Neodymium-iron-boron sintered magnet with high corrosion resistance and high magnetic properties and method for producing same
Uneven distribution of Co in the grain boundary phase of neodymium iron boron magnets addresses corrosion and magnetic property trade-offs, achieving improved corrosion resistance and magnetic properties.
Patent Information
- Application Number
- JP2024527192
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-08
- Filing Date
- 2023-09-01
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-09-01
AI Technical Summary
Neodymium iron boron magnets suffer from poor corrosion resistance and temperature stability, limiting their application range, while adding Co to improve corrosion resistance adversely affects magnetic properties.
Distribute Co unevenly in the grain boundary phase and main phase of neodymium iron boron magnets, with a higher concentration in the grain boundary phase (w1 > w2) to enhance corrosion resistance without compromising magnetic properties.
The uneven distribution of Co significantly improves corrosion resistance and maintains high magnetic properties, reducing weight loss and enhancing overall performance.
Smart Images

Figure 2024543836000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims priority to a prior application, bearing patent application number 2022110983441 and entitled "NED-IRON-BORON BASED SINTERED MAGNET HAVING HIGH CORROSION RESISTANCE AND HIGH MAGNETIC PROPERTIES AND MANUFACTURING METHOD THEREOF," filed with the State Intellectual Property Office of the People's Republic of China on September 8, 2022. The entire text of the prior application is incorporated herein by reference.
[0002] The present invention relates to the technical field of NdFeB sintered magnets, and more particularly to a neodymium-iron-boron sintered magnet having high corrosion resistance and excellent magnetic properties, and a method for producing the same. [Background technology]
[0003] Since its discovery, NdFeB material has been widely used in fields such as communications, medicine, automobiles, electronics, and aviation due to its excellent magnetic properties and high cost performance, making it an ideal material for manufacturing magnetic functional materials with high efficacy, small volume and light weight, and has had a revolutionary impact on many application fields. However, NdFeB material has poor temperature stability, and at the same time, the main components of NdFeB material contain relatively large amounts of rare earth elements, so that NdFeB material has relatively poor corrosion resistance. These two problems greatly limit the expansion of its application range.
[0004] In the prior art, in order to improve the corrosion resistance of NdFeB materials, element Co is usually added to the NdFeB materials, and the more the amount of element Co added, the better the corrosion resistance of the NdFeB materials. However, when the amount of element Co added is increased to 3 wt% or more, it affects the magnetic properties of the NdFeB materials. Therefore, it is ultimately impossible to improve the corrosion resistance of the NdFeB materials by adding element Co while maintaining the high magnetic properties of the NdFeB materials. Summary of the Invention
[0005] The inventor of the present invention has studied the above problem in detail and found that after adding element Co to a NdFeB magnet, most of the element Co is distributed in the main phase of the crystal grains, and a small part of the element Co is distributed in the grain boundary phase of the crystal grains. The element Co distributed in the grain boundary phase of the crystal grains plays a major role in improving the corrosion resistance and magnetic properties of the NdFeB magnet. However, when the content of element Co in the grain boundary phase increases with continued addition of element Co, a phenomenon has appeared in which the magnetic properties of the NdFeB magnet deteriorate. As a result of analysis, the inventor believes that this phenomenon occurs because the content of element Co in the grain boundary phase of the crystal grains increases with the continuous addition of element Co, and the content of element Co in the main phase of the crystal grains further increases, causing the magnetic properties of the NdFeB magnet to deteriorate.
[0006] In order to improve the defects of the prior art, the present invention provides a neodymium-iron-boron based sintered magnet with high corrosion resistance and high magnetic properties and a manufacturing method thereof, in which the neodymium-iron-boron based sintered magnet contains 1.5 wt% to 3.0 wt% of element Co, the element Co being distributed in the grain boundary phase of the crystal grains and the main phase of the crystal grains, and the content of the element Co distributed in the grain boundary phase of the crystal grains is equal to or greater than the content of the element Co distributed in the main phase of the crystal grains. In the neodymium-iron-boron based sintered magnet, the element Co is mainly concentrated in the grain boundary phase, so that the corrosion resistance and magnetic properties of the neodymium-iron-boron based sintered magnet can be significantly improved.
[0007] The technical solution of the present invention is as follows: A neodymium iron boron based sintered magnet, comprising 1.5 wt% to 3.0 wt% of the element Co, the neodymium iron boron based sintered magnet including a main phase and a grain boundary phase, the element Co being distributed in the grain boundary phase of the crystal grains and the main phase of the crystal grains, the neodymium iron boron based sintered magnet satisfying w1≧w2, where w1 is the content of the element Co distributed in the grain boundary phase of the crystal grains and w2 is the content of the element Co distributed in the main phase of the crystal grains.
[0008] In the present invention, unless otherwise specified, the above contents all refer to contents in mass percentage.
[0009] According to an embodiment of the present invention, the content w1 of the element Co distributed in the grain boundary phase of the crystal grains is greater than the average content of the element Co in a NdFeB-based sintered magnet. The content w2 of the element Co distributed in the main phase of the crystal grains is less than the average content of the element Co in a NdFeB-based sintered magnet.
[0010] According to an embodiment of the present invention, the above-mentioned neodymium iron boron based sintered magnet satisfies w1≧1.5×w2, where w1 is the content of the element Co distributed in the grain boundary phase of the crystal grains, and w2 is the content of the element Co distributed in the main phase of the crystal grains.
[0011] According to an embodiment of the present invention, the distribution of the element Co in the main phase and grain boundary phase at any position (eg, surface and center) of the above-mentioned neodymium iron boron based sintered magnet satisfies w1≧w2, and preferably satisfies w1≧1.5×w2.
[0012] According to an embodiment of the present invention, in the neodymium-iron-boron based sintered magnet, the Co-enriched regions and the heavy rare earth-enriched regions of the grain boundary phase incompletely overlap each other.
[0013] According to an embodiment of the present invention, in the neodymium-iron-boron based sintered magnet, the Co-enriched regions of the grain boundary phase are Fe-deficient regions.
[0014] According to an embodiment of the present invention, in the neodymium-iron-boron-based sintered magnet, the grain boundary phase includes a phase composed of RFeCoM, where R is a rare earth element, Fe is iron, Co is cobalt, and M is one or more of Ga, Cu, Al, Zr, and Ti.
[0015] According to an embodiment of the present invention, in the neodymium-iron-boron based sintered magnet, the content of the R element in the grain boundary phase is equal to or greater than the content of the R element in the main phase.
[0016] According to an embodiment of the present invention, in the neodymium-iron-boron based sintered magnet, the content of the M element in the grain boundary phase is equal to or greater than the content of the M element in the main phase.
[0017] According to an embodiment of the present invention, in the neodymium-iron-boron based sintered magnet, the Fe element content in the grain boundary phase is equal to or less than the Fe element content in the main phase.
[0018] According to an embodiment of the present invention, the NdFeB based sintered magnet contains 1.5 wt%, 1.6 wt%, 1.7 wt%, 1.8 wt%, 1.9 wt%, 2.0 wt%, 2.1 wt%, 2.2 wt%, 2.3 wt%, 2.4 wt%, 2.5 wt%, 2.6 wt%, 2.7 wt%, 2.8 wt%, 2.9 wt%, or 3.0 wt% content of the element Co.
[0019] According to an embodiment of the present invention, the chemical formula of the neodymium iron boron based sintered magnet is RFeCoBM, in which R is a rare earth element, Fe is iron, B is boron, and M is one or more of Ga, Cu, Al, Zr, and Ti, in which the R content is 26 wt% to 35 wt%, the B content is 0.8 wt% to 1.3 wt%, the Co content is 1.5 wt% to 3.0 wt%, the Ga content is 0.05 wt% to 0.5 wt%, the Cu content is 0.05 wt% to 0.6 wt%, the Al content is 0 wt% to 1.5 wt%, the Zr content is 0 wt% to 0.5 wt%, the Ti content is 0 wt% to 0.5 wt%, and the remainder is iron and unavoidable impurities.
[0020] According to an embodiment of the present invention, R is a rare earth element, such as at least one of lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), yttrium (Y), and scandium (Sc).
[0021] According to an embodiment of the present invention, in the neodymium iron boron based sintered magnet, the C element content is ≦800 ppm, the O element content is ≦800 ppm, and the N element content is ≦800 ppm.
[0022] According to an embodiment of the present invention, the crystal grain size of the neodymium-iron-boron sintered magnet is ≦8 μm.
[0023] The present invention further provides a method for producing the above-mentioned neodymium-iron-boron based sintered magnet, 1) obtaining R-Fe-Co-BM alloy fine powder by stripping-hydrogen crushing; 2) jet milling the R-Fe-Co-BM alloy fine powder of step 1) to obtain a magnetic powder, and then pressing the magnetic powder into a green compact; 3) sintering the green compact of step 2), optionally with or without aging treatment, to obtain a sintered magnet; 4) processing the sintered magnet of step 3) into a required size, arranging a diffusion source on the surface of the processed product, and then heating the product under vacuum conditions. When the heating temperature reaches the diffusion treatment temperature, inert gas is filled in, and the product is kept warm and then cooled to room temperature. 5) performing an aging treatment on the magnet after the diffusion treatment in step 4) to produce and obtain the neodymium-iron-boron based sintered magnet.
[0024] According to an embodiment of the present invention, in step 1), the R content is 26 wt% to 35 wt%, the B content is 0.8 wt% to 1.3 wt%, the Co content is 1.5 wt% to 3.0 wt%, and M is one or more of Ga, Cu, Al, Zr, and Ti, in which the Ga content is 0.05 wt% to 0.5 wt%, the Cu content is 0.05 wt% to 0.6 wt%, the Al content is 0 wt% to 1.5 wt%, the Zr content is 0 wt% to 0.5 wt%, the Ti content is 0 wt% to 0.5 wt%, and the remainder is iron and unavoidable impurities.
[0025] According to an embodiment of the present invention, in step 1), R is a rare earth element, and illustratively, R is at least one of lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), yttrium (Y), and scandium (Sc).
[0026] According to an embodiment of the present invention, in step (2), the average particle size of the magnetic powder is 2 μm to 5 μm.
[0027] According to an embodiment of the present invention, in step 2), the magnetic powder after jet milling polishing is mixed with a lubricant accounting for 0.1 wt% to 0.5 wt% of the total mass of the magnetic powder after jet milling polishing for 0.1 h to 3 h, and then the magnetic powder is pressed into a green compact in an orienting field environment at 20°C to 40°C and with a magnetic field strength of 1 T to 5 T.
[0028] According to an embodiment of the present invention, in step 3), the green compact of step 2) is sintered to obtain a sintered magnet, or the green compact of step 2) is first sintered and then aged to obtain a sintered magnet.
[0029] According to an embodiment of the present invention, in step 3), the sintered material is cooled to room temperature and then subjected to an aging treatment.
[0030] According to an embodiment of the present invention, in step 3), the sintering temperature is 900°C-1100°C (e.g., 900°C, 950°C, 1000°C, 1050°C or 1100°C), and the sintering time is 2h-10h (e.g., 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h). The sintering is performed under vacuum conditions, and the degree of vacuum is ≦20 Pa.
[0031] According to an embodiment of the present invention, in step 3), the aging treatment is a secondary aging treatment including a first stage aging treatment and a second stage aging treatment, in which the temperature of the first stage aging treatment is 700 to 950°C (for example, 700°C, 750°C, 800°C, 850°C, 900°C or 950°C), the time of the first stage aging treatment is 1 to 12 h (for example, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h or 12 h), the temperature of the second stage aging treatment is 400 to 600°C (for example, 400°C, 450°C, 500°C, 550°C or 600°C), and the time of the second stage aging treatment is 1 to 12 h (for example, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h or 12 h). h).
[0032] According to an embodiment of the present invention, in step 3), the raw material after the first stage aging treatment is cooled to room temperature, and then the second stage aging treatment is performed; According to an embodiment of the present invention, in step 4), the diffusion source is a rare earth element source, illustratively at least one of a Dy source (e.g., metallic Dy), a Tb source (e.g., metallic Tb), a Ho source (e.g., metallic Ho), a Nd source (e.g., metallic Nd), and a Pr source (e.g., metallic Pr).
[0033] According to an embodiment of the present invention, in step 4), the mass of the diffusion source is 0.2% to 1.5% of the total mass of the sintered magnet, for example, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4% or 1.5%.
[0034] According to an embodiment of the present invention, in step 4), the disposing method may be at least one of a thermal spraying method, a coating method, a sputtering method, a dipping method, and the like.
[0035] According to an embodiment of the present invention, in step 4), the vacuum condition has a vacuum degree of ≦20 Pa, for example, 1 Pa to 20 Pa, for example, 1 Pa, 2 Pa, 5 Pa, 8 Pa, 10 Pa, 12 Pa, 15 Pa, 18 Pa or 20 Pa.
[0036] According to an embodiment of the present invention, in step 4), the temperature of the diffusion treatment is 800 to 1000°C, for example, 800°C, 850°C, 900°C, 950°C, or 1000°C.
[0037] According to an embodiment of the present invention, in step 4), when the heating temperature is increased to the temperature of the diffusion treatment, an inert gas of 5 kPa or more is filled, preferably an inert gas of 10 kPa to 30 kPa is filled, for example, an inert gas of 10 kPa, 15 kPa, 20 kPa, 25 kPa, or 30 kPa is filled.
[0038] According to an embodiment of the present invention, in step 4), the inert gas atmosphere is, for example, at least one of argon gas, helium gas, and nitrogen gas.
[0039] According to an embodiment of the present invention, in step 4), the incubation time is 3 h or more, for example, 3 to 24 h, for example, 3 h, 6 h, 8 h, 9 h, 10 h, 12 h, 15 h, 18 h, 20 h, 22 h, or 24 h.
[0040] According to an embodiment of the present invention, step 4) further includes the steps of cleaning, degreasing and pickling the processed sintered magnet.
[0041] According to an embodiment of the present invention, in step 5), the temperature of the aging treatment is 400 to 600°C (e.g., 400°C, 450°C, 500°C, 550°C, or 600°C), and the time of the aging treatment is 1 to 12 h (e.g., 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, or 12 h).
[0042] According to an embodiment of the present invention, the method includes the following steps: a) Obtain R-Fe-Co-BM alloy fine powder by stripping-hydrogen crushing, in which R is a rare earth element, the R content is 26 wt%-35 wt%, the B content is 0.8 wt%-1.3 wt%, the Co content is 1.5 wt%-3.0 wt%, and M is one or more of Ga, Cu, Al, Zr, and Ti, in which Ga content is 0.05 wt%-0.5 wt%, Cu content is 0.05 wt%-0.6 wt%, Al content is 0 wt%-1.5 wt%, Zr content is 0 wt%-0.5 wt%, Ti content is 0 wt%-0.5 wt%, and the balance is iron and unavoidable impurities.
[0043] b) The R-Fe-Co-BM alloy fine powder of step a) is jet milled to obtain a magnetic powder, and the average particle size of the magnetic powder is 2-5 μm. A lubricant is added to the magnetic powder after jet milling, the lubricant accounting for 0.1 wt%-0.5 wt% of the total mass of the magnetic powder after jet milling, and then the material is mixed for 0.1 h-3 h. Then, the magnetic powder is pressed into a green compact.
[0044] c) Sintering the green compact of step b) under vacuum conditions, the sintering temperature is 900-1100°C, the sintering time is 2-10°C, and the sintering time is 2-10 h to obtain a sintered magnet.
[0045] d) subjecting the sintered magnet of step c) to a secondary aging treatment, in which the first stage aging treatment temperature is 700-950°C and the second stage aging treatment temperature is 400-600°C.
[0046] e) The magnet of step c) or step d) is processed into a required size, the processed product is treated by cleaning, degreasing and pickling, and a diffusion source which is a rare earth element source is arranged on the surface of the treated product, and the arrangement method can be a thermal spraying method, a coating method, a sputtering method or a dipping method. Then, the product is heated under vacuum conditions, and when the heating temperature is increased to the temperature of the diffusion treatment, an inert gas is filled, and after keeping the temperature, it is cooled to room temperature, and the temperature of the diffusion treatment is 800-1000°C, and the keeping time is 3 hours or more.
[0047] f) The magnet after the diffusion treatment in step e) is subjected to an aging treatment, and the aging temperature is 400 to 600°C. Beneficial Effects of the Invention: The present invention provides a NdFeB based sintered magnet with high corrosion resistance and high magnetic properties, and a manufacturing method thereof, the NdFeB based sintered magnet containing the element Co, the NdFeB based sintered magnet containing a main phase and a grain boundary phase, the Co element being distributed in the grain boundary phase of crystal grains and the main phase of the crystal grains, the NdFeB based sintered magnet satisfying w1≧w2, where w1 is the content of the Co element distributed in the grain boundary phase of the crystal grains, and w2 is the content of the Co element distributed in the main phase of the crystal grains.
[0048] NdFeB magnets mainly include a main phase and a grain boundary phase, and there is a potential difference between the main phase and the grain boundary phase, so electrochemical corrosion occurs. Since the grain boundary phase is a Nd-rich phase, its electrode potential is even lower, and electrochemical corrosion occurs preferentially. The inventors of the present invention have surprisingly found that by concentrating the element Co in the grain boundary phase, the element Co can form a Nd-rich phase and a Nd3Co phase, and the formation of the Nd3Co phase improves the electrode potential of the entire grain boundary phase, reduces the degree of electrochemical corrosion, greatly reduces the weight loss of the magnet, significantly improves the corrosion resistance of the NdFeB magnet, and also significantly improves the magnetic properties of the NdFeB magnet, so that the corrosion resistance and magnetic properties of the NdFeB magnet can be achieved at the same time.
[0049] In the manufacturing method of the present invention, a sintered magnet is obtained by smelting, milling, press molding, and sintering processes, and the sintered magnet is then processed to the required size, and a diffusion source is then placed on the surface. The sintered magnet is then heated under vacuum conditions, and when the heating temperature reaches the temperature for the diffusion process, an inert gas is filled in, the magnet is kept warm, and then the magnet is cooled to room temperature, thereby obtaining a NdFeB-based sintered magnet in which the content of the element Co in the grain boundary phase of the crystal grains is equal to or greater than the content of the element Co distributed in the main phase of the crystal grains. The inventors speculate that this is because, in the diffusion process under specific conditions, the diffusion source can enter the grain boundary phase, and element migration occurs between the diffusing element that has entered the grain boundary phase and the element Co in the main phase, causing the element Co in the main phase to migrate to the grain boundary phase. [Brief description of the drawings]
[0050] [Figure 1] 4 is an element distribution diagram after scanning a neodymium-iron-boron sintered magnet in Comparative Example 1 using an EPMA. FIG. [Diagram 2] FIG. 2 is an element distribution diagram after scanning the neodymium-iron-boron sintered magnet in Example 1 using an EPMA. [Diagram 3] FIG. 2 is a graph showing changes in the content of the element Co after a neodymium-iron-boron sintered magnet in Comparative Example 1 is scanned with an EPMA. [Figure 4] FIG. 2 is a graph showing changes in the content of the element Co after scanning the neodymium-iron-boron sintered magnet using an EPMA in Example 1. [Diagram 5] FIG. 1 is a structural diagram of a neodymium-iron-boron sintered magnet according to the present invention. [Figure 6] 1 is a flowchart for producing a neodymium-iron-boron sintered magnet according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0051] The present invention will be described in more detail with reference to the following specific examples. It should be understood that the following examples are merely illustrative and interpretative of the present invention and should not be interpreted as limiting the scope of the claims of the present invention. Any technology realized based on the above content of the present invention is included in the scope of the claims of the present invention.
[0052] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the reagents, materials, etc. used in the following examples are all commercially available, unless otherwise specified. Example 1 (1) NdPr, Dy, Co, Al, Fe, Cu, Ga, Ti and ferroboron with a purity of at least 99% by weight were melted in an argon gas atmosphere by high frequency induction, and the melt was then driven into a quench roll to produce an alloy with a mass percentage of 30.5% NdPr, 0.5% Dy, 1.5% Co, 0.1% Al, 0.2% Cu, 0.2% Ga, 0.18% Ti, 0.98% B, and the balance being iron and unavoidable impurities. The alloy was hydrogenated and pulverized into coarse powder, which was then jet milled and polished, and the particle size D50 of the resulting magnetic powder was 4.0 μm. After adding a lubricant of 0.3 wt% of the total mass of the jet milled powder to the jet milled powder, the materials were mixed for 2 h and pressed into a green compact at room temperature and in an orientation field environment with a magnetic field strength of 2 T. The billet was then placed in a vacuum sintering furnace and sintered at 1070°C for 6 hours. After the end of the warming, it was cooled to room temperature, then heated to 900°C, and subjected to a first stage aging treatment at 900°C for 3 hours. After the end of the warming, it was cooled to room temperature, then heated to 520°C, and subjected to a second stage aging treatment at 520°C for 5 hours. After cooling and removing from the furnace, a neodymium iron boron magnet was obtained.
[0053] (2) The magnet was processed into a square sheet with a size of 25-15-5 mm, and the square sheet was degreased and pickled, and then Tb diffusion treatment was performed in a vacuum state (<20 Pa). The diffusion temperature was 900°C. When the temperature reached 900°C, argon gas of 15 kPa was filled and kept at room temperature for 3 h. After the temperature was kept at room temperature, the magnet was cooled to room temperature, and then heated to 480°C. Ageing treatment was performed at 480°C for 3 h. The amount of Tb diffusion was 0.6 wt% of the total mass of the square sheet magnet with a size of 25-15-5 mm. The diffusion source (metal Tb) in this embodiment was arranged using a thermal spraying method, and the product after the diffusion treatment was called A1. The magnetic properties and weight loss measurements were performed on the product, and the weight loss conditions were a temperature of 121°C, humidity of 100%, pressure of 2.0 Bar, and treatment time of 4 days. Comparative Example 1 The other steps were the same as in Example 1, except that 1.0% Co was added in step (1). After the diffusion treatment in step (2), the product was called B1.
[0054] [Table 1]
[0055] As can be seen from Table 1, Example 1 has the same performance as Comparative Example 1, but the weight loss of the product of Example 1 is smaller, and the overall performance of the product is also better.
[0056] Furthermore, the product A1 of Example 1 and the product B1 of Comparative Example 1 were processed into products of 10-10-5 mm, and 5 mm was the magnetization direction of the product. After grinding and polishing by 0.05 mm along the magnetization direction, a wide surface of 10-10 mm was scanned using EPMA. The structure and composition of the main phase and the grain boundary phase were observed by scanning, among which FIG. 1 is an element distribution diagram after scanning the neodymium iron boron sintered magnet using EPMA in Comparative Example 1. FIG. 2 is an element distribution diagram after scanning the neodymium iron boron sintered magnet using EPMA in Example 1. FIG. 3 is a diagram of the content change of element Co after scanning the neodymium iron boron sintered magnet using EPMA in Comparative Example 1. FIG. 4 is a diagram of the content change of element Co after scanning the neodymium iron boron sintered magnet using EPMA in Example 1.
[0057] 1 and 3, it can be seen that the element Co is distributed in the grain boundary phase of the crystal grains and the main phase of the crystal grains, and the content of the element Co distributed in the grain boundary phase of the crystal grains is less than the content of the element Co distributed in the main phase of the crystal grains. On the other hand, it can be seen from Fig. 2 and Fig. 4 that the element Co is also distributed in the grain boundary phase of the crystal grains and the main phase of the crystal grains, but the content of the element Co distributed in the grain boundary phase of the crystal grains is greater than the content of the element Co distributed in the main phase of the crystal grains. It can also be seen that the content of the element Co in the grain boundary phase is about twice the content of the element Co in the main phase of the crystal grains.
[0058] [Table 2]
[0059] In summary, based on a comparison between Example 1 and Comparative Example 1, it is clear that if the content of the element Co is not in the range of 1.5 wt% to 3.0 wt%, it is impossible to produce a NdFeB-based sintered magnet having the specific grain boundary structure of the present invention, and that the corrosion resistance of the NdFeB-based sintered magnet can be guaranteed only by ensuring sufficient distribution of the element Co in the grain boundary phase of the crystal grains of the NdFeB-based sintered magnet. Example 2 (1) NdPr, Co, Al, Fe, Cu, Ga, Ti and ferroboron with a purity of at least 99% by weight were high-frequency melted in an argon gas atmosphere, and the melt was then driven into a quench roll to produce an alloy with a mass percentage of 30.8% NdPr, 1.5% Co, 0.2% Al, 0.15% Cu, 0.15% Ga, 0.2% Ti, 0.98% B, and the balance being iron and unavoidable impurities. The alloy was hydrogenated and pulverized into coarse powder, which was then jet milled and polished, and the particle size D50 of the resulting magnetic powder was 3.7 μm. After adding a lubricant that accounted for 0.4 wt% of the total mass of the jet milled powder to the jet milled powder, the materials were mixed for 2 h and pressed into a green compact under an environment of room temperature and an orientation field with a magnetic field strength of 2 T. The billet was then placed in a vacuum sintering furnace and sintered at 1065 °C for 6 h. After the end of the heat-holding, the magnet was cooled to room temperature, then heated to 800°C, and subjected to a first-stage aging treatment at 800°C for 3 hours. After the end of the heat-holding, the magnet was cooled to room temperature, then heated to 500°C, and subjected to a second-stage aging treatment at 500°C for 5 hours. After cooling and removing from the furnace, a neodymium iron boron magnet was obtained.
[0060] (2) The magnet was processed into a square sheet with a size of 25-15-2.5 mm, and the square sheet was degreased and pickled, and then Dy diffusion treatment was performed in a vacuum state (<20 Pa). The diffusion temperature was 880°C. When the temperature reached 880°C, argon gas of 20 kPa was filled and kept at room temperature for 3 h. After the temperature was kept at room temperature, the magnet was cooled to room temperature, and then heated to 500°C. Ageing treatment was performed at 500°C for 3 h. The amount of Dy diffusion was 0.8 wt% of the total mass of the square sheet magnet with a size of 25-15-2.5 mm. The diffusion source (metallic Dy) in this embodiment was arranged using a coating method, and the product after the diffusion treatment was called A2. The magnetic properties and weight loss measurements were performed on the product, and the weight loss conditions were temperature 121°C, humidity 100%, pressure 2.0 Bar, and treatment time 4 days. Comparative Example 2 The other steps were the same as in Example 2, except that 3.5% Co was added in step (1). After the diffusion treatment in step (2), the product was called B2.
[0061] [Table 3]
[0062] As can be seen from Table 3, compared to Comparative Example 2, the weight loss of Example 2 is comparable, but the magnetic properties of Example 2 are even better. This is mainly because the magnets manufactured by the methods of Example 2 and Comparative Example 2 can ensure sufficient distribution of element Co in the grain boundary phase, thereby improving the corrosion resistance of the product. However, in Comparative Example 2, the amount of element Co added is too much, which affects the magnetic properties of the magnet and causes a deterioration of the overall performance of the product. Example 3 (1) Nd, Co, Al, Fe, Cu, Ga, Zr and ferroboron with a purity of at least 99% by weight were high-frequency melted in an argon gas atmosphere, and the melt was then driven into a quench roll to produce an alloy with a mass percentage of 31.5% Nd, 1.8% Co, 0.15% Al, 0.10% Cu, 0.15% Ga, 0.15% Zr, 0.98% B, and the balance being iron and unavoidable impurities. The alloy was hydrogenated and pulverized into coarse powder, which was then jet milled and polished, and the particle size D50 of the resulting magnetic powder was 4.8 μm. After adding a lubricant that accounted for 0.2 wt% of the total mass of the jet milled powder to the jet milled powder, the materials were mixed for 2 h and pressed into a green compact under an environment of room temperature and an orientation field with a magnetic field strength of 2 T. The billet was then placed in a vacuum sintering furnace and sintered at 1085 °C for 6 h. After the end of the heat-holding, the magnet was cooled to room temperature, then heated to 900°C, and subjected to a first-stage aging treatment at 900°C for 3 hours. After the end of the heat-holding, the magnet was cooled to room temperature, then heated to 480°C, and subjected to a second-stage aging treatment at 480°C for 5 hours. After cooling and removing from the furnace, a neodymium iron boron magnet was obtained.
[0063] (2) The magnet was processed into a square sheet with a size of 40-10-4 mm, and the square sheet was degreased and pickled, and then Tb diffusion treatment was performed in a vacuum state (<20 Pa). The diffusion temperature was 920°C. When the temperature reached 920°C, argon gas of 25 kPa was filled and kept at room temperature for 3 h. After the temperature was kept at room temperature, the magnet was cooled to room temperature, and then heated to 510°C. Ageing treatment was performed at 510°C for 3 h. The amount of Tb diffusion was 0.8 wt% of the total mass of the square sheet magnet with a size of 40-10-4 mm. The diffusion source (metallic Tb) in this embodiment was arranged using a coating method, and the product after the diffusion treatment was called A3. The magnetic properties and weight loss measurements were performed on the product, and the weight loss conditions were temperature 121°C, humidity 100%, pressure 2.0 Bar, and treatment time 4 days. Comparative Example 3 The other steps were the same as in Example 3, with the only difference being that magnetic property measurements and weight loss measurements were performed on the NdFeB magnet B3 obtained after cooling and removing from the furnace in step (1) (i.e., without diffusion treatment).
[0064] [Table 4]
[0065] As can be seen from Table 4, the corrosion resistance and magnetic properties of Example 3 are better than those of Comparative Example 3. Although the same amount of element Co was added during smelting in both Example 3 and Comparative Example 3, Comparative Example 3, which does not undergo the method of the present invention, cannot ensure that element Co is sufficiently distributed in the grain boundary phase, which will affect the corrosion resistance of the product. The magnet of Example 3 underwent further diffusion treatment, which further improved the magnetic properties of the magnet. Example 4-1 (1) Nd, Co, Al, Fe, Cu, Ga, Ti and ferroboron with a purity of at least 99% by weight were high-frequency melted in an argon gas atmosphere, and the melt was then driven into a quench roll to produce an alloy with a mass percentage of 32% Nd, 1.5% Co, 0.35% Al, 0.15% Cu, 0.10% Ga, 0.15% Ti, 0.98% B, and the balance being iron and unavoidable impurities. The alloy was hydrogenated and pulverized into coarse powder, which was then jet milled and polished, and the particle size D50 of the resulting magnetic powder was 4.5 μm. After adding a lubricant that accounted for 0.4 wt% of the total mass of the jet milled powder to the jet milled powder, the materials were mixed for 2 h and pressed into a green compact at room temperature and in an orientation field environment with a magnetic field strength of 2 T. The billet was then placed in a vacuum sintering furnace and sintered at 1080 °C for 6 h. After the end of the heat-holding, the magnet was cooled to room temperature, then heated to 850°C, and subjected to a first-stage aging treatment at 850°C for 3 hours. After the end of the heat-holding, the magnet was cooled to room temperature, then heated to 510°C, and subjected to a second-stage aging treatment at 510°C for 5 hours. After cooling and removing from the furnace, a neodymium iron boron magnet was obtained.
[0066] (2) The magnet was processed into a square sheet with a size of 38-23-6 mm, and the square sheet was degreased and pickled, and then Dy diffusion treatment was performed in a vacuum state (<20 Pa). The diffusion temperature was 890°C. When the temperature reached 890°C, argon gas of 30 kPa was filled and kept at room temperature for 3 h. After the temperature was kept at room temperature, the magnet was cooled to room temperature, and then heated to 550°C. Ageing treatment was performed at 550°C for 3 h. The amount of Dy diffusion was 0.7 wt% of the total mass of the square sheet magnet with a size of 38-23-6 mm. The diffusion source (metallic Dy) in this embodiment was arranged using the immersion method, and the product after the diffusion treatment was called A4-1. The magnetic properties and weight loss measurements were performed on the product, and the weight loss conditions were temperature 121°C, humidity 100%, pressure 2.0 Bar, and treatment time 4 days. Example 4-2 The other steps are the same as in Example 4-1, with only step (2) being different: (2) The magnet was processed into a square sheet with a size of 38-23-6 mm, and the square sheet was degreased and pickled, and then Dy diffusion treatment was performed in a vacuum state (<20 Pa). The diffusion temperature was 890°C. When the temperature reached 890°C, argon gas of 5 kPa was filled and kept at room temperature for 3 h. After the temperature was kept at room temperature, the magnet was cooled to room temperature, and then heated to 550°C. Ageing treatment was performed at 550°C for 3 h. The amount of Dy diffusion was 0.7 wt% of the total mass of the square sheet magnet with a size of 38-23-6 mm. The diffusion source (metallic Dy) in this embodiment was arranged using the immersion method, and the product after the diffusion treatment was called A4-2. The magnetic properties and weight loss measurements were performed on the product, and the weight loss conditions were temperature 121°C, humidity 100%, pressure 2.0 Bar, and treatment time 4 days. Comparative Example 4 The other steps are the same as in Example 4-1, with only step (2) being different: (2) The magnet was processed into a square sheet with a size of 38-23-6 mm, and the square sheet was degreased and pickled, and then Dy diffusion treatment was performed in a vacuum state (<20 Pa). The diffusion temperature was 890°C, and when the temperature reached 890°C, it was kept at 3 h, cooled after the temperature was kept at 100°C, and aging treatment was performed at 550°C after the cooling, for 3 h. The amount of Dy diffusion was 0.7 wt% of the total mass of the square sheet magnet with a size of 38-23-6 mm, and the diffusion source (metallic Dy) in this comparative example was placed using the immersion method, and the product after the diffusion treatment was called B4. The magnetic properties and weight loss measurements were performed on the product, and the weight loss conditions were temperature 121°C, humidity 100%, pressure 2.0 Bar, and treatment time 4 days.
[0067] [Table 5]
[0068] Product A4-1 of Example 4-1, product A4-2 of Example 4-2, and product B4 of Comparative Example 4 were processed into products of 10-10-6 mm, with 6 mm being the magnetization direction of the product. After grinding and polishing by 0.2 mm along the magnetization direction, a wide surface of 10-10 mm was scanned using an EPMA. The structure and composition of the main phase and grain boundary phase were observed by scanning, and the measurement results are shown in Table 6.
[0069] [Table 6]
[0070] From Tables 5 and 6, it can be seen that, compared with Example 4-2, all the neodymium iron boron sintered magnets of Example 4-1 satisfy w1 ≧ w2, which can improve the corrosion resistance of the product, but Example 4-1 has higher magnetic properties and better corrosion resistance. This is mainly because the magnet obtained by the method of Example 4-1 can ensure sufficient distribution of element Co in the grain boundary phase, and a neodymium iron boron sintered magnet that satisfies w1 ≧ 1.5 × w2 can be obtained, thereby effectively improving the corrosion resistance of the product. At the same time, the diffusion process of heavy rare earth is guaranteed, and the magnetic properties of the product are further improved. In addition, the magnet produced by the method of Example 4-2 also has distribution of element Co in the grain boundary phase, but the method of Example 4-2 cannot ensure sufficient distribution of element Co in the grain boundary phase (i.e., cannot satisfy w1 ≧ 1.5 × w2), and as a result, the degree of improvement in the corrosion resistance of the product is insufficient. In Comparative Example 4, a method of direct diffusion was adopted without filling argon gas, and therefore a product in which the grain boundary phase was enriched with the element Co was not obtained.
[0071] Furthermore, a comparison of Example 4-1, Example 4-2 and Comparative Example 4 showed that when argon was filled in the diffusion process, a product in which the grain boundary phase was enriched with Co could be obtained and w1≧w2 could be satisfied, and when argon gas of ≧10 kPa was filled, a product in which the grain boundary phase was enriched with Co could be obtained and w1≧1.5×w2 could be satisfied. As a result of research, it was found that magnets that satisfy w1≧1.5×w2 have even higher magnetic properties and better corrosion resistance. Comparative Example 5-1 (1) NdPr, Dy, Co, Al, Fe, Cu, Ga, Ti and ferroboron with a purity of at least 99% by weight were high-frequency melted in an argon gas atmosphere, and the melt was then driven into a quench roll to produce an alloy with a mass percentage of 29% NdPr, 2.5% Dy, 1.0% Co, 0.2% Al, 0.20% Cu, 0.15% Ga, 0.18% Ti, 0.96% B, and the balance being iron and unavoidable impurities. The alloy was hydrogenated and pulverized into coarse powder, which was then jet milled and polished, and the particle size D50 of the resulting magnetic powder was 4.2 μm. After adding a lubricant that accounted for 0.2 wt% of the total mass of the jet milled powder to the jet milled powder, the materials were mixed for 2 h and pressed into a green compact at room temperature and in an orientation field environment with a magnetic field strength of 2 T. The billet was then placed in a vacuum sintering furnace and sintered at 1060°C for 6 hours. After the end of the warming, it was cooled to room temperature, then heated to 900°C, and subjected to a first stage aging treatment at 900°C for 3 hours. After the end of the warming, it was cooled to room temperature, then heated to 500°C, and subjected to a second stage aging treatment at 500°C for 5 hours. After cooling and removing from the furnace, a neodymium iron boron magnet was obtained.
[0072] (2) The magnet was processed into a square sheet with a size of 41-18-1.8 mm, and the square sheet was degreased and pickled, and then Tb diffusion treatment was performed in a vacuum state (<20 Pa). The diffusion temperature was 940°C. When the temperature reached 940°C, argon gas of 10 kPa was filled and kept at room temperature for 3 h. After the temperature was kept at room temperature, the magnet was cooled to room temperature, and then heated to 490°C. Ageing treatment was performed at 490°C for 3 h. The amount of Tb diffusion was 1.0 wt% of the total mass of the square sheet magnet with a size of 41-18-1.8 mm. The diffusion source (metallic Tb) in this embodiment was arranged using a sputtering method, and the product after the diffusion treatment was called B5-1. The magnetic properties and weight loss measurements were performed on the product, and the weight loss conditions were a temperature of 121°C, humidity of 100%, pressure of 2.0 Bar, and treatment time of 4 days. Comparative Example 5-2 The other steps are the same as in Comparative Example 5-1, with only the step (2) being different: (2) The magnet was processed into a square sheet with a size of 41-18-1.8 mm, and the square sheet was degreased and pickled, and then Tb diffusion treatment was performed in a vacuum state (<20 Pa). The diffusion temperature was 940°C, and when the temperature reached 940°C, it was kept at room temperature for 3 h, and then it was heated to 490°C and aged at 490°C for 3 h. The amount of Tb diffusion was 1.0 wt% of the total mass of the square sheet magnet with a size of 41-18-1.8 mm, and the diffusion source (metal Tb) in this embodiment was arranged using a sputtering method, and the product after the diffusion treatment was called B5-2. The magnetic properties and weight loss measurements were performed on the product, and the weight loss conditions were temperature 121°C, humidity 100%, pressure 2.0 Bar, and treatment time 4 days.
[0073] [Table 7]
[0074] As can be seen from Table 7, the corrosion resistance of Comparative Example 5-1 is not good compared with Comparative Example 5-2, which is mainly because the content of element Co added during smelting is relatively small, and sufficient distribution of element Co in the grain boundary phase cannot be guaranteed, which affects the corrosion resistance of the product. In addition, the method of Comparative Example 5-2 further reduces the distribution of element Co in the grain boundary phase, which further deteriorates the corrosion resistance of the product.
[0075] The above describes the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention are intended to be included in the scope of the claims of the present invention.
Claims
1. A neodymium-iron-boron based sintered magnet, comprising an element Co in an amount of 1.5 wt% to 3.0 wt%, the neodymium-iron-boron based sintered magnet comprising a main phase and a grain boundary phase, the element Co being distributed in the grain boundary phase of crystal grains and the main phase of crystal grains, the neodymium-iron-boron based sintered magnet satisfying w1≧w2, where w1 is the content of the element Co distributed in the grain boundary phase of crystal grains and w2 is the content of the element Co distributed in the main phase of crystal grains; Neodymium iron boron sintered magnet.
2. The neodymium-iron-boron based sintered magnet satisfies w1≧1.5×w2, in which w1 is the content of the element Co distributed in the grain boundary phase of the crystal grains, and w2 is the content of the element Co distributed in the main phase of the crystal grains.
2. The neodymium-iron-boron sintered magnet according to claim 1.
3. In the neodymium-iron-boron based sintered magnet, the Co-enriched region and the heavy rare earth-enriched region of the grain boundary phase incompletely overlap each other, and / or, in the neodymium-iron-boron based sintered magnet, the Co-enriched regions of the grain boundary phase are Fe-deficient regions; and / or, in the neodymium-iron-boron based sintered magnet, the grain boundary phase includes a phase consisting of RFeCoM, R is a rare earth element, Fe is iron, Co is cobalt, and M is one or more of Ga, Cu, Al, Zr, and Ti; and / or, in the neodymium-iron-boron based sintered magnet, the content of the R element in the grain boundary phase is equal to or greater than the content of the R element in the main phase; and / or, in the neodymium-iron-boron based sintered magnet, the content of the M element in the grain boundary phase is equal to or greater than the content of the M element in the main phase; and / or, in the neodymium-iron-boron based sintered magnet, the content of Fe element in the grain boundary phase is less than or equal to the content of Fe element in the main phase; 2. The neodymium-iron-boron sintered magnet according to claim 1.
4. The chemical formula of the neodymium iron boron based sintered magnet is RFeCoBM, in which R is a rare earth element, Fe is iron, B is boron, and M is one or more of Ga, Cu, Al, Zr, and Ti, in which the R content is 26 wt% to 35 wt%, the B content is 0.8 wt% to 1.3 wt%, the Co content is 1.5 wt% to 3.0 wt%, the Ga content is 0.05 wt% to 0.5 wt%, the Cu content is 0.05 wt% to 0.6 wt%, the Al content is 0 wt% to 1.5 wt%, the Zr content is 0 wt% to 0.5 wt%, the Ti content is 0 wt% to 0.5 wt%, and the balance is iron and unavoidable impurities.
2. The neodymium-iron-boron sintered magnet according to claim 1.
5. 1) Obtaining R-Fe-Co-BM alloy fine powder by stripping-hydrogen crushing; 2) jet milling the R-Fe-Co-BM alloy fine powder of step 1) to obtain a magnetic powder, and then pressing the magnetic powder into a green compact; 3) sintering the green compact of step 2), optionally with or without aging treatment, to obtain a sintered magnet; 4) processing the sintered magnet of step 3) into a required size, disposing a diffusion source on the surface of the processed product, and then heating the product under vacuum conditions. When the heating temperature reaches the diffusion treatment temperature, fill the product with inert gas, keep it warm, and then cool it down to room temperature. 5) performing an aging treatment on the magnet after the diffusion treatment of step 4) to produce and obtain the neodymium-iron-boron based sintered magnet. A method for producing a neodymium-iron-boron sintered magnet according to any one of claims 1 to 4.
6. In step 2), the magnetic powder after jet milling is mixed with a lubricant that accounts for 0.1 wt% to 0.5 wt% of the total mass of the magnetic powder after jet milling for 0.1 h to 3 h, and then the magnetic powder is pressed into a green compact under an orientation field environment at 20°C to 40°C and a magnetic field strength of 1 T to 5 T; The method of claim 5.
7. In step 3), the sintering temperature is 900° C. to 1100° C., and the sintering time is 2 h to 10 h; and / or in step 3), the aging treatment is a secondary aging treatment including a first stage aging treatment and a second stage aging treatment, in which the temperature of the first stage aging treatment is 700-950°C and the time of the first stage aging treatment is 1-12 h, the temperature of the second stage aging treatment is 400-600°C and the time of the second stage aging treatment is 1-12 h; The method of claim 5.
8. In step 4), the diffusion source is at least one of a rare earth element source; And / or, in step 4), an inert gas of 5 kPa or more, for example, an inert gas of 10 kPa to 30 kPa is filled; The method of claim 5.
9. In step 4), the vacuum condition is a vacuum degree of ≦20 Pa; And / or in step 4), the temperature of the diffusion treatment is 800-1000° C., And / or, in step 4), the incubation time is 3 hours or more; The method of claim 5.
10. In step 5), the aging temperature is 400 to 600°C; The method of claim 5.
Citation Information
Patent Citations
Sintered rare-earth magnet having superior corrosion resistance
JP2003031409A
Rare earth sintered magnet
JP2012028704A
Method for preparing rare earth-iron-boron based sintered magnet
JP2014236221A
R-t-b system permanent magnet
JP2020092122A
Method for preparing r-fe-b based sintered magnet
US20140352847A1