Solid electrolyte and all-solid-state battery containing the same

A solid electrolyte composed of Li, Si, B, and Zr, with a specific amorphous structure, addresses the conductivity and thermal stability issues in all-solid-state batteries, facilitating the production of high-performance microchip-type batteries.

JP2024542333APending Publication Date: 2024-11-15SAMSUNG ELECTRO MECHANICS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023554917
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-14
Filing Date
2022-12-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Rechargeable lithium batteries face issues with lower ionic conductivity and interfacial resistance in solid electrolytes, leading to challenges in industrial mass production and thermal stability, particularly in microchip-type all-solid-state batteries.

Method used

Development of a solid electrolyte composed of Li, Si, B, and Zr, with specific mole fractions, forming an amorphous structure based on a -B-O-Si-O-P-O-Zr- network, enhancing ionic conductivity and reducing thermal expansion, and optionally incorporating additional components like Li, Al, or Cl to further improve conductivity.

Benefits of technology

The proposed solid electrolyte achieves high ionic conductivity, low interfacial resistance, and suppressed thermal expansion, enabling the manufacturing of multilayer microchip-type all-solid-state batteries with improved performance and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542333000001_ABST
    Figure 2024542333000001_ABST
Patent Text Reader

Abstract

The present disclosure relates to a solid electrolyte and an all-solid-state battery including the same. Specifically, a solid electrolyte (first solid electrolyte) and a solid electrolyte (second solid electrolyte) are provided that include an oxide of a specific component system as a first component and further include an oxide or salt of another component system as a second component.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a solid electrolyte and an all-solid-state battery including the same. [Background technology]

[0002] Rechargeable lithium batteries are widely used as power sources for powering small electronic devices such as mobile phones, laptops, smartphones, etc., and are finding further application as power sources for powering electric vehicles and for storing power for energy storage devices, etc.

[0003] The most common type of rechargeable lithium battery is the lithium-ion battery, which uses a liquid electrolyte and therefore has problems (eg, potential hazards such as leakage, fire, explosion, etc.).

[0004] In recent years, "all-solid-state batteries" that replace liquid electrolytes with solid electrolytes have been attracting attention as a next-generation battery that solves the problems of lithium-ion batteries. However, solid electrolytes have lower ionic conductivity than liquid electrolytes, and therefore have a problem of interface resistance to ion migration between electrodes and electrolytes. Therefore, for industrial mass production of all-solid-state batteries, it is necessary to reduce the ionic conductivity of solid electrolytes and the interface resistance to ion migration between electrodes and electrolytes.

[0005] On the other hand, when the all-solid-state battery is manufactured to have a microchip shape, the all-solid-state battery basically has battery properties and can be used with IT components such as MLCCs, power inductor components, etc., based on its size and shape. In the microchip-type all-solid-state battery, it is advantageous to use an oxide-based solid electrolyte rather than a sulfide-based solid electrolyte or a polymer-based solid electrolyte from the viewpoints of environmental conservation, product performance, and mass production. However, the commonly known oxide-based solid electrolyte has an amorphous glass structure, and therefore may thermally expand or be easily destroyed during the co-firing process for manufacturing the microchip-type all-solid-state battery. [Disclosure] [Technical issues]

[0006] One embodiment provides an oxide of a specific component system as a solid electrolyte (first solid electrolyte) that can increase ionic conductivity, reduce interfacial resistance between the electrode and the electrolyte, suppress thermal expansion, and increase strength.

[0007] Another embodiment provides a solid electrolyte (second solid electrolyte) having further improved ionic conductivity by simultaneously further including an oxide of a specific component system as a first component and an oxide or salt of another component system as a second component.

[0008] Another embodiment provides an all-solid-state battery including a solid electrolyte, the solid electrolyte being any one of the solid electrolytes according to the first embodiment and the solid electrolyte according to the second embodiment. [Technical solution]

[0009] One embodiment provides a first solid electrolyte.

[0010] The first solid electrolyte may be an oxide containing Li, Si, B, Zr, and P.

[0011] Based on 100 mol% of the total amount of 2Li, Si, 2B, Zr, and 2P, in the first solid electrolyte, 2Li may be contained in an amount greater than or equal to about 40 mol% and less than or equal to about 80 mol%, Si may be contained in an amount greater than about 0 mol% and less than or equal to about 30 mol%, 2B may be contained in an amount greater than about 0 mol% and less than or equal to about 60 mol%, Zr may be contained in an amount greater than about 0 mol% and less than or equal to about 50 mol%, and 2P may be contained in an amount greater than about 0 mol% and less than or equal to about 60 mol%.

[0012] The molar fraction of 2Li / (Si + 2B + Zr) in the first solid electrolyte can be from about 0.5 to about 5.

[0013] The first solid electrolyte can be represented by Chemical Formula 1. [Chemical Formula 1] a(Li2O)·b(SiO2)·c(B2O3)·d(P2O5)·e(ZrO2) Here, in Chemical Formula 1, a to e are real numbers representing molar fractions, and 40 ≦ a ≦ 60, 0 < b ≦ 30, 0 < c ≦ 60, 0 < d ≦ 60, and 0 < e ≦ 50.

[0014] a, b, c, d, and e may satisfy a + b + c + d + e = 100.

[0015] The softening point of the first solid electrolyte may be higher than or equal to about 500 °C and lower than or equal to about 550 °C.

[0016] The first solid electrolyte may be a glass or a glass ceramic.

[0017] The first solid electrolyte may be a glass ceramic, and a crystal phase attributable to Li3PO4 may appear in X-ray diffraction (XRD) analysis using Cu-Kα. Specifically, a Li3PO4 crystal phase having a size greater than or equal to about 1 nm and less than or equal to about 10 nm may be present in the amorphous structure.

[0018] The first solid electrolyte may have an ionic conductivity higher than or equal to about 1.0×10 -8 S / cm.

[0019] Another embodiment provides a second solid electrolyte.

[0020] The second solid electrolyte may include an oxide containing Li, Si, B, Zr, and P; as a second component, it may further include an oxide or salt containing at least one element among Li, Al, Na, Mg, K, Ca, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Se, Rb, S, Y, Nb, Mo, Ag, In, Sn, Sb, Cs, Ba, Hf, Ta, W, Pb, Bi, Au, La, Nd, Eu, I, Cl, Br, or F.

[0021] The molar fraction of 2Li / (Si + 2B + Zr) in the second solid electrolyte can be from about 0.5 to about 5.

[0022] The second solid electrolyte may be represented by Chemical Formula 2. [Chemical Formula 2] a(Li2O)·b(SiO2)·c(B2O3)·d(P2O5)·e(ZrO2)·f(X m Y n ) Here, in Chemical Formula 2, a to f are real numbers representing molar fractions, 40 ≦ a ≦ 60, 0 < b ≦ 30, 0 < c ≦ 60, 0 < d ≦ 60, 0 < e ≦ 50, 0 ≦ f ≦ 50; X is Li, Al, or a combination thereof; Y is Cl, O, or a combination thereof; 0 < m ≦ 5 and 0 < n ≦ 5.

[0023] a, b, c, d, e, and f may satisfy a+b+c+d+e+f=100.

[0024] The softening point of the second solid electrolyte may be greater than or equal to about 500°C and less than or equal to about 550°C.

[0025] The second solid electrolyte may be a glass or a glass-ceramic.

[0026] The second solid electrolyte may be a glass ceramic in which a peak due to Li3PO4 appears in X-ray diffraction (XRD) analysis using Cu-Kα, and specifically, a Li3PO4 crystalline phase having a size greater than or equal to about 1 nm and less than or equal to about 10 nm may be present in an amorphous structure. Optionally, the second solid electrolyte may be a glass ceramic in which a peak due to Li3PO4 appears in X-ray diffraction (XRD) analysis using Cu-Kα, and specifically, a Li3PO4 crystalline phase having a size greater than or equal to about 1 nm and less than or equal to about 10 nm may be present in an amorphous structure. 12 Peaks due to Cl or Al2O3 may further be exhibited.

[0027] The second solid electrolyte is about 1.0×10 -7 The material may have an ionic conductivity greater than or equal to 1.0 S / cm.

[0028] The solid electrolyte may comprise an amorphous structure based on a -BO-Si-OPO-Zr- network.

[0029] The solid electrolyte may further include a Li3PO4 crystalline phase.

[0030] The Li3PO4 crystalline phase may have a size greater than or equal to about 1 nm and less than or equal to about 10 nm.

[0031] The solid electrolyte is Li4B7O 12 It may further include a Cl crystalline phase or an Al2O3 crystalline phase.

[0032] Another embodiment provides an all-solid-state battery comprising: a body including a solid electrolyte layer, and a positive electrode layer and a negative electrode layer stacked alternately with the solid electrolyte layer disposed therebetween; and a first external electrode and a second external electrode disposed on either side of the body, respectively, wherein the solid electrolyte layer includes one of a first solid electrolyte and a second solid electrolyte.

[0033] The positive electrode layer and the negative electrode layer may each independently include a current collecting layer and an electrode active material layer on the current collecting layer; the current collecting layer and the electrode active material layer each independently include one of a first solid electrolyte and a second solid electrolyte, and a carbon-based conductive material; and the electrode active material layer may further include an electrode active material. [Advantageous Effects of the Invention]

[0034] The first solid electrolyte has high ionic conductivity, low interfacial resistance between the electrodes and the electrolyte, suppressed thermal expansion and strong strength, so that multi-layer microchip-type all-solid-state batteries can be fabricated through a co-firing process.

[0035] Furthermore, the second solid electrolyte has a higher ionic conductivity compared to the first solid electrolyte, and therefore the performance of the microchip-type all-solid-state battery can be further improved. [Brief description of the drawings]

[0036] [Figure 1] 1 shows the bonding relationship between elements constituting a solid electrolyte according to an embodiment ((a): first solid electrolyte, (b): second solid electrolyte).

[0037] [Diagram 2] FIG. 1 is a cross-sectional schematic diagram of an all-solid-state battery according to an embodiment.

[0038] [Diagram 3] 3 shows the results of thermomechanical analysis (TMA) for the solid electrolyte according to Example 1.

[0039] [Figure 4]1 shows the results of thermomechanical analysis (TMA) for the solid electrolyte according to Example 8.

[0040] [Diagram 5] 1 shows scanning electron microscope (SEM) images of the solid electrolytes according to two examples 1 and 8 (left: example 1, right: example 8, scale bar is 1 μm).

[0041] [Figure 6] 1 shows the results of X-ray diffraction (XRD, Bruker AXS D4-Endeavor XRD) analysis using Cu-Kα for the solid electrolyte of Example 1.

[0042] [Figure 7] 1 shows the results of X-ray diffraction (XRD, Bruker AXS D4-Endeavor XRD) analysis using Cu-Kα for the solid electrolyte of Example 5.

[0043] [Figure 8] 1 shows the results of X-ray diffraction (XRD, Bruker AXS D4-Endeavor XRD) analysis using Cu-Kα for the solid electrolyte of Example 6.

[0044] [Figure 9] 1 shows the results of X-ray diffraction (XRD, Bruker AXS D4-Endeavor XRD) analysis using Cu-Kα for the solid electrolyte according to Example 7 of the present invention.

[0045] [Figure 10] 1 shows the results of X-ray diffraction (XRD, Bruker AXS D4-Endeavor XRD) analysis using Cu-Kα for the solid electrolyte according to Example 8 of the present invention.

[0046] [Figure 11] 1 shows an image (right magnified view) of a local area of ​​the solid electrolyte according to Example 1 obtained using a TEM device.

[0047] [Figure 12] 1 shows an image of a localized area of ​​the solid electrolyte according to Example 8 using a TEM device.

[0048] [Figure 13] 4 shows the results of resistance measurements for the solid electrolytes of Examples 1 and 8, respectively.

[0049] [Figure 14] 1 shows the electrochemical evaluation results for the all-solid-state battery cell according to Example 1. [Embodiments of the present invention]

[0050] The present disclosure will be described more fully below with reference to the attached drawings, in which embodiments of the present invention are shown. The drawings and descriptions are to be regarded as illustrative in nature, and not limiting. Similar reference numerals refer to similar elements throughout the specification. Furthermore, the attached drawings are provided only to facilitate understanding of the embodiments disclosed herein, and are not to be construed as limiting the spirit disclosed herein, and it is understood that the present invention includes all modifications, equivalents, and substitutions without departing from the scope and spirit of the present invention. Furthermore, some components in the attached drawings are exaggerated, omitted, or shown in a schematic manner, and the size of each component does not completely reflect the actual size.

[0051] Terms including ordinal numbers such as first, second, etc. are used only to describe various components and are not to be construed as limiting these components. These terms are used only to distinguish one component from another.

[0052] When an element is referred to as being "connected" or "coupled" to another element, it is understood that it may be directly connected or coupled to the other element, or it may be connected or coupled to the other element through additional intervening elements. In contrast, when an element is described as being "directly connected" or "directly coupled" to another element, it should be understood that there are no elements present between the element and the other element.

[0053] It should be understood that throughout this specification, the terms "including," "comprising," "having," or "comprising" indicate the presence of features, numbers, steps, operations, components, parts, or combinations thereof described herein, but without precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations. Unless expressly stated otherwise, the word "comprise" and variations such as "comprises" or "comprising" are understood to imply the inclusion of the stated elements rather than the exclusion of any other elements.

[0054] Throughout this specification, "solid electrolyte" refers to a material that is capable of conducting electric current through the movement of ions in the solid state.

[0055] Throughout this specification, "glass" generally refers to a highly transparent material that is not crystallized but is formed by melting a mixture of silica sand, soda ash, carbonate lime, etc. at high temperatures and solidifying it during the cooling process. To distinguish this from "glass ceramics" described later, we may refer to this material as "amorphous glass."

[0056] Throughout this specification, a "glass-ceramic" is a homogeneous collection of microcrystals obtained by heat treating a glass shaped body at or above its transition temperature and at or below its softening temperature, and is referred to as a "glass-ceramic."

[0057] "Glass-ceramics" have an amorphous phase and at least one crystalline phase, and therefore have both amorphous and crystalline properties. Specifically, "glass-ceramics" have high strength, stability, chemical resistance at high temperatures, ionic conductivity, and reduced thermal expansion compared to amorphous glasses.

[0058] Throughout this specification, "ionic conductivity" is a measure of a material's tendency to conduct ions, which theoretically increases proportionally to the concentration of ions, the amount of charge, and the mobility of the charge.

[0059] Various embodiments will now be described in detail with reference to the drawings.

[0060] (First solid electrolyte) One embodiment provides a solid that is a glass or glass-ceramic comprising Li, Si, B, Zr, and P.

[0061] The first solid electrolyte has high ionic conductivity, low interfacial resistance between the electrode and the electrolyte, suppressed thermal expansion and strong strength compared to oxide solid electrolytes containing Li, Si, B, and P but not containing Zr, and therefore can be well fabricated into a multi-layer microchip-type all-solid-state battery through a co-firing process.

[0062] The elements constituting the first solid electrolyte are described as follows.

[0063] Li, Si, and B are essential constituent elements of commonly known amorphous glasses for solid electrolytes, and also form an amorphous structure in the first solid electrolyte.

[0064] Specifically, in the first solid electrolyte, based on 100 mol% of the total amount of 2Li, Si, 2B, Zr, and 2P, 2Li may be contained in an amount greater than or equal to about 40 mol%, less than or equal to about 80 mol%, greater than or equal to about 40 mol%, less than or equal to about 70 mol%, or greater than or equal to about 40 mol% and less than or equal to about 60 mol%. Si may be contained in an amount greater than or equal to about 0 mol%, less than or equal to about 30 mol%, greater than or equal to about 3 mol%, less than or equal to about 20 mol%, or greater than or equal to about 5 mol%, and less than or equal to about 15 mol%. 2B may be included in an amount greater than about 0 mol%, less than or equal to about 60 mol%, greater than or equal to about 5 mol%, less than or equal to about 40 mol%, or greater than or equal to about 10 mol%, less than or equal to about 20 mol%. The meaning of the term "about" may include processing errors, measurement errors, etc. that occur during the manufacturing process that are recognizable to those of ordinary skill in the art. For example, "about X" may mean exactly "X" when "X" is a number, or may include an acceptable deviation from "X" due to processing errors, measurement errors, etc. that occur during the manufacturing process that are recognizable to those of ordinary skill in the art.

[0065] Meanwhile, Zr and P can form an amorphous structure having a specific structure together with Li, Si, and B. Specifically, FIG. 1(a) shows the bonding relationship between the elements constituting the first solid electrolyte. As shown in FIG. 1(a), in the first solid electrolyte, Li, Si, B, Zr, and P provide an amorphous structure based on a -BO-Si-OPO-Zr- network that forms vacancies in a non-bridged oxide (NBO) structure, and therefore properties such as high ionic conductivity, low thermal expansion, and high strength can be realized.

[0066] In contrast, an oxide solid electrolyte containing Li, Si, B, and P but not Zr may form an amorphous structure based on a -BO-Si-OPO- network, which forms an unstable structure with fewer vacancies in the non-bridged oxide (NBO) structure, unlike the amorphous structure based on a -BO-Si-OPO-Zr- network. Therefore, the properties such as ionic conductivity, thermal expansion, and strength may be inferior to those of the first solid electrolyte.

[0067] Specifically, Zr may be present in an amount greater than about 0 mol%, less than or equal to about 50 mol%, greater than or equal to about 1 mol%, less than or equal to about 20 mol%, or greater than or equal to about 1 mol% and less than or equal to about 10 mol%. 2P may be present in an amount greater than about 0 mol%, less than or equal to about 60 mol%, greater than or equal to about 1 mol%, less than or equal to about 20 mol%, or greater than or equal to about 5 mol% and less than or equal to about 15 mol%.

[0068] For reference, the molar content of each element based on 100 mol% of the total amount of 2Li, Si, 2B, Zr, and 2P in the first solid electrolyte can be confirmed through ICP analysis.

[0069] The molar fraction of 2Li / (Si+2B+Zr) in the first solid electrolyte can be from about 0.5 to about 5.

[0070] This is a relational expression of the molar contents of the main elements constituting the first solid electrolyte. As mentioned above, Li, Si, and B are essential elements generally known for amorphous glass, and Zr is an element that contributes to the formation of the amorphous structure of a specific network structure of the first solid electrolyte. When these satisfy the above relational expression, an amorphous structure based on the -BO-Si-OPO-Zr- network, and as a result, vacancies in the non-bridged oxide (NBO) structure can be effectively formed.

[0071] For example, the molar fraction of 2Li / (Si + 2B + Zr) in the first solid electrolyte may be more than or equal to about 0.5, more than or equal to about 1, or more than or equal to about 1.5, and less than or equal to about 5, less than or equal to about 4, less than or equal to about 3, or less than or equal to about 2.

[0072] For reference, the molar fraction of 2Li / (Si + 2B + Zr) in the first solid electrolyte can be calculated from the molar content of each element based on 100 mol% of the total amount of 2Li, Si, 2B, Zr, and 2P in the first solid electrolyte.

[0073] The first solid electrolyte may be represented by Chemical Formula 1. [Chemical Formula 1] a(Li2O)·b(SiO2)·c(B2O3)·d(P2O5)·e(ZrO2) Here, in Chemical Formula 1, a to e are real numbers representing molar fractions, where 40 ≤ a ≤ 80, 40 ≤ a ≤ 0, or 40 ≤ a ≤ 60; 0 < b ≤ 30, 3 ≤ b ≤ 20, or 5 ≤ b ≤ 15; 0 < c ≤ 60, 5 ≤ c ≤ 40, or 10 ≤ c ≤ 20; 0 < d ≤ 60, 1 ≤ d ≤ 20, or 1 ≤ d ≤ 15; and 0 < e ≤ 50, 1 ≤ e ≤ 20, or 1 ≤ e ≤ 10.

[0074] These explanations are the same as the explanations of the molar content of each element based on 100 mol% of the total amount of 2Li, Si, 2B, Zr, and 2P in the first solid electrolyte.

[0075] The first solid electrolyte can soften within a specific temperature range based on its amorphous characteristics.

[0076] The softening point of the first solid electrolyte may be higher than or equal to about 500 °C, higher than or equal to about 505 °C, or higher than or equal to about 510 °C, and lower than or equal to about 550 °C, lower than or equal to about 540 °C, or lower than or equal to about 530 °C.

[0077] For reference, the softening point of the first solid electrolyte can be confirmed through TMA thermal analysis.

[0078] The first solid electrolyte may be a glass or a glass-ceramic.

[0079] As defined above, a "glass" is an amorphous material, and a "glass-ceramic" is a material that contains one or more crystalline phases within an amorphous structure.

[0080] In particular, when the first solid electrolyte is a glass ceramic, compared with the case of amorphous glass, the ion conductivity is high, the interfacial resistance between the electrode and the electrolyte is low, the thermal expansion is suppressed, and the strength is high, and therefore it is advantageous for manufacturing a multi-layer microchip-type all-solid-state battery through a co-firing process.

[0081] Specifically, when the first solid electrolyte is a glass ceramic, a peak due to Li3PO4 may appear in the 2θ range of about 22° to about 25° in an X-ray diffraction (XRD) analysis using Cu-Kα. Here, the amorphous structure is presumed to include a -BO-Si-OPO-Zr-network, and the amorphous structure based on the -BO-Si-OPO-Zr-network may have vacancies in the non-bridging oxide (NBO) structure.

[0082] Furthermore, when the first solid electrolyte is a glass ceramic, crystalline phases having a size greater than or equal to about 1 nm, or greater than or equal to about 3 nm, less than or equal to about 10 nm, or less than or equal to about 5 nm can be identified in the amorphous structure through analysis such as FE-SEM, TEM, etc.

[0083] In short, when the first solid electrolyte is a glass ceramic, in an amorphous structure including a -BO-Si-OPO-Zr- network, there may be a Li3PO4 crystalline phase having a size greater than or equal to about 1 nm, or greater than or equal to about 3 nm, or less than or equal to about 10 nm, or less than or equal to about 5 nm.

[0084] The first solid electrolyte has a capacitance of about 1.0×10 -8 The solid electrolyte layer may have an ionic conductivity of greater than or equal to 1000 S / cm. This can be done by applying InGa paste, Ag paste, etc. to both sides of the solid electrolyte layer with the first solid electrolyte in between; or by sputtering Au, Pt, Ag, etc. to form metal electrodes, fabricate all-solid-state battery samples, place them on a jig, and measure 1000 mV at a reference frequency of 1000 mV. -6 This is obtained by measuring the EIS voltage in the 50 Hz range.

[0085] The method for producing the first solid electrolyte is not particularly limited, and may follow any generally known method for producing an oxide-based solid electrolyte.

[0086] As commonly known methods for producing oxide-based solid electrolytes, various glass production methods can be employed, such as conventional melt-quenching method, press melt-quenching method, and twin-roller melt-quenching method. The crucibles in the device were manufactured using alumina, high density alumina, platinum coating, or iridium coating.

[0087] The above-mentioned raw materials are mixed according to the stoichiometric molar ratio of the target composition, then heat-treated in the range of about 450°C to about 700°C to fully volatilize the ammonia in the mixed raw materials, and then maintained at about 1200°C for about 2 hours to carry out the vitrification process. The vitrified molten solution is cooled at about 500°C to about 700°C and recovered as cullet-type bulk material. The cullet is powdered and dried without secondary particles (aggregates) in anhydrous ethanol through a constant grinding process, and then classified to obtain glass ceramics in the form of particles with an average particle size (D50) of about 1.5 to about 3.0 μm.

[0088] (Second solid electrolyte) Another embodiment provides a second solid electrolyte comprising an oxide comprising Li, Si, B, Zr, and P; and further comprising as a second component an oxide or salt comprising at least one of the following elements: Li, Al, Na, Mg, K, Ca, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Se, Rb, S, Y, Nb, Mo, Ag, In, Sn, Sb, Cs, Ba, Hf, Ta, W, Pb, Bi, Au, La, Nd, Eu, I, Cl, Br, or F.

[0089] The second solid electrolyte further contains a specific element or atomic group compared to the first solid electrolyte, and therefore can achieve much higher ionic conductivity, greatly improving the performance of the microchip-type all-solid-state battery. 1(b) shows the bonding relationship between the elements constituting the second solid electrolyte. In this specification, the case where Li and Cl are contained as the second component is exemplified.

[0090] Referring to FIG. 1(b), in the second solid electrolyte, similar to the first solid electrolyte, the amorphous structure based on -BO-Si-OPO-Zr- network forms pores of non-bridged oxide (NBO) structure. However, since the second solid electrolyte further contains a second component compared to the first solid electrolyte, the pores of the non-bridged oxide (NBO) structure have a larger size. In addition, a part of the anion component (Cl) as the second component may be replaced by oxygen or electrostatically bonded, thus reducing the electronegativity of the second solid electrolyte. As a result, the second component may form an effective ion path to easily pass Li+ cations released from the active material electrode.

[0091] Based on 100 mol% of the total amount of 2Li, Si, 2B, Zr, and 2P, in the second solid electrolyte, 2Li may be contained in an amount greater than or equal to about 40 mol% and less than or equal to about 80 mol%, Si may be contained in an amount greater than or equal to about 0 mol% and less than or equal to about 30 mol%, 2B may be contained in an amount greater than or equal to about 0 mol% and less than or equal to about 60 mol%, Zr may be contained in an amount greater than or equal to about 0 mol% and less than or equal to about 50 mol%, and 2P may be contained in an amount greater than or equal to about 0 mol% and less than or equal to about 60 mol%. The description is the same as that of the first solid electrolyte.

[0092] Furthermore, the molar fraction of 2Li / (Si+2B+Zr) in the second solid electrolyte may be about 0.5 to about 5. The explanation thereof is also the same as that of the first solid electrolyte.

[0093] For reference, the mole fraction of 2Li / (Si+2B+Zr) may be partially higher in the second solid electrolyte than in the first solid electrolyte because the mole fraction of Li / (Si+B+Zr) is relatively higher due to the presence of the second component.

[0094] Specifically, the second solid electrolyte can be represented by Chemical Formula 2. [Chemical formula 2] a(Li2O)·b(SiO2)·c(B2O3)·d(P2O5)·e(ZrO2)·f(X m Y n )

[0095] In Chemical Formula 2, a to f are real numbers representing mole fractions, where 40 ≤ a ≤ 80, 40 ≤ a ≤ 0, or 40 ≤ a ≤ 60; 0 < b ≤ 30, 3 ≤ b ≤ 20, or 5 ≤ b ≤ 15; 0 < c ≤ 60, 5 ≤ c ≤ 40, or 10 ≤ c ≤ 20; 0 < d ≤ 60, 1 ≤ d ≤ 20, or 1 ≤ d ≤ 15; 0 < e ≤ 50, 1 ≤ e ≤ 20, or 1 ≤ e ≤ 10; 0 ≤ f ≤ 50, 1 ≤ f ≤ 10, or 1 ≤ f ≤ 5; X is Li, Al, or a combination thereof; Y is Cl, O, or a combination thereof; 0 < m ≤ 5 or 1 ≤ m ≤ 3; 0 < n ≤ 5 or 1 ≤ n ≤ 4.

[0096] The second solid electrolyte can also soften within a specific temperature range based on its amorphous characteristics.

[0097] Specifically, the softening point of the second solid electrolyte may be within a temperature range higher than or equal to about 500 °C and lower than or equal to about 550 °C. The explanation is the same as that of the first solid electrolyte.

[0098] The second solid electrolyte may also be a glass or a glass-ceramic, and the explanation is the same as that of the first solid electrolyte.

[0099] In particular, when the second solid electrolyte is a glass-ceramic, in X-ray diffraction (XRD) analysis using Cu-Kα, a peak due to Li3PO4 may appear in the range of 2θ from about 22° to about 25°, or a peak due to Li4B7O 12 Cl may appear, or a peak due to Al2O3 may further appear in the range of 2θ from about 15° to about 20 °C. Common to the case where the first solid electrolyte is a glass-ceramic, a peak due to Li3PO4 appears, and due to the second component, peaks due to Li4B7O 12 Cl and a peak due to Al2O3 appear.

[0100] In summary, when the second solid electrolyte is a glass ceramic, in the amorphous structure containing the -BO-Si-OPO-Zr- network, there is necessarily a LiPO4 crystalline phase having a size greater than or equal to about 1 nm, greater than or equal to about 3 nm, less than or equal to about 10 nm, or less than or equal to about 5 nm, and optionally a LiBO crystalline phase having the same or similar size as that of the LiPO4 crystalline phase. 12 A Cl or Al2O3 crystalline phase may additionally be present.

[0101] As described above, the second solid electrolyte may exhibit a higher ionic conductivity than the first solid electrolyte. Specifically, the ionic conductivity of the second solid electrolyte may be about 1.0×10 -7 The measurement method is as explained above.

[0102] The second solid electrolyte may be prepared by adding additives to the first solid electrolyte in a stoichiometric molar ratio according to the target composition, and then heat treated at about 525°C to about 530°C for about 8 hours to about 10 hours under an air atmosphere.

[0103] (All-solid-state battery) Another embodiment provides an all-solid-state battery comprising a body including a solid electrolyte layer, a positive electrode layer and a negative electrode layer alternately stacked with the solid electrolyte layer disposed therebetween, and a first external electrode and a second external electrode disposed on either side of the body, respectively. The solid electrolyte layer comprises one of the first solid electrolyte and the second solid electrolyte.

[0104] The all-solid-state battery of the above embodiment may be a microchip-type all-solid-state battery. As mentioned above, the microchip-type all-solid-state battery basically has battery characteristics and may be treated as an IT component such as an MLCC or a power inductor component.

[0105] The microchip-type solid-state battery itself, such as a chip, is mounted on a substrate by SMD and can further have circuit design freedom in terms of passive elements, etc.

[0106] In microchip-type all-solid-state batteries, oxide-based solid electrolytes are generally used, rather than sulfide-based solid electrolytes or polymer-based solid electrolytes. Oxide-based solid electrolytes have the advantages of a wide electrochemical potential window, excellent suppression of secondary interfacial reactions, low manufacturing costs, applicability of various composition ranges, etc., and can realize multi-layer microchip-type all-solid-state batteries through co-firing processing.

[0107] In particular, the all-solid-state battery of one embodiment includes any one of the first solid electrolyte and the second solid electrolyte in the solid electrolyte layer, and therefore may exhibit superior performance and durability compared to a case where an oxide solid electrolyte containing Li, Si, B, and P but not containing Zr is applied to the solid electrolyte layer.

[0108] FIG. 2 is a cross-sectional schematic diagram of an all-solid-state battery according to one embodiment.

[0109] 2, the all-solid-state battery may include a body including a solid electrolyte layer 123 and positive and negative electrode layers stacked alternately with the solid electrolyte layer 123 in between. In addition, the all-solid-state battery may further include a first external electrode 131 and a second external electrode 132 disposed on either side of the body, respectively.

[0110] Specifically, the all-solid-state battery includes an electrode layer and a solid electrolyte layer disposed adjacent to the electrode layer in the stacking direction. The electrode layer may essentially include a current collector 125 and electrode active material layers 121 and 122 coated on one or both surfaces of the current collector 125.

[0111] For example, an electrode layer disposed at the top in the stacking direction may be formed by coating one surface of the negative electrode current collector 125 with the negative electrode active material layer 122, and another electrode layer disposed at the bottom may be formed by coating one surface of the positive electrode current collector 125 with the positive electrode active material layer 121. Furthermore, the electrode layers disposed at the top and bottom may be formed by coating both surfaces of the positive electrode current collector 125 with the positive electrode active material layer 121 and both surfaces of the negative electrode current collector 125 with the negative electrode active material layer 122.

[0112] The solid electrolyte layer 123 may be disposed between the positive electrode layer and the negative electrode layer and stacked. Thus, the solid electrolyte layer 123 may be disposed adjacent to the positive electrode active material layer 121 of the positive electrode layer and the negative electrode active material layer 122 of the negative electrode layer in the stacking direction. Thus, in an all-solid-state battery, a plurality of positive electrode layers and a plurality of negative electrode layers may be alternately disposed, and a plurality of solid electrolyte layers 123 may be disposed between them and stacked.

[0113] The insulating layer 124 may be disposed along the edges of the positive electrode layer and the negative electrode layer. The insulating layer 124 may be disposed on the solid electrolyte layer 123 and formed so as to be laterally adjacent to the edges of the positive electrode layer or the negative electrode layer. Thus, the insulating layer 124 may be disposed on the same layer as the positive electrode layer and the negative electrode layer, respectively. The insulating layer 124 may be formed by using the same material as the solid electrolyte layer 123. Thus, in the all-solid-state battery, the insulating layer 124 and the solid electrolyte layer 123 are not distinguished from each other at the boundary, but are integrally formed as one body of the solid electrolyte layer 123.

[0114] The positive electrode layer, the solid electrolyte layer 123, the negative electrode layer, and the insulating layer 124 are stacked as described above to form a cell stack of an all-solid-state battery. At the upper and lower ends of the cell stack of the all-solid-state battery, a protective layer of insulating material may be formed. Furthermore, at both sides of the cell stack of the all-solid-state battery, the ends of the positive electrode current collector 125 and the negative electrode current collector 125 are exposed, and the external electrodes 131 and 132 are connected to the exposed ends and bonded thereto. In other words, the external electrodes 131 and 132 may be connected to the ends of the positive electrode current collector 125 to have a positive electrode, and to the ends of the negative electrode current collector 125 to have a negative electrode, respectively. When the ends of the positive electrode current collector 125 and the negative electrode current collector 125 are configured to face in opposite directions to each other, the external electrodes 131 and 132 may also be disposed on both sides, respectively.

[0115] The positive electrode layer, the solid electrolyte layer 123, and the negative electrode layer may be stacked, thus forming an all-solid-state battery cell stack. At the top and bottom of the all-solid-state battery cell stack, a protective layer 140 of insulating material may be formed, which may be the same material as the solid electrolyte layer 123.

[0116] The positive electrode active material contained in the positive electrode layer may include a compound capable of intercalating and deintercalating lithium (lithiated intercalation compound). Specifically, a composite oxide of lithium and at least one metal selected from cobalt, manganese, nickel, or a combination thereof may be used, and a specific example thereof may be a compound represented by any one of the following chemical formulas: Li a A 1-b R b D2 (wherein, in the above formula, 0.90≦a≦1.8 and 0≦b≦0.5); Li a E 1-b R b O 2-c D c (wherein, in the above formula, 0.90≦a≦1.8, 0≦b≦0.5, and 0≦c≦0.05); LiE 2-bR b O 4-c D c (wherein, in the above formula, 0≦b≦0.5 and 0≦c≦0.05); Li a Ni 1-b-c Co b R c D α (wherein, in the above formula, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Co b R c O 2-α Z α (wherein, in the above formula, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Co b R c O 2-α Z2 (wherein, in the above formula, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b R c D α (wherein, in the above formula, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Mn b R c O 2-α Z α (wherein, in the above formula, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b R c O 2-α Z2 (wherein, in the above formula, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni b E c G dO2 (wherein, in the above formula, 0.90≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, and 0.001≦d≦0.1); Li a Ni b Co c Mn d G e O2 (wherein, in the above formula, 0.90≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, and 0.001≦e≦0.1); Li a NiG b O2 (wherein, in the above formula, 0.90≦a≦1.8 and 0.001≦b≦0.1); Li a CoG b O2 (wherein, in the above formula, 0.90≦a≦1.8 and 0.001≦b≦0.1); Li a MnG b O2 (wherein, in the above formula, 0.90≦a≦1.8 and 0.001≦b≦0.1); Li a Mn2G b O4 (wherein, in the above chemical formula, 0.90≦a≦1.8 and 0.001≦b≦0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiTO2; LiNiVO4; Li (3-f) J2(PO4)3(0≦f≦2);Li (3-f) Fe2(PO4)3 (0≦f≦2); and LiFePO4.

[0117] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; R is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; Z is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; T is Cr, V, Fe, Sc, Y, or a combination thereof; and J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof.

[0118] The positive active material may include a positive active material with a coating layer, or a compound of the active material and the active material coated with a coating layer. The coating layer may include a coating element compound, such as an oxide or hydroxide of the coating element, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element. The compound for the coating layer may be either amorphous or crystalline. The coating element included in the coating layer may be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The coating process may include any conventional process (e.g., spray coating, dipping, etc.) as long as it does not cause any adverse effect on the properties of the positive active material, which is well known to those skilled in the art, and therefore a detailed description thereof will be omitted.

[0119] The negative electrode active material included in the negative electrode layer may include a material that reversibly intercalates / deintercalates lithium ions, lithium metal, a lithium metal alloy, a material capable of doping and dedoping lithium, or a transition metal oxide.

[0120] The material that reversibly intercalates / deintercalates lithium ions may be a carbon material, which may be any commonly used carbon-based negative active material in lithium ion secondary batteries, examples of which may be crystalline carbon, amorphous carbon, or a combination thereof. Examples of crystalline carbon may be graphite, such as amorphous, sheet, flake, spherical, or fibrous natural or artificial graphite. Examples of amorphous carbon may be soft carbon (low-temperature calcined carbon) or hard carbon, mesophase pitch carbonization products, calcined coke, etc.

[0121] The lithium metal alloy may be an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, or Sn.

[0122] Substances that can be doped and undoped with lithium are Si, SiO x , (0 < x < 2), Si-C composites, Si-Q alloys (where Q is selected from alkali metals, alkaline earth metals, Group 13-16 elements, transition elements, rare earth elements, and combinations thereof and is not Si), Sn, SnO2, Sn-C composites, Sn-R (where R is selected from alkali metals, alkaline earth metals, Group 13-16 elements, transition elements, rare earth elements, and combinations thereof and is not Sn). The elements Q and R may be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, or combinations thereof.

[0123] Transition metal oxides may include vanadium oxide, lithium vanadium oxide, lithium vanadium oxide, lithium vanadium phosphate (Li3V2(PO4)3, LVP), etc.

Mode for Carrying Out the Invention

[0124] Hereinafter, examples and comparative examples of the present disclosure will be described. However, these examples should in no way be construed as limiting the scope of the present disclosure.

[0125] [Example 1] To produce a glass ceramic, Li2CO3 (purity: 99%); SiO2 (purity: 99.8%); B2O3 (purity: 95%); ZrO2 (purity: 98%); and P2O5 (purity: 98%), or (NH4)2HPO4 (purity: 98%) were used as raw materials.

[0126] The twin roller melting and quenching method was used as the method for producing glass ceramics, and the crucible in the apparatus using the twin roller melting and quenching method was made of platinum.

[0127] To obtain a target composition of 57(Li2O)·10(SiO2)·18(B2O3)·12(P2O5)·3(ZrO2) [mol%], the raw materials were mixed according to the stoichiometric molar ratio, heat-treated in the range of 450°C-700°C to fully volatilize the ammonia in the mixed raw materials, and then vitrified after continuously maintaining at 1200°C for about 2 hours. The vitrified molten metal was collected as cullet-type bulk material after cooling in the range of 500°C-700°C. These cullets were crushed through a certain grinding process in anhydrous ethanol to obtain powders without secondary particles (aggregates), and then dried and classified to obtain glass ceramics with particles having an average particle size (D50) of 1.5μm-3.0μm. Glass ceramics were used as the solid electrolyte in Example 1.

[0128] [Example 2] The solid electrolyte of Example 2 was prepared in the same manner as in Example 1, except that the target composition was changed to 57(Li2O)·10(SiO2)·18(B2O3)·14(P2O5)·1(ZrO2) [mol%].

[0129] [Example 3] The solid electrolyte of Example 3 was prepared in the same manner as in Example 1, except that the target composition was changed to 57(Li2O)-10(SiO2)·18(B2O3)·10(P2O5)·5(ZrO2) [mol%].

[0130] [Example 4] The solid electrolyte of Example 4 was prepared in the same manner as in Example 1, except that the target composition was changed to 57(Li2O)-10(SiO2)·18(B2O3)·5(P2O5)·10(ZrO2) [mol%].

[0131] [Example 5] A mixed powder was prepared by post-adding LiCl to the glass ceramic according to Example 1. Based on 100 wt% of the mixed powder, the content of the post-added LiCl was 5 wt%.

[0132] The mixed powder was then heat-treated in an air atmosphere at a temperature range of 525 to 530° C. for 8 to 10 hours.

[0133] Thus, the solid electrolyte of Example 5 was obtained, where the target (expected) composition of the corresponding solid electrolyte was 56(Li2O) 10(SiO2) 16(B2O3) 10(PO 50 )·3(ZrO2)·5(LiCl) [mol%].

[0134] [Example 6] The solid electrolyte of Example 6 was prepared in the same manner as in Example 5, except that Li3PO4 was added later instead of LiCl to have a target composition of 57(Li2O)·10(SiO2)·16(B2O3·14P2O5)·3(ZrO2) [mol %].

[0135] [Example 7] The solid electrolyte of Example 7 was prepared in the same manner as in Example 5, except that Li2CO3 was added later instead of LiCl to have a target composition of 61(Li2O)·10(SiO2)·16(B2O3)·10(P2O5)·3(ZrO2) [mol %].

[0136] [Example 8] The solid electrolyte of Example 8 was prepared in the same manner as in Example 5, except that α-Al2O3 was added later instead of LiCl to have a target composition of 56(Li2O)·10(SiO2)·16(B2O3)·10(P2O5)·3(ZrO2)·5(Al2O3) [mol%].

[0137] [Example 9] The solid electrolyte of Example 9 was prepared in the same manner as in Example 8, except that the target composition was changed to 56(Li2O)·10(SiO2)·16(B2O3)·10(P2O5)·7(ZrO2)·1(Al2O3) [mol%].

[0138] [Example 10] The solid electrolyte of Example 10 was prepared in the same manner as in Example 8, except that the target composition was changed to 56(Li2O)·10(SiO2)·16(B2O3)·10(P2O5)·5(ZrO2)·3(Al2O3) [mol%].

[0139] [Comparative Example 1] The solid electrolyte of Comparative Example 1 was prepared in the same manner as in Example 1, except that the target composition was changed to 57(Li2O)·10(SiO2)·18(B2O3)·15(P2O5) [mol %].

[0140] [Comparative Example 2] The solid electrolyte of Comparative Example 2 was prepared in the same manner as in Example 1, except that the target composition was changed to 57(Li2O)·10(SiO2)·18(B2O3)·12(P2O5)·3(GeO2) [mol%] by using GeO2 instead of ZrO2 as a raw material.

[0141] For reference, the target compositions used to prepare each of the solid electrolytes of Examples 1 to 10 and Comparative Examples 1 and 2 are shown in Table 1. [Table 1] (Unit: mol%) [Table 1] Evaluation example 1: Solid electrolyte (1) Evaluation of ICP analysis

[0142] Each of the solid electrolytes of Examples 1 and 8 was subjected to ICP analysis to determine the mole fractions of the major elements.

[0143] The ICP analysis was carried out by using an inductively coupled plasma optical emission spectrometer (ICP-OES, device name: Optima 7300DV, manufacturer: PerkinElmer Inc.). Specifically, about 0.7 g of the solid electrolyte sample was placed in a platinum (Pt) crucible, to which about 1 mL of concentrated sulfuric acid (98 wt%, EL grade) was added, and then heated at 300°C for 3 hours and incinerated in an electric furnace (Lindberg Blue M, ThermoFisher Scientific Corp.) according to the following program of steps 1 to 3. 1) Stage 1: Initial temperature 0°C, rate (temperature / time) 180°C / hour, temperature (hold time) 180°C (1 hour) 2) Stage 2: Initial temperature 180°C, rate (temperature / time) 85°C / hour, temperature (hold time) 370°C (2 hours) 3) Stage 3: Initial temperature 370°C, rate (temperature / time) 47°C / hour, temperature (holding time) 510°C (3 hours). Then, 1 mL of concentrated nitric acid (48 wt%) and 20 μl of concentrated hydrofluoric acid (50 wt%) were added to the residue, then the platinum crucible was sealed and shaken for 30 minutes or more, after which 1 mL of boric acid was added to it, then it was stored at 0°C for 2 hours or more, then it was diluted with 30 mL of ultrapure water and incinerated to carry out the measurement.

[0144] Therefore, the mole fractions of the major elements of each of the solid electrolytes of Examples 1 and 8 were measured, and the results are shown in Table 2. Furthermore, the target compositions used to prepare each of the solid electrolytes of Examples 1 and 5 are shown in Table 2. [Table 2] (Unit: mol%) [Table 2]

[0145] Referring to Table 2, some elements are lost during the process of preparing each solid electrolyte of Examples 1 and 8, but the target composition is substantially the same as the measured value. Furthermore, each solid electrolyte of Examples 1 and 8 has a molar fraction of 2Li / (Si+2B+Zr) in the range of 0.5 to 5. Specifically, based on the measured value, the solid electrolyte of Example 1 has a molar fraction of 2Li / (Si+2B+Zr) of 1.87, and the solid electrolyte of Example 8 has a molar fraction of 2Li / (Si+2B+Zr) of about 1.99. The reason why the molar fraction of 2Li / (Si+2B+Zr) in the solid electrolyte of Example 8 is higher than that of Example 1 is because the molar fraction of (Si+2B+Zr) is reduced by the presence of the second component.

[0146] In this specification, the solid electrolytes of Examples 1 and 8 were evaluated as representatives, but it was estimated that the solid electrolytes of Examples 2 to 4, 9, and 10 and Comparative Examples 1 and 2 also showed target compositions substantially the same as the actually measured values.

[0147] [(2) TMA thermal analysis] Each of the solid electrolytes of Examples 1 and 8 was subjected to thermomechanical analysis (TMA), and the analysis results are shown in FIGS.

[0148] Specifically, a 10 mm long sample was placed in a TMA machine (Q400, TA Instruments) in air and nitrogen atmosphere, and then exposed to temperature conditions (starting at 30° C. and increasing at 5° C. / min) while a tension of 19.6 mN was applied to it. As the temperature increased, the length of the sample changed accordingly, and the temperature at which the sample broke was measured. After measuring MD and TD, respectively, the higher temperature was defined as the meltdown temperature of the corresponding sample.

[0149] 3 and 4, the solid electrolytes of Examples 1 and 8 softened at 500 to 550° C. Specifically, the solid electrolyte of Example 1 began to melt at 516 to 526° C., and the solid electrolyte of Example 8 began to melt at 527° C.

[0150] On the other hand, each of the solid electrolytes according to Examples 1 and 8 was heated in an electric furnace at 3°C / min, maintained at 530°C for 8 hours under a mixed atmosphere of nitrogen (N2) and air, and then naturally cooled, and its SEM image was obtained and shown in Figure 6. Referring to Figure 5, each of the solid electrolytes according to Examples 1 and 5 softened after heat treatment due to their amorphous properties.

[0151] In this specification, the solid electrolytes of Examples 1 and 8 were evaluated as representatives, but the solid electrolytes of Examples 2 to 4, 9, and 10 were also assumed to have softening points higher than or equal to about 500°C and lower than or equal to about 550°C.

[0152] [(3)XRD analysis] X-ray diffraction (XRD, Bruker AXS D4-Endeavor XRD) analysis of each solid electrolyte of Examples 1 and 5 to 8 was carried out by using Cu-Kα, and the analysis results are shown in Figures 6 to 10.

[0153] The solid electrolytes of Examples 1 and 5 to 8 commonly exhibited a peak due to Li3PO4 in the 2θ range of 22° to 25° (common to FIGS. 6 to 10). Furthermore, the solid electrolyte of Example 5 exhibited a peak due to Li4B7O in the 2θ range of 42° to 45°. 12 The solid electrolyte of Example 8 showed an additional peak due to Cl (FIG. 7), which was caused by the addition of LiCl. Furthermore, the solid electrolyte of Example 8 showed an additional peak due to α-Al2O3 in the 2θ range of 15° to 20° (FIG. 10), which was caused by the addition of α-Al2O3.

[0154] In this specification, the solid electrolytes of Examples 1 and 5 to 8 were evaluated as representatives, but the solid electrolytes of Examples 2 to 4, 6, and 7 are estimated to show results similar to that of Example 1, and the solid electrolytes of Examples 9 and 10 are estimated to show results similar to that of Example 8.

[0155] [(4)FE-SEM and TEM analysis] By using a TEM device, each of the solid electrolytes of Examples 1 and 8 was examined on a localized area, and the results are shown in Figures 11 and 12, respectively.

[0156] 11 and 12, the solid electrolytes of Examples 1 and 8 commonly exhibited a crystal phase of 3 to 5 nm size present in the amorphous structure.

[0157] In this specification, the solid electrolytes of Examples 1 and 8 were evaluated as representatives, but it is estimated that the solid electrolytes of Examples 2 to 4 will show results similar to that of Example 1, and that the solid electrolytes of Examples 5 to 7, 9, and 10 will show results similar to that of Example 8.

[0158] [(5) Evaluation of ionic conductivity] In order to manufacture all-solid-state battery samples in the following manner, the solid electrolytes of Examples 1 to 8 and Comparative Examples 1 and 2 were used to measure the ionic conductivity of the samples.

[0159] First, 0.5 g of each solid electrolyte was taken and pelletized by applying a pressure of 1.5 tons using a circular die with a diameter of 14π to obtain a green sheet-shaped solid electrolyte sample.

[0160] The solid electrolyte sample was heat-treated at 500° C. to 600° C., and metal electrodes were formed on both sides of the sample to obtain an all-solid-state battery sample. In this specification, the metal electrodes were formed through sputtering of InGa paste, Ag paste, or the like.

[0161] The solid-state battery sample was placed on the jig regardless of the positive and negative electrode orientation. The EIS voltage was measured based on 100 mV. -6 The solid electrolytes of Examples 1 to 8 and Comparative Examples 1 and 2 were measured for resistance, which was converted to ionic conductivity, and the results are shown in Table 3. In addition, FIG. 13 in particular shows the resistance results of the solid electrolytes according to Examples 1 and 8. [Table 3] [Table 3]

[0162] Referring to Table 3, the solid electrolyte of Example 1 was a solid electrolyte (first solid electrolyte) consisting of only oxides containing Li, Si, B, Zr, and P, and had a 1×10 -8 13, the solid electrolytes of Examples 5 to 8 were solid electrolytes containing glass ceramic as a main component and a specific trace component (second solid electrolyte), and had an ion conductivity of 1×10 -7 This had the effect of ensuring an ionic conductivity of 1.0 S / cm.

[0163] [(6) Overview] Each solid electrolyte in Examples 1 to 5 corresponds to the first solid electrolyte described above (oxide containing Li, Si, B, Zr, and P). These solid electrolytes are glass ceramics having both amorphous and crystalline properties at the same time, which have a Li3PO4 crystalline phase of 3 to 5 nm size present in an amorphous structure based on a -BO-Si-OPO-Zr- network, and have a crystalline phase of 1×10 -8 The ionic conductivity was ensured at 1.0 S / cm.

[0164] Furthermore, each solid electrolyte of Examples 5 to 10 was the second solid electrolyte described above (containing an oxide containing Li, Si, B, Zr, and P as the first component; and an oxide or salt containing Li, Al, or Cl as the second component). These solid electrolytes were also glass-ceramics with amorphous and crystalline properties at the same time, which consisted of an amorphous structure based on the -BO-Si-OPO-Zr- network and an additional crystalline phase due to the second component (Li4B7O 12 It has a Li3PO4 crystal phase of 3 to 5 nm size in the Cl or Al2O3) and is 1×10 -7 The ionic conductivity was ensured at 1.0 S / cm.

[0165] The solid electrolytes of Examples 1 to 10 had higher ionic conductivity than the solid electrolytes of Comparative Examples 1 and 2, which was presumably caused in particular by Zr.

[0166] [Evaluation example 2: Evaluation of all-solid-state battery cells] All-solid-state battery cells containing each of the solid electrolytes of Examples 1 and 8 were fabricated and measured for charge and discharge performance.

[0167] First, 0.5 g of the solid electrolyte was taken and pelletized by applying a pressure of 1.5 tons using a circular die having a diameter of 14π to obtain a green sheet-shaped solid electrolyte sample.

[0168] Separately, 0.24 g of the solid electrolyte, 0.24 g of Li3V2(PO4)3, and 0.02 g of carbon black were mixed and pelletized by applying a pressure of 1.5 tons using a circular die to obtain a green sheet-type electrode active material layer sample. Two samples of this electrode active material layer were prepared.

[0169] Separately, 0.1 g of the solid electrolyte and 0.4 g of carbon black were mixed and pelletized by applying a pressure of 1.5 tons using a circular die to obtain a green sheet-type current collector layer sample. Two of the current collector layer samples were prepared.

[0170] The current collector layer sample / electrode active material layer sample / electrolyte layer sample / electrode active material layer sample / current collector layer sample were stacked in this order and heat-treated at 500 to 600° C. to obtain all-solid-state battery cells of Examples 1 and 8.

[0171] Each of the all-solid-state battery cells of Examples 1 and 8 was charged once and discharged once, and the charge and discharge graphs are shown in Figure 14. Specifically, each of the all-solid-state battery cells of Examples 1 and 8 was placed on a jig regardless of the + and - electrode directions, and then charged to a voltage of 2.4 V at a current density of 0.025 C rate, and discharged to a voltage of 0.001 V at the same current density.

[0172] 14, the all-solid-state battery cell of Example 1 exhibited an initial discharge capacity of 48 μAh (32.13 mAh / g) and a saturated discharge voltage of 1.5 to 1.6 V. Furthermore, the all-solid-state battery cell of Example 8 exhibited an initial discharge capacity of 63 μAh (40.51 mAh / g) and a saturated discharge voltage of 1.5 to 1.6 V.

[0173] In this specification, the all-solid-state battery cells of Examples 1 and 8 were evaluated as representatives, but the all-solid-state battery cells of Examples 2 to 4 were presumed to be similar to that of Example 1, and the all-solid-state battery cells of Examples 5 to 7, 9, and 10 were presumed to be similar to that of Example 8.

[0174] While the present disclosure has been described in connection with what are presently considered to be working exemplary embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but on the contrary, it is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims. [Explanation of symbols]

[0175] 121: Positive electrode active material layer 122: Negative electrode active material layer 123: Solid electrolyte layer 124: Insulating layer 125: Current collector 131: first external electrode 132: second external electrode 140:Protective layer

Claims

1. A solid electrolyte comprising Li, Si, B, Zr, and P.

2. In the solid electrolyte, 2Li is contained in an amount greater than or equal to about 40 mol% and less than or equal to about 80 mol%, Si is contained in an amount greater than or equal to about 0 mol% and less than or equal to about 30 mol%, 2B is contained in an amount greater than or equal to about 60 mol%, Zr is contained in an amount greater than or equal to about 0 mol% and less than or equal to about 50 mol%, and 2P is contained in an amount greater than or equal to about 0 mol% and less than or equal to about 60 mol%, based on 100 mol% of the total amount of 2Li, Si, 2B, Zr, and 2P. The solid electrolyte according to claim 1 .

3. 2. The solid electrolyte of claim 1, wherein the mole fraction of 2Li / (Si+2B+Zr) in the solid electrolyte is from about 0.5 to about 5.

4. The solid electrolyte is represented by Chemical Formula 1, [Chemical formula 1] a (Li 2 O) b (SiO 2 ) c (B 2 O 3 ) d(P 2 O 5 ) e(ZrO 2 ) In chemical formula 1, a to e are real numbers representing mole fractions, and 40≦a≦60, 0<b≦30, 0<c≦60, 0<d≦60, and 0<e≦50. The solid electrolyte according to claim 1 .

5. 5. The solid electrolyte of claim 4, wherein a+b+c+d+e=100.

6. 10. The solid electrolyte of claim 1, wherein the softening point of the solid electrolyte is greater than or equal to about 500°C and less than or equal to about 550°C.

7. The solid electrolyte of claim 1 , wherein the solid electrolyte is a glass or a glass ceramic.

8. The solid electrolyte was found to have a Li 3 P.O. 4 The solid electrolyte according to claim 7, which is a glass ceramic in which a peak due to

9. The solid electrolyte is comprised of LiFePO4 having a size greater than or equal to about 1 nm and less than or equal to about 10 nm in an amorphous structure. 3 P.O. 4 The solid electrolyte of claim 8 having a crystalline phase.

10. The solid electrolyte is about 1.0×10 -7 2. The solid electrolyte of claim 1 having an ionic conductivity greater than or equal to 1.0 S / cm.

11. An oxide containing Li, Si, B, Zr, and P as a first component; and As the second component, an oxide or salt containing at least one element selected from the group consisting of Li, Al, Na, Mg, K, Ca, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Se, Rb, S, Y, Nb, Mo, Ag, In, Sn, Sb, Cs, Ba, Hf, Ta, W, Pb, Bi, Au, La, Nd, Eu, I, Cl, Br, and F. A solid electrolyte comprising:

12. 12. The solid electrolyte of claim 11, wherein the mole fraction of 2Li / (Si+2B+Zr) in the solid electrolyte is from about 0.5 to about 5.

13. The solid electrolyte is represented by chemical formula 2: [Chemical formula 2] a (Li 2 O) b (SiO 2 ) c (B 2 O 3 ) d(P 2 O 5 ) e(ZrO 2 ) f(X m Y n ) In Chemical Formula 2, a to f are real numbers representing mole fractions, and 40≦a≦60, 0<b≦30, 0<c≦60, 0<d≦60, 0<e≦50, and 0≦f≦50; X is Li, Al, or a combination thereof; Y is Cl, O, or a combination thereof; 0<m≦5, and 0<n≦5 The solid electrolyte according to claim 11.

14. 14. The solid electrolyte of claim 13, wherein a+b+c+d+e+f=100.

15. 12. The solid electrolyte of claim 11, wherein the softening point of the solid electrolyte is greater than or equal to about 500°C and less than or equal to about 550°C.

16. 12. The solid electrolyte of claim 11, wherein the solid electrolyte is a glass or a glass-ceramic.

17. The solid electrolyte was found to have a Li 3 P.O. 4 The solid electrolyte according to claim 16, having a peak due to

18. The solid electrolyte is comprised of LiFePO4 having a size greater than or equal to about 1 nm and less than or equal to about 10 nm in an amorphous structure. 3 P.O. 4 20. The solid electrolyte of claim 17 having a crystalline phase.

19. The solid electrolyte was found to have a Li 4 B 7 O 12 Cl or Al 2 O 3 The solid electrolyte according to claim 17, further comprising a peak due to:

20. The solid electrolyte is about 1.0×10 -7 12. The solid electrolyte of claim 11 having an ionic conductivity greater than or equal to 1.0 S / cm.

21. A solid electrolyte comprising an amorphous structure based on a B--O--Si--O--P--O--Zr- network.

22. Li 3 P.O. 4 22. The solid electrolyte of claim 21 further comprising a crystalline phase.

23. The Li 3 P.O. 4 23. The solid electrolyte of claim 22, wherein the crystalline phase has a size greater than or equal to about 1 nm and less than or equal to about 10 nm.

24. Li 4 B 7 O 12 Cl crystal phase or Al 2 O 3 23. The solid electrolyte of claim 22 further comprising a crystalline phase.

25. a body including a solid electrolyte layer and a positive electrode layer and a negative electrode layer stacked alternately with the solid electrolyte layer disposed therebetween; and a first external electrode and a second external electrode disposed on opposite sides of the body, respectively; Equipped with The solid electrolyte layer comprises the solid electrolyte according to claim 1. All-solid-state battery.

26. The positive electrode layer and the negative electrode layer each include a current collecting layer and an electrode active material layer on the current collecting layer; The current collecting layer and the electrode active material layer each contain the solid electrolyte and the carbon-based conductive material according to any one of claims 1 to 24; The electrode active material layer further includes an electrode active material. The all-solid-state battery according to claim 25.

Citation Information

Patent Citations

  • Glass

    JP2020172410A

  • Lithium ion conductive material and method for producing the same

    JP2022089804A