Phosphors, phosphor mixtures, methods for producing phosphors, and radiation-emitting components - Patents.com
Phosphors with controlled crystal structures and compositions in the Sr1-bBa bLi3Al1-xGaxO4-yNy:Eu formula address the inefficiency of conventional phosphors by achieving narrow emission bands and improved luminous efficiency, benefiting radiation-emitting components like LEDs.
Patent Information
- Application Number
- JP2024529664
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-06
- Filing Date
- 2022-12-06
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional phosphors used in radiation-emitting components, such as LEDs, exhibit broad spectral widths and inefficient luminous performance, limiting their efficiency in converting primary radiation to secondary radiation.
Development of phosphors with the formula Sr1-bBa bLi3Al1-xGaxO4-yNy:Eu, which can crystallize in triclinic, monoclinic, or tetragonal structures, offering narrower emission bands and improved luminous efficiency due to controlled crystal structures and compositions.
The new phosphors achieve a significant reduction in full width at half maximum (FWHM) of the emission spectrum, enhancing luminous efficiency by up to 24% compared to conventional phosphors, suitable for applications in LEDs and other radiation-emitting components.
Smart Images

Figure 2024543532000016 
Figure 2024543532000017 
Figure 2024543532000018
Abstract
Description
Technical Field
[0001] Phosphors, phosphor mixtures, methods for manufacturing phosphors, and radiation-emitting components are disclosed.
Summary of the Invention
[0002] The problem of at least one embodiment is to provide a phosphor with improved properties. The problem of at least one further embodiment is to disclose a phosphor mixture with improved properties. The problem of at least one further embodiment is to disclose a method for manufacturing a phosphor with improved properties. The problem of at least one further embodiment is to disclose a radiation-emitting component with improved properties. These problems are solved by the phosphor, phosphor mixture, method, and radiation-emitting component described in the independent claims.
[0003] A phosphor is disclosed. According to at least one embodiment, the phosphor has the general formula Sr 1-b Ba b Li3Al 1-x Ga x O 4-y N y :Eu(0 ≦ b ≦ 1, 0 < x ≦ 1, and 0 ≦ y ≦ 1). In particular, 0 < y ≦ 1 may apply, for example, 0 < y ≦ 0.25.
[0004] The term "phosphor" is understood here and hereinafter to mean a wavelength-converting substance, i.e., a material configured to absorb and emit electromagnetic radiation. In particular, the phosphor absorbs electromagnetic radiation having a wavelength maximum different from the electromagnetic radiation emitted by the phosphor. For example, the phosphor absorbs radiation having a wavelength maximum at a wavelength shorter than the emission maximum, thereby emitting radiation having an emission maximum shifted towards red. In this case, pure scattering or pure absorption is not considered wavelength conversion.
[0005] Here and below, the phosphors are described by total formulas, whereby the given formula allows the phosphor to contain further elements, for example in the form of contaminants, which are present in the phosphor overall in a proportion of up to 5 mol %, in particular up to 1 mol %, preferably up to 0.1 mol %.
[0006] Phosphors consist of elements that exist in the phosphor as ions (i.e., anions or cations). Here and below, the phosphor components Sr, Ba, Li, Al, Ga, O, N, and Eu are referred to as both elements and ions (cations or anions). For clarity, the specific elements are not necessarily shown with their charge. In particular, Sr, Ba, Li, Al, Ga, and Eu exist as cations, while O and N exist as anions. Eu in particular has a double positive charge, so Eu 2+ You can also specify:
[0007] The phosphor may be nominally uncharged, meaning that there may be a perfect charge balance between positive and negative charges on the exterior of the phosphor, or on the other hand, the phosphor may be slightly less than perfectly balanced in form.
[0008] In particular, the phosphor may comprise a crystalline (eg ceramic) host material in which Eu is incorporated as an activating element. The phosphor is, for example, a ceramic material.
[0009] The activating element Eu changes the electronic structure of the host material in such a way that the phosphor can absorb electromagnetic radiation in a first wavelength range. This so-called primary radiation can excite electronic transitions in the phosphor that can return to the ground state by emitting electromagnetic radiation in a second wavelength range. This is also known as secondary radiation. The activating element introduced into the host material is therefore responsible for the wavelength conversion properties of the phosphor.
[0010] The phosphors described herein can emit secondary radiation in the yellow or yellow-green spectral range when excited by primary radiation, for example, from the blue or UV spectral range. They can therefore be used in particular in radiation-emitting components such as white-emitting LEDs (LEDs: light-emitting diodes), in which the semiconductor chip emits blue primary radiation, which is partially converted by the phosphor into secondary radiation. Alternatively, the phosphors described herein can also be used for example for full yellow or yellow / green conversion in LEDs. This is also suitable for use in displays or projectors, for example.
[0011] Conventionally used YAG (Y3Al5O 12 :Ce 3+ Compared to yellow or greenish-yellow emitting phosphors such as , the phosphors described herein have several advantages. For example, the full width at half maximum (FWHM) is smaller than the full width at half maximum of over 100 nm for YAG (typically 110 nm to 125 nm). Here and below, FWHM is understood to be the spectral width at half the height of the maximum of the emission peak or emission band. The smaller FWHM compared to the prior art allows for improved luminous efficiency, which is advantageous for most conversion applications. Improved visual efficiency compared to conventional phosphors may also result from the lower FWHM of the phosphors described herein.
[0012] Furthermore, the chromaticity coordinates of the emitted radiation in the phosphors described herein can be shifted, firstly, by changing the Al / Ga ratio and secondly, by increasing or decreasing the proportion of Sr compared to the proportion of Ba. For example, the emitted spectrum shifts to the yellow to green spectral range with increasing Ga and / or Ba content.
[0013] Furthermore, the incorporation of nitrogen into the structure of the phosphors described herein provides further stabilization, meaning, for example, that the second emission band (if present) can be suppressed, with the resulting single emission band being significantly narrower than the two superimposed bands. Emission can also be further tuned by the presence of nitrogen.
[0014] The advantages of the phosphors described herein are apparent both when used alone in a conversion element (eg, an LED) and when used in combination with other phosphors.
[0015] According to at least one embodiment, the phosphor crystallizes in a triclinic crystal structure. In particular, the phosphor has a triclinic space group
number
number
[0016] The phosphor has a triclinic space group
number
[0017] According to at least one embodiment, the phosphor crystallizes in a monoclinic crystal structure. In particular, the phosphor crystallizes in the monoclinic space group C2 / m, which can be determined, for example, by single crystal X-ray diffraction. According to at least one embodiment, the phosphor crystallizes in the monoclinic space group C2 / m, whose lattice constants have the following ranges: 1585 pm≦a≦1605 pm, 635 pm≦b≦655 pm, 790 pm≦c≦805 pm, and β is about 90°. For example, a=1596(1), b=647(1), c=797(1) pm, and β=90.00(1)°. In this embodiment, the cell volume is, for example, 0.8238(5) nm 3 It can be said that:
[0018] If the phosphor crystallizes in the monoclinic space group C2 / m, both Ga(O,N)4 and (Ga,Li)(O,N)4 tetrahedra are present, with the Ga sites potentially being occupied instead or in addition by Al. Each tetrahedron has a common edge and / or corner, and two (Ga,Li)(O,N)4 tetrahedra can also have a common edge with each other. Each tetrahedron is spanned by four oxygen atoms, or by three oxygen atoms and one nitrogen atom, or by two oxygen atoms and two nitrogen atoms, or by one oxygen atom and three nitrogen atoms, or by four nitrogen atoms. Li or Ga and / or Al are placed in the gaps of the resulting tetrahedra. Ba and / or Sr (each eight-coordinated) are placed in the respective channels formed by the tetrahedra. There are also channels free of Sr and / or Ba.
[0019] According to at least one embodiment, the phosphor crystallizes in a tetragonal crystal structure. In particular, the phosphor crystallizes in the tetragonal space group I4 / m, which can be determined, for example, by single crystal X-ray diffraction.
[0020] If the phosphor crystallizes in the tetragonal space group I4 / m, then (Li,Ga,Al)(O,N)4 tetrahedra are present, connected at the corners and / or edges. Each tetrahedron is spanned by four oxygen atoms, or by three oxygen and one nitrogen atoms, or by two oxygen and two nitrogen atoms, or by one oxygen and three nitrogen atoms, or by four nitrogen atoms. The tetrahedra form channels in which Sr or Ba atoms are located, or channels in which Ba or Ba atoms are absent.
[0021] The inventors have recognized that the phosphors described herein can be crystallized in different space groups. Thus, they can be crystallized in either the triclinic, monoclinic, or tetragonal space groups mentioned above, or a phosphor mixture or batch can be formed that contains at least two different crystallizations of the phosphor, i.e., different phases in which the phosphor exists in different crystallization states in each case. The different phases can be distinguished by powder X-ray diffraction.
[0022] According to at least one embodiment, the phosphor has an absorption spectrum with an absorption maximum in the range of 400 nm to 500 nm, in particular in the range of 400 nm to 460 nm, and therefore can be excited by blue or UV radiation and in particular emit yellow or yellow-green light upon such excitation.
[0023] According to at least one embodiment, the phosphor has an emission spectrum comprising at least one emission peak in the wavelength range of 510 nm to 580 nm. Here and below, emission peak is understood to mean the emission with the maximum intensity, whereby this can also be a local maximum. According to at least one embodiment, the emission spectrum of the phosphor has exactly one emission peak or exactly two emission peaks in the range of 510 nm to 580 nm. If two emission peaks are present, they can be superimposed to form a common emission band. The phosphor thus emits yellow or yellow-green radiation, especially when excited by radiation from the blue or UV range.
[0024] According to at least one embodiment, the emission spectrum of the phosphor has a dominant wavelength selected from the range of 540 nm to 580 nm, in particular from the range of 545 nm to 575 nm, which is used to characterize the color impression of the emitted radiation.
[0025] According to at least one embodiment, at least one emission peak has a full width at half maximum of less than 75 nm, in particular less than 60 nm, for example less than 50 nm, thereby providing a phosphor with a particularly narrowband emission, which has a significantly reduced full width at half maximum compared to conventional yellow or yellow-green emitting phosphors, and thus, for example, improved efficiency.
[0026] According to at least one embodiment, the concentration of the activator Eu in the phosphor is less than or equal to 10 mol %, in particular less than or equal to 5 mol %, such as less than or equal to 2 mol %, in particular less than or equal to 1 mol %, relative to the total content of Sr and Ba.
[0027] According to at least one embodiment, the phosphor is Sr1Li3Ga1O4:Eu, Sr1Li3Ga1O 3,75 N 0,25 :Eu, Sr1Li3Al 0,8 Ga 0,2 O 3,75 N 0,25 :Eu, Sr1Li3Al 0,8 Ga 0,2 O4: Eu, Sr 0,6 Ba 0,4 Li3Ga1O4:Eu,Sr 0,5B a 0,5 Li3Al 0,5 Ga 0,5 O 3,75 N 0,25 :Eu compositions. In the first four compositions, b=0, so there is no Ba in the phosphor. In the first, second, and fifth compositions, x=1, so there is no Al in the phosphor. In the first, fourth, and fifth compositions, y=0, so there is no N in the phosphor.
[0028] A phosphor blend is further disclosed, which in particular comprises a phosphor according to the above-mentioned embodiments, and therefore all features and embodiments disclosed in relation to the phosphor also apply to the phosphor blend and vice versa.
[0029] According to one embodiment, the phosphor mixture has the general formula Sr 1-b Ba bLi3Al 1-x Ga x O 4-y N y :Eu(0 ≤ b ≤ 1, 0 < x ≤ 1, and 0 ≤ y ≤ 1), having a triclinic crystal structure (especially the triclinic space group
Number
[0030] The phosphor mixture may contain two or three phosphors having the same composition and differing only in their crystal structure, or two or three phosphors differing in both their composition and their crystal structure. Different crystal structures, i.e., different phases formed by the phosphors in the phosphor mixture, can be distinguished from each other by powder X-ray diffraction or single-crystal X-ray diffraction even when all the phosphors in the phosphor mixture have the same composition.
[0031] For example, a phosphor crystallizing in a triclinic crystal structure can form the main phase in the phosphor mixture. When the phosphor crystallizes in a tetragonal crystal structure, it can be present as a secondary phase in the phosphor mixture at a ratio of 5 to 10% by weight. However, for this phosphor, a ratio of about 75% by weight, especially up to 65% by weight, is also considered. When the phosphor crystallizes in a monoclinic crystal structure, it can further form a secondary phase.
[0032] According to one embodiment, the phosphor mixture is a triclinic space group
Number
[0033] A method for manufacturing a phosphor is further disclosed. In particular, this method can be used to form the aforementioned phosphor or the aforementioned phosphor mixture. Therefore, all features and embodiments disclosed in relation to the phosphor or the phosphor mixture are also applicable to this method, and vice versa.
[0034] According to at least one embodiment, the method is of the general formula Sr 1-b Ba b Li3Al 1-x Ga x O 4-y N y :Eu (0 ≦ b ≦ 1, 0 < x ≦ 1, and 0 ≦ y ≦ 1) is used to prepare a phosphor.
[0035] According to at least one embodiment, the method includes preparing a mixture of reactants selected from the group consisting of oxides, nitrides, carbonates, nitrates, oxalates, citrates, and hydroxides of Sr, Ba, Li, Al, Ga, and Eu respectively, and combinations thereof, uniformly mixing the reactants, and heating the reactants to a temperature selected from the range of 600 °C to 1000 °C.
[0036] According to at least one embodiment, during heating, the temperature is selected from the range of 750 °C to 850 °C, for example 800 °C.
[0037] According to at least one embodiment, at least one of SrO, BaO, BaGa2O4, Ga2O3, Li2O, SrAl2O4, SrGa2O4, GaN, Sr3Al2N4, and Eu2O3 is selected as a reactant. For example, Li2O, SrGa2O4, SrO, and Eu2O3 are selected as reactants to produce a phosphor of composition Sr1Li3Ga1O4:Eu, and the reactants Li2O, Ga2O 3、 , GaN, SrO, and Eu2O3 have the composition Sr1Li3Ga1O 3,75 N 0,25 : The reactants Li2O, SrAl2O4, and SrGa2O were selected to produce the Eu phosphor. 4、 , Sr3Al2N4, SrO, and Eu2O3 have the composition Sr1Li3Al 0,8 Ga 0,2 O 3,75 N 0,25 The reactants SrO, Li2O, SrAl2O4, SrGa2O4, and Eu2O3 were selected to produce a phosphor of the composition Sr1Li3Al 0,8 Ga 0,2 The reactants SrO, BaO, Li2O, BaGa2O4, SrGa2O4 and Eu2O3 were selected to produce a phosphor of the composition SrO4:Eu. 0,6 Ba 0,4 The reactants SrO, BaO, Li2O, SrAl2O4, SrGa2O4, BaGa2O4, Sr3Al2N4 and Eu2O3 were selected to produce a phosphor of the composition Li3Ga1O4:Eu. 0,50 Ba 0,50 Li3Al 0,50 Ga 0,50 O 3,75 N 0,25 :Eu phosphor is selected.
[0038] According to at least one embodiment, the heating is performed in a forming gas atmosphere. According to one embodiment, the forming gas atmosphere consists of 91% N2 and 9% H2.
[0039] According to at least one embodiment, heating is carried out for a period of 2.5 hours to 6 hours, in particular 3.5 hours to 4.5 hours, for example 4 hours.
[0040] According to at least one embodiment, the heating is carried out at atmospheric pressure, which is a simplified process compared to conventional methods since it can be carried out in an energy and cost saving manner.
[0041] During heating, the reactants react to form a phosphor.
[0042] According to one embodiment, the method comprises a post-annealing step after the heating step. According to one embodiment, the post-annealing is carried out at a temperature in the range of 600° C. to 800° C. According to one embodiment, the post-annealing is carried out in an H2 atmosphere at a temperature below 600° C. The post-annealing makes it possible to suppress any green emission bands present in favor of longer wavelength emission bands in the phosphor. Furthermore, the proportion of the desired crystal structure into which the phosphor crystallizes can be increased in a targeted manner. The addition of Eu in the phosphor 3+ and Eu 2+ The proportion of can also be reduced by post-annealing.
[0043] Further disclosed is a radiation-emitting component, according to at least one embodiment, comprising a semiconductor chip that, in operation, emits electromagnetic radiation in a first wavelength range from a radiation exit surface, and a conversion element on the radiation exit surface, the conversion element comprising a phosphor as described herein for converting electromagnetic radiation in the first wavelength range to electromagnetic radiation in a second wavelength range, or comprising a phosphor blend as described herein for converting electromagnetic radiation in the first wavelength range to electromagnetic radiation in the second wavelength range.
[0044] The phosphors or phosphor blends described above are particularly suitable and intended for use in radiation-emitting components, and therefore the features and embodiments described in relation to the phosphors, phosphor blends, and / or methods for making the phosphors also apply to radiation-emitting components, and vice versa.
[0045] The electromagnetic radiation in the first wavelength range forms the emission spectrum of the semiconductor chip and is also referred to as primary radiation.
[0046] The semiconductor chip is, for example, a light-emitting diode chip or a laser diode chip. The component can therefore be a light-emitting diode (LED) or a laser. Preferably, the semiconductor chip has an epitaxially grown semiconductor layer sequence with an active zone suitable for generating electromagnetic radiation. For example, the active zone has a pn junction, a double heterostructure, a single quantum well or a multiple quantum well structure for this purpose.
[0047] In operation, the semiconductor chip can emit electromagnetic radiation, for example from the ultraviolet spectral range and / or from the visible spectral range, in particular from the blue spectral range, such that the wavelength of the primary radiation is, for example, in the range from 400 nm to 500 nm, in particular from 400 nm to 460 nm.
[0048] The conversion element is arranged on the radiation exit surface and is in particular located in the beam path of the semiconductor chip, so that at least a portion of the radiation emitted by the semiconductor chip strikes the conversion element.
[0049] The phosphor or phosphor mixture in the conversion element converts electromagnetic radiation in a first wavelength range into electromagnetic radiation in a second wavelength range, which forms the emission spectrum of the phosphor or phosphor mixture, also referred to as secondary radiation.
[0050] The electromagnetic radiation in the second wavelength range is at least partially different from the first wavelength range. The phosphor or phosphor mixture contained in or from which the conversion element is made endows the conversion element with wavelength conversion properties. For example, the conversion element only partially converts the electromagnetic radiation of the semiconductor chip into electromagnetic radiation in the second wavelength range, while a further part of the electromagnetic radiation of the semiconductor chip is transmitted by the conversion element. In this case, the radiation-emitting component emits mixed light consisting of electromagnetic radiation in the first wavelength range and electromagnetic radiation in the second wavelength range. The mixed light can be, for example, white light. If the primary radiation is completely converted by the conversion element and / or there is no transmission of the primary radiation by the conversion element, this is referred to as complete conversion. In this case, the radiation-emitting component emits the secondary radiation emitted by the conversion element, in particular from the yellow or yellow-green spectral range.
[0051] The properties of the phosphors described here, and therefore of the phosphor mixtures they contain, give the components advantages over conventional components. For example, the low full width at half maximum of the spectrum of the phosphor or phosphor mixture leads to a significant increase in luminous efficiency, which contributes to an increase in the efficiency of the component. This applies both for partial or full conversion applications, when only the phosphor or phosphor mixture is present in the conversion element, and when the phosphor or phosphor mixture is present in the conversion element together with other phosphors. In the former case, the increase in luminous efficiency corresponds directly to an efficiency increase, while in the latter case the exact magnitude of the efficiency increase also depends on the other phosphor and the mixture ratio.
[0052] According to at least one embodiment, the conversion element is free of further phosphors. In this case, only the phosphor or phosphor mixture is present in the conversion element, with an efficiency increase that directly corresponds to the luminous efficiency of the phosphor or phosphor mixture. Such a component can be used for full conversion, for example to generate yellow or yellow-green light.
[0053] According to at least one embodiment, at least one further phosphor is present in the conversion element. In particular, the further phosphor is different from the phosphor or phosphor mixture and converts electromagnetic radiation in a first wavelength range into electromagnetic radiation in a third wavelength range. According to an embodiment, the third wavelength range is at least partially different from the first and second wavelength ranges. For example, the further phosphor may emit electromagnetic radiation selected from the red spectral range or from the green spectral range. For example, the further phosphor may be selected from garnet, SCASN, (Ca,Sr,Ba)2Si5N8, or CASN. The phosphor or phosphor mixture described herein and the further phosphor thus form a phosphor mixture that converts the primary radiation in whole or in part. Such a component can be used, for example, for full or partial conversion to generate white light, with increased efficiency due to the phosphor or phosphor mixture present in the conversion element.
[0054] According to at least one embodiment, the conversion element is designed as a conversion layer. The conversion layer can be applied to the radiation exit surface of the semiconductor chip by direct or indirect contact. In the case of indirect contact, it can be applied to the radiation exit surface, for example by an adhesive layer, or a potting can be applied between the radiation exit surface and the conversion element.
[0055] According to at least one embodiment, the conversion element is designed as a rotatable phosphor wheel. In this case, the conversion element is arranged at a distance from the semiconductor chip so that it can rotate about an axis of rotation. The conversion element can be circular. In this embodiment, the semiconductor chip can be a laser diode. The component can then be referred to as a Laser Activated Remote Phosphor (LARP) system, which is particularly suitable for use in projectors and displays.
[0056] According to a further embodiment, the semiconductor chip, the conversion layer and, if applicable, also the adhesive layer can all be surrounded by the potting, for example the semiconductor chip, the conversion element and possibly also the adhesive layer are then arranged in a recess of the housing in which the potting is also arranged.
[0057] The potting may have a transmittance of at least 85%, preferably 95%, for the primary radiation and / or the secondary radiation and / or the radiation emitted by other phosphors present, and may be made, for example, from silicone or epoxy resin.
[0058] According to at least one embodiment, the phosphor or phosphor mixture in the conversion element is present as a ceramic. In such a case, the conversion layer can consist of a phosphor or phosphor mixture that forms a ceramic.
[0059] According to at least one embodiment, the phosphor or phosphor mixture in the conversion element is embedded in a matrix. In particular, the phosphor or phosphor mixture is then present in the form of particles. Any other phosphors that may be present can also be embedded in the matrix, in particular in the form of particles. According to one embodiment, the phosphor or phosphor mixture is present in the form of particles, in particular with a particle size of 500 nm to 50 μm.
[0060] The matrix may, for example, comprise a material selected from the group including polymers and glasses. The polymers may, for example, be selected from polystyrene, polysiloxane, polysilazane, PMMA, polycarbonate, polyacrylate, polytetrafluoroethylene, polyvinyl, silicone resin, silicone, epoxy resin, and transparent synthetic rubber. For example, silicates, water glass, and quartz glass may be selected as glasses.
[0061] Uses of the radiation-emitting components are also disclosed. According to an embodiment, the radiation-emitting components described herein can be used in displays, vehicle headlights, and projectors to generate white light, especially with low color rendering index (CRI).
[0062] Further advantageous and further embodiments of the components and methods can be taken from the exemplary embodiments described below in conjunction with the figures. [Brief description of the drawings]
[0063] [Figure 1] 1 is a schematic cross-sectional view of a radiation-emitting component according to an exemplary embodiment; [Diagram 2] 1 is a schematic cross-sectional view of a radiation-emitting component according to an exemplary embodiment; [Diagram 3] 1 is a crystal structure of a phosphor according to an exemplary embodiment. [Figure 4] 1 is a crystal structure of a phosphor according to an exemplary embodiment. [Figure 5A] FIG. 2 illustrates emission spectra of phosphors according to various exemplary embodiments. [Figure 5B] FIG. 2 illustrates emission spectra of phosphors according to various exemplary embodiments. [Figure 5C] FIG. 2 illustrates emission spectra of phosphors according to various exemplary embodiments. [Figure 5D] FIG. 2 illustrates emission spectra of phosphors according to various exemplary embodiments. [Figure 5E] FIG. 2 illustrates emission spectra of phosphors according to various exemplary embodiments. [Figure 5F] FIG. 2 illustrates emission spectra of phosphors according to various exemplary embodiments. [Figure 6] FIG. 2 illustrates emission spectra of phosphors according to various exemplary embodiments. [Figure 7] FIG. 2 illustrates a split emission spectrum of a phosphor according to an exemplary embodiment. [Figure 8A]FIG. 2 is a diagram showing the emission spectrum of a phosphor according to a typical embodiment in comparison with a comparative example. [Figure 8B] FIG. 2 is a diagram showing the emission spectrum of a phosphor according to a typical embodiment in comparison with a comparative example. [Figure 9] FIG. 1 shows the calculated powder diffraction pattern. [Figure 10] FIG. 2 illustrates the crystal structure of a phosphor according to an exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0064] Identical, similar or identically effective elements are provided with the same reference numbers in the figures. The figures and the proportions of the elements shown in them should not be considered to be to scale. Rather, individual elements, in particular layer thicknesses, may be shown with an exaggerated size for better visualization and / or understanding.
[0065] Figure 1 shows a schematic cross-sectional view of a radiation-emitting component according to an exemplary embodiment. The radiation-emitting component 100 comprises a semiconductor chip 10. In operation, the semiconductor chip 10 emits electromagnetic radiation in a first wavelength range (primary radiation) from a radiation exit surface 11. The semiconductor chip 10 comprises an epitaxially grown semiconductor layer sequence with an active zone 12 suitable for generating electromagnetic radiation. The wavelength of the primary radiation is, for example, in the blue and / or ultraviolet range.
[0066] Furthermore, the component comprises a conversion element 20. The conversion element 20 comprises a matrix in which the phosphor 1 (in particular particles of the phosphor 1) are embedded or the conversion element 20 comprises or consists of a ceramic formed from the phosphor 1. Alternatively, the conversion element 20 comprises a matrix in which the phosphor mixture 1' (in particular particles of the phosphor mixture 1') are embedded or the conversion element 20 comprises or consists of a ceramic formed from the phosphor mixture 1'.
[0067] The phosphor 1 or phosphor mixture 1' has the general formula Sr 1-b Bab Li3Al 1-x Ga x O 4-y N y has Eu(0 ≤ b ≤ 1, 0 < x ≤ 1, and 0 ≤ y ≤ 1). According to an embodiment, the phosphor 1 or the phosphor mixture 1' is one of the embodiments A1 to A6 shown in Table 1.
[0068]
Table 1
[0069] If the phosphor 1 is, for example, one of these embodiments or any other composition within the range of the general formula Sr 1-b Ba b Li3Al 1-x Ga x O 4-y N y :Eu(0 ≤ b ≤ 1, 0 < x ≤ 1, and 0 ≤ y ≤ 1), it crystallizes in the triclinic space group
Number
[0070] In the case of the phosphor mixture 1', it contains two or three phosphors, which may, for example, independently of each other include one of the embodiments A1 to A6 or any other composition within the range of the general formula Sr 1-b Ba b Li3Al 1-x Ga x O 4-y N y :Eu(0 ≤ b ≤ 1, 0 < x ≤ 1, and 0 ≤ y ≤ 1). Each phosphor in the phosphor mixture 1' has a different crystal structure, and as a result, two or three different crystal structures are present in the phosphor mixture 1'. The crystal structures are the triclinic space group
Number
[0071] In addition, at least one further phosphor may be present in the conversion element 20 and form a mixture of phosphors with phosphor 1 or phosphor mixture 1′ described herein.
[0072] If the conversion element 20 has a matrix in which the phosphor 1, phosphor mixture 1' or optionally a mixture of phosphors is embedded, the matrix has a material selected from polymers, such as polystyrene, polysiloxane, polysilazane, PMMA, polycarbonate, polyacrylate, polytetrafluoroethylene, polyvinyl, silicone resins, silicones, epoxy resins, and transparent synthetic rubbers, and glasses, such as silicates, water glass, and quartz glass.
[0073] In operation, the phosphor 1 or phosphor mixture 1' converts electromagnetic radiation in a first wavelength range into electromagnetic radiation in a second wavelength range (secondary radiation). In exemplary embodiments A1-A6, the secondary radiation is in the yellow to yellow-green range, in particular when excited by primary radiation in the blue or UV range. If the primary radiation is not completely converted by the conversion element, the component emits mixed light. The mixed light consists of the primary radiation, the secondary radiation and, if further phosphors are present in the conversion element 20, the emission radiation of these further phosphors. Such a component 100 emits, for example, white light.
[0074] The conversion element 20, here designated as a conversion layer, can either be applied directly to the semiconductor chip 10 or be attached to the semiconductor chip 10, for example by means of an adhesive layer (not explicitly shown here). It is also conceivable to form it as a phosphor wheel.
[0075] The semiconductor chip 10 with the conversion element 20 arranged thereon is placed in a recess in a housing 30. The housing 30 has a bevelled side towards the semiconductor chip 10 and can be reflective. The semiconductor chip 10 and the conversion element 20 can be surrounded by a potting 40 within the housing 30 as shown here, although the presence of the potting 40 is not absolutely necessary. The potting can be made, for example, from silicone or epoxy resin, and the transmittance of the active zone 12 to electromagnetic radiation is at least 85%, preferably 95%.
[0076] Alternatively, the housing 30 can be devoid of side walls and therefore of recesses and can also be designed as a carrier (not shown here).
[0077] Figure 2 shows another exemplary embodiment of a radiation-emitting component. The description given with reference to figure 1 applies to the elements having the same reference numbers. In this exemplary embodiment, the conversion element 20 is not arranged directly on the semiconductor chip 10, but is arranged at a distance therefrom, on the side of the potting 40 facing away from the semiconductor chip 10. Here again, the conversion element 20 is formed as a conversion layer.
[0078] The components shown in Figures 1 and 2 are for example LEDs. For clarity, further elements such as electrical contacts are not shown in Figures 1 and 2.
[0079] In the following, a method for producing phosphor 1 is described with reference to exemplary embodiments A1 to A6. The following description applies equally to phosphor mixture 1′, provided that phosphor mixture 1′ comprises different phosphors having the same composition but different crystal structures.
[0080] Table 2 shows the reactants A6 used in the preparation of exemplary embodiments A1-A6 and their respective weights (g). These are weights for theoretical compounds and do not necessarily correspond to the resulting final products, since they are electrically neutral.
[0081] [Table 2]
[0082] To produce the respective phosphor 1 or phosphor mixture 1', a flux can also be added to the reaction mixture, for example Li2BO4, of which 0.3 g (for exemplary embodiments A2 and A6) or 0.6 g (for exemplary embodiments A1 and A3-A5) is added to the reaction mixture.
[0083] For synthesis, a stoichiometric mixture is prepared from each reactant, mixed homogeneously and then heated at 800 °C for 4 h in a nickel crucible in a chamber furnace under forming gas atmosphere (91% N2 / 9% H2). The reactants react and the resulting product contains the respective phosphor 1 or phosphor mixture 1'.
[0084] The structure of the exemplary embodiment is characterized by single crystal X-ray diffraction. The lattice constants, crystallographic data, and basic quality parameters of the X-ray diffraction measurements of exemplary embodiment A2 are shown in Table 3. In the table, another example is shown in the right column, which can be used to show that Al and Ga can be interchanged in the general formula of the phosphor.
[0085] [Table 3]
[0086] The crystallographic location parameters of the microstructure of exemplary embodiment A2 are summarized in Table 4.
[0087] [Table 4-1] [Table 4-2]
[0088] FIG. 3 shows a schematic crystal structure of phosphor 1 having a triclinic crystal structure. The structure is isomorphous with the already known structure of Sr[LiAl3N4]:Eu (described in Pust, P. et al., Nat. Mater, 13, 891-896 (2014)). In FIG. 3, the hatched circles represent Sr or Ba, the densely hatched tetrahedrons represent LiO4 tetrahedrons, and the widely hatched tetrahedrons represent (Al,Ga)O4 tetrahedrons. Each of the tetrahedrons has a common edge and / or corner. The LiO4 tetrahedrons can also be bonded to each other through a common edge, but the GaO4 tetrahedrons cannot. Each of the tetrahedrons is spanned by four oxygen atoms, or by three oxygen atoms and one nitrogen atom, or by two oxygen atoms and two nitrogen atoms, or by one oxygen atom and three nitrogen atoms, or by four nitrogen atoms. Li, Ga or Al are placed in the gaps of the resulting tetrahedra. Sr or Ba (which are eight-coordinated) are placed in the channels formed by the tetrahedra. There are also channels that are free of them.
[0089] Table 5 shows the most significant crystallographic data from X-ray powder diffraction data for exemplary embodiments A1-A6 that crystallize in the triclinic crystal structure.
[0090] [Table 5]
[0091] Table 5 shows that different compositions were formed according to exemplary embodiments A1-A6, resulting in changes in lattice constant.
[0092] 4 shows the crystal structure along the crystal b-axis of monoclinic (Sr,Ba)(Li,Ga)Ga(O,N)Eu. The Ba and Sr layers are shown as hatched circles, the Ga(O,N) tetrahedra are broadly hatched, and the (Ga,Li)(O,N) tetrahedra are narrowly hatched. This exemplary embodiment crystallizes in the space group C2 / m with lattice parameters a=1596(1), b=647(1), c=797(1) pm, and β=90.00(1)°, and a cell volume of 0.8238(5) nm 3 Each of the tetrahedra has a common edge and / or corner, so that two (Ga,Li)(O,N)4 tetrahedra can also have a common edge with each other. Each tetrahedron is spanned by four oxygen atoms, or by three oxygen atoms and one nitrogen atom, or by two oxygen atoms and two nitrogen atoms, or by one oxygen atom and three nitrogen atoms, or by four nitrogen atoms. Li and / or Ga are placed in the gaps of the resulting tetrahedra. Ba and / or Sr (each of which is eight-coordinated) are placed in the respective channels formed by the tetrahedra. There are also empty channels that are devoid of Ba and / or Sr.
[0093] FIG. 10 shows a schematic diagram of the crystal structure of phosphor 1, which crystallizes in a tetragonal crystal structure. The circles represent Sr or Ba layers and the hatched areas represent (Li,Ga,Al)(O,N)4 tetrahedra, which are connected at the corners and edges. The tetrahedra are each spanned by four oxygen atoms, or by three oxygen atoms and one nitrogen atom, or by two oxygen atoms and two nitrogen atoms, or by one oxygen atom and three nitrogen atoms, or by four nitrogen atoms. The tetrahedra form channels in which Sr or Ba atoms are located, or channels in which Sr or Ba atoms are absent. In this embodiment, phosphor 1 crystallizes in the space group I4 / m.
[0094] Emission spectra were also recorded from exemplary embodiments A1 to A6. The respective spectra are shown in Figures 5A to 5F. Excitation was performed at 460 nm in each case.
[0095] In the spectra shown in FIGS. 5 to 8, the wavelength λ is given in nm and the intensity I is given in %.
[0096] The phosphor 1 or phosphor mixture 1′ according to exemplary embodiment A1 emits a light having a dominant wavelength λ dom = 561 nm. The full width at half maximum of the emission spectrum is extremely narrow at 49 nm (Figure 5A).
[0097] The phosphor 1 or phosphor mixture 1′ according to exemplary embodiment A2 emits a light having a dominant wavelength λ dom = 560 nm. The spectral full width at half maximum of the emission is extremely narrow at 43 nm (Figure 5B).
[0098] The phosphor 1 or phosphor mixture 1′ according to exemplary embodiment A3 emits a light having a dominant wavelength λ dom = 573 nm. The full width at half maximum of the emission spectrum is extremely narrow at 44 nm (Figure 5C).
[0099] Phosphor 1 or phosphor blend 1' according to exemplary embodiment A4 emits yellow-green light when excited by blue radiation (FIG. 5D). It consists of two individual emissions, the relative intensity of which can be adjusted by the exact synthesis conditions. The positions of the two individual emissions of exemplary embodiment 4 are shown in detail in FIG. 7, where the solid line represents the total emission, the dotted line represents the individual short-wave emission, and the dashed line represents the individual long-wave emission. The maximum emission of the short-wave single emission is about 524 nm, and the maximum emission of the long-wave single emission is about 567 nm. The individual full width at half maximum of the short-wave single emission is about 44 nm, and that of the long-wave is about 46 nm. The full width at half maximum of the entire emission band, created by overlapping the individual emissions, is 73 nm.
[0100] The phosphor 1 or phosphor blend 1′ according to exemplary embodiment A5 emits a light having a dominant wavelength λ dom = 549 nm. The emission maximum is at λ max= 538 nm (Figure 5E). At 59 nm, the spectral full width at half maximum of the emission is, for example, 12 :Ce 3+ This is 59 nm narrower than that of known yellow-green emitting garnet phosphors.
[0101] The phosphor 1 or phosphor mixture 1′ according to exemplary embodiment A6 emits a light having a dominant wavelength λ dom = 558 nm (Figure 5F). At 58 nm, the spectral full width at half maximum of the emission is 12 :Ce 3+ 58 nm narrower than that of known yellow-green emitting garnet phosphors.
[0102] Figure 6 shows all the emission spectra of the exemplary embodiment superimposed on each other. 1-b Ba b Li3Al 1-x Ga x O 4-y N y It can be seen that by varying the composition of the :Eu phosphor the exact emission position can be altered and therefore adapted to the respective application.
[0103] Phosphor 1 or phosphor blend 1' have clear advantages over previously known phosphors due to their low full width at half maximum of the spectrum. (Y,Lu)3(Al,Ga)5O 12 :Ce 3+ A commercially available garnet phosphor of type B1 will be used as a comparative example below. dom The color impression is equivalent to that of Phosphor 1 as measured by
[0104] Comparative Example B1 is compared to exemplary embodiments A1 and A4 in Table 6. Dominant wavelengths, full width at half maximum FWHM, and relative luminous efficiencies are listed.
[0105] [Table 6]
[0106] Both exemplary embodiments have a significantly lower full width at half maximum spectrum than the comparative example. In both cases, this narrower full width at half maximum results in a higher relative luminous efficiency, as shown in Table 6.
number
[0107] For example, in white light emitting diodes, the efficiency gain from phosphor 1 or phosphor blend 1' can provide a significant improvement even when used as part of a conversion solution using other phosphors in addition to phosphor 1 or phosphor blend 1', although the exact magnitude of the efficiency gain in the blend also depends on the other phosphors in the blend.
[0108] In the figures, the exemplary embodiments A1 (FIG. 8A) and A4 (FIG. 8B) are again shown in comparison with the comparative example B1 in the form of their emission spectra. The solid line represents the emission spectrum of the exemplary embodiment, and the dotted line represents the emission spectrum of the comparative example. It can be clearly seen that the full width at half maximum of the emission spectrum of the exemplary embodiment is significantly reduced compared to the comparative example.
[0109] Figure 9 shows the powder X-ray diffraction patterns calculated from the single crystal data for the monoclinic (middle diffractogram), triclinic (top diffractogram), and tetragonal (bottom diffractogram) phases. The diffraction angle 2θ is plotted in degrees against the intensity. This shows that Phosphor Mixture 1' has different crystallization phases of the phosphors, and the phases of Phosphor Mixture 1' are distinguishable from each other.
[0110] The features and exemplary embodiments described in connection with the figures can be combined with each other to produce further exemplary embodiments, even if not all combinations are explicitly described. Furthermore, the exemplary embodiments described in connection with the figures can instead or in addition have further features as described in the summary section.
[0111] The present invention is not limited to the description based on the exemplary embodiments, but rather, any novel feature and any combination of features, including in particular any combination of features in the claims, is included in the present invention even if this feature or combination itself is not explicitly recited in the claims or in the exemplary embodiments. [Explanation of symbols]
[0112] 1. Phosphor 1' Phosphor mixture 10. Semiconductor Chips 11 Radiation exit area 12 Active Zone 20 Conversion Factors 30 Housing 40 Potting 100 Radiation-emitting parts λ wavelength I strength A1 Exemplary embodiment 1 A2 Exemplary embodiment 2 A3 Exemplary embodiment 3 A4 Exemplary embodiment 4 A5 Exemplary embodiment 5 A6 Exemplary embodiment 6 B1 Comparative Example 2θ Diffraction angle
Claims
1. General formula, Sr 1-b Ba b Li 3 A 1-x G x O 4-y N y A phosphor (1) represented by the formula: Eu (0≦b≦1, 0<x≦1, and 0≦y≦1).
2. The phosphor (1) according to claim 1, which crystallizes in a triclinic crystal structure.
3. The phosphor (1) according to claim 1, which crystallizes in a monoclinic crystal structure.
4. The phosphor (1) according to claim 1, which crystallizes in a tetragonal crystal structure.
5. A phosphor (1) according to any one of claims 1 to 4, having an absorption spectrum with an absorption maximum in the range of 400 nm to 500 nm.
6. The phosphor (1) according to any one of claims 1 to 5, having an emission spectrum including at least one emission peak in a wavelength range of 510 nm to 580 nm.
7. The phosphor (1) according to claim 6, wherein the emission spectrum has a dominant wavelength selected from the range of 540 nm to 580 nm.
8. The phosphor (1) according to claim 6 or 7, wherein the at least one emission peak has a full width at half maximum of less than 75 nm.
9. The phosphor (1) according to any one of claims 1 to 8, wherein the concentration of Eu is 10 mol % or less with respect to the total content of Sr and Ba.
10. Sr 1 Li 3 Ga 1 O 4 :Eu、 Sr 1 Li 3 Ga 1 O 3,75 N 0,25 :Eu、 Sr 1 Li 3 Al 0,8 Ga 0,2 O 3,75 N 0,25 :Eu、 Sr 1 Li 3 Al 0,8 Ga 0,2 O 4 :Eu、 Sr 0,6 Ba 0,4 Li 3 Ga 1 O 4 :Eu、 Sr 0,5B a 0,5 Li 3 A 0,5 G 0,5 O 3,75 N 0,25 The phosphor (1) according to any one of claims 1 to 9, comprising any one of the compositions: ZnO, Fe, Eu.
11. General formula Sr 1-b Ba b Li 3 A 1-x G x O 4-y N y : Eu (0≦b≦1, 0<x≦1, and 0≦y≦1) and a phosphor (1) crystallizing in a triclinic crystal structure; General formula Sr 1-b Ba b Li 3 A 1-x G x O 4-y N y : Eu (0≦b≦1, 0<x≦1, and 0≦y≦1) and a phosphor (1) crystallizing in a monoclinic crystal structure; General formula Sr 1-b Ba b Li 3 A 1-x G x O 4-y N y : Eu (0≦b≦1, 0<x≦1, and 0≦y≦1) and a phosphor (1) crystallizing in a tetragonal crystal structure; A phosphor mixture (1') comprising at least two phosphors selected from the group consisting of:
12. General formula Sr 1-b Ba b Li 3 A 1-x G x O 4-y N y A method for producing a phosphor (1) having: Eu (0≦b≦1, 0<x≦1, and 0≦y≦1), comprising the steps of: providing a mixture of reactants selected from the group consisting of oxides, nitrides, carbonates, nitrates, oxalates, citrates, and hydroxides of Sr, Ba, Li, Al, and Ga, respectively, and combinations thereof; mixing the reactants uniformly; and heating the reactants to a temperature selected from the range of 600°C to 1000°C.
13. The method of claim 12, wherein the temperature is selected from the range of 750°C to 850°C.
14. Reactants: SrO, BaO, BaGa 2 O 4 , Ga 2 O 3 , Li 2 O, SrAl 2 O 4 , SrGa 2 O 4 , GaN, Sr 3 A 2 N 4 , and Eu 2 O 3 The method according to claim 12 or 13, wherein at least one of the group:
15. The method according to any one of claims 12 to 14, wherein the heating is carried out in a forming gas atmosphere.
16. The method of any one of claims 12 to 15, wherein the heating is performed for a period of from 2.5 hours to 6 hours.
17. The method according to any one of claims 12 to 16, wherein the heating is carried out at normal pressure.
18. A radiation-emitting component (100), comprising: a semiconductor chip (10) that, in operation, emits electromagnetic radiation in a first wavelength range from a radiation exit face (11); and a conversion element (20) on the radiation exit surface (11), the conversion element (20) comprising a phosphor (1) according to any one of claims 1 to 10 for converting electromagnetic radiation in the first wavelength range into electromagnetic radiation in a second wavelength range, or a phosphor mixture (1') according to claim 11 for converting electromagnetic radiation in the first wavelength range into electromagnetic radiation in a second wavelength range.
19. 20. The radiation-emitting component (100) of claim 18, which is free of further phosphors.
20. 20. The radiation-emitting component (100) according to claim 18, wherein at least one further phosphor is present in the conversion element (20).
Citation Information