METHOD FOR MANUFACTURING MEMBRANE ELECTRODE ASSEMBLIES (MEAs), MEAS, CELLS, AND USES THEREOF
The additive manufacturing method for MEAs addresses scalability and efficiency issues by reducing thickness and material usage, enhancing performance and connectivity, while maintaining mechanical robustness and cost-effectiveness.
Patent Information
- Application Number
- JP2024532434
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-01
- Filing Date
- 2022-12-01
- Publication Date
- 2024-11-26
AI Technical Summary
Existing methods for manufacturing membrane electrode assemblies (MEAs) face challenges in scalability, efficiency, and performance due to difficulties in thickness reduction and material oxidation, particularly with inkjet and electrospinning techniques.
A method involving additive techniques for manufacturing MEAs, where at least one diffusion layer and the ion exchange membrane are produced, reducing thickness while maintaining mechanical robustness and improving performance, using sustainable materials and enabling automation and scalability.
The method results in MEAs with reduced thickness, enhanced performance, and cost-effectiveness, with improved interlayer connectivity and reduced material usage, achieving comparable performance to conventional MEAs using significantly less material.
Smart Images

Figure 2024543964000002 
Figure 2024543964000003 
Figure 2024543964000004
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of electrochemistry, more specifically to the field of methods for manufacturing membrane electrode assemblies (MEAs). [Background technology]
[0002] Low-cost procedures and materials with low environmental impact have been reported for the fabrication of membrane electrode assemblies (MEAs). Inkjet and screen printing techniques have been used to fabricate parts of the MEAs.
[0003] Garcia et al. (ACS Omega 2019,4,16781-16788) studied the electrochemical properties of capacitors printed on paper as energy storage devices, with a commercially available paper sheet being both the substrate and the separator of the device. Zinc ink was applied to the surface of the paper substrate by bar coating, and a commercially available silver ink was screen printed on the opposite side of the paper substrate. The results showed a capacitor that behaved as an energy storage device with low current output. However, after the electrochemical process, the initial flake-like shape of the Zn particles was no longer observed, limiting the useful life of such devices. Another drawback of the capacitor was that the silver particles used as electrodes suffered oxidation in the charge / discharge cycles of the battery.
[0004] M. Breitwiser et al. (Journal of Power Sources, Vol. 337, 2017, pp. 137-144) described the fabrication of 12 micron thin proton exchange membranes MEA by direct electrospinning of poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP) nanofibers on a commercial gas diffusion electrode containing a catalyst, followed by inkjet printing of Nafion ionomer dispersion into the pore space of the fibers. This fabrication method is difficult to scale up due to the electrospinning process. In addition, only the membrane thickness of the MEA is reduced using this fabrication method.
[0005] Therefore, notwithstanding the methods mentioned above, it is desirable to develop new manufacturing methods for MEAs with increased efficiency and overall performance. Summary of the Invention
[0006] The inventors have developed a method for the manufacture of a membrane electrode assembly (MEA), in which at least one diffusion layer of the MEA is obtained by an additive technique and the ion exchange membrane is obtained by an additive technique. This method makes it possible to obtain MEAs with reduced thickness. This has resulted in a reduction of the diffusion barrier while maintaining the mechanical robustness of said MEA. The MEAs obtained by said method also show better performance than other MEAs of the prior art, with fast membrane activation and resulting current densities in a similar range. The method of the invention shows particular impact as an industrial process, allowing it to be fully automated and scalable. In addition, the method uses low-cost and sustainable materials, resulting in at least an order of magnitude reduction in the cost of manufacture when compared to conventional MEA manufacture.
[0007] Accordingly, a first aspect of the present invention is a manufacturing method for a membrane electrode assembly (MEA), comprising the steps of: i. - an ion exchange membrane having two opposite faces, and - a first diffusion layer and a second diffusion layer comprising a carbon material, the first diffusion layer and the second diffusion layer having two opposite faces; preparing ii. A catalyst; - one side of the ion exchange membrane and one side of one of the first and second diffusion layers; - two faces of an ion exchange membrane, or - one surface of each of the first and second diffusion layers; A step of coating the iii. disposing an ion exchange membrane between the first and second diffusion layers, wherein both sides of the ion exchange membrane are in contact with a catalyst; and iv. optionally bonding the first diffusion layer, the ion exchange membrane and the second diffusion layer under pressure and / or heat; Including, At least one of the first and second diffusion layers and the ion exchange membrane is obtained by an additive technique; The present invention relates to a method for producing a pharmaceutical composition comprising the steps of:
[0008] In a second aspect, the present invention is directed to a membrane electrode assembly (MEA) obtainable by the method of manufacture defined in any of the specific embodiments of the present invention, wherein at least one of the diffusion layers has a thickness of less than 30 microns, and preferably at least one of the diffusion layers is a gas diffusion layer.
[0009] Another aspect is directed to a cell comprising a compartment containing a membrane electrode assembly (MEA) as defined in any one of the embodiments of the present invention, and means for connection to a power / load source.
[0010] An additional aspect is directed to the use of a membrane electrode assembly (MEA) as defined in any of the specific embodiments of the invention, or a cell as defined in any of the specific embodiments of the invention, for the electrochemical detection of an analyte, such as ferrocene.
[0011] A final aspect is directed to the use of a membrane electrode assembly (MEA) as defined in any of the specific embodiments of the invention, or of a cell as defined in any of the specific embodiments of the invention, for storing and / or transmitting energy, preferably electricity, preferably wherein the membrane electrode assembly (MEA) or cell is part of a fuel cell. [Brief description of the drawings]
[0012] [Figure 1] 1 shows an exploded view of the MEA. [Diagram 2] 4 shows an SEM micrograph of the MEA. [Diagram 3]4 shows the polarization curve results, i.e., cell potential (V) versus current density (mA.cm-2), for (a) an MEA containing a paper-Nafion membrane and (b) an MEA containing a commercial Nafion membrane. [Figure 4] Figure 2 shows the linear sweep voltammetry curves for different MEAs. [Diagram 5] 1 shows the results of dynamic mechanical analysis of stress-strain experiments on different MEAs. [Figure 6] shows the results of contact angle tests on different MEAs. [Figure 7] shows a membrane electrode assembly (MEA) with screen printed current collectors that follow the 4 pin / track design of a standard USB series A plug connector. [Figure 8] shows SEM micrographs of a fully printed MEA and a conventional MEA. [Figure 9] shows the polarization curves for the fully printed MEA and the conventional MEA. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] A first aspect of the present invention is a method for manufacturing a membrane electrode assembly (MEA), comprising the steps of: i. - an ion exchange membrane having two opposite faces, and - a first diffusion layer and a second diffusion layer comprising a carbon material, each of the first and second diffusion layers having two opposite faces; preparing ii. A catalyst; - one side of the ion exchange membrane and one side of one of the first and second diffusion layers; - two faces of an ion exchange membrane, or - one surface of each of the first and second diffusion layers; A step of coating the iii. disposing an ion exchange membrane between the first and second diffusion layers, wherein both sides of the ion exchange membrane are in contact with a catalyst; and iv. optionally bonding the first diffusion layer, the ion exchange membrane and the second diffusion layer under pressure and / or heat; Including, At least one of the first and second diffusion layers and the ion exchange membrane is obtained by an additive technique; The present invention relates to a method for producing a pharmaceutical composition comprising the steps of:
[0014] In one embodiment, a method for producing a membrane electrode assembly (MEA) includes the following steps: i. - an ion exchange membrane having two opposite faces, and - a first diffusion layer and a second diffusion layer comprising a carbon material, each of the first and second diffusion layers having two opposite faces; preparing ii. A catalyst; - one side of the ion exchange membrane and one side of one of the first and second diffusion layers; - two faces of an ion exchange membrane, or - one surface of each of the first and second diffusion layers; A step of coating the iii. disposing an ion exchange membrane between the first and second diffusion layers, wherein both sides of the ion exchange membrane are in contact with a catalyst; and iv. optionally bonding the first diffusion layer, the ion exchange membrane and the second diffusion layer, preferably under pressure and / or heat; It consists of: At least one of the first and second diffusion layers and the ion exchange membrane is obtained by an additive technique.
[0015] In the context of the present invention, the expression "addition technique" refers to a technique that allows the addition of either one layer or overlapping layers of a certain material.Non-limiting examples of addition techniques are silk screen printing, screen printing, flexographic printing, bar coating, inkjet printing, slot die printing, spray coating, casting techniques, such as doctor blading techniques, tape casting techniques, and the like, and mixed techniques thereof.In certain embodiments, the addition technique of the present invention is selected from screen printing techniques, spray coating techniques, casting techniques, or mixed techniques thereof.
[0016] In a particular embodiment, the screen printing is performed by a pneumatic screen printer, preferably a pneumatic flat screen printer.
[0017] In another particular embodiment, the casting technique is a tape casting technique, preferably a doctor blading technique, more preferably a doctor blading technique performed by a blade.
[0018] In another particular embodiment, the spray coating technique is carried out by using a pressurized gas such as air, preferably at a flow rate of 1-1000 μl / min, preferably 100-800 μl / min, more preferably 200-700 μl / min. In a particular embodiment, the screen printing technique was carried out at a spray speed of 500-3000 mm / min, preferably 1000-2000 mm / min, more preferably 1200-1800 mm / min.
[0019] Process (i) In certain embodiments, the ion exchange membrane is a proton exchange membrane.
[0020] In one embodiment, the ion exchange membrane comprises: (a) depositing, by an additive technique, on a substrate a composition comprising 1-30 wt % of an ion-conducting polymer in a solvent or solvent mixture; and (b) optionally separating the deposited ion exchange membrane from the substrate; The method is obtained by a method comprising the steps of:
[0021] In a particular embodiment, the ion exchange membrane is obtained by a tape casting technique, preferably a doctor blading technique.
[0022] In an alternative specific embodiment, the application technique is a screen printing technique.
[0023] In some embodiments, the substrate is a cellulosic substrate, such as paper, preferably a paper sheet, hi some embodiments, the cellulosic substrate is pre-soaked in a composition comprising 1-30 wt % of an ion-conducting polymer in a solvent or solvent mixture.
[0024] In the context of the present invention, the term "ion-conducting polymer" refers to a polymer that exhibits electrical conductivity due to the transport of ionic species. Non-limiting examples of ion-conducting polymers are sulfonated polyaniline or perfluorosulfonic acid (PFSA) polymers.
[0025] In certain embodiments, the ion-conducting polymer is a fluorinated polymer, in particular a fluorinated polymer having sulfonic acid moieties, preferably a sulfonated tetrafluoroethylene-based fluoropolymer or a perfluorosulfonic acid (PFSA) polymer, more preferably a tetrafluoroethylene-perfluoro-3,6-dioxa-4-methyl-7-octene sulfonic acid polymer or copolymer.
[0026] In another embodiment, the substrate is a glass sheet.
[0027] In certain embodiments, the ion exchange membrane comprises an ion-conducting polymer.In some embodiments, the ion-conducting polymer is an organic fluorinated polymer selected from homopolymer, copolymer, multicomponent polymer, or a combination thereof.In certain embodiments, the ion-conducting polymer is a fluorinated polymer, particularly a fluorinated polymer having sulfonic acid moieties, preferably a sulfonated tetrafluoroethylene-based fluoropolymer or a perfluorosulfonic acid (PFSA) polymer, more preferably a tetrafluoroethylene-perfluoro-3,6-dioxa-4-methyl-7-octene sulfonic acid polymer or copolymer.
[0028] In an even more specific embodiment, the ion exchange membrane comprises Nafion, which is generally known in the art.
[0029] In certain embodiments, the ion exchange membrane further comprises a cellulosic substrate, preferably a paper substrate, more preferably a paper sheet substrate, even more preferably a paper sheet having a thickness of 1-50 gsm, preferably 2-30 gsm, more preferably 5-25 gsm.
[0030] In a more specific embodiment, the ion exchange membrane is made of an ion-conducting polymer, preferably a fluorinated polymer, preferably a fluorinated polymer having sulfonic acid moieties, more preferably a sulfonated tetrafluoroethylene-based fluoropolymer or a perfluorosulfonic acid (PFSA) polymer, even more preferably a tetrafluoroethylene-perfluoro-3,6-dioxa-4-methyl-7-octene sulfonic acid or copolymer. In an even more specific embodiment, the proton exchange membrane is made of Nafion, which is known in the art.
[0031] In a particular embodiment, each of the faces of the ion exchange membrane of the present invention has a surface area of 0.1 to 100,000 cm 2 , preferably 0.5 to 100 cm 2 , more preferably 1 to 50 cm 2 , and even more preferably, 1 to 20 cm2 , and even more preferably about 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 cm 2 It has an area of.
[0032] In certain embodiments, the thickness of the ion exchange membrane of the present invention is less than 100 microns, preferably less than 90 microns, more preferably less than 70 microns, and even more preferably less than 50 microns.
[0033] In a specific embodiment, the thickness of the ion exchange membrane of the present invention is 1 to 200 microns, preferably 2 to 100 microns, more preferably 3 to 90 microns, even more preferably 5 to 70 microns, and even more preferably 6 to 50 microns.
[0034] In more specific embodiments, the thickness of the ion exchange membrane is less than 40 microns, preferably less than 30 microns, more preferably less than 20 microns, even more preferably less than 15 microns, and even more preferably less than 11 microns.
[0035] In a more specific embodiment, the thickness of the ion exchange membrane is from 1 to 30 microns, preferably from 2 to 20 microns, and more preferably from 3 to 11 microns.
[0036] In some embodiments, the first and second diffusion layers are gas diffusion layers (GDLs). Each of the diffusion layers includes two opposing surfaces (e.g., the diffusion layers have a planar shape).
[0037] In another embodiment, the first diffusion layer and / or the second diffusion layer comprises a conductive material.Non-limiting examples of conductive materials suitable for the diffusion layer include carbon-based materials, such as carbon black, graphite or graphene; metal materials, such as metal particles; conductive organic molecules, such as conductive polymers, or mixtures thereof.
[0038] In a more specific embodiment, the first diffusion layer and / or the second diffusion layer comprises a conductive carbon-based material, preferably the conductive carbon-based material is selected from carbon black, graphite, graphene, or mixtures thereof, more preferably graphite.
[0039] In another more specific embodiment, the first diffusion layer and / or the second diffusion layer is made of a carbon-based material, preferably a conductive carbon-based material, more preferably the conductive carbon-based material is selected from carbon black, graphite, graphene, or mixtures thereof, even more preferably graphite.
[0040] In another embodiment, the first and / or second diffusing layer is obtained by depositing an ink by an additive technique.
[0041] In another embodiment, the first and / or second diffusing layer is obtained by screen printing, preferably by screen printing of an ink comprising a carbon-based material.
[0042] In certain embodiments, the first diffusion layer and / or the second diffusion layer are (a) depositing an ink comprising a carbon-based material on a substrate by an additive technique, preferably by screen printing; and (b) optionally separating the first diffusion layer and / or the second diffusion layer from the substrate; The method is obtained by a method comprising the steps of:
[0043] In a more particular embodiment, the substrate is a cellulosic substrate, such as paper, preferably a paper sheet, hi another embodiment, the substrate is a glass sheet, a flexible inert polymer foil, or a nonwoven fabric.
[0044] In certain embodiments, the ink comprises a carbon-based material. In certain embodiments, the carbon-based material of the ink is a conductive carbon-based material, preferably selected from carbon black, graphite, graphene, or mixtures thereof, more preferably graphite. In certain embodiments, the ink comprises a solid content of 10-90 wt%, more preferably 20-80 wt%, even more preferably 30-70 wt% of the total weight of the ink. In more specific embodiments, the solids of the solid content of the ink consist of conductive carbon-based material particles, preferably selected from carbon black, graphite, graphene, or mixtures thereof. In certain embodiments, the particle size of the solids of the ink is preferably 1 nm to 20 micrometers, preferably 2 nm to 18 micrometers, more preferably 5 nm to 15 micrometers.
[0045] In a more specific embodiment, the ink has a viscosity of 100 to 1000 Pas, preferably at a temperature of about 25° C., as measured by rheometer techniques.
[0046] In a specific embodiment, the surface of the first diffusion layer and / or the second diffusion layer of the present invention has a surface roughness of 0.1 to 100,000 cm 2 , preferably 0.5 to 100 cm 2 , more preferably 1 to 50 cm 2 , and even more preferably, 1 to 20 cm 2 , and even more preferably about 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 cm 2 , and even more preferably about 3 or 4 cm 2 It has an area of.
[0047] In certain embodiments, the thickness of the first diffusion layer and / or second diffusion layer of the present invention is less than 30 microns, preferably less than 20 microns, more preferably less than 12 microns, and even more preferably less than 11, 10, 9, 8, 7 or 6 microns.
[0048] In a specific embodiment, the thickness of the ion exchange membrane of the present invention is 1 to 60 microns, preferably 2 to 20 microns, and more preferably 3 to 16 microns.
[0049] In certain embodiments, the first diffusion layer and / or the second diffusion layer include pores, e.g., macropores, preferably they include slits. In some embodiments, the pores have an area of 1 to 10%, preferably 6 to 9%, of the total area of the diffusion layer.
[0050] Process (ii) In certain embodiments, step (ii) comprises coating two sides of the proton exchange membrane with the catalyst.
[0051] In certain embodiments, step (ii) comprises coating one face of each of the first and second diffusion layers with a catalyst.
[0052] In some embodiments, the coating in step (ii) is carried out by spray coating.
[0053] In a more specific embodiment, the catalyst is applied to the composition by spray coating, the composition comprising (i) 0.1-10 wt % of the catalyst by total weight of the composition, and (ii) a solvent or solvent mixture, preferably 0.5-6 wt % of the catalyst, more preferably 1-5 wt % of the catalyst.
[0054] In certain embodiments, the composition further comprises a polymer, preferably an ion-conducting polymer, more preferably a fluorinated polymer.
[0055] In a more specific embodiment, the solvent or solvent mixture of the composition comprises a polar solvent, preferably comprises water, and more preferably consists of a mixture of water and an organic alcohol.
[0056] In certain embodiments, the catalyst is selected from a metal, a metal oxide, an organometallic compound, a polymer, a biomolecule, or a mixture thereof.
[0057] In some embodiments, the catalyst comprises a metal element. In some embodiments, the metal element of the catalyst is selected from Ag, Pt, Ru, Ni, Co, Cu, Zn, Au, Ir, Fe, Mn, W, Mo, Pd, In, Rh, Re, Sn, La, or a mixture thereof, preferably Ag, Pt, Ru, and a mixture thereof.
[0058] In certain embodiments, the catalyst comprises a metal, a metal oxide, or a mixture thereof. In more particular embodiments, the catalyst comprises a metal deposited on a carbon substrate.
[0059] In another particular embodiment, the catalyst comprises a metal, a metal oxide, or a mixture thereof. In a more particular embodiment, the catalyst comprises a metal deposited on a carbon substrate.
[0060] In certain embodiments, the catalyst is 0.01-10mg / cm 2 , preferably 0.1 to 9 mg / cm 2 , more preferably 0.5 to 6 mg / cm 2 , and even more preferably 0.8 to 3 mg / cm 2 , and even more preferably about 1, 1.5, 2 or 2.5 mg / cm 2 In the amount of - one side of the ion exchange membrane and one side of one of the first and second diffusion layers; - two faces of an ion exchange membrane, or - one surface of each of the first and second diffusion layers; is coated.
[0061] The inventors have observed that spray coating of the catalyst has the advantage of good control of the amount of catalyst used and uniformity of the coverage. This technique also allows for high control of the roughness of the catalyst, thus improving the contact between the membrane and the catalyst.
[0062] Process (iii) The method of the present invention comprises the step (iii) of disposing an ion exchange membrane between the first and second diffusion layers, wherein both sides of the ion exchange membrane are in contact with a catalyst.
[0063] If two faces of the ion exchange membrane are coated with the catalyst, step (iii) comprises depositing, by an additive technique, one or two diffusion layers on one or two opposite faces of the ion exchange membrane, in particular depositing a diffusion layer on each face of the ion exchange membrane.
[0064] When one side of the diffusion layer is coated with a catalyst, step (iii) comprises: (a) depositing an ion exchange membrane onto the catalyst-coated surface of the diffusion layer, preferably by an additive technique such as screen printing; and (b) optionally, and preferably by an additive technique, such as screen printing, depositing a separate diffusion layer on top of the ion exchange membrane; It may be performed by
[0065] In certain embodiments, one side of the ion exchange membrane or one side of the diffusion layer is coated with a catalyst, such that both sides of the ion exchange membrane are in contact with the catalyst.
[0066] In a more particular embodiment, the first and second diffusing layers are obtained by an additive technique, for example, screen printing.
[0067] Process (iv) Step (iv) of the method of the present invention is directed to joining the first diffusion layer, the ion exchange membrane and the second diffusion layer, optionally under pressure and / or heat.
[0068] Step (iv) of the process of the present invention may be carried out by any technique known in the art, preferably under pressure and / or heat.
[0069] In a particular embodiment, the temperature is between 90 and 150°C, preferably between 100 and 140°C, and even more preferably about 130°C.
[0070] In certain embodiments, the pressure is between 0.1 and 1 ton, preferably between 0.2 and 0.8 ton, and even more preferably about 0.5 ton.
[0071] In the method of the present invention, the ion exchange membrane is obtained by a casting technique or by a screen printing technique, and at least one diffusion layer is obtained by an additive technique. In a particular embodiment, two diffusion layers are obtained by an additive technique.
[0072] In one embodiment, the ion exchange membrane is obtained by a method comprising the steps of: (a) depositing on a substrate a composition comprising 1-30 wt % of an ion-conducting polymer in a solvent or solvent mixture; and (b) optionally separating the deposited ion exchange membrane from the substrate; preferably, the ion-conducting polymer is a fluorinated polymer.
[0073] In certain embodiments, the composition has 1-30 wt% fluorinated polymer of the total weight of the composition, preferably the composition has 2-28 wt% fluorinated polymer, more preferably the composition has 3-24 wt% fluorinated polymer, and even more preferably the composition has about 5 wt%, 10 wt%, 15 wt% or 20 wt% fluorinated polymer.
[0074] In a more specific embodiment, the solvent or solvent mixture comprises a polar solvent, preferably comprises water, and more preferably consists of a mixture of water and an organic alcohol, such as ethanol, propanol, derivatives and mixtures thereof.
[0075] In one embodiment, the ion exchange membrane is obtained by a method comprising the steps of (a) depositing on a substrate a composition comprising 1-30 wt % of a fluorinated polymer in a solvent or solvent mixture, wherein the substrate is a cellulosic substrate, e.g., a paper sheet, and preferably the deposition is carried out by tape casting techniques or drop casting, preferably by doctor blading.
[0076] In certain embodiments, the substrate in step (a) is a cellulosic substrate obtained by immersing the cellulosic substrate in a composition comprising 0.5-50 wt% of fluorinated polymer in a solvent or solvent mixture. In certain embodiments, the fluorinated polymer is present in the composition at 1-30 wt%, preferably 10-25 wt%, more preferably 15-22 wt%, more preferably about 20 wt%. In more specific embodiments, the immersion step is performed under mechanical mixing, preferably ultrasonic mixing.
[0077] In a more specific embodiment, the ion exchange membrane is obtained by a method comprising the steps of: (a) depositing on a substrate a composition comprising 1-30 wt % of a fluorinated polymer in a solvent or solvent mixture; and (b) separating the deposited ion exchange membrane from the substrate, wherein the deposition is carried out by a tape casting technique, preferably by doctor blading, and optionally the substrate is a glass substrate, preferably a glass slide.
[0078] In the context of the present invention, the expression "doctor blading or doctor blade" refers to a coating technique that is performed by placing a sharp blade a fixed distance from the surface to be coated, then placing a coating composition in front of the blade and moving the blade in line across the surface to create a film or layer on said surface, a technique that is commonly understood in the art.
[0079] In certain embodiments, deposition is preferably carried out by applying 1 to 20 layers, preferably by applying 2 to 10 layers, by doctor blading.
[0080] In certain embodiments, the deposited ion exchange membrane is separated from the substrate by adding water and waiting at least 10 minutes, preferably at least 1 hour, more preferably at least 4 hours, and even more preferably 5 to 10 hours, for the membrane to detach from the surface.
[0081] In a more specific embodiment, the ion exchange membrane is pressed, preferably hot pressed, more preferably at 40-100° C., more preferably at 60-90° C., even more preferably at about 80° C. The inventors have observed that by pressing the ion exchange membrane, excess solvent is removed and the ion exchange membrane becomes flat.
[0082] Membrane Electrode Assembly (MEA) One aspect of the present invention is directed to a membrane electrode assembly (MEA) obtainable by the method of manufacture defined in any of the specific embodiments of the present invention.
[0083] Any of the properties described above for the ion exchange membrane, first diffusion layer, second diffusion layer, or catalyst in any of the specific embodiments of the method may apply to the ion exchange membrane, first diffusion layer, second diffusion layer, or catalyst of a membrane electrode assembly (MEA) described herein.
[0084] In certain embodiments, the membrane electrode assembly (MEA) has a thickness that is less than 250 microns, preferably less than 200 microns, more preferably less than 100 microns, even more preferably less than 60 microns, and even more preferably less than 55 microns.
[0085] cell Another aspect of the present invention is a method for producing a a membrane electrode assembly (MEA) as defined in any of the particular embodiments of the present invention, and o Means for connecting to power / load sources; Compartment containing Target cells that contain
[0086] In certain embodiments, the means for connecting to the power source / load source is a means for electrically connecting to the power source / load source and may be any means known in the art, such as an electrical wire, etc. In certain embodiments, the means for connecting is capable of electrically connecting the MEA and / or the current collector to the power source / load source.
[0087] In certain embodiments, the cell further includes a power / load source.
[0088] The power source / load source may be any external electric device, e.g., a power grid, an electric vehicle, a domestic appliance, or a sensor that draws / transfers energy from / to a battery. In general, a power source / load source has a controllable voltage and / or current supply or draw.
[0089] In certain embodiments, the cell further comprises a current collector. In some embodiments, the MEA is sandwiched between the current collectors. In some embodiments, the current collector comprises metal particles, preferably silver particles.
[0090] In certain embodiments, the current collector has a final thickness of at least 1 micron, preferably at least 2 microns, and more preferably between 5 and 15 microns.
[0091] In a more particular embodiment, the current collector of the cell is obtained by depositing a composition comprising metal particles in a solvent or solvent mixture, preferably by depositing silver particles in a solvent or solvent mixture.
[0092] In a more particular embodiment, the current collector of the cell is obtained by screen printing.
[0093] In more particular embodiments, each of the current collectors covers one of the faces of the two MEAs (i.e., the current collectors have areas that coincide with the printed MEA areas), and optionally the current collectors include a means for connecting, preferably a connector having the 4 pin / track design of a standard USB Series A plug connector. In particular embodiments, the connectors are screen printed.
[0094] In one embodiment, a current collector is in contact with each surface of the diffusion layers of the MEA.
[0095] In some embodiments, the cell includes at least one dielectric layer, preferably in contact with a surface of the current collector. In certain embodiments, the at least one dielectric layer includes a polymer, preferably an acrylic polymer. In more specific embodiments, the cell includes at least two dielectric layers, one on each side of the MEA, in contact with the current collector.
[0096] The cells of the present invention may include an outer case.
[0097] use An additional aspect is directed to the use of a membrane electrode assembly (MEA) as defined in any of the specific embodiments of the invention, or of a cell as defined in any of the specific embodiments of the invention, for electrochemical detection, preferably amperometric or potentiometric, of an analyte.
[0098] Certain aspects of the invention are directed to a method for electrochemical detection of an analyte, preferably amperometrically or potentiometrically, comprising using a membrane electrode assembly (MEA) of the invention as defined in any of the specific embodiments, or a cell as defined in any of the specific embodiments of the invention.
[0099] A final aspect is directed to the use of a membrane electrode assembly (MEA) as defined in any of the specific embodiments of the invention, or of a cell as defined in any of the specific embodiments of the invention, for storing and / or transmitting energy, preferably electricity, preferably where the membrane electrode assembly (MEA) or cell is part of a fuel cell.
[0100] One aspect of the invention is directed to a method for storing and / or transmitting energy, preferably electricity, comprising using an MEA or cell of the invention as defined in any of the specific embodiments, preferably wherein the MEA or cell is part of a fuel cell.
[0101] It is to be understood that the scope of the present disclosure includes all possible combinations of the embodiments disclosed herein. EXAMPLES
[0102] The present invention will now be described in further detail with reference to the following examples, which are for illustrative purposes only and are not intended to limit the scope of the invention.
[0103] Example 1: Membrane Electrode Assembly (MEA) with Screen Printed Gas Diffusion Layers (GDL) The catalyst ink was prepared by mixing water, isopropanol and the commercially available Nafion® 117 composition (Nafion is 5 wt% in a mixture of lower aliphatic alcohols and water) with 3 wt% of catalyst. The catalysts used were Pt / C catalyst powder (from Merck), PtB (platinum black) or RuO2 particles (from Thermo Fisher). The ink was sonicated for 30 minutes (Ultrasons Selecta 3000683, 50 / 60 kHz, 110 W). Nafion is understood as a generic name for sulfonated tetrafluoroethylene-based fluoropolymer-copolymer.
[0104] Membrane electrode assemblies (MEAs) were prepared by the catalyst coated membrane (CCM) method: first, electrodes (anodes and / or cathodes) were prepared by depositing the above ink onto one or two opposite sides of a commercial proton exchange membrane Nafion® 212 (tetrafluoroethylene-perfluoro-3,6-dioxa-4-methyl-7-octenesulfonic acid NR-212 membrane with a thickness of about 51 microns) using spray deposition (spray nozzle 2W, catalyst ink flow rate 300 μl / min, air pressure 130 mbar, spray speed 1500 mm / min) to create a catalyst coated membrane (CCM), with a concentration of about 1 mg / cm. 2 of Pt (cathode side) and approximately 2 mg / cm 2 The nanoparticle concentrations on each side of RuO2 (anode side) were obtained.
[0105] Each side of the catalyst coated membrane was then coated with a gas diffusion layer (GDL) by screen printing using carbon paste purchased from Carbon Creative or Sun Chemical (Ref. C2030519P4, with a solid content of 39.0-43.0% at 130 °C). The GDL was printed using a medium size pneumatic flat screen printer (model AT-60FA) manufactured by ATMA and subsequently thermally cured at 130 °C (15 min) in a Memmert UN160 lab oven. The results showed that the carbon layers printed from Carbon Creative (Ref.: 122-49) and Graphite Sun chemical inks had thicknesses of 10-14 and 7-18 μm, respectively.
[0106] Silver nanoparticle ink was then screen printed on top of each GDL as a current collector. The ink was purchased from DuPont (Ref. 5000, with a solids content of 58-62%). The current collectors were printed using an ATMA medium size pneumatic flat screen printer (model AT-60FA) and subsequently thermally cured at 130°C (10 min) in a Memmert UN160 lab oven.
[0107] Alternatively, membrane electrode assemblies (MEAs) were prepared by the catalyst coated substrate (CCS) method: first, GDLs were screen printed as described above. Then, the catalyst ink described above was deposited on one side of the GDL. A Nafion membrane was added on top of the catalyst coated GDL. Then, another GDL coated with catalyst was deposited on top of the Nafion membrane (with the catalyst in contact with the Nafion membrane). Then, silver nanoparticle ink was screen printed on top of each GDL as a current collector.
[0108] When the catalyst was deposited by spray deposition, the average roughness Ra of the surface was measured and the results showed that spray coating of the catalyst had the advantage of good control of the average roughness of the coated surface. Measurements of the average roughness (arithmetic mean deviation from the mean line in the profile being evaluated) were performed using a Dektak 150 surface profilometer. For example, the average roughness of the GDL coated with the catalyst was in the range of 950-1200 nm.
[0109] In addition, the results showed that GDLs with thicknesses significantly less than commercially available ones were prepared using the above method. The conductivity of the GDLs synthesized as described above was tested for their thickness using a four-point probe system. In particular, equidistant and colinear probes were used to make electrical contacts with the characterized materials known in the art. The thickness of the GDLs was measured by profilometry techniques. The GDL results showed that the highest conductivity values were obtained when the thickness of the catalyst-deposited GDLs was about 8.4 microns for the Sun Chemical GDL and about 15.3 microns for the Carbon Creative GDL. The results also showed that an increase in the thickness of the GDLs resulted in a decrease in their conductivity. In addition, the best conductivity results were obtained for the SunChemical GDL.
[0110] The stability of the catalyst-deposited GDL was also tested at different pH and temperature. The screen-printed GDL layer showed easy operation, uniform surface, and high conductivity when compared to the conventional GDL.
[0111] In some cases, a dielectric ink purchased from Sun Chemical (Ref. suntronic 681, acrylate-based ink) was screen printed on top of each side of any of the MEAs described above using a medium-sized pneumatic flat screen printer (model AT-60FA) from ATMA, followed by UV curing using a UV lamp (model HOC-35 / 1-200 / BE OBC, from BCB) to encapsulate the entire device area.
[0112] If both GDLs are screen-printed, no additional bonding process under pressure and / or heat is required. It has also been observed that MEAs with screen-printed GDLs have good adhesion and therefore good charge transfer between the layers of the MEA. In addition, the manufacturing process is simplified.
[0113] In cases where one of the GDLs was commercially available, an additional bonding step was performed, specifically hot pressing for 15 minutes at 130° C. under 0.5 tonnes using a hot pressing machine CARVER Model 4386 Bench Top Laboratory Manual Press with electrically heated platens.
[0114] Example 2: Membrane Electrode Assembly (MEA) with Membrane Synthesized by Doctor Blading Technique The MEA was prepared according to Example 1, except that the membrane was prepared as follows.
[0115] A Nafion perfluorinated resin composition of 5 wt.% in lower aliphatic alcohol and water was deposited on a glass slide by doctor blading technique. Doctor blade coating or doctor blading is a technique used to create a film with a well-defined thickness. This technique works by placing a sharp blade at a fixed distance from the surface that needs to be coated. The coating composition is then placed in front of the blade and the blade is moved across the surface in a straight line to create a layer or a very thin film.
[0116] The membranes were detached from the glass slide substrate by adding water and detaching the membrane from the glass substrate overnight. The thickness of the Nafion membranes ranged from 1 to 7 microns for 2 to 10 layers applied by doctor blade technique.
[0117] Figure 1 shows an exploded view of the MEA, and Figure 2 shows an SEM micrograph of the MEA with a screen-printed Nafion membrane.
[0118] Example 3: Membrane Electrode Assembly (MEA) with Paper-Nafion Membrane The MEA was prepared according to Example 1, except that the membrane was prepared as follows.
[0119] First, a 3 cm x 3 cm piece of paper (LEINE SILK 20 gsm (grams per square meter) paper from SAPPI) was immersed in a Nafion composition in which Nafion was 20 wt% based on the total weight of the composition in low aliphatic alcohol and water, and was sonicated in an Elmasonic S100H for 30 minutes in a closed jar. Then, 200 μl of the Nafion composition was deposited on the top surface of the paper by doctor blade method.
[0120] The membrane was air-dried overnight and then hot-pressed (CARVER PRESS, 0.2 metric ton) at 80° C. for 5 minutes to remove excess solvent and flatten the SAPPI / Nafion membrane before use. The proton exchange membrane obtained by this method has an amount of Nafion of about 50% by weight of the total weight of the membrane. The advantage of the method described above is that the thickness of the proton exchange membrane obtained thereby can be reduced by reducing the amount of Nafion deposited on the paper.
[0121] 3 shows polarization curves for (a) an MEA containing a paper-Nafion membrane prepared according to this example, and (b) an MEA containing a commercial Nafion membrane (Nafion 212 membrane) prepared according to Example 1. Both MEAs show good performance. The MEA containing the paper-Nafion membrane shows a higher current density when compared to a similar MEA containing a commercial membrane.
[0122] In addition, MEAs were prepared using paper-Nafion membranes after the CCM and CCS methods described in Example 1. The MEAs were electrochemically tested. Figure 4 shows the cell potential (V) versus current density (mA.cm) for MEAs containing (a) paper-Nafion membranes obtained by the CCM method and (b) paper-Nafion membranes obtained by the CCS method. -2 ) are shown. Both MEAs show good performance. However, the MEA containing the paper-Nafion membrane obtained by the CCM method shows a higher potential value than the one obtained by the CCS method.
[0123] The properties of a commercial Nafion membrane (Nafion® 212, a commercial proton exchange membrane), a paper membrane (SAPPI LEINE SILK 20 gsm paper), and the paper-Nafion membrane synthesized as described above were compared by contact angle tests, stress-strain curve measurements, and thermogravimetric analysis (results not shown here).
[0124] Figure 5 shows the results of dynamic mechanical analysis of stress-strain experiments on (a) paper membrane, (b) Nafion-paper membrane, and (c) bulk Nafion 212 membrane. At strains below 0.2%, the curves for the paper-Nafion membrane match those of the bulk Nafion membrane, and at strains above 0.2%, the Nafion-paper membrane shows a slope similar to that of paper.
[0125] Figure 6 shows the results of contact angle tests for (a) paper membrane, (b) Nafion-paper membrane, and (c) bulk Nafion membrane. In particular, the paper-Nafion membrane can maintain its shape for at least 20 minutes after contact with a water droplet, while the paper membrane absorbs water and the Nafion membrane deforms. In addition, the mechanical properties of the paper-Nafion membrane are a combination of the mechanical properties of the bulk Nafion and the paper substrate.
[0126] Thermogravimetric analysis results of paper, Nafion-paper and Nafion membranes confirm that the Nafion-paper membrane exhibits a blend of properties of Nafion and paper.
[0127] Example 4: Membrane Electrode Assembly (MEA) with Spray-Coated Membrane MEAs were prepared according to Examples 1, 2 or 3, but by adding a Nafion membrane by spray coating technique. The proton exchange membrane obtained by printing has a thickness of approximately 30 microns. The advantage of this spraying method is that the thickness of the proton exchange membrane obtained thereby can be reduced by reducing the amount of Nafion deposited by spray coating.
[0128] Example 5: Membrane Electrode Assembly (MEA) with Screen Printed Electrodes MEAs were prepared according to Examples 1, 2, 3 or 4, except that the catalyst was added by screen printing technique.
[0129] Example 6: Membrane Electrode Assemblies (MEAs) with Different Gas Diffusion Layer (GDL) Shapes Different MEAs were prepared according to Examples 1, 2, 3 or 4, except that the shape of the gas diffusion layer (GDL) was modified. The GDL was 2×2 cm 2 with an operating area of 2.25×0.5cm 2 The connector was
[0130] In addition, different working areas and porosities were studied: 4 cm 2 3 cm 2 with no macropores (i.e., bulk (B)) and with square and rectangular macropores shaped as windows (W) and slits (S). 2The pore area is 1 mm 2 ~50mm 2 The number of pores also varied from 1 to 100.
[0131] The result was 3cm. 2 The MEA containing a GDL with an area of 4 cm and macropores 2 100 nm and exhibited no loss in performance in terms of current density when compared to having a GDL without pores.
[0132] In addition, the result is 3 cm 2 of operating area and 25mm 2 It was shown that a GDL with rectangular macropores shaped as slits (S) presented better performance.
[0133] Example 7: Characterization of MEAs MEAs prepared according to any of the above examples were characterized by the following techniques.
[0134] Thermogravimetric analysis (TGA) was performed on a TGA / DSC METTLER TOLEDO STAR system from JULABO Labortecknik GmbH. Samples were dried in an oven at 80°C prior to analysis. TGA tests were performed at 37°C for approximately 10 min under nitrogen gas. -1 The experiment was carried out with a temperature gradient of approximately 15 mg of sample.
[0135] Infrared spectra were recorded using a PerkinElmer Spectrum 100 FT-IR spectrometer, scanning the region ranging from 4000 to 750.
[0136] The morphology of the MEAs was studied by an FEI Quanta 650 FEG field emission scanning electron microscope (ESEM). Sample preparation was performed as follows: for cross-sections, samples were prepared by cutting with a razor blade at ambient temperature. No liquid nitrogen was used. The samples were then mounted on a cross-section specimen holder in the Quanta 650 FEG ESEM and operated in low vacuum mode using a backscattered electron detector. For top views, samples were affixed with carbon tape and mounted on aluminum stubs. The samples were then mounted in the Quanta 650 FEG ESEM and, since the sample surface is conductive, the SEM was operated in high vacuum mode using a secondary electron detector and, where necessary, a backscattered electron detector.
[0137] Electrochemical tests were performed using a PGSTAT204 potentiostat / galvanostat from Metrohm Autolab BV equipped with a frequency response analyzer (FRA) and a 10 A booster (BSTR10A) module. Linear sweep voltammetry and cyclic voltammetry (CV) were performed at 50 mV s -1 Electrochemical impedance spectroscopy (EIS) measurements were performed using a potential perturbation of 10 mV.rms. The frequency range was 10 mHz. -1 MHz.
[0138] Water contact angle studies were performed using a KRUSS DSA E20 contact angle goniometer instrument using the stationary drop method.
[0139] The results showed that the reduction in thickness of the MEAs of the examples results in a reduction in the diffusion barrier and better performance than the commercial MEAs with a total thickness of 300-800 microns. This is especially evident in the MEAs obtained in examples 2, 3 and 4. In addition, the paper-Nafion membranes and the screen-printed membranes have additional advantages, such as a reduction in the amount of Nafion used, an increase in water diffusion, and a reduction in the conditioning time of the membrane, thus increasing the performance of the MEA.
[0140] Example 8: Membrane Electrode Assembly (MEA) with screen printed current collectors following the 4 pin / track design of a standard USB Series A plug connector MEAs were prepared according to Examples 1, 2, 3, 4, 5 or 6, but including a printed screen-printed current connector layer that (i) covers the face of the MEA and (ii) also creates a connection printed according to the 4-pin / track design of a standard USB Series A plug connector known in the art (see FIG. 7).
[0141] Example 9: Electrochemical detection of ferrocene using a membrane electrode assembly (MEA) Experimental electrochemical detection of ferrocene is carried out using the membrane electrode assembly (MEA) of the present invention described in any of the previous experiments using cyclic voltammetry technique. In the setup, the MEA is connected to a potentiostat. In addition, the MEA may need to be pre-wetted. A droplet of sample that may contain the analyte to be detected is then inserted by drop casting onto the working area of the MEA and the cyclic voltammetry technique is carried out. The results obtained are compared with those previously obtained for different concentrations of the analyte (i.e., ferrocene) to determine the presence or absence of the analyte.
[0142] Comparative Example 10: Conventional Membrane Electrode Assembly (MEA) The catalyst ink was prepared by mixing water, isopropanol and Nafion® (Nafion is a 5 wt% solution of Nafion® perfluorinated resin in lower aliphatic alcohols and water) and catalyst. The catalysts used were Pt / C catalyst powder for the cathode or RuO2 particles for the anode. The ink was sonicated (Elmasonic S100H) for at least 1 hour before use.
[0143] Electrodes (anodes and / or cathodes) were prepared by depositing the above ink directly onto a carbon GDL (carbon paper H23C2 GDL) using an automated ultrasonic spraying device (spray nozzle AccuMist, catalyst ink flow rate 300 μl / min, air pressure 100 mbar, spray speed 2500 mm / min). A commercial proton exchange membrane Nafion® 212 (Nafion® 212, a commercial proton exchange membrane with a thickness of about 40-60 microns) was added on top of the catalyst-coated GDL. Then, another GDL (carbon paper H23C2 GDL) coated with catalyst was deposited on top of the Nafion membrane (with catalyst in contact with the Nafion membrane) to a concentration of about 1 mg / cm. 2 Pt (cathode side) and RuO2 at approximately 2 mg / cm 2 (anode side) resulting in nanoparticle concentrations on each side. Finally, a Ti foil external current collector pressed on top of the carbon GDL was required to achieve a functional MEA.
[0144] The amounts of reagents and materials used, as well as the thickness of each layer of the resulting MEA, are given in Table 1. For comparison purposes, a fully printed MEA prepared according to an embodiment of the invention (electrodes and current collectors of both GDLs were obtained by screen printing) prepared with a conventional Nafion® 212, a commercially available proton exchange membrane, is also given in Table 1.
[0145] [Table 1]
[0146] The results show a reduction in thickness and amount of material for the fully printed MEAs. As can be seen from Table 1, a significant reduction in the current collector and GDL layers was achieved with the fully printed MEAs of the present invention. Figure 8 provides scanning electron microscopy (SEM) images showing the total thickness of (a) the fully printed MEA and (b) the conventional MEA. Remarkably, the fully printed MEA of the present invention with the printed metal current collector shows a thickness approximately 65 times less than the MEA obtained by the conventional approach using an external Ti foil current collector.
[0147] Furthermore, the results showed that the fully printed MEA of the present invention provides performance comparable to that of a conventional MEA. Figure 9 shows the polarization curve results for (a) a fully printed MEA, and (b) a conventional MEA prepared according to Comparative Example 10. Both MEAs show good performance.
[0148] The inventors have surprisingly found that the reduced thickness of the fully printed MEA of the present invention contributes positively to improved connection at the layer interface, resulting in good performance of the fully printed MEA using a significantly smaller amount of material.
Claims
1. 1. A method for manufacturing a membrane electrode assembly (MEA), comprising the steps of: i. an ion exchange membrane having two opposite faces, and a first diffusion layer and a second diffusion layer comprising a carbon material, each of the first and second diffusion layers having two opposite faces; preparing ii. a catalyst; - one face of the ion exchange membrane and one face of one of the first and second diffusion layers; - the two faces of the ion exchange membrane, or - one face of each of said first and second diffusing layers; A step of coating the iii. disposing the ion exchange membrane between the first and second diffusion layers, wherein both sides of the ion exchange membrane are in contact with the catalyst; and iv. optionally bonding the first diffusion layer, the ion exchange membrane and the second diffusion layer under pressure and / or heat; Including, At least one of the first and second diffusion layers and the ion exchange membrane is obtained by an additive technique; A method comprising:
2. 2. The method of claim 1, wherein the ion exchange membrane is a proton exchange membrane obtained by a method comprising the steps of: (a) depositing, by an addition technique, on a substrate a composition comprising 1-30 wt. % of a fluorinated polymer in a solvent or solvent mixture; and (b) optionally separating the deposited proton exchange membrane from the substrate.
3. 3. The method of claim 2, wherein the substrate is a cellulosic substrate, e.g. paper, preferably pre-soaked in a composition comprising 1-30 wt % of a fluorinated polymer in a solvent or solvent mixture.
4. The method according to any one of claims 2 to 3, wherein the depositing in step (a) is carried out by tape casting technique, preferably by doctor blading technique.
5. A method according to any one of claims 1 to 4, wherein the diffusion layer obtained by an additive technique is obtained by screen printing of an ink comprising a carbon-based material, preferably an ink comprising graphite.
6. The method according to any one of claims 1 to 5, wherein the catalyst comprises a metal element selected from Ag, Pt, Ru, Ni, Co, Cu, Zn, Au, Ir, Fe, Mn, W, Mo, Pd, In, Rh, Re, Sn, La, or a mixture thereof.
7. further comprising a step of coating two sides of the ion exchange membrane with the catalyst to obtain a catalyst-coated ion exchange membrane; The method according to any one of claims 1 to 6, wherein the diffusion layer obtained by an additive technique is obtained by screen printing on at least one face of the catalyst-coated ion exchange membrane.
8. The catalyst is coated by spray coating of a composition, the composition comprising: - 0.1 to 10 wt. % of a catalyst based on the total weight of the composition, and - Solvent or solvent mixture The method according to any one of claims 1 to 7, comprising:
9. The amount of the catalyst is 0.1 to 10 mg / cm 2 The method according to any one of claims 1 to 8,
10. A membrane electrode assembly (MEA) obtainable by the manufacturing method according to any one of claims 1 to 9, wherein at least one of the first and second diffusion layers has a thickness of less than 30 microns.
11. 11. The membrane electrode assembly (MEA) of claim 10, wherein the ion exchange membrane has a thickness of less than 11 microns.
12. - a compartment comprising a membrane electrode assembly (MEA) according to any one of claims 10 or 11, and - Means for connecting to the power / load source The cell that contains
13. 13. The cell of claim 12, further comprising a plurality of current collectors comprising metallic particles, the MEA being sandwiched between said current collectors.
14. Use of a membrane electrode assembly (MEA) according to any one of claims 10 or 11 or of a cell according to any one of claims 12 or 13 for the electrochemical detection of an analyte, preferably for the electrochemical detection of ferrocene.
15. 14. Use of a membrane electrode assembly (MEA) according to any one of claims 10 or 11, or of a cell according to any one of claims 12 or 13, for storing and / or transmitting energy, preferably electricity, preferably wherein said membrane electrode assembly (MEA) or said cell is part of a fuel cell.