Polypropylene multi-layer film for cell pouches
A polypropylene multilayer film with a specific composition and structure addresses flexibility and durability issues in secondary battery pouches, enhancing thermal adhesion and preventing electrolyte leakage, thus ensuring safety and stability.
Patent Information
- Application Number
- JP2024525888
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-11
- Filing Date
- 2022-09-27
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional pouch-type secondary battery packaging materials face issues such as flexibility, damage during processing, chemical reactions with electrolytes leading to corrosion and swelling, and insufficient mechanical strength, which can cause electrolyte leakage and fire hazards.
A polypropylene multilayer film comprising a specific composition of propylene-based binary or ternary copolymers, amorphous propylene rubber, amide-based slip agents, anti-blocking agents, and modified polyolefins, with a sealing layer thickness of 10-15% and rubber domains of 3-10%, providing excellent adhesive performance and mechanical properties.
The film enhances thermal adhesion strength, maintains peel strength after electrolyte exposure, and prevents tearing, ensuring stability and safety of cell pouches under physical and chemical stress.
Smart Images

Figure 2024543336000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polypropylene-based multilayer film, and more particularly to a polypropylene-based multilayer film for a cell pouch.
[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2021-0154954, filed on November 11, 2021, the entire text of which is incorporated herein by reference. [Background technology]
[0003] Secondary batteries generally refer to lithium secondary batteries, which are used in portable terminal devices such as laptops, smartphones, tablet PCs, and video cameras, electric vehicles including hybrid vehicles, and smart grids for energy storage. Research is ongoing to make them smaller, lighter, and thinner, while also overcoming various environmental factors such as harsh thermal environments and mechanical shocks.
[0004] As a packaging material for such lithium batteries, unlike conventional can-type packaging materials, a pouch for secondary batteries is used as an exterior material having a multi-layer structure (e.g., an inner resin layer, an aluminum layer, and an outer resin layer) because it has the advantage of being able to freely change the shape of the battery. A commonly used pouch film for secondary batteries has a multi-layer structure in which an inner resin layer is made of an adhesive layer of polyolefin such as polyethylene (PE), cast polypropylene (cPP), polypropylene (PP), etc., or a copolymer thereof, which has thermal adhesiveness and acts as a sealant, an aluminum layer which is a metal foil that acts as a base material for maintaining mechanical strength and a barrier layer against moisture and oxygen, and an outer resin layer is made of a functional polymer film such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), nylon, or liquid crystal polymer (LCP) to protect the battery cell from external impact.
[0005] Conventionally, packaging materials have mainly been used that are made by pressing metal, especially aluminum, into a cylindrical or parallelepiped shape, etc. However, such metal can packaging materials have limitations in that the outer wall of the container is hard and the shape of the battery itself is determined by the shape of the metal can packaging material.
[0006] In an attempt to overcome such limitations, technologies for packaging materials made of multilayer plastic films have been developed. For example, Patent Document 1 discloses a cell pouch made of a base layer, an adhesive layer, a barrier layer, a dry lamination layer, and a sealant layer, with the sealant layer being made of a low-fluidity polypropylene layer and a high-fluidity polypropylene layer, and Patent Document 2 discloses a cell pouch in which biaxially oriented nylon, polyethylene terephthalate (PET), and polyolefin resin are laminated in the base film and surface protection layer, and a technology for coating the base film with a fluorine-based, silicone-based, or acrylic resin as a secondary processing step.
[0007] Pouch-type secondary batteries have the advantage of being flexible in shape and being able to realize a secondary battery with the same capacity with a smaller volume and mass. However, unlike can-type batteries, pouch-type batteries use a soft pouch as a container, and therefore may be damaged for various reasons during various processes. For example, in the process of storing an electrode assembly inside a pouch, protruding parts such as electrode tabs and electrode leads may cause damage such as cracks in the PP and cPP layers inside the pouch, and if the aluminum layer is exposed due to such damage, a side reaction may occur due to its reactivity with the electrolyte. The aluminum layer exposed to the electrolyte may corrode due to a chemical reaction with the electrolyte that has permeated or diffused inside the battery and oxygen or moisture, which generates corrosive gases, causing a swelling phenomenon that expands the inside of the battery. In particular, lithium hexafluorophosphate (LIPF6) may react with water and oxygen to generate hydrofluoric acid (HF) as a corrosive gas. This hydrofluoric acid can react with aluminum and cause a sudden exothermic reaction. If it is adsorbed to the aluminum surface in a secondary reaction and penetrates into the tissue, the tissue becomes more brittle. Even a small impact can cause the pouch film to crack, and the electrolyte can leak out, causing the lithium to react with the air and ignite.
[0008] Patent Document 3 discloses an aluminum pouch film for secondary batteries that includes an outer resin layer made of polyethylene terephthalate, nylon, or the like, a first adhesive layer, an aluminum layer, a second adhesive layer, and an inner resin layer made of polyolefin. However, it only describes the overall layer structure of the pouch and does not mention the specific composition of the polyolefin that makes up the inner resin layer.
[0009] Patent Document 4 describes a polypropylene composite film including layer A mainly composed of a propylene-based random copolymer obtained by randomly copolymerizing propylene with ethylene or butene, layer B composed of 60 to 90% by weight of a propylene polymer having a comonomer (ethylene or butene) content of 0 to 1.5% by weight and 10 to 40% by weight of a propylene polymer having a comonomer (ethylene or butene) content of 10 to 40% by weight, and layer C composed of a propylene-based ethylene or butene random copolymer, and layer B is characterized by containing 100 to 2000 ppm of a fatty acid amide-based lubricant and 0 to 20% by weight of a metallocene catalyst-based low-density polyethylene, but does not mention in detail the remaining raw materials except for the raw materials of layer B.
[0010] Patent Document 5 describes a polypropylene composite film including a first skin layer (seal) mainly composed of random polypropylene having a Tm of 140 to 150°C and a sleeping agent, a core layer mainly composed of block polypropylene having a Tm of 155 to 165°C and a sleeping agent, and a second skin layer (skin) mainly composed of random polypropylene having a Tm of 140 to 150°C and a sleeping agent, and the sleeping agent used in all layers is a fatty acid amide-based sleeping agent selected from oleamide, erucamide, behenamide, and stearamide, and the first skin layer contains one or more types, and the core layer contains one of behenamide and stearamide and erucamide, but does not mention in detail the proportion of the seal layer in the entire film or characteristics such as the domain of the random polypropylene used. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Korean Patent Publication No. 2003-0029141 [Patent Document 2] Korean Patent Publication No. 2002-0030737 [Patent Document 3] Korean Patent No. 1485523 [Patent Document 4] Korean Patent Publication No. 2019-0047104 [Patent Document 5] Korean Patent No. 1894449 Summary of the Invention [Problem to be solved by the invention]
[0012] The present invention aims to provide a polypropylene-based multilayer film that is mainly used as a sealant layer for cell pouches, which suppresses the occurrence of cracks in the inner adhesive layer of the pouch even when the battery is exposed to physical or chemical shock or electrical stress, and has excellent formability, insulation properties, and electrolyte resistance.
[0013] The present invention also provides a material for a cell pouch that uses the multilayer film as a sealant layer. [Means for solving the problem]
[0014] In order to solve the above problems, the present invention provides a polypropylene-based multilayer film comprising (a) a propylene-based binary or terpolymer, (b) an amorphous propylene rubber, (c) an amide-based sleep agent, (d) an antiblocking agent, and (e) a modified polyolefin, the polypropylene-based multilayer film comprising a skin layer, a core layer, and a seal layer, the thickness of the seal layer being 10 to 15% of the thickness of the multilayer film, and the (a) propylene-based binary or terpolymer forming a rubber domain having a size of 3 to 10% of the thickness of the seal layer.
[0015] The present invention also provides a polypropylene-based multilayer film, characterized in that the (a) propylene-based binary or terpolymer contains 2 to 7 weight % ethylene and 0 to 6 weight % 1-butene, the (b) amorphous propylene rubber contains 10 to 60 weight % ethylene or 1-butene, the (c) amide-based sleeping agent is a saturated or unsaturated amide-based sleeping agent, the (d) antiblocking agent is spherical silica having an average particle size of 1.5 to 3 μm, and the (e) modified polyolefin is grafted with a dicarboxylic acid or its acid anhydride in a content of 1 to 10 weight %.
[0016] In addition, the (a) propylene-based binary or terpolymer has a melting point (Tm) of 125 to 155°C and a melt index (MI, 230°C, 2.16 kg load) of 1 to 12 g / 10 min, the (b) amorphous propylene rubber has a melt index (MI, 230°C, 2.16 kg load) of 1 to 5 g / 10 min, (c) amide-based sleeping agent is a mixture of two or more amide-based sleeping agents having 14 to 22 carbon atoms, and (d) antiblocking agent is a particle having a moisture content of less than 0.5 wt% when dried under conditions of 105°C to 60 min, and the particle bulk density is 0.8 to 1.0 g / cm. 3 The present invention provides a polypropylene-based multilayer film characterized by:
[0017] The skin layer contains (a) 70 to 99 parts by weight of a propylene-based binary or terpolymer, (e) 1 to 30 parts by weight of a modified polyolefin, and (d) 0.1 to 2 parts by weight of an antiblocking agent, the core layer contains (a) 50 to 90 parts by weight of a propylene-based binary or terpolymer, and (b) 10 to 50 parts by weight of an amorphous propylene rubber, and the seal layer contains (a) 60 to 140 parts by weight of a propylene-based binary or terpolymer, and (c) 0.1 parts by weight of an amide-based sleeping agent. and (d) 0.1 to 2 parts by weight of an antiblocking agent, and the polypropylene-based multilayer film is characterized by comprising, relative to the entire film composition, (a) 80 to 90 parts by weight of a propylene-based binary or terpolymer, (b) 10 to 20 parts by weight of an amorphous propylene rubber, (c) 0.1 to 0.3 parts by weight of an amide-based sleep agent, (d) 0.005 to 0.1 parts by weight of an antiblocking agent, and (e) 0.4 to 0.8 parts by weight of a modified polyolefin.
[0018] The multi-layer film has a thermal adhesion strength of 60 N / 15 mm or more, measured by the following method, and maintains a peel strength of 80% or more after immersion in an electrolyte solution. [Method for measuring thermal adhesive strength] The multilayer film (thickness 40 μm), aluminum foil (thickness 50 μm, laminated on the skin layer of the multilayer film), and nylon (thickness 15 μm, laminated on the aluminum foil) are laminated in order, laminated at 130°C, and cured at 50°C for 14 days. The laminate film is then heat-bonded under conditions of 200°C, 2 kgf, and 1 s so that it is in contact with the multilayer film. The film is then cut to a width of 15 mm, and the peel strength is measured at a peel angle of 180° at 23°C and a peel speed of 100 mm / min. [Method for measuring electrolyte resistance] The test piece used in the measurement of the thermal adhesive strength is immersed in an electrolyte at 85° C. for 75 hours, and then the peel strength is measured in the same manner as in the measurement of the thermal adhesive strength.
[0019] In addition, the multi-layer film does not show any tearing phenomenon in a forming test according to the following method, and peeling occurs only between the multi-layer films in a thermal adhesion strength test. [Method of measuring forming performance] The laminate film is placed on a frame-shaped metal mold (10 cm x 10 cm) with the nylon surface touching the edge of the mold, and a square pyramid is used to apply pressure to the surface of the multilayer film, drawing it five times to a minimum depth of 6 mm, and the number of tears in the corners of the laminate film is counted. [Test method for thermal adhesive strength] The multilayer film (thickness 40 μm), aluminum foil (thickness 50 μm, laminated on the skin layer of the multilayer film), and nylon (thickness 15 μm, laminated on the aluminum foil) were laminated in order, laminated at 130°C, and cured at 50°C for 14 days. The laminate film was then heat-bonded to the multilayer film under conditions of 200°C, 2 kgf, and 1 s, and then cut to a width of 15 mm and peeled at 23°C, a peel speed of 100 mm / min, and a peel angle of 180°.
[0020] In order to solve the other problem, the present invention provides a material for a cell pouch, comprising: a sealant layer made of the film; a barrier layer formed on the sealant layer; and an outer resin layer formed on the barrier layer. Effect of the Invention
[0021] According to the present invention, there is provided a polypropylene-based multilayer film comprising a skin layer, a core layer, and a seal layer of a specific composition, which is used as a sealant layer for a cell pouch and has excellent adhesive performance, while simultaneously satisfying moldability in post-processing and having excellent mechanical properties, surface characteristics, and transparency. The relationship between the thickness of the specific layer and the properties of the specific components is presented, and the relationship between the thickness of the seal layer and the size of the rubber domain of a propylene-based binary or terpolymer is presented. [Brief description of the drawings]
[0022] [Figure 1] 1 is a photograph showing the morphology of a cell pouch after peeling of the sealant layer, illustrating the phenomena of peel seal (a), delamination (b), and delamination (c). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The present invention will be described in detail below through preferred embodiments. Prior to this, the terms and words used in this specification and claims should not be interpreted in their ordinary or dictionary sense, but should be interpreted in their meaning and concept consistent with the technical idea of the present invention, based on the principle that the inventor can appropriately define the concept of the term to best describe his / her invention. Therefore, the configuration of the embodiment described in this specification is merely one of the most preferred embodiments of the present invention, and does not fully represent the technical idea of the present invention, so it should be understood that there may be various equivalents and modifications that can replace them at the time of this application.
[0024] The present inventors have conducted research into a film material that satisfies both the required adhesive performance and formability in post-processing as a material including a skin layer, a core layer, and a seal layer used as a sealant layer in a conventional cell pouch. As a result, they have surprisingly discovered that there is a relationship between the thickness of the seal layer and the size of the rubber domain of a propylene-based binary or terpolymer, which allows the film material to have excellent adhesive performance and formability in post-processing when used as a sealant layer in a cell pouch, while also having excellent mechanical properties, surface characteristics, and transparency, and have arrived at the present invention.
[0025] Therefore, the present invention discloses a polypropylene-based multilayer film comprising (a) a propylene-based binary or terpolymer, (b) an amorphous propylene rubber, (c) an amide-based sleep agent, (d) an antiblocking agent, and (e) a modified polyolefin, the polypropylene-based multilayer film comprising a skin layer, a core layer, and a seal layer, the thickness of the seal layer being 10 to 15% of the thickness of the multilayer film, and the (a) propylene-based binary or terpolymer forming a rubber domain having a size of 3 to 10% of the thickness of the seal layer.
[0026] When used as a sealant layer of a cell pouch including a sealant layer, a barrier layer formed on the sealant layer, and an outer resin layer formed on the barrier layer, the polypropylene-based multilayer film according to the present invention has excellent adhesive performance and satisfies formability in post-processing, while also having excellent mechanical properties, surface characteristics, and transparency.
[0027] The sealant layer may have a thickness of about 25 to 120 μm for sufficient thermal bonding properties, but may have an appropriate thickness depending on the application of the cell pouch to be realized, for example, a thin film type cell pouch realized with a total thickness of about 88 μm, a general type cell pouch realized with a total thickness of about 113 μm, or a medium to large size cell pouch realized with a total thickness of about 153 μm.
[0028] The outer resin layer is the outermost layer of the packaging material for the lithium secondary battery that may be provided on the barrier layer and exposed to the outside, and is preferably formed using a material having heat resistance, cold resistance, pinhole resistance, insulating properties, chemical resistance, formability, etc., as well as wear resistance, so as to protect the barrier layer. The outer resin layer made of such a heat-resistant resin film may include a polyamide-based resin or a polyester-based resin. The polyamide-based resin may be nylon, which has a high elongation rate and is favorable for forming, and the polyester-based resin may be polybutylene terephthalate (PBT) or polyethylene terephthalate (PET), which may realize high chemical resistance, pinhole resistance, insulating properties, mechanical strength, etc.
[0029] The outer resin layer may have a thickness of about 15 to 30 μm, taking into consideration sufficient wear resistance, heat resistance, pinhole resistance, chemical resistance, moldability, insulation, etc. If the thickness of the outer resin layer is too thin, the moldability of the packaging material for the secondary battery may be reduced due to insufficient strength of the outer resin layer. On the other hand, if the thickness is too thick, the sealant layer and the barrier layer provided under the outer resin layer must be implemented with a relatively thin thickness, which may cause problems such as a decrease in thermal adhesion strength and a decrease in peel strength between layers in the packaging material for the secondary battery. However, the thickness of the outer resin layer is not limited to the above range and may have an appropriate thickness depending on the intended use of the cell pouch, for example, a thin-film cell pouch implemented with a total thickness of about 88 μm, a general-type cell pouch implemented with a total thickness of about 113 μm, or a medium-sized or large-sized cell pouch implemented with a total thickness of about 153 μm.
[0030] In the present invention, a first adhesive resin layer for adhering the outer resin layer and the barrier layer may be further formed.
[0031] The first adhesive resin layer is formed by an adhesive capable of bonding the outer resin layer and the barrier layer, and the adhesive used to form the first adhesive resin layer may be a two-component curing adhesive or a one-component curing adhesive. The adhesive bonding tool used to form the first adhesive resin layer is also not particularly limited, and may be selected from a chemical reaction type, a solvent volatilization type, a thermal melting type, a thermal pressure type, and the like.
[0032] Examples of the resin components of the adhesive that can be used to form the first adhesive resin layer include polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, polycarbonate, and copolymerized polyester, polyether-based adhesives, polyurethane-based adhesives, epoxy-based resins, phenolic resin-based resins, polyamide-based resins such as nylon 6, nylon 66, nylon 12, and copolymerized polyamide, polyolefin-based resins such as polyolefin, acid-modified polyolefin, and metal-modified polyolefin, polyvinyl acetate-based resins, cellulose-based adhesives, (meth)acrylic resins, polyimide-based resins, amino resins such as urea resins and melamine resins, rubbers such as chloroprene rubber, nitrile rubber, and styrene-butadiene, silicone-based resins, and fluorinated ethylene propylene copolymers. One of these adhesive components may be used alone, or two or more may be used in combination. The deformation pattern of two or more adhesive components is not particularly limited, and examples of the adhesive components include a mixed resin of polyamide and acid-modified polyolefin, a mixed resin of polyamide and metal-modified polyolefin, a mixed resin of polyamide and polyester, a mixed resin of polyester and acid-modified polyolefin, a mixed resin of polyester and metal-modified polyolefin, etc. Among these, from the viewpoint of excellent stretchability, durability and suppression of flexural deformation under high humidity conditions, and suppression of thermal deterioration during heat stitching, and of suppressing a decrease in lamination strength between the outer resin layer and the barrier layer to effectively suppress the occurrence of delamination, preferred are polyurethane-based two-component curing adhesives, polyamide, polyester, or mixed resins of these with modified polyolefins.
[0033] Meanwhile, the thickness of the first adhesive resin layer may be, for example, 2 to 10 μm.
[0034] The barrier layer is a metal foil gas barrier layer for blocking the ingress and egress of moisture and air from the outside and gas generated from the inside, and may be in contact with the sealant layer. The barrier layer includes a metal having gas barrier and moisture barrier properties, and may include, for example, one or more selected from the group consisting of aluminum (Al), iron (Fe), copper (Cu), nickel (Ni), tin (Sn), zinc (Zn), indium (In), tungsten (W), etc. (single metal or mixture of single metals), or an alloy of two or more selected from the group. In a preferred embodiment, the barrier layer may include aluminum (Al) or an aluminum alloy, taking into consideration all of moisture barrier properties, gas barrier properties, and formability. The barrier layer may have a thickness of about 25 to 45 μm in order to have sufficient gas barrier and moisture barrier properties. However, the thickness of the barrier layer is not limited thereto, and may have an appropriate thickness depending on the use of the cell pouch to be realized, i.e., generally, a thin-film cell pouch realized with a total thickness of about 88 μm, a general-type cell pouch realized with a total thickness of about 113 μm, or a medium-sized or large cell pouch realized with a total thickness of about 153 μm.
[0035] It is preferable that at least one surface of the barrier layer, preferably at least the surface on the sealant layer side, more preferably both surfaces, are chemically treated in order to stabilize adhesion and prevent dissolution and corrosion. Here, the chemical conversion treatment is a treatment for forming an acid-resistant coating on the surface of the barrier layer. Examples of the chemical conversion treatment include a chromate treatment using a chromium acid compound such as chromium nitrate, chromium fluoride, chromium sulfate, chromium acetate, chromium oxalate, chromium biphosphate, chromate acetylacetate, chromium chloride, and calcium chromium sulfate, a phosphate chromate treatment using a phosphoric acid-capable substance such as sodium phosphate, potassium phosphate, ammonium phosphate, and polyphosphoric acid, and a chromate treatment using an aminated phenol polymer.
[0036] As a chemical conversion treatment method for imparting corrosion resistance to the barrier layer, a method of forming a corrosion-resistant layer on the surface of the barrier layer by coating a material in which fine particles of metal oxides such as aluminum oxide, titanium oxide, cerium oxide, and tin oxide, or barium sulfate are dispersed in phosphoric acid, and baking is performed at 150°C or higher. In addition, a resin layer in which a cationic polymer is crosslinked with a crosslinking agent can be formed on the corrosion-resistant layer. Here, examples of the cationic polymer include polyethyleneimine, an ionic polymer complex consisting of a polymer having polyethyleneimine and carboxyl acid, a primary amine-grafted acrylic resin in which a primary amine is grafted to the main skeleton of acrylic, polyallylamine or its derivative, and aminophenol. These cationic polymers may be used alone or in combination of two or more. Examples of the crosslinking agent include a compound having at least one functional group selected from the group consisting of an isocyanate group, a glycidyl group, a carboxyl group, and an oxazoline group, and a silane coupling agent. These crosslinking agents may be used alone or in combination of two or more.
[0037] The chemical conversion treatment may be performed using one type of chemical conversion treatment alone, or may be performed using two or more types of chemical conversion treatment in combination. The chemical conversion treatment may be performed using one type of compound alone, or may be performed using two or more types of compounds in combination. Among these, a chromate treatment with chromate acid is preferred, and a chromate treatment using a combination of a chromate compound, a phosphoric acid compound, and an aminated phenol polymer is more preferred.
[0038] The chemical conversion treatment is carried out by applying a solution containing a compound used to form an acid-resistant coating to the surface of the barrier layer by a method such as bar coating, roll coating, bravia coating, or immersion, and then heating the metal foil so that its temperature is around 70 to 200°C.
[0039] In the present invention, a second adhesive resin layer for adhering the barrier layer and the sealant layer may further be formed.
[0040] The second adhesive resin layer may be formed by an adhesive capable of bonding the outer resin layer and the barrier layer. The adhesive used to form the second adhesive resin layer may be a two-component curing adhesive or a one-component curing adhesive. The adhesive bonding tool used to form the second adhesive resin layer is not particularly limited, and may be any of a chemical reaction type, a solvent volatilization type, a thermal melting type, a thermal pressure type, and the like.
[0041] Examples of the resin components of the adhesive that can be used to form the second adhesive resin layer include polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, polycarbonate, and copolymerized polyester, polyether-based adhesives, polyurethane-based adhesives, epoxy-based resins, phenolic resin-based resins, polyamide-based resins such as nylon 6, nylon 66, nylon 12, and copolymerized polyamide, polyolefin-based resins such as polyolefin, acid-modified polyolefin, and metal-modified polyolefin, polyvinyl acetate-based resins, cellulose-based adhesives, (meth)acrylic resins, polyimide-based resins, amino resins such as urea resins and melamine resins, rubbers such as chloroprene rubber, nitrile rubber, and styrene-butadiene, silicone-based resins, and fluorinated ethylene propylene copolymers. These adhesive components may be used alone or in combination of two or more. The deformation pattern of two or more adhesive components is not particularly limited, and examples of the adhesive components include a mixed resin of polyamide and acid-modified polyolefin, a mixed resin of polyamide and metal-modified polyolefin, a mixed resin of polyamide and polyester, a mixed resin of polyester and acid-modified polyolefin, a mixed resin of polyester and metal-modified polyolefin, etc. Among these, from the viewpoint of excellent stretchability, durability and suppression of flexural deformation under high humidity conditions, and suppression of thermal deterioration during heat stitching, and of suppressing a decrease in lamination strength between the sealant layer and the barrier layer and effectively suppressing the occurrence of delamination, preferred are a polyurethane-based two-component curing adhesive, a polyolefin-based resin, or a mixed resin of these and a modified polyolefin.
[0042] On the other hand, the thickness of the second adhesive resin layer may be, for example, 2 to 60 μm.
[0043] The method for producing the packaging material for secondary batteries according to the present invention is not particularly limited as long as it can produce a laminate in which layers of predetermined composition are laminated together. The following method is exemplified.
[0044] First, a laminate (laminate A) is formed in which an outer resin layer, a first adhesive resin layer, and a barrier layer are laminated in this order. More specifically, the laminate A can be formed by a dry lamination method in which an adhesive used to form the first adhesive resin layer is applied to a barrier layer whose surface has been chemically treated by a coating method such as extrusion, gravure coating, or roll coating, and then dried, and the outer resin layer is laminated and the first adhesive resin layer is cured.
[0045] Next, a sealant layer is laminated on the barrier layer of the laminate A. When a second adhesive resin layer is provided between the barrier layer and the sealant layer, for example, the following method may be used: (1) a method in which an adhesive for forming a second adhesive resin layer is solution-coated on the metal foil of the laminate A and then laminated by a drying method at high temperature, and a sealant layer previously formed into a two- or three-layer sheet is laminated on the second adhesive resin layer by a thermal lamination method (dry lamination method), (2) a method in which a sealant layer consisting of two or three layers is co-extruded onto the barrier layer of the laminate A (co-extrusion lamination method), or (3) a method in which a molten second adhesive resin layer is poured between the barrier layer of the laminate A and the sealant layer previously formed into a two- or three-layer sheet, while bonding the laminate A and the sealant layer via the second adhesive resin layer (sandwich lamination method).
[0046] The sealant layer of the cell pouch is an element that affects the stability of the battery, so it is important to prevent electrolyte leakage. To prevent this, the shape after peeling should be looked at. There are three types of shapes after peeling, which are peel seal (a), delamination (b), and delamination (c) as shown in Figure 1. In peel seal, the seal layers on the two sides peel off while causing uniform efflorescence, which is advantageous in terms of stability as it does not lose its original adhesive strength even when an external impact occurs. In delamination, the inner adhesive surfaces of the multi-layer CPP (cast polypropylene) film peel off, and in delamination, the CPP film and aluminum foil peel off, and in both cases, the adhesive strength decreases compared to before peeling. In the case of delamination, the thickness of one CPP becomes thinner, and in the case of delamination, the CPP layer and aluminum foil are separated and exposed, increasing the possibility of leakage at the corresponding area.
[0047] In order to satisfy both the peeling phenomenon and adhesive strength, the ratio of the thickness of the sealing layer to the total film thickness should be limited to 10 to 15%. The sealing layer plays the most important role in thermal adhesive properties as the sealing layers of both films butt against each other during thermal adhesive. If the ratio of the thickness of the sealing layer to the total film thickness is less than 10%, the amount of heat absorbed by the core layer is relatively large, causing interlayer peeling and low thermal adhesive strength, and if it exceeds 15%, it will become unusable due to heat fusion and delamination.
[0048] Here, in the present invention, the size of the rubber domain of (a) propylene binary or terpolymer used in the sealing layer is 3 to 10% of the thickness of the sealing layer. If the film is thermally bonded within the range of the rubber domain size, the rubber domain, which has a lower glass transition temperature (Tg) than the matrix, melts and is useful during thermal bonding. If the rubber domain size is large, the area of adhesion when they come into contact with each other becomes wider, increasing the thermal bonding strength, but delamination occurs, and if the rubber domain size is small, the thermal bonding strength decreases. In this case, the size of the rubber domain can be easily adjusted by those skilled in the art by changing polymerization conditions such as the type and content of the comonomer, the catalyst composition and amount used, polymerization temperature, and pressure, and in the present invention, there is no limitation on the relationship between the size of the rubber domain and the polymerization conditions such as the type of the comonomer. Meanwhile, the size of the rubber domain can be measured by preparing a specimen of 2 mm thickness using a press heated to 190°C, etching the specimen with nucleic acid at room temperature, and observing it with FE-SEM to measure its average size.
[0049] In the present invention, the (a) propylene binary or terpolymer is a main component of the multilayer film and is a copolymer of propylene and one or two α-olefins other than propylene, and is preferably a binary copolymer obtained by simultaneously injecting and polymerizing propylene and ethylene, or a terpolymer obtained by simultaneously injecting and polymerizing propylene, ethylene, and 1-butene. The polymerization method of the copolymer is a conventional method known in the art and is not particularly limited in the present invention.
[0050] The (a) propylene-based binary or terpolymer may contain the same propylene as the olefin-based adhesive component as a constituent, which contributes to improving the aluminum peel strength, but the (a) propylene-based binary or terpolymer is a crystalline copolymer, not an amorphous propylene-ethylene copolymer, and may contain 2 to 7 wt% ethylene or 0 to 6 wt% 1-butene, more preferably 3 to 6 wt% ethylene or 0 to 5 wt% 1-butene, and may have a melting point (Tm) of 125 to 155° C., more preferably 140 to 154° C. If the (a) propylene-based binary or terpolymer has an ethylene content of less than 2 wt%, the flexibility may be insufficient, resulting in efflorescence and edge cracking during foaming, and wetting during lamination with an adhesive may be reduced. Also, if the ethylene content exceeds 7% by weight, the heat resistance is insufficient, and appearance problems (deformation and distortion) may occur due to heat generation during use.
[0051] Meanwhile, the (a) propylene-based binary or terpolymer may have a melt index (MI, 230°C, 2.16 kg load) of 1 to 12 g / 10 min, preferably 2 to 8 g / 10 min. If the melt index is less than 1 g / 10 min, the productivity may decrease, and if it exceeds 12 g / 10 min, the improvement effect on aluminum peel strength may be insignificant.
[0052] In the present invention, the (b) amorphous propylene rubber is a copolymer of propylene and one α-olefin other than propylene, and preferably propylene and ethylene or 1-butene are simultaneously injected, and the ethylene and 1-butene may be contained in a content of 10 to 60% by weight, and more preferably, the ethylene may be contained in a content of 10 to 30% by weight, or the 1-butene may be contained in a content of 20 to 40% by weight. If the content of ethylene or 1-butene is less than 10% by weight, the improvement effect of impact resistance may be insignificant, and if it exceeds 60% by weight, a large amount of low molecular weight may be contained, and the surface may become sticky and uneven during film formation, and the tensile strength may be low. The polymerization method of the copolymer is a conventional method known in the art, and is not particularly limited in the present invention.
[0053] In the present invention, the (c) sleeping agent serves to improve formability and workability by lowering the friction coefficient in post-processing such as deep drawing as the organic compound migrates to the surface of the substrate over time and imparts sleeping properties, and the (d) anti-blocking agent serves to improve formability and workability by forming irregularities on the film surface and alleviating the sticky (blocking) phenomenon in post-processing such as deep drawing.
[0054] The (c) sleep aid is preferably an amide-based organic compound synthesized from fatty acid, which has a high melting point and a neutral structure in which the hydroxyl group is replaced with an amino structure.
[0055] The (c) sleep agent is a mixture of two or more amide sleep agents having a carbon number of 14 to 22, and is preferably a primary or secondary, saturated or unsaturated amide organic compound having a carbon number of 14 to 22.
[0056] The (d) antiblocking agent is preferably a silica antiblocking agent having a spherical particle pattern and a uniform particle distribution, and is a particle having a moisture content of less than 0.5% by weight when dried (105°C and 60 min conditions), an average particle size of 1.5 to 3.0 μm, preferably 2 to 3 μm, and a bulk density of 0.8 to 1.0 g / cm. 3 It is preferable that:
[0057] The (e) modified polyolefin is a subcomponent of the skin layer of the multilayer film, and may be modified polypropylene grafted with the polar functional group, dicarboxylic acid or its anhydride, at a content of 1 to 10 wt%, preferably 3 to 5 wt%. If the content of dicarboxylic acid or its anhydride in the modified polypropylene is less than 1 wt%, the adhesive strength with the aluminum foil may be reduced, and if it exceeds 10 wt%, fish eyes (F / E) may be generated by the polar functional group, low molecules may be generated, and the surface tension after corona surface treatment may be reduced, resulting in reduced adhesive strength with the aluminum foil.
[0058] Here, the dicarboxylic acid may include maleic acid, phthalic acid, itaconic acid, citraconic acid, alkenylsuccinic acid, cis-1,2,3,6-tetrahydrophthalic acid, 4-methyl-1,2,3,6-tetrahydrophthalic acid, or a mixture of two or more thereof, and the anhydride of the dicarboxylic acid may be the dicarboxylic acid anhydride examples mentioned above, and preferably the dicarboxylic acid may be maleic acid.
[0059] The above components (a) to (e) constitute the main components and subcomponents of the skin layer, core layer, and seal layer, and may be included in a specific content ratio to realize the desired adhesive performance and molding properties in post-processing when used as a sealant layer of a cell pouch.
[0060] That is, in the present invention, the skin layer contains (a) 70 to 99 parts by weight of a propylene-based binary or terpolymer, (e) 1 to 30 parts by weight of a modified polyolefin, and (d) 0.1 to 2 parts by weight of an antiblocking agent, the core layer contains (a) 50 to 90 parts by weight of a propylene-based binary or terpolymer, and (b) 10 to 50 parts by weight of an amorphous propylene rubber, and the seal layer contains (a) 60 to 140 parts by weight of a propylene-based binary or terpolymer. , (c) 0.1 to 2 parts by weight of an amide-based sleeping agent, and (d) 0.1 to 2 parts by weight of an antiblocking agent, and the total film composition may contain (a) 80 to 90 parts by weight of a propylene-based binary or terpolymer, (b) 10 to 20 parts by weight of amorphous propylene rubber, (c) 0.1 to 0.3 parts by weight of an amide-based sleeping agent, (d) 0.005 to 0.1 parts by weight of an antiblocking agent, and (e) 0.4 to 0.8 parts by weight of a modified polyolefin.
[0061] Meanwhile, the resin composition of each layer constituting the polypropylene-based multilayer film according to the present invention may further contain, as necessary, one or more of various additives, such as antioxidants, catalyst neutralizers, pigments, dispersants, weatherproofing agents, antistatic agents, UV stabilizers, talc, etc., so long as the object of the present invention is not impaired. The amount of such additives used may be adjusted taking into consideration the total production amount and production process, within the ranges known to be usable in producing the polypropylene-based multilayer film according to the present invention without affecting its properties.
[0062] In the present invention, the multilayer film can be manufactured using the above components by a conventional method known in the art, for example, the components constituting each layer are mixed in the required amounts in a Henschel mixer, pelletized at 180 to 240°C using an extruder, and melt-molded into a film using a multilayer film molding machine to manufacture the multilayer film.
[0063] The polypropylene-based multilayer film according to the present invention as described above can be used as a sealant layer of a cell pouch, and can have excellent adhesive performance, excellent formability in post-processing, and excellent mechanical properties, surface characteristics, and transparency. More specifically, the polypropylene-based multilayer film according to the present invention can provide a polypropylene-based multilayer film having a thermal adhesion strength of 60 N / 15 mm or more measured by the method described below, a peel strength after immersion in an electrolyte solution of 80% or more, no tearing phenomenon in a forming test by the method described below, and peeling only between the multilayer films during a thermal adhesion strength test. [Method for measuring thermal adhesive strength] The multilayer film (thickness 40 μm), aluminum foil (thickness 50 μm, laminated on the skin layer of the multilayer film), and nylon (thickness 15 μm, laminated on the aluminum foil) are laminated in order, laminated at 130°C, and cured at 50°C for 14 days. The laminate film is then heat-bonded under conditions of 200°C, 2 kgf, and 1 s so that it is in contact with the multilayer film. The film is then cut to a width of 15 mm, and the peel strength is measured at a peel angle of 180° at 23°C and a peel speed of 100 mm / min. [Method for measuring electrolyte resistance] The test piece used in the measurement of the thermal adhesive strength is immersed in an electrolyte at 85° C. for 75 hours, and then the peel strength is measured in the same manner as in the measurement of the thermal adhesive strength. [Method of measuring forming performance] The laminate film is placed on a frame-shaped metal mold (10 cm x 10 cm) with the nylon surface touching the edge of the mold, and a square pyramid is used to pressurize the surface of the multilayer film five times to a minimum depth of 6 mm, and the number of tears in the corners of the laminate film is counted.
[0064] The polypropylene-based multilayer film according to the present invention described above is primarily used for forming cell pouches, but is not limited thereto, and may of course also be used for forming packaging films, retort pouches, pouches for electronic materials, and the like. EXAMPLES
[0065] The present invention will now be described in more detail with reference to specific examples and comparative examples.
[0066] First, the preparation examples or specifications of the components used in the examples and comparative examples are as follows.
[0067] (a) Production of propylene-based copolymers or terpolymers Propylene and ethylene or 1-butene are injected into the reactor to carry out a bulk polymerization reaction. The content of the comonomers is adjusted within the range of 2-7% by weight of ethylene and 0-6% by weight of 1-butene so that the size of the rubber domain in the copolymer is the size shown in Table 1. Propylene-based binary or terpolymers (melting point (Tm): 140-165°C, melt index (230°C, 2.16 kg load): about 2-10g / 10min) were produced. The size of the rubber domain was measured by preparing a 2T sample using a press, etching it with hexane, and observing it with an FE-SEM. The melt index, melting point, and ethylene / 1-butene content of the copolymer were measured as follows. -Melt Index Measured according to ASTM D1238 at 230°C and a load of 2.16 kg. Melting point (Tm) Using a differential scanning calorimeter (trade name DSC, manufactured by Perkin-Elmer Co.), 10 mg of a specimen was pre-melted at 220°C for 5 minutes under nitrogen gas atmosphere, and then the temperature was lowered to 40°C at a rate of 5°C / min. The temperature was then increased at a rate of 5°C / min, and the peak temperature of the maximum peak of the melting endothermic curve obtained was defined as the melting point (Tm). The melting point of indium (In) measured using the same measuring device at a heating rate of 5°C / min was 156.6°C. -Ethylene and 1-butene content Using infrared absorption spectroscopy (FT-IR), -1 The ethylene content was measured using a characteristic peak at 767 cm -1 The specific peak was used to measure the 1-butene content.
[0068] (b) Amorphous propylene rubber Propylene-based elastomers (MI1-4, EL10-30 wt %, or BN-1 20-40 wt %) were used.
[0069] (c) Amide-based sleep aids Erucamide was used.
[0070] (d) Antiblocking Agent Spherical silica particles (water content less than 0.5% by weight, average particle size 2 to 3 μm, and bulk density 0.8 to 1.0 g / cm 3 ) was used.
[0071] (e) Modified polyolefin Polypropylene grafted with 3-5 wt.% maleic anhydride content was used.
[0072] [Examples 1 to 5, Comparative Examples 1 to 4] The skin layer is comprised of 70 to 99 parts by weight of (a) a propylene-based binary or terpolymer, 1 to 30 parts by weight of (e) a modified polyolefin, and 0.1 to 2 parts by weight of (d) an antiblocking agent. The core layer is comprised of 50 to 90 parts by weight of (a) a propylene-based binary or terpolymer, and 10 to 50 parts by weight of (b) an amorphous propylene rubber. The seal layer is comprised of 96 to 99.8 parts by weight of (a) a propylene-based binary or terpolymer, and (c) an amine. The mixture is composed of 0.1 to 2 parts by weight of (d) dopant and 0.1 to 2 parts by weight of antiblocking agent, and the total composition is as shown in Table 1 below (unit: parts by weight, usually added phenol-based antioxidant, phosphate-based antioxidant, and hydrotalcite as catalyst neutralizer) and melt-mixed at 220 ° C by a single screw extruder to form pellets, and a propylene block copolymer mixed resin composition is prepared for each layer. Next, the mixed resin composition for each layer is melt-formed at 220 ° C by a multilayer film forming machine to form a film, and a multilayer film having a thickness of 40 μm and a thickness ratio of the sealing layer as shown in Table 1 is prepared.
[0073] Next, an oriented polyamide film (15 μm thick) as an external resin layer and an aluminum thin film (50 μm thick) with chromate phosphate coatings on both sides as a barrier layer are bonded by dry lamination using an adhesive (polyurethane-based two-component curing adhesive, 3 μm thick). The seal layer is made up of three layers and formed by the T-die casting method. The external resin layer, barrier layer bonded film and sealant layer (40 μm thick) are bonded by dry lamination to obtain a packaging material for lithium secondary batteries.
[0074] [Test example] The pellets and films thus prepared were used to prepare test specimens, and their physical properties were measured and evaluated according to the following methods. The results are shown in Table 1 below. [Measurement and evaluation methods of physical properties] (1) Thermal adhesive strength The packaging material produced above was heat-bonded under conditions of 200°C, 2 kgf, and 1 s so that the multilayer film was in contact with each other, and then cut to a width of 15 mm, and the peel strength was measured at a peel speed of 100 mm / min and a peel angle of 180° at 23°C. 80N / 15mm or more was marked with "◎", less than 80N / 15mm and 60N / 15mm or more was marked with "○", and less than 60N / 15mm was marked with "△". (2) Electrolyte resistance The specimens used in the thermal adhesion strength measurement were immersed in an electrolyte at 85°C for 75 hours, and then the peel strength was measured in the same manner as in the thermal adhesion strength measurement method. If the peel strength after immersion in the electrolyte was maintained at 80% or more of the peel strength before immersion in the electrolyte, it was marked with "○". The electrolyte composition was [EC / DEC / DMC=1 / 1 / 1 (v / v parts) + LiPF6 (1 mol / L) + H2O 300 ppm], where EC is ethylene carbonate, DEC is diethyl carbonate, and DMC is dimethyl carbonate. (3) Slip property The coefficient of friction was measured (based on the multilayer film surface). If the coefficient of dynamic friction was 0.3 or less, it was marked with "◎", and if it was more than 0.3 and 0.4 or less, it was marked with "○". (4) Forming performance The packaging material was placed on a frame-shaped metal mold (10 cm x 10 cm) with the outer resin layer touching the edge of the mold, and pressure was applied to the multilayer film surface with a square pyramid to squeeze to a minimum depth of 9 mm. If there was no tearing at the corners of the packaging material, it was indicated as "◎", if there was one to three tearing, it was indicated as "△", and if there was four tearing, it was indicated as "X". (5) Peel seal When measuring the thermal adhesive strength, if the films on both sides were peeled off evenly as shown in Figure 1(a), it was marked as "O". If peeling occurred between the skin layer, core layer, or seal layer inside the film, rather than between the seal layers of both films as shown in Figure 1(b), it was marked as "△". If peeling occurred between the film and the aluminum foil as shown in Figure 1(c), it was marked as "X".
[0075] [Table 1]
[0076] Referring to Table 1, in accordance with the present invention, a polypropylene-based multilayer film having a specific composition range for the skin layer, core layer, and seal layer, in which the thickness ratio of the seal layer in the entire film is within a specific range, and the thickness of the seal layer and the size of the rubber domain of the propylene-based binary or terpolymer are in a specific ratio, when used as a sealant layer for a cell pouch (see thermal adhesive strength and peel seal), it can be confirmed that the film has excellent adhesive performance (see thermal adhesive strength and peel seal), and can simultaneously satisfy formability in post-processing (see forming performance), while also realizing excellent mechanical properties, surface properties, and transparency.
[0077] On the other hand, in terms of thermal adhesion strength, if the ratio of the thickness of the seal layer to the entire film is less than 10% (Comparative Example 1), the amount of heat absorbed by the core layer is relatively large, interlayer delamination occurs, and the thermal adhesion strength is low and forming performance is deteriorated. If it exceeds 15% (Comparative Example 2), the thermal adhesion strength is excellent, but during the thermal adhesion strength test, delamination does not occur between the multilayer film (see Figure 1(a)), and delamination occurs between the multilayer film and the aluminum foil (see Figure 1(c)).
[0078] In addition, when the film is thermally bonded, the rubber domain, which has a lower glass transition temperature (Tg) than the matrix, melts and becomes useful in thermal bonding. However, if the size of the domain exceeds 10% of the thickness of the sealing layer (Comparative Example 3), the area of adhesion when they butt against each other becomes wider, increasing the thermal bonding strength, but causing delamination. On the other hand, if the size of the domain is less than 3% of the thickness of the sealing layer (Comparative Example 4), the thermal bonding strength and forming performance decrease.
[0079] From this, it can be seen that in a multilayer film used as a sealant layer of a cell pouch, there is a relationship between the thickness of the seal layer and the size of the rubber domain of the propylene-based binary or terpolymer that satisfies all of excellent mechanical properties, surface characteristics, and transparency as well as adhesive performance and formability in post-processing, and it can be confirmed that the polypropylene-based multilayer film including a skin layer, a core layer, and a seal layer according to the present invention fully satisfies this relationship.
[0080] The preferred embodiments of the present invention have been described in detail above. The description of the present invention is for illustrative purposes only, and those skilled in the art will understand that the present invention can be easily modified into other specific forms without changing the technical concept or essential features of the present invention.
[0081] Therefore, the scope of the present invention is defined by the claims set forth below rather than the above detailed description, and all modifications and variations that fall within the meaning, scope and equivalent concept of the claims should be interpreted as being included within the scope of the present invention.
Claims
1. A polypropylene-based multilayer film comprising (a) a propylene-based binary or terpolymer, (b) an amorphous propylene rubber, (c) an amide-based sleep agent, (d) an antiblocking agent, and (e) a modified polyolefin, the film comprising a skin layer, a core layer, and a seal layer, The thickness of the sealing layer is 10 to 15% of the thickness of the multilayer film, and the (a) propylene-based binary or terpolymer is a polypropylene-based multilayer film having a rubber domain having a size of 3 to 10% of the thickness of the sealing layer.
2. (a) the propylene-based copolymer or terpolymer contains 2 to 7% by weight of ethylene and 0 to 6% by weight of 1-butene; (b) the amorphous propylene rubber contains 10 to 60% by weight of ethylene or 1-butene; The (c) amide-based sleep aid is a saturated or unsaturated amide-based sleep aid, The (d) antiblocking agent is spherical silica having an average particle size of 1.5 to 3 μm, 2. The polypropylene-based multi-layer film according to claim 1, wherein the modified polyolefin (e) is grafted with a dicarboxylic acid or its acid anhydride in an amount of 1 to 10% by weight.
3. The (a) propylene-based binary or terpolymer has a melting point (Tm) of 125 to 155° C. and a melt index (MI, 230° C., 2.16 kg load) of 1 to 12 g / 10 min; The (b) amorphous propylene rubber has a melt index (MI, 230° C., 2.16 kg load) of 1 to 5 g / 10 min; (c) the amide-based sleeping agent is a mixture of two or more amide-based sleeping agents having 14 to 22 carbon atoms; The (d) antiblocking agent is a particle having a moisture content of less than 0.5 wt % when dried at 105° C. for 60 min, and a bulk density of the particle is 0.8 to 1.0 g / cm 3The polypropylene-based multilayer film according to claim 2,
4. The skin layer comprises: (a) 70 to 99 parts by weight of a propylene-based binary or terpolymer; (e) 1 to 30 parts by weight of a modified polyolefin; and (d) 0.1 to 2 parts by weight of an antiblocking agent; The core layer comprises (a) 50 to 90 parts by weight of a propylene-based binary or terpolymer, and (b) 10 to 50 parts by weight of an amorphous propylene rubber, The sealing layer comprises (a) 60 to 140 parts by weight of a propylene-based binary or terpolymer, (c) 0.1 to 2 parts by weight of an amide-based sleeping agent, and (d) 0.1 to 2 parts by weight of an antiblocking agent, 2. The polypropylene-based multilayer film according to claim 1, comprising, based on the total film composition, (a) 80 to 90 parts by weight of a propylene-based binary or terpolymer, (b) 10 to 20 parts by weight of an amorphous propylene rubber, (c) 0.1 to 0.3 parts by weight of an amide-based sleep agent, (d) 0.005 to 0.1 parts by weight of an antiblocking agent, and (e) 0.4 to 0.8 parts by weight of a modified polyolefin.
5. The polypropylene-based multilayer film according to claim 1, characterized in that the multilayer film has a thermal adhesion strength of 60 N / 15 mm or more, measured by the following method, and maintains a peel strength of 80% or more after immersion in an electrolyte solution: [Method for measuring thermal adhesive strength] The multilayer film (thickness 40 μm), aluminum foil (thickness 50 μm, laminated on the skin layer of the multilayer film), and nylon (thickness 15 μm, laminated on the aluminum foil) were laminated in this order, laminated at 130° C., and cured at 50° C. for 14 days. The laminate film was then heat-bonded under conditions of 200° C., 2 kgf, and 1 s so that the multilayer film was in contact with the laminate film, and then cut to a width of 15 mm. The peel strength was measured at 23° C., a peel speed of 100 mm / min, and a peel angle of 180°. [Method for measuring electrolyte resistance] The test piece used in the measurement of the thermal adhesive strength is immersed in an electrolyte at 85° C. for 75 hours, and then the peel strength is measured in the same manner as in the measurement of the thermal adhesive strength.
6. The polypropylene-based multilayer film according to claim 1, wherein the multilayer film does not show a tearing phenomenon in a forming test according to the following method, and peeling occurs only between the multilayer films in a thermal adhesion strength test: [Method of measuring forming performance] The laminate film was placed on a frame-shaped metal mold (10 cm x 10 cm) with the nylon surface touching the edge of the mold, and a square pyramid was used to apply pressure to the surface of the multilayer film, drawing it to a minimum depth of 6 mm five times, and the number of tears in the corners of the laminate film was counted. [Test method for thermal adhesive strength] The multilayer film (thickness 40 μm), aluminum foil (thickness 50 μm, laminated on the skin layer of the multilayer film), and nylon (thickness 15 μm, laminated on the aluminum foil) were laminated in this order, laminated at 130° C., and cured at 50° C. for 14 days. The laminate film was then heat-bonded under conditions of 200° C., 2 kgf, and 1 s so that the multilayer film was in contact with the laminate film. The laminate was then cut to a width of 15 mm, and peeled at 23° C., at a peel speed of 100 mm / min, and at a peel angle of 180°.
7. A sealant layer comprising the film according to any one of claims 1 to 6; a barrier layer formed on the sealant layer; an outer resin layer formed on the barrier layer; A material for a cell pouch comprising:
Citation Information
Patent Citations
Battery-packaging polypropylene-based resin composition and film
JP2015230777A
Exterior material for power storage device, exterior case for power storage device, and power storage device
JP2018073649A
Exterior material for power storage device and power storage device using the same
JP2018110090A
Exterior material for power storage device, outer casing for power storage device and power storage device
JP2019061938A
Polypropylene-based resin composition, and laminate and biaxially oriented polypropylene film formed from the same
JP2019163358A