Rubber Coating for Tire RFID Devices
A rubber coating with diene elastomer and 2,2'-methylene diphenol structure addresses corrosion issues in RFID devices, ensuring stability and performance while maintaining manufacturing efficiency and safety.
Patent Information
- Application Number
- JP2024524011
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-22
- Filing Date
- 2022-10-21
- Publication Date
- 2024-11-13
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing RFID devices in tires face issues with corrosion of brass antennas, leading to decreased transmission performance, accuracy, and structural instability, which compromises the durability and functionality of the tire.
A rubber coating comprising diene elastomer and a chemical substance with a 2,2'-methylene diphenol structure, optionally polymerized with alkylphenol units, is applied to surround the RFID device, enhancing adhesion and protecting the antenna from corrosion.
The solution ensures structural stability and durability of the RFID module, maintains reading performance, and improves worker safety without complicating the manufacturing process.
Smart Images

Figure 2024541896000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber coating for an RFID (radio frequency identification) device for a tire, an RFID (radio frequency identification) module for a tire comprising an RFID device surrounded by said rubber coating, tires and retread tires comprising said RFID device, and the use of the rubber coating surrounding said RFID device. [Background technology]
[0002] In the tire industry, manufacturers have expressed a need for a method that allows for automatic and unambiguous identification of tires from their manufacture through their use and disposal.
[0003] For example, specifically in tire production, automatic and unambiguous tire identification would enable manufacturers to optimize production processes and logistics operations, support the use of automated control systems, and perform efficient tire location / tracking, thus building smart tire factories.
[0004] Currently, several technical solutions are known to achieve this task, such as RFID (Radio Frequency Identification) technology through the use of RFID devices for tires.
[0005] The device essentially includes an RFID chip and an antenna connected to the chip. In some configurations, it may further include a second antenna electromagnetically coupled to the first antenna. The device is sandwiched and encapsulated between two outer rubber coating layers, one adjacent to the other, to completely enclose the RFID chip and antenna. The assembly of the RFID device and its surrounding rubber coating defines an RFID (radio frequency identification) module.
[0006] Antennas that connect to RFID chips commonly used to implement RFID devices are typically constructed of a multi-layer structure that includes a steel core coated with a layer of brass.
[0007] It is well known that brass is an alloy of copper and zinc, but by varying the ratio of the two materials, the mechanical, electrical and chemical properties can be altered, and brass can contain small percentages of a variety of other elements, including arsenic, lead, phosphorus, aluminum, manganese and silicon.
[0008] Brass is a material that is sensitive to the phenomenon of corrosion, which, under oxygen conditions, can form a product on its surface known as verdigris, and in the worst case scenario, can develop into a destructive corrosion process known as dezincification, in which zinc is dissolved from the alloy.
[0009] Such corrosion can lead to a decrease in the antenna's transmission performance, a decrease in the accuracy of reading the transmitted or received frequency signals, and even the failure of the RFID device. Corrosion of the brass-coated antenna can also affect the adhesion of the RFID device to the rubber coating that surrounds it.
[0010] If the RFID device is not properly secured to the surrounding rubber coating, the RFID module may break apart, preventing proper operation of the device and potentially damaging adjacent rubber layers when the module is assembled into the tire. If the RFID device becomes detached from the module due to poor adhesion to the surrounding rubber coating, it may cause cuts in the adjacent rubber of the tire in which it is assembled, compromising the durability of the tire.
[0011] To overcome the above problems, one solution known to experts in the field is to pretreat the antenna with the brass layer with an adhesion promoter. This method has the disadvantage that the pretreatment of the antenna adds a manufacturing step, which complicates the RFID manufacturing process and reduces productivity. Furthermore, the adhesion promoter is based on chemicals, which creates health and safety problems.
[0012] Therefore, a solution is needed that can ensure the structural stability and durability of tire RFID modules while maintaining the antenna reading performance and ensuring that the device will function properly over the long term.
[0013] The inventors of the present invention have devised a solution that meets the above-mentioned needs, does not impair the productivity of the RFID manufacturing process, and can ensure the safety of workers. Summary of the Invention
[0014] Therefore, the technical problem underlying the present invention is to overcome at least some of the above mentioned drawbacks with reference to the state of the art.
[0015] In a first aspect, the present invention relates to a rubber coating for an RFID (radio frequency identification) device, characterized in that it comprises: (a) 100 phr of at least one diene-based elastomer (b) at least one chemical entity according to formula 1 [ka] Here, the chemical substance contains at least a 2,2'-methylenediphenol structure in its structure, and the 2,2'-methylenediphenol may be substituted at the ortho-, para-, or meta-positions, or any combination thereof, with an aliphatic, linear or branched, hydrocarbon chain having 1 to 10 carbon atoms, or may be polymerized with one or more additional alkylphenol units at the ortho-, para-, or meta-positions, or any combination thereof.
[0016] In a second aspect, the present invention relates to an RFID module for a tire, said RFID module comprising at least an RFID device, said device comprising at least an antenna, said antenna having an outer surface, at least the outer surface of said antenna being surrounded by a rubber coating, said coating rubber being characterised in that (a) 100 phr of at least one diene-based elastomer (b) at least one chemical entity according to formula 1 [ka] Here, the chemical substance contains at least a 2,2'-methylenediphenol structure in its structure, and the 2,2'-methylenediphenol may be substituted at the ortho-, para-, or meta-positions, or any combination thereof, with an aliphatic, linear or branched, hydrocarbon chain having 1 to 10 carbon atoms, or may be polymerized with one or more additional alkylphenol units at the ortho-, para-, or meta-positions, or any combination thereof.
[0017] In a third aspect, the present invention relates to a tire or a retread tire comprising an RFID module according to the second aspect of the invention.
[0018] In a fourth aspect, the present invention relates to the use of a rubber coating according to the first aspect of the invention for enclosing an RFID device for a tyre, said RFID device comprising at least an antenna, said antenna having an outer surface, at least the outer surface of said antenna being surrounded by a rubber coating, characterised in that the rubber coating comprises: (a) 100 phr of at least one diene-based elastomer (b) at least one chemical entity according to formula 1 [ka] Here, the chemical substance contains at least a 2,2'-methylenediphenol structure in its structure, and the 2,2'-methylenediphenol may be substituted at the ortho-, para-, or meta-positions, or any combination thereof, with an aliphatic, linear or branched, hydrocarbon chain having 1 to 10 carbon atoms, or may be polymerized with one or more additional alkylphenol units at the ortho-, para-, or meta-positions, or any combination thereof.
[0019] Preferred features of the invention are the subject of the dependent claims. [Brief description of the drawings]
[0020] [Figure 1] Schematic diagram of an RFID module (E), which consists of an RFID device (C) consisting of an RFID chip (A) and one antenna electrically coupled thereto, which consists of two antenna branches (B1 and B2) and is surrounded by two layers of a coating compound (D). [Diagram 2] A second schematic diagram of an RFID module (E), which consists of an RFID chip (A) and an RFID device (C) consisting of one antenna electrically coupled to it, which in turn consists of two antenna branches (B1 and B2) and is surrounded by two layers of a coating compound (D). <rubber coating>
[0021] According to a first aspect, the present invention is directed to a rubber coating for an RFID device.
[0022] The rubber coating disclosed herein comprises: (a) 100 phr of at least one diene based elastomer; (b) at least one chemical entity according to Formula 1. [ka] Here, the chemical substance contains at least a 2,2'-methylenediphenol structure in its structure, and the 2,2'-methylenediphenol may be substituted at the ortho-, para-, or meta-positions, or any combination thereof, with an aliphatic, linear or branched, hydrocarbon chain having 1 to 10 carbon atoms, or may be polymerized with one or more additional alkylphenol units at the ortho-, para-, or meta-positions, or any combination thereof.
[0023] In a preferred embodiment, a rubber coating is disclosed for application to an RFID device. The rubber coating includes: (a) 100 phr of at least one diene-based elastomer (b) at least one chemical entity according to formula 1 [ka] Here, the chemical substance contains at least a 2,2'-methylenediphenol structure in its structure, and the 2,2'-methylenediphenol may be substituted at the ortho-, para-, or meta-positions, or any combination thereof, with an aliphatic, linear or branched, hydrocarbon chain having 1 to 10 carbon atoms, or may be polymerized with one or more additional alkylphenol units at the ortho-, para-, or meta-positions, or any combination thereof.
[0024] As used herein and hereinafter, the term "applied to," when used in relation to the rubber coating and the RFID device, means that the rubber coating effectively surrounds the RFID device, i.e., is disposed around all or at least a portion of the RFID device, and preferably directly contacts the RFID device.
[0025] As used herein and hereinafter, the terms "surrounding" and "surrounded by," when used in relation to a rubber coating and another element, such as an antenna or RFID device, mean that the rubber coating is disposed around all or at least a portion of that element (e.g., the antenna or RFID device), and preferably in direct contact with the element, independent of the method used to assemble the RFID module.
[0026] All descriptions of rubber coatings and components thereof provided herein should be understood to apply equally to each embodiment of the present invention, unless stated to the contrary.
[0027] Diene-based elastomers and chemicals according to the above structures are described in further detail below.
[0028] In the present specification and the following, the term "diene-based elastomer" refers to a polymer, copolymer, or combination thereof that contains a diene monomer. Non-limiting examples of diene-based elastomers suitable for use in rubber coatings include at least one of styrene-butadiene rubber (also referred to as SBR or styrene-butadiene copolymer), polybutadiene (also referred to as BR), natural rubber (also referred to as NR), ethylene propylene diene monomer rubber (also referred to as EPDM rubber), butyl rubber (also referred to as IIR), polyisobutylene rubber, epoxidized natural rubber (also referred to as ENR), neoprene, synthetic polyisoprene (also referred to as IR), polyurethane (also referred to as PU), etc.
[0029] The diene-based elastomer of the coating rubber may include a functionalized diene-based elastomer.
[0030] The term "functionalized diene-based elastomer" should be understood to include elastomers having functional groups at one or both chain ends, or in the backbone of the elastomer, and any combination thereof. For example, a silica-reactive functional group-containing elastomer can have functional groups at one or both chain ends, or in the backbone, or both.
[0031] Non-limiting examples of silica-reactive functional groups suitable for use in rubber coatings and known to be available for functionalizing diene-based elastomers include nitrogen-containing functional groups, silicon-containing functional groups, oxygen- or sulfur-containing functional groups, and metal-containing functional groups.
[0032] Preferably, the diene-based elastomer is selected from natural rubber, polyisoprene, or a mixture of the two.
[0033] The term "natural rubber" refers to naturally occurring 1,4-cis polyisoprene polymer that can be obtained from Hevea brasiliensis and sources other than Hevea brasiliensis (e.g., guayule shrub and dandelion such as TKS).
[0034] The term "natural rubber" should be understood to exclude synthetic polyisoprene. Polyisoprene can be understood to mean a homopolymer of the isoprene monomer and should not be understood to include naturally occurring rubber. However, the term polyisoprene should be understood to include polyisoprene produced from natural sources of isoprene monomer.
[0035] The coating rubber in the first to fourth embodiments further contains a chemical substance according to formula 1 that contains at least a 2,2'-methylenediphenol structure in its structure. [ka] Here, 2,2'-methylenediphenol may be substituted at the ortho-, para-, or meta-positions, or any combination thereof, with an aliphatic, linear or branched, hydrocarbon chain having 1 to 10 carbon atoms, or may be polymerized with one or more additional alkylphenol units at the ortho-, para-, or meta-positions, or any combination thereof.
[0036] Ortho, para or meta positions are understood to refer to the position of a substituent on a carbon atom of a benzene relative to an -OH which would be assumed to occupy the 1 position. The positions are numbered in a clockwise direction. Thus, if a substituent occupies the position adjacent to the -OH (2 or 6 position), it is referred to as an ortho substituent, if a substituent occupies the 3 or 5 position relative to the -OH, it is referred to as a meta substituent, and if a substituent occupies the position opposite the -OH (4 position), it is referred to as a para substituent.
[0037] According to a preferred embodiment, the chemical is derived from 2'2-methylenediphenol by polymerizing it with one or more additional alkylphenol units at the ortho, para, meta positions or any combination thereof.
[0038] As used herein, the term "polymerizing" refers to the act of carrying out the chemical process of polymerization, which refers to any process in which relatively small molecules called monomers react together under specific conditions to produce much larger chains or networks of molecules called polymers.
[0039] According to a preferred embodiment, the chemical is an alkylphenol formaldehyde (APF) resin.
[0040] The terms "phenol formaldehyde resin" and "alkylphenol formaldehyde" refer to synthetic polymeric structures obtained by the reaction of phenol or substituted phenols (alkylphenols) with formaldehyde.
[0041] Generally, phenol-formaldehyde or alkylphenol-formaldehyde resins are formed by a step-growth polymerization reaction, either acid- or base-catalyzed, in which a phenol or alkylphenol reacts with formaldehyde at the ortho and / or para positions to form methylene bridges at either the ortho or para positions of the phenol ring, producing methylene bisphenol dimers that participate in further reactions as the polymerization proceeds. As known to those skilled in the art, the para position is approximately twice as reactive as the ortho position, but because there are twice as many ortho positions (two per phenol molecule), the structure contains roughly equal proportions of ortho-ortho, para-para, and ortho-para bridges, resulting in random orientation and branching of the structure as the reaction proceeds, resulting in a highly complex mixture of polymers of different sizes and structures.
[0042] According to a further preferred embodiment, the alkylphenol formaldehyde resin is a novolac resin.
[0043] Novolac resins are alkylphenol-formaldehyde resins obtained by reacting formaldehyde and phenol in a molar ratio of formaldehyde to phenol less than 1. The polymerization is completed using an acid catalyst. Novolac resins are often produced by polymerization of cresol (methylphenol) monomers. The monomer ratio and acidic reaction environment allow for control of random orientation and branching of the structure, producing long linear structures with little branching. Polymerization preferably occurs at the ortho position of the phenolic groups, resulting in a structure with the phenolic groups oriented in approximately the same direction, as depicted in Equation 3. [ka]
[0044] According to a further preferred embodiment, the chemical is 2,2'-methylenebis(4-methyl-6-tert-butylphenol).
[0045] The methylene diphenol dimer is substituted at the para position with a methyl group and at the ortho position with a t-butyl group, as depicted in Formula 2. [ka]
[0046] According to a further preferred embodiment, the chemical may be a mixture of APF resin, preferably a novolac resin and 2,2'-methylenebis(4-methyl-6-tert-butylphenol).
[0047] According to a preferred embodiment, the chemicals may be introduced into the rubber coating in an amount ranging from 0.1 to 10 phr, preferably from 0.1 to 7 phr. In a particularly preferred embodiment, 2,2'-methylenedi(4-methyl-6-tert-butylphenol) may be added in an amount ranging from 0.1 to 3 phr. In a further preferred embodiment, an APF resin, preferably a novolac resin, may be introduced in an amount ranging from 0.1 to 7 phr.
[0048] The rubber coating may further comprise at least one filler. The at least one filler may be selected from carbon black, silica, graphite, graphene, carbon nanotubes, recycled carbon black, clay, titanium dioxide, magnesium dioxide, aluminum oxide, starch, boron nitride, silicon nitride, aluminum nitride, calcium silicate, silicon carbide, or mixtures thereof. In certain embodiments, the rubber coating comprises 1-120 phr of filler, preferably 10-110, more preferably 20-100, more preferably 30-90, and even more preferably 40-80 phr of filler. In certain embodiments, the rubber coating may not comprise any filler (i.e., 0 phr). In a preferred embodiment, the filler comprises silica. In a more preferred embodiment, the only component of the filler is silica.
[0049] When silica is used in the rubber composition disclosed herein, in certain embodiments, at least one silane coupling agent may be used. According to certain embodiments, the silane coupling agent is present in an amount of 0.01-40%, preferably 0.01-30%, more preferably 0.01-25% by weight of the silica. In general, any conventional silane coupling agent can be used, including those having silicon groups and moieties and capable of reacting with rubber, particularly vulcanizable rubber. The silane coupling agent acts as a bridge connecting the silica to the rubber. Suitable silane coupling agents include those containing groups such as mercapto, blocked mercapto, polysulfide, amino, vinyl, epoxy, and combinations thereof. Preferably, the silane used in the present invention is bis-(3-triethoxy-silylpropyl) disulfide (Si75).
[0050] According to certain embodiments, the rubber coating may further comprise one or more additional components, non-limiting examples of which are described below.
[0051] The rubber coating may further include one or more process oils, which are useful for improving processability by reducing the Mooney viscosity of the rubber coating before curing. In such embodiments, the one or more process oils may be added to the rubber coating as free oils, or as part of at least one diene-based elastomer (i.e., as extender oils), or a combination of both. Non-limiting examples of oils useful in rubber coatings include paraffinic, naphthenic, aromatic, and the like. Preferably, the oil used in the present summary invention is a RAE oil. The coating rubber may include 0 (any) to 40 phr (process, extender, or both) of oil, and may consist of one or more oils as described above, preferably 1 to 35 phr, more preferably 5 to 25 phr, and even more preferably 5 to 20 phr.
[0052] The rubber coating may further include other conventional rubber additives, including, for example, antidegradants such as antioxidants and antiozonants.
[0053] Antidegradants are components added to protect rubber from oxidative attack. Examples of antidegradants include phenylenediamines such as N-(1,3-dimethylbutyl)-N'-phenyl-1,4-benzenediamine (6PPD), trimethyldihydroquinolines such as 2,2,4-trimethyl 1-1,2-dihydroquinoline-containing (TMQ), phenols, alkylated diphenylamines (DPAs), paraffin waxes or microcrystalline waxes or blends thereof, aromatic phosphites, and diphenylamine-ketone condensates. The appropriate amounts of these components can be determined by those skilled in the art.
[0054] The rubber coating may further include a curing package. In general, the curing package includes at least one of a vulcanizing agent, a vulcanization accelerator, a vulcanization activator (e.g., zinc oxide, stearic acid, etc.), a vulcanization inhibitor, and an anti-scorching agent. The vulcanization package usable in the present invention includes at least one vulcanizing agent, at least one vulcanization accelerator, at least one vulcanization activator, and optionally a vulcanization inhibitor and / or an anti-scorching agent. The vulcanization accelerator and the vulcanization activator act as a catalyst for the vulcanization agent. The vulcanization inhibitor and the anti-scorching agent are known in the art and can be selected by a person skilled in the art based on the desired vulcanization properties.
[0055] Examples of vulcanizing agents suitable for use in rubber coatings include, but are not limited to, sulfur-based or peroxide-based vulcanizing components. Specific examples of suitable sulfur vulcanizing agents include soluble sulfur; sulfur donating vulcanizing agents such as amine disulfides, polymeric polysulfides, or sulfur olefin adducts; and insoluble polymeric sulfur. Preferably, the sulfur vulcanizing agent is insoluble sulfur or a mixture of soluble and insoluble polymeric sulfur. Vulcanizing agents can be used alone or in combination. Generally, the vulcanizing agent is used in an amount ranging from 0.1 to 10 phr, preferably from 1 to 8 phr.
[0056] Vulcanization accelerators are used to control the time and / or temperature required for vulcanization and to improve the properties of the vulcanizate. Examples of vulcanization accelerators suitable for use in the rubber coating of the present invention include, but are not limited to, thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole and 2,2'-dithiobis(benzothiazole) (MTBS); sulfenamide-based accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide (CBS) and N,N-dicyclohexyl-2-benzothiazole sulfenamide (DCBS); guanidine-based vulcanization accelerators such as diphenylguanidine (DPG); carbamate-based vulcanization accelerators; hexamethylene-1,6-bisthiosulfuric acid (HTS); and the like. Preferably, the vulcanization accelerator used in the present invention is CBS or DPG, or a mixture thereof. In general, the amount of the vulcanization accelerator used is 0.1 to 10 phr, preferably 0.5 to 5 phr.
[0057] Vulcanization activators are additives used to assist vulcanization. Generally, vulcanization activators include inorganic and organic components. Zinc oxide is the most widely used inorganic vulcanization activator. Commonly used organic vulcanization activators include stearic acid, palmitic acid, lauric acid, and their zinc salts. Generally, the amount of vulcanization activator used ranges from 0.1 to 9 phr, more preferably 0.5 to 6 phr.
[0058] Vulcanization inhibitors are used to control the vulcanization process, typically slowing or inhibiting vulcanization until a desired time and / or temperature is reached. Common vulcanization inhibitors include, but are not limited to, PVI (cyclohexylthiophthalimide). Generally, the amount of vulcanization inhibitor is 0.1-3 phr, preferably 0.5-2 phr.
[0059] According to certain embodiments, the rubber coating may further include an organic salt or complex of cobalt as an additive as an adhesion promoter. As known to those skilled in the art, the adhesive interface between the rubber coating and the metal surface of the antenna plays a major role in the durability of the RFID module. To improve adhesion, an organic salt or complex of cobalt may be included in the composition as an additive. Examples of cobalt salts suitable for use in the coating rubber of the present invention include, but are not limited to, cobalt neodecanoate borate or cobalt neodecanoate. Generally, the amount of cobalt salt used is 0.1-5 phr, more preferably 0.5-3 phr.
[0060] <RFIDデバイス> In a second aspect, an RFID module for a tire is disclosed, the RFID module comprising at least an antenna, the antenna preferably having a core covered with a brass layer, the antenna having an outer surface, at least the outer surface of the antenna being surrounded by a rubber coating, the rubber coating comprising: (a) 100 phr of at least one diene-based elastomer (b) at least one chemical entity according to formula 1 [ka] Here, the chemical substance contains at least a 2,2'-methylenediphenol structure in its structure, and the 2,2'-methylenediphenol may be substituted at the ortho-, para-, or meta-positions, or any combination thereof, with an aliphatic, linear or branched, hydrocarbon chain having 1 to 10 carbon atoms, or may be polymerized with one or more additional alkylphenol units at the ortho-, para-, or meta-positions, or any combination thereof.
[0061] The RFID device includes at least one antenna electrically connected to the chip, the antenna having an outer surface, the outer surface of the antenna surrounded by a rubber coating. According to a particular embodiment, at least a majority of the outer surface of one antenna is surrounded by the rubber coating. In this specification, the expression "a majority" means more than 50% and 100%. According to a preferred embodiment, the antenna is a dipole antenna, the dipole antenna including two antenna branches protruding in opposite and different directions of the chip of the RFID device. According to a particular embodiment, a majority of the outer surface of both antenna branches is surrounded by the coating rubber. According to a further embodiment, the RFID device includes two antennas electromagnetically coupled to each other, one of the two antennas being electrically connected to the chip. According to a particular embodiment, a majority of the outer surfaces of the two antennas are surrounded by the rubber coating. According to yet another embodiment, the entire outer surface of the RFID device is surrounded by the rubber coating.
[0062] The rubber coating can be disposed on the RFID device in a variety of ways. According to certain embodiments, the rubber coating is disposed on the RFID device as a sheet or layer of rubber. More specifically, according to such embodiments, the rubber coating is calendered or otherwise formed into an uncured sheet of rubber of uniform thickness (e.g., 0.2 mm to about 1.2 mm). The RFID device is placed on top of the rubber sheet such that a portion of the bottom surface of the RFID device is in contact with the rubber sheet. A second rubber sheet (typically having the same thickness as the first rubber sheet) is placed over the top of the RFID device such that the exterior surface of the RFID device is coated with two rubber layers. The two rubber layers are then pressed together to promote adhesion between the first and second rubber layers with the RFID device substantially trapped between them. The adhesion of the two rubber layers can be assisted in a variety of ways, such as using a dual roller assembly to press the parts together and expel trapped air, sewing the layers together (e.g., by using a sewing roller), by manual finger pressure, using an inflatable bladder, using a compression molding tool, or any method suitable for assisting in the adhesion of the two rubber layers. Preferably, the RFID module, including the RFID device and the rubber coating, has a total thickness of 6 mm.
[0063] According to an embodiment of the present invention, an RFID device comprises an RFID chip and at least one antenna connected to the chip.
[0064] Typically, RFID antennas are formed in a layered structure and include a core and a covering layer. Several materials are known in the art for the manufacture of RFID antennas. In particular, the core is generally a metal core. The covering layer can be formed of brass or copper or a copper alloy, such as a copper-nickel (Cu-Ni) alloy.
[0065] According to a preferred embodiment of the present invention, the antenna that connects to the RFID chip includes a multi-layer structure consisting of a steel core covered with a layer of brass.
[0066] <Tires> According to a third aspect of the invention, the RFID module described herein is incorporated into a tire or a retread tire. In other words, the third embodiment is directed to tires and retread tires, the tires and retread tires comprising an RFID module, the RFID module including an RFID device, the RFID device including at least an antenna, the antenna preferably having a core covered with a brass layer, the antenna having an outer surface, at least the outer surface of the antenna being surrounded by a rubber coating, and including: (a) 100 phr of at least one diene-based elastomer (b) at least one chemical entity according to formula 1 [ka] Here, the chemical substance contains at least a 2,2'-methylenediphenol structure in its structure, and the 2,2'-methylenediphenol may be substituted at the ortho-, para-, or meta-positions, or any combination thereof, with an aliphatic, linear or branched, hydrocarbon chain having 1 to 10 carbon atoms, or may be polymerized with one or more additional alkylphenol units at the ortho-, para-, or meta-positions, or any combination thereof.
[0067] According to further embodiments, the RFID modules may be incorporated into various components of the tire, such as the tread, sidewall, belt skim, or carcass.
[0068] In this specification and hereinafter, the term "tire" includes used or worn tires that have had a new tread strip applied to the outer surface of the tire casing in a process called retreading. Tires that have undergone such a process are commonly referred to as retread tires.
[0069] As used herein and hereinafter, the term "retread tire" includes the meaning of a pre-prepared tread slip that is applied to the tire casing in the tire retreading process.
[0070] As used herein and hereinafter, the terms "incorporated" or "incorporated into" include not only embedding or inserting within a tire or retreaded tire, but also other methods such as associating with the tire or retreaded tire, for example, using a patch on the exterior surface of the tire, such as in an innerliner or sidewall.
[0071] According to a further embodiment, a patch used to associate an RFID module with a tire or retread tire may have the rubber coating configuration disclosed according to the first embodiment of the present invention.
[0072] According to a further embodiment, the rubber coating surrounding at least an outer surface of the at least one antenna of the RFID device is cured (vulcanized) prior to incorporation of the RFID module into the tire or tire component.
[0073] According to such an embodiment, when a rubber coating surrounding at least an outer surface of at least one antenna of an RFID device in an RFID module is cured prior to incorporation of the rubber coating into a tire or tire component, the RFID module may be adhered to the cured rubber coating of the tire or tire component using a patch, a suitable adhesive, or a cement capable of withstanding the operating conditions of the tire. In certain embodiments, the patch may include a rubber coating surrounding at least an outer surface of at least one antenna of the RFID device.
[0074] Additionally, the coating rubber surrounds at least an outer surface of at least one antenna of the RFID device in the RFID module and may be incorporated into the tire or retread tire prior to curing the rubber coating of the RFID module. In such an embodiment, the RFID module including the uncured rubber coating is incorporated into the tire or retread tire at a desired location. The uncured rubber coating of the RFID module is cured simultaneously with the tire or retread tire.
[0075] Generally, when the rubber coatings described herein are used on tires or retread tires, the compositions are incorporated into the tire or retread tire in accordance with conventional tire manufacturing techniques, including standard rubber molding, shaping, and curing techniques.
[0076] In a fourth aspect, the present invention is directed to the use of a rubber coating comprising: (a) 100 phr of at least one diene-based elastomer (b) at least one chemical entity according to formula 1 [ka] wherein the chemical compound includes in its structure at least the structure of 2,2'-methylenediphenol, which may be substituted at the ortho, para, meta or any combination thereof with an aliphatic, linear or branched, hydrocarbon chain having 1 to 10 carbon atoms, or may be polymerized at the ortho, para, meta or any combination thereof, and may be incorporated into the tire or retread tire according to the third embodiment to surround the RFID device. EXAMPLES
[0077] The following examples illustrate specific and exemplary embodiments and / or features of the present disclosure. The examples are disclosed for illustrative purposes only and should not be construed as limitations of the present disclosure. Many modifications to the specific examples are possible without departing from the scope of the present invention.
[0078] More specifically, the diene-based elastomers, fillers, and other ingredients (e.g., curable package ingredients, antidegradants, or process oils, etc.) used in the following examples are not to be construed as limiting, and other or additional ingredients consistent with the disclosure in the detailed description may be substituted.
[0079] A control composition (Example C) and two different examples of the present invention were prepared: Examples A (1-3) and Examples B (1-3). Examples A (1-3) are different from the control composition of Example C in that they have a different content of one chemical substance in the present invention, namely, the content of alkylphenol formaldehyde resin (APF resin), especially the content of novolac resin. Examples B (1-3) are different from the control composition of Example C in that they have a different content of one chemical substance in the present invention, namely, the content of 2,2'-methylenebis(4-methyl-6-tert-butylphenol) (NS6). The composition of all the examples of coating rubber (control and present invention) was prepared according to the formulation shown in Table 1, and all the components in Table 1 are shown in phr.
[0080] [Table 1]
[0081] The silane coupling agent used was bis-(3-triethoxy-silylpropyl) disulfide silane (Si75).
[0082] The accelerator used was N-cyclohexyl-2-benzothiazole sulfenamide (CBS).
[0083] The oil used was residual aromatic extract (RAE).
[0084] The cobalt used was neodecanoate.
[0085] The APF resin used is a novolac resin.
[0086] All example rubber compositions in Table 1 were mixed according to the following mixing procedure:
[0087] The crosslinkable polymer base and carbon black were charged into a mixer with an internal volume of 230-270 liters equipped with a tangential rotor before mixing began, reaching a filling rate of 66-72%.
[0088] (First mixing step) The mixer was operated at a speed in the range of 40-60 revolutions per minute, and the resulting mixture was discharged after reaching a temperature in the range of 140-160°C.
[0089] (Second mixing step) The mixture obtained in the previous step was treated again in a mixer operated at a range of 40-60 revolutions per minute, and then discharged after reaching a temperature in the range of 130-15°C.
[0090] (Final Mixing Step) The vulcanization system (sulfur, accelerators, antireversion agents, antioxidants / antiozonants, zinc oxide) was added to the mixture obtained in the previous step until the filling rate reached 63–67%.
[0091] The kneading was carried out at a rotation speed in the range of 20 to 40 revolutions per minute, and the resulting mixture was discharged after reaching a temperature in the range of 100 to 110°C.
[0092] Each rubber composition in Table 1 was used to prepare an RFID module consisting of an RFID device surrounded by a coating rubber and was used according to each example in Table 1. Such an RFID module was prepared by the following method.
[0093] The rubber coating according to the embodiment was calendered into a sheet or layer form with an average thickness of 0.6 mm and placed on the RFID device. The RFID device was placed on the upper surface of the rubber sheet, and a part of the lower surface of the RFID device was brought into contact with the rubber sheet. A second rubber sheet (the same thickness as the first rubber sheet) was placed on the upper surface of the RFID device, and the outer surface of the RFID device was covered with two rubber layers. Next, the two rubber layers were pressed together with the RFID device sandwiched therebetween to promote the adhesion between the first rubber layer and the second rubber layer. The adhesion of the two rubber layers was assisted by pressing the parts together using a roller assembly and discharging the trapped air.
[0094] At the end of this process, the total thickness of the RFID module composed of the RFID device and the surrounding rubber coating is 6 mm.
[0095] The above RFID module was tested to evaluate the adhesion of the rubber coating to the following RFID devices: CRA force evaluation and CRA coverage rate.
[0096] <CRA Force Evaluation> By this test method, the force required to pull the RFID device from the rubber pad can be measured. The test was carried out according to the following procedure: A sample of the RFID device to be evaluated was coated with the coating rubber according to the present invention. The test was performed by pulling the RFID device at a peeling angle of 180° from the coating rubber, and using a constant tensile force (CRE) tester, the maximum force applied to pull the device from the rubber pad was measured. The test procedure was to place approximately 2 mm of the exposed end of the RFID antenna at the center of the upper clamp of the tester, and place approximately 2 mm of the end of the pad from which the RFID needed to be peeled at the lower clamp. The axis of the pad needs to be parallel to the vertical axis of the tester. The RFID device was pulled from the pad, and the maximum peel force (Newton) required to peel the device was recorded. The test was carried out at room temperature.
[0097] The value of the peel force was normalized with respect to an RFID device coated with a conventional coating compound (C). For the compound in Control C, the peel force when the RFID device peels off from the coating agent was set to 100 as before.
[0098] The higher the value of the example of the present invention is compared to the control, the higher the adhesive force to the RFID coating compound, because this means that the force applied to remove the RFID from the rubber pad becomes larger.
[0099] <CRA coating rate> By this test method, after peeling the RFID device from the rubber pad, the amount of rubber coating the RFID device can be ranked to evaluate the adhesion characteristics. This is by visual judgment.
[0100] Samples of the RFID devices to be evaluated were coated with the coating rubber of the present invention. The test was performed by pulling the RFID device at a peeling angle of 180° from the coating rubber, using a constant tensile force (CRE) tester. The test procedure was to place approximately 2 mm of the exposed end of the RFID antenna at the center of the upper clamp of the tester, and place approximately 2 mm of the end of the pad from which the RFID needs to be peeled at the lower clamp. The axis of the pad needs to be parallel to the vertical axis of the tester. The RFID device was pulled out from the pad, and the test was stopped when the pulled-out RFID reached a line of approximately 30 mm. The test was performed at room temperature.
[0101] Before removing the pad from the clamp, the rubber coating rate of the RFID device was visually determined and recorded. The rank is represented by the ratio of the rubber still covering the RFID antenna surface.
[0102] The rank of the rubber coating rate was recorded in comparison with a control RFID device coated with a conventional coating compound (C). The rank of Control C was conventionally 10%.
[0103] Higher values for the inventive examples versus the control indicate stronger adhesion due to less exposed RFID antenna surface.
[0104] The test results for each RFID device coated with the example rubber coating are shown in Table 2. The results were indexed against the results for the control Compound C, which represents a rubber coating commonly used for RFID devices, as described above.
[0105] [Table 2]
[0106] As shown in the results table above, the values obtained by the CRA force evaluation test indicate that each rubber coating of the present invention can increase adhesion to the control compound after aging with water or oxygen, respectively. Consistently, the CRA coverage evaluation showed a higher adhesion performance of the rubber coating of the present invention compared to the control compound. The increase in adhesion of the rubber coating to the RFID device was achieved without treating the antenna with an adhesion promoter. Thus, the present invention can therefore meet the need to ensure the structural stability and durability of the RFID module inserted into the tire and at the same time maintain the reading performance of the antenna without compromising the productivity and safety of the workers in the RFID manufacturing process.
Claims
1. 1. A rubber coating for an RFID device for tires, comprising: (a) 100 phr of at least one diene-based elastomer. (b) at least one chemical entity according to Formula 1 [Formula 1] Including, wherein the chemical comprises in its structure at least a 2,2'-methylenediphenol structure, the 2,2'-methylenediphenol being optionally substituted at the ortho, para, meta or any combination thereof with an aliphatic, linear or branched, hydrocarbon chain having 1 to 10 carbon atoms, or optionally polymerized with one or more additional alkylphenol units at the ortho, para, meta or any combination thereof. A rubber coating comprising:
2. 2. The rubber coating according to claim 1, characterized in that the chemical is selected from phenol formaldehyde resins, preferably selected from novolac resins or 2,2'-methylenebis(4-methyl-6-tert-butylphenol), or a combination of the two.
3. A rubber coating according to claim 1 or 2, characterized in that it contains 0.1 to 10 phr, preferably 0.1 to 7 phr, of said chemical substance.
4. A rubber coating according to any one of claims 1 to 3, further comprising at least one filler.
5. 5. The rubber coating of claim 4, wherein the filler is silica.
6. A rubber coating according to any one of the preceding claims, characterised in that the diene based elastomer is natural rubber or polyisoprene or a mixture of the two.
7. 7. An RFID module for a tire, comprising an RFID device including at least an antenna, the antenna having an outer surface, at least a portion of the outer surface of the antenna being surrounded by a rubber coating according to any one of claims 1 to 6.
8. 8. The RFID module of claim 7, wherein the antenna includes a core, the core being at least partially coated with a layer of brass.
9. An RFID module according to any one of claims 7 to 9, characterized in that the RFID device is largely surrounded by the rubber coating, preferably the entire RFID device is surrounded by the rubber coating.
10. Tyre or retread tyre, characterised in that it comprises an RFID module according to any one of claims 7 to 9.
11. 7. Use of a rubber coating according to any one of claims 1 to 6 to surround an RFID device for a tire, said RFID device comprising at least an antenna, said antenna having an outer surface, such that at least the outer surface of the antenna is surrounded by the rubber coating.
12. 13. The use of the coating rubber according to claim 12, characterized in that the antenna includes a core, the core being at least partially coated with a brass layer.
Citation Information
Patent Citations
Pneumatic tire
JP2017222294A
Rubber coating for electronic communication modules, electronic modules including the same, and related methods
JP2019502769A
Tire equipped with a radio frequency communication module
JP2021514891A
Rubber-covered textile cords, tires containing same, and related methods
US20180147888A1
Method to manufacture an electronic device for a rubber article
WO2021014278A1