 2 μm to 8 μm. 50 It can have a particle size.

[0103] Composite particle D 10 The particle size is preferably at least 0.5 μm, or at least 0.8 μm, or at least 1 μm. 10 Maintaining particle size at or above 0.5 μm reduces the potential for undesirable agglomeration of submicron sized particles, improving dispersibility of the particulate material and improving capacity retention.

[0104] Composite particle D 90The particle size is preferably 50 μm or less, or 40 μm or less, or 30 μm or less, or 25 μm or less, or 20 μm or less, or 15 μm or less. The presence of very large particles leads to uneven particle packing in the electrode active layer, which hinders the formation of a dense electrode layer, especially an electrode layer having a thickness in the range of 20 μm to 50 μm. Therefore, D 90 Preferably the particle size is up to 40 μm, more preferably even smaller.

[0105] The composite particles preferably have a narrow particle size distribution span. For example, the particle size distribution span (D 90 -D 10 ) / D 50 (defined as) is preferably 5 or less, more preferably 4 or less, more preferably 3 or less, more preferably 2 or less, and most preferably 1.5 or less. By maintaining a narrow particle size distribution span, efficient packing of the particles into a dense electrode layer can be more easily achieved.

[0106] For the avoidance of doubt, the term "particle size" as used herein refers to the equivalent spherical diameter (esd), i.e., the diameter of a sphere having the same volume as a given particle, where the volume of the particle is understood to include the volume of the pores within the particle. 50 " and "D 50 The term "particle size" refers to the median particle size on a volume basis, i.e., the diameter below which 50% by volume of the particle population lies. 10 " and "D 10 The term "particle size" refers to the 10th percentile median particle size on a volume basis, i.e., the diameter below which 10% by volume of the particle population lies. 90 " and "D 90 The term "particle size" refers to the volume-based 90th percentile median particle diameter, i.e., the diameter below which 90% of the particle population falls, by volume.

[0107] Particle size and size distribution can be determined by standard laser diffraction techniques according to ISO 13320:2009. Laser diffraction is based on the principle that particles scatter light at angles that vary with the size of the particle, and a collection of particles produces a scattered light pattern defined by intensity and angle that can be correlated to particle size distribution. Many laser diffraction instruments are commercially available for quickly and reliably determining particle size distribution. Unless otherwise stated, particle size distribution measurements specified or reported herein are measured by a conventional Malvern Mastersizer™ 3000 particle size analyzer manufactured by Malvern Instruments™. The Malvern Mastersizer™ 3000 particle size analyzer works by projecting a helium neon gas laser beam through a transparent cell containing particles of interest suspended in an aqueous solution. The light that strikes the particles is scattered at angles that are inversely proportional to the particle size, and a photodetector array measures the light intensity at several predetermined angles, and the intensities measured at the various angles are processed by a computer using standard theoretical principles to determine the particle size distribution. Laser diffraction values ​​as reported herein are obtained using a wet dispersion of particles in 2-propanol with the addition of 5% by volume of the surfactant SPAN™-40 (sorbitan monopalmitate). The particle refractive index is taken to be 2.68 for porous particles and 3.50 for composite particles, and the dispersant refractive index is taken to be 1.378. The Mie scattering model is used to calculate the particle size distribution.

[0108] The composite particles are preferably 0.35 cm 3 / g or less, or 0.25 cm 3 / g or less, or 0.15 cm 3 / g or less, or 0.1cm 3 / g or less, or 0.05 cm 3 / g or less, or 0.03 cm 3 / g or less, or 0.02 cm 3The composite particles have a total volume of micropores and / or mesopores, as measured by nitrogen gas adsorption as described herein, that is 20% by volume or less, more preferably 15% by volume or less, or 10% by volume or less, or 5% by volume or less, of the total volume of micropores and / or mesopores of the porous particle framework. A lower total volume of micropores and / or mesopores in the composite particles reduces the penetration of the composite particles by electrolyte solvents that cause SEI formation therein, reducing the overall surface area and providing better control over avoiding undesirable surface reactions during use.

[0109] The composite particles are preferably 300 mm 2 / g or less, or 250m 2 / g or less, or 200m 2 / g or less, or 150m 2 / g or less. More preferably, it has a BET surface area of ​​100 m 2 / g or less, or 80m 2 / g or less, or 60m 2 / g or less, or 50m 2 / g or less, or 40m 2 / g or less, or 30m 2 / g or less, or 25m 2 / g or less, or 20m 2 / g or less, or 15m 2 / g or less, or 10m 2 / g or less, or 5m 2 Preferably, the composite particles have a particle size of 30m 2 / g or less, or 25m 2 / g or less, or 20m 2 / g or less, or 15m 2 / g or less, or 10m 2 / g or less, or 5m 2The composite particles have a BET surface area of ​​0.1 m / g or less. Generally, a low BET surface area is preferred to minimize the formation of a solid electrolyte interfacial (SEI) layer on the surface of the composite particles during the first charge-discharge cycles of the anode. However, if the BET surface area is too low, the charge rate and capacity will be unacceptably low due to the inaccessibility of the metal ions to the bulk of the electroactive material in the surrounding electrolyte. For example, the BET surface area is 0.1 m 2 / g~100m 2 / g, or 0.1m 2 / g~80m 2 / g, or 0.5m 2 / g~60m 2 / g, or 0.5m 2 / g~40m 2 / g, or 1m 2 / g~30m 2 / g, or 1m 2 / g~25m 2 / g, or 2m 2 / g~20m 2 / g.

[0110] The composite particles can have an irregular or spheroidal shape. The spheroidal particles as defined herein can include both spherical and spheroidal particles, and the shape of the composite particles of the present invention can be preferably defined by referring to the sphericity and aspect ratio of the particles of the present invention. It has been found that spheroidal particles are particularly suitable for dispersion in slurries without forming agglomerates. It has also been found that the use of porous spheroidal particles surprisingly provides additional strength improvement when compared to irregularly shaped porous particles and porous particle fragments.

[0111] The sphericity of an object is conventionally defined as the ratio of the surface area of ​​the object to that of a sphere, where the object and the sphere have the same volume. However, in practice, it is difficult to measure the surface area and volume of individual micron-scale particles. However, by scanning electron microscopy (SEM) and dynamic image analysis, where the shadow cast by the particle is recorded using a digital camera, highly accurate two-dimensional projection images of micron-scale particles can be obtained. The term "sphericity" as used herein shall be understood as the ratio of the area of ​​the particle projection image to the area of ​​a circle, where the particle projection image and the circle have the same circumference. Thus, for an individual particle, the sphericity S may be defined as follows:

number

number

[0112] The term "spheroidal" as used herein as applied to the composite particles of the present invention shall be understood to refer to materials having an average sphericity of at least 0.70. The composite particles of the present invention preferably have an average sphericity of at least 0.85, more preferably at least 0.90, more preferably at least 0.92, more preferably at least 0.93, more preferably at least 0.94, more preferably at least 0.95. The composite particles can optionally have an average sphericity of at least 0.96, or at least 0.97, or at least 0.98, or at least 0.99.

[0113] It will be appreciated that the circumference and area of ​​a two-dimensional particle projection image will depend on the particle orientation for any particle that is not perfectly spheroidal. However, the effect of particle orientation can be countered by reporting sphericity and aspect ratio as average values ​​obtained from multiple particles with random orientation. Many SEM and dynamic image analyzers are commercially available that can rapidly and reliably determine the sphericity and aspect ratio of particulate materials. Unless otherwise stated, sphericity values ​​specified or reported herein are measured by a CamSizer XT particle analyzer manufactured by Retsch Technology GmbH. The CamSizer XT is a dynamic image analyzer that can obtain highly accurate distributions of size and shape of particulate materials for sample volumes between 100 mg and 100 g, and properties such as average sphericity and aspect ratio can be calculated directly with this instrument.

[0114] The composite particles may be further characterized by their performance under thermogravimetric analysis (TGA) in air, which is based on the principle that when an electroactive material is oxidized in air and at elevated temperatures, a weight gain is observed.

[0115] As defined herein, "surface silicon" is calculated from the initial mass increase in a TGA trace from a minimum between 150°C and 500°C to a maximum mass measured in the temperature range between 550°C and 650°C, the TGA being performed in air at a heating rate of 10°C / min. This mass increase is assumed to result from oxidation of the surface silicon and is therefore calculated according to the following formula: Y = 1.875 × [(M max -M min ) / M f ]×100% where Y is the percentage of surface silicon as a proportion of the total silicon in the sample, and M max is the maximum mass of the sample measured in the temperature range between 550°C and 650°C, and M min is the minimum mass of the sample at temperatures greater than 150°C and less than 500°C, and M fThe percentage of surface silicon as a proportion of the total amount of silicon can be determined according to (where 1.875 is the mass of the sample at the completion of oxidation at 1400°C). For completeness, it will be understood that 1.875 is the molar mass ratio of SiO2 to O2 (i.e., the mass ratio of SiO2 formed to the mass increase due to the addition of oxygen). Typically, TGA analysis is performed using a sample size of 10 mg ± 2 mg.

[0116] It has been found that reversible capacity retention over multiple charge / discharge cycles is significantly improved when surface silicon, as determined by the TGA method described above, is at least 20% by weight of the total silicon in the material.Preferably, at least 22% by weight of the silicon, or at least 25% by weight, at least 30% by weight, or at least 35% by weight of the silicon, or at least 40% by weight of the silicon, or at least 45% by weight of the silicon is surface silicon, as determined by thermogravimetric analysis (TGA).

[0117] In addition to a high surface silicon content, the particulate material of the present invention preferably has a low content of coarse bulk silicon as determined by TGA. Coarse bulk silicon is defined herein as silicon that undergoes oxidation above 800° C. as determined by TGA, where the TGA is performed in air at a heating rate of 10° C. / min. Thus, the coarse bulk silicon content is calculated according to the following formula: Z = 1.875 × [(M f -M 800 ) / M f ]×100% (where Z is the percentage of unoxidized silicon at 800°C, M 800 is the mass of the sample at 800 °C, M f is the mass of ash at completion of oxidation at 1400°C). For the purposes of this analysis, any mass increase above 800°C corresponds to the oxidation of silicon to SiO2, and it is assumed that the total mass at completion of oxidation is SiO2. Typically, TGA analysis is performed using a sample size of 10 mg ± 2 mg.

[0118] Silicon that undergoes oxidation above 800° C. is less desirable. Preferably, no more than 10% by weight, or no more than 8% by weight, or no more than 6% by weight, or no more than 5% by weight, or no more than 4% by weight, or no more than 3% by weight, or no more than 2% by weight, or no more than 1.5% by weight of the silicon is crude bulk silicon as determined by TGA.

[0119] Preferably, at least 20% by weight of the silicon is surface silicon and not more than 10% by weight of the silicon is crude bulk silicon, both as determined by TGA. More preferably, at least 30% by weight of the silicon is surface silicon and not more than 10% by weight of the silicon is crude bulk silicon, both as determined by TGA. More preferably, at least 35% by weight of the silicon is surface silicon and not more than 8% by weight of the silicon is crude bulk silicon, both as determined by TGA. More preferably, at least 40% by weight of the silicon is surface silicon and not more than 5% by weight of the silicon is crude bulk silicon, both as determined by TGA. More preferably, at least 45% by weight of the silicon is surface silicon and not more than 2% by weight of the silicon is crude bulk silicon, both as determined by TGA.

[0120] The composite particles preferably have a specific charge capacity of 1200 mAh / g to 2340 mAh / g upon initial lithiation. Preferably, the composite particles have a specific charge capacity of at least 1400 mAh / g upon initial lithiation.

[0121] The composite particles may include a coating of a lithium ion permeable material, such as a carbon coating. The lithium ion permeable material coating has the advantage of further reducing the BET surface area of ​​the composite particles by smoothing any surface defects and filling any remaining surface microporous structure, thereby further reducing first cycle losses. In addition, the lithium ion permeable material coating improves the electrical conductivity of the composite particle surface, reducing the need for conductive additives in the electrode composition, and also creates an optimal surface for the formation of a stable SEI layer, resulting in improved capacity retention upon cycling.

[0122] The reduction in the composite particle surface area also has the effect of reducing the amount of binder required to form an electrode active layer that includes the composite particles. Excess binder is known to contribute to reduced rate performance. A further advantage of the present invention is that the filler contributes to improving the compressive strength of the composite particles by providing structural reinforcement to the porous particle framework.

[0123] When a carbon coating is present, the composite particles are preferably 2 / g or less, or 100m 2 / g or less, or 80m 2 / g or less, or 60m 2 / g or less, or 40m 2 / g or less, or 30m 2 / g or less, or 25m 2 / g or less, or 20m 2 / g or less, or 15m 2 / g or less, or 10m 2 / g or less, or 5m 2 / g or less, or 3m 2 / g or less BET surface area.

[0124] In a second aspect, the present invention provides a method for preparing a composite particle, comprising the steps of: (a) The total pore volume of micropores and mesopores as measured by gas adsorption is 0.4 cm 3 / g~2.2cm 3providing a plurality of porous particles comprising micropores and / or mesopores, the micropores and / or mesopores being in the range of 0.1 μm / g; (b) contacting the porous particles with a precursor of an electroactive material at a temperature effective to cause deposition of a plurality of electroactive material domains in the pores of the porous particles; (c) forming a plurality of modifier material domains in the pores of the porous particles and adjacent to the electroactive material domains deposited in step (b); (d) contacting the particles from step (c) with a precursor of an electroactive material at a temperature effective to cause deposition of additional electroactive material domains in the pores of the porous particles and adjacent to the modifier material domains formed in step (c); The present invention provides a method comprising:

[0125] The method of the invention is therefore a multi-step process comprising, in sequence, a first step of depositing an electroactive material, a step of forming a modifier material adjacent to the electroactive material, and a further step of depositing an electroactive material adjacent to the modifier material. This sequence of steps results in a product from step (d) where at least a portion of the modifier material domain is located between the electroactive material deposited in step (b) and the electroactive material deposited in step (d). The product of the method of the second aspect of the invention is therefore a particulate material according to the first aspect of the invention.

[0126] As discussed above, the porous particles used in step (a) form a porous particle skeleton in the composite particle. The term "porous particle skeleton" is used in the context of the composite particle product, while the term "porous particle" is used to describe the starting material that ultimately forms the porous particle skeleton. Thus, the porous particles used in step (a) of the method of the second aspect of the invention may have any of the features of the porous particle skeleton described herein in the context of the first aspect of the invention. The features of the porous particle skeleton may optionally be combined with any of the further features of the porous particle as set forth below.

[0127] Generally, porous particles have a D in the range of 0.5 μm to 200 μm. 50 Optionally, the porous particles may have a particle size D 50 The particle size may be at least 1 μm, or at least 1.5 μm, or at least 2 μm, or at least 2.5 μm, or at least 3 μm, or at least 4 μm, or at least 5 μm. Optionally, the D of the porous particles 50 The particle size may be 150 μm or less, or 100 μm or less, or 70 μm or less, or 50 μm or less, or 40 μm or less, or 30 μm or less, or 25 μm or less, or 20 μm or less, or 18 μm or less, or 15 μm or less, or 12 μm or less, or 10 μm or less, or 8 μm or less.

[0128] For example, the porous particles may have a diameter of 0.5 μm to 150 μm, or 0.5 μm to 100 μm, or 0.5 μm to 50 μm, or 0.5 μm to 30 μm, or 1 μm to 25 μm, or 1 μm to 20 μm, or 2 μm to 25 μm, or 2 μm to 20 μm, or 2 μm to 18 μm, or 2 μm to 15 μm, or 2 μm to 12 μm, or 2.5 D in the range of μm to 15 μm, or 2.5 μm to 12 μm, or 2 μm to 10 μm, or 3 μm to 20 μm, or 3 μm to 18 μm, or 3 μm to 15 μm, or 4 μm to 18 μm, or 4 μm to 15 μm, or 4 μm to 12 μm, or 5 μm to 15 μm, or 5 μm to 12 μm, or 5 μm to 10 μm, or 5 μm to 8 μm 50 Particles within these size ranges and having porosities and pore size distributions as set forth herein are ideally suited for the preparation of composite particles for use in anodes for metal ion batteries by the CVI process.

[0129] D of porous particles 10 The particle size is preferably at least 0.2 μm, or at least 0.5 μm, or at least 0.8 μm, or at least 1 μm, or at least 1.5 μm, or at least 2 μm. 10 Maintaining particle size above 0.2 μm reduces the potential for undesirable agglomeration of submicron sized particles and improves dispersibility of the composite particles.

[0130] D of porous particles 90 The particle size is preferably 300 μm or less, or 250 μm or less, or 200 μm or less, or 150 μm or less, or 100 μm or less, or 80 μm or less, or 60 μm or less, or 40 μm or less, or 30 μm or less, or 25 μm or less, or 20 μm or less.

[0131] The porous particles preferably have a narrow particle size distribution span. For example, the particle size distribution span (D 90 -D 10 ) / D 50 (defined as) is preferably 5 or less, more preferably 4 or less, more preferably 3 or less, more preferably 2 or less, and most preferably 1.5 or less. By maintaining a narrow particle size distribution span, efficient packing of particles into a dense powder bed is more easily achievable.

[0132] The porous particles preferably have a diameter of at least 100 mm. 2 / g, or at least 500m 2 / g, or at least 750m 2 / g, or at least 1000m 2 / g. The term "BET surface area" as used herein should be taken to refer to the surface area per unit mass calculated from measurements of the physical adsorption of gas molecules on a solid surface using the Brunauer-Emmett-Teller theory and in accordance with ISO 9277. Preferably, the BET surface area of ​​the porous particles is greater than 4000 m 2 / g or less, or 3500m 2 / g or less, or 3250m 2 / g or less, or 3000m 2 / g, or 2500m 2 / g or less, or 2000m 2 For example, the porous particles have a particle size of 100 m 2 / g~4000m 2 / g, or 500m 2 / g~4000m 2 / g, or 750m 2 / g~3500m2 / g, or 1000m 2 / g~3250m 2 / g, 1000m 2 / g~3000m 2 / g, or 1000m 2 / g~2500m 2 / g, or 1000m 2 / g~2000m 2 / g.

[0133] The porous particles may have an average sphericity (as defined above) of greater than 0.5. Preferably, the porous particles have an average sphericity of at least 0.55, or at least 0.6, or at least 0.65, or at least 0.7, or at least 0.75, or at least 0.8, or at least 0.85. Preferably, the porous particles have an average sphericity of at least 0.90, or at least 0.92, or at least 0.93, or at least 0.94, or at least 0.95.

[0134] Preferably, the porous particles are (i) 0.4 cm 3 / g~2.2cm 3 the total pore volume of micropores and mesopores as measured by nitrogen gas adsorption in the range of 1 / g; (ii) PD less than 20 nm 50 Pore ​​diameter, preferably PD of 30 nm or less 90 Pore ​​size, preferably PD of 15 nm or less 30 Pore ​​size, and (iii) D in the range of 0.5 μm to 30 μm 50 particle size, and optionally (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), has.

[0135] More preferably, the porous particles are (i) 0.6 cm 3 / g~1.8cm 3the total pore volume of micropores and mesopores as measured by nitrogen gas adsorption in the range of 1 / g; (ii) PD less than 10 nm 50 Pore ​​diameter, preferably PD of 20 nm or less 90 Pore ​​size, preferably 8 nm or less PD 30 Pore ​​size, and (iii) D in the range of 1 μm to 25 μm 50 particle size, and optionally (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), has.

[0136] More preferably, the porous particles are (i) 0.7 cm 3 / g~1.6cm 3 the total pore volume of micropores and mesopores as measured by nitrogen gas adsorption in the range of 1 / g; (ii) PD less than 10 nm 50 Pore ​​diameter, preferably PD of 20 nm or less 90 Pore ​​size, preferably 8 nm or less PD 30 Pore ​​size, and (iii) D in the range of 1 μm to 20 μm 50 particle size, and optionally (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), has.

[0137] More preferably, the porous particles are (i) 0.7 cm 3 / g~1.5cm 3 the total pore volume of micropores and mesopores as measured by nitrogen gas adsorption in the range of 1 / g; (ii) PD less than 5 nm 50 Pore ​​diameter, preferably PD of 10 nm or less 90 Pore ​​size, preferably 3 nm or less PD 30 Pore ​​size, and (iii) D in the range of 2 μm to 20 μm50 particle size, and optionally (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), has.

[0138] More preferably, the porous particles are (i) 0.7 cm 3 / g~1.4cm 3 the total pore volume of micropores and mesopores as measured by nitrogen gas adsorption in the range of 1 / g; (ii) PD less than 5 nm 50 Pore ​​diameter, preferably PD of 10 nm or less 90 Pore ​​size, preferably 3 nm or less PD 30 Pore ​​size, and (iii) D in the range of 2 μm to 20 μm 50 particle size, and optionally (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), has.

[0139] More preferably, the porous particles are (i) 0.7 cm 3 / g~1.4cm 3 the total pore volume of micropores and mesopores as measured by nitrogen gas adsorption in the range of 1 / g; (ii) PD less than 5 nm 50 Pore ​​diameter, preferably PD of 10 nm or less 90 Pore ​​size, preferably 3 nm or less PD 30 Pore ​​size, and (iii) D in the range of 2 μm to 18 μm 50 particle size, and optionally (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), has.

[0140] More preferably, the porous particles are (i) 0.7 cm 3 / g~1.4cm 3 the total pore volume of micropores and mesopores as measured by nitrogen gas adsorption in the range of 1 / g; (ii) PD of 2 nm or less 50 Pore ​​size, preferably 5 nm or less PD 90 Pore ​​diameter, preferably PD of 1 nm or less 30 Pore ​​size, and (iii) D in the range of 2 μm to 15 μm 50 particle size, and optionally (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), has.

[0141] The composite particles are (i) D of at least 0.5 μm 10 Particle size, (ii) D of 50 μm or less 90 Particle size, and (iii) 0.35 cm 3 / g or less total volume of micropores and mesopores, and optionally (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), may have the following structure:

[0142] The composite particles are (i) D of at least 0.8 μm 10 Particle size, (ii) D of 40 μm or less 90 Particle size, and (iii) 0.35 cm 3 / g or less total volume of micropores and mesopores, and optionally (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), may have the following structure:

[0143] The composite particles are (i) D of at least 0.8 μm 10 Particle size, (ii) D of 30 μm or less 90 Particle size, and (iii) 0.35 cm 3 / g or less total volume of micropores and mesopores, and optionally (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), may have the following structure:

[0144] The composite particles are (i) D of at least 1 μm 10 Particle size, (ii) D of 25 μm or less 90 Particle size, and (iii) 0.25 cm 3 / g or less total volume of micropores and mesopores, and optionally (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), may have the following structure:

[0145] The composite particles are (i) a total oxygen content of less than 5% by weight, based on the total mass of the composite particles; (ii) 40% to 70% by weight of silicon, based on the total mass of the composite particles; and (iii) 30m 2 / g or less, and optionally, (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), may have the following structure:

[0146] The composite particles are (i) a total oxygen content of less than 5% by weight, based on the total mass of the composite particles; (ii) 40% to 60% by weight of silicon, based on the total mass of the composite particles; and (iii) 20m 2 / g or less, and optionally, (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), may have the following structure:

[0147] The composite particles are (i) a total oxygen content of less than 5% by weight, based on the total mass of the composite particles; (ii) 40% to 60% by weight of silicon, based on the total mass of the composite particles; and (iii) 15m 2 / g or less, and optionally, (iv) A particle size distribution span of 5 or less ((D 90 -D 10 ) / D 50 ), may have the following structure:

[0148] Composite particles having these preferred total oxygen contents, silicon contents and BET surface areas are believed to have improved cycle life and energy capacity.

[0149] The composite particles are (i) D of at least 0.5 μm 10 Particle size, (ii) D of 50 μm or less 90 Particle size, (iii) 0.35 cm 3 / g or less of the total volume of micropores and mesopores, (iv) a total oxygen content of less than 5% by weight, based on the total mass of the composite particles; (v) 40% to 70% by weight of silicon, based on the total mass of the composite particles; and (vi) 30m 2 / g or less, and optionally, (vii) A particle size distribution span of 5 or less (D 90 -D 10 ) / D 50 ), may have the following structure:

[0150] The composite particles are (i) D of at least 0.8 μm 10 Particle size, (ii) D of 40 μm or less 90 Particle size, (iii) 0.35 cm 3 / g or less of the total volume of micropores and mesopores, (iv) a total oxygen content of less than 5% by weight, based on the total mass of the composite particles; (v) 40% to 60% by weight of silicon, based on the total mass of the composite particles; and (vi) 20m 2 / g or less, and optionally, (vii) A particle size distribution span of 5 or less (D 90 -D 10 ) / D 50 ), may have the following structure:

[0151] The composite particles are (i) D of at least 0.8 μm 10 Particle size, (ii) D of 30 μm or less 90 Particle size, (iii) 0.35 cm 3 / g or less of the total volume of micropores and mesopores, (iv) a total oxygen content of less than 5% by weight, based on the total mass of the composite particles; (v) 40% to 60% by weight of silicon, based on the total mass of the composite particles; and (vi) 15m 2 / g or less, and optionally, (vii) A particle size distribution span of 5 or less (D 90 -D 10 ) / D 50 ), may have the following structure:

[0152] The composite particles are (i) D of at least 1 μm 10 Particle size, (ii) D of 25 μm or less 90 Particle size, (iii) 0.25 cm 3 / g or less of the total volume of micropores and mesopores, (iv) a total oxygen content of less than 5% by weight, based on the total mass of the composite particles; (v) 40% to 60% by weight of silicon, based on the total mass of the composite particles; and (vi) 15m 2 / g or less, and optionally, (vii) A particle size distribution span of 5 or less (D 90 -D 10 ) / D 50 ), may have the following structure:

[0153] The aforementioned preferred features of the porous particles also apply to the porous particle scaffold in the composite particle of the first aspect of the invention.

[0154] The electroactive materials deposited in steps (b) and (d) may be the same or different and may optionally be independently selected from silicon, tin, germanium, aluminum, and mixtures and alloys thereof. A preferred electroactive material is silicon. Preferably, the electroactive material deposited in at least one of steps (b) and (d) is silicon. More preferably, both electroactive materials deposited in each of steps (b) and (d) are silicon.

[0155] Suitable precursors for silicon include silane (SiH4), disilane (Si2H6), trisilane (Si3H8), and tetrasilane (Si4H 10 ), methylsilane (CH3SiH3), dimethylsilane ((CH3)2SiH2), or chlorosilanes such as trichlorosilane (HSiCl3) or methylchlorosilanes such as methyltrichlorosilane (CH3SiCl3) or dimethyldichlorosilane ((CH3)2SiCl2). The preferred precursor of silicon is silane.

[0156] Suitable precursors of tin include bis[bis(trimethylsilyl)amino]tin(II) ([[(CH3)3Si]2N]2Sn), tetraallyltin ((H2C=CHCH2)4Sn), tetrakis(diethylamido)tin(IV) ([(C2H5)2N]4Sn), tetrakis(dimethylamido)tin(IV) ([(CH3)2N]4Sn), tetramethyltin (Sn(CH3)4), tetravinyltin (Sn(CH=CH2)4), tin(II) acetylacetonate (C 10 H 14 O4Sn), trimethyl(phenylethynyl)tin (C6H5C≡CSn(CH3)3), and trimethyl(phenyl)tin (C6H5Sn(CH3)3). The preferred precursor of tin is tetramethyltin.

[0157] Suitable precursors of aluminum include aluminum tris(2,2,6,6-tetramethyl-3,5-heptanedionate) (Al(OCC(CH3)3CHCOC(CH3)3)3), trimethylaluminum ((CH3)3Al), and tris(dimethylamido)aluminum(III) (Al(N(CH3)2)3). The preferred precursor of aluminum is trimethylaluminum.

[0158] Suitable precursors of germanium include germane (GeH4), hexamethyldigermanium ((CH3)3GeGe(CH3)3), tetramethylgermanium ((CH3)4Ge), tributylgermanium hydride ([CH3(CH2)3]3GeH), triethylgermanium hydride ((C2H5)3GeH), and triphenylgermanium hydride ((C6H5)3GeH). The preferred precursor of germanium is germane.

[0159] When the precursor is a chlorinated compound, such as a chlorosilane, the precursor is used in a mixture with hydrogen gas, preferably in at least a 1:1 atomic ratio of hydrogen to chlorine.

[0160] Optionally, the precursor is chlorine-free. By chlorine-free, it is meant that the precursor contains less than 1% by weight, preferably less than 0.1% by weight, preferably less than 0.01% by weight of chlorine-containing compounds.

[0161] In steps (b) and (d), the precursors may be used either in pure form (or substantially pure form) or as a dilute mixture with an inert carrier gas, such as nitrogen or argon. When in a dilute mixture with an inert carrier gas, the precursors may be used in an amount ranging from 1% to 95% by volume, or from 1% to 85% by volume, or from 1% to 70% by volume, or from 1% to 50% by volume, or from 2% to 40% by volume, or from 5% to 30% by volume, or from 5% to 25% by volume, based on the total gas volume of the precursors and the inert carrier gas. In accordance with conventional practice for working in an inert atmosphere, the presence of oxygen should be minimal to prevent undesired oxidation of the deposited electroactive material. Preferably, the oxygen content is less than 0.01% by volume, more preferably less than 0.001% by volume, based on the total volume of the gases used in steps (b) and (d).

[0162] The temperatures in steps (b) and (d) are any temperature effective to decompose the precursor to form the electroactive material. Preferably, the temperatures in steps (b) and (d) are independently in the range of 300°C to 800°C, or 350°C to 800°C, or 380°C to 700°C, or 380°C to 650°C, or 380°C to 600°C, or 380°C to 550°C, or 380°C to 500°C, or 400°C to 450°C, or 450°C to 500°C. More preferably, the temperatures in steps (b) and (d) are each independently in the range of 380°C to 500°C, preferably 420°C to 480°C. Optionally, the temperatures are substantially the same in steps (b) and (d).

[0163] The operating pressure in steps (b) and (d) may be below atmospheric pressure, above atmospheric pressure, or at atmospheric pressure. Optionally, the pressure in at least one of steps (b) and (d) is maintained below 200 kPa, or below 150 kPa, or below 120 kPa, or below 110 kPa, or below 100 kPa, or below 90 kPa, or below 80 kPa, or below 70 kPa, or below 60 kPa, or below 50 kPa.

[0164] For example, the pressure in at least step (b) is maintained at less than 200 kPa, or 150 kPa or less, or 120 kPa or less, or 110 kPa or less, or 100 kPa or less, or 90 kPa or less, or 80 kPa or less, or 70 kPa or less, or 60 kPa or less, or 50 kPa or less.

[0165] Optionally, the pressure in both step (b) and step (d) may be maintained at less than 200 kPa, or 150 kPa or less, or 120 kPa or less, or 110 kPa or less, or 100 kPa or less, or 90 kPa or less, or 80 kPa or less, or 70 kPa or less, or 60 kPa or less, or 50 kPa or less.

[0166] References to pressure in any step of the claimed process refer to the absolute pressure in the reaction zone, which may include any type of reactor vessel.

[0167] Deposition of the electroactive material by CVI results in the removal of by-products, especially by-product gases such as hydrogen. Step (b) and / or step (d) preferably further comprise separating the by-products. Separation of the by-products from the particles formed in step (b) and / or step (d) can be achieved by flushing the reactor with an inert gas and / or by evacuating the reactor by reducing the pressure. For example, separation of the by-products from the intermediate particles formed in step (b) can be achieved by evacuating the reactor to a pressure of less than 100 kPa, or less than 80 kPa, or less than 60 kPa, or less than 40 kPa, or less than 20 kPa, or less than 10 kPa, or less than 5 kPa, or less than 2 kPa, or less than 1 kPa. Evacuating the reactor to low pressure can be effective not only to remove gas phase by-products, but also to desorb any by-products that may be adsorbed on the deposited electroactive material surface.

[0168] The modifier material formed in step (c) may optionally be a passivation layer formed on the electroactive material surface deposited in step (b). Thus, step (c) may further comprise contacting the intermediate particles from step (b) with a passivator. As mentioned above, the passivator is a compound or mixture of compounds capable of reacting with the electroactive material surface deposited in step (b) to form a modified surface. Any of the passivators described in connection with the first aspect of the invention may be used in step (c).

[0169] The contacting of the electroactive material with the passivating agent in step (c) may be carried out at a temperature in the range of 25°C to 800°C, preferably in the range of 50°C to 500°C, more preferably in the range of 100°C to 300°C.

[0170] The formation of the natural oxide layer is exothermic and thus requires careful process control to prevent overheating or even combustion of the particulate material. When the modifier material formed in step (c) is a natural oxide layer, step (c) may include cooling the material formed in step (b) to less than 300 °C, preferably less than 200 °C, optionally less than 100 °C, before contacting the surface of the electroactive material domain with an oxygen-containing gas.

[0171] The modifier material formed in step (c) may be a nitride of the electroactive material domain. Step (c) may include contacting ammonia with the surface of the electroactive material domain. The nitride layer can be formed by contacting the surface of the electroactive material domain with ammonia at a temperature in the range of 200 °C to 700 °C, preferably 400 °C to 700 °C, more preferably 400 °C to 600 °C. Then, if necessary, the temperature can be raised to the range of 500 °C to 1000 °C to form a nitride surface (e.g., a silicon nitride surface of the formula SiN x (where x ≤ 4 / 3)). For example, when using ammonia, step (c) may be carried out at the same or a similar temperature as that used for depositing the electroactive material domain in step (b). Since stoichiometric silicon nitride is conductive, this step will also result in the formation of a conductive network that enables more rapid charging and discharging of the electroactive material.

[0172] Another type of modifier material is an oxynitride layer. Step (c) may include exposing the surface of the electroactive material domain to ammonia (or another nitrogen-containing molecule) and oxygen gas. When the electroactive material domain contains silicon, the modifier material domain may include silicon oxynitride of the formula SiO x N y (where 0 < x < 2, 0 < y < 4 / 3, and 0 < (2x + 3y) ≤ 4). The silicon nitride is preferably amorphous silicon oxynitride.

[0173] As a further option, an amorphous or nanocrystalline carbide layer may be formed. Step (c) may include contacting the electroactive material domain surface with a carbon-containing precursor, such as methane or ethylene, at a temperature in the range of 250°C to 700°C. At lower temperatures, covalent bonds are formed between the electroactive material surface and the carbon-containing precursor, which is converted to a single layer of crystalline silicon carbide as the temperature increases. When the electroactive material domain contains silicon, the modifier material domain may contain silicon carbide of the formula SiC x (where 0 < x ≦ 1). The silicon carbide is preferably amorphous silicon carbide.

[0174] Other suitable passivating agents include compounds containing alkene, alkyne or carbonyl functional groups, more preferably terminal alkenes, terminal alkynes, aldehyde or ketone groups. Suitable passivating agents of these types are described above.

[0175] Other suitable passivating agents include compounds containing active hydrogen atoms bonded to oxygen, nitrogen, sulfur or phosphorus. For example, the passivating agent may be an alcohol, an amine, a thiol or a phosphine. The reaction of the -XH group with the hydride group on the electroactive material surface is understood to result in the removal of H2 and the formation of a direct bond between X and the electroactive material surface. Suitable passivating agents of these types are described above.

[0176] The modifier material formed in step (c) may optionally include a pyrolytic carbon material deposited on the electroactive material surface by thermal decomposition of a carbon-containing precursor, i.e., by chemical vapor infiltration (CVI). The deposition of the pyrolytic carbon material in step (c) may be suitable for forming a conductive network between electroactive material domains that can facilitate electron transfer within the composite particles. Step (c) may thus include contacting the intermediate particles resulting from step (b) with a carbon-containing precursor, preferably a hydrocarbon, at a temperature effective to cause deposition of the pyrolytic carbon material in the pores of the intermediate particles.

[0177] Suitable hydrocarbons include polycyclic hydrocarbons containing 10 to 25 carbon atoms and optionally 1 to 3 heteroatoms, optionally the polycyclic aromatic hydrocarbons being selected from naphthalene, substituted naphthalenes such as dihydroxynaphthalene, anthracene, tetracene, pentacene, fluorene, acenaphthene, phenanthrene, fluoranthene, pyrene, chrysene, perylene, coronene, fluorenone, anthraquinone, anthrone and alkyl-substituted derivatives thereof. Suitable pyrolytic carbon precursors also include bicyclic monoterpenoids, optionally the bicyclic monoterpenoids being selected from camphor, borneol, eucalyptol, camphene, careen, sabinene, thujene and pinene. Further suitable pyrolytic carbon precursors include C2-C 10 Included are hydrocarbons, optionally selected from alkanes, alkenes, alkynes, cycloalkanes, cycloalkenes, and arenes, such as methane, ethylene, propylene, limonene, styrene, cyclohexane, cyclohexene, α-terpinene, and acetylene. Other suitable pyrolytic carbon precursors include phthalocyanine, sucrose, starch, graphene oxide, reduced graphene oxide, pyrene, perhydropyrene, triphenylene, tetracene, benzopyrene, perylene, coronene, and chrysene. A preferred carbon precursor is acetylene.

[0178] Suitable temperatures for the deposition of the pyrolytic carbon material in step (c) range from 300°C to 800°C, or from 400°C to 800°C. For example, the temperature may be 750°C or less, or 700°C or less, or 680°C or less, or 660°C or less, or 640°C or less, or 620°C or less, or 600°C or less, or 580°C or less, or 560°C or less, or 540°C or less, or 520°C or less, or 500°C or less. The minimum temperature varies depending on the type of carbon precursor used. Preferably, the temperature is at least 300°C, or at least 350°C, or at least 400°C, or at least 450°C, or at least 500°C.

[0179] The carbon-containing precursor used in step (c) may be used in pure form or in a mixture diluted with an inert carrier gas such as nitrogen or argon. For example, the carbon-containing precursor may be used in an amount ranging from 0.1% to 100% by volume, or from 0.5% to 20% by volume, or from 1% to 10% by volume, or from 1% to 5% by volume, based on the total volume of the precursor and the inert carrier gas. The presence of oxygen should be minimal to prevent undesired oxidation of the deposited electroactive material. Preferably, the oxygen content is less than 0.01% by volume, more preferably less than 0.001% by volume, based on the total volume of the gas.

[0180] If a pyrolytic carbon material is deposited in step (c), the same compound can function as both the passivator and the pyrolytic carbon precursor. For example, if styrene is selected as the pyrolytic carbon precursor, it will also function as the passivator, provided that the intermediate particles from step (b) are not exposed to oxygen prior to contact with the styrene. In this case, the passivation and deposition of the conductive carbon material in the process can be carried out simultaneously, for example at a temperature in the range of 300°C to 700°C. Alternatively, the passivation and deposition of the conductive carbon material can be carried out sequentially, if the passivator and the pyrolytic carbon precursor are the same material, but the deposition of the pyrolytic carbon precursor is carried out at a higher temperature than the passivation. For example, the passivation can be carried out at a temperature in the range of 25°C to less than 300°C, and the deposition of the pyrolytic carbon can be carried out at a temperature in the range of 300°C to 700°C. These two steps can be suitably carried out sequentially by increasing the temperature while maintaining contact with the compound that functions as both the passivator and the pyrolytic carbon precursor. At lower temperatures (e.g., in the range of 25°C to less than 300°C), passivation would be the predominant process. As the temperature increases (e.g., to 300°C to 700°C), deposition of pyrolytic carbon would likely ensue.

[0181] As a further option, step (c) may comprise depositing a layer of a conductive metal or metal alloy as a modifier material on the electroactive material domain surface. The conductive metal layer or metal alloy may be obtained by chemical vapor infiltration (CVI). Examples of suitable conductive metals include silver, gold, copper and titanium.

[0182] The formation of the conductive metal or metal alloy modifier material in step (c) may optionally be followed by passivation of the electroactive material domain surface by one of the processes described above. Thus, the modifier material formed in step (c) may include both a passivation layer and a conductive metal or metal alloy layer on the electroactive material domain surface.

[0183] As a further alternative, step (c) may include forming a modifier material domain comprising an electroactive material comprising a dopant selected from the group consisting of boron, aluminum, gallium, indium, phosphorus, arsenic, antimony, and bismuth. The doped electroactive material may be formed by a CVI process in which the porous particles are simultaneously contacted with both a precursor of the electroactive material and a dopant. Alternatively, the doped electroactive material may be formed by contacting the dopant with the deposited electroactive material.

[0184] As a further alternative, step (c) may include forming a solid state electrolyte as the modifier material.

[0185] As a further alternative, step (c) may include forming an inert filler as the modifier material.

[0186] Depending on the amount of electroactive material to be deposited in each step, the method of the present invention may be operated as a multi-pass process in which steps (c) and (d) are repeated as many times as necessary to deposit the target amount of electroactive material. For example, steps (c) and (d) may be performed 2-15 times, resulting in 3-16 deposition steps of electroactive material, including repetitions of steps (b) and (d).

[0187] When repeating steps (c) and (d), each process of step (c) and step (d) is independently as described above. For example, each repetition of step (c) may include the formation of the same or different modifier material. Similarly, the electroactive material deposited in each repetition of step (d) may be the same or different, and may also be the same or different from the electroactive material deposited in step (b). Preferably, the electroactive material deposited in at least one of step (b) and repeated step (d) is silicon. More preferably, the electroactive material deposited in each of step (b) and repeated step (d) is silicon.

[0188] When steps (c) and (d) are repeated, the particles used during the repetition of step (c) are intermediate particles obtained from the preceding step (d). Thus, any reference herein to "particles from step (b)" in the description of step (c) should be interpreted as "particles from the preceding step (d)" when step (c) is optionally repeated.

[0189] The method of the invention optionally further comprises: (e) forming a plurality of modifier material domains in the pores and / or on the exterior surface of the composite particles from step (d); Further includes:

[0190] Step (e) is performed immediately after the last electroactive material deposition step (i.e., step (d) or the last iteration of step (d) if steps (c) and (d) are repeated). The formation of modifier material domains in step (e) is a similar process to step (c) described above, except that step (e) is performed after the last electroactive material deposition step (the last step (d)), whereas step (c) is performed between successive electroactive material deposition steps. All of the modifier materials and deposition conditions set forth above in relation to step (c) also apply to step (e).

[0191] The modifier material domains formed in step (e) may comprise the same or a different modifier material as the modifier material domains formed in step (c).

[0192] Optionally, step (e) includes contacting the composite particles from step (d) with a passivation agent. The preferred passivation agents and passivation conditions set forth above in relation to step (c) also apply to the passivation in step (e).

[0193] The modifier material domains formed in step (e) may be a native oxide of the electroactive material, in which case it is preferred that the modifier material domains formed in step (c) (and any repetitions of step (c)) are not a native oxide of the electroactive material.

[0194] Optionally, step (e) includes depositing a lithium-ion permeable material within the pores and / or on the outer surface of the composite particles from step (d), which provides further improvement in the performance of the composite particles when used as an electroactive material for lithium-ion batteries by reducing the surface area of ​​the composite particles and by blocking electroactive material domains from access to electrolyte.

[0195] The lithium ion permeable material may be deposited immediately after the last electroactive material deposition step (i.e., step (d), or after the last step (d) if steps (c) and (d) are repeated one or more times). Alternatively, the lithium ion permeable material may be deposited after first carrying out a passivation step in step (e), as discussed above.

[0196] A suitable lithium ion permeable material is a pyrolytic carbon material, which can be obtained by chemical vapor infiltration (CVI) method, i.e., by pyrolysis of a volatile carbon-containing gas (e.g., ethylene) on the surface of silicon-containing composite particles.

[0197] A suitable process for depositing a pyrolyzable carbon material includes combining the composite particles from step (d) with a pyrolyzable carbon precursor and heating the pyrolyzable carbon precursor to a temperature effective to cause deposition of a pyrolyzable conductive carbon material within the pores and / or on the exterior surfaces of the composite particles.

[0198] The preferred pyrolyzable carbon precursors and pyrolysis conditions set forth above in relation to step (c) also apply to the formation of the pyrolyzable carbon material in step (e).

[0199] When the lithium ion permeable material is a pyrolytic carbon material, the same compound may function as both the passivator and the pyrolytic carbon precursor in step (e). Suitable conditions for passivating and forming a pyrolytic carbon material using the same compound as the passivator and the pyrolytic carbon precursor in step (e) are the same as those set forth above in connection with step (c).

[0200] Alternatively, different compounds may be used as the passivating agent and as the pyrolyzable carbon precursor, for example the passivating agent may be styrene and the pyrolyzable carbon precursor may be a compound such as cyclohexane that is capable of forming a pyrolyzable carbon material but is unable to passivate the electroactive material surface.

[0201] In a preferred embodiment, the electroactive material deposited in steps (b) and (d) is elemental silicon, and the modifier material domains formed in step (c) are passivation layers comprising organic moieties covalently bonded to a surface of at least a portion of the elemental silicon domains formed in step (b). Optionally, the method includes step (e), where the modifier material domains formed in step (e) are silicon oxide domains formed by passivation using an oxygen-containing gas.

[0202] In a further preferred embodiment, the electroactive material deposited in steps (b) and (d) is elemental silicon and the modifier material domains formed in step (c) are pyrolytic carbon domains. Optionally, the method includes step (e), where the modifier material domains formed in step (e) are silicon oxide domains formed by passivation using an oxygen-containing gas.

[0203] In a further preferred embodiment, the electroactive material deposited in steps (b) and (d) is elemental silicon and the modifier material domains formed in step (c) are metal or metal alloy domains. Optionally, the method includes step (e), where the modifier material domains formed in step (e) are silicon oxide domains formed by passivation using an oxygen-containing gas.

[0204] In a further preferred embodiment, the electroactive material deposited in steps (b) and (d) is elemental silicon and the modifier material domains formed in step (c) are silicon oxide domains formed by passivation using an oxygen-containing gas.

[0205] The process of the present invention may be carried out in any reactor capable of contacting solids and gases at elevated temperatures. The porous particles and the resulting composite particles may be present in the reactor in the form of a fixed bed of particles or in the form of a moving or stirred bed of particles.

[0206] The product resulting from the process of the invention may have any of the characteristics described herein in relation to the particulate material of the first aspect of the invention.

[0207] In a third aspect of the present invention, there is provided a composition comprising a composite particle according to the second aspect of the present invention and at least one other component. In particular, there is provided a composition comprising a composite particle according to the second aspect of the present invention and at least one other component selected from (i) a binder, (ii) a conductive additive, and (iii) an additional particulate electroactive material. The composition according to the present invention is useful as an electrode composition and can thus be used to form the active layer of an electrode.

[0208] The composition may be a hybrid electrode composition comprising the composite particles and at least one additional particulate electroactive material. Examples of the additional particulate electroactive material include graphite, hard carbon, silicon, tin, germanium, aluminum, and lead. The at least one additional particulate electroactive material is preferably selected from graphite and hard carbon. The at least one additional particulate electroactive material is most preferably graphite.

[0209] For hybrid electrode compositions, the composition may comprise 1 wt% to 95 wt%, or 2 wt% to 90 wt%, or 5 wt% to 85 wt%, or 10 wt% to 80 wt% of particulate material based on the total dry weight of the composition. The composition preferably comprises 3 wt% to 60 wt%, or 3 wt% to 50 wt%, or 5 wt% to 50 wt%, or 10 wt% to 50 wt%, or 15 wt% to 50 wt% of composite particles based on the total dry weight of the composition.

[0210] The at least one additional particulate electroactive material is suitably present in an amount of from 20% to 95% by weight, or from 25% to 90% by weight, or from 30% to 75% by weight of the at least one additional particulate electroactive material.

[0211] The at least one additional particulate electroactive material preferably has a diameter in the range of 10 μm to 50 μm, preferably 10 μm to 40 μm, more preferably 10 μm to 30 μm, most preferably 10 μm to 25 μm, for example 15 μm to 25 μm. 50 It has a particle size.

[0212] D of at least one additional particulate electroactive material 10 The particle size is preferably at least 5 μm, more preferably at least 6 μm, more preferably at least 7 μm, more preferably at least 8 μm, more preferably at least 9 μm, and even more preferably at least 10 μm.

[0213] D of at least one additional particulate electroactive material 90 The particle size is preferably at most 100 μm, more preferably at most 80 μm, more preferably at most 60 μm, more preferably at most 50 μm, most preferably at most 40 μm.

[0214] The at least one additional particulate electroactive material is preferably selected from carbon-containing particles, graphite particles, and / or hard carbon particles, where the graphite particles and hard carbon particles have a D in the range of 10 μm to 50 μm. 50 More preferably, the at least one additional particulate electroactive material is selected from graphite particles, wherein the graphite particles have a D in the range of 10 μm to 50 μm. 50 It has a particle size.

[0215] The composition may be a non-hybrid (i.e., "highly loaded") electrode composition that is substantially free of additional particulate electroactive material. In this context, the term "substantially free of additional particulate electroactive material" should be interpreted to mean that the composition contains less than 15 wt. %, preferably less than 10 wt. %, preferably less than 5 wt. %, preferably less than 2 wt. %, more preferably less than 1 wt. %, more preferably less than 0.5 wt. %, of any additional electroactive material (i.e., additional material capable of inserting and releasing metal ions during charging and discharging the battery), based on the total dry weight of the composition.

[0216] A "highly loaded" electrode composition of this kind preferably comprises at least 50% by weight, or at least 60% by weight, or at least 70% by weight, or at least 80% by weight, or at least 90% by weight of composite particles according to the invention, based on the total dry weight of the composition.

[0217] The composition may optionally include a binder. The binder functions to adhere the composition to the current collector and maintain the integrity of the composition. Examples of binders that may be used according to the present invention include polyvinylidene fluoride (PVDF), polyacrylic acid (PAA) and its alkali metal salts, modified polyacrylic acid (mPAA) and its alkali metal salts, carboxymethyl cellulose (CMC), modified carboxymethyl cellulose (mCMC), sodium carboxymethyl cellulose (Na-CMC), polyvinyl alcohol (PVA), alginates and their alkali metal salts, styrene-butadiene rubber (SBR), and polyimides. The composition may include a mixture of binders. Preferably, the binder includes a polymer selected from polyacrylic acid (PAA) and its alkali metal salts, modified polyacrylic acid (mPAA) and its alkali metal salts, SBR, and CMC.

[0218] The binder may suitably be present in an amount of from 0.5% to 20% by weight, preferably from 1% to 15% by weight, preferably from 2% to 10% by weight, most preferably from 5% to 10% by weight, based on the total dry weight of the composition.

[0219] The binder may optionally be present in combination with one or more additives that modify the properties of the binder, such as crosslinking promoters, coupling agents, and / or adhesion promoters.

[0220] The composition may optionally include one or more conductive additives. Preferred conductive additives are non-electroactive materials that are included to improve electrical conductivity between the electroactive components of the composition and between the electroactive components of the composition and the current collector. The conductive additives may be selected from carbon black, carbon fibers, carbon nanotubes, graphene, acetylene black, ketjen black, metal fibers, metal powders, and conductive metal oxides. Preferred conductive additives include carbon black and carbon nanotubes.

[0221] The one or more conductive additives may suitably be present in a total amount of from 0.5% to 20% by weight, preferably from 1% to 15% by weight, preferably from 2% to 10% by weight, most preferably from 5% to 10% by weight, based on the total dry weight of the composition.

[0222] The invention provides an electrode comprising a particulate material according to the invention in electrical contact with a current collector. The particulate material used to manufacture the electrode may be in the form of a composition of the invention.

[0223] The term current collector as used herein refers to any conductive substrate capable of conducting electrical current to and from the electroactive particles in the composition. Examples of materials that can be used as current collectors include copper, aluminum, stainless steel, nickel, titanium, and sintered carbon. Copper is a preferred material. Current collectors typically have the form of a foil or mesh having a thickness of 3 μm to 500 μm. The particulate material of the present invention can be applied to one or both sides of the current collector, preferably to a thickness ranging from 10 μm to 1 mm, for example, from 20 μm to 500 μm, or from 50 μm to 200 μm.

[0224] The electrode of the present invention may be made by combining the particulate material of the present invention with a solvent and optionally one or more viscosity modifying additives to form a slurry. The slurry is then cast onto the surface of a current collector and the solvent is removed to form an electrode layer on the surface of the current collector. Further steps such as heat treatment to harden any binder and / or calendaring the electrode layer may optionally be performed. The electrode layer suitably has a thickness in the range of 20 μm to 2 mm, preferably 20 μm to 1 mm, preferably 20 μm to 500 μm, preferably 20 μm to 200 μm, preferably 20 μm to 100 μm, preferably 20 μm to 50 μm.

[0225] Alternatively, the slurry can be formed into a free-standing film or mat comprising the particulate material of the present invention, for example, by casting the slurry onto a suitable casting template, removing the solvent, and then removing the casting template. The resulting film or mat has the form of a free-standing agglomerate, which can then be adhered to a current collector by known methods.

[0226] The electrode of the present invention can be used as the anode of a metal-ion battery.Thus, the present invention provides a rechargeable metal-ion battery comprising an anode comprising an electrode according to the present invention as described above, a cathode comprising a cathode active material capable of releasing and reabsorbing metal ions, and an electrolyte between the anode and the cathode.

[0227] The metal ions are preferably lithium ions. More preferably, the rechargeable metal ion batteries of the present invention are lithium ion batteries and the cathode active material is capable of releasing and accepting lithium ions.

[0228] The cathode active material is preferably a metal oxide-based composite. Examples of suitable cathode active materials include LiCoO2, LiCo 0.99 Al 0.01 O2, LiNiO2, LiMnO2, LiCo 0.5 Ni 0.5 O2, LiCo 0.7 Ni 0.3 O2, LiCo 0.8 Ni 0.2 O2, LiCo 0.82 Ni 0.18 O2, LiCo 0.8 Ni 0.15 Al 0.05 O2, LiNi 0.4 Co 0.3 Mn 0.3 O2 and LiNi 0.33 Co 0.33 Mn 0.34O2. The cathode current collector usually has a thickness of 3 μm to 500 μm. Examples of materials that can be used as the cathode current collector include aluminum, stainless steel, nickel, titanium, and sintered carbon.

[0229] The electrolyte is preferably a non-aqueous electrolyte containing a metal salt, such as a lithium salt, and may include, but is not limited to, a non-aqueous electrolyte, a solid electrolyte, and an inorganic solid electrolyte. Examples of non-aqueous electrolytes that may be used include aprotic organic solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma butyrolactone, 1,2-dimethoxyethane, 2-methyltetrahydrofuran, dimethylsulfoxide, 1,3-dioxolane, formamide, dimethylformamide, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, sulfolane, methylsulfolane, and 1,3-dimethyl-2-imidazolidinone.

[0230] Examples of organic solid electrolytes include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate ester polymers, polyester sulfides, polyvinyl alcohol, polyvinylidene fluoride, and polymers containing ionically dissociable groups.

[0231] Examples of inorganic solid electrolytes include nitrides, halides, and sulfides of lithium salts, such as Li5NI2, Li3N, LiI, LiSiO4, Li2SiS3, Li4SiO4, LiOH, and Li3PO4.

[0232] The lithium salt is preferably soluble in the selected solvent or mixture of solvents. Examples of suitable lithium salts include LiCl, LiBr, LiI, LiClO4, LiBF4, LiBC4O8, LiPF6, LiCF3SO3, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, and CF3SO3Li.

[0233] When the electrolyte is a non-aqueous organic solution, the metal ion battery preferably includes a separator inserted between the anode and the cathode. The separator is typically formed of an insulating material having high ion permeability and high mechanical strength. The separator typically has a pore size of 0.01 μm to 100 μm and a thickness of 5 μm to 300 μm. An example of a suitable electrode separator is a microporous polyethylene film.

[0234] The separator may be replaced with a polymer electrolyte material, in which case the polymer electrolyte material is present in both the composite anode layer and the composite cathode layer. The polymer electrolyte material may be a solid polymer electrolyte or a gel-type polymer electrolyte.

Claims

1. A particulate material comprising a plurality of composite particles, the composite particles comprising: (a) a porous particle framework containing micropores and / or mesopores, the total pore volume of the micropores and mesopores being less than or equal to 0.4 cm as measured by gas adsorption; 3 / g ~ 2.2 cm 3 / g of porous particle skeleton; (b) a plurality of electroactive material domains and a plurality of modifier material domains disposed within an interior pore volume of the porous particulate framework, at least a portion of the modifier material domains being located between adjacent electroactive material domains; 4. A particulate material comprising:

2. The total pore volume of the micropores and mesopores in the porous particle framework is 0.45 cm 3 / g ~ 2.2 cm 3 / g, or 0.5 cm 3 / g to 2 cm 3 / g, or 0.55 cm 3 / g to 2 cm 3 / g, or 0.6 cm 3 / g ~ 1.8 cm 3 / g, or 0.65 cm 3 / g ~ 1.8 cm 3 / g, or 0.7 cm 3 / g ~ 1.6 cm 3 / g, or 0.7 cm 3 / g ~ 1.5 cm 3 / g, or 0.7 cm 3 / g ~ 1.4 cm 3 The particulate material of claim 1, wherein the molecular weight is in the range of 1 / g.

3. PD of the porous particle skeleton 50 3. The particulate material of claim 1 or 2, having a pore size of 30 nm or less, or 25 nm or less, or 20 nm or less, or 15 nm or less, or 12 nm or less, or 10 nm or less, or 8 nm or less, or 6 nm or less, or 5 nm or less, or 4 nm or less, or 3 nm or less, or 2.5 nm or less, or 2 nm or less, or 1.5 nm or less.

4. PD of the porous particle skeleton 30 4. The particulate material according to any one of claims 1 to 3, wherein the pore size is 25 nm or less, or 20 nm or less, or 15 nm or less, or 12 nm or less, or 10 nm or less, or 8 nm or less, or 6 nm or less, or 5 nm or less, or 4 nm or less, or 3 nm or less, or 2.5 nm or less, or 2 nm or less, or 1 nm or less.

5. The porous particle skeleton is 100 mm 2 / g to 4000m 2 / g, or 500m 2 / g to 4000m 2 / g, or 750m 2 / g~3500m 2 / g, or 1000m 2 / g~3250m 2 / g, or 1000m 2 / g to 3000m 2 / g, or 1000m 2 / g~2500m 2 / g, or 1000m 2 / g to 2000m 2 5. The particulate material according to any one of claims 1 to 4, having a BET surface area in the range of 1 / g.

6. A particulate material according to any one of claims 1 to 5, wherein the porous particle skeleton is an electrically conductive porous particle skeleton.

7. 7. The particulate material of claim 6, wherein the conductive porous particle skeleton is a conductive porous carbon particle skeleton.

8. 8. The particulate material of claim 7, wherein the electrically conductive porous carbon particle skeleton comprises at least 80% by weight carbon, or at least 85% by weight carbon, or at least 90% by weight carbon, or at least 95% by weight carbon.

9. 9. A particulate material according to any one of the preceding claims, wherein the porous particle scaffold has a volume ratio of micropores to mesopores of from 90:10 to 30:70, or from 85:15 to 40:60, or from 80:20 to 50:50, or from 70:30 to 55:

45.

10. PD of the porous particle skeleton 10 10. The particulate material according to any one of claims 1 to 9, wherein the pore size is 10nm or less, or 9nm or less, or 8nm or less, or 7nm or less, or 6nm or less, or 5nm or less, or 4nm or less, or 3nm or less, or 2.5nm or less, or 2nm or less, or 1.5nm or less, or 1nm or less.

11. PD of the porous particle skeleton 90 11. A particulate material according to any one of claims 1 to 10, wherein the pore size is 35nm or less, or 30nm or less, or 25nm or less, or 20nm or less, or 15nm or less, or 12nm or less, or 10nm or less, or 8nm or less, or 6nm or less, or 5nm or less, or 4nm or less, or 3nm or less, or 2.5nm or less, or 2nm or less.

12. 12. A particulate material according to any one of claims 1 to 11, wherein each of the electroactive material domains comprises an electroactive material independently selected from silicon, tin, germanium, aluminium, and mixtures and alloys thereof.

13. 13. A particulate material according to any one of claims 1 to 12, wherein at least some of the electroactive material domains comprise or consist of silicon, or all of the electroactive material domains comprise or consist of silicon.

14. 14. A particulate material according to any preceding claim, wherein the modifier material comprises one or more of carbon, nitrogen and oxygen.

15. The modifier material is an oxide, nitride, oxynitride or carbide passivation layer formed on the surface of at least a portion of the electroactive material domain, and preferably the modifier material is SiO x (wherein 0<x≦2), or an oxide selected from SiN x (wherein 0<x≦4 / 3), or SiC x (wherein 0<x≦1), more preferably the modifier material is optionally a carbide selected from the formula SiN x 15. The particulate material of claim 1, wherein the nitride passivation layer is formed on a surface of at least a portion of the electroactive material domains, the nitride passivation layer having the formula:

16. 15. The particulate material of any one of claims 1 to 14, wherein the modifier material is a passivation layer comprising carbon-containing organic moieties covalently bonded to a surface of at least a portion of the electroactive material domains.

17. The modifier material is covalently bonded to a surface of at least a portion of the electroactive material domains. 2~22 A particulate material according to any one of claims 1 to 14, comprising a hydrocarbyl.

18. The modifier material is covalently bonded to a surface of at least a portion of the electroactive material domains. 2~22 Alkyl, C 2~22 Alkenyl, C 2~22 Alkynyl, C 3~22 Cycloalkyl, C 3~22 Cycloalkenyl, C 3~22 Cycloalkynyl or C 6~22 A particulate material according to any preceding claim, comprising an aralkyl.

19. the modifier material is covalently bonded to a surface of at least a portion of the electroactive material domain; 【Chemistry 1】 The particulate material according to any one of claims 1 to 14, selected from the group consisting of:

20. A particulate material according to any preceding claim, wherein the modifier material comprises a pyrolytic carbon material.

21. A particulate material according to any preceding claim, wherein the modifier material comprises a conductive metal or metal alloy.

22. A particulate material according to any preceding claim, wherein the modifier material comprises an electroactive material comprising a dopant selected from boron and phosphorus.

23. 23. A particulate material according to any one of the preceding claims, further comprising an outer modifier material domain located between the outermost electroactive material domain and the exterior of the composite particle, optionally said modifier material selected from the modifier materials described in any one of the preceding claims 14 to 22.

24. 24. A particulate material according to any one of the preceding claims, wherein the composite particle comprises from 5% to 85% by weight, or from 10% to 85% by weight, or from 15% to 85% by weight, or from 20% to 80% by weight, or from 25% to 80% by weight, or from 30% to 75% by weight, or from 35% to 75% by weight, or from 40% to 70% by weight, or from 45% to 65% by weight of the electroactive material, relative to the total mass of the composite particle.

25. 25. A particulate material according to any one of the preceding claims, wherein the composite particle comprises from 40wt% to 70wt%, or from 45wt% to 70wt%, or from 48wt% to 70wt%, or from 50wt% to 70wt%, or from 40wt% to 65wt%, or from 45wt% to 65wt%, or from 48wt% to 65wt%, or from 50wt% to 65wt%, or from 40wt% to 60wt%, or from 45wt% to 60wt%, or from 48wt% to 60wt%, or from 50wt% to 60wt% of the electroactive material relative to the total mass of the composite particle.

26. 26. A particulate material according to any one of the preceding claims, wherein the composite particles comprise from 10wt% to 85wt%, or from 15wt% to 85wt%, or from 20wt% to 80wt%, or from 25wt% to 80wt%, or from 30wt% to 75wt%, or from 35wt% to 75wt%, or from 40wt% to 70wt%, or from 45wt% to 65wt% silicon based on the total mass of the composite particle.

27. 27. A particulate material according to any one of the preceding claims, wherein the composite particles comprise 40wt% to 70wt%, or 45wt% to 70wt%, or 48wt% to 70wt%, or 50wt% to 70wt%, or 40wt% to 65wt%, or 45wt% to 65wt%, or 48wt% to 65wt%, or 50wt% to 65wt%, or 40wt% to 60wt%, or 45wt% to 60wt%, or 48wt% to 60wt%, or 50wt% to 60wt% silicon relative to the total mass of the composite particle.

28. A particulate material according to any preceding claim, wherein the amount of electroactive material occupies at least 25% and at most 90% of the internal pore volume of the porous particulate framework.

29. 29. A particulate material according to any one of the preceding claims, wherein at least 85% by weight, more preferably at least 90% by weight, more preferably at least 95% by weight, more preferably at least 98% by weight of the electroactive material mass in the composite particles is located within the internal pore volume of the porous particle framework.

30. The composite particles have a D in the range of 0.5 μm to 30 μm, or 1 μm to 25 μm, or 1 μm to 20 μm, or 1 μm to 18 μm, or 1 μm to 16 μm, or 2 μm to 16 μm, or 2 μm to 14 μm, or 2 μm to 12 μm, or 2 μm to 10 μm, or 2 μm to 8 μm. 50 30. The particulate material according to any one of claims 1 to 29, having a particle size.

31. The composite particles are 0.1 m 2 / g to 100m 2 / g, or 0.1 m 2 / g ~ 80m 2 / g, or 0.5m 2 / g ~ 60m 2 / g, or 0.5m 2 / g to 40m 2 / g, or 1m 2 / g to 30m 2 / g, or 1m 2 / g to 25m 2 / g, or 2m 2 / g to 20m 2 31. The particulate material of any one of claims 1 to 30, having a BET surface area in the range of 1 / g.

32. 32. The particulate material of any one of claims 1 to 31, wherein the composite particles comprise a total oxygen content of less than 15% by weight, or less than 10% by weight, or less than 5% by weight, or less than 4% by weight, or less than 3% by weight, or less than 2% by weight, or less than 1% by weight, or less than 0.5% by weight, relative to the total mass of the composite particle.

33. 33. The particulate material of any one of the preceding claims, wherein the composite particles comprise a total chlorine content of less than 100 ppm, or less than 90 ppm, or less than 80 ppm, or less than 70 ppm, relative to the total mass of the composite particle.

34. 34. A particulate material according to any one of the preceding claims, wherein the composite particle comprises a total transition metal and alkali metal content of less than 0.5 wt.-%, relative to the total weight of the composite particle.

35. 35. A particulate material according to any preceding claim, wherein the composite particle comprises from 0.0001% to 0.5% by weight of zirconium, relative to the total weight of the composite particle.

36. The composite particles have a D of at least 0.5 μm, or at least 0.8 μm, or at least 1 μm. 10 A particulate material according to any one of claims 1 to 35, having a particle size.

37. The composite particles have a D of 50 μm or less, or 40 μm or less, or 30 μm or less, or 25 μm or less, or 20 μm or less, or 15 μm or less. 90 A particulate material according to any one of claims 1 to 36 having a particle size.

38. The composite particles have a particle size distribution span (D 90 -D 10 ) / D 50 38. The particulate material according to any one of claims 1 to 37, having a molecular weight of 1.2 or more.

39. The composite particles are 0.35 cm 3 / g or less, or 0.25 cm 3 / g or less, or 0.15 cm 3 / g or less, or 0.1 cm 3 / g or less, or 0.05 cm 3 / g or less, or 0.03 cm 3 / g or less, or 0.02 cm 3 39. A particulate material according to any one of the preceding claims having a total volume of micropores and mesopores of less than or equal to 1 / g.

40. 1. A method for preparing a composite particle, comprising: (a) The total pore volume of micropores and mesopores measured by gas adsorption is 0.4 cm 3 / g ~ 2.2 cm 3 providing a plurality of porous particles comprising micropores and / or mesopores, the micropores and / or mesopores being in the range of .mu.m / g; (b) contacting the porous particle with a precursor of an electroactive material at a temperature effective to cause deposition of a plurality of electroactive material domains in the pores of the porous particle; (c) forming a plurality of modifier material domains in the pores of the porous particles and adjacent to the electroactive material domains deposited in step (b); (d) contacting the particles from step (c) with a precursor of an electroactive material at a temperature effective to cause deposition of additional electroactive material domains in the pores of the porous particles and adjacent the modifier material domains formed in step (c); A method comprising:

41. The method according to claim 40, wherein the porous particles have any of the characteristics described for the porous particle scaffolds according to claims 2 to 11.

42. The porous particles have a D in the range of 0.5 μm to 30 μm, or 1 μm to 25 μm, or 1 μm to 20 μm, or 2 μm to 25 μm, or 2 μm to 20 μm, or 2 μm to 18 μm, or 2 μm to 15 μm, or 2 μm to 12 μm, or 2.5 μm to 15 μm, or 2.5 μm to 12 μm, or 2 μm to 10 μm. 50 42. The method of claim 40 or 41, wherein the particle size is

43. 43. A method according to any one of claims 40 to 42, wherein the electroactive material deposited in steps (b) and (d) is independently selected from silicon, tin, germanium, aluminium, and mixtures and alloys thereof, preferably the electroactive material deposited in at least one of steps (b) and (d) is silicon.

44. 44. A method according to any one of claims 40 to 43, wherein the electroactive material deposited in each of steps (b) and (d) is the same electroactive material, preferably the electroactive material deposited in each of steps (b) and (d) is silicon.

45. The precursor of the electroactive material in each of steps (b) and (d) is independently silane (SiH 4 ), disilane (Si 2 H 6 ), trisilane (Si 3 H 8 ), tetrasilane (Si 4 H 10 ), methylsilane, dimethylsilane, and chlorosilane.

46. 46. ​​A method according to any one of claims 40 to 45, wherein steps (b) and (d) are independently carried out at a temperature in the range of from 300°C to 800°C, or from 350°C to 800°C, or from 380°C to 700°C, or from 380°C to 650°C, or from 380°C to 600°C, or from 380°C to 550°C, or from 380°C to 500°C, or from 400°C to 450°C, or from 450°C to 500°C.

47. 47. The method of any one of claims 40 to 46, wherein step (b) and / or step (d) further comprises separating by-products from the particles.

48. 48. The method of any one of claims 40 to 47, wherein step (c) further comprises contacting the intermediate particles from step (b) with a passivating agent.

49. 49. The method of claim 48, wherein the passivation agent is selected from (i) an oxygen-containing gas, (ii) ammonia, (iii) a gas comprising ammonia and oxygen, and (iv) phosphine, preferably wherein the passivation agent is ammonia.

50. The passivation agent is (i)R 1 -CH=CH-R 1 、 ())) 1 .≡.!R 1 、 (iii)O=CR 1 R 1 、 (iv) HX-R 2 , and (v)HX-C(O)-R 1 (Wherein, X is O, S, NR 1 Or PR 1 indicates, Each R 1 independently represent H or an unsubstituted or substituted aliphatic or aromatic hydrocarbyl group having 1 to 20 carbon atoms, or two R 1 The group forms an unsubstituted or substituted ring structure containing from 3 to 8 carbon atoms in the ring; R 2 represents an unsubstituted or substituted aliphatic or aromatic hydrocarbyl group having 1 to 20 carbon atoms, or R 1 and R 2 together form an unsubstituted or substituted ring structure containing 3 to 8 carbon atoms in the ring; 49. The method of claim 48.

51. 49. The method of claim 48, wherein the passivation agent is selected from the group consisting of ethylene, propylene, 1-butene, butadiene, 1-pentene, 1,4-pentadiene, 1-hexene, 1-octene, styrene, divinylbenzene, acetylene, phenylacetylene, norbornene, norbornadiene, and bicyclo[2.2.2]oct-2-ene.

52. 52. The method of any one of claims 40-51, wherein step (c) comprises contacting the intermediate particles from step (b) with a carbon-containing precursor at a temperature effective to cause deposition of a pyrolyzable carbon material in the pores of the intermediate particles.

53. 53. The method of any one of claims 40 to 52, wherein steps (c) and (d) are repeated one or more times.

54. (e) forming a plurality of modifier material domains in the pores and / or on the exterior surface of the composite particles from step (d); The method of any one of claims 40 to 53, further comprising:

55. 55. The method of claim 54, wherein step (e) comprises contacting the surface of the composite particles from the last step (d) with a passivating agent, optionally wherein the passivating agent is as defined in any one of claims 49 to 51.

56. 56. The method of claim 54 or 55, wherein step (e) comprises combining the composite particles from step (d) with a pyrolytic carbon precursor and heating the pyrolytic carbon precursor to a temperature effective to cause deposition of a pyrolytic conductive carbon material within the pores and / or on the exterior surfaces of the composite particles.

57. The porous particles have a particle size distribution span (D 90 -D 10 ) / D 50 57. The method of any one of claims 40 to 56, comprising the steps of:

58. A composition comprising a particulate material according to any one of claims 1 to 39 and at least one other component.

59. 58. An electrode comprising a particulate material according to any one of claims 1 to 39 or a composition according to claim 58.

60. 60. A rechargeable metal-ion battery comprising the electrode of claim 59.

Citation Information

Patent Citations

  • Lithium secondary battery

    JP2003100284A

  • Lithium secondary battery

    JP2010262914A

  • Composite and method for producing the same

    JP2016132608A

  • Composite material and method of producing the same

    JP2018163776A

  • Composite core-shell particles

    JP2018524246A