Reinforced composite membrane, membrane-electrode assembly including same, and fuel cell

The reinforced composite membrane addresses poor water retention and conductor separation issues by modifying one surface with hydrophilic groups, improving water diffusion and conductivity while maintaining structural integrity.

JP2024543886AActive Publication Date: 2024-11-26KOLON INDUSTRIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024530587
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-30
Filing Date
2022-11-23
Publication Date
2024-11-26
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

Conventional reinforced composite membranes in fuel cells suffer from poor water retention and separation of hydrophilic ion conductors from hydrophobic porous supports, leading to degraded hydrogen ion conductivity and mechanical stability.

Method used

A reinforced composite membrane with a porous support modified on one surface with hydrophilic functional groups, such as hydroxy, carboxyl, or sulfate groups, to enhance water diffusion and retention, while maintaining the other surface unmodified, ensuring the ion conductor and support remain bonded.

Benefits of technology

Improves water retention and ionic conductivity, preventing separation of the ion conductor and porous support, thereby enhancing the membrane's performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543886000001_ABST
    Figure 2024543886000001_ABST
Patent Text Reader

Abstract

A reinforced composite membrane with improved ionic conductivity and wettability is provided. One embodiment of the present invention is a reinforced composite membrane comprising a porous support and an ionomer layer containing an ion conductor filling the internal pores of the porous support, the porous support having a first surface and a second surface opposite to the first surface, the first surface being modified to contain a first hydrophilic functional group.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reinforced composite membrane, a membrane-electrode assembly including the same, and a fuel cell, and more particularly to a reinforced composite membrane in which one side of a porous support is modified to contain a hydrophilic functional group, thereby improving ionic conductivity and water retention, and a membrane-electrode assembly and a fuel cell including the same. [Background technology]

[0002] 2. Description of the Related Art Fuel cells are cells that directly convert chemical energy produced by the oxidation of fuel into electrical energy. Fuel cells have been attracting attention as a next-generation energy source due to their environmentally friendly features of high energy efficiency and low pollutant emissions.

[0003] A fuel cell generally has a structure in which an anode and a cathode are formed on either side of a polymer electrolyte membrane, and such a structure is called a membrane electrode assembly (MEA).

[0004] Fuel cells can be classified into alkaline electrolyte fuel cells, polymer electrolyte membrane fuel cells (PEMFCs), etc. depending on the type of electrolyte membrane. Among them, polymer electrolyte membrane fuel cells are attracting attention as portable, vehicular, and home power sources due to their advantages such as low operating temperature of less than 100°C, fast start-up and response characteristics, and excellent durability.

[0005] A representative example of such a polymer electrolyte membrane fuel cell is a proton exchange membrane fuel cell (PEMFC), which uses hydrogen gas as fuel.

[0006] To summarize the reactions that occur in a polymer electrolyte membrane fuel cell, first, when a fuel such as hydrogen gas is supplied to the oxidizing electrode (or anode), hydrogen ions and electrons are generated at the oxidizing electrode by an oxidation reaction of the hydrogen gas. The generated hydrogen ions are transferred to the reducing electrode (or cathode) through the polymer electrolyte membrane, and the generated electrons are transferred to the reducing electrode (or cathode) through an external circuit. Oxygen gas is supplied to the reducing electrode, and the oxygen gas combines with the hydrogen ions and electrons to generate water through a reduction reaction.

[0007] The polymer electrolyte membrane is a path through which hydrogen ions generated at the oxidizing electrode are transferred to the reducing electrode, so it must have excellent hydrogen ion conductivity. In addition, the polymer electrolyte membrane must have excellent separation ability to separate hydrogen gas supplied to the oxidizing electrode from oxygen supplied to the reducing electrode, and other required properties include excellent mechanical strength, dimensional stability, chemical resistance, etc., and low ohmic loss at high current density.

[0008] Meanwhile, the porous support used in the conventional reinforced composite membrane does not have hydrophilic functional groups on its surface, so the water generated at the cathode does not diffuse well to the anode, resulting in a decrease in the water retention of the reinforced composite membrane. This causes an additional problem of a decrease in the conductivity of hydrogen ions that must move through water. In addition, it is very difficult to uniformly impregnate a hydrophilic ion conductor into the inside of a superhydrophobic porous support, and even if impregnation is achieved, the ion conductor and the porous support are separated. Summary of the Invention [Problem to be solved by the invention]

[0009] SUMMARY OF THE PRESENT EMBODIMENT In order to solve the above problems, an object of the present invention is to provide a reinforced composite membrane having improved water retention and ionic conductivity while maintaining dimensional stability.

[0010] Another object of the present invention is to provide a reinforced composite membrane which overcomes the above problems and directs water produced at the cathode to the anode for reaction or wetting purposes.

[0011] It is still another object of the present invention to provide a reinforced composite membrane in which the hydrophilic ion conductor and the hydrophobic porous support are not separated, thereby solving the above problems.

[0012] It is yet another object of the present invention to provide a membrane-electrode assembly comprising said reinforced composite membrane.

[0013] It is still another object of the present invention to provide a fuel cell comprising the membrane-electrode assembly.

[0014] The object of the present invention is not limited to the object mentioned above, and other objects and advantages of the present invention not mentioned can be understood from the following description and will be more clearly understood from the embodiment of the present invention. In addition, it will be easily understood that the object and advantages of the present invention can be realized by the means and combinations thereof described in the claims. [Means for solving the problem]

[0015] One embodiment of the present invention to achieve the above-mentioned object provides a reinforced composite membrane comprising a porous support and an ionomer layer containing an ion conductor filling the internal pores of the porous support, wherein the porous support has a first surface and a second surface opposite to the first surface, and the first surface is modified to contain a first hydrophilic functional group. Effect of the Invention

[0016] According to the present invention, the water produced at the cathode can be returned to the anode for reaction or wetting purposes, thereby increasing the water retention and ionic conductivity. Also, according to the present invention, the problem of separation between the hydrophilic ion conductor and the superhydrophobic porous support can be solved.

[0017] In addition to the above-mentioned effects, specific effects of the present invention will be described below while explaining specific contents for carrying out the invention. [Brief description of the drawings]

[0018] [Figure 1] 1 is a cross-sectional view showing a reinforced composite membrane according to one embodiment of the present invention.

[0019] [Diagram 2] FIG. 2 is a cross-sectional view of a reinforced composite membrane according to another embodiment of the present invention.

[0020] [Diagram 3] FIG. 1 is a cross-sectional view showing a membrane-electrode assembly according to one embodiment of the present invention.

[0021] [Figure 4] FIG. 1 is a schematic diagram for explaining a fuel cell according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, each component of the present invention will be described in more detail so that a person having ordinary skill in the art to which the present invention pertains can easily implement the present invention. However, this is merely an example, and the scope of the present invention is not limited to the following content.

[0023] The reinforced composite membrane according to the present invention comprises a porous support and an ionomer layer containing an ion conductor filling the internal pores of the porous support. The porous support has a first surface and a second surface opposite to the first surface, and the first surface is modified to contain a first hydrophilic functional group. The porous support used in the conventional reinforced composite membrane has a problem that the water generated at the cathode is not well diffused to the anode because a hydrophilic functional group is not introduced on the surface, and the water retention capacity of the reinforced composite membrane is reduced. Therefore, there is an additional problem that the conductivity performance of hydrogen ions that must move through water is reduced. In addition, it is very difficult to uniformly impregnate the hydrophilic ion conductor into the inside of the superhydrophobic porous support, and even if it is impregnated, there is a problem that the ion conductor and the porous support are separated. According to one aspect of the present invention, the first surface is modified to contain a first hydrophilic functional group, thereby allowing water produced at the cathode to be returned to the anode for reaction or wetting purposes, and improving water retention and ionic conductivity. According to another aspect of the present invention, the first surface is modified to contain a first hydrophilic functional group, thereby solving the problem of separation between the hydrophilic ion conductor and the superhydrophobic porous support.

[0024] The configuration of the present invention will be described in more detail below with reference to the drawings.

[0025] 1. Reinforced composite membrane 50

[0026] FIG. 1 is a cross-sectional view showing a reinforced composite membrane according to one embodiment of the present invention.

[0027] As shown in FIG. 1, a reinforced composite membrane 50 according to the present invention can include a porous support 52 and an ionomer layer 55 .

[0028] The porous support 52 according to the present invention may have a first surface 52a and a second surface 52b opposite to the first surface 52a.

[0029] Specifically, the first surface 52a of the porous support 52 may be modified to include a first hydrophilic functional group. Specifically, the first surface may be modified by any one of the following methods: irradiation with radiation such as plasma, UV or ion beam, gamma ray, or electron beam, and reaction with a chemical agent, and preferably by a plasma method. For example, the first hydrophilic functional group introduced into the first surface 52a of the porous support 52 may be analyzed by infrared spectroscopy or a method of measuring the contact angle of deionized water with respect to the first surface of the porous support.

[0030] The first hydrophilic functional group may be any one selected from the group consisting of a hydroxyl group, a carboxyl group, a sulfate group, and a phosphate group. The first surface 52a of the porous support 52 is modified with a hydrophilic functional group, which may improve the wettability of the reinforced composite membrane and increase the ionic conductivity of hydrogen ions.

[0031] In order to introduce a hydroxyl group to the first surface, for example, a dry air (oxygen) / moisture supply method can be used, in order to introduce a carboxyl group to the first surface, for example, a carbon dioxide supply method can be used, in order to introduce a sulfate group to the first surface, for example, a sulfur dioxide gas (SO2) supply method can be used, and in order to introduce a phosphate group to the first surface, for example, a solution spraying method containing a compound containing a phosphate group can be used.

[0032] The second surface 52b of the porous support 52 according to an embodiment of the present invention may not be modified to contain a hydrophilic functional group. Therefore, only the first surface 52a is selectively modified to contain a hydrophilic functional group, which facilitates the process of water generated at the cathode moving to the anode, thereby improving the water retention and ionic conductivity of the reinforced composite membrane. In addition, the bonding strength between the hydrophilic ion conductor and the porous support is improved, which solves the problem of separation of the ion conductor and the porous support.

[0033] A contact angle of the first solvent with respect to the first surface 52a may be lower than a contact angle of the first solvent with respect to the second surface 52b. The first solvent may be any one selected from the group consisting of water, ethylene glycol, and mixtures thereof, and may be preferably distilled water.

[0034] Since the contact angle of the first solvent on the first surface 52a is smaller than the contact angle of the first solvent on the second surface 52b, not only can the wettability of the reinforced composite membrane be improved to increase the ionic conductivity of hydrogen ions, but also the product water generated at the cathode can be easily transported to the anode.

[0035] A contact angle of the first solvent with respect to the first surface 52a may be 75 to 105°, and a contact angle of the first solvent with respect to the second surface 52b may be 110 to 145°. Preferably, a contact angle of the first solvent with respect to the first surface 52a may be 80 to 100°, and a contact angle of the first solvent with respect to the second surface 52b may be 120 to 140°.

[0036] The second surface 52b of the porous support 52 according to another embodiment of the present invention may be modified to include a second hydrophilic functional group. Specifically, the second hydrophilic functional group may be any one selected from the group consisting of a hydroxyl group, a carboxyl group, a sulfate group, and a phosphate group. The first hydrophilic functional group and the second hydrophilic functional group may be the same or different from each other.

[0037] However, the degree to which the second surface 52b of the porous support 52 is modified may be less than that of the first surface 52a, and a method for achieving this may be to adjust the output of an electrode in a method using plasma.

[0038] As in the above-described embodiment, the contact angle of the second solvent with respect to the first surface 52a may be smaller than the contact angle of the second solvent with respect to the second surface 52b. Specifically, the contact angle of the second solvent with respect to the first surface 52a may be 75 to 105°, and the contact angle of the second solvent with respect to the second surface 52b may be 108 to 120°. Preferably, the contact angle of the second solvent with respect to the first surface 52a may be 80 to 100°, and the contact angle of the second solvent with respect to the second surface 52b may be 108 to 118°, and more preferably, the contact angle of the second solvent with respect to the first surface 52a may be 85 to 95°, and the contact angle of the second solvent with respect to the second surface 52b may be 110 to 115°.

[0039] The second solvent can be the same as or different from the first solvent, preferably the same.

[0040] The porous support 52 according to an embodiment of the present invention may include a highly fluorinated polymer, preferably a perfluorinated polymer, having excellent resistance to thermal and chemical decomposition, such as polytetrafluoroethylene (PTFE) or tetrafluoroethylene and CF2=CFC. n F 2n+1 (n is a real number from 1 to 5) or CF2 = CFO-(CF2CF(CF3)O) m C n F 2n+1 (m is a real number of 0 to 15, and n is a real number of 1 to 15).

[0041] The porous support 52 according to another embodiment of the present invention may be expanded polytetrafluoroethylene (e-PTFE) having a microstructure of polymer fibrils or a microstructure in which nodes are connected to each other by fibrils. Also, a film having a microstructure of polymer fibrils without nodes may be used as the porous support 52.

[0042] In yet another embodiment of the present invention, the porous support 52 can include a perfluorinated polymer, which can be formed by extruding dispersion-polymerized PTFE into a tape in the presence of a lubricant and stretching the resulting material to form a more porous and stronger porous support.

[0043] The amorphous content of PTFE can also be increased by heat treating the e-PTFE at a temperature exceeding the melting point of PTFE (about 342°C). The e-PTFE film produced by the above method can have micropores with various diameters and porosity. The e-PTFE film produced by the above method can have at least 35% pores, and the diameter of the micropores can be about 0.01 to 1 μm.

[0044] The porous support 52 according to an embodiment of the present invention may be a nonwoven fibrous web made of a plurality of randomly oriented fibers. The nonwoven fibrous web refers to a sheet having a structure of individual fibers or filaments that are interlaid but not in the same manner as a woven fabric. The nonwoven fibrous web may be manufactured by any one method selected from the group consisting of carding, garneting, air-laying, wet-laying, melt blowing, spun bonding, and stitch bonding.

[0045] The fibers may include one or more polymeric materials, and generally, any of those used as fiber-forming polymeric materials may be used, and specifically, hydrocarbon-based fiber-forming polymeric materials may be used. For example, the fiber-forming polymeric material may include any one selected from the group consisting of polyolefins, such as polybutylene, polypropylene, and polyethylene, polyesters, such as polyethylene terephthalate and polybutylene terephthalate, polyamides (nylon-6 and nylon-6,6), polyurethanes, polybutenes, polylactic acids, polyvinyl alcohols, polyphenylene sulfides, polysulfones, fluid crystalline polymers, polyethylene-co-vinyl acetates, polyacrylonitriles, cyclic polyolefins, polyoxymethylenes, polyolefin-based thermoplastic elastomers, and combinations thereof. However, the technical idea of ​​the present invention is not limited thereto.

[0046] The porous support 52 according to an embodiment of the present invention may include a nanoweb in which nanofibers are accumulated in the form of a nonwoven fabric having a plurality of pores.

[0047] The nanofibers are preferably made of a hydrocarbon-based polymer that exhibits excellent chemical resistance, has hydrophobicity, and is not likely to deform due to moisture in a high humidity environment. Specifically, the hydrocarbon-based polymer may be selected from the group consisting of nylon, polyimide, polyaramid, polyetherimide, polyacrylonitrile, polyaniline, polyethylene oxide, polyethylene naphthalate, polybutylene terephthalate, styrene butadiene rubber, polystyrene, polyvinyl chloride, polyvinyl alcohol, polyvinylidene fluoride, polyvinyl butylene, polyurethane, polybenzoxazole, polybenzimidazole, polyamideimide, polyethylene terephthalate, polyphenylene sulfide, polyethylene, polypropylene, copolymers thereof, and mixtures thereof. Among these, polyimide is preferably used because of its excellent heat resistance, chemical resistance, and dimensional stability.

[0048] The nanoweb is an aggregate of nanofibers that are randomly arranged and manufactured by electrospraying. In this case, the nanofibers preferably have an average diameter of 40 to 5000 nm, calculated from the average of diameters of 50 fibers measured using a scanning electron microscope (JSM6700F, JEOL) while taking into account the porosity and thickness of the nanoweb.

[0049] If the average diameter of the nanofibers is less than the above range, the mechanical strength of the porous support may be reduced, and if the average diameter of the nanofibers is more than the above range, the porosity may be significantly reduced and the thickness may be increased.

[0050] The nonwoven fibrous web may have a thickness of 10 to 50 μm, specifically, 15 to 43 μm. If the thickness of the nonwoven fibrous web is less than the above range, the mechanical strength may be reduced, and if it exceeds the above range, the resistance loss may be increased, and the weight and integration may be reduced.

[0051] The nonwoven fibrous web has a basic weight of 5 to 30 mg / cm 2 If the basis weight of the nonwoven fibrous web is less than the above range, visible pores may be formed and it may be difficult to function as a porous support, and if it exceeds the above range, it may be manufactured in the form of paper or fabric with almost no pores.

[0052] The porosity can be calculated as a ratio of the air volume in the porous support to the total volume of the porous support according to the following mathematical formula 1. Here, the total volume is calculated by preparing a rectangular sample and measuring its width, length, and thickness, and the air volume can be obtained by measuring the mass of the sample and then subtracting the polymer volume, which is calculated back from the density, from the total volume.

[0053] [Mathematical formula 1]

[0054] Porosity (%) = (air volume in the porous support / total volume of the porous support) x 100

[0055] The porosity of the porous support according to the present invention may be 30 to 90%, and preferably 60 to 85%. If the porosity of the porous support is less than the above range, the impregnation of the ion conductor may be reduced, and if it exceeds the above range, the shape stability may be reduced, which may hinder smooth post-processing.

[0056] The ionomer layer 55 according to the present invention may include an ion conductor that fills the interior pores of the porous support 52 .

[0057] The ion conductor according to the present invention may be a cation conductor having a cation exchange functional group such as a hydrogen ion, or an anion conductor having an anion exchange functional group such as a hydroxyl ion, carbonate, or bicarbonate. The cation exchange functional group may be any one selected from the group consisting of a sulfonic acid group, a carboxyl group, a boronic acid group, a phosphate group, an imide group, a sulfonimide group, a sulfonamide group, a sulfonyl fluoride group, and combinations thereof, and may generally be a sulfonic acid group or a carboxyl group.

[0058] Examples of the cationic conductor include a fluorine-based polymer containing the cationic exchange functional group and containing fluorine in the main chain, a hydrocarbon polymer such as benzimidazole, polyamide, polyamideimide, polyimide, polyacetal, polyethylene, polypropylene, acrylic resin, polyester, polysulfone, polyether, polyetherimide, polyester, polyethersulfone, polyetherimide, polycarbonate, polystyrene, polyphenylene sulfide, polyetheretherketone, polyetherketone, polyarylethersulfone, polyphosphazene, or polyphenylquinoxaline, a partially fluorinated polymer such as a polystyrene-graft-ethylenetetrafluoroethylene copolymer or a polystyrene-graft-polytetrafluoroethylene copolymer, a sulfonimide, or a mixture thereof.

[0059] More specifically, when the cation conductor is a hydrogen ion cation conductor, the polymer may contain a cation exchange group selected from the group consisting of a sulfonic acid group, a carboxylic acid group, a phosphoric acid group, a phosphonic acid group, and derivatives thereof in a side chain. Specific examples thereof include poly(perfluorosulfonic acid), poly(perfluorocarboxylic acid), a copolymer of tetrafluoroethylene and fluorovinyl ether containing a sulfonic acid group, a fluorine-based polymer containing defluorinated sulfurized polyether ketone, or a mixture thereof, sulfonated polyimide (S-PI), sulfonated polyarylethersulfone (S-PAES), sulfonated polyetheretherketone (S-PEEK), sulfonated polybenzimidazole (S-PBI), sulfonated polysulfone (S-PSU), sulfonated polystyrene (S-PS ... polystyrene, S-PS), sulfonated polyphosphazene, sulfonated polyquinoxaline, sulfonated polyketone, sulfonated polyphenylene oxide, sulfonated polyether sulfone, sulfonated polyether ketone, sulfonated polyphenylene sulfone, sulfonated polyphenylene sulfide, sulfonated polyphenylene sulfide sulfoneExamples of the sulfonated polyarylene ether include sulfonated polyphenylene sulfide sulfone nitrile, sulfonated polyarylene ether, sulfonated polyarylene ether nitrile, sulfonated polyarylene ether ether nitrile, sulfonated polyarylene ether sulfone ketone, and hydrocarbon polymers including mixtures thereof, but the technical idea of ​​the present invention is not limited thereto.

[0060] The anion conductor is a polymer capable of transporting anions such as hydroxyl ions, carbonates, or bicarbonates. The anion conductor is commercially available in the form of hydroxide or halide (generally chloride). The anion conductor can be used in industrial water purification, metal separation, catalytic processes, etc.

[0061] The anion conductor may generally be a polymer doped with a metal hydroxide. Specifically, poly(ether sulfone), polystyrene, vinyl polymer, poly(vinyl chloride), poly(vinylidene fluoride), poly(tetrafluoroethylene), poly(benzimidazole), or poly(ethylene glycol) doped with a metal hydroxide may be used.

[0062] The ionomer layer 55 according to the present invention may include a first resin layer 54 and a second resin layer 56 facing the first resin layer 54. Specifically, the first resin layer 54 may be disposed on the first surface 52a, and the second resin layer 56 may be disposed on the second surface 52b. Thus, the ionomer layer 55 may be formed on the surface of the porous support 52.

[0063] 2 is a cross-sectional view showing a reinforced composite membrane according to another embodiment of the present invention. The repeated explanations of the above-mentioned parts will be simplified or omitted.

[0064] 2, the porous support 52 according to the present invention may include at least two sub-porous supports. Specifically, the porous support 52 may include a first sub-porous support 52_1 and a second sub-porous support 52_2 disposed on the first sub-porous support 52_1.

[0065] The first sub-porous support 52_1 and the second sub-porous support 52_2 may be the same as or different from the above-described porous supports, each independently.

[0066] The first sub-porous support 52_1 may have a thickness of, for example, 1 to 50 μm, and the second sub-porous support 52_2 may have a thickness of, for example, 1 to 50 μm.

[0067] The porosity of each of the first sub-porous support 52_1 and the second sub-porous support 52_2 may be the same as or different from the above-mentioned porous supports, and the composition may be the same as or different from the above-mentioned porous supports.

[0068] The first sub-porous support 52_1 may comprise the first surface 52a, and the second sub-porous support 52_2 may comprise the second surface 52b.

[0069] Unlike the above-described embodiment, the ionomer layer 55 according to the present invention may further include a third resin layer 58. The third resin layer 58 may be disposed between the first sub-porous support 52_1 and the second sub-porous support 52_2.

[0070] The equivalent weight of the ion conductor constituting each of the first to third resin layers 54, 56, and 58 may be the same or different from each other. The ion conductor constituting the resin layers may be any one selected from the group consisting of a fluorine-based ion conductor, a hydrocarbon-based ion conductor, and a mixture thereof, similar to the above-mentioned ion conductor.

[0071] 2. Membrane-electrode assembly 100

[0072] 3 is a cross-sectional view showing a membrane-electrode assembly according to an embodiment of the present invention. The repeated explanations of the above-mentioned parts will be simplified or omitted.

[0073] As shown in FIG. 3, the membrane-electrode assembly 100 according to the present invention includes the reinforced composite membrane 50 and the fuel cell electrodes 20, 20' disposed on both sides of the reinforced composite membrane 50, respectively.

[0074] The membrane-electrode assembly 100 according to one embodiment of the present invention may include the reinforced composite membrane 50 described above, an anode 20 disposed on the first side (not shown), and a cathode 20' disposed on the second side (not shown). The ionomer layer (not shown) according to the present invention may include a first resin layer and a second resin layer facing the first resin layer.

[0075] The electrodes 20, 20' include an electrode substrate 40, 40' and a catalyst layer 30, 30' formed on a surface of the electrode substrate 40, 40'. In order to facilitate diffusion of materials in the electrode substrate 40, 40', a microporous layer (not shown) containing conductive fine particles such as carbon powder or carbon black may be further provided between the electrode substrate 40, 40' and the catalyst layer 30, 30'.

[0076] In the membrane-electrode assembly 100, the electrode 20 that is disposed on one side of the reinforced composite membrane 50 and causes an oxidation reaction to generate hydrogen ions and electrons from the fuel transferred to the catalyst layer 30 via the electrode substrate 40 is called an anode.

[0077] The electrode 20' disposed on the other side of the reinforced composite membrane 50 and performing a reduction reaction to generate water from hydrogen ions supplied through the reinforced composite membrane 50 and an oxidant transferred to the catalyst layer 30' via the electrode substrate 40' is called a cathode electrode.

[0078] The catalyst layers 30, 30' of the anode and cathode electrodes 20, 20' contain a catalyst. The catalyst participates in the cell reaction and can be any catalyst that can be used as a catalyst for a fuel cell. Preferably, a platinum-based metal can be used.

[0079] The platinum-based metal may include one selected from the group consisting of platinum (Pt), palladium (Pd), ruthenium (Ru), iridium (Ir), osmium (Os), platinum-M alloys, non-platinum alloys, and combinations thereof. More preferably, a combination of two or more metals selected from the platinum-based catalytic metal group may be used, but is not limited thereto. Any platinum-based catalytic metal that can be used in this technical field may be used without limitation.

[0080] The M may be at least one selected from the group consisting of palladium (Pd), ruthenium (Ru), iridium (Ir), osmium (Os), gallium (Ga), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), silver (Ag), gold (Au), zinc (Zn), tin (Sn), molybdenum (Mo), tungsten (W), lanthanum (La), and rhodium (Rh). Specifically, the platinum alloy may be selected from the group consisting of Pt-Pd, Pt-Sn, Pt-Mo, Pt-Cr, Pt-W, Pt-Ru, Pt-Ru-W, Pt-Ru-Mo, Pt-Ru-Rh-Ni, Pt-Ru-Sn-W, Pt-Co, Pt-Co-Ni, Pt-Co-Fe, Pt-Co-Ir, Pt-Co-S, Pt-Co-P, Pt-Fe, Pt-Fe-Ir, Pt-Fe-S, Pt-Fe-P, Pt-Au-Co, Pt-Au-Fe, Pt-Au-Ni, Pt-Ni, Pt-Ni-Ir, Pt-Cr, Pt-Cr-Ir, and combinations thereof, either alone or in combination of two or more thereof.

[0081] Furthermore, the non-platinum alloy may be selected from the group consisting of Ir-Fe, Ir-Ru, Ir-Os, Co-Fe, Co-Ru, Co-Os, Rh-Fe, Rh-Ru, Rh-Os, Ir-Ru-Fe, Ir-Ru-Os, Rh-Ru-Fe, Rh-Ru-Os, and combinations thereof, either alone or in combination of two or more thereof.

[0082] The catalyst may be a catalyst itself (black) or may be supported on a carrier.

[0083] 3.Fuel cell 200

[0084] FIG. 4 is a schematic diagram for explaining a fuel cell according to one embodiment of the present invention.

[0085] One embodiment of the present invention relates to a fuel cell comprising the membrane-electrode assembly.

[0086] As shown in FIG. 4, a fuel cell 200 according to the present invention may include a fuel supply unit 210 for supplying a mixed fuel obtained by mixing fuel and water, a reforming unit 220 for reforming the mixed fuel to generate a reformed gas containing hydrogen gas, a stack 230 for generating electrical energy by electrochemically reacting the reformed gas containing hydrogen gas supplied from the reforming unit 220 with an oxidant, and an oxidant supply unit 240 for supplying an oxidant to the reforming unit 220 and the stack 230.

[0087] The stack 230 may include a plurality of unit cells that generate electrical energy by conducting an oxidation / reduction reaction between the reformed gas including hydrogen gas supplied from the reformer 220 and an oxidant supplied from the oxidant supplying unit 240.

[0088] Each unit cell means a unit cell that generates electricity, and may include the membrane-electrode assembly that oxidizes / reduces oxygen in a reformed gas containing hydrogen gas and an oxidant, and a separator plate (also called a bipolar plate, hereinafter referred to as "separator plate") for supplying the reformed gas containing hydrogen gas and the oxidant to the membrane-electrode assembly. The separator plates are disposed on both sides of the membrane-electrode assembly. In this case, the separator plates located at the outermost sides of the stack are also referred to as end plates.

[0089] Of the separation plates, the end plate may be provided with a pipe-shaped first supply pipe 231 for injecting the reformed gas containing hydrogen gas supplied from the reforming section 220, and a pipe-shaped second supply pipe 232 for injecting oxygen gas, and the other end plate may be provided with a first exhaust pipe 233 for discharging the reformed gas containing hydrogen gas that is ultimately left unreacted in the multiple unit cells to the outside, and a second exhaust pipe 234 for discharging the oxidant that is ultimately left unreacted in the unit cells to the outside.

[0090] In the fuel cell, the separator, the fuel supply section, and the oxidant supply section constituting the electricity generating section are the same as those used in ordinary fuel cells, and therefore detailed description thereof will be omitted in this specification.

[0091] Hereinafter, the embodiments of the present invention will be described in detail so that a person having ordinary skill in the art to which the present invention pertains can easily carry out the embodiments. However, this is merely an example, and the scope of the present invention is not limited to the following contents.

[0092] [Example of manufacturing preparation: manufacturing of porous support]

[0093] Porous supports were prepared according to the following working examples, comparative examples, and reference examples.

[0094] <Example 1: When only the first surface is modified>

[0095] The flow rate of oxygen gas was set to 20sccm, the power of plasma was set to 2W, and the plasma treatment time was set to 5 seconds, and the first surface of the porous support (e-PTFE) was modified to have hydroxyl groups (-OH) by RF (radio frequency) plasma method, and the second surface opposite to the first surface was not modified. The porosity of the porous support according to Preparation Example 1 was 70%, the thickness was 10μm, and the pore size was 0.2μm.

[0096] <Preparation Example 2: Second surface modified less than the first surface>

[0097] A porous support was produced in the same manner as in Preparatory Example 1, but the second surface was additionally modified by setting the oxygen gas flow rate to 20 sccm, the plasma power to 2 W, and the plasma treatment time to 2 seconds, i.e., the first surface was modified so that the concentration of hydroxyl groups per unit area was greater than that of the second surface.

[0098] <Preparation Example 3: Porous support having two sub-porous supports>

[0099] A porous support was manufactured in the same manner as in Preparation Example 1, but a second subporous support (e-PTFE) was formed on a first subporous support (e-PTFE) to finally manufacture a porous support. The first subporous support had a porosity of 65%, a thickness of 5 μm, and a pore size of 0.15 μm, and the second subporous support had a porosity of 75%, a thickness of 5 μm, and a pore size of 0.2 μm. The first surface of the first subporous support (e-PTFE) was modified to have a hydroxyl group (-OH) by a radio frequency (RF) plasma method. Specifically, in the method of forming a second subporous support on the first subporous support, alcohol was sprayed on the surface of the first subporous support, and then a heat pressing process using a roll press was used.

[0100] Comparative Preparation Example 1: Unmodified Porous Support

[0101] A porous support (e-PTFE) with a porosity of 70%, a thickness of 10 μm, and a pore size of 0.2 μm, whose surface was not modified, was prepared.

[0102] <Reference Preparation Example 1: Porous support having first and second surfaces both modified identically>

[0103] A porous support was manufactured in the same manner as in Preparation Example 2, but both the first and second surfaces were modified with the same oxygen gas flow rate of 100 sccm, plasma power of 3 W, and plasma treatment time of 5 seconds.

[0104] [Experimental Example 1: Contact angle measurement]

[0105] A porous support was prepared according to the above Preparation Example, and the contact angle of distilled water was measured for each of the first and second surfaces.

[0106] 1) Contact angle measurement method

[0107] Distilled water was filled into a syringe at 25°C and RH 40%, and a water droplet with a diameter of 3 mm was dropped onto one side of the porous support, and the water droplet was allowed to spread for 5 minutes. After 5 minutes, the contact angle between the one side of the porous support and the water droplet was measured. The smaller the contact angle, the more hydrophilic modification was performed on the one side of the porous support.

[0108] [Table 1]

[0109] [Manufacturing example: Manufacturing of reinforced composite membrane]

[0110] Reinforced composite membranes were prepared according to the following examples and comparative examples.

[0111] Example 1: Reinforced composite membrane with porous support of Preparation Example 1

[0112] The porous support of Preparation Example 1 was pretreated for 5 minutes in a reaction vessel containing isopropyl alcohol at room temperature. The pretreated porous support was immersed in a 10 wt.% solution of Nafion dispersed in an emulsion state (product name: Nafion D1021) for 5 minutes, and then dried at 60°C for 4 hours to produce a reinforced composite membrane.

[0113] <Example 2: Reinforced composite membrane with porous support of Preparation Example 2>

[0114] A reinforced composite membrane was produced in the same manner as in Example 1, but the porous support according to Preparative Example 2 was used instead of the porous support according to Preparative Example 1.

[0115] <Example 3: Reinforced composite membrane with porous support of Preparation Example 3>

[0116] A reinforced composite membrane was produced in the same manner as in Example 1, but the porous support according to Preparative Example 3 was used instead of the porous support according to Preparative Example 1.

[0117] <Example 4: Different from Example 1, in which the ionic conductor was different>

[0118] A reinforced composite membrane was prepared in the same manner as in Example 1, but a sulfonated poly(ether sulfone) having an ion exchange capacity of 1.7 meq / g was used instead of the 10 wt % Nafion solution in Preparative Example 1.

[0119] <Comparative Example 1: Reinforced composite membrane with porous support of Comparative Preparation Example 1>

[0120] A reinforced composite membrane was produced in the same manner as in Example 1, but the porous support of Comparative Preparation Example 1 was used instead of the porous support of Working Preparation Example 1.

[0121] <Reference Example 1: Reinforced composite membrane with porous support of Reference Preparation Example 1>

[0122] A reinforced composite membrane was produced in the same manner as in Example 1, but the porous support of Reference Preparation Example 1 was used instead of the porous support of Working Preparation Example 1.

[0123] <Comparative Example 2: Different porous support from Example 4>

[0124] A reinforced composite membrane was produced in the same manner as in Example 4, but the porous support of Comparative Preparation Example 1 was used instead of the porous support of Working Preparation Example 1.

[0125] [Experimental Example 2: Measurement of water absorption rate and dimensional change rate of reinforced composite membrane]

[0126] The water absorption rate and dimensional change rate of the reinforced composite membrane according to the above Preparation Example were measured.

[0127] 1) Water absorption rate

[0128] The reinforced composite membrane according to the above Preparation Example was washed several times with deionized water, and the washed reinforced composite membrane was dried in a vacuum dryer at 120° C. for 24 hours, and then weighed (W dry The same membrane was then immersed in deionized water for 24 hours, taken out, the water present on the surface was removed, and the weight was measured again (W wet The water absorption rate was calculated using the following mathematical formula 2.

[0129] [Mathematical formula 2]

[0130]

number

[0131] 4) Dimensional change rate

[0132] The dimensional change rate of the reinforced composite membrane according to the above Preparation Example was measured in the same manner as the water absorption rate measurement method, but instead of measuring the weight, the volume change of the reinforced composite membrane was measured and calculated according to the following Equation 3.

[0133] [Mathematical formula 3]

[0134]

number

[0135] [Table 2]

[0136] Referring to Table 2, it can be seen that the Examples have a lower water absorption rate and a significantly lower dimensional change rate than the Reference Example. This confirms that the problem of reduced dimensional stability occurs when both sides of a porous support are modified in the same way, and that the dimensional stability is improved by modifying one side of the porous support as in the Examples, or by modifying both sides differently by adjusting the plasma treatment time.

[0137] [Experimental Example 3: Performance evaluation of membrane-electrode assembly]

[0138] The electrode slurry was directly coated on both sides of the reinforced composite membrane according to the above Preparation Example, and then dried to prepare a membrane-electrode assembly. The ionic conductivity of the membrane-electrode assembly including the reinforced composite membrane according to the above Preparation Example was measured by the following method.

[0139] 1) Ionic conductivity (experimental conditions: 80℃ / 50%RH)

[0140] The ionic conductivity of the membrane-electrode assembly having the reinforced composite membrane according to the above Preparation Example was measured using a measuring device (Solatron-1280 Impedance / Gain-Phase analyzer) at a measuring temperature of 80° C. In particular, the ohmic resistance or bulk resistance was measured using a four point probe AC ​​impedance spectroscopic method, and then the ionic conductivity was calculated according to the following Equation 4.

[0141] [Mathematical formula 4]

[0142]

number

[0143] In the above mathematical formula 4, σ is the ionic conductivity (S / cm), R is the ohmic resistance of the electrolyte membrane (Ω), L is the distance between the electrodes (cm), and S is the area in the electrolyte through which a certain current flows (cm 2 ) applies.

[0144] [Table 3]

[0145] Referring to Table 3, it can be seen that the Examples have higher ionic conductivity than the Comparative Examples. Reference Example 1 had high ionic conductivity, but had a problem of significantly reduced dimensional stability as seen in Experimental Example 2. According to the present invention, it is possible to provide a membrane-electrode assembly having high ionic conductivity while satisfying an appropriate range of dimensional stability.

[0146] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention.

Claims

1. A porous support; an ionomer layer containing an ion conductor filling the internal pores of the porous support; 2. A reinforced composite membrane comprising: The porous support is A first surface; a second surface opposite to the first surface; and Equipped with The first surface of the reinforced composite membrane is modified to contain a first hydrophilic functionality.

2. The first hydrophilic functional group is 2. The reinforced composite membrane of claim 1, wherein the group is any one selected from the group consisting of a hydroxyl group, a carboxyl group, a sulfate group, and a phosphate group.

3. The second surface is 10. The reinforced composite membrane of claim 1 which has not been modified to contain hydrophilic functionalities.

4. 4. The reinforced composite membrane of claim 3, wherein a contact angle of a first solvent with said first surface is lower than a contact angle of the first solvent with said second surface.

5. 5. The reinforced composite membrane of claim 4, wherein a contact angle of the first solvent with respect to the first surface is from 75 to 105 degrees, and a contact angle of the first solvent with respect to the second surface is from 110 to 145 degrees.

6. 5. The reinforced composite membrane of claim 4, wherein the first solvent is any one selected from the group consisting of water, ethylene glycol, and mixtures thereof.

7. The second surface is 10. The reinforced composite membrane of claim 1 which has been modified to contain a second hydrophilic functionality.

8. The second hydrophilic functional group is 8. The reinforced composite membrane of claim 7, wherein the group is any one selected from the group consisting of a hydroxyl group, a carboxyl group, a sulfate group, and a phosphate group.

9. 8. The reinforced composite membrane of claim 7, wherein the contact angle of the second solvent with respect to the first surface is 75 to 105 degrees, and the contact angle of the second solvent with respect to the second surface is 108 to 120 degrees.

10. The porous support is 10. The reinforced composite membrane of claim 1 comprising at least two or more subporous supports.

11. The porous support is a first sub-porous support; a second sub-porous support disposed on the first sub-porous support; 11. The reinforced composite membrane of claim 10, comprising:

12. The first sub-porous support comprises: The first surface is provided. The second sub-porous support comprises: The reinforced composite membrane of claim 11 comprising the second surface.

13. The ion conductor is 2. The reinforced composite membrane according to claim 1, which is any one selected from the group consisting of fluorine-based ion conductors, hydrocarbon-based ion conductors, and mixtures thereof.

14. A reinforced composite membrane according to claim 1; an anode disposed on the first surface; a cathode disposed on the second surface; and A membrane-electrode assembly comprising:

15. The ionomer layer is A first resin layer; a second resin layer facing the first resin layer; The membrane-electrode assembly of claim 14, comprising:

16. A fuel cell comprising the membrane-electrode assembly according to claim 14.

Citation Information

Patent Citations

  • Porous support, method for producing the same, and reinforced film containing the same

    JP2017510722A

  • Porous support with excellent filling characteristics for an ion conductor, method for producing the same, and reinforced film containing the same

    JP2018507096A

  • Membranes and methods

    JP2019517111A

  • Composite polymer electrolyte membrane, as well as electrolyte membrane having catalyst layer, membrane electrode assembly, and solid polymer fuel cell in which said composite polymer electrolyte membrane is used

    WO2016148017A1

  • Polymer electrolyte membrane, membrane-electrode assembly including same, and method for measuring durability thereof

    WO2021133044A1