Atomic Layer Deposition in Acoustic Wave Resonators

Atomic layer deposition of piezoelectric materials addresses the challenges of higher frequency operation and temperature stability in acoustic resonators, enhancing performance through thinner, uniform layers for improved RF communication devices.

JP2024543071APending Publication Date: 2024-11-19MACOM TECH SOLUTIONS HLDG INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024527794
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-16
Filing Date
2022-09-27
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing acoustic resonator technologies face challenges in operating effectively at higher frequencies and maintaining consistent performance across varying temperatures and power levels, particularly in RF communication devices, due to limitations in layer thickness and uniformity of piezoelectric materials.

Method used

The use of atomic layer deposition (ALD) to form thinner, more uniform, and conformal layers of piezoelectric materials such as aluminum nitride (AlN) in acoustic resonators, along with electrodes, to enhance frequency response, quality factor, and temperature stability.

Benefits of technology

ALD enables the production of resonators with improved frequency accuracy, higher piezoelectric coupling, and reduced frequency temperature coefficient, suitable for RF filters and duplexers in wireless communication devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543071000001_ABST
    Figure 2024543071000001_ABST
Patent Text Reader

Abstract

Aspects of acoustic resonators and methods of making acoustic resonators are described, including acoustic resonators with thinner layers of piezoelectric material. In one example, a method of making an acoustic resonator includes providing a substrate (41), depositing a layer of piezoelectric material on the substrate (43) by atomic layer deposition (ALD), and forming electrodes (44, 45) in contact with the layer of piezoelectric material. ALD is used to deposit highly uniform and conformal thin films of piezoelectric material, and possibly electrodes and encapsulation layers (46). The acoustic resonators described herein are better suited to the demands of new radio frequency (RF) filters, duplexers, transformers, and other components in front-end wireless electronics and other applications.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] The piezoelectric effect is exhibited by certain materials and is related to the electromechanical interaction between mechanical and electrical states in a material. Materials that exhibit the piezoelectric effect also exhibit the inverse piezoelectric effect. For example, lead zirconate titanate crystals generate piezoelectricity (i.e., generate a field potential) when a mechanical force is applied to distort the shape of the crystal. Lead zirconate titanate crystals also deform or change shape when an external electric field is applied to the crystal.

[0002] Piezoelectric materials can be classified as either crystalline, ceramic, or polymeric materials. Lead zirconate titanate, barium titanate, and lead titanate are examples of piezoelectric ceramic materials. Certain semiconductor piezoelectric materials are compatible with semiconductor devices and integrated circuits. Gallium nitride and zinc oxide, among others, are examples of piezoelectric materials that are compatible with semiconductor devices and integrated circuits.

[0003] The electromechanical coupling coefficient of a piezoelectric material is a measure of the efficiency of conversion between electrical and mechanical energy in the piezoelectric material. The electromechanical coupling coefficient can include parameters such as the surface to which the electrical potential is applied or formed, and the direction in which the mechanical energy is applied or generated in the material. Summary of the Invention

[0004] Various examples of the use of atomic layer deposition in the fabrication of semiconductor devices, particularly acoustic wave resonators, are described, along with several novel acoustic wave resonator devices that incorporate one or more layers of material deposited using atomic layer deposition. In one example, a method of fabricating an acoustic resonator includes providing a substrate, depositing a layer of piezoelectric material on the substrate by atomic layer deposition, and forming electrodes in contact with the layer of piezoelectric material.

[0005] In some aspects of the embodiment, the electrode is a first electrode and the method also includes forming a second electrode in contact with the piezoelectric material. In one example, the first electrode and the second electrode are formed by sputtering a metal. In another example, the first electrode is formed by atomic layer deposition of a metal and the second electrode is formed by sputtering a metal. In yet another example, the first electrode and the second electrode are both formed by atomic layer deposition of a metal.

[0006] In other aspects, the first electrode and the second electrode are both formed above a layer of piezoelectric material in the stack of material layers of the acoustic resonator, or in other cases, the first electrode is formed below the layer of piezoelectric material and the second electrode is formed above the layer of piezoelectric material in the stack of material layers of the acoustic resonator.

[0007] In another aspect, the method also includes forming an acoustic reflector on the substrate between the substrate and the layer of piezoelectric material. The reflector includes a plurality of layers of material. The layers include alternating layers of materials having different refractive indices. In some cases, the method also includes forming a support layer on the substrate between the substrate and the layer of piezoelectric material. The method also includes forming an air cavity in the substrate in a region beneath the piezoelectric material. In one example, the cavity includes a plurality of support pillars.

[0008] In yet another aspect, the method also includes depositing the layer of piezoelectric material by atomic layer deposition followed by trimming the layer of piezoelectric material. The method can also include forming an encapsulation layer over the electrodes by atomic layer deposition. The piezoelectric material in some cases includes aluminum nitride, although other types of piezoelectric materials can be utilized.

[0009] In another example, an acoustic resonator is described. The acoustic resonator includes a substrate, a layer of piezoelectric material deposited on the substrate by atomic layer deposition, and an electrode in contact with the layer of piezoelectric material. In one example, the layer of piezoelectric material includes a layer of aluminum nitride having a thickness of 100 nm or less. In some cases, the acoustic resonator also includes a second electrode in contact with the piezoelectric material. In one example, at least one of the electrodes, the second electrode, or both electrodes are formed by atomic layer deposition of a metal. The acoustic resonator can include an acoustic reflector on the substrate between the substrate and the layer of piezoelectric material. The acoustic wave reflector can also include a support layer on the substrate between the substrate and the layer of piezoelectric material, among other layers.

[0010] Aspects of the present disclosure can be better understood with reference to the following drawings: It should be noted that the elements in the drawings are not necessarily to scale, emphasis instead being placed upon clearly illustrating the principles of the embodiments. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 illustrates a perspective view of an exemplary bulk acoustic wave (BAW) resonator structure according to various embodiments described herein. [Diagram 2] 1 is a perspective view of an exemplary surface acoustic wave (SAW) resonator structure according to various embodiments described herein. [Diagram 3] 1 is a cross-sectional view of an exemplary solid-mount bulk acoustic wave resonator structure according to various embodiments described herein. [Figure 4] 4 illustrates an exemplary method for fabricating the resonator structure shown in FIG. 3 according to various embodiments described herein. [Diagram 5] 1 is a cross-sectional view of an exemplary thin film bulk acoustic resonator according to various embodiments described herein. [Figure 6] 6 illustrates an exemplary method for fabricating the resonator structure shown in FIG. 5 according to various embodiments described herein. [Figure 7]3 illustrates an exemplary method for fabricating the SAW resonator shown in FIG. 2 according to various embodiments described herein. [Figure 8] 1 is a cross-sectional view of an exemplary laterally excited bulk acoustic wave resonator in accordance with various embodiments described herein. [Figure 9] 4 is a cross-sectional view of another exemplary laterally excited bulk acoustic wave resonator in accordance with various embodiments described herein. [Figure 10] 10 illustrates an exemplary method for fabricating the resonator structure shown in FIGS. 8 and 9 according to various embodiments described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Acoustic resonators can be formed as structures including a layer of piezoelectric material with electrodes in contact with one or more surfaces of the piezoelectric material. Characteristics of high performance acoustic resonators include, among others, precise frequency response, high quality factor, high piezoelectric coupling or bandwidth, and small temperature coefficient of frequency.

[0013] Different types and structures of acoustic wave resonators have been utilized as oscillators, radio frequency (RF) filters, duplexers, and transformers in electrical circuits, as components in micro-electromechanical systems (MEMS), and for other purposes. Examples of acoustic resonators include bulk acoustic wave (BAW) resonators and surface acoustic wave (SAW) resonators. Examples of BAW resonators include solidly mounted resonators (SMR) and thin-film bulk acoustic resonators (FBAR), as described in more detail below. Similar to SAW resonators, the operation of BAW resonators is based on the piezoelectric effect exhibited by a layer of piezoelectric material.

[0014] Several different materials can be utilized as the piezoelectric material in a BAW or SAW. As an example, zinc oxide (ZnO) is a relatively common piezoelectric material for high frequency FBAR structures. With some material processing techniques, the stoichiometry of a binary compound material such as ZnO may be easier to control compared to a ternary compound material when fabricated by thin film methods. Relatively thin layers of piezoelectric materials have been formed by sol-gel wet chemical techniques, sputtering, pulsed laser deposition, and other techniques.

[0015] Today, many cellular communication devices include duplexers, filters, and other RF circuits that include one or more acoustic resonators. Cellular communication devices may include several such RF circuits, with acoustic resonators being adopted and utilized on a larger scale due to the increasing complexity of radio frequency front-end electronics. A common application of acoustic wave structures is RF filters for, for example, cell phones, global positioning systems, Wi-Fi systems, and other systems that utilize RF signals for data communication. Such RF filters are often formed using a network of acoustic resonators in ladder, lattice, or stacked topologies and are designed to prevent the transmission of certain frequencies or frequency bands and allow the reception of certain frequencies or frequency bands. BAW filter technology complements SAW filter technology in areas where improved power handling capabilities are needed. Furthermore, BAW structures can be fabricated in large quantities on silicon substrates and are widely supported by current semiconductor device manufacturing methods.

[0016] However, as new applications utilize higher frequencies in the RF spectrum for communications, advances in acoustic resonator technology are needed. Newer communications devices and standards require components capable of operating properly at higher frequencies and with less variation in characteristic response over a wide range of temperatures and power levels.

[0017] In the context outlined above, aspects of resonators and methods of manufacturing acoustic resonators are described, including acoustic resonators with thinner layers of piezoelectric material, thinner electrode layers, and other features that facilitate higher performance. In one example, a method of manufacturing an acoustic resonator includes providing a substrate, depositing a layer of piezoelectric material on the substrate by atomic layer deposition (ALD), and forming electrodes in contact with the layer of piezoelectric material. ALD is used to deposit highly uniform and conformal thin films of piezoelectric material, and possibly electrodes and encapsulation layers. The acoustic resonators described herein are better suited to the demands of new RF filters, duplexers, transformers, and other components in front-end wireless electronics and other applications.

[0018] Referring to the drawings, FIG. 1 illustrates an exemplary BAW resonator 10 according to various embodiments described herein. A diagram of the BAW resonator 10 is shown in FIG. 1. The positions, shapes, dimensions, and relative sizes of the layers and features of the BAW resonator 10 are not necessarily drawn to scale in FIG. 1. Exemplary dimensions of the BAW resonator 10 are shown below, but the dimensions of the BAW resonator 10 are not particularly limited. The layers and other features shown in FIG. 1 are also not exhaustive, and the BAW resonator 10 can include other layers, features, and elements that are not separately illustrated. In addition, the BAW resonator 10 can be combined with other devices and circuit elements to form part of a larger integrated structure or circuit. Such a larger integrated structure can include several resonators similar to the BAW resonator 10, among other integrated components.

[0019] BAW resonator 10 includes a substrate 11, an intermediate region 12 on substrate 11, a layer of piezoelectric material 13 on substrate 11, a first electrode 14, and a second electrode 15. The first electrode 14 is in contact with a first surface (i.e., bottom surface) of piezoelectric material 13 and is at least partially disposed below piezoelectric material 13, between piezoelectric material 13 and substrate 11. The second electrode 15 is in contact with a second surface (i.e., top surface) of piezoelectric material 13 and is at least partially disposed above piezoelectric material 13. BAW resonator 10 may also include additional layers, such as temperature compensation layers, encapsulation layers, and other layers, which are described below but are not shown in FIG. 1 .

[0020] As shown in FIG. 1, the BAW resonator 10 may be embodied as a solid-state mounted resonator, a thin film bulk acoustic wave resonator, or a related type of BAW resonator. An exemplary solid-state mounted resonator (SMR) is described in more detail below with reference to FIG. 3, and an exemplary thin film bulk acoustic resonator (FBAR) is described in more detail below with reference to FIG. 5. In the case of an SMR, the intermediate region 12 may be embodied as an acoustic mirror or reflector, such as a Bragg reflector, as described further below. In the case of an FBAR, the intermediate region 12 may be embodied as a support layer of silicon or other material, and the FBAR may also include a cavity or opening below the piezoelectric material 13 for acoustic wave isolation. In either case, the piezoelectric properties of the layer of piezoelectric material 13 and the structural arrangement of the BAW resonator 10 enable the BAW resonator 10 to generate bulk acoustic or mechanical waves when an alternating potential input signal, such as an RF input, is applied across the electrodes 14 and 15. Bulk acoustic or mechanical waves can travel or translate in the "Z" direction into the BAW resonator 10, as shown in FIG. 1, in the direction in which the thickness of the piezoelectric material 13 is measured.

[0021] Substrate 11 may be embodied as silicon, silicon carbide, lithium niobate, sapphire, glass, ceramic, or another suitable type of substrate suitable for the application. Silicon substrates may be preferred because they are relatively low cost, scalable for manufacturing, and compatible with manufacturing and processing steps, although other substrates may be utilized. As mentioned above, intermediate region 12 on top of substrate 11 may be embodied as an acoustic mirror or a support layer, depending on the type of resonator to be formed. Examples of intermediate region 12 are described below with reference to Figures 3 and 5.

[0022] The electrodes 14 and 15 may be embodied as layers of highly conductive material, such as a metal or metal alloy, including copper, silver, gold, molybdenum, tungsten, titanium, platinum, or aluminum, alloys thereof, and other conductive layers. One factor in the selection of materials for the electrodes 14 and 15 is the desired thickness of the electrodes 14 and 15, which is also a factor in the response characteristics of the BAW resonator 10. Considerations in the selection of conductive materials for the electrodes 14 and 15 and the method of forming the electrodes 14 and 15 are discussed below.

[0023] The layer of piezoelectric material 13 may be embodied as a layer of lead zirconate titanate (PZT), barium strontium titanate (BST), barium titanate (BaTiO3), aluminum scandium nitride (AlScN), aluminum nitride (AlN), ZnO, or another piezoelectric material. Despite its low electromechanical coupling coefficient compared to ZnO, AlN has a wider band gap and is compatible with silicon integrated circuit technology used in FBARs and other structures. AlN is also compatible with ALD processing techniques as described herein. Thus, in one preferred embodiment, the layer of piezoelectric material 13 is a layer of AlN, although other piezoelectric materials may be utilized. In some cases, the layer of piezoelectric material 13 may include one or more layers of piezoelectric material including two or more different types of piezoelectric material (e.g., a stack of two or more of layers of AlN, PZT, BST, BaTiO3, and AlScN), each of which may be formed using ALD processing techniques according to embodiments. The piezoelectric material 13 may also include a layer of AlN having a particular crystal orientation. In various embodiments, the layer of AlN can be formed with a crystal structure c-axis orientation in the "X", "Y", or "Z" direction shown in Figure 1. In one example, the layer of AlN can have a crystal structure c-axis orientation in the "Z" direction for exciting bulk acoustic or mechanical waves into the BAW resonator 10.

[0024] The operating characteristics of the BAW resonator 10, including frequency response, frequency response accuracy, and quality factor, are determined in part by the thickness, conformality, and uniformity of the layer of piezoelectric material 13. Various sputtering techniques have been utilized to form layers of piezoelectric material having thicknesses of about 300 nm or greater. Current sputtering techniques cannot be reliably used to form thinner (e.g., 200 nm, 150 nm, or 100 nm or less thick) and also uniform and conformal layers of piezoelectric material. Thus, according to one aspect of the embodiment, the layer of piezoelectric material 13 can be embodied as a layer of AlN deposited by ALD. By forming a layer of AlN using ALD rather than sol-gel wet chemical techniques, sputtering, pulsed laser deposition, or other techniques, a thinner, more uniform, and more conformal layer of piezoelectric material can be obtained.

[0025] As mentioned above, ALD is a process for depositing highly uniform and conformal thin films of material. The ALD process deposits a thin film of material on a surface by exposing the surface to two chemical reactants. In one example, the process can begin with initiation of the surface for deposition of the material. Initiation can include annealing the surface, etching the surface, exposing the surface to one or more gases, or other steps that remove contaminants from the surface or otherwise prepare the surface for deposition of material.

[0026] After the initiation treatment, the ALD process typically proceeds with the exposure of the surface to two or more precursor chemicals or reactants in a repeating sequence. The precursors may be gaseous species that are introduced into the ALD chamber separately over time. The precursors react with the surface in a self-limiting manner (i.e., until a finite number of sites for reaction are exhausted), each in its own time. Any excess or residual reactants of the precursor are removed before the next precursor or ALD cycle is applied or repeated. The ALD process is characterized by both a dose time, which is the time that the surface is exposed to each precursor, and a purge time, which is the time between doses when the ALD chamber is evacuated for the next step. For a two reactant ALD process, the first reactant dose, the first purge, the second reactant dose, and the second purge are steps in one ALD cycle.

[0027] Thin films are slowly deposited on a surface by repeatedly exposing the surface to precursors separately over time, with intermediate flushing steps in the ALD process. There is a maximum amount of material that can be deposited on a surface in a single ALD cycle, which is determined by the precursor-surface interactions. The total thickness of the thin film can be determined by the number of ALD cycles used, which can be adjusted to grow a uniform and conformal layer of material at a specific thickness with great precision, even on complex surfaces. ALD processes are often characterized by the growth of material per ALD cycle, in nanometers or another suitable metric.

[0028] According to aspects of the embodiment, ALD can be used to form the layer of piezoelectric material 13 in the BAW resonator 10. The layer of piezoelectric material 13 can be formed as a thinner layer of piezoelectric material than layers in conventional BAW resonators, such as when sputtering is used. In one example, the layer of piezoelectric material 13 can be formed by ALD as an AlN layer having a thickness of 100 nm or less. However, the layer of piezoelectric material 13 can be formed using ALD to be a thinner layer of AlN, such as a layer having a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm, in some cases. The layer of piezoelectric material 13 is not limited to a layer of AlN, as other thin films of piezoelectric material can be formed using ALD.

[0029] The specific thickness of the layer of piezoelectric material 13 can be highly controlled or tailored in the BAW resonator 10, and in some cases can be within less than 10 nm of the target thickness, within less than 5 nm of the target thickness, or even closer to the target thickness by using ALD. In some embodiments, the layer of piezoelectric material 13 can be formed as thin as possible using a minimum number of ALD cycles. The use of ALD rather than sputtering to deposit the layer of piezoelectric material 13 offers many advantages. For example, the use of ALD reduces crystal damage in the layer of piezoelectric material 13, reduces dangling bonds, and reduces surface traps that typically result from sputter or plasma damage, resulting in better resonator performance.

[0030] In some cases, the crystal orientation of the layer 13 of piezoelectric material can be selected to tailor the operating characteristics of the BAW resonator 10. As an example, a thin film of ZnO with its crystal structure c-axis perpendicular (i.e., perpendicular) to the top surface of the support substrate will excite longitudinal waves in the film. A thin film of ZnO with its crystal structure c-axis tilted (i.e., non-perpendicular) to the top surface of the support substrate can excite shear or transverse waves in the film. Depending on the crystal structure orientation, it is also possible to excite a combination of both longitudinal and shear waves. As with the ZnO thin film, the crystal orientation of the AlN thin film also affects the excitation of waves in the thin film and in the surrounding layers.

[0031] The crystal orientation of a thin film of piezoelectric material depends on a variety of factors, including the material processing technique used to form the film or layer of material, the material selected, the surface on which the film is grown or deposited, and the conditions under which the film is grown or deposited, such as temperature, pressure, gas, vacuum conditions, and other factors. The crystal orientation of layer 13 of piezoelectric material in BAW resonator 10 can be oriented using one or more ALD processing steps according to aspects of an embodiment. For example, one or more initiation processing steps of an ALD process, as well as the ALD growth process itself, can be utilized to orient the crystal structure c-axis orientation of layer 13 of piezoelectric material.

[0032] In other aspects of the embodiment, electrode 14 can be formed using ALD, electrode 15 can be formed using ALD, or both electrodes 14 and 15 can be formed using ALD. As an example, electrodes 14 and 15 can be formed as thin copper layers using ALD, while other highly conductive layers can be formed using ALD. When ALD is used to form electrodes 14 and 15, the type of conductive material used to form electrodes 14 and 15 can be determined in part based on the ALD process available for the material. ALD processes are known for depositing thin films of pure metallic materials, such as pure copper, but additional processes are also known for depositing metal alloys.

[0033] As mentioned above, one factor in the material selection of the electrodes 14 and 15 is the desired thickness of the electrodes 14 and 15, which is also a factor in the response characteristics of the BAW resonator 10. For example, if highly conductive and thin electrodes 14 and 15 are desired, an ALD process can be selected to deposit copper for the electrodes 14 and 15. The electrodes 14 and 15 can also be formed from other metals and metal alloys using an ALD process step. In other cases, the electrodes 14 and 15 can be formed by sputtering, physical vapor deposition (PVD), chemical vapor deposition (CVD), or related techniques for depositing conductive material layers for the electrodes 14 and 15. When using sputtering or other process techniques other than ALD, the electrodes 14 and 15 can be relatively thick. The shapes, sizes, and positions of the electrodes 14 and 15 are indicated in FIG. 1. The electrodes 14 and 15 can be formed to have any suitable shape and size.

[0034] The thickness of the BAW resonator 10 can be significantly reduced by using ALD to form the layer of piezoelectric material 13, as compared to sputtering. The overall thickness can be further reduced by using ALD to form one or both of the electrodes 14 and 15. The uniformity and conformity of the layer of piezoelectric material 13 and the electrodes 14 and 15 can also be improved by using ALD. The BAW resonator 10 can be tailored by ALD for steeper stopband attenuation, lower insertion loss, and other improved properties compared to other BAW resonators, for use in RF passband filters operable in the range of 5 to 20 GHz or more. The BAW resonator 10 can also be tailored by ALD for more accurate frequency response, higher quality factor, higher piezoelectric coupling or bandwidth, and smaller frequency temperature coefficient, among other improved properties.

[0035] Although some trimming steps may be required after sputtering, trimming can be reduced or even avoided in many cases where ALD is used. In particular, layers of material deposited by sputtering may lack some thickness uniformity, and trimming is often used to achieve better thickness uniformity across the surface of the material layer. The lack of thickness uniformity may be particularly pronounced in sputtering when considered across the entire wafer. Trimming can be a relatively expensive and time-consuming process that involves measuring the thickness of the layer across the wafer, forming a thickness map, and multiple trimming steps using ion bean or other techniques to smooth the layer profile. This trimming process may be required for both the piezoelectric layer, the electrode layer, and other layers (e.g., temperature compensation layer and / or encapsulation layer) when utilizing sputtering or other deposition techniques. In some cases where ALD is used to form the layer of piezoelectric material 13 and the electrodes 14 and 15, these trimming steps can be reduced or eliminated, resulting in time and cost savings. These benefits are even greater when considered across the entire wafer of an integrated device. Other benefits of using ALD processing steps are discussed below.

[0036] With reference to other embodiments, FIG. 2 illustrates an exemplary SAW resonator 20 according to various embodiments described herein. A diagram of the SAW resonator 20 is shown in FIG. 2. The positions, shapes, dimensions, and relative sizes of the layers and features of the SAW resonator 20 are not necessarily drawn to scale in FIG. 2. Exemplary dimensions of the SAW resonator 20 are shown below, but the dimensions of the SAW resonator 20 are not particularly limited. The layers and other features shown in FIG. 2 are also not exhaustive, and the SAW resonator 20 can include other layers, features, and elements that are not separately illustrated. In addition, the SAW resonator 20 can be combined with other devices and circuit elements to form part of a larger integrated structure or circuit. This type of larger integrated structure can include several resonators similar to the SAW resonator 20, among other integrated components.

[0037] The SAW resonator 20 includes a substrate 21, a layer 23 of piezoelectric material on the substrate 21, a first electrode 24, a second electrode 25, a first reflective grating 26, and a second reflective grating 27. The first electrode 24 is disposed on the piezoelectric material 23 and in contact with a first surface (i.e., top surface) of the piezoelectric material 23. The second electrode 25 is also disposed on the piezoelectric material 23 and in contact with a first surface of the piezoelectric material 23. The first electrode 24 and the second electrode 25 include several interdigitated fingers extending laterally adjacent to one another. The first reflective grating 26 and the second reflective grating 27 are disposed on either side of the first electrode 24 and the second electrode 25 as shown.

[0038] The SAW resonator 20 may also include additional layers, such as temperature compensation layers, encapsulation layers, and other layers, described below but not shown in FIG. 2. The SAW resonator 20 may also optionally include additional structures, such as acoustic mirrors or reflectors (e.g., Bragg reflectors), between the substrate and the layer of piezoelectric material 23. The acoustic mirrors or reflectors may be utilized to tailor the operating characteristics of the SAW resonator 20 to account for any undesired resonances or BAW-type designed resonances in the SAW resonator 20. In some cases, the piezoelectric material 23 may be formed to have a crystal structure c-axis orientation in the "X", "Y", or "Z" directions, and some BAW-type resonances may be created using structures similar to the SAW resonators in some of those cases. Additional examples of such structures are described below with reference to FIGS. 8A and 8B.

[0039] The piezoelectric properties of the layer of piezoelectric material 23 and the structural arrangement of the SAW resonator 20 enable the SAW resonator 20 to generate elastic or mechanical waves when an alternating potential input signal, such as an RF input, is applied across the electrodes 24 and 25. The elastic or mechanical waves may travel or translate in the "Y" direction across or along the top surface of the SAW resonator 20 as shown in Figure 1. The elastic or mechanical waves may be reflected by the first and second reflective gratings 26 and 27 in accordance with the motion of the SAW resonator 20.

[0040] The substrate 21 may be embodied as silicon, silicon carbide, lithium niobate, sapphire, glass, ceramic, or another suitable type of substrate suitable for the application. Silicon substrates may be preferred because they are relatively low cost, scalable for manufacturing, and compatible with manufacturing and processing steps, although other substrates may be utilized.

[0041] The electrodes 24 and 25 may be embodied as layers of highly conductive material, such as a metal or metal alloy, including copper, silver, gold, molybdenum, tungsten, titanium, platinum, or aluminum, alloys thereof, and other conductive layers. One factor in the selection of material for the electrodes 24 and 25 is the desired thickness of the electrodes 24 and 25, which is also a factor in the response characteristics of the SAW resonator 20. The first reflective grating 26 and the second reflective grating 27 may also be embodied as layers of highly conductive material, such as a metal or metal alloy.

[0042] The layer of piezoelectric material 23 may be embodied as a layer of PZT, BST, BaTiO3, AlScN, AlN, ZnO, or another piezoelectric material. In one preferred embodiment, the layer of piezoelectric material 23 is a layer of AlN, although other piezoelectric materials may be utilized. In some cases, the layer of piezoelectric material 23 may include one or more layers of piezoelectric material, including two or more different types of piezoelectric materials, each of which is formed using ALD processing techniques according to embodiments. The piezoelectric material 23 may also include a layer of AlN having a particular crystal orientation. In various embodiments, the layer of AlN may be formed to have a crystal structure c-axis orientation in the "X", "Y", or "Z" directions. In one example, the layer of AlN may have a crystal structure c-axis orientation in the "Y" direction to excite elastic or mechanical waves across or along the top surface of the SAW resonator 20.

[0043] The operating characteristics of the SAW resonator 20, including frequency response, frequency response accuracy, and quality factor, are determined in part by the conformity and uniformity of the layer of piezoelectric material 23. To a lesser extent than for the BAW resonator 10, the operating characteristics of the SAW resonator 20 are also determined in part by the thickness of the layer of piezoelectric material 23. According to one aspect of the embodiment, the layer of piezoelectric material 23 may be embodied as a layer of AlN deposited by ALD. By forming the layer of AlN using ALD, rather than sol-gel wet chemical techniques, sputtering, pulsed laser deposition, or other techniques, a more uniform and conformal layer of piezoelectric material may be obtained. By forming the layer of AlN using ALD, a thinner layer of piezoelectric material may also be obtained.

[0044] The total thickness of the layer of piezoelectric material 23 can be determined by the number of ALD cycles used. In some cases, the layer of piezoelectric material 23 can be formed as a thinner layer of piezoelectric material than a layer in a conventional SAW resonator, such as when sputtering is used. In one example, the layer of piezoelectric material 23 can be formed by ALD as an AlN layer having a thickness of 100 nm or less. However, the layer of piezoelectric material 23 can be formed using ALD to be a thinner layer of AlN, such as a layer having a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm. The layer of piezoelectric material 23 is not limited to a layer of AlN, as other thin films of piezoelectric material can be formed using ALD.

[0045] The specific thickness of the layer of piezoelectric material 23 can be tailored in the SAW resonator 20, in some cases to within less than 10 nm of the target thickness, within less than 5 nm of the target thickness, or even closer to the target thickness, by using ALD. In some embodiments, the layer of piezoelectric material 23 can be formed as thin as possible using a minimum number of ALD cycles. The use of ALD rather than sputtering to deposit the layer of piezoelectric material 23 provides many advantages. For example, the use of ALD reduces crystal damage in the layer of piezoelectric material 23, reduces dangling bonds, and reduces surface traps that typically result from sputter or plasma damage, resulting in better resonator performance.

[0046] The thickness, uniformity, and conformity of the other layers in the SAW resonator 20, including the electrodes 24 and 25 and any temperature compensation and encapsulation layers, may be particularly important in the SAW resonator 20. Thus, in other aspects of the embodiment, the electrode 24 may be formed using ALD, the electrode 25 may be formed using ALD, or both the electrodes 24 and 25 may be formed using ALD. As an example, the electrodes 24 and 25 may be formed as thin copper layers using ALD, while other highly conductive layers may be formed using ALD. If ALD is used to form the electrodes 24 and 25, the type of conductive material used to form the electrodes 24 and 25 may be determined in part based on the ALD process available for the material. ALD processes are known for depositing thin films of pure metallic materials, such as pure copper, although additional processes are known for depositing metal alloys. The first reflective grating 26 and the second reflective grating 27 may also be formed using ALD.

[0047] As shown in FIG. 2, the use of ALD to form the electrodes 24 and 25 can be particularly beneficial in the SAW resonator 20 because the elastic or mechanical waves generated by the SAW resonator 20 travel in the “Y” direction across or along the top surface of the SAW resonator 20 at the interface between the layer of piezoelectric material 23 and the electrodes 24 and 25. Thus, the thickness, conformity, and uniformity of the electrodes 24 and 25 may affect or have a greater impact on the operating characteristics of the SAW resonator 20 than the thickness, conformity, and uniformity of the electrodes 14 and 15 in the BAW resonator 10. As an example, forming thinner and more uniform electrodes 24 and 25 can help reduce the effects of undesirable BAW mode resonances in the SAW resonator 20. In addition, the thickness of any temperature compensating and encapsulating layers formed over the layer of piezoelectric material 23 and the electrodes 24 and 25 may also have a greater impact on the operating characteristics of the SAW resonator 20 than they do in the BAW resonator 10. Forming thinner and more uniform temperature compensating and encapsulating layers can also help reduce the effects of undesirable BAW mode resonances in SAW resonator 20.

[0048] One factor in the material selection of the electrodes 24 and 25 is the desired thickness of the electrodes 24 and 25, which is also a factor in the response characteristics of the SAW resonator 20. For example, if highly conductive and thin electrodes 24 and 25 are desired, an ALD process can be selected to deposit copper for the electrodes 24 and 25. The electrodes 24 and 25 can also be formed from other metals and metal alloys using an ALD process step. In other cases, the electrodes 24 and 25 can be formed by a sputtering process, PVD, or related techniques for depositing conductive material layers for the electrodes 24 and 25. When using sputtering or other process techniques other than ALD, the electrodes 24 and 25 can be relatively thick. The shape, size, and position of the electrodes 24 and 25 are indicated in FIG. 2. The electrodes 24 and 25 can be formed to have any suitable shape and size. In other cases, the first reflective grating 26 and the second reflective grating 27 may be formed by a sputtering process, PVD, or related techniques for depositing a conductive material layer for the reflective gratings 26 and 27. The shapes, sizes, and positions of the reflective gratings 26 and 27 are indicated in Figure 2. The reflective gratings 26 and 27 may be formed to have any suitable shape and size.

[0049] The overall thickness of the SAW resonator 20 can be significantly reduced by using ALD to form the layer 23 of piezoelectric material, as compared to sputtering. The overall thickness can be further reduced by using ALD to form one or both of the electrodes 24 and 25. The uniformity and conformity of the layer 23 of piezoelectric material and the electrodes 24 and 25 can also be improved by using ALD. The SAW resonator 20 can be tailored by ALD for steeper stopband attenuation, lower insertion loss, and other improved properties compared to other SAW resonators, for use in RF passband filters operable in the range of 10-20 GHz or greater. The SAW resonator 20 can also be tailored by ALD for more accurate frequency response, higher quality factor, higher piezoelectric coupling or bandwidth, and smaller temperature coefficient of frequency, among other improved properties.

[0050] FIG. 3 illustrates an exemplary SMR 30 in cross-section, according to various embodiments described herein. A diagram of the SMR 30 is displayed in FIG. 3. The locations, shapes, dimensions, and relative sizes of the layers and features of the SMR 30 are not necessarily drawn to scale in FIG. 3. Exemplary dimensions of the SMR 30 are provided below, but the dimensions of the SMR 30 are not particularly limited. The layers and other features illustrated in FIG. 3 are also not exhaustive, and the SMR 30 can include other layers, features, and elements that are not separately illustrated. In addition, the SMR 30 can be combined with other devices and circuit elements to form part of a larger integrated structure or circuit. Such a larger integrated structure can include several resonators similar to the SMR 30, among other integrated components.

[0051] The SMR 30 includes a substrate 31, an acoustic mirror 32 on the substrate 31, a layer of piezoelectric material 33 on the substrate 31, a first electrode 34, a second electrode 35, and an encapsulation layer 36. The first electrode 34 is in contact with a first surface (i.e., bottom surface) of the piezoelectric material 33 and is at least partially disposed below the piezoelectric material 33 between the piezoelectric material 33 and the substrate 31. The second electrode 35 is in contact with a second surface (i.e., top surface) of the piezoelectric material 33 and is at least partially disposed above the piezoelectric material 33. The substrate 31 may be similar to the substrate 11 shown in FIG. 1 and may be embodied as silicon, silicon carbide, lithium niobate, sapphire, glass, ceramic, or another suitable type of substrate suitable for the application.

[0052] Acoustic mirror 32 is an example of intermediate region 12 in the embodiment shown in FIG. 1. Acoustic mirror 32 can be embodied as a reflector of acoustic waves, such as a Bragg reflector. As an example, acoustic mirror 32 can be embodied as an odd number of layers of materials having high and low acoustic impedance, with the high and low acoustic impedance layers alternating in a layer stack. In some cases, acoustic mirror 32 can be formed using ALD, with one or more material layers in acoustic mirror 32 being formed using ALD. The thickness of the layers in the stack can be optimized, for example, to a quarter wavelength of the acoustic waves generated by SMR 30, to increase acoustic wave reflectivity. Acoustic mirror 32 provides acoustic wave isolation between substrate 31 and the resonator formed by piezoelectric material 33 and electrodes 34 and 35.

[0053] The piezoelectric properties of the layer of piezoelectric material 33 and the structural arrangement of SMR 30 enable SMR 30 to generate elastic or mechanical waves when an alternating potential input signal, such as an RF input, is applied between electrodes 34 and 35. The elastic or mechanical waves may travel or translate in the "Z" direction and may be substantially reflected by acoustic mirror 32.

[0054] The electrodes 34 and 35 may be embodied as layers of highly conductive material, such as metals or metal alloys, including copper, silver, gold, molybdenum, tungsten, titanium, platinum, or aluminum, alloys thereof, and other conductive layers. The layer of piezoelectric material 33 may be embodied as a layer of PZT, BST, BaTiO3, AlScN, AlN, ZnO, or another piezoelectric material. In one preferred embodiment, the layer of piezoelectric material 33 is a layer of AlN, although other piezoelectric materials may be utilized. The piezoelectric material 33 may also include a layer of AlN having a specific crystal orientation. In one example, the layer of AlN may have a crystal structure c-axis orientation to excite elastic or mechanical waves in the "Z" direction. The encapsulation layer 36 may be embodied as a thin film of material to protect the SMR 30. The encapsulation layer 36 may be, for example, aluminum oxide (Al 2 O 3 ), another oxide material, or another suitable layer of material to protect the SMR 30.

[0055] The operating characteristics of the SMR 30, including frequency response, frequency response accuracy, and quality factor, are determined in part by the thickness, conformality, and uniformity of the layer of piezoelectric material 33. According to one aspect of the embodiment, the layer of piezoelectric material 33 may be embodied as a layer of AlN deposited by ALD. By forming the layer of AlN using ALD rather than sol-gel wet chemical techniques, sputtering, pulsed laser deposition, or other techniques, a thinner, more uniform, and more conformal layer of piezoelectric material can be obtained.

[0056] The layer of piezoelectric material 33 can be formed as a thinner layer of piezoelectric material than in conventional SMR resonators, such as when sputtering is used. In one example, the layer of piezoelectric material 33 can be formed by ALD as an AlN layer having a thickness of 100 nm or less. However, the layer of piezoelectric material 33 can be formed using ALD to be a thinner layer of AlN, such as a layer less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm thick, in some cases. The layer of piezoelectric material 33 is not limited to a layer of AlN, as other thin films of piezoelectric material can be formed using ALD. In some cases, the layer of piezoelectric material 33 can include one or more layers of piezoelectric material including two or more different types of piezoelectric materials (e.g., a stack of two or more of layers of AlN, PZT, BST, BaTiO3, and AlScN), each of which can be formed using ALD processing techniques according to embodiments.

[0057] The specific thickness of the layer of piezoelectric material 33 can be highly controlled or tailored in the SMR 30, and in some cases can be within less than 10 nm of the target thickness, within less than 5 nm of the target thickness, or even closer to the target thickness by using ALD. In some embodiments, the layer of piezoelectric material 33 can be formed as thin as possible using a minimum number of ALD cycles. The use of ALD rather than sputtering to deposit the layer of piezoelectric material 33 provides many advantages. For example, the use of ALD reduces crystal damage in the layer of piezoelectric material 33, reduces dangling bonds, and reduces surface traps that typically result from sputter or plasma damage, resulting in better resonator performance.

[0058] In other aspects of the embodiment, electrode 34 can be formed using ALD, electrode 35 can be formed using ALD, or both electrodes 34 and 35 can be formed using ALD. As an example, electrodes 34 and 35 can be formed as thin copper layers using ALD, while other highly conductive layers can be formed using ALD. When ALD is used to form electrodes 34 and 35, the type of conductive material used to form electrodes 34 and 35 can be determined in part based on the ALD process available for the material. ALD processes are known for depositing thin films of pure metallic materials, such as pure copper, although additional processes are known for depositing metal alloys.

[0059] As mentioned above, one factor in the material selection of the electrodes 34 and 35 is the desired thickness of the electrodes 34 and 35, which is also a factor in the response characteristics of the SMR 30. For example, if highly conductive and thin electrodes 34 and 35 are desired, an ALD process can be selected to deposit copper for the electrodes 34 and 35. The electrodes 34 and 35 can also be formed from other metals and metal alloys using an ALD process step. In other cases, the electrodes 34 and 35 can be formed by a sputtering process, PVD, or related techniques for depositing conductive material layers for the electrodes 34 and 35. When using sputtering or other process techniques other than ALD, the electrodes 34 and 35 can be relatively thick. The shape, size, and location of the electrodes 34 and 35 are indicated in FIG. 3. The electrodes 34 and 35 can be formed to have any suitable shape and size.

[0060] According to one aspect of the embodiment, the encapsulation layer 36 may be formed using ALD. The encapsulation layer 36 may be formed as a uniform and conformal thin film. In one example, the encapsulation layer 36 may be formed using ALD to form 100 nm or less of Al. 2 O 3 The encapsulation layer 36 can also be formed using ALD as a layer of Al, such as a layer of less than 10 nm, 5 nm, or even thinner in some cases.2 O 3 Since other thin films of protective material can be formed using ALD, the encapsulation layer 36 can be formed as a thinner layer of Al. 2 O 3 The present invention is not limited to this layer.

[0061] The overall thickness of the SMR 30 can be significantly reduced by using ALD to form the layer of piezoelectric material 33, as compared to sputtering. The overall thickness can be further reduced by using ALD to form one or both of the electrodes 34 and 35, and the encapsulation layer 36. The uniformity and conformality of the layer of piezoelectric material 33, the electrodes 34 and 35, and the encapsulation layer 36 can also be improved by using ALD. The SMR 30 can be tailored by ALD for steeper stopband attenuation, lower insertion loss, and other improved properties compared to other SMR structures, for use in RF passband filters operable in the range of 5 to 20 GHz or greater. The SMR 30 can also be tailored by ALD for more accurate frequency response, higher quality factor, higher piezoelectric coupling or bandwidth, and smaller temperature coefficient of frequency, among other improved properties.

[0062] FIG. 4 illustrates an exemplary method of fabricating the SMR 30 shown in FIG. 3 according to various embodiments described herein. Although the method is described in connection with the SMR 30 shown in FIG. 3, the method can also be utilized to fabricate solid-state mounted resonators similar to those shown in FIG. 3. In addition, although the method illustrates a particular order of steps in FIG. 4, the order of the steps may differ from the order illustrated. For example, two or more steps illustrated in succession may be performed at least partially simultaneously. In some cases, one or more of the steps may be skipped or omitted. In other cases, additional steps not illustrated in FIG. 4 may be utilized, such as steps between or after the steps illustrated in FIG. 4.

[0063] In step 100, the process includes providing a substrate for SMR 30. With reference to the example shown in FIG. 3, substrate 31 is shown as one example of a substrate that may be provided in step 100. Substrate 31 may be embodied as silicon, silicon carbide, lithium niobate, sapphire, glass, ceramic, or another suitable type of substrate suitable for the application. Substrate 31 may be manufactured, provided by a vendor, or formed or provided in any other suitable manner in step 100.

[0064] In step 102, the process includes forming an acoustic mirror 32 on a substrate 31. By way of example, the acoustic mirror 32 may be formed as alternating layers of materials having high and low acoustic impedances or refractive indices, such as Bragg reflectors. The acoustic mirror 32 provides acoustic wave isolation between the substrate 31 and a resonator formed by piezoelectric material 33 and electrodes 34 and 35, which are formed in a later process step.

[0065] In step 104, the process includes forming a first electrode 34 on the acoustic mirror 32. The first electrode 34 may be embodied as a layer of a highly conductive material as described herein. In one example, the electrode 34 may be formed as a thin or film layer of copper using ALD. The electrode 34 may be formed using ALD to a thickness of 300 nm, 200 nm, or 100 nm or less. However, the electrode 34 may be formed using ALD to a thinner layer of copper, such as a layer less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm thick, in some cases.

[0066] One factor in the selection of the material for the electrode 34 is the desired thickness of the electrode 34, which is also a factor in the response characteristics of the SMR 30. For example, if a highly conductive and thin electrode 34 is required, an ALD process can be selected to deposit copper for the electrode 34. The electrode 34 can also be formed from other metals and metal alloys using an ALD process in step 104. In other cases, the electrode 34 can be formed as molybdenum or another metal or metal alloy in step 104 by sputtering, PVD, CVD, or related techniques. When using process techniques other than ALD, the electrode 34 can be formed relatively thicker than when using ALD.

[0067] In step 106, the process includes depositing a layer 33 of piezoelectric material on the substrate 31 by an ALD processing step. The layer 33 of piezoelectric material can be deposited on the electrode 34 as shown in FIG. 3. The ALD process can begin with an initiation of the surface of the electrode 34 to deposit a piezoelectric material, such as AlN, on the electrode 34. In a reaction chamber for the ALD processing step, the initiation can include annealing the electrode 34 or the top surface of the electrode 34, etching the electrode 34, exposing the electrode 34 to one or more gases, or other steps to remove contaminants from the top surface of the electrode 34 or otherwise provide a surface of the electrode 34 for material deposition. In step 106, the crystal orientation of the layer 33 of piezoelectric material can also be oriented. For example, the initiation can be tailored to form the layer 33 of piezoelectric material having a crystal structure c-axis orientation for elastic or mechanical waves in the "Z" direction as shown in FIG. 3.

[0068] After the initiation process, the ALD process in step 106 can proceed with exposure of the electrode 34 to two or more precursor chemicals or reactants in a repeating sequence. The precursors may be gaseous species that are introduced separately into the ALD chamber over time. The precursors react in a self-limiting manner, each in time. Any excess or residual reactants of the precursors are washed away before the next precursor or ALD cycle is applied or repeated. The ALD process is characterized by both a dose time, which is the time that the surface is exposed to each precursor, and a purge time, which is the time between doses when the ALD chamber is evacuated for the next step. For a two reactant ALD process, the sequence of first reactant dose, first purge, second reactant dose, second purge are steps in one ALD cycle.

[0069] In a first reactant dose cycle, a first precursor may be introduced into the ALD reaction chamber, exposing the top surface of the electrode 34 to the first precursor along with the application of heat. The time of the first reactant dose cycle may be selected to saturate the top surface of the electrode 34 with the first precursor. The ALD reaction chamber may then be purged in a first purge cycle to remove any by-products of the first reactant dose cycle. The ALD reaction chamber may be purged by introducing an inert gas, by evacuating using, for example, a vacuum, or by other steps.

[0070] In a second reactant dose cycle, a second precursor can be introduced into the ALD reaction chamber. The duration of the second reactant dose cycle can be sufficient for the second precursor to fully or substantially react with the first precursor until sites for reaction between the precursors are exhausted. The ALD reaction chamber can then be purged in a second purge cycle to remove any by-products of the second reactant dose cycle. The ALD reaction chamber can be purged by introducing an inert gas, e.g., by evacuating with a vacuum, or by other steps. Another ALD cycle can then be initiated.

[0071] The thickness of the layer of piezoelectric material 33 can be determined by the number of ALD cycles used in step 106, which can be adjusted to grow the layer of piezoelectric material 33 uniformly and conformally with great precision. In one example, the layer of piezoelectric material 33 can be formed by ALD as an AlN layer having a thickness of 100 nm or less. However, the layer of piezoelectric material 33 can be formed using ALD in step 106 to be a thinner layer of AlN, such as a layer having a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm, in some cases. The layer of piezoelectric material 33 is also not limited to a layer of AlN, as other thin films of piezoelectric material can be formed using ALD in step 106.

[0072] Optionally, step 106 may also include trimming the layer of piezoelectric material 33 to further improve layer uniformity, adjust the layer thickness, or otherwise modify the layer of piezoelectric material 33. Trimming may be a relatively expensive and time consuming process, but any trimming performed in step 106 may be relatively minor as compared to if sputtering was used to form the layer of piezoelectric material 33.

[0073] In step 108, the process includes forming a second electrode 35 on the layer of piezoelectric material 33. The second electrode 35 may be embodied as a layer of highly conductive material as described herein. In one example, the electrode 35 may be formed as a thin or film layer of copper using ALD. The electrode 35 may be formed using ALD to a thickness of 300 nm, 200 nm, or 100 nm or less. However, the electrode 35 may be formed using ALD to be a thinner layer of copper, such as a layer less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm thick, in some cases.

[0074] One factor in the selection of the material for electrode 35 is the desired thickness of electrode 35, which is also a factor in the response characteristics of SMR 30. For example, if a highly conductive and thin electrode 35 is required, an ALD process can be selected to deposit copper for electrode 35. Electrode 35 can also be formed from other metals and metal alloys using an ALD process in step 108. In other cases, electrode 35 can be formed as molybdenum or another metal or metal alloy in step 108 by sputtering, PVD, CVD, or related techniques. When using process techniques other than ALD, electrode 35 can be formed relatively thicker than when using ALD.

[0075] In step 110, the process includes forming the encapsulation layer 36. The encapsulation layer 36 may be formed as a uniform and conformal thin film. In one example, the encapsulation layer 36 is formed by an ALD processing step, with 100 nm or less of Al. 2 O 3 The encapsulation layer 36 can also be formed using ALD as a layer of Al, such as a layer of less than 10 nm, 5 nm, or even thinner in some cases. 2 O 3 Since other thin films of protective material can be formed using ALD, the encapsulation layer 36 can be formed as a thinner layer of Al. 2 O 3 The present invention is not limited to this layer.

[0076] Compared to other deposition processes, the encapsulation layer 36 can be formed very thin using ALD to tune the frequency response, frequency response accuracy, quality factor, and insertion loss of the SMR 30. The encapsulation layer 36 can cover and encapsulate the layer of piezoelectric material 33, the first electrode 34, and the second electrode 35, as shown in FIG. 3. In some cases, the encapsulation layer 36 can cover more or less area compared to the area shown in FIG.

[0077] 4 may include additional steps, such as forming one or more temperature compensating layers within the SMR 30. For example, the process may include forming a silicon dioxide (SiO 2 It may be possible to include between steps 104 and 106 forming a temperature compensation layer, such as a layer of SiO 2 , or a layer of other material for temperature compensation, between the first electrode 34 and the piezoelectric material 33 using ALD. 2 A layer of SiO 2 can be formed between the piezoelectric material 33 and the second electrode 35 using ALD between steps 106 and 108, and the first electrode can be formed on the temperature compensation layer rather than on the piezoelectric material 33. 2 By using ALD processing steps, the temperature compensating layer(s) can be more uniform, more conformal, and thinner than when formed using other deposition techniques. As some examples, SiO 2 The layer may be formed to a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm.

[0078] FIG. 5 illustrates an exemplary FBAR 40 according to various embodiments described herein. A diagram of the FBAR 40 is shown in FIG. 5. The positions, shapes, dimensions, and relative sizes of the layers and features of the FBAR 40 are not necessarily drawn to scale in FIG. 5. Exemplary dimensions of the FBAR 40 are shown below, but the dimensions of the FBAR 40 are not particularly limited. The layers and other features shown in FIG. 5 are also not exhaustive, and the FBAR 40 can include other layers, features, and elements that are not separately illustrated. In addition, the FBAR 40 can be combined with other devices and circuit elements to form a part of a larger integrated structure or circuit. Such a larger integrated structure can include several resonators similar to the FBAR 40, among other integrated components.

[0079] The FBAR 40 includes a substrate 41, a support layer 42 on the substrate 41, a layer of piezoelectric material 43 on the substrate 41, a first electrode 44, a second electrode 45, an encapsulation layer 46, and an insulating cavity 47. The first electrode 44 is in contact with a first surface (i.e., bottom surface) of the piezoelectric material 43 and is at least partially disposed below the piezoelectric material 43 between the piezoelectric material 43 and the substrate 41. The second electrode 45 is in contact with a second surface (i.e., top surface) of the piezoelectric material 43 and is at least partially disposed above the piezoelectric material 43. The substrate 41 may be similar to the substrate 11 shown in FIG. 1 and may be embodied as silicon, silicon carbide, lithium niobate, sapphire, glass, ceramic, or another suitable type of substrate suitable for the application.

[0080] Support layer 42 is an example of intermediate region 12 in the embodiment shown in Figure 1. Support layer 42 may be embodied as a layer of support material, such as silicon, formed on substrate 41. Support layer 42 supports a resonator formed by piezoelectric material 43 and electrodes 44 and 45, as will be further described below.

[0081] The piezoelectric properties of layer of piezoelectric material 43 and the structural arrangement of FBAR 40 enable FBAR 40 to generate elastic or mechanical waves when an alternating potential input signal, such as an RF input, is applied across electrodes 44 and 45. The elastic or mechanical waves may travel or be translated in the "Z" direction and may be isolated by insulating cavity 47, as also described below.

[0082] The electrodes 44 and 45 can be embodied as layers of highly conductive material, such as metals or metal alloys, including copper, silver, gold, molybdenum, tungsten, titanium, platinum, or aluminum, alloys thereof, and other conductive layers. The layer of piezoelectric material 43 can be embodied as a layer of PZT, BST, BaTiO3, AlScN, AlN, ZnO, or another piezoelectric material. In one preferred embodiment, the layer of piezoelectric material 43 is a layer of AlN, although other piezoelectric materials can be utilized. The piezoelectric material 43 can also include a layer of AlN with a specific crystal orientation. In one example, the layer of AlN can have a crystal structure c-axis orientation to excite elastic or mechanical waves in the "Z" direction. The encapsulation layer 46 can be embodied as a thin film of material to protect the FBAR 40. The encapsulation layer 46 can be, for example, Al 2 O 3 , another oxide material, or another suitable layer of material to protect the FBAR 40.

[0083] The operating characteristics of FBAR 40, including frequency response, frequency response accuracy, and quality factor, are determined in part by the thickness, conformality, and uniformity of layer of piezoelectric material 43. According to one aspect of an embodiment, layer of piezoelectric material 43 may be embodied as a layer of AlN deposited by ALD. By forming the layer of AlN using ALD rather than sol-gel wet chemical techniques, sputtering, pulsed laser deposition, or other techniques, a thinner, more uniform, and more conformal layer of piezoelectric material can be obtained.

[0084] The layer of piezoelectric material 43 can be formed as a thinner layer of piezoelectric material than a layer in a conventional FBAR resonator, such as when sputtering is used. In one example, the layer of piezoelectric material 43 can be formed by ALD as an AlN layer with a thickness of 100 nm or less. However, the layer of piezoelectric material 43 can be formed using ALD to be a thinner layer of AlN, such as a layer with a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm, in some cases. The layer of piezoelectric material 43 is not limited to a layer of AlN, as other thin films of piezoelectric material can be formed using ALD. In some cases, the layer of piezoelectric material 43 can include one or more layers of piezoelectric material including two or more different types of piezoelectric materials (e.g., a stack of two or more of layers of AlN, PZT, BST, BaTiO3, and AlScN), each of which can be formed using ALD processing techniques according to embodiments.

[0085] The specific thickness of the layer of piezoelectric material 43 can be highly controlled or tailored in the FBAR 40, and in some cases can be within less than 10 nm of the target thickness, within less than 5 nm of the target thickness, or even closer to the target thickness by using ALD. In some embodiments, the layer of piezoelectric material 43 can be formed as thin as possible using a minimum number of ALD cycles. The use of ALD rather than sputtering to deposit the layer of piezoelectric material 43 provides many advantages. For example, the use of ALD reduces crystal damage in the layer of piezoelectric material 43, reduces dangling bonds, and reduces surface traps that typically result from sputter or plasma damage, resulting in better resonator performance.

[0086] In other aspects of the embodiment, the electrode 44 can be formed using ALD, the electrode 45 can be formed using ALD, or both the electrodes 44 and 45 can be formed using ALD. As an example, the electrodes 44 and 45 can be formed as thin copper layers using ALD, while other highly conductive layers can be formed using ALD. If ALD is used to form the electrodes 44 and 45, the type of conductive material used to form the electrodes 44 and 45 can be determined in part based on the ALD process available for the material. One factor in the material selection for the electrodes 44 and 45 is the desired thickness of the electrodes 44 and 45, which is also a factor in the response characteristics of the FBAR 40. For example, if very thin and conductive electrodes 44 and 45 are desired, an ALD process can be selected to deposit copper for the electrodes 44 and 45. In other cases, the electrodes 44 and 45 can be formed by a sputtering process, PVD, or related techniques. If sputtering or other process techniques other than ALD are used, the electrodes 44 and 45 can be relatively thick.

[0087] According to one aspect of the embodiment, the encapsulation layer 46 may be formed using ALD. The encapsulation layer 46 may be formed as a uniform and conformal thin film. In one example, the encapsulation layer 46 may be formed using ALD to form up to 100 nm of Al. 2 O 3 The encapsulation layer 46 can also be formed using ALD as a layer of Al, such as a layer of less than 10 nm, 5 nm, or even thinner. 2 O 3 Since other thin films of protective material can be formed using ALD, the encapsulation layer 46 can be formed as a thinner layer of Al. 2 O 3 The present invention is not limited to this layer.

[0088] Insulation cavity 47 is a space or cavity formed under support layer 42, layer of piezoelectric material 43, and electrodes 44 and 45. Insulation cavity 47 may be of different size and proportions compared to that shown in Figure 5. In some cases, insulation cavity 47 may be wider than that shown in Figure 5, and insulation cavity 47 may be larger (i.e., have larger length and width dimensions in top view) than layer of piezoelectric material 43. In other cases, at least a portion of layer of piezoelectric material 43 may extend beyond insulation cavity 47 above substrate 41, as shown in Figure 5.

[0089] The insulating cavity 47 may be formed by etching or other material removal process steps, typically after the support layer 42 and other layers of the FBAR 40 are formed. In some cases, the insulating cavity 47 may be formed with one or more support pillars 48 that remain in the insulating cavity 47. The substrate 41 may be selectively etched to form the insulating cavity such that the support pillars 48 remain in the insulating cavity 47. The support pillars 48 may provide additional support to the support layer 42. The number and location of the support pillars 48 may be different compared to those shown in FIG. 5, and in some cases the support pillars 48 may be omitted.

[0090] The overall thickness of the FBAR 40 can be significantly reduced by using ALD to form the layer of piezoelectric material 43, as compared to sputtering. The overall thickness can be further reduced by using ALD to form one or both of the electrodes 44 and 45, and the encapsulation layer 46. The uniformity and conformity of the layer of piezoelectric material 43, the electrodes 44 and 45, and the encapsulation layer 46 can also be improved by using ALD. The FBAR 40 can be tailored by ALD for steeper stopband attenuation, lower insertion loss, and other improved properties compared to other FBAR structures, for use in RF passband filters operable in the range of 10-20 GHz or greater. The FBAR 40 can also be tailored by ALD for more precise frequency response, higher quality factor, higher piezoelectric coupling or bandwidth, and smaller frequency temperature coefficient, among other improved properties.

[0091] FIG. 6 illustrates an exemplary method of fabricating the exemplary FBAR 40 illustrated in FIG. 5 according to various embodiments described herein. Although the method is described in connection with the FBAR 40 illustrated in FIG. 5, the method can also be utilized to fabricate thin film bulk acoustic wave resonators similar to those illustrated in FIG. 5. In addition, although the method illustrates a particular order of steps in FIG. 6, the order of the steps may differ from the order illustrated. For example, two or more steps illustrated in succession may be performed at least partially simultaneously. In some cases, one or more of the steps may be skipped or omitted. In other cases, additional steps not illustrated in FIG. 6 may be utilized, such as steps between or after the steps illustrated in FIG. 6.

[0092] In step 200, the process includes providing a substrate for the FBAR 40. With reference to the example shown in FIG. 5, a substrate 41 is shown as one example of a substrate that may be provided in step 200. The substrate 41 may be embodied as silicon, silicon carbide, lithium niobate, sapphire, glass, ceramic, or another suitable type of substrate suitable for the application. The substrate 41 may be manufactured, provided by a vendor, or formed or provided in any other suitable manner in step 200.

[0093] In step 202, the process includes forming a support layer 42 on the substrate 41. By way of example, the support layer 42 may be embodied as a layer of support material, such as silicon, formed on the substrate 41. The support layer 42 may be deposited using a suitable deposition technique, such as PVD, CVD, or related techniques. The support layer 42 may be formed to any suitable thickness, and the support layer 42 need not be formed as a thin film. The support layer 42 supports the resonator formed by the piezoelectric material 43 and the electrodes 44 and 45, as will be further described below.

[0094] In step 204, the process includes forming a first electrode 44 on the support layer 42. The first electrode 44 may be embodied as a layer of a highly conductive material as described herein. In one example, the electrode 44 may be formed as a thin or film layer of copper using ALD. The electrode 44 may be formed using ALD to a thickness of 300 nm, 200 nm, or 100 nm or less. However, the electrode 44 may be formed using ALD to a thinner layer of copper, such as a layer less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm thick, in some cases.

[0095] One factor in the selection of the material for electrode 44 is the desired thickness of electrode 44, which is also a factor in the response characteristics of FBAR 40. For example, if a highly conductive and thin electrode 44 is desired, an ALD process can be selected to deposit copper for electrode 44. Electrode 44 can also be formed from other metals and metal alloys using an ALD process in step 204. In other cases, electrode 44 can be formed as molybdenum or another metal or metal alloy in step 204 by sputtering, PVD, CVD, or related techniques. When using process techniques other than ALD, electrode 44 can be formed relatively thicker than when using ALD.

[0096] In step 206, the process includes depositing a layer 43 of piezoelectric material on the substrate 41 by an ALD processing step. The layer 43 of piezoelectric material can be deposited on an electrode 44 as shown in FIG. 5. The ALD process can begin with an initiation of the surface of the electrode 44 to deposit a piezoelectric material, such as AlN, on the electrode 44. In a reaction chamber for the ALD processing step, the initiation can include annealing the electrode 44 or the top surface of the electrode 44, etching the electrode 44, exposing the electrode 44 to one or more gases, or other steps to remove contaminants from the top surface of the electrode 44 or otherwise provide a surface of the electrode 44 for material deposition. In step 206, the crystal orientation of the layer 43 of piezoelectric material can also be oriented. For example, the initiation can be tailored to form the layer 43 of piezoelectric material having a crystal structure c-axis orientation for elastic or mechanical waves in the "Z" direction as shown in FIG. 5.

[0097] After the initiation process, the ALD process in step 206 can proceed with exposure of the electrode 44 to two or more precursor chemicals or reactants in a repeating sequence. The precursors may be gaseous species that are introduced separately into the ALD chamber over time. The precursors react in a self-limiting manner, each in time. Any excess or residual reactants of the precursors are washed away before the next precursor or ALD cycle is applied or repeated. The ALD process is characterized by both a dose time, which is the time that the surface is exposed to each precursor, and a purge time, which is the time between doses when the ALD chamber is evacuated for the next step. For a two reactant ALD process, the sequence of first reactant dose, first purge, second reactant dose, second purge are steps in one ALD cycle.

[0098] In a first reactant dose cycle, a first precursor may be introduced into the ALD reaction chamber, exposing the top surface of the electrode 44 to the first precursor along with the application of heat. The time of the first reactant dose cycle may be selected to saturate the top surface of the electrode 44 with the first precursor. The ALD reaction chamber may then be purged in a first purge cycle to remove any by-products of the first reactant dose cycle. The ALD reaction chamber may be purged by introducing an inert gas, by evacuating using, for example, a vacuum, or by other steps.

[0099] In a second reactant dose cycle, a second precursor can be introduced into the ALD reaction chamber. The duration of the second reactant dose cycle can be sufficient for the second precursor to fully or substantially react with the first precursor until sites for reaction between the precursors are exhausted. The ALD reaction chamber can then be purged in a second purge cycle to remove any by-products of the second reactant dose cycle. The ALD reaction chamber can be purged by introducing an inert gas, e.g., by evacuating with a vacuum, or by other steps. Another ALD cycle can then be initiated.

[0100] The thickness of the layer of piezoelectric material 43 can be determined by the number of ALD cycles used in step 206, which can be adjusted to grow the layer of piezoelectric material 43 uniformly and conformally with great precision. In one example, the layer of piezoelectric material 43 can be formed by ALD as an AlN layer having a thickness of 100 nm or less. However, the layer of piezoelectric material 43 can be formed using ALD in step 206 to be a thinner layer of AlN, such as a layer having a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm, in some cases. The layer of piezoelectric material 43 is also not limited to a layer of AlN, as other thin films of piezoelectric material can be formed using ALD in step 206.

[0101] In some cases, step 206 may also include trimming the layer of piezoelectric material 43 to improve layer uniformity, adjust layer thickness, or otherwise modify the layer of piezoelectric material 43. Trimming may be a relatively expensive and time consuming process, but any trimming performed in step 206 may be relatively minor as compared to if sputtering were used to form the layer of piezoelectric material 43.

[0102] In step 208, the process includes forming a second electrode 45 on the layer of piezoelectric material 43. The second electrode 45 may be embodied as a layer of highly conductive material as described herein. In one example, the electrode 45 may be formed as a thin or film layer of copper using ALD. The electrode 45 may be formed using ALD to a thickness of 300 nm, 200 nm, or 100 nm or less. However, the electrode 45 may be formed using ALD to be a thinner layer of copper, such as a layer less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm thick, in some cases.

[0103] One factor in the selection of the material for electrode 45 is the desired thickness of electrode 45, which is also a factor in the response characteristics of FBAR 40. For example, if a highly conductive and thin electrode 45 is required, an ALD process can be selected to deposit copper for electrode 45. Electrode 45 can also be formed from other metals and metal alloys using an ALD process in step 208. In other cases, electrode 45 can be formed as molybdenum or another metal or metal alloy in step 208 by sputtering, PVD, CVD, or related techniques. When using process techniques other than ALD, electrode 45 can be formed relatively thicker than when using ALD.

[0104] In step 210, the process includes forming the encapsulation layer 46. The encapsulation layer 46 may be formed as a uniform and conformal thin film. In one example, the encapsulation layer 46 is formed by an ALD processing step, with 100 nm or less of Al. 2 O 3 The encapsulation layer 46 can also be formed using ALD as a layer of Al, such as a layer of less than 10 nm, 5 nm, or even thinner. 2 O 3 Since other thin films of protective material can be formed using ALD, the encapsulation layer 46 can be formed as a thinner layer of Al. 2 O 3 The present invention is not limited to this layer.

[0105] Compared to other deposition processes, the encapsulation layer 46 can be formed very thin using ALD to tailor the frequency response, frequency response accuracy, quality factor, and insertion loss of the FBAR 40. The encapsulation layer 46 can cover and encapsulate the layer of piezoelectric material 43, the first electrode 44, and the second electrode 45, as shown in FIG. 5. In some cases, the encapsulation layer 46 can cover more or less area compared to the area shown in FIG.

[0106] In step 212, the process includes forming an insulating cavity 47 under the support layer 42, the layer of piezoelectric material 43, and the electrodes 44 and 45. The insulating cavity 47 can be formed to any size suitable for the purpose of isolating the acoustic waves generated by the layer of piezoelectric material 43. In some cases, the insulating cavity 47 can be wider than that shown in FIG. 5, and the insulating cavity 47 can be larger (i.e., larger length and width dimensions in top view) than the layer of piezoelectric material 43. In other cases, at least a portion of the layer of piezoelectric material 43 can extend beyond the insulating cavity 47 and above the substrate 41, as shown in FIG. 5. The insulating cavity 47 can be formed by etching or other material removal process steps. In some cases, the insulating cavity 47 can be formed with one or more support pillars 48 (FIG. 5) that remain in the insulating cavity 47 to provide additional support to the support layer 42. The number and location of the support pillars 48 can be different compared to that shown in FIG. 5, and in some cases the support pillars 48 can be omitted.

[0107] 6 may include additional steps, such as forming one or more temperature compensating layers within FBAR 40. For example, the process may include forming a SiO 2 It may be possible to include between steps 204 and 206 forming a temperature compensation layer, such as a layer of SiO 2 or other material for temperature compensation, between the first electrode 44 and the piezoelectric material 43 using ALD. 2Between steps 206 and 208, a layer of SiO can be formed between the piezoelectric material 43 and the second electrode 45 using ALD. 2 By using an ALD processing step, the temperature compensating layer(s) can be more uniform, more conformal, and thinner than when formed using other deposition techniques. As some examples, SiO 2 The layer may be formed to a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm.

[0108] FIG. 7 illustrates an exemplary method for fabricating the SAW resonator 20 shown in FIG. 2 according to various embodiments described herein. Although the method is described in relation to the SAW resonator 20 shown in FIG. 2, the method can also be utilized to fabricate SAW resonators similar to that shown in FIG. 2. In addition, although the method illustrates a particular order of steps in FIG. 7, the order of the steps may differ from the order illustrated. For example, two or more steps shown in succession may be performed at least partially simultaneously. In some cases, one or more of the steps may be skipped or omitted. In other cases, additional steps not illustrated in FIG. 7 may be utilized, such as steps between or after the steps illustrated in FIG. 7.

[0109] In step 300, the process includes providing a substrate for the SAW resonator 20. With reference to the example shown in FIG. 2, a substrate 21 is shown as one example of a substrate that may be provided in step 300. The substrate 21 may be embodied as silicon, silicon carbide, lithium niobate, sapphire, glass, ceramic, or another suitable type of substrate suitable for the application. The substrate 21 may be manufactured, provided by a vendor, or formed or provided in any other suitable manner in step 300.

[0110] In step 302, the process includes depositing a layer 23 of piezoelectric material on the substrate 21 by an ALD processing step. The ALD process can begin with an initiation of the surface of the substrate 21 for depositing a piezoelectric material, such as AlN, on the substrate 21. In a reaction chamber for the ALD processing step, the initiation can include etching the substrate 21, exposing the substrate 21 to one or more gases, or other steps that remove contaminants from the top surface of the substrate 21 or otherwise prepare the surface of the substrate 21 for material deposition. In step 302, the crystal orientation of the layer 23 of piezoelectric material can also be oriented. For example, the initiation can be tailored to form the layer 23 of piezoelectric material having a crystal structure c-axis orientation for elastic or mechanical waves in the "Y" direction shown in FIG. 2.

[0111] After the initiation process, the ALD process in step 302 can proceed with exposure of the substrate 21 to two or more precursor chemicals or reactants in a repeating sequence. The precursors may be gaseous species that are introduced separately into the ALD chamber over time. The precursors react in a self-limiting manner, each in time. Any excess or residual reactants of the precursor are washed away before the next precursor or ALD cycle is applied or repeated. The ALD process is characterized by both a dose time, which is the time that the surface is exposed to each precursor, and a purge time, which is the time between doses when the ALD chamber is evacuated for the next step. For a two reactant ALD process, the sequence of first reactant dose, first purge, second reactant dose, second purge are steps in one ALD cycle.

[0112] In a first reactant dose cycle, a first precursor may be introduced into the ALD reaction chamber, exposing an upper surface of the substrate 21 to the first precursor along with the application of heat. The time of the first reactant dose cycle may be selected to saturate the upper surface of the substrate 21 with the first precursor. The ALD reaction chamber may then be purged in a first purge cycle to remove any by-products of the first reactant dose cycle. The ALD reaction chamber may be purged by introducing an inert gas, by evacuating, for example, with a vacuum, or by other steps.

[0113] In a second reactant dose cycle, a second precursor can be introduced into the ALD reaction chamber. The duration of the second reactant dose cycle can be sufficient for the second precursor to fully or substantially react with the first precursor until sites for reaction between the precursors are exhausted. The ALD reaction chamber can then be purged in a second purge cycle to remove any by-products of the second reactant dose cycle. The ALD reaction chamber can be purged by introducing an inert gas, e.g., by evacuating with a vacuum, or by other steps. Another ALD cycle can then be initiated.

[0114] The thickness of the layer of piezoelectric material 23 can be determined by the number of ALD cycles used in step 302, which can be adjusted to grow the layer of piezoelectric material 23 uniformly and conformally with great precision. In one example, the layer of piezoelectric material 23 can be formed by ALD as an AlN layer having a thickness of 100 nm or less. However, the layer of piezoelectric material 23 can be formed using ALD in step 206 to be a thinner layer of AlN, such as a layer having a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm, as the case may be. The layer of piezoelectric material 23 is also not limited to a layer of AlN, as other thin films of piezoelectric material can be formed using ALD in step 302.

[0115] In some cases, step 302 may also include trimming the layer of piezoelectric material 23 to improve layer uniformity, adjust layer thickness, or otherwise modify the layer of piezoelectric material 23. Trimming may be a relatively expensive and time consuming process, but any trimming performed in step 306 may be relatively minor as compared to if sputtering was used to form the layer of piezoelectric material 23.

[0116] In step 304, the process includes forming a first electrode 24, a second electrode 25, and reflective gratings 26 and 27 on the layer of piezoelectric material 23. The electrodes 24 and 25 can be embodied as layers of highly conductive material. In one example, the electrodes 24 and 25 can be formed as thin or thin layers of copper using ALD. The electrodes 24 and 25 can be formed using ALD with a thickness of 300 nm, 200 nm, or 100 nm or less. However, the electrodes 24 and 25 can be formed using ALD to be thinner layers of copper, such as layers with a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm, in some cases. The reflective gratings 26 and 27 can be omitted in some cases. The reflective gratings 26 and 27, if included, can also be formed using ALD with the same or similar thickness as the electrodes 24 and 25.

[0117] One factor in the selection of the material for the electrodes 24 and 25 is the desired thickness of the electrodes 24 and 25, which is also a factor in the response characteristics of the SAW resonator 20. For example, if highly conductive and thin electrodes 24 and 25 are required, an ALD process can be selected to deposit copper for the electrodes 24 and 25. The electrodes 24 and 25 can also be formed from other metals and metal alloys using an ALD process in step 304. In other cases, the electrodes 24 and 25 can be formed as molybdenum or another metal or metal alloy in step 304 by sputtering, PVD, CVD, or related techniques. When using process techniques other than ALD, the electrodes 24 and 25 can be formed relatively thicker than when using ALD.

[0118] In step 306, the process includes forming an encapsulation layer over the electrodes 24 and 25, the reflective gratings 26 and 27, and the layer of piezoelectric material 23. Although the encapsulation layer is not shown in Figure 2, an encapsulation layer similar to the encapsulation layers 36 and 46 shown in Figures 3 and 5 can be formed as a uniform and conformal thin film over the electrodes 24 and 25, the reflective gratings 26 and 27, and the layer of piezoelectric material 23. The encapsulation layer 46 is formed by an ALD processing step, with 100 nm or less of Al. 2 O 3 The encapsulation layer 46 can also be formed using ALD as a layer of Al, such as a layer of less than 10 nm, 5 nm, or even thinner. 2 O 3 Since other thin films of protective material can be formed using ALD, the encapsulation layer 46 can be formed as a thinner layer of Al. 2 O 3 The present invention is not limited to this layer.

[0119] The structures and methods described herein can be used to fabricate a wide variety of useful integrated circuits. For example, the acoustic resonators described herein can be integrated with various components in a monolithic circuit configuration suitable for microwave circuit applications. Although embodiments have been described in detail herein, the description, including dimensional aspects, is by way of example.

[0120] 7 may include additional steps, such as forming one or more temperature compensating layers within the SAW resonator 20. For example, the process may include forming a SiO 2 It may be possible to include between steps 302 and 304 forming a temperature compensating layer, such as a layer of SiO 2 or other material for temperature compensation, between the layer of piezoelectric material 23 and the electrodes 24 and 25 using ALD. 2 By using ALD processing steps, the temperature compensating layer(s) can be more uniform, more conformal, and thinner than when formed using other deposition techniques. As some examples, SiO 2 The layer may be formed to a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm.

[0121] FIG. 8 is a cross-sectional view of an exemplary laterally excited bulk acoustic wave resonator 50 ("resonator 50") according to various embodiments described herein. A diagram of the resonator 50 is displayed in FIG. 8. The positions, shapes, dimensions, and relative sizes of the layers and features of the resonator 50 are not necessarily drawn to scale in FIG. 8. Exemplary dimensions of the resonator 50 are shown below, but the dimensions are not particularly limited. The layers and other features shown in FIG. 8 are also not exhaustive, and the resonator 50 can include other layers, features, and elements that are not separately illustrated. In addition, the resonator 50 can be combined with other devices and circuit elements to form part of a larger integrated structure or circuit. Such a larger integrated structure can include several resonators similar to the resonator 50, among other integrated components.

[0122] The resonator 50 includes a substrate 51, a layer 53 of piezoelectric material on the substrate 51, first electrodes 54A-54C interdigitated with second electrodes 55A-55C, a sealing layer 56, and an insulating cavity 57. The interdigitated electrodes 54A-54C and 55A-55C are similar to the interdigitated electrodes 24 and 25 shown in FIG. 2, except that cross sections of the electrodes 54A-54C and 55A-55C are shown in FIG. 8. Although a limited number of electrodes 54A-54C and 55A-55C are shown in FIG. 8, it should be understood that in practice a greater number of electrodes may be utilized. The electrodes 54A-54C and 55A-55C are in contact with the top surface of the piezoelectric material 53. Substrate 51 may be similar to substrate 11 shown in Figure 1 and may be embodied as silicon, silicon carbide, lithium niobate, sapphire, glass, ceramic, or another suitable type of substrate suitable for the application. Although not shown in Figure 8, resonator 50 may also optionally include a support layer similar to support layer 42 of Figure 5. Such a layer of support material may be formed, for example, from silicon and may be disposed above substrate 51 and below layer 53 of piezoelectric material.

[0123] The resonator 50 can generate elastic or mechanical waves when an AC potential input signal is applied across the first electrodes 54A-54C and the second electrodes 55A-55C. The electrodes 54A-54C and 55A-55C of the resonator 50 are not disposed on two different opposite surfaces of the piezoelectric material 53 as in the SMR 30 shown in FIG. 3 and the FBAR 40 shown in FIG. 5. Instead, both the first electrodes 54A-54C and the second electrodes 55A-55C are formed on the top surface of the piezoelectric material 53, similar to the SAW resonator 20 shown in FIG. 2. However, the resonator 50 is not designed to excite elastic or mechanical waves along the top surface of the resonator 50 as in the SAW resonator 20. Instead, the crystal structure c-axis orientation of the piezoelectric material 53 is oriented to excite bulk elastic or mechanical waves in the "Z" direction. That is, the c-axis orientation of the piezoelectric material 53 is oriented in the "Z" direction perpendicular to the top surface of the piezoelectric material 53. Resonator 50 is therefore referred to as a laterally excited bulk acoustic wave resonator.

[0124] Electrodes 54A-54C and 55A-55C may be embodied as layers of highly conductive material, such as metals or metal alloys, including copper, silver, gold, molybdenum, tungsten, titanium, platinum, or aluminum, alloys thereof, and other conductive layers. Electrodes 54A-54C and 55A-55C are formed to have a width "W" and a pitch "P" separates them. Width "W" in resonator 50 is less than pitch "P". For example, width "W" may be approximately 100 nm and pitch "P" may be 1-5 μm, although other dimensions may be utilized.

[0125] The layer of piezoelectric material 53 may be embodied as a layer of PZT, BST, BaTiO3, AlScN, AlN, ZnO, or another piezoelectric material. In one preferred embodiment, the layer of piezoelectric material 53 is a layer of AlN, although other piezoelectric materials may be utilized. In some cases, the layer of piezoelectric material 13 may include one or more layers of piezoelectric material including two or more different types of piezoelectric material (e.g., a stack of two or more of layers of AlN, PZT, BST, BaTiO3, and AlScN), each of which may be formed using ALD processing techniques according to embodiments. The encapsulation layer 56 may be embodied as a thin film of material to protect the resonator 50. The encapsulation layer 56 may be, for example, Al 2 O 3 , another oxide material, or another suitable layer of material to protect the resonator 50 .

[0126] The operating characteristics of resonator 50, including frequency response, frequency response accuracy, and quality factor, are determined in part by the thickness, conformality, and uniformity of layer of piezoelectric material 53. According to one aspect of the embodiment, layer of piezoelectric material 53 may be embodied as a layer of AlN deposited by ALD. By forming the layer of AlN using ALD, rather than sol-gel wet chemical techniques, sputtering, pulsed laser deposition, or other techniques, a thinner, more uniform, and more conformal layer of piezoelectric material can be obtained.

[0127] The layer of piezoelectric material 53 can be formed as a thinner layer of piezoelectric material than a layer in a conventional resonator, such as when sputtering is used. In one example, the layer of piezoelectric material 53 can be formed by ALD as an AlN layer having a thickness of 100 nm or less. However, the layer of piezoelectric material 53 can be formed using ALD to be a thinner layer of AlN, such as a layer having a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm, in some cases. The layer of piezoelectric material 53 is not limited to a layer of AlN, as other thin films of piezoelectric material can be formed using ALD.

[0128] The particular thickness of layer of piezoelectric material 53 can be highly controlled or tuned in resonator 50, and in some cases can be within less than 10 nm of the target thickness, within less than 5 nm of the target thickness, or even closer to the target thickness, by using ALD. In some embodiments, layer of piezoelectric material 53 can be made as thin as possible using a minimum number of ALD cycles.

[0129] The electrodes 54A-54C and 55A-55C can also be formed using ALD. As an example, the electrodes 54A-54C and 55A-55C can be formed as thin copper layers using ALD, while other highly conductive layers can be formed using ALD. If ALD is used to form the electrodes 54A-54C and 55A-55C, the type of conductive material used can be determined in part based on the ALD process available for the material. One factor in the selection of the material for the electrodes 54A-54C and 55A-55C is the desired thickness of the electrodes 54A-54C and 55A-55C, which is also a factor in the response characteristics of the resonator 50. For example, if very thin and conductive electrodes 54A-54C and 55A-55C are desired, an ALD process can be selected to deposit copper. In other cases, electrodes 54A-54C and 55A-55C may be formed by a sputtering process, PVD, or related techniques.

[0130] According to one aspect of the embodiment, the encapsulation layer 56 may be formed using ALD. The encapsulation layer 56 may be formed as a uniform and conformal thin film. In one example, the encapsulation layer 56 may be formed using ALD to form 100 nm or less of Al. 2 O 3 The encapsulation layer 56 can also be formed using ALD as a layer of Al, such as a layer of less than 10 nm, 5 nm, or even thinner in some cases. 2 O 3 Since other thin films of protective material can be formed using ALD, the encapsulation layer 56 can be formed as a thinner layer of Al. 2 O 3 The present invention is not limited to this layer.

[0131] The insulating cavity 57 is a space or cavity formed under the layer of piezoelectric material 53. The insulating cavity 57 may be of different size and proportions compared to that shown in FIG. 8. In some cases, the insulating cavity 57 may be wider than that shown in FIG. 8, and the insulating cavity 57 may be larger (i.e., have larger length and width dimensions in top view) than the layer of piezoelectric material 53. The insulating cavity 57 may be formed by an etching or other material removal process step. In some cases, the insulating cavity 57 may be formed with one or more support pillars similar to the support pillars 48 shown in FIG. 5.

[0132] The overall thickness of resonator 50 can be significantly reduced as compared to sputtering by using ALD to form layer of piezoelectric material 53. The overall thickness can be further reduced by using ALD to form electrodes 54A-54C and 55A-55C and encapsulation layer 56. The uniformity and conformality of layer of piezoelectric material 53, electrodes 54A-54C and 55A-55C, and encapsulation layer 56 can also be improved by using ALD.

[0133] FIG. 9 is a cross-sectional view of another exemplary laterally excited bulk acoustic wave resonator 60 ("resonator 60") according to various embodiments described herein. A diagram of resonator 60 is displayed in FIG. 9. The locations, shapes, dimensions, and relative sizes of layers and features of resonator 60 are not necessarily drawn to scale in FIG. 9. Exemplary dimensions of resonator 60 are shown below, but the dimensions are not particularly limited. The layers and other features shown in FIG. 9 are also not exhaustive, and resonator 60 can include other layers, features, and elements that are not separately illustrated. In addition, resonator 60 can be combined with other devices and circuit elements to form part of a larger integrated structure or circuit. Such a larger integrated structure can include several resonators similar to resonator 60, among other integrated components.

[0134] The resonator 60 includes a substrate 61, a layer 63 of piezoelectric material on the substrate 61, first electrodes 64A-64C interdigitated with second electrodes 65A-65C, a sealing layer 66, an insulating cavity 67, and a floating metal plate 68. The interdigitated electrodes 64A-64C and 65A-65C are similar to the interdigitated electrodes 24 and 25 shown in FIG. 2, but cross sections of the electrodes 64A-64C and 65A-65C are shown in FIG. 9. Although a limited number of electrodes 64A-64C and 65A-65C are shown in FIG. 9, it should be understood that in practice a greater number of electrodes may be utilized. The electrodes 64A-64C and 65A-65C are in contact with the top surface of the piezoelectric material 63. The floating metal plate 68 is in contact with the bottom surface of the piezoelectric material 63.

[0135] Substrate 61 may be similar to substrate 11 shown in Figure 1 and may be embodied as silicon, silicon carbide, lithium niobate, sapphire, glass, ceramic, or another suitable type of substrate suitable for the application. Although not shown in Figure 9, resonator 60 may also optionally include a support layer similar to support layer 42 of Figure 5. Such a layer of support material may be formed, for example, from silicon and may be disposed above substrate 61 and below the layer of floating metal plate 68.

[0136] The resonator 60 can generate acoustic or mechanical waves when an AC potential input signal is applied across the first electrodes 64A-64C and the second electrodes 65A-65C. No potential is applied to the floating metal plate 68. The electrodes 64A-64C and 65A-65C of the resonator 50 are not disposed on two different opposite surfaces of the piezoelectric material 63 as in the SMR 30 shown in FIG. 3 and the FBAR 40 shown in FIG. 5. Instead, both the first electrodes 64A-64C and the second electrodes 65A-65C are formed on the top surface of the piezoelectric material 63 as in the SAW resonator 20 shown in FIG. 2, and the floating metal plate 68 is in contact with the bottom surface of the piezoelectric material 63. The crystal structure c-axis orientation of the piezoelectric material 53 is oriented to excite bulk acoustic or mechanical waves in the "X" direction, which faces into the page of FIG. 9. That is, the c-axis orientation of piezoelectric material 53 is oriented in the "X" direction, parallel to the top surface of piezoelectric material 63 and pointing into the page of FIG.

[0137] The electrodes 64A-64C and 65A-65C and the floating metal plate 68 may be embodied as layers of highly conductive material, such as metals or metal alloys, including copper, silver, gold, molybdenum, tungsten, titanium, platinum, or aluminum, alloys thereof, and other conductive layers. The electrodes 64A-64C and 65A-65C are formed to have a width "W" and a pitch "P" separates them. The width "W" in the resonator 60 is greater than the pitch "P". For example, the width "W" may be approximately 50-300 μm and the pitch "P" may be 1-20 μm, although other dimensions may be utilized.

[0138] The layer of piezoelectric material 63 may be embodied as a layer of PZT, BST, BaTiO3, AlScN, AlN, ZnO, or another piezoelectric material. In one preferred embodiment, the layer of piezoelectric material 63 is a layer of AlN, although other piezoelectric materials may be utilized. In some cases, the layer of piezoelectric material 63 may include one or more layers of piezoelectric material, including two or more different types of piezoelectric material (e.g., a stack of two or more of layers of AlN, PZT, BST, BaTiO3, and AlScN), each of which may be formed using ALD processing techniques according to an embodiment. The encapsulation layer 66 may be embodied as a thin film of material to protect the resonator 60. The encapsulation layer 66 may be, for example, Al 2 O 3 , another oxide material, or another suitable layer of material to protect the resonator 60 .

[0139] The operating characteristics of the resonator 60, including frequency response, frequency response accuracy, and quality factor, are determined in part by the thickness, conformality, and uniformity of the layer of piezoelectric material 63. According to one aspect of the embodiment, the layer of piezoelectric material 63 may be embodied as a layer of AlN deposited by ALD. By forming the layer of AlN using ALD, rather than sol-gel wet chemical techniques, sputtering, pulsed laser deposition, or other techniques, a thinner, more uniform, and more conformal layer of piezoelectric material can be obtained.

[0140] The layer of piezoelectric material 63 can be formed as a thinner layer of piezoelectric material than a layer in a conventional resonator, such as when sputtering is used. In one example, the layer of piezoelectric material 63 can be formed by ALD as an AlN layer having a thickness of 100 nm or less. However, the layer of piezoelectric material 53 can be formed using ALD to be a thinner layer of AlN, such as a layer having a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm, in some cases. The layer of piezoelectric material 63 is not limited to a layer of AlN, as other thin films of piezoelectric material can be formed using ALD.

[0141] The particular thickness of layer of piezoelectric material 63 can be highly controlled or tuned in resonator 60, and in some cases can be within less than 10 nm of the target thickness, within less than 5 nm of the target thickness, or even closer to the target thickness by using ALD. In some embodiments, layer of piezoelectric material 63 can be made as thin as possible using a minimum number of ALD cycles.

[0142] The electrodes 64A-64C and 65A-65C and the floating metal plate 68 can also be formed using ALD. As an example, the electrodes 64A-64C and 65A-65C and the floating metal plate 68 can be formed as a thin copper layer using ALD, although other highly conductive layers can be formed using ALD. If ALD is used to form the electrodes 64A-64C and 65A-65C and the floating metal plate 68, the type of conductive material used can be determined in part based on the ALD process available for the material. One factor in the selection of the material for the electrodes 64A-64C and 65A-65C and the floating metal plate 68 is the desired thickness of the electrodes 64A-64C and 65A-65C and the floating metal plate 68, which is also a factor in the response characteristics of the resonator 60. In other cases, the electrodes 64A-64C and 65A-65C and the floating metal plate 68 may be formed by a sputtering process, PVD, or related techniques.

[0143] According to one aspect of the embodiment, the encapsulation layer 66 may be formed using ALD. The encapsulation layer 66 may be formed as a uniform and conformal thin film. In one example, the encapsulation layer 66 may be formed using ALD to form 100 nm or less of Al. 2 O 3 The encapsulation layer 66 can also be formed using ALD as a layer of Al, such as a layer of less than 10 nm, 5 nm, or even thinner in some cases. 2 O 3 Since other thin films of protective material can be formed using ALD, the encapsulation layer 66 can be formed as a thinner layer of Al. 2 O3 The present invention is not limited to this layer.

[0144] The insulating cavity 67 is a space or cavity formed under the layer of piezoelectric material 63. The insulating cavity 67 may be of different size and proportions compared to that shown in FIG. 9. In some cases, the insulating cavity 67 may be wider than that shown in FIG. 9, and the insulating cavity 67 may be larger (i.e., have larger length and width dimensions in top view) than the layer of piezoelectric material 63. The insulating cavity 67 may be formed by an etching or other material removal process step. In some cases, the insulating cavity 67 may be formed with one or more support pillars similar to the support pillars 48 shown in FIG. 5.

[0145] The overall thickness of resonator 60 can be significantly reduced as compared to sputtering by using ALD to form layer of piezoelectric material 63. The overall thickness can be further reduced by using ALD to form electrodes 64A-64C and 65A-65C and encapsulation layer 66. The uniformity and conformality of layer of piezoelectric material 63, electrodes 64A-64C and 65A-65C, and encapsulation layer 66 can also be improved by using ALD.

[0146] FIG. 10 illustrates an exemplary method for fabricating the resonator structures 50 and 60 shown in FIGS. 8 and 9 according to various embodiments described herein. Although the method is described in relation to the resonator structures 50 and 60 shown in FIGS. 8 and 9, the method can also be utilized to fabricate resonator structures similar to those illustrated. In addition, although the method illustrates a particular order of steps in FIG. 10, the order of steps may differ from the order illustrated. For example, two or more steps illustrated in succession may be performed at least partially simultaneously. In some cases, one or more of the steps may be skipped or omitted. In other cases, additional steps not illustrated in FIG. 10 may be utilized, such as steps between or after the steps illustrated in FIG. 10.

[0147] In step 400, the process includes providing a substrate. With reference to the examples shown in Figures 8 and 9, substrates 51 and 61 are shown as exemplary substrates that may be provided in step 400. The substrate may be embodied as silicon, silicon carbide, lithium niobate, sapphire, glass, ceramic, or another suitable type of substrate suitable for the application. The substrate may be manufactured, provided by a vendor, or formed or provided in any other suitable manner in step 400.

[0148] In step 402, the process includes forming a floating metal plate 68 on the substrate. As an example, the floating metal plate 68 can be embodied as a layer of highly conductive material, such as a metal or metal alloy, including copper, silver, gold, molybdenum, tungsten, titanium, platinum, or aluminum, alloys thereof, and other conductive layers. The floating metal plate 68 can be formed using ALD. As an example, the floating metal plate 68 can be formed as a thin copper layer using ALD, although other highly conductive layers can be formed using ALD. In other cases, the floating metal plate 68 can be formed by a sputtering process, PVD, or related techniques. It should also be noted that step 402 can be omitted in some cases, such as when forming the resonator 50 of FIG. 8.

[0149] In step 404, the process includes depositing a layer of piezoelectric material by an ALD processing step. For example, a layer of piezoelectric material 53 can be deposited on or above a substrate 51, as shown in FIG. 8. In another example, a layer of piezoelectric material 63 can be deposited on or above a floating metal plate 68, as shown in FIG. 9. The ALD process can begin with an initiation process to deposit a piezoelectric material, such as AlN. In a reaction chamber for an ALD processing step, the initiation process can include annealing, etching, or exposing a surface to one or more gases, or other steps to remove contaminants or otherwise prepare a surface for depositing material using ALD. In step 404, the crystal orientation of the layer of piezoelectric material can also be oriented. For example, the initiation process can be tailored to form a layer of piezoelectric material with a crystal structure c-axis orientation for elastic or mechanical waves in the "Z" direction shown in FIG. 8 or the "Y" direction shown in FIG. 9. In some cases, the layer of piezoelectric material can be formed to have another crystal structure c-axis orientation. After the initiation step, the ALD process in step 404 can proceed with exposure using precursor chemicals or reactants in a repeating sequence, as described herein.

[0150] The thickness of the layer of piezoelectric material formed in step 404 can be determined by the number of ALD cycles used, which can be adjusted to grow the layer of piezoelectric material uniformly and conformally with great precision. In some cases, step 404 can also include trimming the layer of piezoelectric material formed to improve the uniformity of the layer, adjust the thickness of the layer, or otherwise modify the layer of piezoelectric material. Trimming can be a relatively expensive and time-consuming process, but any trimming performed in step 404 can be relatively minor compared to when sputtering is used.

[0151] In step 406, the process includes forming first and second electrodes on the layer of piezoelectric material. For example, first electrodes 54A-54C and second electrodes 55A-55C can be formed on layer 53 of piezoelectric material as shown in FIG. 8. As another example, first electrodes 64A-64C and second electrodes 65A-65C can be formed on layer 63 of piezoelectric material as shown in FIG. 9. The first and second electrodes can be formed as thin layers or films of highly conductive material using ALD. The first and second electrodes can be formed using ALD to a thickness of 300 nm, 200 nm, or 100 nm or less. However, the first and second electrodes can be formed using ALD to be thinner layers, such as layers less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm thick, in some cases.

[0152] In step 408, the process includes forming an encapsulation layer over the first and second electrodes. By way of example, encapsulation layer 56 shown in FIG. 8 or encapsulation layer 66 shown in FIG. 9 may be formed. The encapsulation layer may be formed by an ALD processing step, with 100 nm or less of Al. 2 O 3 The encapsulation layer 46 can also be formed as a uniform and conformal thin film of Al using ALD, in some cases, such as a layer less than 10 nm, 5 nm, or even thinner. 2 O 3 Since other thin films of protective material can be formed using ALD, the encapsulation layer 46 can be formed as a thinner layer of Al. 2 O 3 The present invention is not limited to this layer.

[0153] In step 410, the process includes forming an isolation cavity, such as one of isolation cavities 57 shown in FIG. 8 or isolation cavities 67 shown in FIG. 9. The isolation cavity can be formed to any size suitable for the purpose of isolating acoustic waves. In some cases, the isolation cavity can be wider than those shown in FIGS. 8 and 9, and the isolation cavity can be larger (i.e., larger in length and width dimensions in top view) than the layer of piezoelectric material above it. The isolation cavity can be formed by etching or other material removal process steps. In some cases, the isolation cavity can be formed with one or more support pillars to provide additional support, as described herein.

[0154] 10 may include additional steps, such as forming one or more temperature compensating layers. For example, the process may include forming a SiO 2 It may be possible to include between steps 404 and 406 forming a temperature compensating layer, such as a layer of SiO 2 or other material for temperature compensation, between the first and second electrodes and the piezoelectric material using ALD. 2 By using ALD processing steps, the temperature compensating layer(s) can be more uniform, more conformal, and thinner than when formed using other deposition techniques. As some examples, SiO 2 The layer may be formed to a thickness of less than 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, or 20 nm.

[0155] In other cases, the process may include forming a support layer over the substrate after step 400 and before step 402. The support layer may be embodied as a layer of silicon, although other support layers may be used. The support layer may be deposited using a suitable deposition technique, such as PVD, CVD, or related techniques. The support layer may be formed to any suitable thickness, and it is not necessary for the support layer to be formed as a thin film.

[0156] Additionally, the process may include forming an acoustic mirror on the substrate after step 400 and before step 402. The acoustic mirror may be formed as alternating layers of materials having high and low acoustic impedances or refractive indices, such as Bragg reflectors. The acoustic mirror may provide acoustic wave isolation between the substrate and the resonator formed by the piezoelectric material later formed in step 404.

[0157] The above-described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments, and features described in various embodiments may be interchanged among the embodiments. In the foregoing description, specific details are provided to fully present the embodiments of the present disclosure. However, those skilled in the art will understand that the technical solutions of the present disclosure may be implemented without one or more of these specific details, or other methods, components, materials, and the like may be used. In other instances, well-known structures, materials, or operations have not been shown or described in detail to avoid obscuring aspects of the present disclosure.

[0158] Relative terms such as "on," "below," "upper," "lower," "top," "bottom," "right," and "left" may be used to describe the relative spatial relationships of certain structural features, but these terms are used only as directions in the examples for convenience. It should be understood that if the device were turned upside down, the "upper" component would become the "lower" component. When a structure or feature is described as being "on" (or formed on) another structure or feature, the structure may be disposed directly on (i.e., in contact with) the other structure, without any other structure or feature intervening between the structure and the other structure. When a structure or feature is described as being "over" (or formed on) another structure or feature, the structure may be disposed over the other structure, with or without the other structure or feature intervening between them. When two components are described as being "coupled" to one another, the components may be electrically coupled to one another with or without other components being electrically coupled and intervening between them. When two components are described as being "directly coupled" to one another, the components may be electrically coupled to one another with or without other components being electrically coupled between them. The "thickness" of a layer described herein may be measured from the top of the page to the bottom (i.e., in the Z direction) in a cross-sectional view.

[0159] Terms such as "a," "an," "the," and "said" are used to indicate the presence of one or more elements and components. The terms "comprise," "include," "have," "contain," and variations thereof are used to be open-ended and, unless otherwise specified, may include or encompass additional elements, components, etc., in addition to the listed elements, components, etc. Terms such as "first," "second," etc. are used only as labels and not limitations on several objects.

[0160] Although the embodiments have been described in detail herein, this description is for illustrative purposes. The embodiments described herein are representative, and alternative embodiments may add or omit certain features and elements. In addition, those skilled in the art may make modifications to aspects of the embodiments described herein without departing from the spirit and scope of the present invention as defined in the following claims, and the scope should be accorded the broadest interpretation to encompass modifications and equivalent structures.

Claims

1. 1. A method for manufacturing an acoustic resonator, comprising the steps of: Providing a substrate; depositing a layer of piezoelectric material on the substrate by atomic layer deposition; forming an electrode in contact with the layer of piezoelectric material; The method includes:

2. 10. The method of claim 1 , The electrodes include a first electrode, The method further includes forming a second electrode in contact with the piezoelectric material.

3. The method of claim 2 , wherein the first electrode and the second electrode are formed by sputtering a metal.

4. 3. The method of claim 2, the first electrode is formed by atomic layer deposition of a metal; The method of claim 1, wherein the second electrode is formed by sputtering a metal.

5. The method of claim 2 , wherein the first electrode and the second electrode are formed by atomic layer deposition of a metal.

6. The method of claim 2 , wherein in the acoustic resonator stack of material layers, both the first electrode and the second electrode are formed at least partially on the layer of piezoelectric material.

7. 3. The method of claim 2, wherein the stack of material layers of the acoustic resonator comprises: the first electrode is formed at least partially beneath the layer of piezoelectric material; The method of claim 1, wherein the second electrode is formed at least partially over the layer of piezoelectric material.

8. The method of claim 1 , further comprising forming an acoustic reflector on the substrate between the substrate and the layer of piezoelectric material.

9. The method of claim 8 , wherein the reflector comprises a plurality of layers of material, the plurality of layers comprising alternating layers of materials having varying refractive indices.

10. The method of claim 1 , further comprising forming a support layer on the substrate between the substrate and the layer of piezoelectric material.

11. The method of claim 10 , further comprising forming an air cavity in the substrate in a region beneath the piezoelectric material.

12. The method of claim 11 , wherein the cavity comprises a plurality of support pillars.

13. The method of claim 1 , comprising trimming the layer of piezoelectric material after depositing the layer of piezoelectric material by atomic layer deposition.

14. The method of claim 1 , wherein the piezoelectric material comprises aluminum nitride.

15. The method of claim 1 , further comprising forming an encapsulation layer over the electrode by atomic layer deposition.

16. 1. An acoustic resonator comprising: A substrate; a layer of piezoelectric material deposited on the substrate by atomic layer deposition; an electrode in contact with the layer of piezoelectric material; 1. An acoustic resonator comprising:

17. 17. The acoustic resonator of claim 16, wherein the layer of piezoelectric material comprises a layer of aluminum nitride having a thickness of 100 nm or less.

18. The acoustic resonator according to claim 16 further comprises: a second electrode in contact with the piezoelectric material; At least one of the electrode or the second electrode is formed by atomic layer deposition of a metal.

19. 20. The acoustic resonator of claim 16, further comprising an acoustic reflector on the substrate between the substrate and the layer of piezoelectric material.

20. 17. The acoustic resonator of claim 16, further comprising a support layer on the substrate between the substrate and the layer of piezoelectric material.

Citation Information

Patent Citations

  • Film piezoelectric acoustic wave filter and manufacturing method thereof

    CN112039485A

  • Thin-film piezoelectric bulk wave resonator and its manufacturing method, and thin-film piezoelectric bulk wave resonator filter using thin-film piezoelectric bulk wave resonator

    JP2009124640A

  • Elastic wave device and manufacturing method of the same

    JP2012160979A

  • Depressed frame structure for bulk acoustic wave resonator

    JP2020043566A

  • MULTIPLE LAYER SYSTEM, MANUFACTURING METHOD, AND SAW DEVICE FORMED ON A MULTIPLE LAYER SYSTEM - Patent application

    JP2021516015A