A liquid molding compound, a reaction product that becomes plateable when exposed to laser energy

A thermosetting resin composition with silica and spinel crystals addresses warpage issues in LCM and stencil printing, enabling reliable three-dimensional semiconductor interconnect devices through laser-activated plating.

JP2024542190APending Publication Date: 2024-11-13HENKEL KGAA
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024529403
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-17
Filing Date
2022-11-17
Publication Date
2024-11-13

AI Technical Summary

Technical Problem

Existing liquid compression molding (LCM) and stencil printing techniques face challenges in addressing warpage issues in semiconductor packaging, particularly as package sizes increase and wafer thickness decreases, leading to potential semiconductor package failure.

Method used

A thermosetting resin composition is developed that includes a thermosetting resin matrix, silica filler, and spinel crystals, which can be cured and then laser-activated to form spinel crystal residues for electroless plating, reducing warpage and enabling three-dimensional interconnect devices.

Benefits of technology

The composition exhibits low warpage resistance, maintaining desirable physical properties during curing and subsequent processing, allowing for the construction of three-dimensionally shaped electrically interconnected semiconductor devices with improved reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542190000001_ABST
    Figure 2024542190000001_ABST
Patent Text Reader

Abstract

A flowable thermosetting resin composition useful for liquid compression molding ("LCM") or stencil printing applications is provided, the reaction product of which becomes non-flowable after exposure to elevated temperatures and is then plateable when exposed to laser energy.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] A flowable thermosetting resin composition useful for liquid compression molding ("LCM") or stencil printing applications is provided, the reaction product of which becomes non-flowable after exposure to elevated temperatures and is then plateable upon exposure to laser energy. [Background technology]

[0002] As semiconductor packages continue to evolve, the requirements for encapsulation of materials are also changing. To protect electronic components such as semiconductor devices, a method of applying a solid epoxy resin composition and then transferring molding is commonly used. However, as semiconductor devices become thinner and denser, this method has limitations because of the possibility of poor flow near fine openings and damage to some delicate components.

[0003] Therefore, LCM or stencil printing has been developed as a processing technology to help protect electronic devices. Compared to transfer molding, LCM or stencil printing has the advantage that the resin can easily flow into narrow gaps and is less likely to damage electronic components. Many semiconductor wafer-level packages ("WLP") already use LCM to encapsulate thin and delicate devices.

[0004] However, LCM or stencil printing presents many challenges to meet the commercial volume and reliability demands required by the semiconductor packaging industry, especially WLP.

[0005] Warpage is a common problem found in many cured LCM or liquid encapsulants. This is especially evident as package sizes increase and wafer thickness continues to decrease. These contrasting demands can cause the warpage problem to become too severe to meet processing requirements, leading to semiconductor package failure.

[0006] To address the warpage issue, many LCMs or liquid encapsulants have been formulated to reduce the modulus and glass transition temperature ("Tg"), however, going down this path makes it less likely that the encapsulated package will pass reliability testing.

[0007] Conventional materials used to form molded wafers either do not have the desired physical properties to improve resistance to wafer bow or are not suitable for application with LCM processing techniques.

[0008] Attempts have been made in the past to address the problem of warping. For example, U.S. Patent No. 9,263,360 claims a thermosetting resin composition comprising a thermosetting resin matrix including an epoxy resin component, an epoxy hardener consisting of a phenolic novolac component, and optionally a combination of additional components selected from episulfide resins, oxazines, oxazolines, cyanate esters, maleimides, nadimides, itaconimides, and combinations thereof; block copolymers, silica fillers, and optionally catalysts and accelerators, where the block copolymers are amphiphilic and selected from copolymers made from polystyrene, 1,4-polybutadiene, syndiotactic poly(methyl methacrylate); polymethyl methacrylate-block-polybutyl acrylate-block polymethyl methacrylate copolymers; and combinations thereof. The silica filler constitutes 50-90% by weight of the composition.

[0009] Also, U.S. Patent No. 8,847,415 claims a curable resin composition for liquid compression molding that includes a curable resin matrix, a curing component that includes a cationic catalyst and an oxidizer. Upon curing, the composition exhibits a DSC peak of less than 140° C. and a delta temperature between the onset temperature and the peak on the DSC of less than 20° C.

[0010] In U.S. Patent No. 9,263,360, a thermosetting resin composition is provided that includes a thermosetting resin matrix, a block copolymer, a silica filler, and a curing component that includes a combination of an anhydride or phenolic resin and an imidazole. Upon curing, the composition has a modulus at room temperature in the range of about 22 GPas or less, a CTEα1 of 10 μm / ° C. or less, and a T g1 and T of about 100℃ to 150℃ g2 The figures show several Tgs, including:

[0011] Similarly, U.S. Patent No. 6,727,325 claims an epoxy resin composition comprising an epoxy resin before curing and a clathrate comprising a tetrakisphenol compound represented by a specific formula and a compound capable of reacting with the epoxy resin to cure the resin.

[0012] And International Patent Publication No. WO2020 / 037199 describes a thermosetting resin composition including a thermosetting resin matrix, a silica filler, and a curing component, the curing component including a combination of clathrates including a combination of a tetrakisphenol compound and a nitrogen-containing curing agent, wherein the composition increases in viscosity by less than about 30% after storage at room temperature for 24 hours, and when the composition is cured on a wafer, the composition exhibits a warp of less than about 3 cm after oven curing.

[0013] Currently, the industry is moving towards integrating electrical circuitry directly into or onto molded packages that have dielectric properties.

[0014] For example, U.S. Patent No. 7,547,849 (Lee) states: A. a polymeric binder selected from epoxy resins, silica filled epoxies, bismaleimide resins, bismaleimide triazines, fluoropolymers, polyesters, polyphenylene oxide / polyphenylene ether resins, polybutadiene / polyisoprene crosslinkable resins (and copolymers), liquid crystal polymers, polyamides, cyanate esters, and combinations thereof, the polymeric binder being present in an amount of 50-97% by weight of the total weight of the composite film; and B. a spinel crystal filler present in an amount of 3 to 50 weight percent of the total weight of the composite film; A laser light activatable, plateable, free-standing composite film comprising: The polymer composite has an extinction coefficient from 400 nm to 1,000,000 nm of 0.05 to 0.6 per micron, the spinel crystal filler has the chemical formula AB2O4 or BABO4, where A is a divalent metal cation selected from cadmium, zinc, copper, cobalt, magnesium, tin, titanium, iron, aluminum, nickel, manganese, chromium, and combinations of two or more thereof, and B is a trivalent metal cation selected from cadmium, manganese, nickel, copper, cobalt, iron, tin, titanium, aluminum, chromium, and combinations of two or more thereof, and the film is a free-standing film.

[0015] Furthermore, US Patent Application Publication No. 2019 / 0292386 (Meura) relates to a thermosetting resin composition for laser direct structuring (LDS) comprising a thermosetting resin; an inorganic filler; a non-conductive metal compound that forms a metal core upon irradiation with active energy rays; and a coupling agent. The non-conductive metal compound includes one or more selected from the group consisting of spinel-type metal oxides, metal oxides having two or more transition metal elements in adjacent groups, groups selected from groups 3 to 12 of the periodic table, and tin-containing oxides. The coupling agent includes one or more selected from mercaptosilanes, aminosilanes, and epoxysilanes.

[0016] Notwithstanding these recent efforts, it would be desirable to provide new LCM or stencil printing materials, particularly materials that are flowable, laser activatable, and plateable, while at the same time improving their resistance to wafer bow, thereby providing end users with multiple options and a source of solutions to address the recurring problem of wafer bow.

[0017] Existing technology also allows for improved ability to form thinner dielectric layers during molding, thereby increasing package feature density and removing package design constraints. [Prior art documents] [Patent documents]

[0018] [Patent Document 1] U.S. Patent No. 9,263,360 [Patent Document 2] U.S. Patent No. 8,847,415 [Patent Document 3] U.S. Patent No. 9,263,360 [Patent Document 4] U.S. Patent No. 6,727,325 [Patent Document 5] International Patent Publication No. WO2020 / 037199 [Patent Document 6] U.S. Patent No. 7,547,849 [Patent Document 7] US Patent Application Publication No. 2019 / 0292386 Summary of the Invention [Means for solving the problem]

[0019] The present disclosure provides solutions to these problems and meets a market need in this regard.

[0020] Provided herein is a thermosetting resin composition that can be cured by exposure to high temperature conditions. Once cured, the cured composition can be activated with a laser and plated. In this regard, plating is the basis of laser direct structuring ("LDS") for producing three-dimensional molded interconnect devices ("MIDs"). Here, in LDS, spinel crystals are available at or near the surface of the cured composition and can receive the laser energy applied thereto (the surface may be considered during the through via approach). After laser energy ablation in a predetermined pattern on the surface of the cured composition, the spinel crystals may act as seeds to enable electroless or other plating, thereby forming a plating pattern in the ablated portions.

[0021] In addition, after the thermosetting resin has hardened, the molded substrate is less likely to warp.

[0022] More specifically, the compositions of the present invention are useful as liquid compression molding encapsulants that exhibit low warpage after compression molding and oven curing while maintaining desirable physical properties of the molding compound. The compositions exhibit low storage modulus at room temperature (e.g., about 25 GPas or less, desirably in the range of about 10 to about 20 GPas, e.g., about 5 to about 9 GPas at room temperature) and low coefficient of thermal expansion ("CTE") (α1<20 ppm; α2<40 ppm).

[0023] The cured reaction product of the composition of the present invention can improve the warpage resistance of a molded substrate by about 50%, desirably at least about 65%, and even more desirably at least about 80%, as compared to a molded substrate having a material other than those disclosed herein. The substrate is often a wafer composed of silicon, and the composition is disposed on the wafer at a thickness that is less than about 50% of the thickness of the wafer, for example, less than about 33% of the thickness of the wafer.

[0024] That is, and importantly, the composition exhibits less than about 3 cm (e.g., less than about 2 cm) warpage after curing under liquid compression molding conditions. This combination of physical properties shows promise in overcoming some of the significant technical hurdles currently facing the semiconductor packaging industry, particularly liquid encapsulant substrate warpage. Through the use of the compositions of the present invention, warpage resistance is not only improved during curing, but also during subsequent processing such as LDS.

[0025] Thus, in one aspect, a thermosetting resin composition is provided, the reaction product of which includes a thermosetting resin matrix (such as an epoxy resin component), a filler comprising silica, a spinel crystal, and a curing component comprising a combination of (1) a clathrate comprising a tetrakisphenol compound and (2) a nitrogen-containing curing agent, such as imidazole and its derivatives.

[0026] In another aspect, a method for improving warpage resistance of a molded wafer is provided, the method comprising the steps of: Providing a wafer having one or more silicon chips disposed thereon; providing a thermosetting resin composition as described above in contact with a wafer; exposing the wafer and the thermosetting resin composition to conditions favorable for the thermosetting resin composition to flow around the wafer; and Thereafter, exposing the thermosetting resin composition to conditions favorable for curing the reaction product of the thermosetting resin composition.

[0027] Once cured, the reaction product of the composition is exposed to laser energy, thereby forming residues or fragments of spinel crystals located at or near the surface of the reaction product, which residues or fragments act as seeds for forming interconnects or circuits through plating.

[0028] Also provided herein is a method for fabricating molded, electrically interconnected semiconductor devices, the method comprising the steps of: providing a wafer; applying a thermosetting resin composition, as disclosed herein, that is in a flowable state at room temperature to at least a portion of a surface of the wafer; exposing the wafer and the thermosetting resin composition to elevated temperature conditions suitable to cure the composition to form a reaction product on the wafer; exposing the reaction product so formed to laser energy in a predetermined pattern to ablate the reaction product in the predetermined pattern, thereby exposing remnants of the spinel crystals; and Plating onto the cured reaction product in a predetermined pattern that has been ablated.

[0029] In some embodiments, the method may include the steps of: dispensing an additional portion of the thermosetting resin composition onto at least a portion of the surface of the cured thermosetting resin composition reaction product; exposing an additional portion of the thermosetting resin composition to elevated temperature conditions suitable to cure the composition to form a reaction product; exposing the reaction product so formed to laser energy in a predetermined pattern to ablate the reaction product in the predetermined pattern, thereby exposing remnants of the spinel crystals; and Plating onto the cured reaction product in a predetermined pattern that has been ablated.

[0030] This method may be repeated multiple times to build three-dimensionally shaped, electrically interconnected semiconductor devices according to a predetermined pattern.

[0031] Of course, molded, electrically interconnected semiconductor devices are also provided that include a wafer having disposed thereon and / or around it a thermosetting resin composition of the present invention that has been cured into a reaction product by exposure to high temperature conditions, exposed to laser energy in a predetermined pattern, and formed onto the metallization in the predetermined pattern through plating. [Brief description of the drawings]

[0032] [Figure 1] FIG. 1 shows a process flow diagram of a liquid compression molding encapsulation method for wafer level packaging applications. [Diagram 2] FIG. 2 shows a process flow diagram of the stencil printing encapsulation method for wafer level packaging applications. [Diagram 3] FIG. 3 shows a process flow diagram of the laser ablation and plating method of hardened material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] The thermosetting resin composition described above includes, among other components, a thermosetting resin matrix (such as an epoxy resin).

[0034] Examples of epoxy resins include epoxies made from bisphenol A, bisphenol F, bisphenol S, bisphenol E, biphenyl, or combinations thereof. Additionally, two or more different bisphenol epoxies (or hydrides thereof) within the same resin type (such as A, F, S, or E) may be used.

[0035] Commercially available examples of bisphenol epoxies suitable for use herein include bisphenol F epoxies (e.g., RE-404-S from Nippon Kayaku Co., Ltd., Epicron 830, 830S, 830A and 830W from Dainippon Ink and Chemicals, Inc., and RSL1738 and YL-983U from Resolution Corporation), bisphenol-A epoxies (e.g., YL-979 and 980 from Resolution Corporation).

[0036] The above bisphenol epoxies, commercially available from Dainippon Ink and Chemicals, Inc., are advertised as liquid undiluted epichlorohydrin-bisphenol F epoxies with lower viscosities than conventional epoxies based on bisphenol A epoxies, and have similar physical properties to liquid bisphenol A epoxies. The bisphenol F epoxies have lower viscosities than the bisphenol A epoxies, all else being the same between the two epoxies, resulting in lower viscosities and faster flowing underfill sealant materials. The EEWs of these four bisphenol F epoxies are 165-180. The viscosities at 25°C are 3,000-4,500 cps (except RE1801, which has a viscosity upper limit of 4,000 cps). The bisphenol A epoxies have EEWs (g / eq) of 180-195 and viscosities at 25°C of 100-250 cps.

[0037] The bisphenol epoxies available from Resolution, Inc. and discussed above are advertised as low chloride content liquid epoxies. RSL-1738 Bisphenol A Epoxy is reported to have a total chloride content of 500-700 ppm, while YL-983U has a total chloride content of 150-350 ppm.

[0038] Included among the epoxies suitable for use herein are polyglycidyl derivatives of phenolic compounds, such as those commercially available under the trade name EPON, such as EPON 828, EPON 1001, EPON 1009, and EPON 1031 from Resolution, Inc.; EPON trademarks such as DER 331, DER 332, DER 334, and DER 542 from The Dow Chemical Company; and BREN-S from Nippon Kayaku Co. Other suitable epoxies include polyepoxides prepared from polyols and the like, and polyglycidyl derivatives of phenol formaldehyde novolacs, such as DEN 431, DEN 438, and DEN 439 from The Dow Chemical Company. Cresol analogs are commercially available under the trade name Araldite, such as Araldite ECN 1235, Araldite ECN 1273, and Araldite ECN 1299 from Ciba Specialty Chemicals. SU-8 is a bisphenol A type epoxy novolac available from Resolution, Inc. Polyglycidyl adducts of amines, aminoalcohols and polycarboxylic acids are also useful in the present invention, commercially available resins include Glyamine 135, Glyamine 125, and Glyamine 115 from FIC Corporation; Araldite MY-720, Araldite 0500, and Araldite 0510 from Ciba Specialty Chemicals; and PGA-X and PGA-C from Sherwin-Williams.

[0039] In addition to bisphenol epoxies, other epoxy compounds may be included within the epoxy component. For example, cycloaliphatic epoxies such as 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarbonate, or hydrogenated versions of bisphenol or biphenyl epoxies may be used.

[0040] Also used are mono-, di- or polyfunctional reactive diluents to adjust viscosity and / or lower Tg, such as butyl glycidyl ether, cresyl glycidyl ether, polyethylene glycol glycidyl ether or polypropylene glycol glycidyl ether.Suitable monofunctional epoxy co-reactant diluents for use herein include those having a viscosity lower than that of the epoxy component, typically less than about 250 cps.

[0041] The monofunctional epoxy coreactant should have an epoxy group with an alkyl group having from about 6 to about 28 carbon atoms, examples of which include C 6~28 Alkyl glycidyl ether, C 6~28 Fatty acid glycidyl ester and C 10~28 Alkylphenol glycidyl ethers are included.

[0042] When such a monofunctional epoxy coreactant diluent is included, the coreactant diluent should be used in an amount of from about 5% to about 15% by weight, for example from about 8% to about 12% by weight, based on the total weight of the thermoset resin matrix.

[0043] The epoxy resin component should be present in the composition in an amount ranging from about 10% to about 95% by weight, desirably from about 20% to about 80% by weight, for example about 60% by weight, based on the total weight of the thermosetting resin matrix.

[0044] In addition to epoxy resins, other reactive components may be included, such as episulfide resins, oxazines, oxazolines, cyanate esters, and / or maleimide, nadimide or itaconimide containing components.

[0045] As the episulfide resin, any of these epoxies in which the oxirane oxygen atoms are replaced with sulfur atoms may be used.

[0046] The oxazine may be encompassed by the following structure:

[0047] [ka]

[0048] In the formula, R1 to R8 each independently represent hydrogen, C 1~40 Alkyl or C 2~40 alkenyl, the latter two of which are optionally interrupted by one or more of O, N, S, C=O, COO or NHC=O or replaced by one or more of OH, OR, NRR, SH, SR, COOH, COOR, NHCOOH or NHCOOR; R is C 1~40 Alkyl, C 2~40 Alkenyl, or C 6~20 aryl; X is a bond broadly selected from alkylene, alkenylene, or arylene, optionally interrupted by one or more of O, NR, S, C=O, COO, or NHC=O, or substituted by one or more of OH, OR, NRR, SH, SR, COOH, COOR, NHCOOH, or NHCOOR; R is C 1~40 Alkyl, C 2~40 Alkenyl, or C 6~20 aryl; m and n are each 1 or 2; k is 0 to 6.

[0049] If used, the oxazine should be present in the composition in an amount ranging from about 10% to about 95% by weight, desirably from about 20% to about 80% by weight, for example about 60% by weight, based on the total weight of the thermosetting resin matrix.

[0050] More specific examples of oxazines are benzoxazines, examples of which include the following:

[0051] [ka]

[0052] where o is 1 to 4, X is defined below, and R1 is alkyl, such as methyl, ethyl, propyl, or butyl; or

[0053] [ka]

[0054] In the formula, p is 1 to 4, Y is defined below, and R4 is selected from hydrogen, halogen, alkyl, or alkenyl.

[0055] X and Y in the above benzoxazine structures may be independently selected from monovalent or polyvalent groups, including: - a hydrocarbyl or substituted hydrocarbyl species typically having in the range of from about 6 to about 500 carbon atoms, where the hydrocarbyl species is selected from alkyl, alkenyl, alkynyl, cycloalkyl, cycloalkenyl, aryl, alkylaryl, arylalkyl, arylalkenyl, alkenylaryl, arylalkynyl, or alkynylaryl, with the proviso that X may be aryl only if X includes a combination of two or more different species; - a hydrocarbylene or substituted hydrocarbylene species typically having in the range of from about 6 to about 500 carbon atoms, where the hydrocarbylene species is selected from alkylene, alkenylene, alkynylene, cycloalkylene, cycloalkenylene, arylene, alkylarylene, arylalkylene, arylalkenylene, alkenylarylene, arylalkynylene, or alkynylarylene; -heterocyclic or substituted heterocyclic species typically having in the range of from about 6 to about 500 carbon atoms, -polysiloxanes, -polysiloxane-polyurethane block copolymers, and -One or more of the above and a covalent bond, -O-, -S-, -NR-, -NR-C(O)-, -NR-C(O)-O-, -NR-C(O)-NR-, -SC(O)-, -SC(O)-O -, -SC(O)-NR-, -OS(O)2-, -OS(O)2-O-, -OS(O)2-NR-, -OS(O)-, -OS(O)-O-, -OS(O)-NR-, -O-NR-C( O)-, -O-NR-C(O)-O-, -O-NR-C(O)-NR-, -NR-OC(O)-, -NR-OC(O)-O-, -NR-OC(O)-NR-, -O-NR-C(S)- , -O-NR-C(S)-O-, -O-NR-C(S)-NR-, -NR-OC(S)-, -NR-OC(S)-O-, -NR-OC(S)-NR-, -OC(S)-, -OC(S) -O-, -OC(S)-NR-, -NR-C(S)-, -NR-C(S)-O-, -NR-C(S)--NR-SS(O)2-, -SS(O)2-O-, -SS(O)2-NR-, - NR-OS(O)-, -NR-OS(O)-O-, -NR-OS(O)-NR-, -NR-OS(O)2-, -NR-OS(O)2-O-, -NR-OS(O)2-NR-, -O-N in combination with a linker selected from R-S(O)-, -O-NR-S(O)-O-, -O-NR-S(O)-NR-, -O-NR-S(O)2-O-, -O-NR-S(O)2-NR-, -O-NR-S(O)2-, -OP(O)R2-, -SP(O)R2-, or -NR-P(O)R2-; where each R is independently hydrogen, alkyl, or substituted alkyl.

[0056] As will be readily recognized by one of ordinary skill in the art, one or more of the above "X" or "Y" bonds, when combined to form the attachment of a benzoxazine group, can be any of a variety of groups, including, for example, oxyalkyl, thioalkyl, aminoalkyl, carboxylalkyl, oxyalkenyl, thioalkenyl, aminoalkenyl, carboxyalkenyl, oxyalkynyl, thioalkynyl, aminoalkynyl, carboxyalkynyl, oxycycloalkyl, thiocycloalkyl, aminocycloalkyl, carboxycycloalkyl, oxychloroalkenyl, thiocycloalkenyl, aminocycloalkenyl, carboxycycloalkenyl, heterocyclic, oxyheterocyclic, thioheterocyclic, aminoheterocyclic, carboxyheterocyclic, oxyaryl, thioaryl, aminoaryl, carboxyaryl, heteroaryl, oxyheterocyclic, aryl ... Heteroaryl, thioheteroaryl, aminoheteroaryl, carboxyheteroaryl, oxyalkylaryl, thioalkylaryl, aminoalkylaryl, carboxyalkylaryl, oxyarylalkyl, thioarylalkyl, aminoarylalkyl, carboxyarylalkyl, oxyarylalkenyl, thioarylalkenyl, aminoarylalkenyl, carboxyarylalkenyl, oxyalkenylaryl, thioalkenylaryl, aminoalkenylaryl, carboxyalkenylaryl, oxyarylalkynyl, thioarylalkynyl, aminoarylalkynyl, carboxyarylalkynyl, oxyalkynylaryl, thioalkynylaryl, aminoalkynylaryl or carboxyalkynylaryl.Oxyalkylene, thioalkylene, aminoalkylene, carboxyalkylene, oxyalkenylene, thioalkenylene, aminoalkenylene, carboxyalkenylene, oxyalkynylene, thioalkynylene, aminoalkynylene, carboxyalkynylene, oxycycloalkylene, thiocycloalkylene, aminocycloalkylene, carboxycycloalkylene, oxycycloalkenylene, thiocycloalkenylene, aminocycloalkenylene, carboxycycloalkenylene, oxyarylene, thioarylene, aminoarylene, carboxyarylene, oxyalkylarylene, thioalkylarylene, aminoalkylarylene, carboxyalkylarylene, oxyarylalkylene, thioarylalkylene, aminoarylalkylene, carboxyarylalkylene, oxyarylalkenylene, thioarylalkene A wide variety of organic chains can be produced, such as arylenes, aminoarylalkenylenes, carboxyarylalkenylenes, oxyalkenylarylenes, thioalkenylarylenes, aminoalkenylarylenes, carboxyalkenylarylenes, oxyarylalkynylenes, thioarylalkynylenes, aminoarylalkynylenes, carboxyarylalkynylenes, oxyalkynylarylenes, thioalkynylarylenes, aminoalkynylarylenes, carboxyalkynylarylenes, heteroarylenes, oxyheteroarylenes, thioheteroarylenes, aminoheteroarylenes, carboxyheteroarylenes, heteroatom-containing divalent or polyvalent cyclic moieties, oxyheteroatom-containing divalent or polyvalent cyclic moieties, thioheteroatom-containing divalent or polyvalent cyclic moieties, aminoheteroatom-containing divalent or polyvalent cyclic moieties, carboxyheteroatom-containing divalent or polyvalent cyclic moieties, etc.

[0057] The benzoxazine should be present in an amount ranging from about 10% to about 95% by weight, desirably from about 20% to about 80% by weight, for example about 60% by weight, based on the total weight of the thermoset resin matrix.

[0058] As cyanate esters, compounds having the following general structural formula may be used:

[0059] [ka]

[0060] In the formula, m is 2 to 5; R 1 is an aromatic nucleus-containing residue. 1 should contain at least six carbon atoms and may be derived from an aromatic hydrocarbon, such as, for example, benzene, biphenyl, naphthalene, anthracene, pyrene, etc. The aromatic residue may be derived from a polynuclear aromatic hydrocarbon in which at least two aromatic rings are linked together via a bridging group. For example, the bridging element may have the formula:

[0061] [ka]

[0062] In the formula, R a and R b R may be the same or different and represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1 R also includes residues derived from novolak-type phenolic resins, i.e., cyanate esters of these phenolic resins. 1 may further contain non-reactive substituents attached to the ring.

[0063] Examples of useful cyanate esters include, for example, 1,3-dicyanatobenzene; 1,4-dicyanatobenzene; 1,3,5-tricyanatobenzene; 1,3-, 1,4-, 1,6-, 1,8-, 2,6- or 2,7-dicyanatonaphthalene; 1,3,6-tricyanatonaphthalene; 4,4'-dicyanato-biphenyl; bis(4-cyanatophenyl)methane and 3,3',5,5'-tetramethyl, bis(4-cyanatophenyl)methane; 2,2-bis(3,5-dichloro-4-cyanatophenyl)propane; 2,2-bis(3,5-dichloro-4-cyanatophenyl)propane; bromo-4-dicyanatophenyl)propane; bis(4-cyanatophenyl)ether; bis(4-cyanatophenyl)sulfide; 2,2-bis(4-cyanatophenyl)propane; tris(4-cyanatophenyl)-phosphite; tris(4-cyanatophenyl)phosphate; bis(3-chloro-4-cyanatophenyl)methane; cyanated novolaks; 1,3-bis[4-cyanatophenyl-1-(methylethylidene)]benzene as well as cyanated bisphenol terminated polycarbonates or other thermoplastic oligomers.

[0064] Other cyanate esters include those disclosed in U.S. Pat. Nos. 4,477,629 and 4,528,366, the disclosures of each of which are expressly incorporated herein by reference; those cyanate esters disclosed in British Patent No. 1,305,702, and those cyanate esters disclosed in International Patent Publication No. WO 85 / 02184, the disclosures of each of which are expressly incorporated herein by reference.

[0065] Particularly preferred cyanate esters for use herein are commercially available from Huntsman Advanced Materials, Inc. (Tarrytown, NY) under the registered trademark Alloy [1,1-di(4-cyanatophenylethane)]. The structures of the four preferred Alloy cyanate esters are as follows:

[0066] [ka]

[0067] [ka]

[0068] [ka]

[0069] [ka]

[0070] If used, the cyanate ester should be present in an amount ranging from about 10% to about 95% by weight, desirably from about 20% to about 80% by weight, for example about 60% by weight, based on the total weight of the thermoset resin matrix.

[0071] As maleimides, nadimides, and itaconimides, compounds having the following general structural formula may be used:

[0072] [ka]

[0073] In the formula, m is 1 to 15, p is 0 to 15, and each R 2 are independently hydrogen or lower alkyl (e.g., C 1-5 ), where J is a mono- or polyvalent group including organic or organosiloxane radicals, and combinations of two or more thereof, for example, as defined as "X" and "Y" with respect to the benzoxazine structure above.

[0074] The monovalent or polyvalent groups include hydrocarbyl or substituted hydrocarbyl species, typically having carbon atoms in the range of about 6 to about 500. The hydrocarbyl species can be alkyl, alkenyl, alkynyl, cycloalkyl, cycloalkenyl, aryl, alkylaryl, arylalkyl, arylalkenyl, alkenylaryl, arylalkynyl, and alkynylaryl.

[0075] Additionally, X may be a hydrocarbylene or substituted hydrocarbylene species, typically having carbon atoms in the range of about 6 to about 500. Examples of hydrocarbylene species include, but are not limited to, alkylene, alkenylene, alkynylene, cycloalkylene, cycloalkenylene, arylene, alkylarylene, arylalkylene, arylalkenylene, alkenylarylene, arylalkynylene, and alkynylarylene.

[0076] The maleimide, itaconamide or nadamide may be in liquid or solid form.

[0077] In desirable embodiments, the maleimide, itaconamide or nadimide functional groups are separated by a polyvalent group having sufficient length and branching to render the maleimide-containing compound liquid. The maleimide, itaconamide or nadimide compound may contain a spacer between the maleimide functional groups that includes a branched alkylene between the maleimide, itaconamide or nadimide functional groups.

[0078] In the case of maleimide-containing compounds, the maleimide compound is desirably stearylmaleimide, oleylmaleimide, biphenylmaleimide, or 1,20-bismaleimide-10,11-dioctyl-eixoxane, or a combination of the above.

[0079] Again, in the case of maleimide-containing compounds, the maleimide compounds may be prepared by the reaction of maleic anhydride with a dimer amide, or may be prepared from aminopropyl-terminated polydimethylsiloxane, polyoxypropyleneamine, polytetramethyleneoxide-di-p-aminobenzoate, or combinations thereof.

[0080] Particularly preferred maleimides and nadimides include the following:

[0081] [ka]

[0082] In the formula, R 5 and R 6 are each selected from alkyl, aryl, aralkyl, or alkaryl groups having from about 6 to about 100 carbon atoms, with or without substitution or interruption with members selected from silane, silicon, oxygen, halogen, carbonyl, hydroxyl, ester, carboxylic acid, urea, urethane, carbamate, sulfur, sulfonate, and sulfone.

[0083] Other desirable maleimides, nadimides, and itaconimides include the following:

[0084] [ka]

[0085] [ka]

[0086] [ka]

[0087] [ka]

[0088]

change

[0089]

change

[0090]

change

[0091]

change

[0092]

change

[0093]

change

[0094]

change

[0095]

change

[0096]

change

[0097]

change

[0098]

change

[0099] [ka]

[0100] [ka]

[0101] [ka]

[0102] [ka]

[0103] [ka]

[0104] [ka]

[0105] The thermosetting resin matrix should be present in an amount ranging from about 10% to about 95% by weight, desirably from about 20% to about 80% by weight, for example about 60% by weight, based on the total weight of the thermosetting resin composition (excluding silica and spinel crystal fillers).

[0106] Silica as a filler can be useful to modify the CTE between the semiconductor chip and the substrate to which it is mated and encapsulated to more closely match or tune the respective CTEs. Because silica fillers affect the CTE, they can be used to reduce the thermal expansion of the cured material, thereby reducing warpage.

[0107] Silica fillers often include reinforcing silicas such as fused spherical silica, and may be untreated or may be treated to change their surface chemistry. The silica filler component should include particles having an average particle size distribution in the range of 0.1 to 75 microns, for example 0.1 to 50 microns. Commercial examples of such particles are sold by Tatsumori or Denka in Japan. Additionally, nano-sized silica powders may be added, such as those sold under the trade name Nanopox by Nanoresin, Germany. Nanopox fillers are monodisperse silica filler dispersions in epoxy resins at levels up to about 50% by weight, available from Nanoresin, Germany. Nanopox fillers are typically believed to have a particle size of about 5 nm to about 80 nm.

[0108] Nanoresin also manufactures materials under the trade name Nanopox E. For example, Nanoresin reports that Nanopox E branded products enable complete impregnation of electronic components that are otherwise difficult to encapsulate, and offer a wide range of mechanical and thermal properties, including reduced shrinkage and thermal expansion, fracture toughness and elastic modulus. The table below provides information on four notable Nanopox E products offered by Nanoresin.

[0109] [Table 1]

[0110] NanoResins reports that the use of Nanopox E brand products can significantly improve important properties of epoxy formulations, including: -Low formulation viscosity compared to traditional reinforcing fillers -No precipitation -Improved fracture toughness, impact resistance and elastic modulus -Improved scratch and abrasion resistance -Reduced shrinkage and thermal expansion Many desirable properties such as thermal stability, chemical resistance, glass transition temperature, weatherability, and dielectric properties are improved or at least not adversely affected.

[0111] Processability is essentially unchanged compared to the respective base resins.

[0112] According to the manufacturer, Nanopox E brand products are colloidal silica sols in an epoxy resin matrix. According to the manufacturer, the dispersed phase consists of surface-modified, spherical SiO2 nanoparticles with a diameter of less than 50 nm and a very narrow particle size distribution. These spheres are only a few nanometers in size and are dispersed without agglomeration in the resin matrix. This produces a dispersion with a very low viscosity and a SiO2 content of up to 40% by weight, according to the manufacturer. The manufacturer reports that the nanoparticles are chemically synthesized from an aqueous sodium silicate solution. In this process, the binder is not damaged, in contrast to processes in which powder fillers are dispersed in dissolvers or other equipment that uses high shear energy.

[0113] The silica filler should be present in an amount ranging from about 10% to about 95% by weight, desirably from about 20% to about 80% by weight, for example about 60% by weight, based on the total weight of the thermosetting resin composition.

[0114] The compositions of the present invention also include spinel crystals.

[0115] Spinel crystals may be formed from one or more metallic elements of the periodic table, such as cadmium, chromium, manganese, nickel, zinc, copper, cobalt, iron, magnesium, tin, gold, silver, and titanium.

[0116] More specifically, the spinel crystals are double oxides and may be metal oxides of the type found in AB2O4 type compounds or B(AB)O4 type compounds, where A and B are metal elements as described above, and preferably A is copper.

[0117] Spinel crystals are generally stable to high temperature conditions and can withstand acidic or alkaline conditions such as those found in aqueous metallization baths.

[0118] While the spinel crystals are substantially uniformly dispersed throughout the compositions of the present invention, some spinel crystals are disposed on or about the surface of the cured reaction product and, upon exposure to laser energy, may be laser ablated to form a predetermined pattern that can then be plated according to that pattern.

[0119] A particularly desirable spinel crystal is commercially available from Shepherd Color under the trade name LD-38 (described as a high performance copper chromite seed forming LDS additive, which Shepherd recommends using in amounts of 1-8% by weight).

[0120] Here, the spinel crystal may be used in the composition of the present invention in an amount of about 1 to about 15% by weight, for example, about 3 to about 12% by weight, based on the total weight of the thermosetting resin composition, but desirably, the spinel crystal should be used in the composition of the present invention in an amount of about 9 to about 10% by weight.

[0121] In this manner, the MID may be formed in a layer-by-layer process, as desired. More specifically, after an initial laser ablation, a new portion of the thermosetting resin composition may be placed thereon and exposed to elevated temperature conditions to form a hardened reaction product, and then that pattern or a different predetermined pattern may be exposed to laser energy ablation to expose a plateable surface. This process may be repeated as many times as desired, for example by an end user, to create a desired three-dimensional shaped interconnect device.

[0122] The MID has a three-dimensional circuit constructed on, within, or around a molded device formed with the thermosetting resin composition described herein. For example, a three-dimensional MID may include a molded article having a three-dimensional structure and a three-dimensional circuit formed on the surface of the molded article.

[0123] As mentioned above, MIDs may be made using LDS, which produces metal nuclei on or around the surface of spinel crystals or the cured reaction product of a thermosetting resin composition containing the LDS additive.

[0124] When exposed to the energy emitted by a laser, metal nuclei may form as seeds from the spinel crystals, and electroless plating may be used to form a predetermined plating pattern (e.g., a wire or circuit) in the areas exposed to the laser, followed by ablation according to that pattern.

[0125] The laser may be selected from lasers such as YAG lasers and excimer lasers, and electron beams, with YAG lasers being preferred. Furthermore, the wavelength of the laser energy may be selected, for example, in the range of 200 nm to 12,000 nm, and is preferably 248 nm, 308 nm, 355 nm, 532 nm, 1064 nm, 3,000 nm, or 10,600 nm.

[0126] For example, a 50 watt YAG laser may be used to activate the surface of the cured reaction product by emitting energy at about 355, 532, or 1064 nm.

[0127] Typically, the laser can be modulated using an acousto-optic modulator / splitter / attenuator arrangement to produce up to 23 watts in a single beam. The diameter of the laser beam can be 1, 2, 4, 6, 8, 10, 15, 18, 20 or 25 microns, with a focal length between any two numbers of typically 18 or 12 microns. Typical exposure doses (or energy doses (J / cm 2 )) may be between any two of the following values ​​0.1, 0.5, 1.0, 2, 4, 6, 8, 10, 15 or 20.

[0128] Plating may occur after exposure to the energy emitted by the laser through electroplating or electroless plating, and plating can be performed in the areas irradiated by the laser to form a plated circuit in those areas.

[0129] Plating typically uses a carrier liquid in which metal components, such as one or more of copper, nickel, gold, silver, and palladium, are dispersed (or sometimes dissolved). The metal components may be present in the form of a salt, chelate, or complex. The liquid to be carried may be any suitable liquid, such as water. For example, the carrier liquid may be aqueous, forming a solution of 3.0 g / L copper(II), 9.0 g / L caustic acid, and 4.0 g / L formaldehyde.

[0130] The plating process may be carried out at a temperature of 55° C. for approximately 60 minutes.

[0131] The hardening component must be latent.

[0132] The curing component may be a combination of (1) a clathrate (such as a tetrakisphenol compound) and (2) a nitrogen-containing compound.

[0133] Examples of such clathrates include 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3-methyl-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3,5-dimethyl-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3-chloro-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3,5-dichloro-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3-bromo-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3 ,5-dibromo-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3-t-butyl-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3,5-di-t-butyl-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3-fluoro-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3,5-difluoro-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3-methoxy-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3,5-dimethoxy-4-hydroxyphenyl)ethane 1,1,2,2-tetrakis(3-chloro-5-methyl-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3-bromo-5-methyl-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3-methoxy-5-methyl-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3-t-butyl-5-methyl-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3-chloro-5-bromo-4-hydroxyphenyl)ethane, 1,1,2,2-tetrakis(3-chloro-5-phenyl 1,1,2,2-tetrakis[(4-hydroxy-3-phenyl)phenyl]ethane, 1,1,3,3-tetrakis(4-hydroxyphenyl)propane, 1,1,3,3-tetrakis(3-methyl-4-hydroxyphenyl)propane, 1,1,3,3-tetrakis(3,5-dimethyl-4-hydroxyphenyl)propane, 1,1,3,3-tetrakis(3-chloro-4-hydroxyphenyl)propane, 1,1,3,3-tetrakis(3,5-dichloro-4-hydroxyphenyl)propane, 1,1,3,3-tetrakis(3-bromo-4-hydroxyphenyl)propane, 1,1,3,3-tetrakis(3,5-dibromo-4-hydroxyphenyl)propane, 1,1,3,3-tetrakis(3-phenyl-4-hydroxyphenyl)propane, 1,1,3,3-tetrakis(3,5-diphenyl-4-hydroxyphenyl)propane, 1,1,3,3-tetrakis(3-methoxy-4-hydroxyphenyl)propane, 1,1,3,3-tetrakis(3,5-dimethoxy-4-hydroxyphenyl)propane, 1,1,3,3-tetrakis(3-t-butyl-4-hydroxyphenyl)propane, 1,1,3,3-tetrakis(3,5-di-t-butyl-4-hydroxyphenyl)propane, 1,1,4,4-tetrakis(4-hydroxyphenyl)butane, 1,1,4,4-tetrakis(3-methyl-4-hydroxyphenyl)butane, Examples of tetrakisphenol compounds include 1,1,4,4-tetrakis(3,5-dimethyl-4-hydroxyphenyl)butane, 1,1,4,4-tetrakis(3-chloro-4-hydroxyphenyl)butane, 1,1,4,4-tetrakis(3,5-dichloro-4-hydroxyphenyl)butane, 1,1,4,4-tetrakis(3-methoxy-4-hydroxyphenyl)butane, 1,1,4,4-tetrakis(3,5-dimethoxy-4-hydroxyphenyl)butane, 1,1,4,4-tetrakis(3-bromo-4-hydroxyphenyl)butane, 1,1,4,4-tetrakis(3,5-dibromo-4-hydroxyphenyl)butane, 1,1,4,4-tetrakis(3-t-butyl-4-hydroxyphenyl)butane, 1,1,4,4-tetrakis(3,5-di-t-butyl-4-hydroxyphenyl)butane, and combinations thereof.

[0134] Nitrogen-containing compounds include amines, amides, and imidazoles, to name a few.

[0135] As the amine, for example, aliphatic amines, alicyclic and heterocyclic amines, aromatic amines, modified amines, etc. may be used.

[0136] As the aliphatic amine, some or all of ethylenediamine, trimethylenediamine, tetramethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetraamine, tetraethylenepentamine, dipropylenediamine, dimethylaminopropylamine, diethylaminopropylamine, trimethylhexamethylenediamine, pentanediamine, bis(2-dimethylaminoethyl)ether, pentamethyldiethylenetriamine, alkyl-t-monoamines, 1,4-diazabicyclo(2,2,2)octane (triethylenediamine), N,N,N',N'-tetramethylhexamethylenediamine, N,N,N',N'-tetramethylpropylenediamine, N,N,N',N'-tetramethylethylenediamine, N,N-dimethylcyclohexylamine, dimethylaminoethoxyethoxyethanol, dimethylaminohexanol, and combinations thereof may be used.

[0137] As alicyclic and heterocyclic amines, some or all of piperidine, piperidine, menthane diamine, isophorone diamine, methylmorpholine, ethylmorpholine, N,N′,N″-tris(dimethylaminopropyl)hexahydro-S-triazine, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxyspiro(5,5)undecane adduct, N-aminoethylpiperazine, trimethylaminoethylpiperazine, bis(4-aminocyclohexyl)methane, N,N′-dimethylpiperazine, 1,8-diazabicyclo(4,5,0)undecene-7, and combinations thereof may be used.

[0138] As aromatic amines, O-phenylenediamine, m-phenylenediamine, p-phenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, benzylmethylamine, dimethylbenzylamine, m-xylylenediamine, pyridine, picoline and combinations thereof may be used.

[0139] The modified polyamine may be an epoxy compound-added polyamine, a Michael reaction-added polyamine, a Mannich reaction-added polyamine, a thiourea-added polyamine, a ketone-blocked polyamine, or a combination thereof.

[0140] The imidazole may be any part or all of imidazole and its derivatives, such as isoimidazole, imidazole, and alkyl-substituted imidazoles, such as 2-methylimidazole, 2-ethyl-4-methylimidazole, 2,4-dimethylimidazole, butylimidazole, 2-heptadecenyl-4-methylimidazole, 2-methylimidazole, 2-undecenylimidazole, 1-vinyl-2-methylimidazole, 2-n-heptadecylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, and 2-phenylimidazole. , 2-ethyl 4-methylimidazole, 1-benzyl-2-methylimidazole, 1-propyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-guanaaminoethyl-2-methylimidazole, and addition products of imidazole, methylimidazole, and addition products of imidazole and trimellitic acid, 2-n-heptadecyl-4-methylimidazole, etc. (generally each aryl group) the alkyl substituent contains up to about 17 carbon atoms, desirably up to about 6 carbon atoms; aryl substituted imidazoles, such as phenylimidazole, benzylimidazole, 2-methyl-4,5-diphenylimidazole, 2,3,5-triphenylimidazole, 2-styrylimidazole, 1-(dodecylbenzyl)-2-methylimidazole, 2-(2-hydroxyl-4-t-butylphenyl)-4,5-diphenylimidazole, 2-(2-methoxyphenyl)-4,5-diphenylimidazole, 2-(3-hydroxyphenyl)-4, 5-diphenylimidazole, 2-(p-dimethylaminophenyl)-4,5-diphenylimidazole, 2-(2-hydroxyphenyl)-4,5-diphenylimidazole, di(4,5-diphenyl-2-imidazole)-benzene-1,4,2-naphthyl-4,5-diphenylimidazole, 1-benzyl-2-methylimidazole, 2-p-methoxystyrylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole (commercially available under the registered trademark 2PHZ from Shikoku, Tokyo, Japan) and combinations thereof may be used.

[0141] Commercially available examples of imidazoles include imidazole from Sigma-Aldrich, Curesol 1B2MZ (benzyl-2-methylimidazole) and Curesol 2P4MZ (2-phenyl-4-methylimidazole), each available from Air Products and Chemicals, and Arbor 9719-1 (2-ethyl-4-methylimidazole) from Huntsman Advanced Materials America.

[0142] Examples of the amide compound include polyamides obtained by polymerization of dimalic acid and polyamines, and examples of the ester compound include active carbonyl compounds such as aryl esters and thioaryl esters of carboxylic acids.

[0143] Other nitrogen-containing compounds that may be used include dicyandiamide, guanidine, organic acid hydrazides, diaminomaleonitrile, aminimides, trifluoroboron-piperidine complex, trifluoroboron-monoethylamine complex, and combinations thereof.

[0144] The ratio of clathrate to nitrogen-containing compound should be from about 2.5:1 to about 0.5:1 on a molar basis.

[0145] Commercially available curing components include those sold by Nippon Soda under the trade name Nisso Cure.

[0146] The curing component should be included in an amount of about 0.1% to about 20% by weight, for example about 2% to about 12% by weight, based on the total resin composition.

[0147] Various additives may be included, as illustrated in the examples below, but of particular note are dispersants, such as those available from BYK Chemie under the trade name Disuper BYK.

[0148] Also provided herein is a method for manufacturing a molded, electrically interconnected semiconductor device, the method including the steps of: providing a wafer; dispensing a thermosetting resin composition, as disclosed herein, that is in a flowable state at room temperature onto at least a portion of a surface of the wafer; exposing the wafer and the thermosetting resin composition to elevated temperature conditions suitable to cure the composition to form a reaction product on the wafer; exposing the reaction product so formed to laser energy in a predetermined pattern to ablate the reaction product in the predetermined pattern, thereby exposing remnants of the spinel crystals; and Plating onto the cured reaction product in a predetermined pattern that has been ablated.

[0149] In some embodiments, the method may include: dispensing an additional portion of the thermosetting resin composition onto at least a portion of the surface of the cured thermosetting resin composition reaction product; exposing an additional portion of the thermosetting resin composition to elevated temperature conditions suitable to cure the composition to form a reaction product; exposing the reaction product so formed to laser energy in a predetermined pattern to ablate the reaction product in the predetermined pattern, thereby exposing remnants of the spinel crystals; and Plating onto the cured reaction product in a predetermined pattern that has been ablated.

[0150] This method may be repeated multiple times to build up three-dimensionally shaped, electrically interconnected semiconductor devices according to a predetermined pattern.

[0151] Of course, molded, electrically interconnected semiconductor devices are also provided that include a wafer having disposed thereon and / or around it the thermosetting resin composition of the present invention that has been cured into a reaction product by exposure to high temperature conditions, exposed to laser energy in a predetermined pattern, and plated to form metallization on the predetermined pattern.

[0152] The following examples are provided for illustrative purposes only. EXAMPLES

[0153] Currently, reconstituted wafers are typically made to be 8 or 12 inch in diameter. In use, the thermosetting resin composition used to encapsulate the wafer may be dispensed by air pressure or by piston dispensing onto or around the central portion of the wafer. In addition to reconstituted wafers, the compositions of the present invention may also be molded onto blank wafers and trenched wafers.

[0154] This is followed by exposure to liquid compression molding conditions at a temperature of about 110° C. to 130° C. for about 120 to 420 seconds. See, e.g., FIG. 1. After such exposure, the compression molded wafer may be placed in a conventional oven for post-molding cure at a temperature of about 120° C. to less than about 150° C., e.g., about 120° C. to about 130° C., for about 15 minutes to 1 hour. Desirably, an 8 inch, 600 μm thick molded wafer should exhibit less than about 3 mm of warp in the transverse direction of the wafer.

[0155] In a typical stencil printing method, a liquid molding compound is applied onto a substrate at room temperature, on which a shim or stencil is used as a spacer. The liquid molding compound is spread onto the substrate surface with a metal squeegee to form a film layer. The thickness of the shim or stencil determines the thickness of the film layer formed on the substrate. See, for example, FIG. 2. After stencil printing, the stencil printed wafer may be placed in a conventional oven for post-molding cure at a temperature of about 120° C. to less than about 150° C., e.g., about 120° C. to about 130° C., for about 15 minutes to 1 hour. Desirably, an 8-inch, 600 μm thick molded wafer should exhibit less than about 3 mm of warpage across the wafer.

[0156] Control compositions (sample numbers 2 and 4) were prepared from additives including a thermosetting resin, silica filler, hardener, and colorant. Additionally, two other compositions (sample numbers 1 and 3) were prepared according to the present invention. The first two compositions were formulated for application as a printable encapsulant type liquid molding compound (see FIG. 2). The remaining two compositions were formulated for liquid compression molding applications (see FIG. 1). The viscosity stability of the compositions was evaluated and they were applied to a carrier with a silicon chip placed on it and molded as described above.

[0157] The bow of the molded wafer can be measured by a Nikon NEXIV scanning system, or by using shadow moire in X and Y directions, or by estimation with a ruler.

[0158] The warpage of the molded wafers was measured after molding and post-molding processes.

[0159] Referring to Table 1 below, there are shown control compositions (Sample Nos. 2 and 4) and compositions of the present invention (Sample Nos. 1 and 3) incorporating the indicated ingredients in the indicated amounts.

[0160] [Table 2]

[0161] Each composition was prepared by mixing the listed ingredients together using a mechanical mixer until dissolution into a homogenous solution was observed. The silica filler was then added with continuous mixing at room temperature for about 30 to about 60 minutes until a viscous paste having a substantially uniform consistency was obtained. The samples were then transferred to containers until ready for use.

[0162] The first two compositions were each dispensed onto and around the center of a silicon wafer as a carrier. After compression molding at a temperature of about 120° C. to less than about 130° C. for about 200 seconds to about 400 seconds, the compositions were observed to be about 60 to about 80% cured and the surface was non-tacky. The so-formed wafer was then placed in a conventional oven for post-molding curing at a temperature of about 120° C. to about 150° C. for about 15 minutes to about 1 hour.

[0163] In intended use, the compositions of the invention in LCM format may be dispensed onto the active side of a reconstituted wafer and molded under pressure (about 98 KN) at an elevated temperature of about 110° C. to about 130° C. for about 3 minutes to about 7 minutes. The molded wafer assembly may then be exposed to an elevated temperature of about 130° C. to about 150° C. for about 1 hour to about 2 hours. Desirably, with 200 μm of cured material, an 8 inch, 600 μm thick silicon wafer should exhibit less than about 3 cm of warpage after post-molding cure, desirably less than about 2 cm.

[0164] The molded wafer is peeled, coated with a redistribution layer, solder bumps are applied, and then diced into single semiconductor packages.

[0165] Table 2 below lists certain physical properties, including mechanical properties such as elastic modulus and CTE (α1 or 1, and α2 or 2), that were observed and measured after the samples were first exposed to compression molding conditions at temperatures of about 120° C. to less than about 130° C. for about 200 seconds to about 400 seconds, and then further exposed in an oven to temperatures of about 120° C. to about 150° C. for about 15 minutes to about 1 hour.

[0166] [Table 3]

[0167] As shown in Table 2, the liquid molding compound sealants containing the spinel crystal filler additive (samples Nos. 2 and 4) have similar physical properties as the control compositions (samples Nos. 1 and 3). Stated differently, the addition of the spinel crystal filler has little effect on the application processing conditions of the material, such as dispensing, printing, and coating onto a substrate, and surprisingly does not significantly affect the properties of the resulting cured reaction product. Thus, little, if any, compositional modification may be required for the end use applications herein.

[0168] "Standard Test Method for Linear Thermal Expansion of Solid Materials by Thermomechanical Analysis," ASTM International Designation: E831-06, published April 2006 ("E831-06"), describes a test method "for determining the apparent coefficient of thermal expansion of solid materials using thermomechanical analysis techniques." See paragraph 1.1 of E831-06. This general method was used to measure CTE α1 or 1.

[0169] "Standard Test Methods for Plastics: Dynamic Mechanical Properties: Flexure (Three-Point Bend)" ASTM International Designation: D5023-01, published November 2001 ("D5023-01") discloses a test method "intended to provide a means for determining the elastic modulus as a function of temperature for a variety of plastic materials." See paragraph 1.2 of D5023-01. This general method was used to measure the storage modulus.

[0170] To achieve high Tg and low warpage in flip chip semiconductor packages, low temperature cure conditions (below about 130°C) are necessary, and compositions that exhibit rapid gelation after exposure to such low temperature cure conditions have been shown to affect warpage. The Tg of the cured composition must be equal to or greater than the temperature used to cure the composition; the Tg should be equal to or greater than 90°C, and preferably equal to or greater than 125°C. If the composition cures slowly or at a higher temperature, the stress-free point between the mold and the substrate set is high.

[0171] To achieve reliable thermal cycling performance from -55°C to 125°C for such compression molded semiconductor packages, the liquid compression molding material should have a Tg of 90°C or higher, preferably 125°C or higher, by TMA after reflow at 260°C, and a delta temperature between onset and peak by DSC of 20°C or lower.

[0172] The compositions of the present invention achieve the following properties upon curing: a) The storage modulus at room temperature (25°C), measured by DMA (three-point bending method, 5°C / min), is in the range of 25GPas or less. b) CTEα1 measured by TMA (ramp rate 5°C / min) is 15 ppm / °C or less, and CTEα2 is 30 ppm or less. c) At least one Tg greater than or equal to 135°C as measured by TMA (3-point bending, ramp rate 5°C / min).

[0173] As shown in Figure 3, the hardened reaction product is laser activated by laser ablation, causing the spinel crystals to condense and become exposed at the surface, where they can be plated.

[0174] Table 3 below shows the data observed and collected on the plating performance of the LDS materials represented by Sample Nos. 1 and 3 compared to the Pocan Standard. Sample Nos. 1 and 3 were applied and cured on silicon wafer substrates as shown in Figures 2 and 1, respectively. Each of the cured Sample Nos. 1 and 2, as well as the Pocan Standard, were evaluated using the same laser ablation and plating process as shown in Figure 3. The Pocan Standard is a commercially available thermoplastic material containing a spinel crystal filler used as a standard.

[0175] [Table 4]

[0176] The Average Plating Index indicates the degree to which the laser ablated cured reaction product will plate compared to a commercially available thermoplastic LDS material used as a control. Generally, the higher the Average Plating Index value, the better the plateability.

Claims

1. Thermosetting resin matrix, Silica filler, Spinel crystals, and a curing component comprising a combination of clathrates comprising a combination of a tetrakisphenol compound and a nitrogen-containing curing agent; A thermosetting resin composition that is in a flowable state at room temperature, comprising:

1. A thermosetting resin composition, when disposed on at least a portion of a substrate and cured to a non-flowable state on or around a portion of said substrate after exposure to elevated temperature conditions, wherein said cured composition is plateable upon exposure to laser energy, and wherein said substrate on or around which said cured composition is disposed exhibits a warpage of less than about 3 cm.

2. Upon curing, it has the following physical properties: (a) a storage modulus in the range of about 25 GPa or less at room temperature; (b) a CTEα1 of 20 ppm / ° C. or less; (c) a CTE α2 of 40 ppm / ° C. or less; The composition of claim 1 having at least one of the following:

3. 10. The composition of claim 1, wherein the substrate is a wafer composed of silicon and the composition is disposed on or around the wafer at a thickness that is less than about 50% of a thickness of the wafer.

4. 10. The composition of claim 1, wherein the spinel crystals are formed from a metal selected from one or more of cadmium, chromium, manganese, nickel, zinc, copper, cobalt, iron, magnesium, tin, gold, silver, and titanium.

5. A method for improving warpage resistance of an encapsulated molded wafer, comprising the steps of: providing a wafer; providing the thermosetting resin composition of claim 1 in contact with the wafer; and and exposing the wafer and the thermosetting resin composition to conditions favorable for the thermosetting resin composition to flow around the wafer and cure to form a reaction product of the thermosetting resin composition, which can improve warpage resistance by about 50% or more.

6. 6. The method of claim 5, wherein warp resistance is improved by about 65% or more.

7. 6. The method of claim 5, wherein warp resistance is improved by about 80% or more.

8. 6. An article formed by the method of claim 5.

9. 2. The composition of claim 1, wherein the thermosetting resin component comprises an epoxy resin, an episulfide resin, an oxazine, an oxazoline, a cyanate ester, and / or a maleimide, nadimide, or itaconimide containing component.

10. A. Providing a substrate; B. A step of applying the thermosetting resin composition according to claim 1, which is in a flowable state at room temperature, to at least a portion of the surface of the substrate; C. exposing the substrate and the thermosetting resin composition to elevated temperature conditions suitable to cure the composition to form a reaction product on the substrate; D. exposing the reaction product so formed to laser energy in a predetermined pattern to ablate said reaction product in the predetermined pattern, thereby exposing remnants of the spinel crystals; and E. plating onto the ablated predetermined pattern in the hardened reaction product; 1. A method for manufacturing molded electrically interconnected semiconductor devices, comprising:

11. F. applying an additional portion of said thermosetting resin composition onto at least a portion of the surface of the cured thermosetting resin composition reaction product from step C; G. exposing an additional portion of said thermosetting resin composition to elevated temperature conditions suitable to cure said composition to form a reaction product; H. exposing the reaction product so formed to laser energy in a predetermined pattern to ablate said reaction product in the predetermined pattern, thereby exposing remnants of the spinel crystals; and I. plating onto the ablated predetermined pattern in the cured reaction product; The method of claim 10 further comprising:

12. The method of claim 10, further comprising repeating steps F through I.

13. 11. An electrically interconnected semiconductor device three-dimensionally formed by the method of claim 10.

14. A substrate; a thermosetting resin composition that is cured into a reaction product by exposure to elevated temperature conditions and exposed to laser energy in a predetermined pattern to form metallization on the predetermined pattern by plating disposed on or around the substrate; 1. A molded, electrically interconnected semiconductor device comprising:

Citation Information

Patent Citations

  • Epoxy resin composition for sealing semiconductor and semiconductor device

    JP2010195998A

  • Curing agent for thermosetting epoxy resins and method for producing insulating systems for electrical engineering

    JP2018517018A

  • Semiconductor device and method for manufacturing the same

    JP2021150344A

  • Thermosetting resin composition for LDS, resin molded article and three-dimensional molded circuit component

    WO2017199639A1

  • Liquid compression molding or encapsulant compositions

    WO2020037199A1