Silicone rubber composition

The hydrosilylation-curable silicone rubber composition addresses fast curing and thermal stability issues by incorporating specific components, ensuring high tear strength and compliance with international standards for electric vehicle cables.

JP2024543072AInactive Publication Date: 2024-11-19DOW SILICONES CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024527796
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-11-19
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing hydrosilylation-curable silicone rubber compositions face challenges in achieving fast curing at lower temperatures without odor, requiring post-curing treatments, and ensuring high tear strength and thermal stability, particularly in high-temperature applications like electric vehicles and hybrid electric vehicles.

Method used

A hydrosilylation-curable silicone rubber composition comprising an organopolysiloxane polymer with unsaturated groups, reinforcing silica filler, a filler treatment agent, an organosilicon compound with Si-H groups, and a hydrosilylation catalyst, along with specific heat stabilizers like dodecanedioic acid and metal phthalocyanine complexes, which allows for rapid curing at lower temperatures and enhanced thermal stability.

Benefits of technology

The composition achieves rapid curing without odor, high tear strength, and meets stringent thermal stability requirements, passing ISO6722 and LV216 standards for long-term heat aging, making it suitable for high-voltage power cables in electric vehicles and hybrid electric vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543072000001
    Figure 2024543072000001
  • Figure 2024543072000002
    Figure 2024543072000002
  • Figure 2024543072000003
    Figure 2024543072000003
Patent Text Reader

Abstract

The present invention relates to a hydrosilylation (addition) curable heat stabilized silicone rubber composition, a silicone rubber elastomer produced upon curing of the composition, and their applications and uses. The heat stabilizer additives utilized in the composition include one or more of dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide], 1,2-di[-(3,5-di-tert-butyl-4-hydroxy-phenyl)propionyl]hydrazine, metal or non-metal phthalocyanine complexes, salicyloylaminotriazole, triazole, benzotriazole, dilauryl 3,3'-thiodipropionate, ditridecyl 3,3'-thiodipropionate, diphenyl sulfide, and / or pentaerythritol β-laurylthiopropionate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to hydrosilylation (addition) curable heat stabilized silicone rubber compositions, silicone rubber elastomers produced upon curing of the compositions, and their applications and uses.

[0002] Hydrosilylation-curable silicone rubber compositions containing an organopolysiloxane polymer having unsaturated (alkenyl and / or alkynyl) groups and a compound containing silicon-bonded hydrogen atoms curable by a hydrosilylation reaction in the presence of a hydrosilylation catalyst are known in the art.

[0003] Such compositions are usually stored prior to use in two or more parts to prevent premature curing, but have the following advantages over radical (i.e., peroxide) reaction curable silicone rubber compositions, which tend to be used when the silicone polymer is a high viscosity silicone rubber: - Can be cured faster and at lower temperatures The curing process is virtually odorless The curing process does not usually require post-curing treatment The resulting elastomer usually has higher tear strength

[0004] It is known that the hydrosilylation-curable silicone rubber compositions may have improved thermal stability through the incorporation of one or more inorganic heat stabilizers, such as hydrated cerium oxide, hydrated aluminum oxide, cerium hydroxide, red iron oxide, carbon black, graphite, and zinc oxide, used alone or in combination.

[0005] The silicone elastomer products cured from the above composition are used in various fields due to their excellent physical and thermal stability properties.For example, the silicone elastomer products made from such compositions are used in various high temperature applications due to their excellent thermal stability compared to organic rubbers.Applications include, for example, electronics, which tend to be used to cover / encapsulate solid electronic devices such as transistors, integrated circuits and circuit boards, and are increasingly used in both automotive and power applications, for example for power cable insulation.

[0006] Therefore, increasingly, hydrosilylation-curable silicone rubber compositions are being used for power cable insulation purposes in electric vehicles (EVs) and / or hybrid electric vehicles (HEVs).The hydrosilylation-curable silicone rubber compositions can be extruded onto large diameter high voltage power cables to provide a continuous outer sheath on the cables.

[0007] Such high voltage power cables are used in EVs and HEVs to connect the charge port to the battery and to hardwire the battery to the engine through an inverter, where low voltage power is transferred from the battery module / pack to the inverter, where the voltage is amplified to a significantly larger voltage, e.g., 500V or more, and then transferred to the drive motor to provide power for sustained periods of time to allow acceptable long trips between recharges. Furthermore, because HEV and EV power cables may be exposed to other heat sources in the engine, e.g., exhaust heat, the ability to maintain sufficient thermal stability over long periods of time is an important feature of such cables.

[0008] Considering the increasing demands from HEV and EV manufacturers, power cables are required to meet very high performance requirements according to international standards due to the harsh environment in which they are placed within the vehicle. For example, the increase in the operating voltage platform of the battery modules and / or battery packs of EVs and HEVs requires high voltage cables to have excellent heat aging performance and pass the Class E requirements for ISO6722 and LV216 standards, i.e., the ability to withstand long-term heat aging at 175 or 180°C for 3,000 hours and short-term heat aging at 200°C for 240 hours, after which the resulting aged cable must again pass the winding test.

[0009] Provided herein is a hydrosilylation-curable, heat-stabilized silicone rubber composition comprising the following components: a) an organopolysiloxane polymer having a Williams plasticity of at least 100 mm / 100 as measured in accordance with ASTM D-926-08 and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups; b) a reinforcing silica filler; and c) a linear or branched organopolysiloxane filler treating agent comprising a plurality of units of the structure: -((R 10 )2SiO)- In the formula, each R 10 may be the same or different and are alkyl groups having 1 to 10 carbons, alternatively alkyl groups having 1 to 6 carbons, or aromatic groups having 6 to 12 carbons, the number average degree of polymerization being in the range of 1 to 50, and each end group containing at least one hydroxyl or alkoxy; d) an organosilicon compound having at least two, or at least three, Si-H groups per molecule; e) Dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide], 1,2-di[-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, a heat stabilizer additive selected from one or more of metal or non-metal phthalocyanine complexes, salicyloylaminotriazole, triazole, benzotriazole, dilauryl 3,3′-thiodipropionate, ditridecyl 3,3′-thiodipropionate, diphenyl sulfide, and / or pentaerythritol β-lauryl thiopropionate; f) a hydrosilylation catalyst comprising or consisting of a platinum group metal or a compound thereof.

[0010] Also described herein is a process for the preparation of a hydrosilylation cured, heat stabilized silicone rubber, comprising: (i) preparing a silicone rubber base composition, the composition comprising: a) an organopolysiloxane polymer having a Williams plasticity of at least 100 mm / 100 as measured in accordance with ASTM D-926-08 and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups; b) a reinforcing silica filler; and c) a linear or branched organopolysiloxane filler treating agent comprising a plurality of units of the structure: -((R 10 )2SiO)- In the formula, each R 10 may be the same or different and are alkyl groups having 1 to 10 carbons, alternatively alkyl groups having 1 to 6 carbons, or aromatic groups having 6 to 12 carbons, the number average degree of polymerization being in the range of 1 to 50, and each end group containing at least one hydroxyl or alkoxy; (ii) adding to the silicone rubber base of step (i), d) an organosilicon compound having at least two, or at least three, Si-H groups per molecule; e) Dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide], 1,2-di[-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, simultaneously or sequentially with a heat stabilizer additive selected from one or more of metal or non-metal phthalocyanine complexes, salicyloylaminotriazole, triazole, benzotriazole, dilauryl 3,3'-thiodipropionate, ditridecyl 3,3'-thiodipropionate, diphenyl sulfide and / or pentaerythritol β-lauryl thiopropionate; f) a hydrosilylation catalyst comprising or consisting of a platinum group metal or a compound thereof; (iii) curing the composition.

[0011] In addition, in this specification, e) Dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide], 1,2-di[-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, There is also provided the use of an additive selected from one or more of metal or non-metal phthalocyanine complexes, salicyloylaminotriazole, triazole, benzotriazole, dilauryl 3,3'-thiodipropionate, ditridecyl 3,3'-thiodipropionate, diphenyl sulfide and / or pentaerythritol β-laurylthiopropionate as a heat stabilizer in a composition, which composition further comprises the following components: a) an organopolysiloxane polymer having a Williams plasticity of at least 100 mm / 100 as measured in accordance with ASTM D-926-08 and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups; b) a reinforcing silica filler; and c) a linear or branched organopolysiloxane filler treating agent comprising a plurality of units of the structure: -((R10 )2SiO)- In the formula, each R 10 may be the same or different and are alkyl groups having 1 to 10 carbons, alternatively alkyl groups having 1 to 6 carbons, or aromatic groups having 6 to 12 carbons, the number average degree of polymerization being in the range of 1 to 50, and each end group containing at least one hydroxyl or alkoxy; d) Organosilicon compounds having at least two or at least three Si-H groups per molecule. and, f) a hydrosilylation catalyst comprising or consisting of a platinum group metal or a compound thereof.

[0012] There is also provided herein an electric power cable, comprising: A conductive core; one or more insulating layers around said core; an outer sheath made from a heat stabilized silicone rubber that is the cured product of the above composition.

[0013] Also provided herein is the use of a heat stabilized silicone rubber, which is the cured product of the above composition, as an outer sheath for a power cable.

[0014] Also provided herein is a method for manufacturing a power cable, comprising the steps of applying and curing an outer sheath about the cable, the outer sheath being the cured product of the composition described herein above.

[0015] In each case, the total weight (wt.) percentage of each composition given herein is 100 wt.%.

[0016] Surprisingly, it was found that the use of additive (e) in the above compositions improved the short-term (240 hours at 200°C) and long-term (3000 hours at 180°C) thermal stability in hydrosilylation curable compositions using silicone rubbers (having a viscosity of more than 1,000,000 mPa·s at 25°C), i.e., having a Williams plasticity of at least 100 mm / 100 as measured according to the above-mentioned ASTM D-926-08. More importantly, it enabled such compositions to pass the international thermal stability tests ISO 6722 and LV 216 standards (class E for long-term heat aging at 175 or 180°C for 3,000 hours, and short-term heat aging at 200°C for 240 hours).

[0017] The components of the composition are as follows: Component (a) Component (a) is an organopolysiloxane polymer having a Williams plasticity of at least 100 mm / 100 as measured according to ASTM D-926-08 and at least two unsaturated groups per molecule. The unsaturated groups are selected from alkenyl and / or alkynyl groups.

[0018] Each organopolysiloxane polymer of component (a) contains a plurality of siloxy units of formula (I). R' a SiO (4-a) / 2 (I)

[0019] The subscript "a" is 0, 1, 2, or 3.

[0020] Siloxy units may be described by shorthand nomenclature, i.e., "M," "D," "T," and "Q," where R' is as above or is an alkyl group, typically a methyl group. M units are siloxy units where a=3, i.e., R'SiO 1 / 2 and D units are siloxy units where a=2, i.e., R'SiO 2 / 2 where T units are siloxy units where a=1, i.e., R'SiO 3 / 2and Q units are siloxy units where a=0, i.e., SiO 4 / 2 The organopolysiloxane polymer of component (a) is substantially linear, but may contain a percentage of branching due to the presence of T units (as described above) within the molecule, such that the average value of a in structure (I) is about 2.

[0021] The unsaturated groups of component (a) may be located at either the terminal or pendant positions of the organopolysiloxane polymer, or at both positions. The unsaturated groups of component (a) may be alkenyl or alkynyl groups as described above. Each alkenyl group, if present, may contain, for example, 2 to 30, alternatively 2 to 24, alternatively 2 to 20, alternatively 2 to 12, alternatively 2 to 10, alternatively 2 to 6 carbon atoms. If present, the alkenyl groups may be exemplified by, but are not limited to, vinyl, allyl, methallyl, isopropenyl, propenyl, and hexenyl, and cyclohexenyl groups. Each alkynyl group, if present, may have 2 to 30, alternatively 2 to 24, alternatively 2 to 20, alternatively 2 to 12, alternatively 2 to 10, alternatively 2 to 6 carbon atoms. Examples of alkynyl groups may be exemplified by, but are not limited to, ethynyl, propynyl, and butynyl groups. Preferred examples of the unsaturated groups of component (a) include vinyl, propenyl, isopropenyl, butenyl, allyl, and 5-hexenyl.

[0022] In formula (I), each R' other than the above unsaturated groups is independently selected from an aliphatic hydrocarbyl group, a substituted aliphatic hydrocarbyl group, an aromatic group, or a substituted aromatic group. Each aliphatic hydrocarbyl group may be exemplified by, but is not limited to, an alkyl group having 1-20 carbons per group, alternatively 1-15 carbons per group, alternatively 1-12 carbons per group, alternatively 1-10 carbons per group, alternatively 1-6 carbons per group, or a cycloalkyl group such as cyclohexyl. Specific examples of alkyl groups include methyl, ethyl, propyl, pentyl, octyl, undecyl, and octadecyl groups, or methyl and ethyl groups. The substituted aliphatic hydrocarbyl group is preferably a non-halogenated substituted alkyl group.

[0023] Aliphatic non-halogenated organyl groups are exemplified by suitable nitrogen-containing groups, such as the above alkyl groups with substituents, such as amide or imide groups; oxygen-containing groups, such as polyoxyalkylene groups, carbonyl groups, alkoxy groups, and hydroxyl groups, but are not limited thereto.Further organyl groups may include sulfur-containing groups, phosphorus-containing groups, and boron-containing groups.Examples of aromatic groups or substituted aromatic groups are phenyl groups and substituted phenyl groups with the above substituents.

[0024] Component (a) may be selected, for example, from polydimethylsiloxanes, alkylmethylpolysiloxanes, alkylarylpolysiloxanes, or copolymers thereof (where reference to alkyl means any suitable alkyl group, or alternatively, alkyl groups having 2 or more carbons), provided that each polymer contains at least two unsaturated groups, typically alkenyl groups as described above, and has a degree of polymerization of at least 2,500. They may be, for example, trialkyl-terminated, alkenyldialkyl-terminated, alkynyldialkyl-terminated, or terminated with any other suitable combination of end groups, provided that each polymer has a Williams plasticity of at least 100 mm / 100 as measured according to ASTM D-926-08 and at least two unsaturated groups.

[0025] Thus, component (a) may, for example, be: dialkylalkenyl-terminated polydimethylsiloxanes, such as dimethylvinyl-terminated polydimethylsiloxanes, dialkylalkenyl-terminated dimethylmethylphenylsiloxanes, such as dimethylvinyl-terminated dimethylmethylphenylsiloxanes, trialkyl-terminated dimethylmethylvinylpolysiloxanes, dialkylvinyl-terminated dimethylmethylvinylpolysiloxane copolymers, dialkylvinyl-terminated methylphenylpolysiloxanes, dialkylalkenyl-terminated methylvinylmethylphenylsiloxanes, dialkylalkenyl-terminated methylvinyldiphenylsiloxanes, dialkylalkenyl-terminated methylvinylmethylphenyldimethylsiloxanes, trimethyl-terminated methylvinylmethylphenylsiloxanes, trimethyl-terminated methylvinyldiphenylsiloxanes, or trimethyl-terminated methylvinylmethylphenyldimethylsiloxanes.

[0026] In each case, component (a) has a Williams plasticity of at least 100 mm / 100 as measured according to ASTM D-926-08. Organopolysiloxane polymers of this magnitude are commonly referred to in the industry as organopolysiloxane polymer gums, siloxane gums or silicone gums (hereafter referred to as silicone gums) because of their very high viscosity (at least 1,000,000 mPa.s at 25° C., often several million mPa.s at 25° C.) and high molecular weight. Because of the difficulty in measuring the viscosity of such high viscosity fluids, silicone gums tend to be defined in terms of Williams plasticity values, as opposed to viscosity. Component (a) is a silicone gum and has a Williams plasticity of at least 100 mm / 100 as measured according to ASTM D-926-08, alternatively at least 125 mm / 100 as measured according to ASTM D-926-08, alternatively at least 140 mm / 100 as measured according to ASTM D-926-08. Typically, silicone rubbers have a Williams plasticity of about 100 mm / 100 to 300 mm / 100, measured according to ASTM D-926-08.

[0027] The number average molecular weight (Mn) and weight average molecular weight (Mw) of such polymers are typically determined by gel permeation chromatography using polystyrene standards. In this disclosure, the number average molecular weight and weight average molecular weight values ​​of the silicone rubber used as component (a) herein were determined using a Waters 2695 Separations Module equipped with a vacuum degasser and a Waters 2414 refractive index detector (Waters Corporation, MA, USA). Analysis was performed using certified grade toluene flowing at 1.0 mL / min as the eluent. Data collection and analysis were performed using Waters Empower GPC software.

[0028] The degree of polymerization of the polymer was approximately the number average molecular weight of the polymer divided by 74 (the molecular weight of one component (I) above).

[0029] Typically, the alkenyl and / or alkynyl content, e.g., vinyl content, of the polymer is 0.01 to 3% by weight of component (a) for the or each organopolysiloxane polymer containing at least two silicon-bonded alkenyl groups per molecule, alternatively 0.01 to 2.5% by weight of component (a), alternatively 0.01 to 2.0% by weight of component (a), alternatively 0.01 to 1.5% by weight of the organopolysiloxane polymer containing at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups per molecule of component (a). The alkenyl / alkynyl content of component (a) is determined using quantitative infrared analysis according to ASTM E168.

[0030] Component (a) may be present in the composition in an amount from 40% to about 90% by weight of the composition, alternatively 45-85% by weight of the composition, alternatively 50-80% by weight of the composition. Typically, component (a) is present in an amount which is the difference between 100% by weight and the cumulative weight % of the other components / ingredients of the composition.

[0031] Ingredient (b) Component (b) is at least one reinforcing silica filler. Preferably, the reinforcing silica filler is in finely divided form. Reinforcing silica filler (b) may be exemplified by fumed silica, colloidal silica and / or precipitated silica.

[0032] Precipitated silica, fumed silica and / or colloidal silica are typically at least 50 ml 2 / g (BET method according to ISO9277:2010), alternatively 50-450m 2 / g (BET method according to ISO9277:2010), alternatively between 50 and 300 m 2 / g (BET method according to ISO 9277:2010). All of these types of silica are commercially available.

[0033] The reinforcing silica fillers of component (b) are hydrophilic in nature and are treated with one or more treating agents (c) to render them hydrophobic. These surface-modified reinforcing fillers of component (b) do not agglomerate and can be homogeneously incorporated into the organopolysiloxane polymer (a) described below, since the surface treatment renders the fillers easily wetted by the organopolysiloxane polymer (a).

[0034] Component (b) is present in an amount up to 50% by weight of the composition, alternatively from 1.0 to 50% by weight of the composition, alternatively from 5.0 to 45% by weight of the composition, alternatively from 10.0 to 40% by weight of the composition.

[0035] Ingredient (c) The reinforcing silica filler (b) is hydrophobically treated by treatment with component (c), which component (c) of the compositions herein comprises a dialkylhydroxy- or dialkylalkoxy-terminated short chain linear or branched polydiorganosiloxane comprising a plurality of units of the structure: -((R 10 )2SiO)- In the formula, each R10 may be the same or different and are an alkyl group having 1 to 10 carbons, alternatively an alkyl group having 1 to 6 carbons, alternatively methyl, ethyl or propyl, alternatively an aromatic group having 6 to 12 carbons, alternatively phenyl, and the number average degree of polymerization ranges from 2 to 50, alternatively 2 to 25. 10 is selected from methyl, ethyl, propyl and phenyl. Each terminal alkoxy group, when present, typically has 1 to 6 carbons, but is preferably ethoxy or methoxy. Thus, the short chain linear or branched polydiorganosiloxane may be selected from dimethylhydroxy-terminated polydimethylsiloxane, dimethylmethoxy-terminated polydimethylsiloxane or dimethylethoxy-terminated polydimethylsiloxane having a number average degree of polymerization of 2 to 25, alternatively 2 to 20, dimethylhydroxy-terminated polymethylphenylsiloxane, dimethylmethoxy-terminated polymethylphenylsiloxane or dimethylethoxy-terminated polymethylphenylsiloxane having a number average degree of polymerization of 2 to 25, alternatively 5 to 20, and / or dimethylhydroxy-terminated polydimethylmethylphenylsiloxane copolymer, dimethylmethoxy-terminated polydimethylmethylphenylsiloxane copolymer or dimethylethoxy-terminated polydimethylmethylphenylsiloxane copolymer having a number average degree of polymerization of 2 to 25, alternatively 2 to 20, for example: HO-((R 10 )2SiO) x -H, where x is the number average degree of polymerization.

[0036] Molecular weight values ​​can also be determined by gel permeation chromatography, but polymers at the lower end of the range, for example having a DP of about 2 to 20, can be analyzed by gas chromatography mass spectrometry (GC-MS).

[0037] The surface treatment of the untreated reinforcing filler of component (b) may be carried out prior to introduction into the composition or in situ (i.e., by blending the other ingredients together at room temperature or above in the presence of at least a portion of the other ingredients of the composition herein until the filler is completely treated). Typically, the untreated reinforcing filler (b) is treated in situ in the presence of the organopolysiloxane polymer (a) with a treating agent comprising or consisting of component (c), thereby preparing a silicone rubber base material which can then be mixed with the other ingredients. Component (c) may be present in the composition in an amount of 0.1 to 20% by weight of the composition, alternatively 0.5 to 15% by weight of the composition, alternatively 1 to 10% by weight of the composition.

[0038] Ingredient (d) Component (d) functions as a crosslinker and is provided in the form of an organosilicon compound having at least two, or alternatively at least three, Si-H groups per molecule. Component (d) typically contains three or more silicon-bonded hydrogen atoms so that the hydrogen atoms can react with the unsaturated alkenyl and / or alkynyl groups of component (a) to form a network therewith, thereby curing the composition. Alternatively, when polymer (a) has more than two unsaturated groups per molecule, some or all of component (d) can have two silicon-bonded hydrogen atoms per molecule.

[0039] The molecular architecture of the organosilicon compound (d) having at least two, alternatively at least three, terminal -Si-H groups per molecule is not particularly limited and can be linear, branched (linear with some branching through the presence of T groups), cyclic, or silicone resin-based.

[0040] The molecular weight of component (d) is not particularly limited, but in order to obtain good miscibility with polymer (a), the viscosity is typically less than 10 s at a shear rate of 10 s. -1 When measured using a TA instruments AR2000 Rheometer in a plate-plate model, the resistance is 5 to 50,000 mPa.s at 25°C.

[0041] The silicon-bonded organic groups used in component (d) may be exemplified by alkyl groups such as methyl, ethyl, propyl, n-butyl, t-butyl, pentyl, hexyl, etc.; aryl groups such as phenyl, tolyl, xylyl, or similar aryl groups; 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl groups, and are preferably alkyl groups having 1 to 6 carbons, particularly methyl, ethyl, or propyl groups, or phenyl groups. Preferably, the silicon-bonded organic groups used in component (b) are alkyl groups, or methyl, ethyl, or propyl groups.

[0042] Examples of organosilicon compounds (d) having at least two, or at least three, Si-H groups per molecule include, but are not limited to, the following: (a) trimethylsiloxy-terminated methylhydrogenpolysiloxane, (b) trimethylsiloxy-terminated polydimethylsiloxane-methylhydrogensiloxane; (c) dimethylhydrogensiloxy-terminated dimethylsiloxane-methylhydrogensiloxane copolymer; (d) dimethylsiloxane-methylhydrogensiloxane cyclic copolymers; (e)(CH3)2HSiO 1 / 2 Unit: (CH3)3SiO 1 / 2 Units, and SiO 4 / 2 copolymers and / or silicone resins consisting of units; (f)(CH3)2HSiO 1 / 2 Units and SiO 4 / 2 copolymers and / or silicone resins consisting of units; (g) methylhydrogensiloxane cyclic homopolymers having 3 to 10 silicon atoms per molecule; Alternatively, the crosslinker, component (d), can be a filler, such as silica treated with one of the above, and mixtures thereof.

[0043] In one embodiment, component (d) is selected from the group consisting of methylhydrogenpolysiloxanes having both molecular terminals blocked with trimethylsiloxy groups; copolymers of methylhydrogensiloxanes and dimethylsiloxanes having both molecular terminals blocked with trimethylsiloxy groups; dimethylsiloxanes having both molecular terminals blocked with dimethylhydrogensiloxy groups; and copolymers of methylhydrogensiloxanes and dimethylsiloxanes having both molecular terminals blocked with dimethylhydrogensiloxy groups.

[0044] The crosslinker (d) is generally present in the hydrosilylation curable heat stabilized silicone rubber composition such that the molar ratio of the total number of silicon-bonded hydrogen atoms in component (d) to the total number of alkenyl and / or alkynyl groups in polymer (a) or the composition, if different, is 0.5:1 to 20:1. If this ratio is less than 0.5:1, a sufficiently cured composition is not obtained. If this ratio exceeds 20:1, the hardness of the cured composition tends to increase when heated. Preferably, it is present in an amount such that the molar ratio of silicon-bonded hydrogen atoms of component (d) to the alkenyl / alkynyl groups or alkenyl groups in component (a) or the composition is in the range of 0.7:1.0 to 5.0:1.0, preferably 0.9:1.0 to 2.5:1.0, and most preferably 0.9:1.0 to 2.0:1.0.

[0045] The silicon-bonded hydrogen (Si-H) content of component (d) is determined using quantitative infrared analysis according to ASTM E168. In the present invention, the ratio of silicon-bonded hydrogen to alkenyl (vinyl) and / or alkynyl is important when relying on a hydrosilylation cure process. Generally, this is determined by calculating the total weight percent of alkenyl groups in the composition, e.g., vinyl [V], and the total weight percent of silicon-bonded hydrogen [H] in the composition, where the molecular weight of hydrogen is 1 and the molecular weight of vinyl is 27, resulting in a molar ratio of silicon-bonded hydrogen to vinyl of 27 [H] / [V].

[0046] Typically, depending on the number of unsaturated groups in component (a) and the number of Si-H groups in component (d), component (d) is present in an amount from 0.1 to 10 weight percent of the hydrosilylation-curable, heat-stabilized silicone rubber composition, alternatively from 0.1 to 7.5 weight percent of the hydrosilylation-curable, heat-stabilized silicone rubber composition, alternatively from 0.5 to 7.5 weight percent of the hydrosilylation-curable, heat-stabilized silicone rubber composition, and alternatively from 0.5% to 5 weight percent.

[0047] Ingredient (e) Ingredient (e) A heat stabilizer additive selected from one or more of dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide], 1,2-di[-(3,5-di-tert-butyl-4-hydroxy-phenyl)propionyl]hydrazine, dilauryl 3,3'-thiodipropionate, ditridecyl 3,3'-thiodipropionate, diphenyl sulfide, pentaerythritol β-laurylthiopropionate, metal or non-metal phthalocyanine complexes, salicyloylaminotriazole, triazole, benzotriazole, and mixtures thereof. Component (e) may be present in the composition in an amount of 0.001 to 5% by weight of the composition, alternatively 0.01 to 5% by weight of the composition, alternatively 0.01 to 3% by weight of the composition.

[0048] Component (f) Component (f) of the hydrosilylation curable heat-stabilized silicone rubber composition is a hydrosilylation catalyst that includes or consists of a platinum group metal or its compound. They are usually selected from catalysts of platinum group metals (platinum, ruthenium, osmium, rhodium, iridium, and palladium) or one or more compounds of such metals. Alternatively, platinum and rhodium compounds are preferred due to the high activity level of these catalysts in hydrosilylation reactions, with platinum compounds being most preferred. In hydrosilylation (or addition) reactions, hydrosilylation catalysts such as component (f) herein catalyze the reaction between unsaturated groups, usually alkenyl groups, such as vinyl, and Si-H groups.

[0049] The hydrosilylation catalyst of component (f) can be a platinum group metal, a platinum group metal deposited on a support, such as activated carbon, a metal oxide such as aluminum oxide or silicon dioxide, silica gel or powdered charcoal, or a compound or complex of a platinum group metal. Preferably, the platinum group metal is platinum.

[0050] Examples of preferred hydrosilylation catalysts of component (f) are platinum-based catalysts such as platinum black, platinum oxide (Adams' catalyst), platinum on various solid supports, chloroplatinic acid such as hexachloroplatinic acid (Pt oxidation state IV) (Speyer's catalyst), chloroplatinic acid in a solution of an alcohol such as isooctanol or amyl alcohol (Lamoreaux's catalyst), and complexes of chloroplatinic acid with ethylenically unsaturated compounds such as olefins and organosiloxanes containing ethylenically unsaturated silicon-bonded hydrocarbon groups, such as tetra-vinyl-tetramethylcyclotetrasiloxane-platinum complex (Ashby's catalyst). Usable soluble platinum compounds include, for example, platinum-olefin complexes of the formula (PtCl2.(olefin)2 and H(PtCl3.olefin), in which in this context it is preferred to use alkenes having 2 to 8 carbon atoms, such as ethylene, propylene, isomers of butene and isomers of octene, or cycloalkanes having 5 to 7 carbon atoms, such as cyclopentene, cyclohexene and cycloheptene. Other soluble platinum catalysts are, for example, platinum-cyclopropane complexes of the formula (PtCl2C3H6)2. , the reaction products of hexachloroplatinic acid with alcohols, ethers, and aldehydes, or mixtures thereof, or the reaction products of hexachloroplatinic acid and / or its conversion products with vinyl-containing siloxanes, such as methylvinylcyclotetrasiloxane, in the presence of sodium bicarbonate in an ethanolic solution. Platinum catalysts with phosphorus, sulfur, and amine ligands can also be used, for example (Ph3P)2PtCl2, and complexes of platinum with vinyl siloxanes, such as sym-divinyltetramethyldisiloxane.

[0051] Therefore, specific examples of suitable platinum-based catalysts of component (f) include: (i) Complexes of chloroplatinic acid with organosiloxanes containing ethylenically unsaturated hydrocarbon groups, as described in U.S. Pat. No. 3,419,593; (ii) Chloroplatinic acid, either in its hexahydrate or anhydrous form; (iii) platinum-containing catalysts obtained by a process comprising reacting chloroplatinic acid with an aliphatically unsaturated organosilicon compound, such as divinyltetramethyldisiloxane; (iv) alkene-platinum-silyl complexes as described in U.S. Pat. No. 6,605,734, such as (COD)Pt(SiMeCl2)2, where "COD" is 1,5-cyclooctadiene, and / or (v) Karstedt's catalyst, which is a platinum divinyltetramethyldisiloxane complex, typically containing about 1% by weight of platinum in a vinylsiloxane polymer. Historically, solvents such as organic solvents such as toluene have been used as alternatives, but the use of vinylsiloxane polymers is a much more preferred choice. These are described in U.S. Pat. Nos. 3,715,334 and 3,814,730. In a preferred embodiment, component (f) can be selected from platinum coordination compounds. In one embodiment, hexachloroplatinic acid and its conversion products with vinyl-containing siloxanes, Karstedt's catalyst, and Speier's catalyst are preferred.

[0052] The catalytic amount of the hydrosilylation catalyst is generally from 0.01 ppm to 10,000 ppm, alternatively from 0.01 to 5000 ppm, alternatively from 0.01 to 3,000 ppm, alternatively from 0.01 to 1,000 ppm, based on the weight of the composition in parts per million (ppm). In certain embodiments, the catalytic amount of the catalyst may range from 0.01 to 1,000 ppm, alternatively from 0.01 to 750 ppm, alternatively from 0.01 to 500 ppm, alternatively from 0.01 to 100 ppm, based on the weight of the composition. The ranges may relate to only the metal content in the catalyst, or to the entire catalyst (including its ligands), as specified, but typically these ranges relate to only the metal content in the catalyst. The catalyst may be added as a single species or as a mixture of two or more different species. Typically, depending on, for example, the form / concentration in which the catalyst is provided in the polymer or solvent, the amount of component (f) present will be in the range of 0.001 to 3.0 weight percent of the composition, alternatively 0.001 to 2.5 weight percent of the composition, alternatively 0.01 to 2.0 weight percent of the hydrosilylation-curable heat stabilized silicone rubber composition.

[0053] Additional Optional Ingredients Additional optional components may be present in the hydrosilylation-curable heat-stabilized silicone rubber composition described above depending on its intended end use. Examples of such optional components include cure inhibitors, compression set additives, additional hydrophobic treatments other than component (c), pigments and / or colorants, and other additional additives such as pot life extenders, flame retardants, mold release agents, UV light stabilizers, fungicides, and mixtures thereof.

[0054] Optional hydrosilylation inhibitors The hydrosilylation curable heat-stabilized silicone rubber composition described herein may also contain one or more optional hydrosilylation reaction inhibitors. Hydrosilylation reaction inhibitors are used to prevent or delay the hydrosilylation reaction inhibitor curing process when necessary, especially during storage. The optional hydrosilylation reaction inhibitors of platinum-based catalysts are well known in the art and include hydrazines, triazoles, phosphines, mercaptans, organic nitrogen compounds, acetylene alcohols, silylated acetylene alcohols, maleates, fumarates, ethylenically or aromatically unsaturated amides, ethylenically unsaturated isocyanates, olefinic siloxanes, unsaturated hydrocarbon monoesters and diesters, conjugated ene-ynes, hydroperoxides, nitriles, and diaziridines. Alkenyl-substituted siloxanes such as those described in US Pat. No. 3,989,667 may also be used, of which cyclic methylvinyl siloxanes are preferred.

[0055] One class of known hydrosilylation reaction inhibitors are the acetylenic compounds disclosed in U.S. Patent No. 3,445,420. Acetylenic alcohols such as 2-methyl-3-butyn-2-ol constitute a preferred class of inhibitors which suppress the activity of platinum-containing catalysts at 25° C. Typically, compositions containing these inhibitors must be heated at temperatures above 70° C. in order to cure at a practical rate.

[0056] Examples of acetylenic alcohols and their derivatives include 1-ethynyl-1-cyclohexanol (ETCH), 2-methyl-3-butyn-2-ol, 3-butyn-1-ol, 3-butyn-2-ol, propargyl alcohol, 1-phenyl-2-propyn-1-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-ethynylcyclopentanol, 3-methyl-1-penten-4-yn-3-ol, and mixtures thereof. Derivatives of acetylenic alcohols may include those compounds having at least one silicon atom.

[0057] In some cases, low hydrosilylation inhibitor concentrations, which may be as little as one mole of hydrosilylation inhibitor per mole of metal of catalyst (f), if present, still impart satisfactory storage stability and cure speed. In other cases, hydrosilylation inhibitor concentrations of up to 500 moles of inhibitor per mole of metal of catalyst may be required. The optimum concentration of a given hydrosilylation inhibitor in a given composition is readily determined by routine experimentation. Depending on the concentration and form in which the selected hydrosilylation inhibitor is commercially provided / available, if present in the composition, the inhibitor is typically present in an amount of 0.0125-10% by weight of the composition.

[0058] In one embodiment, the inhibitor, if present, is selected from 1-ethynyl-1-cyclohexanol (ETCH) and / or 2-methyl-3-butyn-2-ol and is present in an amount of greater than 0 to 0.1% by weight of the composition.

[0059] Optional Additional Hydrophobizing Treatment Agent The reinforcing silica filler is treated with component (c) as described herein above. Optionally, additional hydrophobizing agents such as organosilanes or organosilazanes, such as hexaalkyldisilazanes and short chain methylvinylsiloxane diols, can be utilized. Specific examples include, but are not limited to, silanol-terminated trifluoropropylmethylsiloxane, silanol-terminated vinylmethyl (ViMe) siloxane, hexaorganodisiloxanes, such as hexamethyldisiloxane, divinyltetramethyldisiloxane. Hexaorganodisilazanes, such as hexamethyldisilazane (HMDZ), divinyltetramethyldisilazane, and tetramethyldi(trifluoropropyl)disilazane; hydroxyldimethyl-terminated polydimethylmethylvinylsiloxane, octamethylcyclotetrasiloxane, and silanes, including but not limited to methyltrimethoxysilane, dimethyldimethoxysilane, vinyltrimethoxysilane, methyltriethoxysilane, vinyltriethoxysilane, chlorotrimethylsilane, dichlorodimethylsilane, and trichloromethylsilane. In one embodiment, the treating agent may be selected from silanol-terminated vinylmethyl (ViMe) siloxanes, hexaorganodisiloxanes, such as hexamethyldisiloxane, and divinyltetramethyldisiloxane. Silanes may be selected from, but are not limited to, hexaorganodisilazanes such as hexamethyldisilazane (HMDZ), divinyltetramethyldisilazane; and hydroxyldimethyl terminated polydimethylmethylvinylsiloxane, octamethylcyclotetrasiloxane, and methyltriethoxysilane, dimethyldiethoxysilane, and / or vinyltriethoxysilane. A small amount of water may be added with the silica treating agent as a processing aid.

[0060] Any pigment / colorant The hydrosilylation-curable, heat-stabilized silicone rubber compositions described herein may further include one or more pigments and / or colorants that may be added if desired. The pigments and / or colorants may be colored, white, black, metallic effect, and luminescent, such as fluorescent and phosphorescent.

[0061] Suitable white pigments and / or colorants include titanium dioxide, zinc oxide, lead oxide, zinc sulfide, lithopone, zirconium oxide, and antimony oxide.

[0062] Suitable non-white inorganic pigments and / or colorants include, but are not limited to, iron oxide pigments such as goethite, lepidocrite, hematite, maghemite, and magnetite, black iron oxide, yellow iron oxide, brown iron oxide, and red iron oxide; blue iron pigments; chromium oxide pigments; cadmium pigments such as cadmium yellow, cadmium red, cadmium cinnabar; bismuth pigments such as bismuth vanadate and bismuth vanadate molybdate; mixed metal oxide pigments such as cobalt titanate green; chromate pigments and molybdate pigments such as chrome yellow, molybdate red, and molybdate orange; ultramarine pigments; cobalt oxide pigments; nickel antimony titanate; lead chromium; carbon black; lamp black, and metallic effect pigments such as aluminum, copper, copper oxide, bronze, stainless steel, nickel, zinc, and brass.

[0063] Suitable organic non-white pigments and / or colorants include phthalocyanine pigments such as phthalocyanine blue and phthalocyanine green; monoarylide yellow, diarylide yellow, benzimidazolone yellow, heterocyclic yellow, DAN orange, quinacridone pigments such as quinacridone magenta and quinacridone violet; organic reds including metallized azo reds and non-metallized azo reds and other azo pigments, monoazo pigments, diazo pigments, azo pigment lakes, β-naphthol pigments, naphthol AS pigments, benzimidazolone pigments, diazo condensed pigments, isoindolinone and isoindoline pigments, polycyclic pigments, perylene and perinone pigments, thioindigo pigments, anthrapyrimidone pigments, flavanthrone pigments, anthanthrone pigments, dioxazine pigments, triarylcarbonium pigments, quinophthalone pigments, and diketopyrrolopyrrole pigments.

[0064] Pigments and / or colorants, when present, are present in an amount ranging from 2% by weight of the composition, alternatively from 3% by weight, alternatively from 5% by weight to 15% by weight of the composition, alternatively to 10% by weight of the composition.

[0065] Further optional additives herein include pot-life extenders such as triazoles, which may be used but are not considered essential within the scope of the present invention, and thus the hydrosilylation-curable, heat-stabilized silicone rubber composition may not include a pot-life extender.

[0066] Examples of flame retardants include aluminum trihydrate, chlorinated paraffins, hexabromocyclododecane, triphenyl phosphate, dimethylmethylphosphonate, tris(2,3-dibromopropyl)phosphate (brominated tris), and mixtures or derivatives thereof.

[0067] Thus, in one alternative form, the present disclosure thus provides a hydrosilylation-curable, heat-stabilized silicone rubber composition, which comprises: a) an organopolysiloxane polymer having a maximum Williams plasticity of about 300 mm / 100 as measured according to ASTM D-926-08, at least 100 mm / 100 as measured according to ASTM D-926-08, alternatively at least 125 mm / 100 as measured according to ASTM D-926-08, alternatively at least 140 mm / 100 as measured according to ASTM D-926-08, and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups present in the composition in an amount of from 40% to about 90% by weight of the composition, alternatively from 45 to 85% by weight of the composition, alternatively from 50 to 80% by weight of the composition; b) a reinforcing silica filler, alternatively a fumed silica, colloidal silica and / or precipitated silica having a BET surface area (ISO 9277:2010) of at least 50 m2 / g, alternatively a surface area (ISO 9277:2010) of 50 to 450 m2 / g, alternatively a surface area (BET method according to ISO 9277:2010) of 50 to 300 m2 / g, typically used in an amount of up to 50% by weight of the composition, alternatively 1.0 to 50% by weight of the composition, alternatively 5.0 to 45% by weight of the composition, alternatively 10.0 to 40% by weight of the composition; c) a linear or branched organopolysiloxane filler treating agent comprising a plurality of units of the structure: -((R 10 )2SiO)- In the formula, each R 10 may be the same or different and are alkyl groups having 1 to 10 carbons, alternatively alkyl groups having 1 to 6 carbons, alternatively methyl, ethyl or propyl, alternatively an aromatic group having 6 to 12 carbons, alternatively phenyl, the number average degree of polymerization being in the range of 1 to 50, alternatively 1 to 25, and / or each end group contains at least one hydroxyl or alkoxy, in an amount of 0.1 to 20% by weight of the composition, alternatively 0.5 to 15% by weight of the composition, alternatively 1 to 10% by weight of the composition; d) component (b) an organosilicon compound having at least two, alternatively at least three Si-H groups per molecule, present in an amount of 0.1 to 10% by weight of the hydrosilylation curable, heat stabilized silicone rubber composition, alternatively 0.1 to 7.5% by weight of the hydrosilylation curable, heat stabilized silicone rubber composition, alternatively 0.5 to 7.5% by weight of the hydrosilylation curable, heat stabilized silicone rubber composition, and further alternatively 0.5% to 5% by weight; e) Dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide], 1,2-di[-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, a heat stabilizer additive selected from one or more of a metal or non-metal phthalocyanine complex, salicyloylaminotriazole, triazole, benzotriazole, dilauryl 3,3'-thiodipropionate, ditridecyl 3,3'-thiodipropionate, diphenyl sulfide, and / or pentaerythritol β-laurylthiopropionate, in an amount of 0.001 to 5% by weight of the composition, alternatively 0.01 to 5% by weight of the composition, alternatively 0.01 to 3% by weight of the composition; f) a hydrosilylation catalyst comprising or consisting of a platinum group metal or a compound thereof in an amount ranging from 0.001 to 3.0% by weight of the composition, alternatively from 0.001 to 2.5% by weight of the composition, or alternatively from 0.01 to 2.0% by weight of the hydrosilylation curable heat stabilized silicone rubber composition, depending on the form / concentration in which the catalyst is provided.

[0068] The total weight percent of any combination of ingredients in the above compositions is 100 weight percent.

[0069] The composition may also contain one or more of the optional additives listed above, again in the specified amounts, so long as the total weight percent of the composition is 100 weight percent.

[0070] The mixture of components (a), (d), and (f) above can begin to cure at ambient temperature. Thus, the hydrosilylation-curable heat-stabilized silicone rubber composition described above may be stored in two parts that are mixed together immediately prior to use if the composition is not prepared for immediate use. In such cases, the two parts are generally referred to as part (A) and part (B) and are designed to keep components (d) the crosslinker and (f) the catalyst apart to avoid premature curing.

[0071] Typically, in such cases, the Part A composition comprises components (a), (b), (c), and (f), and Part B comprises components (a), (d), (b), and (c) and, if present, an inhibitor.

[0072] If present in the composition, other optional additives may be present in either Part A or Part B, so long as they do not adversely affect the properties of any other components (e.g., catalyst deactivation). Parts A and B of the hydrosilylation-curable heat-stabilized silicone rubber composition are mixed together immediately prior to use to initiate the cure of the entire composition into a silicone elastomeric material. The composition can be designed to be mixed in any suitable weight ratio, for example, Part A:Part B may be mixed together in any suitable weight ratio. Typically, the Part A and Part B compositions are mixed together using a two-roll mill or kneading mixer.

[0073] However, if component (a) is a silicone rubber, then if the composition is to be used immediately, it may generally be prepared by combining all of the components together at ambient temperature into a one-part composition. Typically, the base is prepared first to allow the reinforcing silica filler to be treated in situ with component (c) and, if additionally present, any other additional treating agents, and then the remaining components may be introduced into the mixture in any suitable order.

[0074] For this purpose, any mixing technique and equipment described in the prior art can be used. The specific equipment used is determined by the viscosity of the components and the final curable coating composition. Suitable mixers include, but are not limited to, paddle-type mixers, such as planetary mixers, and kneader-type mixers. However, when component (a) is a rubber, mixing is preferably performed using a kneading mixer, as previously specified. It may be desirable to cool the components during mixing to avoid premature curing of the composition.

[0075] Also described herein is a process for the preparation of a hydrosilylation cured, heat stabilized silicone rubber, comprising: (i) preparing a silicone rubber base composition comprising components (a), (b) and (c) described above; (ii) mixing components (d), (e) and simultaneously or subsequently (f) into the silicone rubber base of step (i); (iii) curing the composition.

[0076] Step (i) may be accomplished by mixing components (a) and (b) together with treating agent (c) at a temperature in the range of 80° C. to 250° C., alternatively 100° C. to 220° C., alternatively 120° C. to 200° C., for a period of 30 minutes to 2 hours, alternatively 40 minutes to 2 hours, alternatively 45 minutes to 90 minutes, to ensure that the reinforcing silica filler is treated in situ with component (c) and thoroughly mixed into component (a). The resulting base may then be cooled to about room temperature (23° C. to 25° C.).

[0077] Components (d), (e) and simultaneously or sequentially component (f) the catalyst (catalyst composition, e.g., Karstedt's catalyst), as well as optional inhibitors (e.g., ethynylcyclohexanol (ETCH)) and any other optional additives are then added in any suitable order or simultaneously and mixed until homogeneous.

[0078] Once prepared, the composition cures due to the reactivity of components (a), (d), and (f). Typically, curing is carried out at a temperature of 80°C to 180°C, alternatively 100°C to 170°C, alternatively 120°C to 170°C. This can be done in any suitable manner, such as by introducing the composition into a mold and then press curing for a suitable time, such as 2 to 10 minutes, or otherwise as desired or required. Alternatively, the hydrosilylation-curable, heat-stabilized silicone rubber composition of the present invention may be further processed by injection molding, encapsulation molding, press molding, dispenser molding, extrusion molding, transfer molding, press vulcanization, centrifugal casting, calendar molding, bead application, or blow molding. If desired and if necessary, the sample may be further post-cured by heating to a temperature of 130°C to 200°C for up to 4 hours.

[0079] In the process for making a two-part hydrosilylation-curable heat-stabilized silicone rubber composition as described above, the process comprises: (i) the same step as step (i) for preparing the one-part composition described above; (ii) dividing the resulting mixture into two portions, part A and part B, and introducing the catalyst (f) into part A and the crosslinker and inhibitor (if any) into the part B composition; (iii) introducing any other optional additives into either or both of parts A and B; (iv) storing the part A composition and the part B composition separately.

[0080] Typically, when utilized, the Part A and Part B compositions are thoroughly mixed in an appropriate weight ratio as described above, for example, about 1:100, immediately prior to use to avoid premature curing. Curing is then carried out as described above for the one-part composition. The respective components of Part A and / or Part B may be mixed together individually, or may be combined and introduced into the composition in a pre-prepared state, for example to facilitate mixing of the final composition. For example, components (a) and (b) may be mixed together to form a base composition. In such a case, the treating agent of component (c) is typically introduced into the mixture so that the reinforcing silica filler (b) can be treated in situ. Alternatively, the reinforcing silica filler (b) may be pretreated with component (c), although this is not preferred. The resulting substrate may be split into two or more parts, typically Part A and Part B, and appropriate additional components and additives may be added, if necessary. Also provided herein is the use of additive e) as a heat stabilizer in a composition comprising components (a), (b), (c), (d) and (f) as described hereinabove. Surprisingly, it has been found that additive (e) seemingly has no significant heat stabilizing effect on liquid silicone rubber compositions utilizing organopolysiloxane polymers that are not considered to be rubbers, i.e., have a viscosity of less than 1,000,000 mPa.s at 25°C, typically much less (<<) than 1,000,000 mPa.s at 25°C, for example, from 1000 mPa.s at 25°C to 500,000 mPa.s at 25°C, or even from 1000 mPa.s at 25°C to 150,000 mPa.s at 25°C (viscosity is measured as specified in the Examples below). However, the compositions described herein above can improve elongation and tear after both short-term heat aging at 200° C. for 240 hours (h) and long-term heat aging at 180° C. for 3000 h to meet Class E requirements for, for example, ISO 6722 and LV216 standards, and can also pass winding tests after heat aging.This allows such compositions and the resulting cured silicone rubber materials to be used in the automotive and cable markets as heat resistant rubber materials, e.g., high heat resistant rubbers for electrical cables, e.g., outer sheaths in high voltage power cables for electric vehicles and high speed trains, turbocharger hoses, etc. In particular, they are suitable for use in EVs and HEVs, given the increasing operating voltage platforms of EVs and HEVs' battery modules and / or packs, which require high voltage cables.

[0081] Thus, as mentioned above, there is also provided herein an electric power cable, comprising: A conductive core; one or more insulating layers around said core; an outer sheath made from a heat stabilized silicone rubber that is the cured product of the above composition.

[0082] Also provided herein is a method for producing a power cable, comprising applying and curing an outer sheath around the cable, the outer sheath being a cured product of the composition described herein above. Application can be by any suitable method, for example, extrusion. The hydrosilylation curable heat stabilized silicone rubber composition can be used in a wide variety of applications, including, for example, automotive and electronics applications as an outer sheath for power cables, but also outer sheaths for power cables, conductor insulation, cables and outer sheaths for electric vehicles, automotive wire cables, industrial wire cables for underfloor heating systems, cables for trains and high speed trains, silicone rubber materials for high temperature resistant applications, automotive turbocharger hoses, and jackets for high temperature industrial equipment. EXAMPLES

[0083] All viscosities were measured at 25° C. unless otherwise indicated. Viscosities of individual components in the following examples were measured at a shear rate of 10 s using a TA instruments AR2000 Rheometer in a plate-plate model unless otherwise noted. -1The Williams plasticity results were prepared according to ASTM D-926-08. The following number average molecular weight (Mn) values ​​were determined using a Waters 2695 Separations Module equipped with a vacuum degasser and a Waters 2414 refractive index detector (Waters Corporation of MA, USA). Analysis was performed using certified grade toluene flowing at 1.0 mL / min as the eluent using polystyrene make-up standards. Data collection and analysis were performed using Waters Empower™ GPC software (Waters Corporation of MA, USA).

[0084] A series of base compositions were prepared, as shown in Table 1 below.

[0085] [Table 1]

[0086] Silicone Rubber 1 is a dimethylvinyl terminated polydimethylsiloxane having a vinyl content of 0.012% by weight, a Williams plasticity of about 155 mm / 100 and a Mn of 702,000. Silicone Rubber 2 is a dimethylvinyl terminated polydimethylmethylvinylsiloxane having a vinyl content of 0.725% by weight, a Williams plasticity of about 147 mm / 100 and a Mn of 700,000. Silicone Rubber 3 is a dimethylvinyl terminated polydimethylmethylvinylsiloxane having a vinyl content of 0.0654% by weight, a Williams plasticity of about 157 mm / 100 and a Mn of 702,000. Polymer 1 is a dimethylvinyl-terminated polydimethylsiloxane having a viscosity of 55,000 mPa·s at 25° C. and a vinyl content of 0.088 wt %. The fumed silica has a BET surface area of ​​270-330 m2 / g, tested according to DIN ISO9277 DIN 66132 (supplier details), and is commercially available from Wacker Chemie under the trade name HDK™ T30P. Hydrophobizing agent 1 is HO(Me2SiO) x H(x=1~18). Hydrophobizing agent 2 is HO(MePhSiO) x H(x=8~15). Hydrophobizing agent 3 is HO(Me2SiO) x (MeViSiO) y H(x+y=4~17).

[0087] The silicone rubber base compositions in Table 1 were prepared by mixing together silicone rubber or silicone polymer (used for comparison in Base 6), fumed silica and treating agents in a kneading mixer, then heating the base to a target temperature of 170° C., followed by stripping for about 120 minutes. The resulting base mixture was then cooled to room temperature. The fumed silica was hydrophobically treated in situ during the base heating and stripping process using a specific hydrophobizing treating agent.

[0088] Next, 100 parts by weight of the relevant base in Table 1 was taken, and the necessary amounts of the components other than the catalyst according to the compositions shown in Tables 2a to 2d were introduced into the base using a kneading mixer to prepare a silicone rubber composition. The resulting mixture was then mixed with the indicated amount of catalyst using a two-roll mill. The base and additives were mixed homogeneously in the kneading mixer using cooling water.

[0089] [Table 2]

[0090] Heat stabilizer 1 is dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide]. The acid scavenger was a masterbatch of 34 wt % magnesium oxide in silicone polymer. DCBP 50% is a masterbatch containing 50% by weight bis-(2,4-dichlorobenzoyl) peroxide in a silicone polymer.

[0091] [Table 3]

[0092] The crosslinker used throughout was trimethylsilyl-terminated dimethylmethylhydrogensiloxane having a viscosity of 5 mPa.s at 25°C. The catalyst used in all hydrosilylation cure cases was Karstedt's catalyst (5,000 ppm Pt) in a polydimethylsiloxane polymer. ETCH is ethynylcyclohexanol.

[0093] [Table 4]

[0094] The heat stabilizer (HS)2 was 1,2-di[-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine. Heat stabilizer (HS) 3 was 40 wt % copper (II) phthalocyanine in dimethylvinyl terminated polydimethylsiloxane having a viscosity of 9000 mPa.s at 25°C. Heat stabilizer (HS) 4 was salicyloylaminotriazole. Heat stabilizer (HS) 5 was pentaerythritol β-lauryl thiopropionate. Polymer 2 was a dimethylvinyl terminated polydimethylmethylvinylsiloxane having a viscosity of 350 mPa.s at 25°C. X-Linker 2 was a trimethyl terminated dimethyl, methylhydrogensiloxane with a viscosity of 50 mPa.s at 25°C.

[0095] [Table 5]

[0096] The resulting compositions were then molded into 2 mm sheets using a compression mold, after which the resulting compositions were cured at 120° C. for 10 minutes. No post-cure was utilized. The samples were then tested for their physical properties, while the other resulting cured sheets were subsequently aged at the required temperature for the required time. With regard to the physical property tests, they are as follows: Shore A hardness was measured according to ASTM D2240. Tensile strength, elongation at break and modulus at 100% elongation were measured according to ASTM D412. Specific gravity was measured according to ASTM D792. Tear strength was measured using Die B according to ASTM D624. Tear was measured using Die C and Nick according to ASTM D624.

[0097] [Table 6] Modulus of elasticity@100% = modulus of elasticity at 100% elongation.

[0098] [Table 7] Modulus of elasticity@100% = modulus of elasticity at 100% elongation.

[0099] It can be seen that dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide], Heat Stabilizer 1, does not provide heat stability to the peroxide cured examples of Table 3a.

[0100] [Table 8]

[0101] [Table 9]

[0102] Similar to Table 3a, the results in Table 3b show that in the absence of dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide] (Heat Stabilizer 1), there is a clear lack of heat stability in the cured product after 240 hours of heat aging at 200° C. C12, C13 and C14 clearly show that additives HS1 and HS3 do not positively affect heat stability for the Polymer 1 (Base 6) composition, i.e., a polymer with a much lower viscosity than the silicone rubber according to the present description. This was considered surprising.

[0103] [Table 10]

[0104] [Table 11]

[0105] The results in Table 3c show that the presence of dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide] (heat stabilizer 1) in the composition resulted in a significant improvement in thermal stability, especially with respect to elongation and tear strength, after aging at 200° C. for 240 hours.

[0106] [Table 12]

[0107] [Table 13]

[0108] The results shown in Table 3d(i) and (ii) show that 1,2-di[-(3,5-di-tert-butyl-4-hydroxy-phenyl)propionyl]hydrazine (Heat Stabilizer 2), 40 wt % copper (II) phthalocyanine in a dimethylvinyl terminated polydimethylsiloxane having a viscosity of 9000 mPa.s at 25°C (Heat Stabilizer 3), salicyloylaminotriazole (Heat Stabilizer 4) and pentaerythritol β-laurylthiopropionate (Heat Stabilizer 5) improve the heat stability in hydrosilylation cured systems by improving the elongation and tear strength after aging at 200°C for 240 hours.

[0109] [Table 14]

[0110] [Table 15]

[0111] [Table 16]

[0112] [Table 17]

[0113] [Table 18]

[0114] [Table 19]

[0115] After comparing the results in Table 4a with those of the metal oxide in dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide] formulation, it can be seen that Heat Stabilizer 1 also works in platinum cure systems to improve elongation and tear strength after short term heat aging at 200°C for 240 hours, and long term aging at 180°C for 1000, 2000 and 3000 hours.

Claims

1. 1. A hydrosilylation curable, heat stabilized silicone rubber composition comprising the following components: a) an organopolysiloxane polymer having a Williams plasticity of at least 100 mm / 100 as measured in accordance with ASTM D-926-08 and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups; b) a reinforcing silica filler; and c) a linear or branched organopolysiloxane filler treating agent comprising a plurality of units of the structure: -((R 10 ) 2 SiO)- In the formula, each R 10 a filler treating agent, which may be the same or different and are alkyl groups having 1 to 10 carbons, alternatively alkyl groups having 1 to 6 carbons, or aromatic groups having 6 to 12 carbons, the number average degree of polymerization being in the range of 1 to 50, and each end group containing at least one hydroxyl or alkoxy; d) an organosilicon compound having at least two, or alternatively at least three, Si—H groups per molecule; e) Dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide], 1,2-di[-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, a heat stabilizer additive selected from one or more of metal or non-metal phthalocyanine complexes, salicyloylaminotriazole, triazole, benzotriazole, dilauryl 3,3′-thiodipropionate, ditridecyl 3,3′-thiodipropionate, diphenyl sulfide, and / or pentaerythritol β-lauryl thiopropionate; f) a hydrosilylation catalyst comprising or consisting of a platinum group metal or a compound thereof.

2. 10. The hydrosilylation-curable, heat-stabilized silicone rubber composition of claim 1, also including a cure inhibitor.

3. 3. The hydrosilylation-curable, heat stabilized silicone rubber composition of claim 1, wherein component (c), said linear or branched organopolysiloxane filler treating agent, forms 0.1 to 10 weight percent of said composition.

4. The hydrosilylation-curable, heat-stabilized silicone rubber composition of any one of claims 1 to 3, wherein the heat stabilizer additive, component (e), comprises 0.001 to 5.0 weight percent of the composition.

5. The hydrosilylation-curable, heat-stabilized silicone rubber composition of any one of claims 1 to 4, wherein the composition comprises one or more optional additives selected from a compression set additive, an additional hydrophobic treatment other than component (c), a pigment and / or colorant, a pot life extender, a flame retardant, a mold release agent, a UV light stabilizer, a fungicide, and mixtures thereof.

6. The hydrosilylation-curable, heat-stabilized silicone rubber composition of any one of claims 1 to 5, wherein said organopolysiloxane polymer of component (a) has a Williams plasticity of at least 125 mm / 100 measured according to ASTM D-926-08.

7. A silicone-based product cured from the hydrosilylation-curable, heat-stabilized silicone rubber composition of any one of claims 1 to 6.

8. 8. A silicone-based product cured from the hydrosilylation-curable, heat-stabilized silicone rubber composition of claim 7, which passes Class E for ISO 6722 and LV216 standards.

9. 1. The process described herein for the preparation of a hydrosilylation cured, heat stabilized silicone rubber, comprising: (i) preparing a silicone rubber base composition, said composition comprising: a) an organopolysiloxane polymer having a Williams plasticity of at least 100 mm / 100 as measured in accordance with ASTM D-926-08 and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups; b) a reinforcing silica filler; and c) a linear or branched organopolysiloxane filler treating agent comprising a plurality of units of the structure: -((R 10 ) 2 SiO)- In the formula, each R 10 may be the same or different and are alkyl groups having 1 to 10 carbons, alternatively alkyl groups having 1 to 6 carbons, or aromatic groups having 6 to 12 carbons, the number average degree of polymerization being in the range of 1 to 50, and each end group containing at least one hydroxyl or alkoxy; (ii) adding to the silicone rubber base of step (i), d) an organosilicon compound having at least two, or alternatively at least three, Si—H groups per molecule; e) Dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide], 1,2-di[-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, simultaneously or sequentially with a heat stabilizer additive selected from one or more of metal or non-metal phthalocyanine complexes, salicyloylaminotriazole, triazole, benzotriazole, dilauryl 3,3′-thiodipropionate, ditridecyl 3,3′-thiodipropionate, diphenyl sulfide, and / or pentaerythritol β-lauryl thiopropionate; f) mixing with a hydrosilylation catalyst comprising or consisting of a platinum group metal or a compound thereof; (iii) curing the composition.

10. A silicone-based product obtained or obtainable by the process according to claim 9.

11. 2. Use of an additive e) selected from one or more of dodecanedioic acid, bis[2-(2-hydroxybenzoyl)hydrazide], 1,2-di[-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, metal or non-metal phthalocyanine complexes, salicyloylaminotriazole, triazole, benzotriazole, dilauryl 3,3′-thiodipropionate, ditridecyl 3,3′-thiodipropionate, diphenyl sulfide and / or pentaerythritol β-laurylthiopropionate as a heat stabilizer in or as said heat stabilizer in a composition, said composition further comprising the following components: a) an organopolysiloxane polymer having a Williams plasticity of at least 100 mm / 100 as measured in accordance with ASTM D-926-08 and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups; b) a reinforcing silica filler; and c) a linear or branched organopolysiloxane filler treating agent comprising a plurality of units of the structure: -((R 10 ) 2 SiO)- In the formula, each R 10 a filler treating agent, which may be the same or different and are alkyl groups having 1 to 10 carbons, alternatively alkyl groups having 1 to 6 carbons, or aromatic groups having 6 to 12 carbons, the number average degree of polymerization being in the range of 1 to 50, and each end group containing at least one hydroxyl or alkoxy; d) Organosilicon compounds having at least two, or at least three, Si-H groups per molecule. and, f) a hydrosilylation catalyst comprising or consisting of a platinum group metal or a compound thereof.

12. 1. A power cable, comprising: A conductive core; one or more insulating layers around said core; an outer sheath made from said heat stabilized silicone rubber which is the cured product of the composition according to any one of claims 1 to 6.

13. Use of the heat-stabilized silicone rubber, which is the cured product of claim 7, as an outer sheath for a power cable.

14. 7. A method for producing an electric power cable, comprising the steps of applying and curing an outer sheath about said cable, said outer sheath being a cured product of the hydrosilylation-curable, heat-stabilized silicone rubber composition according to any one of claims 1 to 6.

15. Use of the hydrosilylation-curable, heat-stabilized silicone rubber composition according to any one of claims 1 to 6 in the manufacture of automotive and electronic applications.

16. The use according to claim 15, wherein the automotive and electronics applications can be selected from: outer sheath for power cables, conductor insulation, cables and outer sheath for electric vehicles, automotive wire cables, industrial wire cables for underfloor heating systems, train and high speed train cables, silicone rubber materials for high temperature resistant applications, automotive turbocharger hoses and jackets for high temperature industrial equipment.

Citation Information

Patent Citations

  • Silicone rubber composition

    JP1995292255A

  • Silicone rubber composition and silicone rubber

    JP2019143047A

  • Adhesive silicone resin composition and adhesive film coated with the same

    JP2021123628A

  • Silicone pressure-sensitive adhesive composition, silicone pressure-sensitive adhesive, pressure-sensitive adhesive film, image display device, and method for evaluating silicone pressure-sensitive adhesive

    JP2023155125A

  • Thermoplastic silicone elastomers formed from nylon resins

    US20020086937A1