High-strength steel with high yield ratio and excellent impact resistance after cold forming and its manufacturing method
A high-strength steel with controlled alloy composition and cooling rates addresses the durability and impact resistance issues in thick materials, achieving uniform microstructures and improved performance for commercial vehicle components.
Patent Information
- Application Number
- JP2024527810
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-17
- Filing Date
- 2022-11-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-09
AI Technical Summary
Conventional high-strength steels face challenges in maintaining durability and impact resistance during spinning and flow forming processes, particularly for thick materials, due to non-uniform microstructures and the formation of coarse carbides and pearlite, which lead to cracks and reduced yield strength.
A high-strength steel composition with specific alloy elements (C, Si, Mn, Al, Cr, P, S, N, Ti, Nb) and controlled cooling rates to achieve a microstructure of equiaxed ferrite, bainitic ferrite, and controlled MA phases, ensuring uniformity and suppressing coarse carbides and pearlite formation.
The solution results in a steel with excellent impact resistance and high yield ratio, suitable for commercial vehicle components, with tensile strength of 590 MPa or more, fracture elongation of 25% or more, and impact toughness of 70 J or more at -20°C, minimizing cracks and ensuring consistent performance.
Smart Images

Figure 2024543074000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a high strength steel and a manufacturing method thereof, and more particularly to a high strength steel having excellent impact resistance after cold forming and a high yield ratio, and a manufacturing method thereof. [Background technology]
[0002] Conventionally, steel materials with a thickness of 8 mm or more are mainly used for chassis parts of commercial vehicles due to the characteristics of the vehicle, and high-strength hot-rolled steel sheets with a tensile strength of 600 MPa or more are used for members, and hot-rolled steel sheets with a tensile strength of 440 MPa or more are used for wheel discs. However, in order to reduce weight recently, there is a tendency to use high-strength steel sheets with a tensile strength of 700 MPa or more for members and 590 MPa or more for wheel discs, to reduce the thickness of the steel sheets, and to change the design of the parts. In addition, wheels were traditionally manufactured by a press forming process, but recently they tend to be manufactured by spinning and flow forming. Since such a forming process gives a large amount of deformation to the hot-rolled steel sheets, hot-rolled steel sheets with a better elongation are required, and the formed parts are required to ensure durability and impact resistance during use.
[0003] However, when conventional high-strength steels are applied to the above-mentioned spinning and flow forming processes, the durability of the parts must be equal to or greater than that of conventional steels. However, there are difficulties in applying such steels, such as the occurrence of fine cracks on shear surfaces during forming of the parts and poor durability in areas with a large amount of forming.
[0004] Conventional high-strength steel, as in Patent Documents 1 and 2, is hot-rolled in the normal austenite region, then coiled at a high temperature to form ferrite as a matrix structure and fine precipitates are formed, and as in Patent Document 3, a technique is applied in which the coiling temperature is cooled to a temperature at which a bainite matrix structure is formed and then coiled in order to prevent the formation of coarse pearlite. In addition, as in Patent Document 4, a technique is proposed in which austenite grains are refined by reducing the roll ratio by 40% or more in the non-recrystallized region during hot rolling using Ti, Nb, etc. Recently, as in Patent Document 5, a technique has been proposed to improve the uniformity of the microstructure between the surface layer and the deep layer of the steel plate and suppress the formation of coarse carbides, and as in Patent Document 6, a technique has been proposed to simultaneously suppress the formation of pearlite, MA phase (Martensite and Austenite), and martensite, which have a negative effect on durability.
[0005] However, Patent Documents 1 to 4 do not take into consideration the occurrence of cracks on the shear surface and its periphery during shear forming of high-strength thick material, and are configured with cooling rate conditions and large rolling conditions that are difficult to ensure during manufacturing of thick materials with a thickness of 8 mm or more. When using precipitate-forming elements such as Ti, Nb, and V to refine the crystal grains of the thick material and ensure strength at the same time, there is a problem that ferrite grows excessively when coiled at a high temperature of 500 to 700 ° C, at which precipitates are likely to form, resulting in a decrease in yield strength and the formation of coarse pearlite. In addition, even when manufacturing at a low coiling temperature to utilize the bainite matrix structure, if the cooling rate in the width direction of the steel sheet during cooling after hot rolling is not uniformly controlled, a non-uniform fine structure is formed in the hot-rolled steel sheet, making it difficult to have a high elongation rate and making it difficult to ensure stable high yield ratio characteristics, and the sensitivity to forming cracks such as cracks on the shear surface during forming also increases. Furthermore, since this technology is intended for hot-rolled steel sheets with a thickness of less than 5 mm used for passenger cars, the required cooling rate is too high and is not suitable for manufacturing thick materials. In addition, applying a large reduction of 40% in the unrecrystallized region can deteriorate the shape quality of the rolled sheet and place a load on the equipment, making it difficult to apply to thick materials with a thickness of 8 mm or more. Patent Documents 5 and 6 are inventions intended for thick materials. First, Patent Document 5 proposes a manufacturing technology in which the crystal grain shape in the deep layer part (1 / 4t to 1 / 2t) of the thickness is equiaxed and has fine crystal grains in order to improve the durability of thick high-strength steel, and the formation of MA phase and martensite is suppressed. Patent Document 6 proposes a technology in which a hot-rolled coil is divided into three equal parts in the length direction through a relational expression derived for a specific component, and the head, mid, and tail parts are cooled to different cooling end temperatures at a constant cooling rate condition, and then coiled to manufacture the steel. This technology is a technology that manufactures a uniform microstructure by controlling the cooling rate after hot rolling through a relational equation derived for specific components in consideration of the quality of the shear surface of the part. Although it is effective in improving the durability of commercial vehicle wheels that contain many punching holes and are constantly subjected to load, it does not take into consideration the impact resistance after forming.In addition, it is difficult to uniformly control the cooling of the steel sheet after hot rolling over the entire width, and when the hot-rolled steel sheet is thick, such as having a thickness of 8 mm or more, it is difficult to control the cooling rate at an actual rate.
[0006] The cooling process after hot rolling is usually performed within several tens of seconds from a 100-120m long ROT (Run-Out Table), but it is difficult to manufacture the hot rolled steel sheet by cooling it to the cooling end temperature or coiling temperature while satisfying the proposed range of cooling rate for the deep part of the thickness. Therefore, in the above-mentioned conventional technology, the hot rolled steel sheet having a thickness of 8mm or more has a problem that it is difficult to obtain the effect of suppressing the formation of coarse carbides, and is insufficient to ensure a high level of impact resistance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Korean Patent Publication No. 10-2010-0029138 (Published on March 15, 2010) [Patent Document 2] Japanese Patent Publication No. 2007-262487 (published on October 11, 2007) [Patent Document 3] Korean Patent Publication No. 10-1528084 (Published on June 10, 2015) [Patent Document 4] Japan Patent Publication No. 9-143570 (published on June 3, 1997) [Patent Document 5] Korean Patent Publication No. 10-2020-0062422 (Published on June 4, 2020) [Patent Document 6] Korean Patent Publication No. 10-2021-0068808 (Published on June 10, 2021) Summary of the Invention [Problem to be solved by the invention]
[0008] An object of one aspect of the present invention is to provide a high-strength steel having excellent impact resistance and a high yield ratio after cold forming, and a manufacturing method thereof.
[0009] The object of the present invention is not limited to the above-mentioned contents, and a person skilled in the art will have no difficulty in understanding further object of the present invention from the entire contents of this specification. [Means for solving the problem]
[0010] One aspect of the present invention is a steel sheet comprising, by weight percent, 0.05-0.15% C, 0.01-0.5% Si, 1.0-2.0% Mn, 0.01-0.1% Al, 0.001-1.0% Cr, 0.001-0.05% P, 0.001-0.01% S, 0.001-0.01% N, 0.001-0.01% Ti, 0.03-0.08% Nb, and the balance being Fe and other unavoidable impurities, with the sum of Nb and Ti being 0.04-0.1%; The microstructure of the surface layer within a thickness range of 50 μm from the surface contains, in terms of area%, 95% or more of equiaxed ferrite and 3% or less of pearlite, and contains a total of 5% or less of one or more of bainitic ferrite, bainite, MA (Martensite-Austenite constituent) phase, and martensite; It is possible to provide a steel sheet in which the microstructure in the center part in the range of 1 / 4 to 3 / 4 of the thickness contains, in area percentage, 80 to 95% bainitic ferrite, 10% or less bainite, 3% or less pearlite, 5 to 10% in total of one or two of the MA (Martensite-Austenite constituent) phase and martensite, and the remainder contains equiaxed ferrite.
[0011] The steel plate may have a thickness of 8 to 25 mm.
[0012] The steel plate may have a tensile strength of 590 MPa or more, a breaking elongation of 25% or more, a yield ratio of 0.75 to 0.9, and an impact toughness of 70 J or more at -20°C after cold forming.
[0013] The steel plate may have a ratio (E / YS) of impact toughness (E) at -20°C after cold forming to yield strength (YS) before cold forming of 0.15 or more.
[0014] The steel plate includes edge portions corresponding to 30% of both ends in the width direction and a central portion of a central 40% region corresponding to the region excluding both edge portions, and the edge portions and central portion may have a difference in tensile strength of 10 MPa or less, a difference in fracture elongation of 8% or less, and a difference in impact toughness at -20°C after cold forming of 20 J or less.
[0015] Another aspect of the present invention is a method for producing a steel slab having a total content of Nb and Ti of 0.04-0.1%, comprising the steps of: reheating a steel slab containing, by weight percent, 0.05-0.15% C, 0.01-0.5% Si, 1.0-2.0% Mn, 0.01-0.1% Al, 0.001-1.0% Cr, 0.001-0.05% P, 0.001-0.01% S, 0.001-0.01% N, 0.001-0.01% Ti, 0.03-0.08% Nb, the balance being Fe and other unavoidable impurities; hot rolling the reheated steel slab; and The hot-rolled steel sheet is cooled to a temperature range of 500 to 650° C. at an average cooling rate within a range of 1 to 30° C. / s, the average cooling rate being equal to or greater than the CR value defined by the following Relation 1, and then coiled. In the cooling and winding step, the edge portions corresponding to 30% of the area at both ends in the coil width direction are cooled at a temperature of 550 to 650 ° C. (TE), and the center portion of the central 40% area corresponding to the area excluding both edges in the width direction is cooled at a temperature of 500 to 550 ° C. (TC). A method for manufacturing a steel sheet in which the average temperature difference between the edge portion and the center portion is 50 to 150°C can be provided. [Equation 1] CR=45-16.3×[C]-5.6×[Si]-16.3×[Mn]-2.9×[Cr]+15×[Ti]+23×[Nb]-0.9×(t-8) (Here, [C], [Si], [Mn], [Cr], [Ti] and [Nb] are the weight percentages of each element, and t is the thickness of the steel plate (mm).)
[0016] The reheating temperature is 1100 to 1350 ° C. The hot rolling temperature may be 800 to 1150°C.
[0017] The method may further include air-cooling the wound coil at a temperature range of 200° C. or less.
[0018] The steel plate may have a thickness of 8 to 25 mm. Effect of the Invention
[0019] According to one aspect of the present invention, it is possible to provide a high-strength steel having excellent impact resistance after cold forming and a high yield ratio, and a manufacturing method thereof.
[0020] According to one aspect of the present invention, it is possible to provide a high strength steel that can be applied to steel materials used for chassis members and wheels of medium and large commercial vehicles, and a method for manufacturing the same. [Brief description of the drawings]
[0021] [Figure 1] 1 is a photograph showing the microstructure of Example 2 according to an embodiment of the present invention, observed with a scanning electron microscope (×3,000). [Diagram 2] 1 is a photograph showing the microstructure of Comparative Example 2 according to an embodiment of the present invention, observed with a scanning electron microscope (×3,000). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, preferred embodiments of the present invention will be described. The embodiments of the present invention can be modified in various ways, and the scope of the present invention should not be construed as being limited to the embodiments described below. The present embodiments are provided to further explain the present invention in detail to those skilled in the art to which the present invention pertains.
[0023] In order to solve the above-mentioned problems and ensure excellent formability and impact resistance, the present inventors have studied the change in impact resistance after cold forming depending on the microstructural characteristics of the steel sheet, and have confirmed that the desired physical properties can be secured by optimizing the alloy composition and manufacturing conditions to control the microstructural characteristics according to the thickness and width directions of the steel sheet, thereby completing the present invention.
[0024] In hot-rolled steel sheets generally manufactured in the form of coils, coarse carbides and pearlite are likely to form when the steel sheet is maintained at a high temperature of about 500 to 700 ° C for a long time. In particular, when the ferrite phase transformation that starts during the cooling process after the completion of hot rolling proceeds slowly, the untransformed phase has a high carbon content, which makes it easy for coarse carbides and pearlite to form. Furthermore, the central part of the coil width has a slower cooling rate than the edge part, so that such a structure develops further. Therefore, in order to suppress the formation of such coarse carbides and pearlite in the central part of the coil width, it is necessary to cool the wound coil to room temperature by forced cooling such as water cooling. In this case, however, the edge part, which has a fast cooling rate, is not preferable because martensite or MA (Martensite and Austenite) phase is excessively formed, the microstructure becomes non-uniform, it becomes difficult to secure a high elongation, and cracks on the shear surface increase. Therefore, the present invention proposes a method for suppressing the formation of coarse carbides and pearlite without forced cooling of the coil.
[0025] The present invention will be described in detail below.
[0026] The steel composition of the present invention will be described in detail below.
[0027] In the present invention, unless otherwise specified, % representing the content of each element is based on weight.
[0028] A steel according to one aspect of the present invention contains, by weight, 0.05-0.15% C, 0.01-0.5% Si, 1.0-2.0% Mn, 0.01-0.1% Al, 0.001-1.0% Cr, 0.001-0.05% P, 0.001-0.01% S, 0.001-0.01% N, 0.001-0.01% Ti, 0.03-0.08% Nb, 0.01-0.05% Nb, the balance being Fe and other unavoidable impurities, and the sum of Ti and Nb can be 0.04-0.1%.
[0029] Carbon (C): 0.05~0.15% Carbon (C) is the most economical and effective element for strengthening steel, and when the amount of carbon added is increased, the precipitation strengthening effect or the bainite phase fraction increases, making it easier to ensure strength. However, when the thickness of a hot-rolled steel sheet is increased, the cooling rate at the center of the thickness during cooling after hot rolling slows down, and when the carbon (C) content is high, coarse carbides and pearlite are likely to form. Therefore, if the carbon (C) content is less than 0.05%, it is difficult to obtain a sufficient strengthening effect, and if the carbon (C) content exceeds 0.15%, there is a problem that impact resistance is reduced due to the formation of pearlite and coarse carbides at the center of the thickness, and weldability may also be deteriorated. The preferable lower limit may be 0.055%, and the more preferable upper limit may be 0.12%.
[0030] Silicon (Si): 0.01 to 0.5% Silicon (Si) is an element that is effective in deoxidizing molten steel and solid-solution strengthening steel, and is also effective in improving formability by delaying the formation of coarse carbides. However, if its content is less than 0.01%, the effect of solid-solution strengthening and delaying the formation of carbides cannot be maximized, and if its content exceeds 0.5%, there are problems in that red scale is formed on the surface of the steel sheet during hot rolling, resulting in very poor quality, as well as reduced ductility and weldability. It may be preferably contained at 0.05% or more, and more preferably at 0.3% or less.
[0031] Manganese (Mn): 1.0-2.0% Manganese (Mn), like Si, is an effective element for solid solution strengthening of steel, and can increase the hardening ability of steel to facilitate the formation of bainite during cooling after hot rolling. However, if the content is less than 1.0%, the above effect of addition cannot be obtained, and if the content exceeds 2.0%, the hardening ability increases significantly, making martensite phase transformation more likely to occur, and there is a risk of segregation developing significantly from the thickness center during slab casting in the continuous casting process. It is preferable to contain 1.3% or more, and more preferably 1.8% or less.
[0032] Aluminum (Al): 0.01 to 0.1% Aluminum (Al) is a component added mainly for deoxidation, and if its content is less than 0.01%, its effect may be insufficient. On the other hand, if its content exceeds 0.1%, it combines with nitrogen to form AlN, which is likely to cause corner cracks in the slab during continuous casting and defects due to inclusion formation. It is preferably contained at 0.015% or more, more preferably 0.06% or less.
[0033] Chromium (Cr): 0.001-1.0% Chromium (Cr) strengthens the steel through solid solution, similar to Mn, and plays a role in delaying the ferrite phase transformation during cooling and aiding in the formation of bainite. However, if the content is less than 0.001%, the above effects of addition cannot be obtained, and if the content exceeds 1.0%, the ferrite phase transformation is excessively delayed, and the elongation rate may deteriorate due to excessive martensite formation. In addition, excessive Cr addition causes large segregation in the center of the thickness, making the microstructure in the thickness direction non-uniform and degrading the impact resistance. The preferable lower limit may be 0.01%, and the more preferable upper limit may be 0.5%.
[0034] Phosphorus (P): 0.001 to 0.05% Phosphorus (P) has the effect of strengthening solid solution and promoting ferrite phase transformation, similar to Si. However, in order to manufacture a steel with a phosphorus (P) content of less than 0.001%, the manufacturing cost is high, which is economically disadvantageous, and the strength is insufficient. On the other hand, if the content exceeds 0.05%, embrittlement occurs due to grain boundary segregation, and fine cracks are easily generated during molding, which can greatly deteriorate the impact resistance.
[0035] Sulfur (S): 0.001-0.01% The above-mentioned S is an impurity present in steel, and if its content exceeds 0.01%, it combines with Mn and the like to form nonmetallic inclusions, which can cause fine cracks during forming and greatly reduce impact resistance. However, in order to manufacture steel with a content of less than 0.001%, it takes a long time during steelmaking operations, resulting in poor productivity.
[0036] Nitrogen (N): 0.001-0.01% Nitrogen (N), along with C, is a representative solid solution strengthening element, and forms coarse precipitates along with Ti, Al, etc. In general, the solid solution strengthening effect of nitrogen (N) is superior to that of C, but there is a problem in that the toughness decreases significantly as the amount of nitrogen (N) in steel increases. Therefore, the upper limit of the nitrogen content can be limited to 0.01%. On the other hand, in order to manufacture steel with a content of less than 0.001%, it takes a long time during steelmaking operations, resulting in poor productivity.
[0037] Titanium (Ti): 0.03-0.08% Titanium (Ti) is a representative precipitation strengthening element, and forms coarse TiN in steel due to its strong affinity with N. TiN has the effect of suppressing the growth of crystal grains during the heating process for hot rolling. In addition, titanium (Ti) remaining after reacting with N dissolves in steel and bonds with C to form TiC precipitates, which are useful components for improving the strength of steel. If the titanium (Ti) content is less than 0.03%, the above effect cannot be obtained, and if the content exceeds 0.08%, there is a problem that the generation of coarse TiN and the coarsening of precipitates deteriorates the impact resistance characteristics during forming. It can be preferably contained at 0.04% or more, and more preferably contained at 0.075% or less.
[0038] Niobium (Nb): 0.01-0.05% Niobium (Nb) is a representative precipitation strengthening element along with Ti, and is effective in improving the strength and impact toughness of steel by precipitating during hot rolling and refining the crystal grains by delaying recrystallization. If the niobium (Nb) content is less than 0.01%, the above effect cannot be obtained, and if the content exceeds 0.05%, there is a problem that the formability is deteriorated due to the formation of elongated crystal grains and the formation of coarse complex precipitates due to excessive delay in recrystallization during hot rolling. The preferable lower limit may be 0.015%, and the more preferable upper limit may be 0.04%.
[0039] The steel of the present invention may contain the remaining iron (Fe) and inevitable impurities in addition to the above-mentioned composition. The inevitable impurities cannot be excluded because they may be unintentionally mixed in during normal manufacturing processes. Since such impurities are known to anyone skilled in the art of normal steel manufacturing, the contents of all of them will not be mentioned in this specification.
[0040] In the steel according to one aspect of the present invention, the total content of niobium (Nb) and titanium (Ti) can be 0.04 to 0.1%.
[0041] Niobium (Nb) and titanium (Ti) precipitate as (Ti, Nb)(C, N)-based composite precipitates, and when they precipitate during hot rolling, the effect of refining crystal grains due to delayed recrystallization increases significantly. However, if the formation of composite precipitates is excessive, there is a problem that the effect of improving strength is small and formability is deteriorated due to the increase in coarse composite precipitates. If the total of niobium (Nb) and titanium (Ti) is less than 0.04%, the effect of refining crystal grains and improving strength may be small. On the other hand, if the total exceeds 0.1%, the formability is deteriorated and it is economically disadvantageous. The preferable lower limit may be 0.045%, and the more preferable upper limit may be 0.09%.
[0042] In the following, the steel microstructure of the present invention will be described in detail.
[0043] Unless otherwise specified in the present invention, the percentages expressing the fraction of the microstructure are based on the area.
[0044] In one aspect of the steel of the present invention, the microstructure of the surface layer within a thickness range of 50 μm from the surface contains, in area %, 95% or more equiaxed ferrite, 3% or less pearlite, and a total of 5% or less of one or more of bainitic ferrite, bainite, MA (Martensite-Austenite constituent) phase, and martensite, while the microstructure of the center portion within a thickness range of 1 / 4 to 3 / 4 contains, in area %, 80 to 95% bainitic ferrite, 10% or less bainite, 3% or less pearlite, and a total of 5 to 10% of one or two of MA (Martensite-Austenite constituent) phase and martensite, with the remainder being equiaxed ferrite.
[0045] In the present invention, if the equiaxed ferrite is less than 95% in the surface layer, the ductility is insufficient during spinning and flow forming applied in manufacturing commercial vehicle wheels, and work hardening in the surface layer is intense, which may cause fine cracks to occur during forming. In particular, if 3% or more of highly brittle pearlite is formed or if one or more of bainitic ferrite, bainite, MA phase, and martensite, which have high hardness, are contained in an amount exceeding 5%, there is a problem that cracks easily propagate along the interface with the base phase. Therefore, in order to suppress the occurrence of fine cracks formed in the surface layer during forming and to prevent the propagation of cracks, it is preferable to contain one or more of bainitic ferrite, bainite, MA phase, and martensite in a total amount of 5% or less. In the present invention, the microstructure of the surface layer may be 100% equiaxed ferrite, and the total amount of pearlite, bainitic ferrite, bainite, MA phase, and martensite may be 0%.
[0046] In addition, if the bainitic ferrite is less than 80% in the center, there is a problem that cracks easily occur on the shear surface during punching and shear forming during wheel manufacturing, and there is a problem that impact resistance is also poor after forming. In addition, in the process of cooling the steel plate after hot rolling during manufacturing the steel plate, after the bainitic ferrite, which is the base structure, is formed in the center of the thickness of the rolled plate, a high concentration of residual C remains in the untransformed austenite, which makes it easy to form pearlite. In this case, if the pearlite is formed in an amount exceeding 3%, cracks are generated severely on the shear surface during the forming process, and impact resistance after forming is also poor. When the pearlite fraction is 3% or less, no cracks occur due to forming such as shearing, and impact resistance at low temperatures can be excellent. In the present invention, carbides and nitrides having a diameter of 1 μm or more can be included in pearlite.
[0047] In contrast, when the MA phase or martensite is contained at 5 to 10%, it can be advantageous to secure impact resistance and high strength after forming without affecting crack generation. The MA phase has an advantageous aspect of forming potential density around it to secure high strength, and when it is formed together with a matrix structure composed of ferrite and bainite, it can have excellent impact resistance even if the potential density increases after cold forming. However, when the MA phase or martensite is contained at less than 5%, the yield strength and tensile strength are insufficient, and when it is contained at more than 10%, there is a problem that the ductility is insufficient and the formability is poor. When bainite is contained at more than 10%, there is also a possibility that there is a problem of insufficient ductility.
[0048] In the present invention, the microstructure at the center can contain 0% bainite and 0% pearlite, and can unavoidably contain equiaxed ferrite in addition to bainitic ferrite, bainite, pearlite, MA phase, and martensite.
[0049] In the present invention, the area fraction of the microstructure can be analyzed using an optical microscope and a scanning electron microscope (SEM), and the area fraction of the phase can be measured from an image observed at a magnification of 3,000 at a position corresponding to the center of thickness of the rolled cross section.
[0050] The steel production method of the present invention will now be described in detail.
[0051] The steel according to one aspect of the present invention can be produced by reheating, rolling, cooling and coiling a steel slab satisfying the alloy composition described above.
[0052] reheating A steel slab satisfying the alloy composition of the present invention can be reheated in the temperature range of 1100 to 1350°C.
[0053] If the reheating temperature is less than 1100°C, the precipitates are not sufficiently redissolved, and the formation of precipitates may be reduced in the process after hot rolling, and coarse TiN may remain. On the other hand, if the temperature exceeds 1350°C, the strength may decrease due to abnormal grain growth of austenite crystal grains.
[0054] Hot rolling The reheated steel slab can be hot rolled in the temperature range of 800 to 1150°C.
[0055] If the hot rolling temperature exceeds 1150°C, the temperature of the hot rolled steel sheet becomes high, the grain size becomes coarse, and the surface quality of the hot rolled steel sheet may deteriorate. On the other hand, if the temperature is less than 800°C, elongated grains may develop due to delayed recrystallization, causing severe anisotropy and poor formability. If the rolling is performed at a temperature below the austenite temperature range, the non-uniform microstructure may develop even more severely.
[0056] Cooling and winding The hot-rolled steel sheet can be cooled to a temperature range of 500 to 650°C at an average cooling rate within a range of 1 to 30°C / s, which is equal to or greater than the CR value defined by the following Relation 1, and then coiled. During the cooling, 30% of the edge portions at both ends in the coil width direction can be cooled to a temperature (TE) of 550 to 650°C, and the central portion of the central 40% of the coil width direction excluding both edges can be cooled to a temperature (TC) of 500 to 550°C. At this time, the average temperature difference between the edge portions and the central portion can be 50 to 150°C.
[0057] In the present invention, Relational formula 1 was derived to induce an appropriate level of ferrite phase transformation during cooling of the steel sheet, form a fine and uniform MA phase, and suppress excessive pearlite formation. If the cooling rate is less than the CR value of Relational formula 1, ferrite in the center of the thickness becomes coarse and pearlite is excessively formed, causing severe cracking on the shear surface, which may deteriorate the impact resistance properties after forming. In addition, if the cooling rate exceeds 30°C / s, bainite, MA phase, and martensite are excessively formed, resulting in insufficient ductility and poor shear surface quality. [Equation 1] CR=45-16.3×[C]-5.6×[Si]-16.3×[Mn]-2.9×[Cr]+15×[Ti]+23×[Nb]-0.9×(t-8) (Here, [C], [Si], [Mn], [Cr], [Ti] and [Nb] are the weight percentages of each element, and t is the thickness of the steel plate (mm).)
[0058] In order to suppress the formation of excessive carbides and pearlite, the cooling temperature after hot rolling must be lower than the end of cooling temperature. However, there is a risk that it will be difficult to ensure the target elongation due to a reduction in ferrite caused by excessive bainite formation or excessive formation of the MA phase and martensite.
[0059] Therefore, in the present invention, in order to increase the cooling rate at the center of the coil in the width direction and reduce the time that the coil after winding is maintained at a high temperature, the cooling end temperature of the center and edge parts in the width direction during cooling after hot rolling can be set differently. However, in this case, the average temperature difference between the edge parts and the center can be 50 to 150°C. If the average temperature difference is less than 50°C, it may be difficult to obtain the above effect. On the other hand, if the temperature exceeds 150°C, the above effect does not increase any more, but it may be difficult to control the temperature of each section of the coil.
[0060] In the present invention, the method of controlling the cooling end temperature of the edge portion and the center portion during coiling is not particularly limited, but as an example, when cooling a hot-rolled steel sheet, a method can be applied in which cooling water injected into the edge portion is stopped before it reaches the steel sheet, or the amount of cooling water injected is adjusted to be different, or the two methods can be used in parallel.
[0061] In the present invention, in order to secure the desired strength, formability, and impact resistance, it is preferable to satisfy all of the conditions of the above Relational Formula 1 and the cooling end temperature. When all of the above cooling conditions are satisfied, the center in the thickness direction has a uniform and fine microstructure with bainitic ferrite as the matrix structure, and coarse carbides and pearlite are reduced in the inner winding part and thickness center of the coil where the cooling rate is slow, so that the non-uniform structure of the hot-rolled steel sheet can be eliminated. In addition, the non-uniform formation of MA phases and the formation of coarse martensite can be suppressed in the outer winding part and edge part of the coil where the cooling rate is relatively fast.
[0062] cooling The wound coil can be air cooled to a temperature range up to 200°C.
[0063] In the present invention, the wound coil can be air-cooled in a temperature range of 200°C or less. Air-cooling the coil means cooling in the air at room temperature at a cooling rate of 0.001 to 10°C / h. At this time, if the cooling rate exceeds 10°C / h, some untransformed phases in the steel at the outer winding part of the coil are likely to transform into MA phase, and the shear formability, punching formability, and durability of the steel may be deteriorated. On the other hand, in order to control the cooling rate to less than 0.001°C / h, separate heating and heat retention equipment are required, which may be economically disadvantageous. The preferable lower limit may be 0.01°C / h, and the more preferable upper limit may be 1°C / h.
[0064] The steel of the present invention thus manufactured has a thickness of 8 to 25 mm, a tensile strength of 590 MPa or more, a fracture elongation of 25% or more, a yield ratio of 0.75 to 0.9, an impact toughness at -20°C after cold forming of 70 J or more, and a ratio of the impact toughness after cold forming to the yield strength before cold forming of 0.15 or more, and thus has excellent properties of impact toughness while having a high yield ratio. The steel also includes edge portions corresponding to a 30% region at both ends based on the width direction, and a central portion of a central 40% region corresponding to the region excluding both edge portions, and the difference in tensile strength between the edge portions and the central portion may be 10 MPa or less, the difference in fracture elongation may be 8% or less, and the difference in impact toughness at -20°C after cold forming may be 20 J or less. EXAMPLES
[0065] The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention.
[0066] (Example) A hot-rolled steel sheet was manufactured from a steel slab having the alloy composition shown in Table 1 below under the conditions shown in Table 2 below. The steel slab was reheated at a temperature of 1100 to 1350°C and then hot-rolled. Table 2 shows the cooling rate applied during manufacturing and the CR value of Relation 1, and the cooling end temperatures are shown as the temperature (TC) in the 40% range at the center in the width direction and the temperature (TE) in the 30% range at each end in the width direction. The difference between the temperature at the center and the temperature at the edge is also shown.
[0067] [Table 1]
[0068] [Table 2] [Relational expression 1] CR=45-16.3×[C]-5.6×[Si]-16.3×[Mn]-2.9×[Cr]+15×[Ti]+23×[Nb]-0.9×(t-8) (Here, [C], [Si], [Mn], [Cr], [Ti] and [Nb] are the weight percentages of each element, and t is the thickness of the steel plate (mm).)
[0069] Table 3 below shows the microstructure of the steel sheets produced after measurement. The microstructure was measured at the surface layer and center in the thickness direction, and the fraction was also measured at the edge and center in the width direction. The microstructure of the surface layer was observed from the surface to a thickness of 50 μm, and the center was observed from the steel sheet surface to the thickness direction at 1 / 4 to 3 / 4t (25 to 75% interval, t is thickness (mm)). The microstructure of the edge was observed in the 30% portion at both ends in the width direction, and the center was observed based on the central 40% portion excluding the edge. The area fraction of MA phase and martensite was measured by etching using the Lepera etching method, followed by analysis at 1,000x magnification using an optical microscope and an image analyzer. In addition, the fractions of equiaxed ferrite (PF), bainitic ferrite (BF), bainite (B) and pearlite (P) were measured from the results of analysis at 3,000x and 5,000x magnifications using a scanning electron microscope (SEM). Here, PF is polygonal ferrite with an equiaxed crystal shape, and BF can include ferrite observed in the low temperature range, such as acicular ferrite and bainitic ferrite. In addition, P includes pearlite and coarse carbides and nitrides with a diameter of 1 μm or more.
[0070] [Table 3]
[0071] Table 4 below shows the physical properties of each manufactured test piece measured at the center and edge in the width direction. Yield strength (YS), tensile strength (TS), yield ratio (YR), and fracture elongation (T-El) were evaluated by performing tensile tests on JIS No. 5 standard test pieces taken perpendicular to the rolling direction. In addition, the impact absorption energy (E) at -20°C after cold forming was measured, and the ratio of impact absorption energy to yield strength (E / YS) at -20°C after cold forming was shown. Impact absorption energy was measured using Charpy V-notch test pieces manufactured according to ASTM standard (ASTM A370) taken perpendicular to the rolling direction.
[0072] [Table 4]
[0073] As shown in Tables 3 and 4, in the case of the examples satisfying the alloy composition and manufacturing conditions of the present invention, the microstructural characteristics proposed in the present invention were satisfied and the physical properties targeted in the present invention were secured. Figure 1 is a photograph showing the microstructure of the hot-rolled steel sheet of the invention example 2 according to one aspect of the present invention, observed with a scanning electron microscope (×3,000).
[0074] On the other hand, in Comparative Example 1, the total content of Ti and Nb exceeded the range of the present invention, and the impact resistance was deteriorated due to the formation of coarse precipitates and TiN caused by excessive precipitates in the ferrite grains.
[0075] In Comparative Example 2, the cooling rate did not reach the standard cooling rate suggested by Relation 1, and as shown in FIG. 2, excessive pearlite was formed in the microstructure.
[0076] As shown in FIG. 2, this did not result in a significant decrease in strength, but it was not possible to ensure the desired impact resistance properties.
[0077] In Comparative Example 3, the winding temperature in the width direction central portion exceeded the range proposed by the present invention. In particular, excessive pearlite was formed in the center portion in the thickness direction in both the central portion and the edge portions, and the target impact resistance properties could not be ensured.
[0078] In Comparative Example 4, the winding temperature of the edge in the width direction exceeded the range proposed in the present invention. As a result, it was shown that the impact resistance was deteriorated due to the formation of excessive pearlite in the center of the thickness direction of the edge. This is because the temperature of the edge was high and the heat transfer of the winding coil proceeded slowly at the edge.
[0079] In Comparative Example 5, the coiling temperature of the widthwise center did not reach the range of the present invention, and bainite was formed excessively in the center of the thickness direction of the center, and pearlite, MA phase, martensite, etc. were formed in the surface layer more than the level proposed in the present invention, resulting in a deterioration in elongation. On the other hand, the edge portion satisfied the coiling temperature range and had relatively good elongation and impact resistance, but the ferrite in the surface layer did not reach the range proposed in the present invention. This is believed to be because the temperature of the edge portion of the coil after coiling also rapidly decreased due to the low cooling end temperature of the widthwise center.
[0080] In Comparative Example 6, it was confirmed that when the coiling temperature of the edge portion in the width direction does not reach the range of the present invention, bainite is excessively formed in the center portion in the thickness direction, resulting in deterioration of elongation. In addition, the surface layer portion of the center portion has insufficient ferrite, and the center portion has insufficient bainitic ferrite, so that the ratio of impact resistance to yield strength does not satisfy the level proposed in the present invention.
[0081] In Comparative Example 7, the steel thickness was less than 8 mm, and an excessive cooling rate was applied for the given steel composition, resulting in a shortage of ferrite in the surface layer, a decrease in bainitic ferrite in the center of the thickness direction, and an excessive formation of pearlite. This is believed to be due to an increase in untransformed phases during the initial cooling process, resulting in the formation of pearlite in areas with a relatively high C content. As a result, the desired level of elongation could not be secured.
[0082] In Comparative Example 8, the total content of Ti and Nb did not reach the range of the present invention. The phase fractions of the microstructure measured at each position satisfied the range proposed by the present invention, but the microstructure became coarse due to the reduction in precipitates during hot rolling, and the fine precipitates after cooling and coiling were also reduced, resulting in insufficient strength and a significant decrease in impact resistance.
[0083] In Comparative Example 9, the cooling rate was equal to or greater than the CR value of Relational Formula 1 and satisfied the range proposed by the present invention, but exceeded 30°C / s. As a result, polygonal ferrite in the surface layer was insufficient, and bainite was excessively formed in the center in the thickness direction, making it impossible to ensure the desired level of elongation.
[0084] Although the present invention has been described in detail with reference to the embodiments, other embodiments are possible and the scope of the claims set forth below should not be construed as being limited to the embodiments.
Claims
1. In weight percent, C: 0.05-0.15%, Si: 0.01-0.5%, Mn: 1.0-2.0%, Al: 0.01-0.1%, Cr: 0.001-1.0%, P: 0.001-0.05%, S: 0.001-0.01%, N: 0.001-0.01%, Ti: 0.03-0.08%, Nb: 0.01-0.05%, the balance being Fe and other unavoidable impurities, with the sum of Nb and Ti being 0.04-0.1%, The microstructure of the surface layer portion within a thickness range of 50 μm from the surface contains, in terms of area percentage, 95% or more of equiaxed ferrite, 3% or less of pearlite, and contains a total of 5% or less of one or more of bainitic ferrite, bainite, MA (Martensite-Austenite constituent) phase, and martensite; The microstructure in the center portion within the range of 1 / 4 to 3 / 4 of the thickness contains, in area percentages, 80 to 95% bainitic ferrite, 10% or less bainite, 3% or less pearlite, 5 to 10% in total of one or two of a martensite-austenite constituent (MA) phase and martensite, and the remainder contains equiaxed ferrite.
2. The steel plate according to claim 1, wherein the steel plate has a thickness of 8 to 25 mm.
3. The steel plate according to claim 1, wherein the steel plate has a tensile strength of 590 MPa or more, a fracture elongation of 25% or more, a yield ratio of 0.75 to 0.9, and an impact toughness of 70 J or more at −20 ° C. after cold forming.
4. The steel plate according to claim 1, wherein the ratio (E / YS) of impact toughness (E) at −20° C. after cold forming to yield strength (YS) before cold forming is 0.15 or more.
5. The steel plate includes edge portions corresponding to 30% of both ends in the width direction and a center portion of a central 40% region corresponding to the region excluding both edge portions, The edge portion and the central portion have a difference in tensile strength of 10 MPa or less, a difference in fracture elongation of 8% or less, and a difference in impact toughness at -20 ° C. after cold forming of 20 J or less. The steel plate according to claim 1.
6. reheating a steel slab containing, by weight, C: 0.05-0.15%, Si: 0.01-0.5%, Mn: 1.0-2.0%, Al: 0.01-0.1%, Cr: 0.001-1.0%, P: 0.001-0.05%, S: 0.001-0.01%, N: 0.001-0.01%, Ti: 0.03-0.08%, Nb: 0.01-0.05%, the balance being Fe and other unavoidable impurities, and the sum of Nb and Ti being 0.04-0.1%; hot rolling the reheated steel slab; and The hot-rolled steel sheet is cooled to a temperature range of 500 to 650° C. at an average cooling rate within a range of 1 to 30° C. / s, the average cooling rate being equal to or greater than a CR value defined by the following Relation 1, and then coiled. In the cooling and winding step, the edge portions corresponding to 30% of the coil width direction at both ends are cooled at a temperature of 550 to 650° C. (TE), and the center portion of the central 40% of the coil width direction excluding both edges is cooled at a temperature of 500 to 550° C. (TC). A method for manufacturing a steel plate, wherein the average temperature difference between the edge portion and the center portion is 50 to 150°C. [Relationship 1] CR=45-16.3×[C]-5.6×[Si]-16.3×[Mn]-2.9×[Cr]+15×[Ti]+23×[Nb]-0.9×(t-8) (Here, [C], [Si], [Mn], [Cr], [Ti] and [Nb] are the weight percentages of each element, and t is the thickness of the steel plate (mm).)
7. The reheating temperature is 1100 to 1350°C, The method for producing a steel sheet according to claim 6, wherein the hot rolling temperature is 800 to 1150°C.
8. The method of claim 6, further comprising the step of air-cooling the wound coil at a temperature range of 200°C or less.
9. The method for manufacturing a steel plate according to claim 6, wherein the steel plate has a thickness of 8 to 25 mm.
Citation Information
Patent Citations
High strength hot rolled steel sheet excellent in shape and workability and its production
JP1999106861A
Steel plate for linepipe, steel pipe for linepipe, and production method therefor
JP2016108648A
Ventilation unit with omniphobic filter
KR102203348B1
High strength steel having high yield ratio and excellent durability, and method for producing same
KR102236851B1
Production of high tensile strength steel plate having extremely fine structure
JP1997143570A