Semiconductor substrate and processing method thereof, solar cell and manufacturing method thereof
The semiconductor substrate processing method for solar cells, featuring a smooth and textured surface region with a protective layer and diffusion annealing, addresses the efficiency issues of conventional cells by enhancing material uniformity and reducing series resistance, thereby improving photoelectric conversion efficiency.
Patent Information
- Application Number
- JP2024510515
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-04
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-23
AI Technical Summary
Conventional solar cells with textured silicon substrates face issues of low photoelectric conversion efficiency due to poor uniformity of material layers, increased series resistance, and reduced open circuit voltage, primarily because of densely arranged pyramid structures on the surface.
A semiconductor substrate processing method that forms a smooth surface region and a textured surface region, where the area of the smooth surface region is greater than or equal to the textured surface region, involving the use of a protective layer and diffusion annealing to enhance material layer uniformity and reduce defects, with transparent conductive films and grid lines only on the smooth surface.
The method improves light trapping and reduces series resistance, leading to enhanced photovoltaic conversion efficiency and overall solar cell performance by ensuring uniform deposition of materials and minimizing defects.
Smart Images

Figure 2024542919000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims priority to a Chinese patent application bearing application number 202211378975.9 and entitled "Semiconductor substrate and processing method thereof, solar cell and manufacturing method thereof" filed with the China Patent Office on November 4, 2022, the entire contents of which are incorporated herein by reference.
[0002] The present application relates to the technical field of solar cells, and in particular to semiconductor substrates and methods for processing same, as well as solar cells and methods for manufacturing same. [Background technology]
[0003] A solar cell is a device that absorbs sunlight and converts the solar radiation into electrical energy directly or indirectly through the photoelectric effect or photochemical effect. Solar cells are clean energy cells and are widely used in daily life and production.
[0004] One of the semiconductor substrates commonly used in solar cells is a silicon substrate. In order to enhance the light absorption ability of solar cells, a textured surface is usually formed on the surface of the silicon substrate to enhance the light trapping ability of the silicon substrate, thereby improving the photoelectric conversion efficiency of the solar cell. However, after the texturing process, densely arranged pyramidal structures are formed on the surface of the silicon substrate, and the height of these pyramidal structures usually reaches 1 μm to 2 μm, which leads to poor uniformity of other material layers formed in subsequent processes, which reduces the open circuit voltage of the solar cell, and also leads to poor contact between each material layer, which limits the transport of carriers and increases the series resistance, resulting in poor photoelectric conversion performance of solar energy.
[0005] As is clear from this, how to improve the photoelectric conversion efficiency of solar cells is an urgent problem to be solved in the solar cell field. Summary of the Invention [Problem to be solved by the invention]
[0006] Therefore, the technical problem to be solved by the present application is to provide a semiconductor substrate and a processing method thereof, and a solar cell and a manufacturing method thereof, by overcoming the problem of low photoelectric conversion efficiency of solar cells in the conventional technology. [Means for solving the problem]
[0007] In a first aspect of the present application, there is provided a method for processing a semiconductor substrate, comprising the steps of forming a smooth surface region and a textured surface region adjacent to the smooth surface region on at least one side of the semiconductor substrate, wherein the area of the smooth surface region is greater than or equal to the area of the textured surface region.
[0008] Optionally, the ratio of the area of the smooth surface region to the area of the textured surface region is between 1:1 and 1.2:1.
[0009] Optionally, the step of forming a smooth surface region and a textured surface region adjacent to the smooth surface region on any one surface of the semiconductor substrate includes the steps of forming a protective layer on any one surface of the semiconductor substrate, and placing a patterned cover layer on a surface of the protective layer opposite the semiconductor substrate, the cover layer having a hollow region, the protective layer including a first region located at a bottom of the hollow region and a second region shielded by the cover layer, thickening the first region of the protective layer using the cover layer after thickening the first region of the protective layer, removing the cover layer, etching and removing the second region of the protective layer using the first region of the protective layer after removing the cover layer as protection, performing a texturing process on the one side of the semiconductor substrate exposed from the protective layer after removing the second region, so that the one side of the semiconductor substrate exposed from the protective layer forms a textured surface region, and after forming the textured surface region, etching and removing the first region corresponding to the protective layer, so that a part of the surface of the one side of the semiconductor substrate forms a smooth surface region.
[0010] Optionally, the hollow region includes at least a plurality of spaced apart strips of openings, the strips being parallel to one another.
[0011] Optionally, the step of forming a protective layer on any one side of the semiconductor substrate includes the steps of coating an undercoat film over the entire surface of any one side of the semiconductor substrate, and performing a diffusion annealing process on the undercoat film, whereby the undercoat film reacts with the surface of the one side of the semiconductor substrate to form an ion-doped protective layer and migrate impurities in the semiconductor substrate to the protective layer.
[0012] Optionally, the step of thickening the first region of the protective layer includes the steps of using the cover layer as a mask to coat a surface of the first region with a surface film, and performing a diffusion annealing process on the surface film to make the surface film part of the protective layer, thereby increasing the thickness of the first region.
[0013] Optionally, the cover layer comprises a quartz material.
[0014] Optionally, the base film and top film are liquid source films.
[0015] Optionally, the undercoat film and the overcoat film are phosphorus-containing liquid source films, with the overcoat film having a phosphorus concentration greater than the undercoat film.
[0016] Optionally, the duration of the diffusion annealing treatment of the top layer is longer than the duration of the diffusion annealing treatment of the underlayer.
[0017] Optionally, the temperature of the diffusion annealing treatment of the top layer is higher than the temperature of the diffusion annealing treatment of the underlayer.
[0018] Optionally, parameters for both the step of etching and removing the first region of the protective layer and the step of etching and removing the second region of the protective layer are as follows: the etching solution used is a mixture of hydrofluoric acid aqueous solution, hydrochloric acid aqueous solution and water-soluble solvent, the concentration of the hydrofluoric acid aqueous solution is 35% by mass to 50% by mass, the concentration of the hydrochloric acid aqueous solution is 30% by mass to 50% by mass, the volume fraction of the hydrofluoric acid aqueous solution is 1% to 4%, the volume fraction of the hydrochloric acid aqueous solution is 1% to 3%, and the etching time is 100 s to 300 s.
[0019] In a second aspect of the present application, there is provided a semiconductor substrate having, on at least one surface thereof, a smooth surface region and a textured surface region adjacent to the smooth surface region, the area of the smooth surface region being equal to or greater than the area of the textured surface region.
[0020] Optionally, the ratio of the area of the smooth surface region to the area of the textured surface region is between 1:1 and 1.2:1.
[0021] In a third aspect of the present application, there is provided a method for manufacturing a solar cell, including the steps of: providing a semiconductor substrate; processing the semiconductor substrate by the above-described semiconductor substrate processing method so as to provide at least one side of the semiconductor substrate with a smooth surface region and a textured surface region adjacent to the smooth surface region; forming a transparent conductive film located only in the smooth surface region on the side of the semiconductor substrate having the smooth surface region and the textured surface region; and forming grid lines in at least a portion of the transparent conductive film on the side opposite the semiconductor substrate.
[0022] Optionally, the method for manufacturing a solar cell further includes, before forming the transparent conductive film, a step of forming a doped semiconductor layer located between the semiconductor substrate and the transparent conductive film on the side of the semiconductor substrate having the smooth surface region and the textured surface region.
[0023] Optionally, prior to forming the doped semiconductor layer, an intrinsic semiconductor layer is formed on the side of the semiconductor substrate having the smooth surface region and the textured surface region, the intrinsic semiconductor layer being located between the semiconductor substrate and the doped semiconductor layer.
[0024] In a fourth aspect of the present application, there is provided a solar cell including a semiconductor substrate having a smooth surface region and a textured surface region adjacent to the smooth surface region on at least one side, the area of the smooth surface region being equal to or greater than the area of the textured surface region, a transparent conductive film located on the side of the semiconductor substrate having the smooth surface region and the textured surface region and located only on the smooth surface region, and grid lines located in at least a portion of the transparent conductive film on the side opposite the semiconductor substrate.
[0025] Optionally, the solar cell further includes a doped semiconductor layer located between the semiconductor substrate and the transparent conductive film.
[0026] Optionally, the solar cell further includes an intrinsic semiconductor layer located between the semiconductor substrate and the doped semiconductor layer. Effect of the Invention
[0027] The technical solutions of the present application can achieve the following beneficial effects: 1. The present application relates to processing a semiconductor substrate such that at least one surface of the semiconductor substrate includes a smooth surface region and a textured surface region adjacent to the smooth surface region, and the textured surface region can provide an excellent light trapping effect, and the smooth surface of the smooth surface region is advantageous for uniform deposition of other material layers in the region, thereby achieving better uniformity of the material film layer, and advantageous for improving photoelectric conversion efficiency and improving cell efficiency. 2. The present application forms a protective layer on the surface of a semiconductor substrate, and by diffusion annealing, the impurity ions in the semiconductor substrate can be transferred to the protective layer, which is advantageous to reducing defects in the semiconductor substrate. Then, by thickening the first region of the protective layer using a cover layer, the impurity ions in the semiconductor substrate can continue to diffuse into the first region of the protective layer, which is advantageous to further reduce defects in the region of the semiconductor substrate corresponding to the first region of the protective layer. Then, when etching and removing the second region, at least a part of the thickness of the first region of the protective layer can be left, and during the texturing process, the region of the semiconductor substrate corresponding to the second region of the protective layer can be ensured to form a textured surface region, and the first region of the protective layer can prevent the corresponding region of the semiconductor substrate from being etched, and then the first region of the protective layer is etched and removed, so that the region of the semiconductor substrate corresponding to the first region of the protective layer forms a smooth surface region having a flat surface, and the concentration of impurity ions in the smooth surface region of the semiconductor substrate is low, so that the defect density of the semiconductor substrate is low. 3. The cover layer used in this application is a high-temperature resistant quartz material, which is low-cost and can be reused after cleaning. The cover layer can also protect the semiconductor substrate during the diffusion annealing process and reduce the risk of damage to the silicon wafer. 4. In the solar cell of the present application, the transparent conductive film and the grid lines are both located only on the smooth surface region, and the smooth surface region has a smooth surface, which is favorable for uniform deposition of the transparent conductive film and the grid lines on the smooth surface region, and the flat and smooth surface region is favorable for sufficient contact between the transparent conductive film and the grid lines and reduced series resistance, while the textured surface region can provide an excellent light trapping effect. The solar cell of the present application can achieve both the light trapping effect and low series resistance, which is favorable for improving the photoelectric conversion efficiency of the solar cell.
[0028] In order to more clearly describe the specific embodiments of the present application or the technical solutions in the prior art, the following will briefly describe the drawings that need to be used in the description of the specific embodiments or the prior art. It is obvious that the drawings in the following description are some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without exerting creative efforts. [Brief description of the drawings]
[0029] [Figure 1] 4 illustrates an exemplary flow chart for forming a smooth surface region and a textured surface region on one side of a semiconductor substrate according to an embodiment of the present application. [Diagram 2] 1A-1D are structural schematic diagrams illustrating a semiconductor substrate during processing according to an embodiment of the present application; [Diagram 3] 1A-1D are structural schematic diagrams illustrating a semiconductor substrate during processing according to an embodiment of the present application; [Figure 4] 1A-1D are structural schematic diagrams illustrating a semiconductor substrate during processing according to an embodiment of the present application; [Diagram 5] 1A-1D are structural schematic diagrams illustrating a semiconductor substrate during processing according to an embodiment of the present application; [Figure 6] 1A-1D are structural schematic diagrams illustrating a semiconductor substrate during processing according to an embodiment of the present application; [Figure 7] 1A-1D are structural schematic diagrams illustrating a semiconductor substrate during processing according to an embodiment of the present application; [Figure 8] 1A-1D are structural schematic diagrams illustrating a semiconductor substrate during processing according to an embodiment of the present application; [Figure 9] 1A-1D are structural schematic diagrams illustrating a semiconductor substrate during processing according to an embodiment of the present application; [Figure 10] 1A-1D are structural schematic diagrams illustrating a semiconductor substrate during processing according to an embodiment of the present application; [Figure 11] FIG. 2 is a structural schematic diagram of a cover layer according to an embodiment of the present application. [Figure 12] 1A-1D are structural schematic diagrams illustrating a manufacturing process of a solar cell according to an embodiment of the present application. [Figure 13] 1A-1D are structural schematic diagrams illustrating a manufacturing process of a solar cell according to an embodiment of the present application. [Figure 14] 1A-1D are structural schematic diagrams illustrating a manufacturing process of a solar cell according to an embodiment of the present application. [Figure 15] 1A-1D are structural schematic diagrams illustrating a manufacturing process of a solar cell according to an embodiment of the present application. [Figure 16] 1A-1D are structural schematic diagrams illustrating a manufacturing process of a solar cell according to an embodiment of the present application. [Figure 17] 1A-1D are structural schematic diagrams illustrating a manufacturing process of a solar cell according to an embodiment of the present application. [Figure 18] 1A-1D are structural schematic diagrams illustrating a manufacturing process of a solar cell according to an embodiment of the present application. [Figure 19] 1A-1D are structural schematic diagrams illustrating a manufacturing process of a solar cell according to an embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] The following clearly and completely describes the technical solutions of the present application with reference to the drawings, but it is clear that the described embodiments are only some embodiments of the present application, and not all embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative labor belong to the protection scope of the present application.
[0031] In the description of this application, the orientation or positional relationship indicated by the terms "upper", "lower", "left", "right", etc., is based on the orientation or positional relationship shown in the drawings, and is merely for the purpose of facilitating and simplifying the description of this application, and does not indicate or imply that such devices or elements must necessarily have a specific orientation, or be configured or operate in a specific orientation, and therefore is not to be understood as limiting this application. Furthermore, the terms "first" and "second" are used for the purpose of description only, and are not to be understood as indicating or implying relative importance.
[0032] In addition, the technical features according to each embodiment of the present application described below may be combined with each other as long as they are not mutually contradictory.
[0033] One or more embodiments of the present application provide a method for processing a semiconductor substrate, comprising forming a smooth surface region and a textured surface region adjacent to the smooth surface region on at least one side of the semiconductor substrate, wherein an area of the smooth surface region is equal to or greater than an area of the textured surface region.
[0034] The present application relates to processing a semiconductor substrate such that at least one surface of the semiconductor substrate includes a smooth surface region and a textured surface region adjacent to the smooth surface region, and the textured surface region can provide an excellent light trapping effect, and the smooth surface of the smooth surface region is advantageous for uniform deposition of other material layers in that region, which is advantageous for improving photoelectric conversion efficiency and improving cell efficiency.
[0035] In one embodiment, the ratio of the area of the smooth surface region to the area of the textured surface region is 1:1 to 1.2:1. For example, the ratio of the area of the smooth surface region to the area of the textured surface region is 1:1, 1.12:1, 1.15:1, 1.17:1, or 1.2:1.
[0036] In one embodiment, the step of forming a smooth surface region and a textured surface region adjacent to the smooth surface region on any one side of a semiconductor substrate comprises: Step S100 of forming a protective layer on any one side of a semiconductor substrate; Step S200 of placing a patterned cover layer on a surface of the protective layer opposite the semiconductor substrate, the cover layer having a hollow region, the protective layer including a first region located at a bottom of the hollow region and a second region shielded by the cover layer; After providing the patterned cover layer, a step S300 of thickening a first region of the protective layer; A step S400 of removing the cover layer after thickening the first region of the protective layer; Step S500 of removing the cover layer, and then etching and removing the second region of the protective layer while protecting the first region of the protective layer; Step S600 of etching and removing the second region of the protective layer, and then performing a texturing process on one side of the semiconductor substrate exposed from the protective layer, so that the one side of the semiconductor substrate exposed from the protective layer forms a textured surface region; The method includes step S700 of etching and removing the first region of the protective layer after forming the textured surface region, so that a portion of the surface of one side of the semiconductor substrate forms a smooth surface region.
[0037] In the present application, by forming a protective layer on the surface of a semiconductor substrate, impurity ions in the semiconductor substrate can be transferred to the protective layer, which is advantageous for reducing defects in the semiconductor substrate. Then, by thickening the first region of the protective layer using a cover layer, the impurity ions in the semiconductor substrate can continue to diffuse into the first region of the protective layer, which is advantageous for further reducing defects in the region of the semiconductor substrate corresponding to the first region of the protective layer. Then, when the second region is etched and removed, at least a part of the thickness of the first region of the protective layer can be left, and during the texturing process, the region of the semiconductor substrate corresponding to the second region of the protective layer forms a textured surface region, and the first region of the protective layer can prevent the corresponding region of the semiconductor substrate from being etched, and then the first region of the protective layer is etched and removed, so that the region of the semiconductor substrate corresponding to the first region of the protective layer forms a smooth surface region, and the concentration of impurity ions in the smooth surface region of the semiconductor substrate is low, so that the defect density of the semiconductor substrate is low.
[0038] In one embodiment of the present application, the hollow area includes at least a plurality of spaced apart strip-shaped openings, the strip-shaped openings being parallel to one another, and the hollow area can be used to fabricate a primary grid and form a structure without a secondary grid electrode.
[0039] In one embodiment, the step of forming a protective layer on any one side of the semiconductor substrate includes the steps of coating an undercoat film over the entire surface of any one side of the semiconductor substrate, and performing a diffusion annealing process on the undercoat film, whereby the undercoat film reacts with a surface on one side of the semiconductor substrate to form an ion-doped protective layer and migrate impurities in the semiconductor substrate to the protective layer.
[0040] As can be understood, by performing a diffusion annealing process on the underlayer, the impurity ions in the semiconductor substrate can diffuse into the protective layer faster and react more thoroughly.
[0041] In one embodiment, the step of thickening the first region of the protective layer includes the steps of using the cover layer as a mask to coat a surface film on the surface of the first region, and performing a diffusion annealing treatment on the surface film to increase the thickness of the first region.
[0042] As can be understood, the cover layer can limit the coating position and area of the surface film, and cover layers having different shapes and structures are used according to specific application scenarios. The embodiments of the present application do not specifically limit the shape and structure of the cover layer.
[0043] In one embodiment, the cover layer comprises a quartz material, and the present embodiment is not specifically limited thereto, so long as the cover layer does not melt or deform under high temperature conditions.
[0044] In one embodiment, the base film and the overcoat film are liquid source films, hi other embodiments, the base film and the overcoat film may be formed by vapor deposition.
[0045] In one embodiment, the base film and the top film are phosphorus-containing liquid source films, and the top film has a phosphorus concentration greater than the phosphorus concentration of the base film.
[0046] As can be seen, the protective layer has a sparse structure, the surface film can penetrate into the protective layer made of the undercoat film and contact and react with the surface of the semiconductor substrate, and the phosphorus concentration of the surface film is greater than the phosphorus concentration of the undercoat film, which is favorable for the phosphorus element in the surface film to diffuse into the protective layer made of the undercoat film, and the protective layer made of the undercoat film can continue to react with the semiconductor substrate.
[0047] In one embodiment, the duration of the diffusion annealing treatment of the top film is longer than the duration of the diffusion annealing treatment of the undercoat film.
[0048] In one embodiment, the temperature of the diffusion annealing treatment of the top film is higher than the temperature of the diffusion annealing treatment of the base film.
[0049] In one embodiment, the parameters for both the step of etching and removing the first region of the protective layer and the step of etching and removing the second region of the protective layer are as follows: the etching solution used is a mixture of an aqueous hydrofluoric acid solution, an aqueous hydrochloric acid solution, and a water-soluble solvent; the concentration of the aqueous hydrofluoric acid solution is 35% by mass to 50% by mass, the concentration of the aqueous hydrochloric acid solution is 30% by mass to 50% by mass, the volume fraction of the aqueous hydrofluoric acid solution is 1% to 4%, and the volume fraction of the aqueous hydrochloric acid solution is 1% to 3%, and the etching time is 100 s to 300 s.
[0050] In one or more embodiments of the present application, the step of forming a smooth surface region and a textured surface region adjacent to the smooth surface region on at least one side of the semiconductor substrate includes a step of forming a first smooth surface region and a first textured surface region adjacent to the first smooth surface region on one side of the semiconductor substrate, where the area of the first smooth surface region is equal to or larger than the area of the first textured surface region, and / or a step of forming a second smooth surface region and a second textured surface region adjacent to the second smooth surface region on the other side of the semiconductor substrate, where the area of the second smooth surface region is equal to or larger than the area of the second textured surface region. Hereinafter, the method for processing a semiconductor substrate of the present application will be described in detail by taking as an example a case in which a first smooth surface region and a first textured surface region are formed on one side of a semiconductor substrate and a second smooth surface region and a second textured surface region are formed on the other side of the semiconductor substrate.
[0051] Hereinafter, the process of processing the semiconductor substrate will be specifically described with reference to FIGS.
[0052] FIG. 2 shows an unprocessed semiconductor substrate 100 according to an embodiment of the present application.
[0053] The material of the semiconductor substrate 100 includes single crystal silicon. In other embodiments, the material of the semiconductor substrate is other semiconductor materials such as germanium or silicon germanium. The material of the semiconductor substrate can also be other semiconductor materials.
[0054] In this embodiment, the conductivity type of the semiconductor substrate 100 is N-type, and the semiconductor substrate is used for manufacturing solar cells.
[0055] Referring to FIG. 3, a first protective layer is formed on one side of a semiconductor substrate 100 .
[0056] Specifically, a first base film is coated over the entire one side of the semiconductor substrate 100, and a first diffusion annealing process is performed so that the first base film reacts with the one side of the semiconductor substrate to form a first protective layer doped with ions, and impurities in the semiconductor substrate are transported to the first protective layer.
[0057] Specifically, the first undercoat film is a liquid source film. In one embodiment, the first undercoat film is a phosphorus-containing liquid source film.
[0058] Specifically, the first diffusion annealing process is a high-temperature annealing process in which the semiconductor substrate 100 coated with the first underlayer is placed in an oven or a hot stage and baked, so that phosphorus in the first underlayer is sufficiently diffused into the semiconductor substrate 100 and reacts with impurities in the semiconductor substrate 100 to form the first protective layer 210 having a sparse structure. The baking temperature is 650°C to 900°C, for example, 650°C, 700°C, 800°C, 850°C, or 900°C, and the baking time is 120s to 1200s, for example, 120s, 150s, 200s, 250s, 300s, 350s, 400s, 450s, 500s, 600s, 700s, 800s, 900s, 950s, 1000s, 1050s, 1100s, 1150s, or 1200s.
[0059] Referring to FIG. 4, a second protective layer is formed on the other side of the semiconductor substrate 100 .
[0060] Specifically, a second base film is coated over the entire other side of the semiconductor substrate 100, and a third diffusion annealing process is performed to cause the second base film to react with the other side of the semiconductor substrate to form a second protective layer doped with ions, and impurities in the semiconductor substrate are transported to the second protective layer.
[0061] Specifically, the second priming film is a liquid source film and may be the same or different from the first priming film, hi one embodiment, the second priming film and the first priming film are the same.
[0062] Specifically, the third diffusion annealing is a high temperature annealing process. It can be understood that the process method and effect of the third diffusion annealing are basically similar to those of the first diffusion annealing, and will not be described again here.
[0063] Referring to FIG. 5, a patterned first cover layer is provided on a surface of the first protective layer 210 opposite the semiconductor substrate 100, the first cover layer having a first hollow area with a plurality of parallel strip-shaped openings, the first protective layer 210 including a first area 310 located at the bottom of the first hollow area and a second area shielded by the first cover layer, and after providing the patterned first cover layer, the first area 310 of the first protective layer 210 is thickened.
[0064] Specifically, referring to FIG. 11 , the first cover layer includes a first cover body 810 and a first hollow area 820. In this embodiment, the first hollow area 820 is a hollow structure with a plurality of strip-shaped openings uniformly distributed in the first cover body 810. In other embodiments, the first hollow area 820 may have other shapes, for example, the first hollow area is a mesh-like hollow structure regularly arranged in the first cover body 810, which is suitable for forming a grid electrode structure including a main grid and a secondary grid, where a plurality of main grids are parallel to each other, the main grids and the primary grids are arranged parallel to each other, the main grids and the secondary grids are arranged perpendicularly or at any angle, and the width and height of the secondary grids are smaller than the width and height of the main grids, respectively; and the first hollow area may also be a hollow structure irregularly arranged in the first cover body 810 or a hollow structure having a different shape, which is suitable for forming grid lines with a special pattern. The shape and layout of the first hollow area 820 corresponds to the shape and layout of the grid lines of the final formed solar cell, and there is no limitation here as to what hollow structure the cover layer may have.
[0065] Specifically, the first surface layer is coated on the surface of the first region 310, and the second diffusion annealing process is performed to make the first surface layer a part of the first protective layer 210, thereby increasing the thickness of the first region 310. The first surface layer and the first undercoat film have the same components. The phosphorus concentration of the first surface layer is higher than that of the first undercoat film, which is advantageous for the phosphorus of the first surface layer to sufficiently penetrate the first protective layer 210 and react with the impurities in the semiconductor substrate 100.
[0066] In the above embodiment, because the first protective layer 210 has a sparse structure, the first surface layer film can directly penetrate into the surface of the semiconductor substrate 100 through the first region 310 of the first protective layer 210, and diffuse into the semiconductor substrate 100 to react with the impurities in the semiconductor substrate 100; and the phosphorus inside the first region 310 of the first protective layer 210 can still participate in the gettering reaction to provide a high concentration of the first surface layer film, and can supplement the first region 310 of the first protective layer 210 with phosphorus, so that the first region 310 of the first protective layer 210 can continue to react with the impurities in the semiconductor substrate 100, and finally increase the thickness of the first region 310 of the first protective layer 210. As can be seen, although a part of the first surface layer film can penetrate into the second region of the first protective layer 210, the amount of the first surface layer film that penetrates into the second region is very small and can be negligible compared with the first region 310 of the first protective layer 210.
[0067] Specifically, the second diffusion annealing is a high-temperature annealing process. The process method of the second diffusion annealing is the same as that of the first diffusion annealing, only the temperature and time are different. The temperature of the second diffusion annealing is higher than that of the first diffusion annealing, and the time of the second diffusion annealing is longer than that of the first diffusion annealing, which is favorable for the phosphorus of the first surface layer to fully penetrate the first protective layer 210 and react with the impurities in the semiconductor substrate 100, and can improve the reaction activity between the phosphorus of the first surface layer and the phosphorus in the first protective layer 210 and the impurities in the semiconductor substrate.
[0068] In one embodiment, the first cover layer is a quartz material, which has low cost, can be reused after cleaning, and can play a buffering role during the second diffusion annealing process to protect the semiconductor substrate 100 and reduce the risk of damage to the silicon wafer.
[0069] Specifically, after forming the first protective layer, a first cover layer is placed on the surface of the first protective layer opposite to the semiconductor substrate 100. During the subsequent second diffusion annealing treatment, the semiconductor substrate 100 can be protected due to the presence of the first cover layer.
[0070] Referring to FIG. 6, a patterned second cover layer is provided on the surface of the second protective layer 220 opposite the semiconductor substrate 100, the second cover layer having a second hollow region, the second protective layer 220 including a third region 320 located at the bottom of the second hollow region and a fourth region shielded by the second cover layer, and after providing the patterned second cover layer, the third region 320 of the second protective layer 220 is thickened.
[0071] Specifically, depending on the particular application scenario, the second cover layer may be the same as or different from the first cover layer, and the shape and layout of the second hollow region of the second cover layer may correspond to the shape and layout of the gridlines of the ultimately formed solar cell.
[0072] Specifically, the surface of the third region 320 is coated with a second surface layer film, and a fourth diffusion annealing process is performed to make the second surface layer film a part of the second protective layer, thereby increasing the thickness and forming the third region 320. The second surface layer film and the second underlayer film have the same components. The phosphorus concentration of the second surface layer film is higher than the phosphorus concentration of the second underlayer film, which is advantageous for the phosphorus of the second surface layer film to sufficiently penetrate the second protective layer 220 and react with the impurities in the semiconductor substrate 100.
[0073] In the above embodiment, because the second protective layer 220 has a sparse structure, the second surface layer film can directly penetrate into the surface of the semiconductor substrate 100 through the third region 320 of the second protective layer 220, and diffuse into the semiconductor substrate 100 to react with the impurities in the semiconductor substrate 100; and the phosphorus in the third region 320 of the second protective layer 220 can still participate in the gettering reaction to provide a high concentration of the second surface layer film, and can supplement the third region 320 of the second protective layer 220 with phosphorus, so that the third region 320 of the second protective layer 220 can continue to react with the impurities in the semiconductor substrate 100, and finally increase the thickness of the third region 320 of the second protective layer 220. As can be seen, although a part of the second surface layer film can penetrate into the fourth region of the second protective layer 220, the amount of the second surface layer film that penetrates into this region is very small and can be negligible compared with the third region 320 of the second protective layer 220.
[0074] Specifically, the fourth diffusion annealing is a high-temperature annealing process. The process method of the fourth diffusion annealing is the same as that of the third diffusion annealing, only the temperature and time are different. The temperature of the fourth diffusion annealing is higher than that of the third diffusion annealing, and the time of the fourth diffusion annealing is longer than that of the third diffusion annealing, which is favorable for the phosphorus of the second surface layer to fully penetrate the second protective layer 220 and react with the impurities in the semiconductor substrate 100, and can improve the reaction activity between the phosphorus of the second surface layer and the phosphorus in the second protective layer 220 and the impurities in the semiconductor substrate.
[0075] In one embodiment, the second cover layer is a quartz material, which has low cost, can be reused after cleaning, and can play a buffering role in the fourth diffusion annealing process to protect the semiconductor substrate 100 and reduce the risk of damage to the silicon wafer.
[0076] In this embodiment, after the second diffusion annealing process, a second cover layer is installed on the surface of the second protective layer, and during the process of performing the fourth diffusion annealing process, the second cover layer is not removed and continues to play a buffering role, protecting the semiconductor layer substrate 100 and reducing the risk of damage to the silicon wafer.
[0077] Referring to FIG. 7, after thickening the first region 310 of the first protective layer 210, the first cover layer is removed, and after removing the first cover layer, the second region of the first protective layer 210 is etched and removed using the first region 310 of the first protective layer 210 as protection.
[0078] Specifically, the parameters for etching and removing the second region of the first protective layer 210 are as follows: the etchant used is a mixture of hydrofluoric acid solution, hydrochloric acid solution, and water-soluble solvent, the concentration of the hydrofluoric acid solution is 35% by mass to 50% by mass, the concentration of the hydrochloric acid solution is 30% by mass to 50% by mass, the volume fraction of the hydrofluoric acid solution is 1% to 4%, the volume fraction of the hydrochloric acid solution is 1% to 3%, and the etching time is 100 s to 300 s. For example, the parameters for etching and removing the second region of the first protective layer 210 are as follows: the etchant is a 48% hydrofluoric acid solution and a 37% hydrochloric acid solution, the volume fraction of the hydrofluoric acid solution is 3%, the volume fraction of the hydrochloric acid solution is 2%, and the etching time is 150 s.
[0079] Referring to FIG. 8 , after thickening the third region 320 of the second protective layer 220, the second cover layer is removed, and after removing the second cover layer, the fourth region of the second protective layer 220 is removed while using the third region 320 of the second protective layer 220 as protection.
[0080] Specifically, the fourth region of the second protective layer 220 is etched and removed, and the parameters for etching and removing the fourth region of the second protective layer 220 are similar to the parameters for etching and removing the second region of the first protective layer 210 described above, and will not be described repeatedly here.
[0081] In this embodiment, the second region of the first protective layer 210 of the semiconductor substrate 100 is etched and removed, and then the fourth region of the second protective layer 220 of the semiconductor substrate 100 is etched and removed. In another embodiment, the fourth region of the second protective layer 220 of the semiconductor substrate 100 is etched and removed, and then the second region of the first protective layer 210 of the semiconductor substrate 100 is etched and removed. In yet another embodiment, the second region of the first protective layer 210 of the semiconductor substrate 100 and the fourth region of the second protective layer 220 of the semiconductor substrate 100 are etched and removed simultaneously.
[0082] 9, the semiconductor substrate 100 exposed from the first region 310 is subjected to a texturing process to form a first textured surface region 111 of the semiconductor substrate 100, and the semiconductor substrate 100 exposed from the third region 320 is subjected to a texturing process to form a second textured surface region 121 of the semiconductor substrate 100. In one embodiment, the semiconductor substrate 100 exposed from the first region 310 is first subjected to a texturing process to form the first textured surface region 111 of the semiconductor substrate 100, and then the semiconductor substrate 100 exposed from the third region 320 is subjected to a texturing process to form the second textured surface region 121 of the semiconductor substrate 100. In another embodiment, the semiconductor substrate 100 exposed from the third region 320 is first subjected to a texturing process to form the second textured surface region 121 of the semiconductor substrate 100, and then the semiconductor substrate 100 exposed from the first region 310 is subjected to a texturing process to form the first textured surface region 111 of the semiconductor substrate 100. In yet another embodiment, a step of performing a texturing process on the semiconductor substrate 100 exposed from the first region 310 to form a first textured surface region 111 of the semiconductor substrate 100 and a step of performing a texturing process on the semiconductor substrate 100 exposed from the third region 320 to form a second textured surface region 121 of the semiconductor substrate 100 are performed simultaneously.
[0083] Specifically, the texturing treatment includes treatment with a texturing agent. In one embodiment, the texturing agent is a 2% to 5% potassium hydroxide aqueous solution, for example, the texturing agent is a 2% potassium hydroxide aqueous solution, a 3% potassium hydroxide aqueous solution, a 4% potassium hydroxide aqueous solution, or a 5% potassium hydroxide aqueous solution, the time of the texturing treatment is 150s to 300s, for example, 150s, 180s, 200, 250s, 280s, or 300s, and the temperature is 60°C to 70°C, for example, 60°C, 62°C, 65°C, 67°C, or 70°C.
[0084] 10, the first region 310 is etched away to form the first smooth surface region 112 of the semiconductor substrate 100, and the third region 320 is etched away to form the second smooth surface region 122 of the semiconductor substrate 100. In one embodiment, the first region 310 is etched away to form the first smooth surface region 112 of the semiconductor substrate 100, and then the third region 320 is etched away to form the second smooth surface region 122 of the semiconductor substrate 100. In another embodiment, the third region 320 is etched away to form the second smooth surface region 122 of the semiconductor substrate 100, and then the first region 310 is etched away to form the first smooth surface region 112 of the semiconductor substrate 100. In yet another embodiment, the steps of etching away the first region 310 to form the first smooth surface region 112 of the semiconductor substrate 100 and etching away the third region 320 to form the second smooth surface region 122 of the semiconductor substrate 100 are performed simultaneously.
[0085] Specifically, the first region 310 and the third region 320 are etched away. The parameters for etching away the first region 310 and the third region 320 are similar to the parameters for etching away the second region of the first protective layer 210 and the parameters for etching away the fourth region of the second protective layer 220, and will not be described again here.
[0086] In another embodiment of the present application, one side of the semiconductor substrate 100 is processed to form a first smooth surface region 112 and a first textured surface region 111 adjacent to the first smooth surface region 112, and then the other side of the semiconductor substrate 100 is processed to form a second smooth surface region 122 and a second textured surface region 121 adjacent to the second smooth surface region 122.
[0087] Specifically, a first region 310 and a second region of the first protective layer 210 are formed on one side of the semiconductor substrate 100, and using the first region 310 of the first protective layer 210 as protection, the second region of the first protective layer 210 is etched and removed, and a texturing process is performed on the semiconductor substrate 100 exposed from the first region 310 of the first protective layer 210 to form a first textured surface region 111, and the first region 310 of the first protective layer 210 is etched and removed to form a first smooth surface region 112. Then, a third region 320 and a fourth region of the second protective layer 220 are formed on the other side of the semiconductor substrate 100, and using the third region 320 of the second protective layer 220 as protection, the fourth region of the second protective layer 220 is etched and removed, and a texturing process is performed on the semiconductor substrate 100 exposed from the third region 320 of the second protective layer 220 to form a second textured surface region 121, and the third region 320 of the second protective layer 220 is etched and removed to form a second smooth surface region 122.
[0088] One or more embodiments of the present application further provide a semiconductor substrate having, on at least one surface thereof, a smooth surface region and a textured surface region adjacent to the smooth surface region, the area of the smooth surface region being equal to or greater than the area of the textured surface region.
[0089] Referring to FIG. 10, in one embodiment, one side of the semiconductor substrate 100 has a first smooth surface region 112 and a first textured surface region 111 adjacent to the first smooth surface region 112, and / or the other side of the semiconductor substrate 100 has a second smooth surface region 122 and a second textured surface region 121 adjacent to the second smooth surface region 122.
[0090] As can be understood, the semiconductor substrate 100 in the above embodiment is manufactured by the above semiconductor substrate processing method, and has the same beneficial effects, which will not be described again here.
[0091] In one embodiment, the area of the first smooth surface region 112 is greater than or equal to the area of the first textured surface region 111, for example, the ratio of the area of the first smooth surface region 112 to the area of the first textured surface region 111 is 1:1 to 1.2:1, for example, the ratio of the area of the first smooth surface region 112 to the area of the first textured surface region 111 is 1:1, 1.05:1, 1.1:1, 1.15:1 or 1.2:1, and / or the area of the second smooth surface region 122 is greater than or equal to the area of the second textured surface region 121, for example, the ratio of the area of the second smooth surface region 122 to the area of the second textured surface region 121 is 1:1 to 1.2:1, for example, the ratio of the area of the second smooth surface region 122 to the area of the second textured surface region 121 is 1:1, 1.05:1, 1.1:1, 1.15:1 or 1.2:1.
[0092] As can be seen, in the solar cell, the first smooth surface region 112 or the second smooth surface region 122 corresponds to the transparent conductive film and the grid line, and by increasing the area of the first smooth surface region 112 or the area of the second smooth surface region 122, the above-mentioned functional layers can be in sufficient contact with each other, which is advantageous for reducing the series resistance of the solar cell, increasing the current, reducing unnecessary power loss, and improving the photoelectric conversion performance of the solar cell. In addition, the first smooth surface region 112 and the second smooth surface region 122 both have flat surfaces, which is advantageous for uniform deposition of other material layers in the regions, and the concentration of impurity ions inside the first smooth surface region 112 and the second smooth surface region 122 is low, which reduces the probability that photogenerated carriers are captured by defects in the semiconductor substrate, and is further advantageous for improving the photoelectric conversion efficiency.
[0093] One or more embodiments of the present application further provide a method for manufacturing a solar cell, including the steps of: providing a semiconductor substrate; processing the semiconductor substrate using the above-described semiconductor substrate processing method so as to provide at least one surface of the semiconductor substrate with a smooth surface region and a textured surface region adjacent to the smooth surface region; forming a transparent conductive film located only on the smooth surface region on the side of the semiconductor substrate having the smooth surface region and the textured surface region; and forming grid lines in at least a portion of the transparent conductive film on the side opposite the semiconductor substrate.
[0094] Specifically, the transparent conductive film is disposed opposite the smooth surface region, that is, the area of the orthogonal projection of the transparent conductive film on the textured surface region is zero.
[0095] In one embodiment, the method for manufacturing a solar cell further includes, prior to forming the transparent conductive film, forming a doped semiconductor layer located between the semiconductor substrate and the transparent conductive film on the side of the semiconductor substrate having the smooth surface region and the textured surface region.
[0096] In one embodiment, prior to forming the doped semiconductor layer, an intrinsic semiconductor layer is formed on the side of the semiconductor substrate having the smooth surface region and the textured surface region, the intrinsic semiconductor layer being located between the semiconductor substrate and the doped semiconductor layer.
[0097] In the solar cell according to the present application, the transparent conductive film and the grid lines are both located only in the smooth surface region, and the smooth surface region has a smooth surface, which is favorable for uniform deposition of the transparent conductive film and the grid lines in the smooth surface region, the flat and smooth surface region is favorable for sufficient contact between the transparent conductive film and the grid lines and reduced series resistance, and the textured surface region can provide an excellent light trapping effect. The solar cell according to the present application can achieve both the light trapping effect and low series resistance, which is favorable for improving the photoelectric conversion efficiency of the solar cell.
[0098] As can be understood, the smooth surface region and the textured surface region may be formed on only one surface of the semiconductor substrate, and then a solar cell may be manufactured, or the smooth surface region and the textured surface region may be formed on both surfaces of the semiconductor substrate, and then a solar cell may be manufactured. In the following, the solar cell manufacturing method of the present application will be described in detail, taking as an example the simultaneous formation of solar cells on both sides of the semiconductor substrate.
[0099] Hereinafter, the manufacturing process of the solar cell will be specifically described with reference to FIGS.
[0100] 12 and 13, a first intrinsic semiconductor layer 410 is formed on a side of the semiconductor substrate 101 having a first smooth surface region and a first textured surface region, and a second intrinsic semiconductor layer 420 is formed on a side of the semiconductor substrate 101 having a second smooth surface region and a second textured surface region. For example, the first intrinsic semiconductor layer 410 and the second intrinsic semiconductor layer 420 include amorphous silicon or microcrystalline silicon and play a role of passivation.
[0101] As can be seen, since the first smooth surface region has a flat surface, the first intrinsic semiconductor layer 410 can be uniformly deposited on the first smooth surface region, thereby improving the uniformity of the first intrinsic semiconductor layer 410, further improving the passivation effect, and finally achieving the purpose of improving the photoelectric conversion efficiency of the solar cell.
[0102] 14 and 15, a first doped semiconductor layer 510 is formed on the side of the first intrinsic semiconductor layer 410 opposite the semiconductor substrate 101, and a second doped semiconductor layer 520 is formed on the side of the second intrinsic semiconductor layer 420 opposite the semiconductor substrate 101. For example, the first doped semiconductor layer 510 is N-type doped amorphous silicon or N-type doped microcrystalline silicon, and the second doped semiconductor layer 520 is P-type doped amorphous silicon or P-type doped microcrystalline silicon, or vice versa.
[0103] 16 and 17, a first transparent conductive film 610 is formed on a portion of the first doped semiconductor layer 510 opposite to the first smooth surface region, and a second transparent conductive film 620 is formed on a portion of the second doped semiconductor layer 520 opposite to the second smooth surface region, in a second transparent conductive film 620. For example, the first transparent conductive film 610 and the second transparent conductive film 620 are indium-doped tin oxide.
[0104] Specifically, the first transparent conductive film 610 is disposed opposite the first smooth surface region, and the area of the orthogonal projection of the first transparent conductive film 610 on the first textured surface region is 0. The second transparent conductive film 620 is disposed opposite the second smooth surface region, and the area of the orthogonal projection of the second transparent conductive film 620 on the second textured surface region is 0.
[0105] 18 and 19, a first grid line 710 is formed on the first transparent conductive film 610 on the side opposite to the first doped semiconductor layer 510, and a second grid line 720 is formed on the second transparent conductive film 620 on the side opposite to the second doped semiconductor layer 520. Exemplarily, the first grid line 710 and the second grid line 720 are made of silver.
[0106] In another embodiment, a method for manufacturing a solar cell includes the steps of sequentially forming a first intrinsic semiconductor layer 410, a first doped semiconductor layer 510, a first transparent conductive film 610 and a first grid line 710 on a side of the semiconductor substrate 101 having a first smooth surface region 112 and a first textured surface region 111, and then sequentially forming a second intrinsic semiconductor layer 420, a second doped semiconductor layer 520, a second transparent conductive film 620 and a second grid line 720 on a side of the semiconductor substrate 101 having a second smooth surface region 122 and a second textured surface region 121.
[0107] Specifically, the method for manufacturing a solar cell in this embodiment differs from the method for manufacturing a solar cell in the above embodiment only in the order in which each functional layer is formed on both sides of the semiconductor substrate 101; the other parameters are the same, and therefore will not be repeatedly described here.
[0108] One or more embodiments of the present application further provide a solar cell including: a semiconductor substrate having, on at least one side thereof, a smooth surface region and a textured surface region adjacent to the smooth surface region, the area of the smooth surface region being equal to or greater than the area of the textured surface region; a transparent conductive film located on the side of the semiconductor substrate having the smooth surface region and the textured surface region, and located only on the smooth surface region; and grid lines located on at least a portion of the transparent conductive film on the side opposite the semiconductor substrate, and located only on the transparent conductive film.
[0109] In one embodiment, the semiconductor substrate includes a first smooth surface region located on one side of the semiconductor substrate and a first textured surface region adjacent to the first smooth surface region, and / or a second smooth surface region located on the other side of the semiconductor substrate and a second textured surface region adjacent to the second smooth surface region, and a doped semiconductor layer located between the semiconductor substrate and the transparent conductive film. Optionally, the solar cell further includes an intrinsic semiconductor layer located between the semiconductor substrate and the doped semiconductor layer. The above structure is an important structure for generating photogenerated carriers.
[0110] In one specific example of the present application, a solar cell includes a first intrinsic semiconductor layer and a second intrinsic semiconductor layer, the first intrinsic semiconductor layer being located between a first doped semiconductor layer and a side of a semiconductor substrate having a first smooth surface region and a first textured surface region, and the second intrinsic semiconductor layer being located between the second doped semiconductor layer and a side of the semiconductor substrate having a second smooth surface region and a second textured surface region, a first doped semiconductor layer and a second doped semiconductor layer, the first doped semiconductor layer being located on a side opposite the first intrinsic semiconductor layer to the semiconductor substrate, and the second doped semiconductor layer being located on a side opposite the second intrinsic semiconductor layer to the semiconductor substrate, and a first transparent conductive film and a second transparent conductive film, the first transparent conductive film being the first doped semiconductor layer. a first transparent conductive film and a second transparent conductive film, each of which is located on an opposite side of the first intrinsic semiconductor layer of the second doped semiconductor layer, the first transparent conductive film being located only in the first smooth surface region and the second transparent conductive film being located on an opposite side of the second doped semiconductor layer to the second intrinsic semiconductor layer and the second transparent conductive film being located only in the second smooth surface region; and a first grid line and a second grid line, each of which is located on an opposite side of the first transparent conductive film to the first doped semiconductor layer, the first grid line being located only in the first smooth surface region and an area of the first grid line is equal to or less than an area of the first transparent conductive film, and the second grid line is located on an opposite side of the second transparent conductive film to the second doped semiconductor layer, the second grid line being located only in the second smooth surface region and an area of the second grid line is equal to or less than an area of the second transparent conductive film.
[0111] As can be understood, the solar cell of the above embodiment includes the semiconductor substrate obtained in the above embodiment, and therefore can achieve the same beneficial effects as the semiconductor substrate, which will not be described again here.
[0112] The solar cell of the present application will be described below with reference to test examples and comparative examples of specific embodiments.
[0113] Test Example: A semiconductor substrate is provided, the material of the semiconductor substrate is single crystal silicon and has a thickness of 100 μm to 180 μm, one side of the semiconductor substrate has a first smooth surface region and a first textured surface region adjacent to the first smooth surface region, and the other side of the semiconductor substrate has a second smooth surface region and a second textured surface region adjacent to the second smooth surface region. A first intrinsic semiconductor layer is formed on the side of the semiconductor substrate having the first smooth surface region and the first textured surface region, the material of the first intrinsic semiconductor layer is amorphous silicon and has a thickness of 5 nm to 10 nm, and a second intrinsic semiconductor layer is formed on the side of the semiconductor substrate having the second smooth surface region and the second textured surface region, the material of the second intrinsic semiconductor layer is amorphous silicon and has a thickness of 5 nm to 10 nm. A first doped semiconductor layer is formed on the first intrinsic semiconductor layer, the material of the first doped semiconductor layer is N-type doped amorphous silicon and has a thickness of 5 nm to 15 nm, and a second doped semiconductor layer is formed on the second intrinsic semiconductor layer, the material of the second doped semiconductor layer is P-type doped amorphous silicon and has a thickness of 5 nm to 15 nm. A first transparent conductive film is formed on the first doped semiconductor layer, the material of the first transparent conductive film is ITO and has a thickness of 80 nm to 100 nm, the first transparent conductive film is disposed opposite the first smooth surface region, and the area of the orthogonal projection on the first textured surface region is 0. A second transparent conductive film is formed on the second doped semiconductor layer, the material of the second transparent conductive film is ITO and has a thickness of 80 nm to 100 nm, the second transparent conductive film is disposed opposite the second smooth surface region, and the area of the orthogonal projection on the second textured surface region is 0. A silver paste was deposited on the first transparent conductive film to form the first grid lines, which had a thickness of 10 μm to 20 μm, and a silver paste was deposited on the second transparent conductive film to form the second grid lines, which had a thickness of 10 μm to 20 μm.
[0114] Comparative Example: Except that both sides of the semiconductor substrate are textured, the other manufacturing methods and parameters of this comparative example are the same as those of the test example.
[0115] A photoelectric conversion performance conversion test was carried out on the solar cells manufactured in the above test examples and comparative examples, and the data in Table 1 was obtained. [Table 1]
[0116] Here, I SC : Short circuit current, U OC : Open circuit voltage, FF: Fill factor, E ta : Photoelectric conversion efficiency, R ser : Series resistance, R shunt :Parallel resistance.
[0117] From the data in Table 1, it can be seen that compared to the solar cell using the conventional semiconductor substrate having textured surfaces on both sides in the comparative example, the fill factor of the solar cell in the test example was 0.84% higher, the short circuit current increased by 5 mA, the open circuit voltage increased by 1 mV, the series resistance decreased by 0.56 mΩ, and the photoelectric conversion efficiency increased by 0.2604%.
[0118] As can be seen from this, in the test example, a semiconductor substrate having a surface with a smooth surface region and a textured surface region is used, the first grid line and the first transparent conductive film are arranged opposite the first smooth surface region and are designed not to cover the first textured surface region, and the second grid line and the second transparent conductive film are arranged opposite the second smooth surface region and are designed not to cover the second textured surface region, so that the deposition of each functional layer is more uniform, which is favorable for reducing the series resistance and increasing the open circuit voltage, and the contact resistance between the polished region (smooth surface region) and the metallized electrode is lower, and the series resistance (R ser ) is also significantly reduced, which is beneficial for improving the extraction efficiency of photo-generated carriers by the first grid lines and the second grid lines. Even if the area of the textured surface region is reduced, the short-circuit current can still be increased, which can ultimately improve the photoelectric conversion efficiency of the solar cell and increase the cell efficiency.
[0119] Obviously, the above test examples are merely illustrative and do not limit the embodiments. Those skilled in the art can make various other changes or modifications based on the above description. It is not necessary and cannot be possible to cover all the embodiments here. And, the obvious changes or modifications derived in this way are also within the scope of protection of the present invention. [Explanation of symbols]
[0120] 100 Semiconductor substrate 101 Semiconductor substrate 210 1st protective layer 220 Second protective layer 310 1st area 320 Third area 111 First Texture Surface Area 112 1st smooth surface area 121 Second Texture Surface Area 122 2nd smooth surface area 410 First intrinsic semiconductor layer 420 Second intrinsic semiconductor layer 510 First doped semiconductor layer 520 Second doping semiconductor layer 610 First transparent conductive film 620 Second transparent conductive film 710 First Grid Line 720 Second Grid Line 810 First cover body 820 1st hollow area
Claims
1. A method for processing a semiconductor substrate, comprising the steps of: forming a smooth surface region and a textured surface region adjacent to the smooth surface region on at least one side of the semiconductor substrate; 13. A method for processing a semiconductor substrate, comprising: forming a surface region on a substrate; forming a surface region on the substrate;
2. 2. The method for treating a semiconductor substrate according to claim 1, wherein a ratio of an area of the smooth surface region to an area of the textured surface region is 1:1 to 1.2:
1.
3. The step of forming a smooth surface region and a textured surface region adjacent to the smooth surface region on any one surface of the semiconductor substrate includes: forming a protective layer on any one surface of the semiconductor substrate; providing a patterned cover layer on a surface of the protective layer opposite the semiconductor substrate, the cover layer having a hollow region, the protective layer including a first region at a bottom of the hollow region and a second region shielded by the cover layer; thickening the first region of the protective layer using the cover layer; removing the cover layer after thickening the first region of the protective layer; removing the second region of the protective layer by etching while protecting the first region of the protective layer after removing the cover layer; performing a texturing process on the side of the semiconductor substrate exposed from the protective layer after removing the second region, so that the side of the semiconductor substrate exposed from the protective layer forms the textured surface region; and after forming the textured surface region, etching and removing the first region corresponding to the protective layer so that a portion of the one side surface of the semiconductor substrate forms the smooth surface region; 2. The method of claim 1, wherein the hollow area includes at least a plurality of spaced apart strip-shaped openings, the strip-shaped openings being parallel to one another.
4. forming a protective layer on any one side of the semiconductor substrate, coating an undercoat film over the entire surface of any one side of the semiconductor substrate; performing a diffusion annealing process on the undercoat film, whereby the undercoat film reacts with one surface of the semiconductor substrate to form the protective layer doped with ions, and impurities in the semiconductor substrate are transferred to the protective layer; Preferably, the step of thickening the first region of the protective layer includes the steps of: coating a surface layer film on a surface of the first region using the cover layer as a mask; and performing a diffusion annealing treatment on the surface layer to make the surface layer a part of the protective layer, thereby increasing the thickness of the first region; Preferably, the cover layer comprises a quartz material; Preferably, the undercoat film and the top layer film are liquid source films; Preferably, the undercoat film and the surface layer film are phosphorus-containing liquid source films, and the phosphorus concentration of the surface layer film is greater than the phosphorus concentration of the undercoat film; Preferably, the time of the diffusion annealing treatment of the surface film is longer than the time of the diffusion annealing treatment of the base film, Preferably, the temperature of the diffusion annealing treatment of the surface film is higher than the temperature of the diffusion annealing treatment of the base film, Preferably, for parameters in both the step of etching away the first region of the protective layer and the step of etching away the second region of the protective layer, the etching solution used is a mixture of an aqueous hydrofluoric acid solution, an aqueous hydrochloric acid solution and a water-soluble solution, the concentration of the aqueous hydrofluoric acid solution is 35% by mass to 50% by mass, the concentration of the aqueous hydrochloric acid solution is 30% by mass to 50% by mass, the volume fraction of the aqueous hydrofluoric acid solution is 1% to 4%, the volume fraction of the aqueous hydrochloric acid solution is 1% to 3%, and the etching time is 100 s to 300 s.
5. A semiconductor substrate having, on at least one surface thereof, a smooth surface region and a textured surface region adjacent to the smooth surface region, the area of the smooth surface region being equal to or greater than the area of the textured surface region.
6. 6. The semiconductor substrate of claim 5, wherein a ratio of an area of the smooth surface region to an area of the textured surface region is 1:1 to 1.2:
1.
7. Providing a semiconductor substrate; A step of processing the semiconductor substrate by the method for processing a semiconductor substrate according to any one of claims 1 to 4 so as to provide at least one surface of the semiconductor substrate with a smooth surface region and a textured surface region adjacent to the smooth surface region; forming a transparent conductive film located only on the smooth surface region on a side of the semiconductor substrate having the smooth surface region and the textured surface region; and forming grid lines in at least a portion of the transparent conductive film on a side opposite to the semiconductor substrate.
8. Before forming the transparent conductive film, a doped semiconductor layer is formed on the side of the semiconductor substrate having the smooth surface region and the textured surface region, the doped semiconductor layer being located between the semiconductor substrate and the transparent conductive film; The method for manufacturing a solar cell according to claim 7, characterized in that, preferably, before forming the doped semiconductor layer, an intrinsic semiconductor layer is formed between the semiconductor substrate and the doped semiconductor layer on the side of the semiconductor substrate having the smooth surface region and the textured surface region.
9. a semiconductor substrate having a smooth surface region and a textured surface region adjacent to the smooth surface region on at least one side, the smooth surface region having an area equal to or larger than an area of the textured surface region; a transparent conductive film located on a side of the semiconductor substrate having the smooth surface region and the textured surface region, the transparent conductive film being located only on the smooth surface region; and a grid line located in at least a portion of the transparent conductive film on the side opposite to the semiconductor substrate.
10. The semiconductor substrate further includes a doped semiconductor layer disposed between the semiconductor substrate and the transparent conductive film, 10. The solar cell according to claim 9, further comprising an intrinsic semiconductor layer preferably located between said semiconductor substrate and said doped semiconductor layer.
Citation Information
Patent Citations
Structure for back-face contact solar cells with trench treatment and polysilicon doped areas
JP2011523231A
Photoelectric conversion element
JP2013187287A
Method for manufacturing hetero junction back contact type solar battery and solar battery
JP2018014537A
Solar cell emitter region fabrication with differentiated p-type and n-type architectures and incorporating a multi-purpose passivation and contact layer
US20170077322A1