Regenerated positive electrode active material, regenerating method thereof, and secondary battery including the same

The method of oxidation heat treatment with oxygen and lithium precursor addition effectively recycles lithium secondary battery positive electrode materials, addressing environmental and cost issues while improving performance.

JP2024542708AActive Publication Date: 2024-11-15LG ENERGY SOLUTION LTD

Patent Information

Application Number
JP2024532549
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-23
Filing Date
2023-06-26
Publication Date
2024-11-15
Estimated Expiration
2043-06-26

AI Technical Summary

Technical Problem

Conventional methods for recycling lithium secondary battery positive electrode active materials face environmental pollution, high costs, and reduced performance due to the use of acids and organic solvents, which generate toxic gases and require complex processes.

Method used

A method involving oxidation heat treatment with oxygen, followed by lithium precursor addition and annealing, to remove fluorine and lithium residues, and divide the oxidation heat treatment into two steps to clean-burn the binder, resulting in a positive electrode active material with improved charging capacity and resistance characteristics.

Benefits of technology

The method produces an environmentally friendly, cost-effective positive electrode active material with enhanced charging capacity and resistance characteristics, eliminating the need for acids and organic solvents, and reducing waste generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542708000001_ABST
    Figure 2024542708000001_ABST
Patent Text Reader

Abstract

The present invention relates to a regenerated positive electrode active material, a regenerating method thereof, and a secondary battery including the same, and more particularly to a regenerated positive electrode active material which is at least one selected from the group consisting of a lithium nickel oxide (LNO)-based positive electrode active material, a nickel cobalt manganese (NCM)-based positive electrode active material, a nickel cobalt aluminum (NCA)-based positive electrode active material, and a nickel cobalt manganese aluminum (NCMA)-based positive electrode active material, and which is characterized in that it contains 60 mol % or more of Ni, has a fluorine (F) content of 250 mg / kg or less, and has an average crystal size of 122 nm or less, a regenerating method thereof, and a secondary battery including the same. According to the present invention, a waste positive electrode using a high-nickel (High-Ni) positive electrode material is subjected to an oxidative heat treatment by introducing oxygen, and then the waste positive electrode is washed for the first time. Then, a lithium precursor is added, annealed, and then washed for the second time, so that the fluorine (F) content on the surface of the regenerated positive electrode active material is reduced. Furthermore, by dividing the oxidative heat treatment step into two steps, the binder is burned cleanly, and the fluorine (F) and residual lithium generated in the heat treatment step are reduced, and the crystal size is reduced, thereby providing a positive electrode active material with excellent charging capacity, resistance characteristics, and capacity characteristics. In addition, since no acid is used in the recovery and regeneration process, it is environmentally friendly, and since there is no need for neutralization and wastewater treatment, the process cost is reduced. Since the positive electrode active material is regenerated as it is without being decomposed, there are no metal elements to be discarded, and since no organic solvent is used, there is no risk of toxic gas generation or explosion. In particular, since the water washing process is omitted, there is an effect of providing a method for regenerating a positive electrode active material with greatly improved economic efficiency and productivity.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0082984 filed on July 6, 2022 and Korean Patent Application No. 10-2022-0082985 filed on July 6, 2022, and Korean Patent Application No. 10-2023-0081265 refiled on June 23, 2023, and all contents disclosed in the documents of the Korean patent application are incorporated as part of this specification.

[0002] The present invention relates to a regenerated positive electrode active material, a regenerating method thereof, and a secondary battery including the same. More specifically, the present invention relates to a method for regenerating a positive electrode active material, which comprises: a waste positive electrode using a high-nickel (High-Ni) positive electrode material; a first cleaning step; a lithium precursor; an annealing step; and a second cleaning step. The method removes fluorine (F) and lithium precursor that did not participate in the reaction from the surface of the regenerated positive electrode active material; and a method for regenerating a positive electrode active material, which is environmentally friendly because no acid is used in the recovery and regeneration process; a method for regenerating a positive electrode active material, which is environmentally friendly because no neutralization and wastewater treatment are required; a method for regenerating a positive electrode active material without decomposing the positive electrode active material, which does not require metal elements to be discarded; a method for regenerating a positive electrode active material, which is environmentally friendly because no organic solvent is used, which does not require the generation of toxic gases or explosions; and a method for regenerating a positive electrode active material, which is economically and productively improved because a water washing step is omitted. [Background technology]

[0003] A lithium secondary battery generally comprises a positive electrode in which a layer of positive electrode active material is coated on a metal foil such as aluminum, a negative electrode in which a layer of negative electrode active material is coated on a metal foil such as copper, a separator that prevents the positive electrode and the negative electrode from mixing, and an electrolyte that allows lithium ions to move between the positive electrode and the negative electrode.

[0004] The positive electrode active material layer mainly uses a lithium-based oxide as an active material, and the negative electrode active material layer mainly uses a carbon material as an active material. Since the lithium-based oxide generally contains rare metals such as cobalt, nickel, or manganese, much research has been conducted into recovering and reusing rare metals from the positive electrodes of lithium secondary batteries that are discarded after use or from positive electrode scraps generated during the manufacturing process of lithium secondary batteries (hereinafter referred to as "scrap positive electrodes").

[0005] Conventional technology for recovering rare metals from used positive electrodes mostly involves dissolving the used positive electrodes with hydrochloric acid, sulfuric acid, or nitric acid, then extracting cobalt, manganese, nickel, etc. with an organic solvent and using them again as raw materials for synthesizing positive electrode active materials.

[0006] However, the method of extracting rare metals using acid has the disadvantages of causing environmental pollution, requiring a neutralization process and a wastewater treatment process, which significantly increases the process cost, and making it impossible to recover lithium, the main metal in the positive electrode active material.

[0007] In order to overcome these drawbacks, recent studies have been conducted on direct recycled methods that directly recycle the cathode active material from waste cathodes without decomposing it. There are roughly four types of such methods, namely calcination, solvent dissolution, aluminum foil dissolution, and crushing & screening.

[0008] Although the calcination method is a simple process, it has the disadvantages of generating foreign matter on the surface of the regenerated positive electrode active material that reduces the output performance of the battery, generating waste gas, and consuming a large amount of energy.

[0009] In addition, the solvent dissolution method can obtain a regenerated positive electrode active material with a relatively clean surface, but has the disadvantage that the solvent used to dissolve the binder, such as N-methyl-2-pyrrolidone (NMP), is a toxic gas and has a risk of explosion, making it poor in stability and requiring an expensive solvent recovery process.

[0010] In addition, the aluminum foil dissolving method has good process stability, low process costs, and easy binder removal, but has the disadvantages of generating foreign matter that is difficult to remove on the surface of the recycled positive electrode active material, and generating hydrogen gas during the aluminum foil removal process, which may cause an explosion.

[0011] Finally, the crushing and screening method has the advantage of being the simplest process, but has the disadvantages that it is difficult to completely separate the current collector from the positive electrode active material, the particle size distribution of the positive electrode active material changes during the crushing process, and the binder remains, causing the battery characteristics of the recycled positive electrode active material to deteriorate.

[0012] Therefore, there is an urgent need to develop a method for regenerating a positive electrode active material with improved output performance, in an environmentally friendly and safe manner, with fewer steps and at fewer costs, without the metal elements discarded from used positive electrodes. Summary of the Invention [Problem to be solved by the invention]

[0013] In order to solve the above problems of the prior art, the present invention provides a method for regenerating a positive electrode active material by subjecting a waste positive electrode using a high-nickel (High-Ni) positive electrode material to an oxidative heat treatment by introducing oxygen, followed by a first wash, and then adding a lithium precursor, annealing, and then a second wash, thereby removing fluorine (F) and lithium precursor that did not participate in the reaction from the surface of the regenerated positive electrode active material. Furthermore, the oxidative heat treatment step is divided into two steps, so that the binder is burned cleanly, and the fluorine (F) and residual lithium generated in the heat treatment step are reduced, thereby reducing the crystallite size, thereby providing a positive electrode active material with excellent charging capacity, resistance characteristics, and capacity characteristics. In addition, the present invention provides a method for regenerating a positive electrode active material, which is environmentally friendly because no acid is used in the recovery and regeneration process of the positive electrode active material, and which does not require neutralization or wastewater treatment, thereby reducing process costs, and which regenerates the positive electrode active material without decomposing it, so there are no metal elements to be discarded, and there is no risk of toxic gas generation or explosion because no organic solvent is used, and in particular, the water washing process is omitted, thereby greatly improving economy and productivity.

[0014] Another object of the present invention is to provide a secondary battery that is excellent in initial discharge capacity, rate performance, and capacity characteristics.

[0015] The above and other objects of the present invention can be achieved by the present invention described below. [Means for solving the problem]

[0016] In order to achieve the above object, the present invention provides I) a cathode active material which is at least one selected from the group consisting of lithium nickel oxide (LNO)-based cathode active materials, nickel cobalt manganese (NCM)-based cathode active materials, nickel cobalt aluminum (NCA)-based cathode active materials, and nickel cobalt manganese aluminum (NCMA)-based cathode active materials, and which is characterized in that it contains 60 mol % or more of Ni, has a fluorine (F) content of 250 mg / kg or less, and has an average crystallite size of 122 nm or less.

[0017] II) In the above I), the surface of the positive electrode active material may be coated with a coating agent containing metal or carbon.

[0018] III) In I) or II), the metal may be boron (B), tungsten (W), or a mixture thereof.

[0019] IV) In the above I) to III), the positive electrode active material may be a regenerated positive electrode active material.

[0020] The present invention also provides a method for regenerating a positive electrode active material, comprising the steps of: V) subjecting a waste positive electrode, having a positive electrode active material layer containing 60 mol % or more of Ni formed on a current collector, to an oxidative heat treatment by introducing oxygen to thermally decompose the binder and the conductive material in the positive electrode active material layer, thereby separating the current collector from the positive electrode active material layer and recovering the positive electrode active material in the positive electrode active material layer; a primary washing of the recovered positive electrode active material; a step of adding a lithium precursor to the primarily washed positive electrode active material and annealing it; and a second washing of the annealed positive electrode active material.

[0021] VI) In the above V), the oxidation heat treatment can be carried out at 300 to 650°C.

[0022] VII) In the above V) or VI), the oxidation heat treatment can be a primary heat treatment at 300 to 450°C, followed by a secondary heat treatment at 500 to 650°C.

[0023] VIII) In the above V) to VII), the first heat treatment can be carried out for 10 minutes to 3 hours, and the second heat treatment can be carried out for 10 minutes to 2 hours.

[0024] IX) In the above V) to VIII), the oxygen may have a purity of 59% or more.

[0025] X) In the above V) to IX), the primary washing can be carried out by immersing the recovered positive electrode active material in water or a basic lithium compound aqueous solution as a washing liquid, or by immersing and stirring the material at the same time.

[0026] XI) In the above V) to X), the basic lithium compound aqueous solution may contain more than 0 wt % and 15 wt % or less of a lithium compound.

[0027] XII) In the above V) to XI), the method of adding a lithium precursor to the primarily washed positive electrode active material in the annealing step can be to mix the primarily washed positive electrode active material with a lithium precursor solution and spray dry it.

[0028] XIII) In V) to XII), the second washing may include mixing the annealed positive electrode active material with water as a washing solution, filtering the mixture, and drying the solid positive electrode active material obtained after the filtration.

[0029] XIV) In V) to XIII), the lithium precursor may include one or more of LiOH, Li2CO3, LiNO3, and Li2O.

[0030] XV) In the above V) to XIV), the lithium precursor may be added in an amount corresponding to 1 mol % to 40 mol % when the total amount of lithium in the raw material positive electrode active material used in the positive electrode active material layer is 100 mol %.

[0031] XVI) In the above V) to XV), the annealing can be carried out at 400 to 1000°C.

[0032] XVII) In the above V) to XVI), the method for regenerating a positive electrode active material may further include a step of surface-coating the second washed positive electrode active material to obtain a reusable positive electrode active material.

[0033] XVIII) In the above V) to XVII), the surface coating can be performed by coating the surface with one or more of metals, organometallics, and carbon components in a solid or liquid phase manner, followed by heat treatment at 100 to 1200°C.

[0034] The present invention also provides XIX) a regenerated positive electrode active material, which is produced by the method for regenerating a positive electrode active material according to any one of V) to XVIII).

[0035] The present invention also provides XX) a positive electrode active material which is at least one selected from the group consisting of lithium nickel oxide (LNO)-based positive electrode active materials, nickel cobalt manganese (NCM)-based positive electrode active materials, nickel cobalt aluminum (NCA)-based positive electrode active materials, and nickel cobalt manganese aluminum (NCMA)-based positive electrode active materials, and which contains 60 mol% or more of Ni, has a fluorine (F) content of 305 mg / kg or less, and has an average crystallite size of 139 nm or less.

[0036] XXI) In the above XX), the positive electrode active material may have a residual Li2CO3 content of 0.16 wt% or less.

[0037] XXII) In the above XX) or XXI), the positive electrode active material may be a regenerated positive electrode active material.

[0038] The present invention also provides, in part XXIII, a secondary battery comprising the positive electrode active material according to any one of I) to IV), XIX), XX), and XXII). Effect of the Invention

[0039] According to the present invention, a waste positive electrode using a high-nickel (High-Ni) positive electrode material is subjected to an oxidative heat treatment by introducing oxygen, and then the waste positive electrode is washed for the first time. Then, a lithium precursor is added, and the waste positive electrode is annealed and washed for the second time. As a result, fluorine (F) and lithium precursor that could not participate in the reaction are removed from the surface of the regenerated positive electrode active material, and the crystallite size is reduced. Furthermore, the oxidative heat treatment step is divided into two steps, and the binder is burned cleanly, and the fluorine (F) and residual lithium generated in the heat treatment step are reduced, and the crystallite size is reduced, thereby providing a positive electrode active material with excellent charging capacity, resistance characteristics, and capacity characteristics. In addition, since no acid is used in the recovery and regeneration process of the positive electrode active material, it is environmentally friendly and does not require neutralization or wastewater treatment, thereby reducing process costs. Since the positive electrode active material is regenerated as it is without being decomposed, there are no metal elements to be discarded. Since no organic solvent is used, there is no risk of toxic gas generation or explosion. In particular, since the water washing process is omitted, there is an effect of providing a method for regenerating a positive electrode active material with greatly improved economic efficiency and productivity. [Brief description of the drawings]

[0040] The following drawings attached to this specification are illustrative of embodiments of the present invention and, together with the detailed description below, serve to further understand the technical ideas of the present invention. Therefore, the present invention should not be interpreted as being limited to the matters described in these drawings. [Figure 1] FIG. 13 is a diagram showing positive electrode scraps that are discarded after cutting electrode plates from a positive electrode sheet. [Diagram 2] 1 shows SEM photographs of the positive electrode active materials regenerated in Example 1 and Comparative Examples 1 to 3. [Diagram 3] 1 is a graph showing the results of charge capacity of coin cells to which the positive electrode active materials regenerated in Example 1 and Comparative Examples 1 to 3 are applied. [Figure 4] FIG. 1 is a graph showing the results of charge-discharge cycles of monocells using the positive electrode active materials regenerated in Example 1 and Comparative Examples 1 to 3, and showing the changes in capacity retention rate (%) and resistance increase rate (%) depending on the number of cycles. [Diagram 5] 13 is a graph showing the results of charging capacity of coin cells to which the positive electrode active materials regenerated in Additional Examples 1 to 3 and Additional Comparative Examples 1 and 2 are applied. [Figure 6] FIG. 1 is a graph showing the results of charge-discharge cycles of monocells using the positive electrode active materials regenerated in Additional Examples 1 to 3 and Additional Comparative Examples 1 and 2, and showing the change in capacity retention rate (%) depending on the number of cycles. [Figure 7] 2 is a flow chart of a process for regenerating a positive electrode active material according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0041] The inventors were researching a direct recycled method for recycling used positive electrodes into positive active materials with excellent battery performance without decomposing the positive active materials. They found that when used positive electrodes using high-nickel (High-Ni) positive electrode materials are subjected to oxidation heat treatment with oxygen, first washing, and then annealing with a lithium precursor and then second washing, fluorine (F) and lithium precursor that did not participate in the reaction are removed from the surface of the recycled positive active material, reducing the crystallite size. Furthermore, when the oxidation heat treatment step is divided into two steps, the binder is burned cleanly, and the fluorine (F) and residual lithium generated in the heat treatment step are reduced, reducing the crystallite size, thereby improving the battery characteristics of the recycled positive active material. Based on this, they continued their research and completed the present invention.

[0042] The regenerated positive electrode active material, the regenerating method thereof, and the secondary battery including the same will be described in detail below.

[0043] However, the terms and words used in the present specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as meanings and concepts that correspond to the technical ideas of the present invention, based on the principle that the inventor can appropriately define the concepts of terms to best describe his / her invention. Therefore, it should be understood that the embodiments described in the present specification and the configurations shown in the drawings are merely one embodiment of the present invention and do not fully represent the technical ideas of the present invention, and therefore there are various equivalents and modifications that can replace them, and they can be arranged, substituted, combined, separated or designed in various other configurations.

[0044] All technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs, unless otherwise defined.

[0045] positive electrode active material The positive electrode active material of the present invention is at least one selected from the group consisting of lithium nickel oxide (LNO)-based positive electrode active materials, nickel cobalt manganese (NCM)-based positive electrode active materials, nickel cobalt aluminum (NCA)-based positive electrode active materials, and nickel cobalt manganese aluminum (NCMA)-based positive electrode active materials, and is characterized in that it contains 60 mol % or more of Ni, has a fluorine (F) content of 250 mg / kg or less, and has an average crystal size of 122 nm or less, and in this case, has the effect of being excellent in charge capacity, resistance characteristics, and capacity characteristics.

[0046] The positive electrode active material preferably includes one or more selected from the group consisting of lithium cobalt oxides such as LiCoO2 (hereinafter referred to as "LCO"); lithium manganese oxides such as LiMnO2 or LiMn2O4; lithium iron phosphate compounds such as LiFePO4; lithium nickel cobalt aluminum oxide (NCA); lithium nickel oxides such as LiNiO2; nickel manganese-based lithium composite metal oxides in which a part of nickel (Ni) in the lithium nickel oxide is substituted with manganese (Mn); and NCM-based lithium composite transition metal oxides in which a part of nickel (Ni) in the lithium nickel oxide is substituted with manganese (Mn) and cobalt (Co). In this case, there is an effect of excellent electrochemical performance, resistance characteristics, capacity characteristics, etc.

[0047] Specific examples of the positive electrode active material include the following Chemical Formula 1 [Chemical Formula 1] Li a Ni x Mn y Co z M w O 2+δ (In the Chemical Formula 1, M includes one or more selected from the group consisting of B, W, Al, Ti, and Mg, 1 < a ≤ 1.1, 0 < x < 0.95, 0 < y < 0.8, 0 < z < 1.0, 0 ≤ w ≤ 0.1, -0.02 ≤ δ ≤ 0.02, and x + y + z + w = 1.) The compound represented by this can be included. In this case, there is an effect of excellent electrochemical performance, resistance characteristics, capacity characteristics, etc.

[0048] The positive electrode active material preferably contains 80 mol% or more of Ni, more preferably 81 mol% or more, and still more preferably 81 to 95 mol%. Within this range, there is an effect of excellent charge capacity, resistance characteristics, and capacity characteristics.

[0049] In the present description, the Ni content is not particularly limited as long as it is measured by a method using IC (Ion Chromatography) or the like that is commonly used in the technical field to which the present invention belongs, and as a specific example, it can be measured using an IC-ICP (Inductively Coupled Plasma) analyzer, an IC-ICP-MS analyzer, or an IC-ICP-AEC analyzer.

[0050] For example, the positive electrode active material may have a fluorine (F) content of 250 mg / kg or less, preferably 200 mg / kg or less, and more preferably 10 to 200 mg / kg. Within this range, there is an advantage in that the charge capacity, resistance characteristics, and capacity characteristics are excellent.

[0051] In this description, the fluorine (F) content can be measured using an ICP analyzer. In this case, the measurement can be performed using a general ICP analyzer commonly used in laboratories, and there is no deviation due to the measurement device or method.

[0052] For example, the positive electrode active material may have an average crystal size of 122 nm or less, preferably 115 to 122 nm, and more preferably 120 to 122 nm. Within this range, the smaller crystal size can reduce strain and minimize cycle cracking, which is advantageous in extending the battery life.

[0053] In this description, the average crystal size can be measured by XRD crystal analysis, and there is no deviation due to the measurement device or method. Specifically, the average crystal size can be obtained by placing 5 g of positive electrode active material particles in a holder, irradiating the particles with X-rays, and analyzing the diffraction grating that is generated. The method for obtaining the average crystal size can be obtained from the half-width of the main peak or three or more peaks, which can be considered to correspond to the average crystal size of the primary particles of the positive electrode active material particles.

[0054] For example, the positive electrode active material may have 0.32 wt % or less, preferably 0.31 wt % or less, and more preferably 0.01 to 0.31 wt % of LiOH remaining on the surface. Within this range, there is an advantage in that the charging capacity, resistance characteristics, and capacity characteristics are excellent.

[0055] For example, the positive electrode active material may have 0.19% by weight or less, preferably 0.01 to 0.19% by weight, of Li2CO3 remaining on the surface. Within this range, there is an advantage in that the charging capacity, resistance characteristics and capacity characteristics are excellent.

[0056] For example, the positive electrode active material may have a total of 0.51 wt % or less, preferably 0.50 wt % or less, and more preferably 0.01 to 0.50 wt % of LiOH and Li2CO3 remaining on the surface. Within this range, the positive electrode active material has the advantage of having excellent charging capacity, resistance characteristics, and capacity characteristics.

[0057] In this description, the amount of LiOH and Li2CO3 remaining on the surface of the positive electrode active material can be measured using a pH titrator (T5 manufactured by Mettler Toledo). Specifically, 5 g of the positive electrode active material is dispersed in 100 ml of distilled water, mixed at 300 rpm for 5 minutes, and then filtered to remove the active material. The filtrate is titrated with a 0.1 M HCl solution to measure the change in pH value, and a pH titration curve is obtained. The amount of LiOH and the amount of Li2CO3 remaining in the positive electrode active material are calculated using the obtained pH titration curve.

[0058] In addition, the positive electrode active material of the present invention is at least one selected from the group consisting of lithium nickel oxide (LNO)-based positive electrode active materials, nickel cobalt manganese (NCM)-based positive electrode active materials, nickel cobalt aluminum (NCA)-based positive electrode active materials, and nickel cobalt manganese aluminum (NCMA)-based positive electrode active materials, and is characterized in that it contains 60 mol % or more of Ni, has a fluorine (F) content of 305 mg / kg or less, and has a crystallite size of 139 nm or less, and in this case, has the effect of having excellent capacity characteristics and life characteristics.

[0059] The positive electrode active material preferably contains Ni at 80 mol % or more, more preferably at 81 mol % or more, and even more preferably 81 to 95 mol %. Within this range, the positive electrode active material has the effect of providing excellent charge capacity, resistance characteristics, and capacity characteristics.

[0060] For example, the positive electrode active material may have a fluorine (F) content of 305 mg / kg or less, preferably 250 mg / kg or less, more preferably 200 mg / kg or less, and further preferably 10 to 200 mg / kg. Within this range, there is an advantage in that the capacity characteristics are excellent.

[0061] For example, the positive electrode active material may have an average crystal size of 139 nm or less, preferably 120 to 139 nm, more preferably 130 to 139 nm, even more preferably 133 to 139 nm, and even more preferably 133 to 136 nm. Within this range, the crystal size is small, which has the advantage of reducing distortion and minimizing cycle cracks, thereby extending the battery life.

[0062] As an example, the positive electrode active material may have a surface-residual Li2CO3 content of 0.16 wt % or less, preferably 0.14 wt % or less, more preferably 0.1 wt % or less, and even more preferably 0.01 to 0.1 wt %. Within this range, there is an advantage in that the charging capacity, resistance characteristics, and capacity characteristics are excellent.

[0063] As an example, the positive electrode active material may have 0.32 wt % or less of LiOH remaining on the surface, preferably 0.3 wt % or less, more preferably 0.01 to 0.3 wt %, and even more preferably 0.01 to 0.28 wt %. Within this range, there is an advantage in that the charging capacity, resistance characteristics, and capacity characteristics are excellent.

[0064] As an example, the positive electrode active material may have a total of LiOH and Li2CO3 remaining on the surface of 0.45 wt % or less, preferably 0.42 wt % or less, more preferably 0.40 wt % or less, and even more preferably 0.01 to 0.4 wt %. Within this range, there is an advantage in that the charging capacity, resistance characteristics, and capacity characteristics are excellent.

[0065] For example, the surface of the positive electrode active material may be coated with metal or carbon, and is preferably coated with metal. In this case, the structural stability of the positive electrode active material is improved without chemical and physical changes to the positive electrode active material itself, thereby improving electrochemical properties such as output performance, life characteristics, and capacity, and the physicochemical properties are also improved by the effect of adjusting the amount of residual lithium and reducing the pH due to substitution with a different element on the surface of the positive electrode active material.

[0066] The metal is preferably at least one selected from the group consisting of B, W, Al, Ti, Mg, Ni, Co, Mn, Si, Zr, Ge, Sn, Cr, Fe, V, and Y, more preferably at least one selected from the group consisting of B, W, Al, Ti, and Mg, even more preferably boron (B), tungsten (W), or a mixture thereof, and even more preferably tungsten (W) and boron (B). A specific example is tungsten boride (WB), in which case there is an effect of improving resistance characteristics and life characteristics.

[0067] The coating agent may be contained in an amount of, for example, 0.001 to 0.3 mol % relative to 1 mol % of the metal in the positive electrode active material before the coating treatment, preferably 0.01 to 0.3 mol %, more preferably 0.01 to 0.15 mol %, even more preferably 0.01 to 0.1 mol %, and even more preferably 0.01 to 0.05 mol %. Within this range, the properties of the positive electrode active material itself are maintained as they are, while the structural stability and electrochemical performance are improved.

[0068] The surface coating is preferably performed by coating the surface with a coating agent containing at least one of a metal, an organometallic, and a carbon component in a solid or liquid phase manner, followed by heat treatment at 100 to 1200°C. In this case, there is an effect of improving structural stability and electrochemical performance while maintaining the properties of the positive electrode active material itself.

[0069] The positive electrode active material may preferably be a regenerated positive electrode active material, which has the advantages of being economical and productive.

[0070] Method for regenerating positive electrode active material The method for regenerating a positive electrode active material of the present invention includes the steps of: subjecting a waste positive electrode, in which a positive electrode active material layer containing 60 mol % or more of Ni is formed on a current collector, to an oxidative heat treatment by introducing oxygen to thermally decompose a binder and a conductive material in the positive electrode active material layer, thereby separating the current collector from the positive electrode active material layer and recovering the positive electrode active material in the positive electrode active material layer; primarily washing the recovered positive electrode active material; adding a lithium precursor to the primarily washed positive electrode active material and annealing it; and secondarily washing the annealed positive electrode active material. In this case, fluorine (F) and the lithium precursor that could not participate in the reaction are removed from the surface of the regenerated positive electrode active material, and the crystallite size becomes smaller, thereby achieving excellent charging capacity, resistance characteristics, and capacity characteristics.

[0071] Hereinafter, the method for regenerating the positive electrode active material will be described in detail step by step.

[0072] (a) A step of recovering a positive electrode active material from a waste positive electrode The step (a) of recovering a positive electrode active material from a waste positive electrode according to the present invention may be a step of recovering a positive electrode active material by subjecting a waste positive electrode including a current collector and a positive electrode active material layer coated thereon to an oxidative heat treatment by introducing oxygen, in which case the process is simple and has the effect of completely removing the binder, conductive material, and current collector.

[0073] The discarded positive electrodes may preferably be positive electrodes separated from lithium secondary batteries discarded after use, defective positive electrode sheets generated in the manufacturing process of lithium secondary batteries, or positive electrode scraps, and more preferably positive electrode scraps remaining after punching out positive electrode plates from positive electrode sheets.

[0074] The positive electrode active material layer in step (a) may preferably include a positive electrode active material, a binder, and a conductive material.

[0075] The positive electrode active material may include at least one selected from the group consisting of a lithium nickel oxide (LNO)-based positive electrode active material, a nickel cobalt manganese (NCM)-based positive electrode active material, a nickel cobalt aluminum (NCA)-based positive electrode active material, and a nickel cobalt manganese aluminum (NCMA)-based positive electrode active material.

[0076] The positive electrode active material is preferably one or more selected from the group consisting of lithium cobalt oxides such as LiCoO2 (hereinafter referred to as "LCO"); lithium manganese oxides such as LiMnO2 or LiMn2O4; lithium iron phosphate compounds such as LiFePO4; lithium nickel cobalt aluminum oxide (NCA); lithium nickel oxides such as LiNiO2; nickel manganese-based lithium composite metal oxides in which a part of nickel (Ni) in the lithium nickel oxide is substituted with manganese (Mn); and NCM-based lithium composite transition metal oxides in which a part of nickel (Ni) in the lithium nickel oxide is substituted with manganese (Mn) and cobalt (Co), and can contain 60 mol% or more of Ni, more preferably, it is a nickel manganese-based lithium composite metal oxide, an NCM-based lithium composite transition metal oxide, or a mixture thereof, and in this case, there is an effect of excellent reversible capacity and thermal stability.

[0077] As still another specific example, the positive electrode active material has the following Chemical Formula 1 [Chemical Formula 1] Li a Ni x Mn y Co z M w O 2+δ (In Chemical Formula 1 above, M contains one or more selected from the group consisting of B, W, Al, Ti, and Mg, 1 < a ≤ 1.1, 0 < x < 0.95, 0 < y < 0.8, 0 < z < 1.0, 0 ≤ w ≤ 0.1, -0.02 ≤ δ ≤ 0.02, and x + y + z + w = 1.) It may be a compound represented by

[0078] The positive electrode active material preferably contains 80 mol% or more of Ni, more preferably 81 mol% or more, and still more preferably 81 to 95 mol%. Within this range, there is an effect of excellent initial discharge capacity, output performance, capacity characteristics, and resistance characteristics.

[0079] The conductive material may be, for example, a carbon-based conductive material, and may be preferably carbon black, CNT, or a mixture thereof.

[0080] The binder may be, for example, a polymer binder, preferably polyvinylidene fluoride (PVdF), acrylonitrile-butadiene rubber (NBR), or a mixture thereof, and more preferably polyvinylidene fluoride.

[0081] The oxidation heat treatment temperature may be preferably 400 to 600°C, more preferably 500 to 600°C, and even more preferably 530 to 580°C. Within this range, the current collector does not melt, and the carbon substances in the binder and conductive material react with oxygen to produce CO and CO2 gas and are removed by combustion, which has the advantage that almost all of the binder and conductive material are easily removed without leaving any residue.

[0082] The oxidation heat treatment time may be preferably 10 minutes to 5 hours, more preferably 30 minutes to 5 hours, even more preferably 30 minutes to 2 hours, and even more preferably 30 minutes to 1 hour. Within this range, the current collector is not dissolved and only the binder and the like are removed, which has the advantage that the positive electrode active material can be easily separated from the current collector.

[0083] In this description, the oxidation heat treatment time refers to the time during which the treatment is performed at the oxidation heat treatment temperature, and does not include the time required to reach the heat treatment temperature.

[0084] The oxidation heat treatment may be performed in two steps, for example. Preferably, the first heat treatment is performed at 300 to 450°C, and the second heat treatment is performed at 500 to 650°C. In this case, the process is simple, and the binder, conductive material, and current collector are completely removed, fluorine (F) and residual lithium generated during the pyrolysis process are reduced, and the crystallite size is reduced.

[0085] The primary heat treatment temperature may more preferably be 300 to 430° C., and further preferably 320 to 400° C., and within this range, there is an advantage that the thermal decomposition of the binder and organic substances occurs smoothly.

[0086] The primary heat treatment time may be preferably 10 minutes to 3 hours, more preferably 20 minutes to 160 minutes. Within this range, the current collector is not dissolved and only the binder and the like are removed, which has the advantage that the positive electrode active material can be easily separated from the current collector.

[0087] The secondary heat treatment temperature may be more preferably 510 to 630°C, and further preferably 520 to 630°C. Within this range, there are advantages in that the binder and the conductive material are completely combusted, the amount of fluorine (F) generated during the pyrolysis process and residual lithium are reduced, and the crystal size is made smaller.

[0088] The second heat treatment time may be preferably 10 minutes to 2 hours, more preferably 20 minutes to 100 minutes. Within this range, the current collector is not dissolved and only the binder and the like are removed, which has the advantage that the positive electrode active material can be easily separated from the current collector.

[0089] The total time of the first heat treatment and the second heat treatment may be, for example, 20 minutes to 5 hours, and preferably 30 minutes to 4 hours. Within this range, the current collector is not dissolved and only the binder is removed, so that the positive electrode active material is easily separated from the current collector, fluorine (F) generated during the thermal decomposition process and residual lithium are reduced, and the crystal size is reduced.

[0090] The oxygen used in the oxidation heat treatment may have a purity of, for example, 59% or more, preferably 70% or more, more preferably 80% or more, even more preferably 90% or more, and even more preferably 90 to 99%. Within this range, the binder and conductive material are removed without remaining, and there are advantages in that the stability of Ni in the active material is increased and the crystal size is reduced.

[0091] The oxygen purity % may be volume % or mol %.

[0092] The purity of oxygen described herein is not particularly limited, and can be measured by a measurement method commonly used in the technical field to which the present invention pertains.

[0093] FIG. 1 shows the cathode scrap that is discarded after cutting the cathode plates from the cathode sheet.

[0094] 1, a positive electrode active material layer 20 including a positive electrode active material, a conductive material, a binder, etc. is coated on an aluminum foil 10, which is a long sheet-shaped positive electrode current collector, to produce a positive electrode sheet 30, which is then punched out to a certain size to produce a positive electrode plate 40, and the remaining portion is generated as a positive electrode scrap 50. The punching is one method for cutting the positive electrode sheet.

[0095] In addition, the positive electrode active material layer 20 is formed by coating a slurry, in which a positive electrode active material, a conductive material, a binder, a solvent, etc. are mixed, on the aluminum foil 10. Since the slurry is very sensitive to environmental factors such as temperature, it is very difficult to determine the coating conditions. Therefore, waste positive electrode sheets are generated until the conditions for manufacturing a positive electrode sheet 30 of desired quality through predetermined tests are found.

[0096] For reference, in the following examples, scrap positive electrodes were used as waste positive electrodes.

[0097] (b) A step of first washing the recovered positive electrode active material The method for regenerating a positive electrode active material of the present invention includes (b) a step of primarily washing the recovered positive electrode active material. In this case, there is an advantage that metal fluorides such as LiF that may be present on the surface of the regenerated positive electrode active material are removed and the surface is modified.

[0098] During the oxidation heat treatment, CO2 and H2O from the binder and conductive material in the active material layer may react with the lithium on the surface of the active material to form Li2CO3 and LiOH, or fluorine (F) present in the binder such as PVdF may react with the metal elements that make up the positive electrode active material to form LiF or metal fluorides. If LiF or metal fluorides remain, the battery characteristics will deteriorate when the active material is reused.

[0099] In the first washing, for example, water or an aqueous solution of a basic lithium compound may be used as a washing liquid, and more preferably, water may be used.

[0100] The water may be preferably distilled water or deionized water, and more preferably distilled water. In this case, metal fluorides such as LiF, which tend to remain on the surface of the positive electrode active material, are removed, thereby providing an excellent effect of modifying the surface.

[0101] The basic lithium compound aqueous solution may preferably contain more than 0 wt% to 15 wt% or less of lithium compound, more preferably more than 0 wt% to 10 wt% or less of lithium compound, in which case metal fluorides such as LiF that tend to remain on the surface of the positive electrode active material are removed, and the surface is not only modified, but also has the advantage of not dissolving transition metals present in the positive electrode active material, and replenishing lithium that may dissolve during the cleaning process. If the lithium compound is contained in an amount greater than the above range, an excess amount of LiOH may remain on the surface of the active material even after cleaning, which may affect the subsequent annealing process.

[0102] The lithium compound may be, for example, LiOH, LiNO3, or a mixture thereof, and preferably LiOH. In this case, there is an effect of removing fluorine (F) on the surface of the positive electrode active material and lithium precursors that could not participate in the reaction.

[0103] In the first washing, the weight ratio of the recovered positive electrode active material to the washing solution may be, for example, 1:1 to 1:40, preferably 1:1 to 1:35, more preferably 1:1 to 1:30, and further preferably 1:1 to 1:20. Within this range, there is an advantage that metal fluorides such as LiF are effectively removed.

[0104] The primary washing can be performed, for example, by immersing the recovered positive electrode active material in a washing solution. The immersion can be performed, for example, for one week, preferably within one day, more preferably within one hour, and further preferably for 10 minutes to 50 minutes. If the immersion time is one week or longer, there is a risk of a decrease in capacity due to excessive elution of lithium.

[0105] The first cleaning may preferably include stirring the positive electrode active material while immersed in the cleaning solution. In this case, the cleaning process can be performed quickly, thereby suppressing the dissolution of lithium and shortening the process time.

[0106] The first washing may preferably include a step of filtering the positive electrode active material and the washing solution after washing, and a step of drying the solid positive electrode active material obtained after the filtration, in which case metal fluorides such as LiF may be more effectively removed.

[0107] The filtration may preferably be reduced pressure filtration using a filter.

[0108] The drying may be carried out at a temperature of preferably 100 to 500°C, more preferably 120 to 400°C, further preferably 120 to 300°C, and even more preferably 120 to 200°C.

[0109] The drying may preferably be carried out under vacuum.

[0110] In the present description, the vacuum drying is not particularly limited as long as it is vacuum drying that is commonly performed in the technical field to which the present invention belongs.

[0111] (c) adding a lithium precursor to the first washed positive electrode active material and annealing it; The method for regenerating a positive electrode active material of the present invention includes (c) a step of adding a lithium precursor to the primarily washed positive electrode active material and annealing the same. In this case, the crystal structure of the positive electrode active material is restored, thereby having the effect of restoring or further improving the characteristics of the reused active material to the level of a new active material that has never been used.

[0112] The annealing step (c) may be preferably a step of adding a lithium precursor to the primarily washed cathode active material and annealing the material in air or oxygen (O2) at 400 to 1000°C, preferably a step of annealing the material in air at 400 to 1000°C. In this case, the battery characteristics of the regenerated cathode active material can be improved by improving the crystallinity, such as by increasing the crystallinity or recovering the crystal structure.

[0113] The lithium precursor may preferably be one or more selected from the group consisting of LiOH, Li2CO3, LiNO3 and Li2O.

[0114] The lithium precursor can be added preferably in an amount that is at least the amount of lithium that is reduced from the molar ratio of lithium in the positive electrode active material in step (a) based on the amount of lithium in the recovered positive electrode active material, and more preferably in an amount of lithium that is 0.0001 to 0.2 molar ratio relative to the molar ratio of lithium in the positive electrode active material in step (a). Within this range, the lithium that is insufficient in the regenerated positive electrode active material is replenished, and the crystallinity is improved, such as by increasing the crystallinity or recovering the crystal structure, thereby improving the battery characteristics of the regenerated positive electrode active material.

[0115] The lithium precursor may be added in an amount of preferably 1 to 40 mol%, more preferably 1 to 15 mol%, and even more preferably 1 to 10 mol%, when the total amount of lithium in the raw material positive electrode active material used in the positive electrode active material layer is 100 mol%. Within this range, no residual precursor that may increase resistance remains in the regenerated positive electrode active material, which is very useful for improving battery characteristics.

[0116] The annealing temperature can be adjusted within a limited range depending on the melting point of the lithium precursor. For example, since the melting point of LiCO3 is 723°C, annealing can be performed preferably at 700 to 900°C, more preferably at 710 to 780°C. Since the melting point of LiOH is 462°C, annealing can be performed preferably at 400 to 600°C, more preferably at 450 to 480°C. Within this range, the crystal structure is restored, resulting in excellent output performance of the battery.

[0117] The annealing temperature may preferably be a temperature exceeding the melting point of the lithium precursor, but if it exceeds 1000°C, thermal decomposition of the positive electrode active material may occur, resulting in a decrease in battery performance, and therefore, the annealing temperature is preferably 1000°C or less.

[0118] In the (c) annealing step, the method of adding the lithium precursor to the first washed positive electrode active material may be to add the lithium precursor in a solid or liquid phase after drying the washed positive electrode active material. As another example, a lithium precursor solution may be added to the washed positive electrode active material and spray-dried to perform drying and addition of the lithium precursor in one step. In this case, there are advantages in that particle aggregation due to drying is reduced and the process of mixing the lithium precursor in a solid phase can be omitted, and the spray drying has the advantage that the product is produced in the form of a powder rather than a lump.

[0119] The lithium precursor solution may be, for example, a lithium compound that is soluble in an aqueous solution or an organic solvent.

[0120] (d) Secondary washing of the annealed positive electrode active material The method for regenerating a positive electrode active material of the present invention includes a step (d) of secondly washing the annealed positive electrode active material. In this case, the lithium precursor that is unable to participate in the reaction and exists on the surface of the positive electrode active material in the form of LiOH, Li2CO3, etc. after the addition of the lithium precursor is removed, which has the advantage of preventing the deterioration of battery performance and the generation of gas due to the subsequent reaction between the remaining lithium precursor and the electrolyte.

[0121] The second cleaning may be performed using water as a cleaning solution, for example, and preferably distilled water or deionized water. In this case, lithium precursors such as LiOH, Li2CO3, etc. that tend to remain due to excessive lithium added in the (c) annealing step can be effectively removed.

[0122] The second washing may preferably include a step of mixing the annealed positive electrode active material and a washing solution in a weight ratio of 1:1 to 1:20, followed by filtering, and a step of drying the solid positive electrode active material obtained after the filtration. In this case, there is an effect that lithium precursors such as LiOH, Li2CO3, etc. that tend to remain due to excessive lithium added in the (c) annealing step can be effectively removed.

[0123] The annealed active material and the cleaning solution may be mixed in a weight ratio of preferably 1:1 to 1:20, more preferably 1:1 to 1:15, further preferably 1:1 to 1:10, and even more preferably 1:1 to 1:5. In this case, there is an effect that lithium precursors such as LiOH, Li2CO3, etc. that tend to remain due to excessive lithium added in the annealing step (c) are effectively removed.

[0124] The second washing may include a step of mixing the annealed positive electrode active material with a washing solution, followed by filtering, and a step of drying the solid positive electrode active material obtained after the filtration. In this case, it is possible to achieve excellent charging capacity, resistance characteristics, and capacitance characteristics.

[0125] (e) A step of surface-coating the second washed positive electrode active material to obtain a reusable positive electrode active material. The method for regenerating a positive electrode active material of the present invention includes a step (e) of surface-coating the second washed positive electrode active material to obtain a reusable positive electrode active material, which has the effect of improving structural stability and electrochemical performance while maintaining the properties of the positive electrode active material itself.

[0126] The surface coating is preferably performed by coating the surface with a coating agent containing at least one of a metal, an organometallic, and a carbon component in a solid or liquid phase manner, followed by heat treatment at 100 to 1200°C. In this case, there is an effect of improving structural stability and electrochemical performance while maintaining the properties of the positive electrode active material itself.

[0127] The metal-containing coating agent is preferably a coating agent containing one or more selected from the group consisting of B, W, Al, Ti, Mg, Ni, Co, Mn, Si, Zr, Ge, Sn, Cr, Fe, V, and Y, more preferably a coating agent containing one or more selected from the group consisting of B, W, Al, Ti, and Mg, still more preferably a coating agent containing boron (B), tungsten (W) or a mixture thereof, and even more preferably a coating agent containing tungsten (W) and boron (B). A specific example is a coating agent containing tungsten boride (WB), in which case there is an effect of improving resistance characteristics and life characteristics.

[0128] The coating agent containing the metal may be, for example, an oxide or an acid containing the metal as an element in its molecule.

[0129] The coating agent containing the organometallic is not particularly limited as long as it is a coating agent that is commonly used in the technical field to which the present invention belongs and contains an organometallic compound containing the metal. A specific example of the coating agent may be a metal alkoxide.

[0130] The carbon component-containing coating agent is not particularly limited as long as it is a carbon component-containing coating agent commonly used in the technical field to which the present invention pertains, and a specific example thereof may be a sugar such as sucrose.

[0131] For example, the coating agent may be contained in an amount of 0.001 to 0.3 mol %, preferably 0.01 to 0.3 mol %, more preferably 0.01 to 0.15 mol %, even more preferably 0.01 to 0.1 mol %, and even more preferably 0.01 to 0.05 mol %, based on the components excluding the solvent that are actually coated on the surface of the positive electrode active material, relative to 1 mol % of the metal in the positive electrode active material before the coating treatment. Within this range, there is an effect of improving structural stability and electrochemical performance while maintaining the properties of the positive electrode active material itself.

[0132] The heat treatment temperature may be preferably 100 to 1000°C, more preferably 200 to 1000°C, and even more preferably 200 to 500°C. Within this range, there is an effect of preventing performance degradation due to thermal decomposition of the positive electrode active material and improving structural stability and electrochemical performance.

[0133] The heat treatment time is preferably 1 to 16 hours, more preferably 3 to 7 hours. Within this range, the properties of the positive electrode active material itself are maintained as they are, while the structural stability and electrochemical performance are improved.

[0134] The coating method is not particularly limited as long as it is a coating method commonly used in the technical field to which the present invention belongs, and examples thereof include a liquid phase method in which a liquid coating agent is prepared and mixed with a positive electrode active material, a mechanochemical method using high mechanical energy of ball milling, a fluidized bed coating method, a spray drying method, a precipitation method in which a coating agent in an aqueous solution state is precipitated on the surface of the positive electrode active material, a method utilizing a reaction between a gas-phase coating agent and a positive electrode active material, a sputtering method, etc.

[0135] The metal, organometallic and carbon components may be, for example, spherical, plate-like, angular or needle-like, and such shapes can be adjusted by changing process conditions during the manufacturing process. The definition of each shape is not particularly limited as long as it follows the definition generally accepted in the technical field to which the present invention belongs.

[0136] The coating agent preferably has an average diameter of 1 to 1000 nm and a specific surface area of ​​10 to 100 m 2 / g, and more preferably, the average diameter is 10 to 100 nm and the specific surface area is 20 to 100 m 2 / g, and within this range, the positive electrode active material can be uniformly attached to the surface thereof to impart structural stability to the positive electrode active material, thereby improving the problems of deterioration in life characteristics and electrochemical performance caused by lattice deformation and collapse of the crystal structure of the positive electrode active material.

[0137] In this description, the average diameter can be measured by a measurement method commonly used in the technical field to which the present invention belongs, for example, by using a laser diffraction method. Specifically, particles of the positive electrode active material are dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measurement device such as Microtrac MT 3000. Ultrasonic waves of about 28 kHz are irradiated at an output of 60 W, and the average particle size (D50) based on 50% of the particle size distribution in the measurement device can be calculated.

[0138] In this description, the specific surface area can be measured by a measurement method commonly used in the technical field to which the present invention pertains, for example, by the BET (Brunauer-Emmett-Teller) method, and specifically, it can be calculated from the amount of nitrogen gas adsorbed at liquid nitrogen temperature (77K) using a BELSORP-mino II from BEL Japan.

[0139] The positive electrode active material produced by the method for regenerating a positive electrode active material of the present invention may have a fluorine (F) content of, for example, 250 mg / kg or less, preferably 200 mg / kg or less, and more preferably 10 to 200 mg / kg. Within this range, the positive electrode active material has the advantage of being excellent in charge capacity, resistance characteristics, and capacity characteristics.

[0140] For example, the positive electrode active material may have 0.32 wt % or less, preferably 0.31 wt % or less, and more preferably 0.01 to 0.31 wt % of LiOH remaining on the surface. Within this range, there is an advantage in that the charging capacity, resistance characteristics, and capacity characteristics are excellent.

[0141] For example, the positive electrode active material may have 0.19% by weight or less, preferably 0.01 to 0.19% by weight, of Li2CO3 remaining on the surface. Within this range, there is an advantage in that the charging capacity, resistance characteristics and capacity characteristics are excellent.

[0142] For example, the positive electrode active material may have a total of 0.51 wt % or less, preferably 0.50 wt % or less, and more preferably 0.01 to 0.50 wt % of LiOH and Li2CO3 remaining on the surface. Within this range, the positive electrode active material has the advantage of having excellent charging capacity, resistance characteristics, and capacity characteristics.

[0143] For example, the positive electrode active material may have an average crystal size of 122 nm or less, preferably 115 to 122 nm, and more preferably 120 to 122 nm. Within this range, the smaller crystal size can reduce distortion and minimize cycle cracks, which is advantageous in extending the battery life.

[0144] In addition, the positive electrode active material produced by the method for regenerating a positive electrode active material of the present invention may have a fluorine (F) content of, for example, 305 mg / kg or less, preferably 250 mg / kg or less, more preferably 200 mg / kg or less, and even more preferably 10 to 200 mg / kg. Within this range, the positive electrode active material has the advantage of having excellent capacity characteristics.

[0145] As an example, the positive electrode active material may have a surface-residual Li2CO3 content of 0.16 wt % or less, preferably 0.14 wt % or less, more preferably 0.10 wt % or less, and even more preferably 0.01 to 0.10 wt %. Within this range, there is an advantage in that the charging capacity, resistance characteristics, and capacity characteristics are excellent.

[0146] As an example, the positive electrode active material may have a surface-residual LiOH content of 0.32% by weight or less, preferably 0.30% by weight or less, more preferably 0.01 to 0.30% by weight, and even more preferably 0.01 to 0.28% by weight. Within this range, the positive electrode active material has the advantage of having excellent charging capacity, resistance characteristics, and capacity characteristics.

[0147] As an example, the positive electrode active material may have a total of LiOH and Li2CO3 remaining on the surface of 0.45% by weight or less, preferably 0.42% by weight or less, more preferably 0.40% by weight or less, and even more preferably 0.01 to 0.40% by weight. Within this range, there is an advantage in that the charging capacity, resistance characteristics, and capacity characteristics are excellent.

[0148] For example, the positive electrode active material may have an average crystal size of 139 nm or less, preferably 120 to 139 nm, more preferably 130 to 139 nm, even more preferably 133 to 139 nm, and even more preferably 133 to 136 nm. Within this range, the crystal size is small, which has the advantage of reducing distortion and minimizing cycle cracks, thereby extending the battery life.

[0149] FIG. 7 is a flow chart of a process for regenerating a positive electrode active material according to one embodiment of the present invention.

[0150] 7, first, cathode scraps are prepared as waste cathodes (step S10). For example, NCM-based lithium transition metal composite oxide, carbon black, and polyvinylidene fluoride are mixed with NMP (N-methyl pyrrolidone) to produce a slurry, which is coated on aluminum foil and dried in a vacuum oven at about 120° C. to produce a cathode sheet. After punching out a cathode plate of a certain size, the remaining cathode scraps can be prepared.

[0151] In particular, the present invention can be effectively applied to waste positive electrodes in which a positive electrode active material containing 60 mol % or more of Ni has been used, preferably a positive electrode active material containing 80 mol % or more of Ni, more preferably a positive electrode active material containing 81 mol % or more of Ni, and even more preferably a positive electrode active material containing 81 to 95 mol % of Ni.

[0152] The positive electrode scrap has a positive electrode active material layer on an aluminum foil, and the positive electrode active material layer has a structure in which the positive electrode active material and the conductive material are bound by the binder after the solvent is evaporated, and therefore, when the binder is removed, the positive electrode active material is separated from the aluminum foil.

[0153] Next, the prepared cathode scrap is crushed into an appropriate size (step S20). Here, crushing includes cutting or shredding the cathode scrap into a size that is easy to handle. As a specific example, the crushed cathode scrap may have a size of 1 cm x 1 cm. The crushing may be performed using various dry grinding equipment such as a hand mill, a pin mill, a disc mill, a cutting mill, or a hammer mill, or may be performed using a high-speed cutter to increase productivity.

[0154] The crushing may be performed or the size of the pieces may be determined in consideration of the handling of the cathode scrap and the properties required for equipment used in subsequent processes. For example, when equipment capable of continuous processing is used, the cathode scrap should have good fluidity and therefore should be crushed into smaller pieces.

[0155] Next, oxygen is introduced into the positive electrode scrap to perform an oxidation heat treatment, and the positive electrode active material is recovered (step S30). Here, the heat treatment is performed to thermally decompose the binder in the active material layer.

[0156] The oxidation heat treatment is preferably performed with oxygen having a purity of 80% or more, and more preferably with oxygen having a purity of 90% or more. In this case, the stability of Ni can be ensured in the waste cathode using a high-nickel (High-Ni) cathode material, and the binder and conductive material are cleanly removed. When the heat treatment is performed in a reducing gas or inert gas atmosphere, the binder and conductive material are carbonized without being thermally decomposed. When carbonized, the carbon component remains on the surface of the cathode active material, which reduces the performance of the reused cathode active material. In contrast, when the oxidation heat treatment is performed by introducing oxygen, the carbon component in the binder and conductive material reacts with the oxygen and disappears as gas such as CO and CO2, so that both the binder and conductive material are removed.

[0157] The oxidation heat treatment is preferably carried out at 300 to 650°C, specifically at 590°C. If the temperature is less than 300°C, it is difficult to remove the binder, making it impossible to separate the current collector. If the temperature exceeds 650°C, the current collector melts, causing a problem that it is impossible to separate the current collector.

[0158] The oxidation heat treatment is preferably performed at a temperature increase rate of 1 to 20° C. / min, more preferably 3 to 10° C. / min, and specifically 5° C. / min. Within this range, the heat treatment can be performed without putting strain on the heat treatment equipment, and there are advantages in that no thermal shock is caused to the cathode scrap.

[0159] The oxidation heat treatment can be carried out for a period of time that allows the binder to be sufficiently pyrolyzed, for example, and is preferably carried out for 30 minutes or more, and more preferably for 30 minutes to 5 hours, and specifically for about 30 minutes. Within this range, the binder is sufficiently pyrolyzed, and there is an effect of excellent pyrolysis efficiency.

[0160] In this description, a high-nickel positive electrode active material refers to a positive electrode active material that contains 60 mol % or more of nickel.

[0161] The oxidation heat treatment step may be preferably divided into two steps, and more preferably, a first oxidation heat treatment may be performed at 300 to 430°C, followed by a second heat treatment at 510 to 630°C. In this case, the two-step heat treatment has the advantage that fluorine (F) and residual lithium generated during the thermal decomposition process are reduced, resulting in a smaller crystal size.

[0162] The primary oxidation heat treatment may more preferably be performed at a temperature of 320 to 400°C.

[0163] The primary heat treatment may be performed for a time period of preferably 10 minutes to 3 hours, and more preferably 20 minutes to 160 minutes.

[0164] The secondary oxidation heat treatment temperature may more preferably be 520 to 630°C. Within this range, the binder and the conductive material are sufficiently pyrolyzed, and the amount of fluorine (F) and residual lithium generated during the pyrolysis process is reduced, resulting in a smaller crystal size.

[0165] The second heat treatment time may be preferably 10 minutes to 2 hours, more preferably 20 minutes to 100 minutes. Within this range, the current collector is not dissolved and only the binder and the like are removed, which has the advantage that the positive electrode active material can be easily separated from the current collector.

[0166] The oxidation heat treatment is preferably performed at a temperature increase rate of 1 to 20° C. / min, more preferably 3 to 10° C. / min, and specifically 5° C. / min. Within this range, the heat treatment can be performed without putting strain on the heat treatment equipment, and there are advantages in that no thermal shock is caused to the cathode scrap.

[0167] The oxidation heat treatment may be carried out using various types of furnaces, for example, a box-type furnace, or, in consideration of productivity, a rotary kiln capable of continuous treatment.

[0168] After the oxidation heat treatment, the material can be cooled slowly or rapidly in air.

[0169] Next, the recovered positive electrode active material is subjected to a primary washing (step S40).

[0170] Since fluorine (F) and lithium remain on the surface of the positive electrode active material recovered in the oxidation heat treatment step S30, a cleaning step is required to remove them.

[0171] In the first washing step, the recovered positive electrode active material is washed with water or a basic aqueous solution of a lithium compound, preferably with water, as a washing liquid.

[0172] The water may preferably be distilled or deionized water, which has the advantage that metal fluorides such as LiF are removed, thereby modifying the surface.

[0173] The basic lithium compound aqueous solution contains lithium compounds in an amount of more than 0% by weight to less than 15% by weight, preferably more than 0% by weight to less than 10% by weight, and in this case, metal fluorides such as LiF that may be present on the surface of the regenerated positive electrode active material are removed, thereby improving the surface. If the lithium compound exceeds 15% by weight, an excessive amount of lithium compounds such as LiOH and LiNO3 may remain on the surface of the positive electrode active material even after washing, which may affect the subsequent annealing process.

[0174] The lithium compound may specifically be LiOH.

[0175] The first washing can be performed by immersing the recovered active material in the washing solution. After immersion, washing can be performed within one week, preferably within one day, and more preferably within one hour. If washing is performed for more than one week, there is a risk of a decrease in capacity due to excessive elution of lithium. Therefore, it is preferable to perform the washing within one hour. The first washing includes immersing the active material in the washing solution and stirring the material while immersed. It is preferable to perform stirring in parallel as much as possible. When using an aqueous lithium compound solution as the washing solution, if only immersion is performed without stirring, the washing process will be slow, which may cause lithium to dissolve. If stirring is performed in parallel, the process time can be minimized, so it is preferable to perform stirring at the same time as impregnation with the aqueous lithium compound solution.

[0176] After the first washing, filtering and drying in air in an oven (convection type) may be further performed.

[0177] In the first washing, the weight ratio of the recovered positive electrode active material to the washing solution may be 1:1 to 1:40, preferably 1:1 to 1:35, and more preferably 1:1 to 1:30. Within this range, there is an advantage that metal fluorides such as LiF can be effectively removed.

[0178] The first washing may preferably include filtering the positive electrode active material and the washing solution after washing, and drying the positive electrode active material in solid form obtained after the filtration.

[0179] The filtration is preferably reduced pressure filtration using a filter, and the drying is preferably vacuum drying at 120 to 140°C.

[0180] Next, a lithium precursor is added to the primarily washed positive electrode active material, and annealing is performed (step S50).

[0181] It is important that the annealing step S50 involves adding a lithium precursor to the primarily washed positive electrode active material and annealing it. During the previous steps S30 and S40, lithium may be lost in the positive electrode active material, and this loss of lithium is replenished in step S50.

[0182] Moreover, in step S50, the crystal structure of the active material is restored through annealing, thereby restoring or even improving the properties of the reused active material to the level of a new active material that has never been used.

[0183] During the steps S30 and S40, a deformed structure may occur on the surface of the positive electrode active material. For example, in the active material that is an NCM-based lithium transition metal composite oxide, Ni may be converted into rock salt [NiCO3·2Ni(OH)2)H2O] by moisture in step S40, forming a spinel structure. If a battery is manufactured in this state, the battery characteristics may deteriorate, such as a decrease in capacity. In the present invention, the crystal structure is restored through step S50. For example, the positive electrode active material that is an NCM-based lithium transition metal composite oxide is restored to a hexagonal crystal structure. This allows the initial characteristics to be restored or improved to a level similar to that of an unused positive electrode active material.

[0184] The lithium precursor in step S50 may be any one or more of LiOH, Li2CO3, LiNO3, and Li2O.

[0185] The method of adding the lithium precursor to the first washed active material may be to add the lithium precursor in a solid or liquid phase after drying the washed positive electrode active material. As another example, a lithium precursor solution may be added to the washed positive electrode active material, and the material may be spray-dried, thereby performing drying and addition of the lithium precursor in one step. The lithium precursor solution may be a lithium compound that is soluble in an aqueous solution or an organic solvent.

[0186] If the surface modification process by the first cleaning is immediately dried in an oven, the positive electrode active material particles may aggregate and become lumps. In order to mix the lithium precursor with the aggregated particles, grinding of the lumps may be required, which may make the process complicated and difficult to perform continuously. In addition, especially in the case of NCM-based positive electrode active materials, if the lithium precursor is mixed with the powder and milled in a water-containing state, the positive electrode active material absorbs water and agglomeration occurs severely. Therefore, if the positive electrode active material is mixed with the lithium precursor solution after the first cleaning, dispersed, and spray-dried, the aggregation of particles due to drying and the trouble of mixing the solid-phase lithium precursor can be eliminated. In other words, spray drying has the advantage of producing the product in the form of powder rather than lumps.

[0187] During spray drying, the lithium precursor solution is dried immediately after spraying, and the lithium precursor components are coated or contacted with the surface of the positive electrode active material. At this time, when the lithium precursor solution, which is the solvent, dries, the particles aggregate due to capillary force, which has the advantage of controlling the particle size. In the case of positive electrode scraps made from electrodes, the surface particles may be pressed and cracked or broken during the rolling process. In particular, compared to LCO, NCM-based positive electrode active materials have a problem in that the particles are more likely to crack due to rolling during the formation of the electrode, and therefore the recovered positive electrode active material contains more small particles than unused positive electrode active materials, resulting in non-uniform particle size.

[0188] In addition, NCM-based active materials include large particles that are formed by aggregating primary particles having a size of tens to hundreds of nm into secondary particles. In a positive electrode made from such an active material, the secondary particles may be cracked and turned into primary particles during rolling to adjust the porosity within the electrode, or may be turned into small particles that are larger in size but smaller than the large particles.

[0189] The more particles are broken by rolling, the greater the specific surface area of ​​the active material becomes. Therefore, in the case of reused active materials obtained from rolled electrodes, there may be problems in that the slurry properties, electrode adhesive strength, and electrode performance may be adversely affected when reused.

[0190] As described above, the surface of the positive electrode active material is coated with the lithium precursor through the spray drying step, and the positive electrode active material is obtained by adjusting the particles. The addition of the lithium precursor, granulation, and drying are performed in one step, which has the effect of simplifying the process. In addition, spray drying is unique in that it is not a means for simply obtaining an active material, but a means for re-granulating particles that have already been used and broken by rolling, etc.

[0191] In addition, the cathode active material particles washed in the previous step are mixed and dispersed in a lithium precursor solution of a certain concentration, so that washing and spray drying can be performed as continuous processes. Thus, the cathode active material regeneration method according to the present embodiment has the advantage that the process is continuous, and the coating, drying, and granulation of the lithium precursor (in other words, re-adjustment of the particles) are performed simultaneously in one step.

[0192] In addition, since lithium is lost in the positive electrode active material during the steps S30 and S40, the amount of lithium lost is replenished in step S50. Furthermore, since a deformed structure (e.g., Co3O4 in the case of an LCO active material) may occur on the surface of the positive electrode active material during the steps, the crystal structure of the positive electrode active material is restored through annealing in step S50, improving the battery characteristics of the regenerated positive electrode active material and restoring it to the level of a fresh positive electrode active material. Here, "fresh" is the opposite concept of "regenerated" and means something that has been made for the first time, and is the same word as "raw material" used in the examples.

[0193] As the lithium precursor, LiOH is specifically used.

[0194] The lithium precursor is preferably added in an amount at least equal to the molar ratio of the lost lithium, compared to the molar ratio of lithium to other metals in the new positive electrode active material used in the positive electrode active material layer. Addition of an amount of lithium precursor that is excessively greater than the amount of lost lithium leaves unreacted lithium precursor in the regenerated positive electrode active material, which increases resistance, so it is necessary to add an appropriate amount of lithium precursor. For example, when the molar ratio of lithium to other metals in the new positive electrode active material is 1, the lithium precursor may be added in an amount such that the lithium is in a molar ratio of 0.001 to 0.4, preferably, the lithium precursor may be added in an amount such that the lithium is in a molar ratio of 0.01 to 0.2.

[0195] As a specific example, when the lithium precursor is added in a molar ratio (based on lithium metal) of 0.09 to 0.1, which is the ratio of the lithium content lost in the new positive electrode active material based on the results of ICP analysis, the capacity improvement effect is shown to the same level as that of the new positive electrode active material. Here, the results of ICP analysis have an error value of about ±0.02.

[0196] Specifically, the lithium precursor may be added in an amount of lithium corresponding to 1 mol% to 40 mol%, more preferably 1 to 15 mol%, and even more preferably 1 to 10 mol%, when the total amount of lithium in the raw material positive electrode active material used in the positive electrode active material layer is 100 mol%.

[0197] The annealing is carried out in air at a temperature of, for example, 400 to 1000° C., preferably 600 to 900° C., and this temperature must be modified within a limited range depending on the type of lithium precursor.

[0198] The annealing temperature is preferably a temperature exceeding the melting point of the lithium precursor. However, at temperatures exceeding 1000°C, thermal decomposition of the positive electrode active material occurs, resulting in a decrease in performance, so the temperature should not exceed 1000°C. For example, when Li2CO3 is used as the lithium precursor, the annealing temperature is suitably 700 to 900°C, more preferably 710 to 780°C, and most preferably 750 to 780°C. When LiOH is used as the lithium precursor, the annealing temperature is suitably 400 to 600°C, more preferably 450 to 480°C, and most preferably 470 to 480°C.

[0199] The annealing time is, for example, 1 hour or more, preferably 15 hours or less, and more preferably 4 to 6 hours. If the annealing time is long, the crystal structure may be sufficiently restored, but even if the annealing time is long, the performance is not significantly affected. In this case, the annealing equipment may be the same as or similar to that of the heat treatment step S30.

[0200] Next, the annealed positive electrode active material is subjected to a second cleaning (step S60).

[0201] The lithium precursors that did not participate in the reaction in the annealing step S50 remain on the surface of the positive electrode active material in the form of LiOH and Li2CO3, so a residual lithium removal process is required to remove them. In particular, high-nickel (High-Ni) positive electrode active material requires an excess amount of Li due to the cation mixing phenomenon, which makes it easy for lithium impurities such as lithium carbonate (Li2CO3) to remain on the surface, and these impurities must be thoroughly removed because they may later react with the electrolyte to reduce battery performance and generate gas.

[0202] In the second washing, distilled water can be preferably used as the washing liquid. In this case, there is an advantage that it is safe and inexpensive, and does not dissolve the transition metal present in the positive electrode active material.

[0203] The washing may include a step of mixing the annealed cathode active material and a washing solution in a weight ratio of 1:1 to 1:10, more preferably in a weight ratio of 1:1 to 1:5, followed by filtering, and a step of drying the solid cathode active material obtained after the filtration. In this case, there is an effect that lithium precursors such as LiOH, Li2CO3, etc. that are likely to remain due to the excessive lithium added in step S50 are effectively removed.

[0204] The annealed positive electrode active material and the distilled water are preferably mixed by stirring, which may be, but is not limited to, mechanical stirring or ultrasonic stirring.

[0205] The filtration is preferably reduced pressure filtration using a filter, and the drying is preferably vacuum drying at 120 to 140°C.

[0206] Next, as an optional step, the washed positive electrode active material can be surface coated (step S70).

[0207] The surface coating, for example, is performed by coating the surface with a coating agent containing a metal, an organic metal, or a carbon component in a solid or liquid phase manner, followed by heat treatment. If the heat treatment temperature is too low, the desired surface protective layer made of a different metal is not formed, and if the heat treatment temperature is too high, the performance of the battery is reduced due to thermal decomposition of the positive electrode active material.

[0208] Specifically, when a metal oxide or acid containing B, W, BW, etc. is coated on a washed positive electrode active material and then heat-treated, a surface protection layer such as a lithium boron oxide layer is formed on the surface of the positive electrode active material.

[0209] The solid or liquid phase method of the surface coating may be, for example, a method such as mixing, milling, spray drying, or grinding.

[0210] If the molar ratio of lithium:other metals in the positive electrode active material is set to 1:1 in the annealing step S50, the lithium in the positive electrode active material reacts with the coating agent in the surface coating step S70, and the molar ratio of lithium:other metals in the positive electrode active material becomes less than 1:1, and such a regenerated positive electrode active material cannot fully demonstrate 100% of the battery capacity. However, if the lithium precursor is excessively added in the annealing step S50 so that it is contained in an amount of 0.0001 to 0.1 molar ratio more than the other metals in the positive electrode active material, a surface protective layer is formed in the surface coating step S70, and the molar ratio of lithium:other metals in the positive electrode active material becomes 1:1, and thus the capacity reduction of the battery does not occur.

[0211] secondary battery The secondary battery of the present invention includes the positive electrode active material. In this case, fluorine (F) and lithium precursor that could not participate in the reaction are removed from the surface of the positive electrode active material, and the crystallite size is reduced, resulting in excellent charging capacity, resistance characteristics, and capacity characteristics. In addition, since no acid or organic solvent is used in the recovery and regeneration process of the positive electrode active material, the secondary battery is environmentally friendly. In particular, since the initial water washing process is omitted, the secondary battery has excellent economic efficiency and productivity.

[0212] The secondary battery of the present invention may include all of the above-mentioned positive electrode active material and the regeneration method thereof, and therefore, a duplicate description thereof will be omitted here.

[0213] Below, preferred examples are presented to aid in understanding the present invention. However, the following examples are merely illustrative of the present invention, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical spirit of the present invention. Naturally, such changes and modifications also fall within the scope of the appended claims.

[0214] [Example] Example 1 The cathode scraps discarded after punching out the cathode plates (current collector: aluminum foil, cathode active material: NCM-based lithium composite transition metal oxide with nickel content of 85 mol%) were crushed and oxidized at 590°C for 30 minutes in 95% pure oxygen to remove the binder and conductive material, and the cathode active material was separated from the current collector and then recovered. Here, the temperature was raised at a rate of 5°C / min until the heat treatment temperature was reached, and oxygen (O2) was supplied at 10 L / min.

[0215] The recovered positive electrode active material was immersed in distilled water and stirred at the same time for the primary washing. At this time, the weight ratio of the recovered positive electrode active material to distilled water was 1:30, and the mixture was stirred at 500 rpm for 10 minutes, and then the active material was removed by vacuum filtration using a filter. The positive electrode active material that had been primarily washed had a reduction of 0.11 moles based on 1 mole of lithium in the positive electrode active material compared to the raw material.

[0216] The first-washed positive electrode active material was dried overnight at 100° C., and then LiOH was added as a lithium precursor, followed by annealing in air at 750° C. for 5 hours. Here, air was supplied at 3 L / min. The lithium precursor was added in an amount equivalent to 18 mol% when the total amount of lithium in the positive electrode active material raw material was 100 mol%.

[0217] The annealed positive active material was mixed with distilled water in a weight ratio of 1:1, stirred at 500 rpm for 5 minutes, and then filtered under reduced pressure to obtain a solid content, which was then vacuum-dried at 100° C. for 12 hours to obtain a washed positive active material.

[0218] The washed positive active material was coated with boric acid and heated at 300° C. for 5 hours to prepare a final regenerated positive active material. Here, boric acid was added in an amount corresponding to 1000 ppm of boron lost in the previous process, the temperature was increased at a rate of 2° C. / min until the heat treatment temperature was reached, and air was supplied at a rate of 3 L / min.

[0219] In this description, the molar ratio of lithium to other metals in the positive electrode active material, the remaining amount of LiF, etc. were measured using an ICP analyzer. In this case, the measurements can be performed using a general ICP analyzer commonly used in laboratories, and there is no deviation due to the measurement device or method.

[0220] Comparative Example 1 A regenerated positive electrode active material was produced in the same manner as in Example 1, except that in the oxidative heat treatment step in Example 1, air (containing 21% oxygen) was used instead of oxygen for the heat treatment.

[0221] Comparative Example 2 A regenerated positive electrode active material was prepared in the same manner as in Example 1, except that in the oxidative heat treatment step of Example 1, air (containing 21% oxygen) was used instead of oxygen to perform the heat treatment, and the first washing step was not performed.

[0222] Comparative Example 3 A regenerated positive electrode active material was prepared in the same manner as in Example 1, except that the first washing step was not performed.

[0223] [Test Example I: SEM Analysis] The regenerated positive electrode active materials obtained in Example 1 and Comparative Examples 1 to 3 were photographed by a SEM device and are shown in FIG. 2. The SEM photographs were taken by a general SEM device commonly used in laboratories. Specifically, the SEM photographs were taken by using a Hitachi S-4200. However, there is no deviation due to the measurement device or method.

[0224] As can be seen from Fig. 2, the recycled positive electrode active material produced in Example 1 was broken into small particles, and these broken particles were in contact with or dispersed among larger particles. In contrast, in Comparative Examples 1 to 3, the particles were not broken into small particles but were agglomerated.

[0225] [Test Example II: XRD Analysis] The crystal size of the regenerated positive active materials obtained in Example 1 and Comparative Examples 1 to 3 was measured by XRD crystal analysis.

[0226] Specifically, 5 g of each of the regenerated positive electrode active material particles obtained in Example 1 and Comparative Examples 1 to 3 was placed in a holder, and the particles were irradiated with X-rays to generate diffraction gratings, which were then analyzed. The diffraction gratings were determined from the half-width of the main peak or three or more peaks, which corresponded to the average crystal size of the primary particles of the regenerated positive electrode active material particles. The average crystal size of the primary particles of the regenerated positive electrode active material obtained as a result of this is shown in Table 1 below.

[0227] [Table 1]

[0228] As shown in Table 1, the crystal size of the regenerated positive electrode active material prepared in Example 1 was smaller than those of Comparative Examples 1 to 3. The smaller crystal size reduces distortion and minimizes cycle cracks, which is advantageous in extending the battery life.

[0229] [Test Example III: Residual fluorine (F) content] The content of fluorine (F) remaining in the regenerated positive active materials obtained in Example 1 and Comparative Examples 1 to 3 was measured using an ICP analyzer, and the results are shown in Table 2. The measurement can be performed using a general ICP analyzer commonly used in laboratories, and there is no deviation due to the measurement device or method.

[0230] [Table 2]

[0231] As can be seen from Table 2, Example 1 according to the present invention had a significantly reduced residual fluorine content compared to Comparative Examples 1 to 3.

[0232] [Test Example IV: Residual Lithium Content] The residual lithium content of the regenerated positive electrode active materials obtained in Example 1 and Comparative Examples 1 to 3 was measured as follows, and the results are shown in Table 3 below. * Residual lithium content: 5 g of the positive active material was dispersed in 100 ml of distilled water, mixed at 300 rpm for 5 minutes, and filtered to remove the active material. The filtrate was titrated with 0.1 M HCl solution to measure the change in pH value and obtain a pH titration curve. The amount of LiOH and Li2CO3 remaining in the positive active material was calculated using the obtained pH titration curve.

[0233] [Table 3]

[0234] As shown in Table 3, it was confirmed that the content of residual lithium in the regenerated positive electrode active material in Example 1 was reduced compared to Comparative Examples 1 to 3.

[0235] [Test Example V: Evaluation of CHC Cell] The electrochemical performance of the regenerated positive electrode active materials obtained in Example 1 and Comparative Examples 1 to 3 was measured through the CHC cell evaluation as described below, and the results are shown in FIG. *Evaluation of CHC cell: 97.5% by weight of recycled positive electrode active material, 1% by weight of carbon black as conductive material, and 1.5% by weight of PVdF as binder were weighed and mixed with NMP to produce a slurry. This was coated on aluminum foil to produce a positive electrode, and then a coin half cell (CHC) was produced. The voltage was set to 3-4.3V, charging and discharging was performed at 0.1C / 0.1C, and the electrochemical performance (charge capacity, discharge capacity, and efficiency) was evaluated under conditions that included ethylene carbonate (EC): ethyl methyl carbonate (EMC) = 3:7 (weight ratio) as electrolyte and other additives.

[0236] FIG. 3 shows the results of evaluating coin cells for each of the recycled positive electrode active materials manufactured or prepared in Example 1 and Comparative Examples 1 to 3. It was confirmed that the recycled positive electrode active material of the present invention (Example 1) has superior charging capacity compared to Comparative Examples 1 to 3.

[0237] [Test Example VI: Evaluation of Mono Cell] The capacity retention rate and resistance increase rate of the mono-cells prepared using the regenerated positive electrode active materials obtained in Example 1 and Comparative Examples 1 to 3 were measured through the following mono-cell evaluation, and the results are shown in FIG. * Manufacturing of monocell: The same positive electrode active material slurry as that used for the coin cell was applied to an aluminum foil having a thickness of 20 μm, dried at 130°C for 1 hour, and then punched out to a size of 30 mm x 42 mm to manufacture a positive electrode.

[0238] Meanwhile, a negative electrode active material slurry was prepared by mixing 95.6 wt% of a 5:5 mixture of natural graphite and artificial graphite with 3.3 wt% of conductive material and 1.1 wt% of binder. The slurry was applied to a copper foil having a thickness of 10 μm, rolled and dried, and then punched into a size of 31 mm×43 mm to prepare a negative electrode.

[0239] The prepared positive and negative electrodes were joined with a separator, and an electrolyte solution with a weight ratio of ethylene carbonate (EC): ethyl methyl carbonate (EMC) = 3: 7 was injected, and then vacuum sealed to prepare a mono cell. This was aged for 10 hours, and then electrochemical evaluation was performed.

[0240] *Measurement of capacity retention rate at high temperature (45°C): Each of the mono cells manufactured with the regenerated positive electrode active materials obtained in Example 1 and Comparative Examples 1 to 3 was subjected to formation at a rate of 0.1C, and then gas in the battery was removed (degas process). Then, 4.2V, 1C, 0.05C cut-off CC / CV charging and 2.5V, 0.5C CC discharging were performed 200 times at high temperature (45°C), and the discharge capacity at the first time and the discharge capacity after the 200th time were measured using a PNE-0506 charger / discharger (manufacturer: PNE Solution Co., Ltd., 5V, 6A), and the discharge capacity at the first time was set as the initial capacity. Then, the 200th discharge capacity was compared with the initial capacity (100%), and the capacity retention rate was calculated according to the following formula 1, and the results are shown in FIG. 4.

[0241] [Formula 1] Capacity retention rate (%) = (discharge capacity after high-temperature cycle / initial discharge capacity) x 100

[0242] *Measurement of resistance increase rate at high temperature (45°C): Each of the mono cells manufactured with the regenerated positive electrode active materials obtained in Example 1 and Comparative Examples 1 to 3 was subjected to formation at a rate of 0.1C, and then gas in the battery was removed (degas process). The lithium secondary battery from which the gas was removed was transferred to a charger / discharger at room temperature (25°C), and then charged at a rate of 0.33C under constant current / constant voltage conditions up to 4.2V, and charged with a cutoff charge of 0.05C, and discharged at 0.33C 2.5V. The SOC (State Of Charge) was adjusted to 50% based on the discharge capacity after three charge / discharge cycles. At this time, the DC internal resistance was measured using a PNE-0506 charger / discharger (manufacturer: PNE Solution Co., Ltd., 5V, 6A) through the voltage drop that appears when a discharge pulse is applied at 2.5C for 10 seconds, and the resistance at this time was set as the initial resistance.

[0243] After that, 4.2V, 1C, 0.05C cutoff CC / CV charging and 2.5V, 0.5C CC discharging were performed 200 times at high temperature (45℃), and the lithium secondary battery was then moved to a charger / discharger at room temperature (25℃), and the SOC (State of Charge) was adjusted to 50%, and the DC internal resistance was measured using a PNE-0506 charger / discharger (manufacturer: PNE Solution Co., Ltd., 5V, 6A) through the voltage drop that occurred when a discharge pulse was applied at 2.5C for 10 seconds. This was compared with the initial resistance (0%) to calculate the resistance increase rate (%) using the following formula 2, and the result is shown in Figure 4.

[0244] [Formula 2] Resistance increase rate (%) = {(resistance after high-temperature cycle - initial resistance) / initial resistance} x 100

[0245] As shown in FIG. 4, it was confirmed that, as the number of cycles increased, Example 1 had a higher capacity retention rate and a lower resistance increase rate than Comparative Examples 1 to 3.

[0246] [Additional Example] Additional Example 1 The cathode scraps discarded after punching out the cathode plates (current collector: aluminum foil, cathode active material: NCM-based lithium composite transition metal oxide with nickel content of 86 mol%) were crushed and subjected to a primary heat treatment at 350°C for 2 hours in oxygen with a purity of 95%, and then the temperature was raised to 590°C for a secondary heat treatment for 30 minutes to remove the binder and conductive material, and the current collector and cathode active material were separated and the cathode active material was recovered. Here, the temperature was increased at a rate of 5°C / min until the heat treatment temperature was reached, and oxygen (O2) was supplied at 10 L / min.

[0247] The recovered positive electrode active material was immersed in distilled water as a cleaning solution and stirred at the same time for primary washing. At this time, the weight ratio of the recovered positive electrode active material to the cleaning solution was 1:30, and the mixture was stirred at 500 rpm for 10 minutes, and then the active material was removed by reduced pressure filtration using a filter. The positive electrode active material that had been primarily washed had a reduction of 0.11 moles based on 1 mole of lithium in the positive electrode active material compared to the raw material.

[0248] The washed cathode active material was dried overnight at 100° C., and then LiOH was added as a lithium precursor, followed by annealing in air at 750° C. for 5 hours. Air was supplied at 3 L / min. The lithium precursor was added in an amount equivalent to 18 mol% when the total amount of lithium in the cathode active material, which was the raw material used in the cathode active material layer, was taken as 100 mol%.

[0249] The annealed positive active material was mixed with distilled water in a weight ratio of 1:10, stirred at 500 rpm for 5 minutes, and then filtered under reduced pressure to obtain a solid content, which was then vacuum-dried at 100° C. for 12 hours to obtain a washed positive active material.

[0250] The washed positive active material was coated with boric acid and heated at 300° C. for 5 hours to prepare a final regenerated positive active material. Here, boric acid was added in an amount corresponding to 1000 ppm of boron lost in the previous process, the temperature was increased at a rate of 2° C. / min until the heat treatment temperature was reached, and air was supplied at a rate of 3 L / min.

[0251] In this description, the molar ratio of lithium to other metals in the positive electrode active material, the remaining amount of LiF, etc. were measured using an ICP analyzer. In this case, the measurements can be performed using a general ICP analyzer commonly used in laboratories, and there is no deviation due to the measurement device or method.

[0252] In this description, ppm is by weight unless otherwise specified.

[0253] Additional Example 2 A regenerated positive electrode active material was prepared in the same manner as in Additional Example 1, except that the first heat treatment was performed at 350° C. for 30 minutes and the second heat treatment was performed at 590° C. for 30 minutes.

[0254] Additional Example 3 A regenerated positive electrode active material was prepared in the same manner as in Additional Example 1, except that the first heat treatment was performed at 350° C. for 30 minutes and the second heat treatment was performed at 570° C. for 30 minutes.

[0255] Additional Comparative Example 1 A regenerated positive electrode active material was prepared in the same manner as in Additional Example 1, except that the first and second heat treatment steps were performed at 550° C. for 30 minutes.

[0256] Additional Comparative Example 2 A regenerated positive electrode active material was prepared in the same manner as in Additional Example 1, except that the recovered positive electrode active material was not subjected to a first washing step and was immediately subjected to an annealing step.

[0257] [Test Example I: XRD Analysis] The crystal size of the regenerated positive electrode active materials obtained in Additional Examples 1 to 3 and Additional Comparative Example 1 was measured by XRD crystal analysis.

[0258] Specifically, 5 g of the regenerated positive electrode active material particles obtained in Additional Examples 1 to 3 and Additional Comparative Example 1 were placed in a holder, and the particles were irradiated with X-rays to analyze the diffraction grating. The method of determination was from the half-width of the main peak or three or more peaks, which corresponded to the average crystal size of the primary particles of the regenerated positive electrode active material particles. The average crystal size of the primary particles of the regenerated positive electrode active material obtained from this result is shown in Table 4 below.

[0259] [Table 4]

[0260] As shown in Table 4, the crystal size of the regenerated positive electrode active material prepared in Additional Examples 1 to 3 was smaller than that of Additional Comparative Example 1. The smaller crystal size reduces distortion and minimizes cycle cracking, which is advantageous in extending the battery life.

[0261] [Test Example II: Residual fluorine (F) content] The content of fluorine (F) remaining in the regenerated positive electrode active materials obtained in Additional Examples 1 to 3 and Additional Comparative Examples 1 and 2 was measured using an ICP analyzer, and the results are shown in Table 5. At this time, the measurement can be performed using a general ICP analyzer commonly used in laboratories, and there is no deviation due to the measurement device or method.

[0262] [Table 5]

[0263] As can be seen from Table 5, Additional Examples 1 to 3 according to the present invention had reduced residual fluorine contents compared to Additional Comparative Examples 1 and 2. In particular, Additional Comparative Example 2, in which the first cleaning was not performed, had a very high residual fluorine content.

[0264] [Test Example III: Residual Lithium Content] The residual lithium content of the regenerated positive electrode active materials obtained in Additional Examples 1 to 3 and Additional Comparative Examples 1 and 2 was measured as follows, and the results are shown in Table 6 below. * Residual lithium content: 5 g of the positive active material was dispersed in 100 ml of distilled water, mixed at 300 rpm for 5 minutes, and filtered to remove the active material. The filtrate was titrated with 0.1 M HCl solution to measure the change in pH value and obtain a pH titration curve. The amount of LiOH and Li2CO3 remaining in the positive active material was calculated using the obtained pH titration curve.

[0265] [Table 6]

[0266] As shown in Table 6, it was confirmed that the residual lithium content of the regenerated positive electrode active material in Additional Examples 1 to 3 was reduced compared to Additional Comparative Examples 1 and 2.

[0267] [Test Example IV: Evaluation of CHC Cell] The electrochemical performance of the regenerated positive electrode active materials obtained in Additional Examples 1 to 3 and Additional Comparative Examples 1 and 2 was measured through the CHC cell evaluation as described below, and the results are shown in FIG. *Evaluation of CHC cell: 97.5% by weight of recycled positive electrode active material, 1% by weight of carbon black as conductive material, and 1.5% by weight of PVdF as binder were weighed and mixed with NMP to prepare slurry. This was coated on aluminum foil to prepare a positive electrode, and a coin half cell (CHC) was prepared by adding ethylene carbonate (EC): ethyl methyl carbonate (EMC) = 3:7 (weight ratio) as electrolyte and other additives. The prepared coin cell was charged at 25°C with a constant current of 0.1C up to 4.3V with a 0.05C cut off. It was then discharged at a constant current of 0.1C up to 3.0V. The charge capacity at this time was measured and is shown in Figure 5.

[0268] FIG. 5 shows the results of evaluating coin cells for each of the recycled positive electrode active materials produced in Additional Examples 1 to 3 and Additional Comparative Examples 1 and 2. It was confirmed that the recycled positive electrode active materials according to the present invention (Additional Examples 1 to 3) have superior charging capacity compared to Additional Comparative Examples 1 and 2.

[0269] [Test Example V: Evaluation of Mono Cell] The capacity retention rates of the mono-cells prepared using the regenerated positive electrode active materials obtained in Additional Examples 1 to 3 and Additional Comparative Examples 1 and 2 were measured through the following mono-cell evaluation, and the results are shown in FIG. * Manufacturing of monocell: The same positive electrode active material slurry as that used for the coin cell was applied to an aluminum foil having a thickness of 20 μm, dried at 130°C for 1 hour, and then punched out to a size of 30 mm x 42 mm to manufacture a positive electrode.

[0270] Meanwhile, a negative electrode active material slurry was prepared by mixing 95.6 wt% of a 5:5 mixture of natural graphite and artificial graphite with 3.3 wt% of conductive material and 1.1 wt% of binder. The slurry was applied to a copper foil having a thickness of 10 μm, rolled and dried, and then punched into a size of 31 mm×43 mm to prepare a negative electrode.

[0271] The prepared positive and negative electrodes were joined with a separator, and an electrolyte solution with a weight ratio of ethylene carbonate (EC): ethyl methyl carbonate (EMC) = 3: 7 was injected, and then vacuum sealed to prepare a mono cell. This was aged for 10 hours, and then electrochemical evaluation was performed.

[0272] *Measurement of capacity retention rate at high temperature (45°C): Each of the mono cells manufactured with the regenerated positive electrode active materials obtained in the additional examples 1 to 3 and the additional comparative examples 1 and 2 was subjected to formation at a rate of 0.1C, and then the gas in the battery was removed (degas process). Then, 4.2V, 1C, 0.05C cut-off CC / CV charging and 2.5V, 0.5C CC discharging were performed 100 times at high temperature (45°C), and the discharge capacity at the first time and the discharge capacity after the 100th time were measured using a PNE-0506 charger / discharger (manufacturer: PNE Solution Co., Ltd., 5V, 6A), and the discharge capacity at the first time was set as the initial capacity. Then, the 100th discharge capacity was compared with the initial capacity (100%), and the capacity retention rate was calculated according to the following formula 1, and the results are shown in FIG. 6.

[0273] [Formula 1] Capacity retention rate (%) = (discharge capacity after high-temperature cycle / initial discharge capacity) x 100

[0274] As shown in FIG. 6, it was confirmed that Additional Examples 1 to 3 had a higher capacity retention rate than Additional Comparative Examples 1 and 2 as the number of cycles increased. [Explanation of symbols]

[0275] 10 Current collector 20 Active material layer 30 Positive electrode sheet 40 Positive plate 50 Cathode scrap

Claims

1. A positive electrode active material comprising at least one material selected from the group consisting of a lithium nickel oxide (LNO)-based positive electrode active material, a nickel cobalt manganese (NCM)-based positive electrode active material, a nickel cobalt aluminum (NCA)-based positive electrode active material, and a nickel cobalt manganese aluminum (NCMA)-based positive electrode active material, the positive electrode active material comprising at least 60 mol% of Ni, a fluorine (F) content of at most 250 mg / kg, and an average crystal size of at most 122 nm.

2. The positive electrode active material according to claim 1 , wherein the positive electrode active material has a surface coated with a coating agent containing metal or carbon.

3. The positive electrode active material according to claim 2 , wherein the metal is boron (B), tungsten (W), or a mixture thereof.

4. The positive electrode active material according to claim 1 , wherein the positive electrode active material is a regenerated positive electrode active material.

5. a step of subjecting a waste positive electrode having a positive electrode active material layer containing 60 mol % or more of Ni formed on a current collector to an oxidative heat treatment by introducing oxygen to thermally decompose a binder and a conductive material in the positive electrode active material layer, thereby separating the current collector from the positive electrode active material layer and recovering the positive electrode active material in the positive electrode active material layer; A step of primarily washing the recovered positive electrode active material; adding a lithium precursor to the first washed positive electrode active material and annealing the same; and a second step of cleaning the annealed positive electrode active material.

6. 6. The method for regenerating a positive electrode active material according to claim 5, wherein the oxidation heat treatment is carried out at 300 to 650° C.

7. 7. The method of claim 5, wherein the oxidation heat treatment is a first heat treatment at 300 to 450° C. and a second heat treatment at 500 to 650° C.

8. 8. The method of claim 7, wherein the first heat treatment is performed for 10 minutes to 3 hours, and the second heat treatment is performed for 10 minutes to 2 hours.

9. 6. The method for regenerating a positive electrode active material according to claim 5, wherein the oxygen has a purity of 59% or more.

10. 6. The method for regenerating a positive electrode active material according to claim 5, wherein the primary washing is performed by immersing the recovered positive electrode active material in water or a basic lithium compound aqueous solution as a washing liquid, or by immersing and stirring the recovered positive electrode active material at the same time.

11. The method for regenerating a positive electrode active material according to claim 10, wherein the basic lithium compound aqueous solution contains more than 0 wt % and not more than 15 wt % of a lithium compound.

12. 6. The method of claim 5, wherein the method of adding a lithium precursor to the primarily washed positive electrode active material in the annealing step comprises mixing the primarily washed positive electrode active material with a lithium precursor solution and spray-drying the mixture.

13. 6. The method of claim 5, wherein the second cleaning comprises mixing the annealed positive active material with water as a cleaning solution, filtering the mixed solution, and drying the solid positive active material obtained after the filtration.

14. The lithium precursor is LiOH, Li 2 CO 3 , LiNO 3 and Li 2 The method for regenerating a positive electrode active material according to claim 5 , wherein the positive electrode active material contains one or more of O.

15. The method of claim 5, wherein the lithium precursor is added in an amount corresponding to 1 mol% to 40 mol% when the total amount of lithium in the raw material positive electrode active material used in the positive electrode active material layer is 100 mol%.

16. The method for regenerating a positive electrode active material according to claim 5, wherein the annealing is performed at a temperature of 400 to 1000°C.

17. 6. The method of claim 5, further comprising the step of: surface-coating the second washed positive active material to obtain a reusable positive active material.

18. The method of claim 17, wherein the surface coating is performed by coating the surface with at least one of a metal, an organic metal, and a carbon component in a solid or liquid phase manner, and then heat-treating the surface at 100 to 1200°C.

19. A positive electrode active material comprising at least one material selected from the group consisting of a lithium nickel oxide (LNO)-based positive electrode active material, a nickel cobalt manganese (NCM)-based positive electrode active material, a nickel cobalt aluminum (NCA)-based positive electrode active material, and a nickel cobalt manganese aluminum (NCMA)-based positive electrode active material, the positive electrode active material comprising at least 60 mol% of Ni, a fluorine (F) content of at most 305 mg / kg, and an average crystal size of at most 139 nm.

20. The positive electrode active material is 2 CO 3 The positive electrode active material according to claim 19, wherein the content of is 0.16 wt % or less.

21. A secondary battery comprising the positive electrode active material according to any one of claims 1 to 4, 19 and 20.

Citation Information

Patent Citations

  • Lithium metal composite oxide, positive electrode active material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery

    JP2021177460A

  • Non-aqueous electrolyte secondary battery

    WO2015141179A1

  • Positive electrode active material for secondary battery, and secondary battery

    WO2020162277A1

  • Method for reusing active material using positive electrode scrap

    WO2021241835A1

Cited By

  • Method for regenerating positive electrode active material and the positive electrode active material regenerated therefrom

    JP7844760B1